Gel-type thermal interface material
A silicone-based thermal interface material with specific molecular weight oils and fillers, along with addition inhibitors, addresses the limitations of conventional materials by providing improved thermal conductivity and resistance to cracking and dripping, ensuring effective heat transfer in electronic components.
Patent Information
- Application Number
- JP2021003897
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-07-05
- Filing Date
- 2021-01-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2037-07-11
AI Technical Summary
Conventional thermal interface materials face challenges in meeting thin thickness requirements for automated manufacturing and exhibit issues such as dripping and cracking during temperature cycling, limiting their effectiveness in transferring heat from electronic components.
A thermal interface material comprising a combination of low and high molecular weight silicone oils, thermally conductive fillers, and addition inhibitors, including alkynyl compounds, which are formulated to provide improved thermal conductivity and resistance to cracking and dripping.
The material demonstrates enhanced thermal conductivity and resistance to temperature cycling, maintaining integrity and position during high stress testing, ensuring effective heat transfer without significant cracking or dripping.
Smart Images

Figure 0007584307000011 
Figure 0007584307000012 
Figure 0007584307000013
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application is a continuation of U.S. Provisional Patent Application No. 62 / 366,704, filed July 26, 2016. No. 62 / 436,746 filed on December 20, 2016. The disclosures of which are expressly incorporated herein by reference in their entireties. Be absorbed.
[0002] The present disclosure relates generally to thermal interface materials, and more specifically to gel-type thermal interface materials. . [Background technology]
[0003] Thermal interface materials (TIM) are , central processing units, video graphics arrays, servers, game consoles, smartphones, It is widely used to dissipate heat from electronic components such as LED boards. Thermal interface materials are Typically, a heat sink is used to transfer excess heat from an electronic component to a heat spreader, such as a heat sink. It is used for this purpose.
[0004] A typical electronic packaging structure 10 including a thermal interface material is shown in FIG. The cage structure 10 illustratively includes a heat generating component, such as an electronic chip 12, and a heat spreader 14. and one or more heat dissipation components, such as a heat sink 16. The heat sink may be made of copper, copper alloy, aluminum, aluminum alloy, or nickel. Examples of suitable materials include metals such as tin-plated copper, metal alloys, or metal-plated substrates. A TIM material, such as M20, provides a thermal connection between a heat-generating component and one or more heat-dissipating components. The electronic packaging structure 10 includes a first electrode that connects an electronic chip 12 to a heat spreader 14. TIM18 is usually called "TIM1". The structure 10 includes a second TIM 20 that connects the heat spreader 14 and the heat sink 16. TIM20 is typically referred to as "TIM2." In another embodiment, The package structure 10 does not include a heat spreader 14, and the TIM (not shown) is The electronic chip 12 is directly connected to the heat sink 16. Such a connecting TIM is typically referred to as TIM1.5.
[0005] Conventional thermal interface materials include components such as gap pads. The chap pad cannot meet the requirements of very thin thickness, automated manufacturing However, it has several disadvantages, such as being difficult to use.
[0006] Other thermal interface materials include gel products, which are suitable for large scale production. The gel can be automatically dispensed and formed into a desired shape and thickness. The product may be subjected to a variety of temperature changes, including, in extreme cases, a higher likelihood of the product failing. It has problems with dripping and cracking during cycle testing.
[0007] Improvements to the above are desirable. Summary of the Invention
[0008] The present disclosure relates to a heat spreader and a heat dissipation device for removing heat from a heat generating electronic device such as a computer chip. A thermal interface material useful for transferring heat to a heat dissipating structure, such as a sink, is provided. The thermal interface material comprises: At least one silicone oil, at least one thermally conductive filler, and at least one Includes additional inhibitors.
[0009] In one exemplary embodiment, a thermal interface material is provided. The thermal interface material is 50,000 daltons. at least one low molecular weight silicone oil having a weight (Mw) average molecular weight of less than a ton; At least one thermally conductive filler, at least one additive catalyst, and at least one high and a high molecular weight silicone oil, the high molecular weight silicone oil having a molecular weight of at least 60,000 Daltons. The vinyl-functional silicone oil has a weight (Mw) average molecular weight of In the embodiment, at least one low molecular weight silicone oil is a first silicone oil and a second silicone oil. and corn oil, wherein the first silicone oil is a vinyl-functional silicone oil and the second silicone oil is a vinyl-functional silicone oil. Licorice oil is a hydride-functional silicone oil.
[0010] In a more specific embodiment, the thermally conductive filler comprises a first thermally conductive filler and a second thermally conductive filler. and a thermally conductive filler, the first thermally conductive filler having a particle size greater than 1 micron. and the second thermally conductive filler has a particle size of less than 1 micron. In another more specific embodiment, the thermally conductive filler is a first thermally conductive metal oxide. a first thermally conductive filler, a second thermally conductive filler, and a third thermally conductive filler, The filler is a metal oxide having an average particle size greater than 10 microns, and the second heat The conductive filler is a metal oxide having an average particle size of 1 micron to 10 microns. and the third thermally conductive filler is a metal oxide having an average particle size of less than 1 micron. .
[0011] In yet another more specific embodiment, the thermal interface material comprises between 2% and 20% by weight of a low molecular weight Silicone oil, 50% to 95% by weight of a thermally conductive filler, and 0.1% to 5% by weight of In yet another more specific embodiment, the silicone oil comprises a low molecular weight silicone oil. The silicone oil comprises a first silicone oil and a second silicone oil, and the first silicone oil is the first silicone oil is a hydride-functional silicone oil and the second silicone oil is a hydride-functional silicone oil. be.
[0012] In a more specific embodiment of any of the above embodiments, a thermal interface material is provided. The thermal interface material comprises at least one silicone oil and at least one thermally conductive filler. and at least one addition inhibitor, the addition inhibitor comprising an alkynyl compound. In a more specific embodiment, the addition inhibitor is a multivinyl functional polysiloxane, ethynyl Polydimethylsiloxane vinyl terminated with cyclohexanol, 2-methyl-3-butyne -2-ol, and 3-methyl-1-pentyn-3-ol. In more specific embodiments of any of the above embodiments, the at least one silicone The silicone oil comprises a first silicone oil and a second silicone oil, and the first silicone oil is the first silicone oil is a hydride-functional silicone oil and the second silicone oil is a hydride-functional silicone oil. be.
[0013] In a more specific embodiment of any of the above embodiments, the thermally conductive filler is a first and a second thermally conductive filler, the first thermally conductive filler being 1 mm. The second thermally conductive filler is a metal having a particle size smaller than 1 micron. A more specific embodiment of any of the above embodiments is a metal oxide having a particle size of less than 100 nm. In one embodiment, the ratio of the first thermally conductive filler to the second thermally conductive filler is 1.5:1 to The ratio is 3:1.
