Coated Cutting Tools
The multilayer (Ti,Al)N coating with controlled Ti to Al ratio enhances flank wear resistance, addressing the inadequacies of single-phase coatings by extending tool life and maintaining cutting performance.
Patent Information
- Application Number
- JP2021575344
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-19
- Filing Date
- 2020-06-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-06-17
AI Technical Summary
Existing (Ti,Al)N PVD coatings in cutting tools suffer from inadequate flank wear resistance, leading to poor surface profiles and increased friction during metalworking, limiting tool life.
A coated cutting tool with a multilayer structure comprising alternating cubic (Ti,Al)N and mixed cubic-hexagonal (Ti,Al)N sublayers, where the Ti to Al ratio is closely controlled, and the sublayers are deposited using PVD, enhancing flank wear resistance.
The multilayer structure significantly improves flank wear resistance, resulting in longer tool life and maintaining superior cutting performance.
Smart Images

Figure 0007584456000004 
Figure 0007584456000005 
Figure 0007584456000006
Abstract
Description
[Technical field]
[0001] The present invention relates to coated cutting tools that include multiple (Ti,Al)N cubic and hexagonal sub-layers. [Background technology]
[0002] (Ti,Al)N coatings produced by physical vapor deposition (PVD) are commonly used in the field of cutting tools for metalworking.
[0003] The crystal structure of (Ti,Al)N in PVD coatings can be cubic (NaCl(=B1)) or hexagonal (wurtzite) structure. Prior art studies have generally shown that low Al contents, such as <60% of Al+Ti in (Ti,Al)N, result in a cubic structure, whereas high Al contents, such as >70%, result in a hexagonal structure. Specific limits for the level of Al content that result in either a single-phase cubic structure or a mixed structure containing both cubic and hexagonal structures have been reported, varying to some extent depending, for example, on the deposition conditions.
[0004] For example, Tanaka et al., “Properties of (Ti1-xAlx)N coatings for cutting tools” prepared by the cathodic arc ion "Effects of Al content on hardness, lattice parameter and microstructure of (Ti1-xAlx)N films", Surface and Coatings Technology 120-121 (1999) 438-441 reported (Ti1-xAlx)N films synthesized by the arc ion plating method, in which the NaCl structure with x≦0.6 was transformed into the wurtzite structure with x≧0.7.
[0005] Flank wear occurs primarily on the flank of the cutting edge due to abrasive wear mechanisms. The flank is exposed to the workpiece movement and excessive flank wear will lead to poor surface geometry of the workpiece, inaccuracies in the cutting process and increased friction as the cut progresses.
[0006] In order to provide cutting tools with superior properties over currently available cutting tools, there is a continuing need for coated cutting tools whose coatings have superior properties in terms of flank wear resistance. When better flank wear resistance is realized, longer tool life is realized in certain metalworking applications. It is therefore an object of the present invention to provide a coated cutting tool with superior flank wear resistance. Summary of the Invention
[0007] Provided herein is a coated cutting tool for metalworking having a coating comprising multiple alternating sub-layers of cubic (Ti,Al)N and cubic and hexagonal mixed phase (Ti,Al)N that exhibits surprisingly good flank wear resistance without performance degradation in crater wear resistance in metal cutting operations.
[0008] There is further provided a coated cutting tool having a coating comprising multiple alternating sublayers of cubic (Ti,Al)N and cubic and hexagonal mixed phase (cubic+hexagonal) (Ti,Al)N, where the Ti to Al ratio in the cubic phase sublayers and the cubic+hexagonal sublayers, respectively, may be kept very close or substantially the same, as required. In the latter case, the same target can be used to deposit both the cubic and the cubic+hexagonal sublayers, which is advantageous for cost reasons and in manufacturing efficiency.
[0009] The present invention relates to a coated cutting tool for metal machining comprising a substrate and a coating, the coating being made of alternating cubic Ti 1-x Al x N sublayer, 0.60≦x≦0.75, and cubic + hexagonal Ti 1-y Al y N sublayers, (Ti,Al)N multilayers with 0.60≦y≦0.75, with the average cubic Ti 1-x Al x The thickness of the N sublayer is 75-450 nm, and the average cubic + hexagonal Ti 1-y Al y The thickness of the N sublayer is 50 to 300 nm, and the cubic Ti 1-x Al x N sublayer and cubic + hexagonal Ti 1-y Al y The number of each of the N sub-layers is 2-50.
