Solvent Composition
A solvent composition with ketone and lactone compounds addresses hump formation and pre-wet performance issues in EBR, enhancing efficiency and reducing coating solution usage in semiconductor manufacturing.
Patent Information
- Application Number
- JP2022569540
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-08-11
AI Technical Summary
Existing solvent compositions for edge bead removal (EBR) in semiconductor manufacturing processes fail to effectively suppress the formation of humps at the wafer peripheral edge while also providing pre-wet performance, leading to inefficiencies and increased use of expensive coating solutions.
A solvent composition comprising a ketone compound with 5 or more carbon atoms, a lactone compound, and optionally alkylene glycol alkyl ether or its carboxylic acid ester, with specific mass ratios, is used to suppress hump formation during EBR and provide pre-wet performance.
The solvent composition effectively reduces hump formation during EBR, enhances pre-wet performance, and minimizes the amount of coating solution used, thereby improving process efficiency and reducing costs.
Smart Images

Figure 0007584540000001 
Figure 0007584540000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a solvent composition having EBR performance capable of suppressing the height of a hump that occurs at the edge of a coating film during Edge Bead Removal (EBR) of a wafer, which is performed after a coating liquid such as an antireflection agent, resist, etc. is applied onto a wafer with a spin coater in a coating film formation step on a wafer in a semiconductor manufacturing process, and also having pre-wetting performance having an effect of reducing the amount of coating liquid such as an antireflection agent, resist, etc. used. [Background technology]
[0002] In the lithography process to form a pattern on a semiconductor wafer, a spin coater is used to apply coating liquids such as anti-reflection agents and resists to the wafer surface. During this process, a bead of thick coating film is formed on the wafer periphery, and EBR processing is performed to dissolve and remove this with a solvent. In this EBR processing, a method is generally used in which a solvent (called an EBR solvent) is ejected from a nozzle onto the surface of the coating film on the periphery and onto the back surface of the wafer while the wafer is rotating.
[0003] After the bead on the wafer periphery is dissolved and removed by EBR, the wafer is left with a ring-shaped area where the coating film has been removed and an area where the coating film remains. At the periphery of the coating film near the boundary between these areas, a raised area of the coating film called a hump is formed during EBR. The ratio of the thickness of the part of the coating film where the hump is formed divided by the thickness of the flat coating film inside the periphery where there is no hump is called the hump ratio. Because this hump causes a decrease in yield in the lithography process, it is necessary to suppress the hump in the coating film during EBR, that is, to keep the hump ratio as close to 1 as possible.
[0004] In Patent Document 1 (JP Patent Publication No. 2017-92445), when performing EBR processing, gas is sprayed in a circumferential direction from a slit-shaped nozzle near the nozzle from which the removal liquid is ejected, thereby applying a force in the circumferential outward direction to the removal liquid that comes into contact with the wafer surface, thereby suppressing the height of the hump.
[0005] In Patent Document 2 (JP Patent Publication No. 2018-181963), an attempt is made to reduce the height of the hump by adding dilution water with high surface tension to OK-73 thinner (a mixture of propylene glycol monomethyl ether (PGME) / propylene glycol monomethyl ether acetate (PGMEA) = 0.7 / 0.3) and cooling the solvent and piping to control the surface tension of the EBR treatment liquid.
[0006] Patent Document 3 (JP 2018-121045 A) attempts to suppress humps by optimizing processing conditions during EBR processing, such as the rotation speed of the spin coater wafer, the angle of the EBR solvent nozzle, and the EBR processing time.
[0007] In this way, attempts have been made to provide spin coaters with functions to suppress humps and to optimize operating conditions. In addition, attempts have been made to suppress humps by using EBR solvents with appropriate compositions for the coating film.
[0008] For example, Patent Document 4 (JP Patent Publication No. 2007-179043) describes a mixture of γ-butyrolactone, anisole, and methyl ethyl ketone (MEK) as the composition of a cleaning liquid for photolithography.
[0009] Patent Document 5 (JP 2006-189518 A) describes a mixture of butyl acetate and cyclohexanone as the composition of a cleaning liquid for lithography.
[0010] Patent Document 6 (JP 2007-178589 A) describes a mixture of butyl acetate and cyclohexanone, and a mixture of butyl acetate, cyclohexanone, and propylene glycol monomethyl ether acetate (PGMEA) as the composition of a cleaning liquid for photolithography.