[0014] In a more specific embodiment of any of the above embodiments, the thermal interface material comprises 2% by weight ~20% by weight of silicone oil, 0.1% by weight to 5% by weight of a silane coupling agent, 0% to 95% by weight of a thermally conductive filler and 0.01% to 5% by weight of an addition inhibitor; In a more specific embodiment, the addition inhibitor is terminated with ethynylcyclohexanol. In a more specific embodiment, the silicone oil is polydimethylsiloxane vinyl. , a first silicone oil and a second silicone oil, the first silicone oil being vinyl the first silicone oil is a hydride-functional silicone oil and the second silicone oil is a hydride-functional silicone oil. .
[0015] In one exemplary embodiment, an electronic component is provided. The electronic component includes a heat sink and an electronic A thermal interface material including a chip, a first surface layer, and a second surface layer, the thermal interface material being and a thermal interface material disposed between the heat sink and the electronic chip, the thermal interface material being at least one silicone. oil, at least one thermally conductive filler, and at least one addition inhibitor; In a more specific embodiment, the inhibitor comprises an alkynyl compound. The silicone oil comprises at least one low molecular weight silicone oil and at least one high molecular weight silicone oil. Contains oil.
[0016] In a more specific embodiment, the at least one high molecular weight silicone oil has at least 6 The vinyl-functional silicone oil has a weight (Mw) average molecular weight of 0,000 Daltons. In another more specific embodiment, the first surface layer is in contact with the surface of the electronic chip and the second The surface layer is in contact with the heat sink. In another more specific embodiment, the electronic component comprises: a heat spreader disposed between the heat sink and the electronic chip; A first surface layer contacts the surface of the electronic chip, and a second surface layer contacts the heat spreader. In a more specific embodiment, the electronic component is disposed between the heat sink and the electronic chip. The first surface layer contacts a surface of the heat spreader, and the second surface layer contacts a surface of the heat spreader. The surface layer of 2 is in contact with the heat sink. [Brief description of the drawings]
[0017] Reference is now made to the following description of several embodiments of the invention in conjunction with the accompanying drawings, in which: Thus, the above and other features and advantages of the present disclosure, and the manner in which they are achieved, will become more apparent. This will make it clearer and the invention itself will be better understood.
[0018] [Figure 1] 1 illustrates a schematic diagram of a typical electronic packaging structure. [Figure 2A] 1 is related to Example 1 and shows a sample formed from Example 1 prior to thermal cycling testing. [Figure 2B] 1 shows a sample made from a comparative example before a thermal cycling test in relation to Example 1. [Figure 3A] 1 is related to Example 1 and shows a sample formed from Example 1 after thermal cycling testing. [Figure 3B] 1 is related to Example 1 and shows a sample formed from Example 1 after thermal cycling testing. [Figure 4A] 1 shows a sample formed from Comparative Example 2 prior to thermal cycling testing in relation to Example 2. [Figure 4B] 11 is related to Example 2 and shows a sample formed from Example 2A prior to thermal cycling testing. [Figure 4C] 11 is related to Example 2 and shows a sample formed from Example 2B prior to thermal cycling testing. [Figure 5A] 1 shows a sample formed from Comparative Example 2 after thermal cycling testing in relation to Example 2. [Figure 5B] 11 is related to Example 2 and shows a sample formed from Example 2A after thermal cycling testing. [Figure 5C] 11 is related to Example 2 and shows a sample formed from Example 2B after thermal cycling testing. [Figure 6A] 1 illustrates a dispenser device according to one embodiment of the present disclosure. [Figure 6B] 6B shows the dispenser device of FIG. 6A in operation.
[0019] Corresponding reference characters indicate corresponding parts throughout the several views. The illustrated embodiments are illustrative of exemplary implementations of the invention, and such examples are not intended to be limiting. They should not be construed as limiting the scope of the invention in any manner whatsoever. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] A. Thermal interface material The present invention relates to thermal interface materials (TIMs) that are useful for transferring heat away from electronic components. In one embodiment, the TIM comprises at least one silicone oil, at least one catalyst, At least one thermally conductive filler, and a composition comprising both amine and alkyl functional groups. Contains at least one adhesion promoter.
[0021] In some embodiments, the TIM is a silane coupling agent, an organic plasticizer, a surfactant, and a flux.
[0022] 1. Silicone oil A. Overview The present disclosure relates to a silicone oil composition comprising at least one low molecular weight silicone oil and at least one high molecular weight silicone oil. The silicone oil is catalyzed by the corn oil to provide a matrix for the TIM material. Crosslinking is achieved by the addition of one or more functional groups such as vinyl, hydroxide, hydroxyl, and acrylate functional groups. In one embodiment, the one or more silicone oils include a first silicone oil and a second silicone oil, the first silicone oil being a vinyl functional silicone oil; The second silicone oil is a hydride-functional silicone oil. The silicone oil is a thermally conductive filler. It wets the filler and forms a dispensable fluid for the TIM.
[0023] In one exemplary embodiment, the silicone oil is K available from Shin-Etsu. E-Series Products, SILBIONE® available from Bluestar, Wa ELASTOSIL®, SilGel®, available from cker SILPURAN®, SEMICOSIL®, and Momenti Silopren® available from Dow Corning, available from Dow Corning®, Silastic®, XIAME TER®, Syl-off®, and SYLGARD®, SQUARE® available from Square Silicone, AB sp Silicones such as Andril® available from Ecialty Silicones Other polysiloxanes include those from Wacker, Shin-etets, Do wcoring, Momentive, Bluestar, RUNHE, AB Spec ialty Silicones, Gelest, and United Chemical Available from Technologies.
[0024] b. Low molecular weight silicone oil 1. Vinyl-functional silicone oil TIM is a method for gel permeation chromatography (GPC). It contains silicone oils with low weight average molecular weight as measured by gel permeation chromatography (GPC). Suitable low molecular weight silicone oils may include vinyl silicone oils having the general formula: .
[0025] [ka]
[0026] Exemplary low molecular weight vinyl silicone oils may also contain small amounts of platinum catalysts.
[0027] Vinyl-functional silicone oils contain organosilicone components with Si-CH=CH2 groups. Exemplary vinyl-functional silicone oils include vinyl-terminated silicone oils, Si-CH Vinyl-grafted silicone oils in which =CH2 groups are grafted onto the polymer chain, and combinations thereof Examples include combinations.
[0028] Exemplary vinyl-terminated silicone oils include, respectively, those available from Gelest, Inc. DMS-V00 (weight average molecular weight (M) of 186 Daltons) w ) DMS-V 03 (M of about 500 Daltons w DMS-V05 (having an M of about 800 Daltons) w of DMS-V21 (having an M of about 6,000 daltons) w ), DMS-V22( M of about 9,400 Daltons w DMS-V25 (having an M of approximately 17,200 daltons) w DMS-V25R (having an M of approximately 17,200 daltons) w DMS- V35 (approximately 49,500 daltons M w ), DMS-V35R (approx. 49,500 Dalton's M w Exemplary vinyl-terminated polydimethylsiloxanes include those having the formula: Suitable vinyl-terminated silicone oils include PD V-0325 (approximately 15,500 daltons M w ), PDV-0331 (approximately 27, 000 Dalton M w PDV-0525 (having an M of approximately 14,000 daltons) w of PDV-1625 (having an M of approximately 9,500 daltons) w PDV-163 1 (M of about 19,000 Daltons) w PDV-2331 (approximately 12,500 daltons) Ton of M w Vinyl-terminated diphenylsiloxane-dimethylsiloxane copolyols such as Exemplary vinyl-terminated silicone oils include those available from Gelest, Inc. PMV-9925 (M of approximately 2,000-3,000 daltons) available from w (having Exemplary vinyl-terminated polyphenylmethylsiloxanes include: An example of a glycerin oil is EDV-2025 (approximately 16 M from ,500 to 19,000 Daltons wVinyl-terminated diethylsiloxanes such as Dimethylsiloxane copolymers are included.