[0010] Average cubic Ti 1-x Al x The thickness of the N sublayer is suitably 100 to 400 nm, preferably 150 to 400 nm, more preferably 150 to 350 nm, and most preferably 200 to 350 nm.
[0011] Average cubic + hexagonal Ti 1-y Al y The thickness of the N sublayer is suitably from 70 to 250 nm, preferably from 90 to 200 nm.
[0012] Cubic Ti1-x Al x N sublayer and cubic + hexagonal Ti 1-y Al y The thickness ratio of the N sublayers is suitably from 5:1 to 1:1, preferably from 4:1 to 1.5:1.
[0013] Cubic Ti 1-x Al x In the N sublayers, suitably, 0.64≦x≦0.70, preferably 0.66 to 0.68.
[0014] Cubic + hexagonal Ti 1-y Al y In the N sublayers, suitably 0.64≦y≦0.70, preferably 0.66 to 0.68.
[0015] Cubic Ti 1-x Al x N sublayer and cubic + hexagonal Ti 1-y Al y The number of each of the N sublayers is suitably 3-40, preferably 4-20, most preferably 5-15.
[0016] In one embodiment, cubic Ti 1-x Al x x and cubic + hexagonal Ti in the N sublayer 1-y Al y The difference with y in the Nth sublayer is less than 0.09, or 0.05 or less, or 0.03 or less.
[0017] In one embodiment, x is substantially equal to y.
[0018] The total thickness of the (Ti,Al)N multilayer is 0.5-10 μm, alternatively 1-8 μm, alternatively 2-6 μm.
[0019] In 2θXRD of the entire (Ti,Al)N multilayer, the ratio of the peak area intensity of the hexagonal (0 0-1 0) reflection to the peak area intensity of the cubic (2 0 0) reflection, I(0 0-1 0) / I(2 0 0), is 0.05 to 0.75, preferably 0.08 to 0.35.
[0020] Cubic Ti 1-x Al x N sublayer and cubic + hexagonal Ti 1-y Al y The N sublayer is suitably a PVD layer, preferably a cathodic arc vapour deposition layer.
[0021] In one embodiment, the coating comprises one or more further layers of metal nitride under the (Ti,Al)N multilayer. The metal nitride is suitably a nitride / nitrides of one or more metals belonging to groups 4 to 6 of the IUPAC Periodic Table of the Elements, and optionally Al and / or Si. Examples of such metal nitrides are TiN and (Ti,Al)N. The total thickness of these one or more metal nitride layers may be from about 0.1 to about 2 μm, or from about 0.2 to about 1 μm.
[0022] The substrate of the coated cutting tool may be selected from the group of cemented carbide, cermet, ceramic, cubic boron nitride, and high speed steel.
[0023] The coated cutting tool may be a cutting tool insert for metalworking, a drill or a solid end mill. The cutting tool insert is suitably a milling insert, a drill insert or a turning insert.
[0024] As used herein, "cubic" in the term "cubic sublayer" refers to the absence of point-like diffraction spots from hexagonal crystallographic planes to be seen in electron diffraction analysis and / or the absence of hexagonal peaks to be seen in XRD θ-2θ analysis. [Brief description of the drawings]
[0025] [Figure 1] 1 is a schematic diagram of a substrate having a coating according to one embodiment of the present invention. [Diagram 2] FIG. 1 shows the electron diffraction pattern of a cubic+hexagonal sublayer. [Diagram 3] FIG. 2 shows the electron diffraction pattern of the cubic sublayer. [Figure 4] FIG. 1 shows an X-ray diffractogram of a cubic crystal layer. [Diagram 5] FIG. 1 shows an X-ray diffractogram of a cubic + hexagonal crystal layer. [Figure 6] FIG. 1 shows an X-ray diffractogram of a (Ti,Al)N multilayer. EXAMPLES
[0026] Example 1: Ti, both according to the present invention and outside the present invention 0.33 Al 0.67 Different coatings of N were deposited on sintered cemented carbide cutting tool insert blanks in the form of CNMG120804-MM. The cemented carbide composition was 10 wt% Co, 0.4 wt% Cr, and the balance WC. The cemented carbide blanks were coated by cathodic arc evaporation in a vacuum chamber containing four arc flanges. Targets of Ti-Al were attached to all flanges.
[0027] An uncoated blank is attached to a pin and rotated three times in the PVD chamber.