[0011] Patent Document 7 (JP Patent Publication No. 11-218933) describes a mixture of propylene glycol monomethyl ether (PGME), methyl ethyl ketone (MEK) and γ-butyrolactone as the composition of a solvent for cleaning and removing resist. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] JP 2017-92445 A [Patent Document 2] JP 2018-181963 A [Patent Document 3] JP 2018-121045 A [Patent Document 4] JP 2007-179043 A [Patent Document 5] JP 2006-189518 A [Patent Document 6] JP 2007-178589 A [Patent Document 7] Japanese Patent Application Publication No. 11-218933 Summary of the Invention [Problem to be solved by the invention]
[0013] On the other hand, coating solutions such as anti-reflection agents and resists are particularly expensive, so in order to reduce the amount of these coating solutions used as much as possible and to apply them evenly, an appropriate solvent is applied to the entire wafer surface immediately before spin coating, which is called a pre-wetting process.
[0014] When different solvents are used for the pre-wet treatment and the EBR treatment, it is necessary to install piping lines, tanks, etc. for each solvent. A solvent composition (PGME / PGMEA=0.7 / 0.3) known as OK-73 thinner has been conventionally used for EBR treatment and pre-wet treatment. However, OK-73 thinner has a problem of a high hump ratio after EBR treatment. For this reason, it is desirable to develop a solvent composition that can suppress the formation of humps and has the performance of both EBR treatment and pre-wet treatment.
[0015] An object of the present invention is to provide a solvent composition that has EBR performance and pre-wetting performance, and can suppress the formation of a hump on the peripheral edge of a wafer during EBR treatment in a semiconductor manufacturing process. [Means for solving the problem]
[0016] The present invention has been made in view of the above circumstances, and the inventors have intensively studied the composition of a solvent composition. As a result, the inventors have found that a solvent composition containing a specific ketone compound and a lactone compound can suppress the formation of a hump formed on the peripheral edge of a wafer during EBR processing, and has pre-wetting performance. That is, the present invention includes the following [1] to
[20] . [1] A solvent composition comprising (a) a ketone compound having 5 or more carbon atoms and (b) a lactone compound, wherein the content of (b) is 5 to 90 mass %. [2] The solvent composition according to [1], wherein the (a) is a cyclic ketone compound. [3] The solvent composition according to [2], wherein (a) is cyclohexanone. [4] The solvent composition according to any one of [1] to [3], wherein the (b) is γ-butyrolactone. [5] The solvent composition according to any one of [1] to [4], wherein the content of (a) is 5 to 80 mass %. [6] The solvent composition according to any one of [1] to [5], further comprising (c) at least one member selected from the group consisting of alkylene glycol alkyl ethers and carboxylates thereof, represented by the following formula (1): R 1 O(C n H 2n O) x R 2 (1) (In formula (1), R 1 R represents an alkyl group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. 2 represents a hydrogen atom or an acyl group selected from the group consisting of -COCH3, -COC2H5, -COC3H7 and -COC4H9. n is 2 or 3, and x is an integer from 1 to 4. [7] The solvent composition according to [6], wherein the content of (c) is 5 to 80 mass %. [8] The solvent composition according to [6], wherein the content of (a) is 5 to 70 mass %, the content of (b) is 5 to 60 mass %, and the content of (c) is 5 to 70 mass %. [9] The solvent composition according to any one of [6] to [8], wherein the (c) is propylene glycol monomethyl ether.
[10] The solvent composition according to any one of [6] to [8], wherein the (c) is propylene glycol monomethyl ether acetate.
[11] The solvent composition according to any one of [6] to [8], wherein the (c) contains both propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.
[12] The solvent composition according to any one of [1] to
[11] , which is used for removing an unnecessary coating film that is formed by applying a coating liquid to a substrate and adheres to an edge portion of the substrate.
[13] The solvent composition according to
[12] , wherein the coating liquid is at least one selected from the group consisting of a resist and an antireflection agent.
[14] The solvent composition according to any one of [1] to
[13] , which is used for pre-wetting a substrate.
[15]
[13] An EBR treatment method, comprising: removing an unnecessary coating film that is formed by applying a coating liquid to a substrate using the solvent composition according to any one of [1] to
[11] and that is attached to an edge portion of the substrate.
[16] The EBR treatment method according to
[15] , wherein the coating liquid is at least one selected from the group consisting of a resist and an anti-reflection agent.
[17] A method for prewetting a substrate, comprising prewetting the substrate with the solvent composition according to any one of [1] to
[11] .