[0029] Exemplary vinyl-grafted silicone oils include, but are not limited to, 1,3-diphenylmethane ... Available VMS-005 (M of about 258 to 431 Daltons) w ), VMS-T11 (M of about 1,000 to 1,500 Daltons w Vinyl methyl siloxane homopolymers such as Exemplary vinyl-grafted silicone oils include trimethylsilane polymers. silanol-terminated silicone oil, vinyl-terminated silicone oil, etc. Examples include vinylmethylsiloxane-dimethylsiloxane copolymers.
[0030] In an exemplary embodiment, the vinyl-grafted silicone oil is selected from the group consisting of Gelest, In VAT-4326 (M of approximately 10,000–12,000 daltons) available from c. w of Vinyl methyl siloxane, octyl methyl siloxane, dimethyl siloxane, etc. Terpolymer, VBT-1323 (M of about 8,000 to 12,000 daltons) w have ) etc. Vinyl methyl siloxane-methoxy polyethylene oxypropyl methyl siloxane -Dimethylsiloxane terpolymer, or vinylmethylsiloxane-phenylmethylsiloxane terpolymer Dimethylsiloxane (M of about 2,500 to 3,000 daltons) w (including The vinyl methyl siloxane terpolymer.
[0031] In one exemplary embodiment, the vinyl functional silicone oil is a vinyl T resin or a vinyl Q resin. Contains fat.
[0032] In one exemplary embodiment, the silicone oil is RUNHE's RH-Vi303, RH-V i301 and other Andril (registered trademark) products from AB Specialty Silicones ) VS200, Andril® VS1000 and other vinyl functional oils.
[0033] 2. Hydride-functional silicone oil Another exemplary low molecular weight silicone oil is a hydrosilicone oil having the general formula: may include.
[0034] [ka]
[0035] In one exemplary embodiment, the silicone oil has an organosilicone component and Si-H groups. Exemplary hydroxide-functional silicone oils include: Hydroxide-terminated silicone oils and hydrides, where the Si-H groups are grafted onto the polymer chain grafted silicone oils, as well as combinations thereof.
[0036] In an exemplary embodiment, the hydride terminated silicone oils include Gelest, DMS-H03 (M of approximately 400-500 daltons) available from w having DMS-H11 (M of about 1,000 to 1,100 daltons) w ), DMS-H21 (M of about 6,000 Daltons w DMS-H25 (having a molecular weight of approximately 17,200 daltons) M w ), or DMS-H31 (having an M of about 28,000 daltons) w Water such as In one exemplary embodiment, hydride-terminated polydimethylsiloxane is used. The silicone oil may be a methylhydrosiloxane such as trimethylsiloxy or hydride terminated oil. Exemplary trimethylsiloxy-terminated copolymers are dimethylsiloxane-copolymers. As an example, HMS-031 (M of about 1,900 to 2,000 daltons) w HM S-071 (M of about 1,900 to 2,000 Daltons) w ), HMS-082 (approx. M of 5,500 to 6,500 Daltons w HMS-151 (approximately 1,900 to 2, 000 Dalton M w HMS-301 (having approximately 1,900 to 2,000 daltons) M w HMS-501 (having an M of approximately 900 to 1,200 daltons) w (having Exemplary hydride-terminated copolymers include HMS-H271 (approximately 2,000 ~2,600 Daltons M w Each of them has the formula: Gelest, In In one exemplary embodiment, the hydride-grafted silicone oil is available from Each was HMS-991 (approximately 1,400 to 1,800 mg) available from Gelest, Inc. 0 Dalton M w HMS-992 (having an M of approximately 1,800 to 2,100 daltons) w HMS-993 (having an M of approximately 2,100 to 2,400 daltons) w (having) etc. is a trimethylsiloxy-terminated polymethylhydrosiloxane.
[0037] Exemplary low molecular weight silicone oils include those having a molecular weight of 50 Daltons, 500 Daltons, 1,000 Daltons, Light as 1000 Daltons, heavy as 5,000 Daltons, 10,000 Daltons, and 50,000 Daltons or any range of weight (M w )flat It may have an average molecular weight.
[0038] An exemplary low molecular weight silicone oil has a viscosity of less than 0.5 cS as measured according to ASTM D445. t, 5cSt, as low as 100cSt, 5,000cSt, 10,000cSt, 50, 000 cSt or any range defined between any two of the above values. The kinematic viscosity may be within the range of
[0039] The TIM is 0.1 wt%, 0.5 wt%, 0.67 wt%, based on the total weight of the TIM. , as little as 1% by weight, 3%, 5%, 10%, 20% by weight, or 0 .1% to 15% by weight, 0.1% to 3% by weight, or 0.67% to 10% by weight %, or any other amount within any range defined between any two of the above values. molecular weight silicone oil.
[0040] c. High molecular weight silicone oil TIM is a silicone oil with a high molecular weight as measured by gel permeation chromatography (GPC). Exemplary high molecular weight silicone oils, as well as the low molecular weight silicone oils described above, are listed below. The silicone oils may include vinyl silicone oils having the general formula:
[0041] [ka]
[0042] Vinyl-functional silicone oils contain organosilicone components with Si-CH=CH2 groups. Exemplary vinyl-functional silicone oils include vinyl-terminated silicone oils, Si-CH Vinyl-grafted silicone oils in which =CH2 groups are grafted onto the polymer chain, and combinations thereof Examples include combinations.
[0043] Exemplary vinyl-terminated silicone oils include, respectively, those available from Gelest, Inc. DMS-V41 (approximately 62,700 Daltons M w ), DMS-V42 (about 7 2,000 Daltons M w DMS-V46 (having an M of approximately 117,000 daltons) w DMS-V51 (having an M of approximately 140,000 daltons) w ), and DM S-V52 (approximately 155,000 daltons M w Vinyl-terminated polydimethylsiloxanes such as Roxane is one example.
[0044] Exemplary vinyl-grafted silicone oils include trimethylsiloxy-terminated silicone oils. vinylmethylsiloxanes such as silanol-terminated silicone oils and vinyl-terminated silicone oils Examples of suitable siloxane copolymers include dimethylsiloxane-copolymers.
[0045] In one exemplary embodiment, the vinyl grafted silicone oil is vinylmethylsiloxane. In an exemplary embodiment, the vinyl functional silicone oil is a vinyl T-polymer. Contains grease or vinyl Q resin.