[0028] Cubic Ti 0.33 Al 0.67 To create the N layer, the chamber was placed in high vacuum (10 -2 The chamber was pumped down to 10 Pa (less than 10 Pa) and heated to about 450° C. by a heater placed inside the chamber. If a layer had to be deposited as the first layer on a substrate, the blank was etched in Ar plasma for 60 min. The chamber pressure (reaction pressure) was set to 10 Pa of N2 gas and a unipolar DC bias voltage of −300 V (with respect to the chamber wall) was applied to the blank assembly. The positive pole was operated in arc discharge mode with a current of 150 A (each).
[0029] Cubic + hexagonal Ti 0.33 Al 0.67 To create the N layer, the chamber was placed in high vacuum (10 -2The chamber was pumped down to a pressure of less than 1 Pa and heated to about 450° C. by a heater placed in the chamber. If a layer had to be deposited as the first layer on a substrate, the blank was etched in Ar plasma for 60 min. The chamber pressure (reaction pressure) was set to 4 Pa of N2 gas and a unipolar pulsed bias voltage of −50 V (with respect to the chamber wall) was applied to the blank assembly at a pulsed bias frequency of 2 kHz and a duty cycle of 10%. The positive pole was operated in arc discharge mode with a current of 150 A (each).
[0030] A total layer thickness of 3 μm was deposited.
[0031] The samples, single layers, and layer combinations that were made are found in Table 1. Sublayer thicknesses are average values. TIFF0007584456000001.tif91170
[0032] Selected area electron diffraction (SAED) analysis by transmission electron microscopy (TEM) was performed on sample 4. Figure 2 shows the diffraction pattern of the cubic + hexagonal sublayers, and Figure 3 shows the diffraction pattern of the cubic sublayers.
[0033] A 300 kV FEG TEM was used with the beam in collimated illumination mode and a selected area aperture with a projected size in the target plane of approximately 150 nm (ie, a size directly comparable to the features of the sample).
[0034] The samples were cross-section samples obtained by focused ion beam lift-out and polishing using Ga+ ions.
[0035] FIG. 2 shows the results with the first type of sublayer, with clear point-like diffraction spots from the cubic crystallographic planes (2 2 0), (2 0 0), and (1 1 1), as well as clear point-like diffraction spots from the hexagonal crystallographic plane (1 0-1 0). and Therefore, this layer is a mixed cubic + hexagonal layer.
[0036] Figure 3 shows the results from the second type of sublayer, where again clear point-like diffraction spots from the cubic crystallographic planes (2 2 0), (2 0 0), and (1 1 1) are seen. However, there are no point-like diffraction spots from the hexagonal crystallographic planes. Only weak and indistinct ring-like reflections from the (1 0-1 0) planes are seen. Thus, this layer does not contain a substantial crystalline hexagonal phase and is considered a single-phase cubic layer.
[0037] As a further investigation, XRD analysis was performed on the cubic and cubic+hexagonal layers. Due to the difficulty in performing XRD on specific sublayers that are present as part of a multilayer structure, XRD measurements were performed on the cubic monolayer, sample 1, and additional samples were prepared following the process parameters used to create the cubic+hexagonal sublayers.
[0038] X-ray diffraction (XRD) analysis was carried out on the flank faces of the coated inserts using a PANalytical CubiX3 diffractometer equipped with a PIXcel detector. The coated cutting tool inserts were mounted in a sample holder, which ensured that the flank faces of the samples were parallel to the reference plane of the sample holder and also that the flank faces were at the appropriate height. The Cu-K α A line was used for the measurements. A 1 / 2 degree anti-scatter slit and a 1 / 4 degree divergence slit were used. The diffraction intensity from the coated cutting tool was measured around the 2θ angle where the relevant peak occurred.
[0039] Figures 4 and 5 show the diffractograms. Figure 4 shows the diffractogram of sample 1, with no sign of a hexagonal (h) peak. Figure 5 shows a diffractogram from another type of layer, containing both cubic (c) and hexagonal (h) peaks.
[0040] Therefore, the XRD analysis also concluded that the cubic phase present can indeed be considered as a single phase cubic phase.
[0041] XRD analysis was further carried out on the entire (Ti,Al)N multilayer using sample 4. The same XRD analysis method as above was used.