[18] Use of the solvent composition according to any one of [1] to
[11] for removing an unnecessary coating film that is formed by applying a coating liquid to a substrate and adheres to an edge portion of the substrate.
[19] The use according to
[18] , wherein the coating liquid is at least one selected from the group consisting of a resist and an antireflection agent.
[20] Use of the solvent composition according to any one of [1] to
[11] for prewetting a substrate. Effect of the Invention
[0017] The solvent composition of the present invention has EBR performance and pre-wetting performance, and can suppress the formation of a hump on the peripheral edge of a wafer during EBR treatment in the semiconductor manufacturing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Preferred embodiments of the present invention will be described below, but it should be understood that the present invention is not limited to these embodiments and that various applications are possible within the spirit and scope of the present invention.
[0019] [Solvent composition] The solvent composition contains (a) a ketone compound having 5 or more carbon atoms and (b) a lactone compound, and the content of (b) in the solvent composition is 5 to 90 mass %.
[0020] (a) Ketone compounds with 5 or more carbon atoms The ketone compound can be used without any particular limitation as long as it is a ketone compound having 5 or more carbon atoms. From the viewpoint of easy availability, the ketone compound preferably has 5 to 11 carbon atoms, and more preferably has 5 to 7 carbon atoms. By having 5 or more carbon atoms, the flash point does not become too low, and the requirements for facilities, working environment, etc. in the production and use of the solvent composition can be reduced.
[0021] The ketone compound may be cyclic or non-cyclic. Examples of the cyclic ketone compound include 2-methylcyclobutanone, cyclopentanone, 2-methylcyclopentanone, 2,5-dimethylcyclopentanone, cyclohexanone, 2-methylcyclohexanone, and cycloheptanone. Examples of the non-cyclic ketone compound include 2-pentanone, 3-pentanone, 4-methyl-2-pentanone, 2,4-dimethyl-3-pentanone, 2-hexanone, 3-hexanone, 5-methyl-2-hexanone, 2-heptanone, 3-heptanone, 4-heptanone, 2,6-dimethyl-4-heptanone, 2-octanone, 3-octanone, 2-nonanone, 3-nonanone, 5-nonanone, and 2-undecanone. The ketone compound is preferably a cyclic ketone compound, and among the above cyclic ketone compounds, cyclohexanone is more preferable.
[0022] The content of (a) in the solvent composition is preferably from 5 to 80% by mass, more preferably from 10 to 70% by mass, and further preferably from 20 to 60% by mass.
[0023] (b) Lactone compounds The lactone compound can be used without any particular limitation. The lactone compound preferably has 4 to 9 carbon atoms, more preferably 4 to 6 carbon atoms. The lactone compound preferably has 4 to 7 ring members, more preferably 5 or 6 ring members. Preferred lactone compounds include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, δ-valerolactone, β-valerolactone, ε-caprolactone, and γ-nonalactone. Among the above lactone compounds, γ-butyrolactone is preferred from the viewpoint of availability.
[0024] The content of (b) in the solvent composition is from 5 to 90% by mass, preferably from 10 to 70% by mass, more preferably from 15 to 50% by mass, and further preferably from 20 to 45% by mass.
[0025] (c) Alkylene glycol alkyl ether It is preferable that the solvent composition further contains (c) at least one selected from the group consisting of alkylene glycol alkyl ethers and carboxylates thereof, which are represented by the following formula (1). R 1 O(C n H 2n O) x R 2 (1) (In formula (1), R 1 R represents an alkyl group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. 2 represents a hydrogen atom or an acyl group selected from the group consisting of -COCH3, -COC2H5, -COC3H7 and -COC4H9. n is 2 or 3, and x is an integer from 1 to 4. R 2 When R is a hydrogen atom, formula (1) represents an alkylene glycol alkyl ether, and R 2 When R is an acyl group, formula (1) represents a carboxylic acid ester of an alkylene glycol alkyl ether. 2is preferably a hydrogen atom or -COCH3 (acetyl group).
[0026] Examples of the alkylene glycol alkyl ether represented by formula (1) include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol isopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monoethyl ether, etc. Examples of the carboxylic acid ester of the alkylene glycol alkyl ether represented by formula (1) include acetate, propionate, butyrate, etc. of the above alkylene glycol alkyl ether.
[0027] The content of (c) in the solvent composition is preferably from 5 to 80% by mass, more preferably from 10 to 75% by mass, and even more preferably from 15 to 70% by mass.
[0028] The content of (c) relative to the total of (a), (b) and (c) is preferably 5 to 70 mass %, more preferably 7 to 65 mass %, and further preferably 10 to 55 mass %.