[0046] Another exemplary high molecular weight silicone oil is a water-soluble silicone oil having an organosilicone component and Si-H groups. Exemplary hydroxide-functional silicone oils include: Hydroxide-terminated silicone oils, in which Si-H groups are grafted onto the polymer chain, hydride group raft silicone oils, and combinations thereof.
[0047] In one exemplary embodiment, the hydride terminated silicone oil is available from Gelest, Inc. Available DMS-H41 (M of approximately 62,700 Daltons) w Hydride ends such as In one exemplary embodiment, the hydride-terminated silicone oil is , trimethylsiloxy- or hydride-terminated methylhydrosiloxane-dimethylsiloxane Exemplary trimethylsiloxy-terminated copolymers include Gel HMS-064 (approximately 60,000-65,000 daltons) available from Est, Inc. M of N w (having the following structure).
[0048] Exemplary low molecular weight silicone oils include those with molecular weights of 60,000 Daltons, 70,000 Daltons, It is as light as 1,000,000 Daltons, 1,000,000 Daltons, or 10,000,000 Daltons. a mass of 100,000,000 daltons, or any two of the above values Weight within any range specified between (M w ) average molecular weight.
[0049] Exemplary high molecular weight silicone oils have a molecular weight of 10,000, as measured according to ASTM D445. 0cSt, 20,000cSt, low 100,000cSt, 1,000,000cS t, 10,000,000 cSt, 100,000,000 cSt or higher The kinematic viscosity may be within any range defined between any two of the values. In an embodiment, an exemplary high molecular weight silicone oil has a kinematic viscosity of 2,000,000 cSt. It is a high molecular weight vinyl silicone oil having the following properties.
[0050] The TIM may be added in amounts of 0.01 wt%, 0.1 wt%, 0.25 wt%, or 10 wt%, based on the total weight of the TIM. %, 0.5 wt%, 0.67 wt%, 0.75 wt%, 1 wt%, 1.5 wt% %, 2% by weight, as much as 5% by weight, or 0.1% to 5% by weight, 0.1% to 1% by weight %, or between any two of the above values, such as 0.25% by weight to 0.67% by weight. The composition may contain one or more high molecular weight silicone oils in an amount within any of the ranges set forth herein. In an embodiment, the TIM comprises a high molecular weight silicone oil in an amount of about 0.6% by weight. In one embodiment, the TIM comprises high molecular weight silicone oil in an amount of about 2.68% by weight.
[0051] 2. Catalyst The TIM further comprises one or more catalysts for catalyzing the addition reaction. Exemplary catalysts are Exemplary platinum-containing catalysts include those having the general formula: It is possible.
[0052] [ka]
[0053] Exemplary platinum-containing catalysts include platinum cyclovinylmethylsiloxane complexes (Ashby Karstedt catalyst), platinum carbonylcyclovinylmethylsiloxane complex (Oss ko catalyst), platinum divinyltetramethyldisiloxane dimethyl fumarate complex, platinum divinyl dimethyl maleate complex. Examples of cyclovinylmethylsiloxane complexes include SIP6829.2, and platinum Examples of divinyltetramethyldisiloxane complexes include SIP6830.3 and SIP6 831.2, and an example of a platinum cyclovinylmethylsiloxane complex is SIP6 833.2, all of which are available from Gelest, Inc. Further examples of gold-containing catalyst materials include those available from Wacker Chemie AG. Catalyst OL and United Chemical Technologi PC065, PC072, PC073, PC074, PC available from es Inc. 075, PC076, PC085, PC086, PC087, and PC088.
[0054] Exemplary rhodium-containing materials include Tris( Dibutylsulfide) rhodium trichloride (product code INRH078) do.
[0055] Without wishing to be bound by any particular theory, the platinum catalyst may be It is believed to react with vinyl silicone oils and hydrosilicone oils.
[0056] [ka]
[0057] TIM is available in concentrations of 5 ppm, 10 ppm, 15 ppm, and 2 ppm based on the total weight of the silicone oil. 0ppm, 25ppm, 30ppm, 40ppm, 50ppm, 100ppm, 2 00ppm, 500ppm, 1000ppm, or as high as 10ppm to 30ppm, Any of the above values, such as 0 ppm to 100 ppm or 5 ppm to 500 ppm. The composition may contain one or more catalysts in an amount within any range defined between the two.
[0058] In one exemplary embodiment, the catalyst is provided in a mixture with one or more silicone oils. In one exemplary embodiment, the platinum-containing material catalyst is obtained from Shin-Etsu. Available KE-1012-A, KE-1031-A, KE-109E-A, KE-1051 JA, KE-1800T-A, KE1204A, KE1218A, etc., Bluestar and SILBIONE® RT Gel 4725 SLD A, available from SilGel® 612A, ELASTOSIL® available from Wacker Registered trademark) LR3153A, ELASTOSIL (registered trademark) LR3003A, ELASTOSIL TOSIL® LR3005A, SEMICOSIL® 961A, S EMICOSIL® 927A, SEMICOSIL® 205A, S EMICOSIL (registered trademark) 9212A, SILPURAN (registered trademark) 2440, etc. Such as Silopren® LSR 2010A available from Momentive , XIAMETER® RBL-920 available from Dow Corning 0A, XIAMETER (registered trademark) RBL-2004A, XIAMETER (registered trademark) )RBL-9050A, XIAMETER(R)RBL-1552A, Silas tic(registered trademark) FL30-9201A, Silastic(registered trademark) 9202A, Silastic(R) 9204A, Silastic(R) 9206A, SYLGARD® 184A, Dow Corning® QP-1A , Dow Corning® C6A, Dow Corning® C It can be combined with a functional silicone oil such as V9204A.
[0059] The TIM is 0.01 wt%, 0.1 wt%, 0.2 wt%, based on the total weight of the TIM. as little as 0.3%, 0.4%, 0.5% by weight, or any of the above values. The catalyst may be present in an amount within any range defined between any two of the above. In another exemplary embodiment, the TIM comprises a catalyst in an amount of about 0.04 wt. %. M comprises a catalyst in an amount of about 0.4 wt.%.
[0060] In another embodiment, the platinum-containing material catalyst is combined with a high molecular weight vinyl functional silicone oil. will be done.
[0061] 3. Thermally conductive filler The TIM includes one or more thermally conductive fillers. Exemplary thermally conductive fillers include metals. , alloys, non-metals, metal oxides and ceramics, and combinations thereof. Metals include aluminum, copper, silver, zinc, nickel, tin, indium, and lead. Non-metallic materials include, but are not limited to, carbon, graphite, and carbon. Examples of such materials include nanotubes, carbon fibers, graphene, boron nitride, and silicon nitride. The metal oxide or ceramic may be, but is not limited to, alumina (aluminum oxide) Examples of suitable oxides include aluminum nitride, aluminum nitride, boron nitride, zinc oxide, and tin oxide. Not limited to.