[0042] The diffractogram is shown in Figure 6. Table 2 below shows the peak intensity values. TIFF0007584456000002.tif29170
[0043] Therefore, the ratio I(1 0-1 0) / I(2 0 0) was 0.11.
[0044] Explanation of terms used in Examples 2 and 3 The following expressions / terms are commonly used in metal cutting and are explained in the table below. V c (m / min) Cutting speed in meters per minute f n (mm / rev) Feed per revolution (turning) a p (mm) Axial depth of cut in millimeters
[0045] The inserts of Example 1 were tested for flank wear and crater wear.
[0046] Example 2 Flank wear test Longitudinal turning Workpiece material Uddeholm Sverker 21 (tool steel), hardness approximately 210HB, D=180, L=700mm, V c =125m / min f n =0.072mm / rev a p =2mm No cutting fluid
[0047] The cut-off criterion for tool life is flank wear VB of 0.15 mm.
[0048] Example 3 Crater Abrasion Test: Longitudinal turning Workpiece material Ovako 825B, ball bearing steel. Hot rolled and annealed, hardness approx. 200HB, D=160, L=700mm, V c =160m / min f n =0.3mm / rev a p =2mm With cutting fluid
[0049] Tool life standard is 0.8mm 2 is the crater area.
[0050] The results of the tests according to Examples 2-3 are shown in Table 3 below. TIFF0007584456000003.tif74170
[0051] It can be concluded that the samples according to the invention (No. 3 and No. 4) have very good flank wear resistance, while the crater wear resistance remains at about the same level as in the single cubic (Ti,Al)N layer.
Claims
1. A coated cutting tool for metalworking comprising a substrate and a coating, the coating being made of alternating cubic Ti 1-x A x N sublayer, 0.60≦x≦0.75, and cubic+hexagonal Ti 1-y A y N sublayers, (Ti,Al)N multilayers with 0.60≦y≦0.75, with the average cubic Ti 1-x A x The thickness of the N sublayer is 100-400 nm, and the average cubic + hexagonal Ti 1-y A y The thickness of the N sublayer is 70 to 200 nm, and the cubic Ti 1-x A x N sublayer and cubic + hexagonal Ti 1-y A y A coated cutting tool, wherein the number of each of the N sub-layers is 2-50.
2. Average cubic Ti 1-x A x The coated cutting tool of claim 1, wherein the N sublayer thickness is 150-400 nm.
3. Cubic Ti 1-x A x N sublayer and cubic + hexagonal Ti 1-y A y 3. The coated cutting tool according to claim 1, wherein the thickness ratio of the N sublayer is from 5:1 to 1:
1.
4. Cubic Ti 1-x A x The coated cutting tool according to claim 1 , wherein in the N sublayers, 0.64≦x≦0.
70.
5. Cubic + hexagonal Ti 1-y A y The coated cutting tool according to claim 1 , wherein in the N sublayer, 0.64≦y≦0.
70.
6. Cubic Ti 1-x A x N sublayer and cubic + hexagonal Ti 1-y A y 6. The coated cutting tool according to claim 1, wherein the number of each of the N sub-layers is between 3 and 40.
7. Cubic Ti 1-x A x x in N sublayer and cubic + hexagonal Ti 1-y A y 7. The coated cutting tool according to claim 1, wherein the difference between y in the N sublayer is less than 0.
09.
8. The coated cutting tool of claim 1 , wherein in one embodiment x is substantially equal to y.
9. Coated cutting tool according to any one of claims 1 to 8, wherein the total thickness of the (Ti,Al)N multilayer is from 0.5 to 10 μm, or from 1 to 8 μm, or from 2 to 6 μm.
10. The coated cutting tool according to claim 1, wherein in 2θ XRD of the entire (Ti,Al)N multilayer, I(0 0-1 0) / I(2 00) is 0.05 to 0.
75.
11. Cubic Ti 1-x A x N sublayer and cubic + hexagonal Ti 1-y A y 11. The coated cutting tool of claim 1, wherein the N sublayer is a cathodic arc vapor deposition layer.
Citation Information
Patent Citations
Surface-coated cutting tool with hard coating layer showing excellent wear resistance and chipping resistance in high-speed cutting work
JP2015066644A
Surface-coated cutting tool with hard coated layer exerting excellent wear resistance and chipping resistance in high-speed cutting working
JP2015104757A
Surface-coated cutting tool
JP2016093857A
Surface-coated cutting tool
JP2016175161A
Surface-coated member
WO2013002385A1