[0029] In one embodiment, (c) is preferably propylene glycol monomethyl ether. When (c) is propylene glycol monomethyl ether, the content of propylene glycol monomethyl ether in the solvent composition is preferably 5 to 70 mass%, more preferably 10 to 60 mass%, and further preferably 15 to 50 mass%.
[0030] In another embodiment, (c) is preferably propylene glycol monomethyl ether acetate. When (c) is propylene glycol monomethyl ether acetate, the content of propylene glycol monomethyl ether acetate in the solvent composition is preferably 5 to 50 mass%, more preferably 10 to 45 mass%, and further preferably 15 to 40 mass%.
[0031] In yet another embodiment, (c) preferably contains both propylene glycol monomethyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA). In this case, the mass ratio of propylene glycol monomethyl ether (PGME) to propylene glycol monomethyl ether acetate (PGMEA) is preferably PGME / PGMEA=1.0 to 3.0, more preferably 1.5 to 2.5. The total content of propylene glycol monomethyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA) in the solvent composition is preferably 5 to 50 mass%, more preferably 7 to 45 mass%, and even more preferably 10 to 40 mass%.
[0032] When the solvent composition contains (c), the content of (a) is preferably 5 to 70 mass%, the content of (b) is preferably 5 to 80 mass%, and the content of (c) is preferably 5 to 70 mass%, and more preferably the content of (a) is 10 to 60 mass%, the content of (b) is 10 to 60 mass%, and the content of (c) is 10 to 50 mass%.
[0033] When (c) is propylene glycol monomethyl ether, the content of (a) is preferably 10 to 70 mass%, the content of (b) is preferably 5 to 60 mass%, and the content of propylene glycol monomethyl ether is preferably 10 to 70 mass%, and more preferably the content of (a) is 15 to 60 mass%, the content of (b) is 10 to 50 mass%, and the content of propylene glycol monomethyl ether is preferably 15 to 50 mass%.
[0034] When (c) is propylene glycol monomethyl ether acetate, the content of (a) is preferably 5 to 60 mass%, the content of (b) is preferably 10 to 70 mass%, and the content of propylene glycol monomethyl ether acetate is preferably 5 to 50 mass%, and more preferably the content of (a) is 10 to 50 mass%, the content of (b) is 20 to 55 mass%, and the content of propylene glycol monomethyl ether acetate is 10 to 45 mass%.
[0035] When (c) contains both propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate, it is preferable that the content of (a) is 5 to 60 mass%, the content of (b) is 10 to 80 mass%, and the total content of propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate is 5 to 50 mass%, and it is more preferable that the content of (a) is 10 to 50 mass%, the content of (b) is 20 to 75 mass%, and the total content of propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate is 7 to 45 mass%.
[0036] [Coating film] The solvent composition can be applied to various coating films such as anti-reflective films and resist films. The coating film is formed by applying a coating liquid onto a substrate such as a silicon wafer using a spin coater or the like. The coating liquid is preferably at least one selected from the group consisting of resists and anti-reflective agents.
[0037] The resist may be either positive or negative, and examples thereof include rubber-based negative resists, g-line photoresists, i-line photoresists, KrF photoresists, ArF photoresists, EUV photoresists, and electron beam photoresists. Chemically amplified resists containing a photoacid generator can also be used. Resists that can be developed with an alkaline aqueous solution are preferably used. Specifically, examples include a positive resist containing a naphthoquinone diazide compound and a base resin such as a novolac resin, a positive resist containing a photoacid generator, a compound that decomposes with an acid to increase its solubility in an alkaline aqueous solution, and an alkali-soluble resin, a positive resist containing a photoacid generator and an alkali-soluble resin having a group that decomposes with an acid to increase its solubility in an alkaline aqueous solution, and a negative resist containing a photoacid generator, a crosslinking agent, and an alkali-soluble resin. Examples of the base resin of the resist include novolac resin, polyhydroxystyrene, (meth)acrylic resin, (meth)acrylic acid ester polymer, hydroxystyrene (meth)acrylic acid copolymer, and silsesquioxane. "(Meth)acrylic" is a general term for acrylic and methacrylic.
[0038] As the antireflection agent, known antireflection agents can be used, and examples thereof include organic antireflection agents, silicon-containing antireflection agents (SiARC) and the like.