[0062] The TIM is preferably used in an amount of 10 wt%, 20 wt%, 25 wt%, 50 wt%, or 60 wt%, based on the total weight of the TIM. % by weight, 75% by weight, 80% by weight, 85% by weight, 90% by weight, 95% by weight, 97% by weight % by weight, or 10% to 95% by weight, 50% to 95% by weight, or 85% by weight Any range defined between any two of the above values, such as % by weight to 97% by weight. The composition may contain an amount of one or more thermally conductive fillers.
[0063] Exemplary thermally conductive fillers are as small as 0.1 microns, 1 micron, 10 microns, As large as 50 microns, 75 microns, 100 microns, or any of the above values It may have an average particle size within any range defined between the two.
[0064] In one exemplary embodiment, the TIM comprises a first thermally conductive filler and a second thermally conductive filler. and wherein the first thermally conductive filer has an average particle size greater than 1 micron. and the second thermally conductive filler has an average particle size of less than 1 micron. In a preferred embodiment, the ratio of the first thermally conductive filler to the second thermally conductive filler is 1:5, 1:2, or 2:3. :4, 1:3, 1:2, 1:1, 1.5:1, 2:1, 3:1, 4:1, 5: 1 size, or 1:5~5:1, 1:1~3:1, or 1.5:1~3:1, etc. The average particle size may be within any range defined between any two of the above values. .
[0065] In one exemplary embodiment, the TIM comprises a first thermally conductive filler and a second thermally conductive filler. and a third thermally conductive filler, the first thermally conductive filer being 10 microns. the second thermally conductive filler has a particle size greater than 1 micron, 2 microns, As small as 4 microns, as large as 6 microns, 8 microns, 10 microns, or any of these and the third thermally conductive filler has a particle size within any range defined between 1 micron and It has an average particle size less than 1.
[0066] In an exemplary embodiment, the TIM is as little as 30%, 35%, or 40% by weight. , 45 wt.%, 50 wt.%, 60 wt.%, or the above values for the entire TIM composition. The thermally conductive filler may be present in an amount within any range defined between any two of the amounts of the first thermally conductive filler. The first thermally conductive filler has an average particle size as small as 30 microns. 40 microns, often 45 microns, 50 microns, 60 microns or values above. The range may be any range defined between any two of the above. An exemplary TIM is 5% by weight, As little as 10% by weight, 15% by weight, as much as 25% by weight, 30% by weight, 40% by weight, or any amount within a range defined between any two of the above values for the total TIM composition The second thermally conductive filler further comprises a second thermally conductive filler having a thickness of 1 micron, 3 microns, It has an average particle size as small as 5 microns, often 10 microns or 15 microns. , 20 microns, or within any range defined between any two of the above values. Exemplary TIMs include those containing as little as 5%, 10%, 15%, 25%, 30% by weight. %, as much as 40% by weight, or any two of the above values with respect to the total TIM composition. The third thermally conductive filler may be present in any amount within any range defined between 0.1 and 0.5. The fillers have an average particle size of 0.1 microns, and as small as 0.3 microns. 5 microns, often 1 micron, 1.5 microns, 2 microns, or any of the values above. The term "substitution" refers to any combination of the two terms that are used interchangeably.
[0067] In an exemplary embodiment, the TIM is present in an amount of as little as 5%, 10%, 15% by weight, As much as 25%, 30%, 40% by weight, or the above values for the entire TIM composition. The thermally conductive filler may be present in an amount within any range defined between any two of the above. A first thermally conductive filler having an average particle size as small as 0.35 microns; 40 microns, often 45 microns, 50 microns, 60 microns, or any of the above values An exemplary TIM is 30% by weight, 3 As little as 5%, 40%, as much as 45%, 50%, 60% by weight, or any amount within a range defined between any two of the above values for the total TIM composition The second thermally conductive filler further comprises a second thermally conductive filler having an average particle size as small as 1 micron, 3 microns. The second thermally conductive filler has a thickness of 5 microns, often 10 microns, 15 microns, 2 0 microns, or within any range defined between any two of the above values. Exemplary TIMs include as little as 5 wt%, 10 wt%, 15 wt%, 25 wt%, 30 wt%, %, as much as 40% by weight, or between any two of the above values with respect to the total TIM composition. 0.1 microns, 0.5 microns, 1.0 microns, 0.6 microns, 1.2 microns, 0.8 microns, 0.9 microns, 1.4 microns, 0.1 microns, 0.2 microns, 0.4 microns, 0.5 microns, 0.6 microns, 0.7 microns, 0.8 microns, 0.9 ... A third thermally conductive filler with an average particle size as small as .3 microns. , often 1 micron, 1.5 microns, 2 microns, or any two of the above values. The term "abbreviated" means that the term "abbreviated" is within any range defined between .
[0068] Exemplary thermally conductive fillers include aluminum oxide and zinc oxide.
[0069] 4. Addition of Inhibitors The TIM includes one or more additional inhibitors to inhibit or limit crosslinking of the silicone oil. The addition inhibitor comprises at least one alkynyl compound, and optionally, an addition inhibitor further comprises a multivinyl functional polysiloxane.
[0070] Exemplary addition inhibitors include 1-ethynyl-1-cyclohexanol, 2-methyl- 3-Butyn-2-ol, 2-phenyl-3-butyn-2-ol, 2-ethynyl-iso Propanol, 2-ethynyl-butan-2-ol, and 3,5-dimethyl-1-hexyl Acetylenic alcohols such as 3,5-dimethyl-1-hexyl ether, dimethyl-bis-(3-methyl-1-butynoxy)silane, Methylvinylbis(3-methyl-1-butyne-3-oxy)silane and ((1,1-di Silylated acetylene alcohols such as methyl-2-propynyloxytrimethylsilane , diallyl maleate, dimethyl maleate, diethyl fumarate, diallyl fumarate, and and bis-2-methoxy-1-methylethyl maleate, monooctyl maleate, Monoisooctyl maleate, Monoallyl maleate, Monomethyl maleate, Monoethyl fumarate Unsaturated carboxylates such as monoallyl fumarate, monoallyl fumarate, and 2-methoxy-1-methylethyl fumarate esters, alcohol is benzyl alcohol or 1-octanol and ethenyl cyclohexane fumaric acid / alcohol mixtures such as mixtures selected from 2-isopropyl-1-oxohexyl-1-ol; 3,5-dimethyl-3-hexen-1-yne, 3-methyl- 3-methyl-3-penten-1-yne, 3-methyl-3-hexen-1-yne, 1-ethynylsilane Cyclohexene, 3-ethyl-3-buten-1-yne, and 3-phenyl-3-buten-1 -yne and other conjugated ene-ynes, I,3,5,7-tetramethyl-1,3,5,7-tetravinyl Vinylcyclosiloxanes such as cyclotetrasiloxane, and conjugated enes and vinylcyclosiloxanes. In an exemplary embodiment, the addition inhibitor is a mixture of 2- methyl-3-butyn-2-ol or 3-methyl-1-pentyn-3-ol can be.
[0071] In some exemplary embodiments, the addition inhibitor is a multivinyl-functional polysiloxane. Exemplary multivinyl-functional polysiloxanes include those available from Wacker Chemi e Ethynylcyclohexanoate such as Pt Inhibitor 88 available from AG The vinyl terminated polydimethylsiloxane in water is a vinyl terminated polydimethylsiloxane in water. Although not the only catalyst, the platinum catalyst is ethynylcyclohexanol and vinyl powder as shown below. It is believed to form a complex with the terminal polydimethylsiloxane.
[0072] [ka]
[0073] The formation of complexes reduces the catalytic activity at room temperature and therefore the dispensability and wettability of the TIM. At higher temperatures during the curing process, Pt is released from the complex and becomes vinyl. It helps hydrosilylation of aryl-functional silicone oil and hydride-functional silicone oil, and promotes "crosslinking" " More control.
[0074] In some exemplary embodiments, the TIM comprises 0.01 weight percent based on the total weight of the TIM. %, 0.02% by weight, 0.05% by weight, 0.1% by weight, 0.15% by weight, .2wt%, 0.25wt%, 0.3wt%, 0.5wt%, 1wt%, 3wt%, 5wt % by weight, or 0.01% to 1% by weight, 0.01% to 0.5% by weight, or or any value between any two of the above values, such as 0.05% by weight to 0.2% by weight. The TIM may include any amount of one or more additional inhibitors. In an exemplary embodiment, the TIM is In another exemplary embodiment, the TIM comprises an additive inhibitor in an amount of 0.1 wt. The additive inhibitor is present in an amount of 3% by weight.
[0075] Without wishing to be bound by any particular theory, it is believed that in the absence of additional inhibitors, Nyl-functional silicone oils react very quickly with hydrogen based on an additive hydrosilylation mechanism. The reaction with the halogen-functional silicone oil produces solid phases that cannot be automatically dispensed by typical methods. Form.
[0076] In an exemplary embodiment, the addition inhibitor is KE-1, available from Shin-Etsu. 056, KE-1151, KE-1820, KE-1825, KE-1830, KE-1 831, KE-1833, KE-1842, KE-1884, KE-1885, KE-1 Syl-o available from Dow Corning, such as 886, FE-57, and FE-61 ff (registered trademark) 7395, Syl-off (registered trademark) 7610, Syl-off (registered trademark) (registered trademark) 7817, Syl-off (registered trademark) 7612, Syl-off (registered trademark) It can be combined with a functional silicone oil such as 7780.
[0077] 5. Optional Ingredients In some embodiments, the TIM is a silane coupling agent, an organic plasticizer, a surfactant, and fluxing agents.
[0078] In some exemplary embodiments, the TIM comprises one or more coupling agents. Examples of suitable coupling agents include those of the general formula Y-(CH2) n -Si-X3 (wherein Y is an organic and X is a hydrolyzable group. The functional group Y is alkyl, glycidoxy, acryloxyl, methylacryloxy. Examples of the hydrolyzable group X include alkyloxy and acetoxy. In some exemplary embodiments, the silane coupling agent is an alkyl silane. Exemplary alkyltrialkoxysilanes include decaalkoxysilanes. Silyltrimethoxysilane, undecyltrimethoxysilane, hexadecyltrimethoxysilane In one exemplary embodiment, the TIM contains hexadecyltrimethoxysilane, shown in the following formula, as a coupling agent.
[0079] [ka]
[0080] Exemplary coupling agents interact with exemplary fillers as shown in the following exemplary reactions: Alumina is the typical packing material used in the following reactions. However, other Alternative fillers may be used. As shown, a coupling agent is added to the water and the ethoxylated The product is then subjected to hydrolysis to remove the silyl group, followed by removal of water and coupling. The catalyst is then subjected to a modification reaction in which the binder and alumina are bonded together.
[0081] [ka]
[0082] In some exemplary embodiments, the TIM comprises 0.1 wt. %, 0.25% by weight, 0.5% by weight, 0.67% by weight, 0.75% by weight, 1 layer %, 1.5%, 2%, 5%, 10% by weight, or as much as 0.1% to 1 0% by weight, 0.1% to 1% by weight, or 0.25% to 0.67% by weight, etc. One or more couplings in an amount within any range defined between any two of the values listed above. In one exemplary embodiment, the TIM may include a coupling agent in an amount of 0.4 wt.%. Includes.
[0083] In some exemplary embodiments, the TIM comprises one or more organic plasticizers. Organic plasticizers include bis(2-ethylhexyl) phthalate (DEHP), dibutyl phthalate, Dioctyl phthalate (DnBP, DBP), dioctyl phthalate (DOP or DnOP), diethyl phthalate diisobutyl phthalate (DEP), diisodecyl phthalate (DIBP), diisodecyl phthalate (DIDP) ), diisononyl phthalate (DINP), butyl benzyl phthalate (BBzP) etc. Contains acid plasticizers.
[0084] In some exemplary embodiments, the TIM comprises 0.01 weight percent based on the total weight of the TIM. Amount%, 0.1% by weight, 0.25% by weight, 0.5% by weight, 0.67% by weight, 0.75% by weight as little as 1%, 1.5%, 2%, 5%, 10% by weight, or 0.01% by weight to 10% by weight, 0.1% by weight to 1% by weight, or 0.25% by weight to 0. 67% by weight, or any amount within a range defined between any two of the above values. The above organic plasticizers may be included.
[0085] In some exemplary embodiments, the TIM comprises one or more surfactants. Surfactants include BYK-307, BYK-306 and BYK-222. Silicone-based surface additives such as BYK surfactants available from Chemie GmbH include.
[0086] In some exemplary embodiments, the TIM comprises 0.01 weight percent based on the total weight of the TIM. Amount%, 0.1% by weight, 0.25% by weight, 0.5% by weight, 0.67% by weight, 0.75% by weight as little as 1%, 1.5%, 2%, 5%, 10% by weight, or 0.1% to 10% by weight, 0.1% to 1% by weight, or 0.25% to 0.6% by weight 7% by weight, or any amount within any range defined between any two of the above values. The surfactant may be one of the above.
[0087] In some exemplary embodiments, the TIM comprises one or more fluxing agents. Exemplary fluxing agents include: An example is fumed silica.
[0088] In some exemplary embodiments, the TIM comprises 0.1 wt. %, 0.25% by weight, 0.5% by weight, 0.67% by weight, 0.75% by weight, 1 layer %, 1.5%, 2%, 5%, 10% by weight, or as much as 0.1% to 1 0% by weight, 0.1% to 1% by weight, or 0.25% to 0.67% by weight, etc. The present invention may include one or more fluxing agents in an amount within any range defined between any two of the values listed above. do.
[0089] 6. Exemplary Formulations of Thermal Interface Materials In a first non-limiting exemplary embodiment, the TIM comprises about 2% to about 20% by weight of silica. corn oil, about 0.1% to about 5% by weight of a coupling agent, about 50% to about 95% by weight of a thermally conductive filler, from about 0.1% by weight to about 5% by weight of an addition inhibitor, and from about 0.1% by weight to about Contains 5% by weight of added catalyst.