[0039] Examples of the organic antireflection agent include a composition containing a light-absorbing compound and a resin, a composition containing a resin having light-absorbing groups linked by a chemical bond and a crosslinking agent, a composition containing a light-absorbing compound and a crosslinking agent, and a composition containing a light-absorbing polymeric crosslinking agent.
[0040] The light absorbing compounds include benzophenone, benzotriazole, azo compounds, naphthalene, anthracene, anthraquinone, triazine, and derivatives thereof.
[0041] Examples of the resin include polyester, polyimide, polystyrene, poly(4-hydroxystyrene), copolymers of 4-hydroxystyrene with alkyl methacrylate, alkyl acrylate and / or styrene, novolac resin, polyacetal resin, (meth)acrylic resin, polyvinyl alcohol, fluorocarbon polymers, polymers having a naphthalene skeleton, polymers having a norbornene skeleton, and alicyclic polymers such as maleic anhydride copolymers.
[0042] Examples of resins having light-absorbing groups linked by chemical bonds include resins having a light-absorbing aromatic ring structure such as anthracene ring, naphthalene ring, benzene ring, quinoline ring, quinoxaline ring, thiazole ring, etc. In particular, (meth)acrylic resins and novolak resins having an anthracene ring, naphthalene ring, or benzene ring structure are preferably used.
[0043] Examples of the crosslinking agent include melamine, benzoguanamine, urea, and glycoluril in which the hydrogen atom of the amino group is substituted with at least one group selected from the group consisting of a methylol group and an alkoxymethyl group.
[0044] The silicon-containing antireflection agent is a composition containing a silicon-containing polymer, and uses silicon-silicon σ-bonds as the light absorbing site for ArF light (193 nm). Examples of the silicon-containing polymer include polysilanes with pendant phenyl groups; polyolefins with pendant silicon-containing groups, poly(meth)acrylates, polyvinyl alcohols, polyvinyl phenols, polyvinyl maleimides, cellulose, amylose, dextran, pullulan, and derivatives thereof.
[0045] [EBR processing method] The solvent composition is preferably used for EBR treatment. EBR treatment is a treatment for removing an unnecessary coating film attached to the edge of a substrate coated with a coating liquid. The EBR treatment method using the solvent composition is not particularly limited, and can be performed by a method known in the art. For example, while a substrate having a coating film formed on its surface is held by a rotating holder and rotated, the solvent composition is discharged from a nozzle toward a position a predetermined distance inside the outer edge of the coating film, and a drying treatment is performed as necessary.
[0046] The hump ratio after the EBR treatment is preferably 1.5 or less, more preferably 1.4 or less, and even more preferably 1.3 or less.
[0047] [Pre-wet processing method] The solvent composition is preferably used for the pre-wet treatment. The pre-wet treatment method using the solvent composition is not particularly limited, and can be carried out by a method known in the art. For example, the substrate is held by a rotating holder, the solvent composition is discharged from a nozzle, and the substrate is started to rotate, and the solvent is applied to the entire surface of the substrate by centrifugal force. By applying the coating liquid after the pre-wet treatment, the amount of coating liquid used can be reduced.
[0048] [substrate] The substrate to which the solvent composition is applied is not particularly limited, and examples thereof include a silicon wafer, a glass substrate, and a metal substrate. EXAMPLES
[0049] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples in any way.
[0050] In the following examples and comparative examples, the following antireflection agents or resists were used. Anti-reflective agent A: "ODL301" manufactured by Shin-Etsu Chemical Co., Ltd. Anti-reflective agent B: Nissan Chemical Co., Ltd. "LT8003" Anti-reflective agent C: Nissan Chemical Co., Ltd. "HM918" (silicon-based anti-reflective agent) Anti-reflective agent D: "SHB961" (silicon-based anti-reflective agent) manufactured by Shin-Etsu Chemical Co., Ltd. Resist A: "X198" (chemically amplified resist) manufactured by Shin-Etsu Chemical Co., Ltd. Resist B: "P6255" manufactured by Tokyo Ohka Kogyo Co., Ltd. (chemically amplified resist, base resin: acrylic resin)
[0051] 1. Preparation of Solvent Composition [Example 1] A solvent composition of Example 1 was prepared by weighing and mixing 6.0 g of cyclohexanone (electronics grade product manufactured by Showa Denko K.K.) and 54.0 g of γ-butyrolactone (electronics grade product manufactured by Showa Denko K.K.) in a 110 mL glass sample bottle at room temperature in the air. [Examples 2 to 22, Comparative Examples 1 to 7] Solvent compositions having the compositions shown in Table 1 were prepared in the same manner as in Example 1. Propylene glycol monomethyl ether (PGME) and propylene glycol monomethyl ether acetate (PGMEA) in the compositions in Table 1 were electronics industry grade products manufactured by Showa Denko K.K.