[0090] In a second non-limiting exemplary embodiment, the TIM comprises about 2% by weight to about 10% by weight of the first of a low molecular weight silicone oil, about 2% by weight to about 10% by weight of a second low molecular weight silicone oil, about 0. 1% by weight to about 5% by weight of high molecular weight silicone oil, about 0.1% by weight to about 5% by weight of coupling agent a first thermally conductive filler of about 25% to about 50% by weight; % by weight of a second thermally conductive filler, about 25% to about 50% by weight of a third thermally conductive filler, 0.1% to about 5% by weight of an addition inhibitor, and about 0.1% to about 5% by weight of an addition catalyst. include.
[0091] 7. Exemplary Properties of Thermal Interface Materials In some exemplary embodiments, the thermal interface materials as described above are resistant to highly accelerated stress testing (HA HAST testing is typically used to evaluate the thermal performance of thermal interface materials. It is understood that the above relates to the resistance of the thermal interface material to humidity and temperature. The HAST test standard is JESD22-A110-B. The interface material is a vertically oriented 1.6 mm gap between the glass and an exemplary copper heat sink. The devices were placed in a storage tank and subjected to 10,000 thermal cycles from -55°C to +125°C for over a week. In another embodiment, the thermal interface material exhibits little or no cracking after thermal cycling testing. This shows that.
[0092] In some exemplary embodiments, the thermal interface materials described above provide resistance to temperature cycling. Temperature cycling is typically performed on the thermal interface to extremes of high and low temperatures. It is understood to relate to the resistance of a material as well as its ability to withstand cyclic thermal stresses. The temperature cycle test standard is JESD22-A104-B. The thermal interface material is a vertically oriented 1.6 mm gap glass and an exemplary copper heat shield. The battery is placed between the battery and the battery pack and is rated for 10,000 cycles at temperatures between -55°C and +125°C for one week. In another embodiment, the thermal interface material exhibits no dripping even when subjected to thermal cycling. Showing little or no cracking following cyclic testing.
[0093] In some exemplary embodiments, the thermal interface material has a thermal resistance of at least 1 W / m K. An exemplary thermal conductivity test method standard is ASTM D5470 In one exemplary modification, such a thermal interface material has a thermal conductivity of about 4 W / m·K. In another exemplary embodiment, the thermal interface material has a thermal conductivity of about 2 W / m·K. has a rate.
[0094] In some exemplary embodiments, the thermal interface material as described above has a thermal conductivity of 10 Pa.s to 10 Pa.s at room temperature. In the range of 100,000 Pa.s, more specifically, 100 Pa.s to 10,000 Pa. An exemplary viscosity test standard is DIN 53018. In one specific embodiment, the viscosity is measured as a function of shear rate using a Brookfield rheometer. degree 2s -1 It is tested at.
[0095] As applied, the thermal interface material has a varying thickness, measured in micrometers. In some exemplary embodiments, the thermal interface material may have a thermal conductivity of 0.05% or more. As small as 5mm, 0.5mm, 1mm, and as large as 3mm, 5mm, 7mm, 10mm or any range defined between any two of the above values, such as 0.05 mm to 5 mm The thickness is within the range.
[0096] In some exemplary embodiments, the thermal interface material, as described above, when cured, has a predetermined In one exemplary embodiment, the thermal interface material is at least compressible at a temperature of about 25° C. It can be compressed by at least 10%.
[0097] In some exemplary embodiments, the thermal interface material as described above has a melting point of 1 g / min to 1,000 g / min. The dispense rate is in the range of 10 g / min to 100 g / min. In one exemplary embodiment, the dispense rate is 100% for a dispense header with a 0.1 inch diameter opening. The test is performed using a 1.5 ml syringe under a pressure of 0.6 MPa.
[0098] B. Method for forming thermal interface material In some exemplary embodiments, the TIM comprises combining the individual components in a heated mixer; The composition is prepared by mixing the compositions together. The mixed composition is then fired. It can be applied directly to the substrate without any need for a pre-coating.
[0099] C. Applications using thermal interface materials Still referring to FIG. 1, in some exemplary embodiments, the thermal interface material is a TIM As shown by 18, a TIM 1 is provided between the electronic component 12 and the heat spreader 14. In some exemplary embodiments, the thermal interface material is provided by TIM 20. As shown, a TIM 2 is disposed between the heat spreader 14 and the heat sink 16. In some exemplary embodiments, the thermal interface material is a material that is bonded to the electronic component 12 and the heat sink 14. 16 as TIM1.5 (not shown). EXAMPLES
[0100] Example 1 The thermal interface materials were prepared according to the formulations provided in Table 1.
[0101] [Table 1]
[0102] Low molecular weight (MW) silicone oil A is a low molecular weight liquid silicone rubber containing vinyl functional groups. The low MW silicone oil has a molecular weight of less than 50,000 Daltons and is platinum-catalyzed. Low MW silicone oil B is a liquid silicone rubber containing hydride functional groups. The silane coupling agent is a hexadecane having a molecular weight of less than 50,000 Daltons. The thermally conductive filler A had a particle size of 1 to 10 microns. The thermally conductive filler B was aluminum particles with a particle size of less than 1 micron. The addition inhibitor was available from Wacker Chemie AG. The most effective inhibitor was Pt Inhibitor88.
[0103] To prepare the formulation of Example 1, silicone oil, silane coupling agent, and additives were added. The inhibitors were combined and mixed in a speed mixer. The thermally conductive filler was then added and mixed. The material was mixed again.
[0104] For comparison purposes, GEL30 thermally conductive material from Parker Chomerics was used. GEL30 is a partially crosslinked silicone rubber and alumina Includes.
[0105] The formulations of Example 1 and the Comparative Example each had a vertical interface between the glass and the exemplary heat sink. The plates were sandwiched with a 1.6mm gap and thermally cycled for one week at -55°C to +125°C. It was put on hold.
[0106] FIG. 2A shows a sample formed from Example 1 before thermal cycling testing, and FIG. 2B shows a sample formed from Example 1 after thermal cycling testing. Figure 3A shows a sample made from the GEL30 Comparative Example before and after thermal cycling testing. FIG. 3B shows a sample formed from Example 1 of GEL30 after thermal cycling testing. 1 shows a sample formed from an example.
[0107] As shown in FIG. 3A, the specimen formed from Example 1 was subjected to a thermal shock test in which the sample was dissolved in water during testing. There is no dripping as indicated by the plate maintaining its original vertical position. In contrast, the sample formed from the comparative example showed a downward shift between FIG. 2B and FIG. 3B. There was significant dripping as indicated by the movement.
[0108] In addition, FIG. 3A shows a limited tumble of the sample formed from Example 1 for thermal cycling testing. In contrast, Figure 3B shows significantly more cracks in the comparative example.
[0109] Example 2 The thermal interface materials were prepared according to the formulations provided in Table 2.
[0110] [Table 2]
[0111] Low molecular weight (MW) silicone oil A was a low molecular weight liquid silicone rubber containing vinyl functionality. The low MW silicone oil had a molecular weight less than 50,000 daltons and further contained a platinum catalyst. Low MW silicone oil B was a low molecular weight liquid silicone rubber containing hydride functionality. The molecular weight of low MW silicone oil B was less than 50,000 daltons. The molecular weight of the high MW silicone oil was greater than 60,000 daltons. The silane coupling agent was hexadecyltrimethoxysilane. Thermally conductive filler A had a particle size of 1-10 microns. Oxidation Thermally conductive filler B was aluminum oxide particles having a particle size of less than 1 micron. The loading inhibitor was Pt Inhibitor 88 available from Wacker Chemie AG.
[0112] After preparing one of Comparative Example 2, Examples 2A, 2B, or 2C, the results shown in Figures 6A and 6B were As shown, the prepared mixture is inserted into a syringe 50 and sealed. The mixture is dispensed by the dispenser tool 52. The air pressure generated can be used to purge the syringe 50. The dispenser tool 52 also controls the diameter of the orifice. By varying two parameters, the orifice diameter and the air pressure, In one embodiment, the compound is dispensed from the syringe 50. 10 cubic centimeters under 90 psi compression through a 0.100 inch orifice The solution is dispensed from a syringe 50 without a tip attachment.
[0113] The formulations of Comparative Example 2, Example 2A, and Example 2B were each dispensed onto an exemplary heat sink. After the injection, if the device is placed vertically, as shown in Figure 2A, for example, the heat Glass on an exemplary heat sink with a 1.6 mm gap between the sink and the glass A pressure plate was placed on the formulation to spread it over the desired area. There is a 1.6mm gap between the heat sink and the glass. The exemplary heat sink device was thermally cycled from -55°C to +125°C for one week on each sub-substrate. The cycles were performed in 40-minute increments. In total, about 250 cycles were performed, with each individual cycle has a duration of 40 minutes.
[0114] 4A to 4C are diagrams showing Comparative Example 2 and Example 2A formed from Example 2 before the thermal cycle test. 5A to 5C, and Example 2B after the thermal cycle test. and the formulation resulting from Example 2B.
[0115] As shown in FIGS. 5A and 5B, in Comparative Example 2 and Example 2A, the samples were galvanized during the test. As shown by the failure to maintain the original vertical position between the lath and the substrate. In contrast, Example 2B showed no significant dripping during testing, as shown in FIG. As shown by the fact that the glass maintains the original vertical position between the glass and the substrate, The drop was observed.
[0116] In addition, Example 2B (FIG. 5C) is formed from Example 1 for example, for thermal cycling testing. In contrast, the samples in Comparative Example 2 and Example 2A (respectively) showed limited cracking. 5A and 5B) show significantly more cracks in the comparative example.
[0117] While the invention has been described as having an exemplary design, the invention can be further modified within the spirit and scope of the disclosure. This application is therefore intended to cover any variations, uses, or adaptations of the invention using its general principles. Further, this application is intended to cover such departures from the disclosure as come within known or customary practice in the art to which this invention pertains and which fall within the scope of the appended claims. The present specification includes the following aspects of the invention. [1] 1. A thermal interface material comprising: Weight less than 50,000 Daltons (M w ) at least one low molecular weight silicone oil having an average molecular weight of at least one thermally conductive filler; and at least one high molecular weight silicone oil, said high molecular weight silicone oil having a weight (M w 1. A thermal interface material comprising a vinyl-functional silicone oil having an average molecular weight of 1.0 to 1.5. [2] 2. The thermal interface material of claim 1, wherein the at least one low molecular weight silicone oil comprises a first silicone oil and a second silicone oil, the first silicone oil being a vinyl-functional silicone oil and the second silicone oil being a hydride-functional silicone oil. [3] 10. The thermal interface material of claim 1, wherein the thermally conductive filler comprises a first thermally conductive filler and a second thermally conductive filler, the first thermally conductive filler being a metal oxide having a particle size greater than 1 micron, and the second thermally conductive filler being a metal oxide having a particle size less than 1 micron. [4] The thermal interface material comprises: 2% by weight to 20% by weight of the low molecular weight silicone oil; 50% to 95% by weight of the thermally conductive filler; and 0.1% by weight to 5% by weight of the high molecular weight silicone oil. [5] 1. A thermal interface material comprising: At least one silicone oil; at least one thermally conductive filler; at least one addition inhibitor, wherein the addition inhibitor comprises an alkynyl compound. [6] 6. The thermal interface material of claim 5, wherein the addition inhibitor is selected from the group consisting of multi-vinyl functional polysiloxanes, polydimethylsiloxane vinyl terminated with ethynylcyclohexanol, 2-methyl-3-butyn-2-ol, and 3-methyl-1-pentyn-3-ol. [7] 5. The thermal interface material of claim 1, wherein the at least one silicone oil comprises a first silicone oil and a second silicone oil, the first silicone oil being a vinyl-functional silicone oil and the second silicone oil being a hydride-functional silicone oil. [8] 10. The thermal interface material of claim 9, wherein the thermally conductive filler comprises a first thermally conductive filler and a second thermally conductive filler, the first thermally conductive filler being a metal having a particle size greater than 1 micron, and the second thermally conductive filler being a metal oxide having a particle size less than 1 micron. [9] The thermal interface material according to [8], wherein a ratio of the first thermally conductive filler to the second thermally conductive filler is 1.5:1 to 3:1.
[10] The thermal interface material comprises: 2% by weight to 20% by weight of the silicone oil; 0.1% by weight to 5% by weight of a silane coupling agent; 50% to 95% by weight of the thermally conductive filler; and 0.01 wt % to 5 wt % of the addition inhibitor.
Claims
1. 1. A thermal interface material comprising: Weight (M) less than 50,000 Daltons w ) at least one low molecular weight silicone oil having an average molecular weight of at least two thermally conductive fillers in an amount of 90% to 97% by weight, based on the total weight of the thermal interface material; at least one high molecular weight silicone oil; At least one additional inhibitor; Including, The high molecular weight silicone oil has a weight (M w ) an average molecular weight of the addition inhibitor is a vinyl terminated polydimethylsiloxane in ethynylcyclohexanol; The thermal interface material, wherein the at least two thermally conductive fillers include a thermally conductive filler that is a metal oxide having a particle size greater than 1 micron and a thermally conductive filler that is a metal oxide having a particle size less than 1 micron.
2. 2. The thermal interface material of claim 1, wherein the at least one low molecular weight silicone oil comprises a first silicone oil and a second silicone oil, the first silicone oil being a vinyl functional silicone oil and the second silicone oil being a hydride functional silicone oil.
3. 3. The thermal interface material of claim 1 or 2, wherein the ratio of thermally conductive fillers that are metal oxides having a particle size greater than 1 micron to thermally conductive fillers that are metal oxides having a particle size less than 1 micron is from 1.5:1 to 3:1.
Citation Information
Patent Citations
Heat radiation member
JP2000204259A
Heat-conductive silicone rubber composition and molded article
JP2005325211A
Thermally conductive resin composition
JP2011144234A
Thermoconductive molding and use thereof
JP2012201106A
Composition for thermal conducive grease, thermal conductive grease and heat dissipating member
JP2016216523A