[0052] 2.EBR processing test According to the following procedure, coating films of antireflection agents A to D or resists A to B were formed, and the hump ratios after EBR treatment were calculated.
[0053] [EBR treatment test of anti-reflective agent A] (1) Pre-wetting A 6-inch silicon wafer was set on the wafer holder (spin chuck) of a spin coater (ACT-300AIIS, manufactured by Active Corporation), and 1.5 to 2.0 g of a processing solution consisting of PGME:PGMEA = 0.700:0.300 (mass ratio) (a composition known as OK-73 thinner) was dispensed from a nozzle onto the center of the stationary wafer. The wafer was then rotated at 1000 rpm for 10.5 seconds to perform a pre-wet process in which the wafer surface was coated with the solvent. (2) Application of anti-reflective agent The pre-wetted wafer was spin-coated with 0.2 to 0.25 g of antireflection agent A at 1300 rpm for 30 seconds and then at 700 rpm for 3 seconds to form an antireflection film with a thickness of 100 nm over the entire wafer. (3) EBR treatment The wafer on which the anti-reflective coating was formed was rotated at 1000 rpm, and 8 g of the solvent composition shown in Table 1 was sprayed over 20 seconds toward a position 2 mm from the edge of the wafer to clean and remove the peripheral portion of the coating film. The wafer was then maintained at a rotation speed of 3000 rpm for 20 seconds to air-dry the cleaned portion. (4) Baking process After the EBR process, the wafer was placed on a hot plate heated to 250° C. for 60 seconds for a baking process, and then placed on a hot plate heated to 350° C. for 60 seconds for a baking process, and then cooled to room temperature. (5) Calculation of hump ratio The thickness of the peripheral and flat parts of the anti-reflective coating formed on the silicon wafer in this way was measured by scanning with a contact profiler (P-12, manufactured by KLA-TENCOR). The hump ratio was calculated by dividing the hump height (height from the surface of the silicon wafer to the top of the hump) by the film thickness of the anti-reflective coating (height from the surface of the silicon wafer to the flat part located from the peripheral part of the anti-reflective coating toward the center of the wafer). The results are shown in Table 1.
[0054] [EBR treatment test of anti-reflective agent B] The hump ratio after EBR treatment was calculated in the same manner as in the "EBR treatment test of anti-reflective agent A", except that the operations of (2) and (4) were as follows. (2) Application of anti-reflective agent 0.2 to 0.25 g of antireflective agent B was spin-coated onto the pre-wetted wafer at 2000 rpm for 30 seconds, 3000 rpm for 5 seconds, and 2000 rpm for 5 seconds to form an antireflective film with a thickness of 190 nm over the entire wafer. (4) Baking process After the EBR process, the wafer was placed on a hot plate heated to 180° C. for 60 seconds for a baking process, and then placed on a hot plate heated to 350° C. for 60 seconds for a baking process, and then cooled to room temperature.
[0055] [EBR treatment test of anti-reflective agent C] The hump ratio after EBR treatment was calculated in the same manner as in the "EBR treatment test of anti-reflective agent A", except that the operations of (2) and (4) were as follows. (2) Application of anti-reflective agent The pre-wetted wafer was spin-coated with 0.2 to 0.25 g of antireflection agent C at 2700 rpm for 30 seconds and then at 700 rpm for 3 seconds to form an antireflection film with a thickness of 40 nm over the entire wafer. (4) Baking process After the EBR process, the wafer was baked on a hot plate at 220° C. for 60 seconds and then cooled to room temperature.
[0056] [EBR treatment test of anti-reflective agent D] The hump ratio after EBR treatment was calculated in the same manner as in the "EBR treatment test of anti-reflective agent A", except that the operations of (2) and (4) were as follows. (2) Application of anti-reflective agent The pre-wetted wafer was spin-coated with 0.2 to 0.25 g of antireflection agent D at 1250 rpm for 30 seconds and then at 700 rpm for 3 seconds to form an antireflection film with a thickness of 40 nm over the entire wafer. (4) Baking process After the EBR process, the wafer was baked on a hot plate at 220° C. for 60 seconds and then cooled to room temperature.
[0057] [EBR processing test of resist A] The hump ratio after EBR treatment was calculated in the same manner as in the "EBR treatment test of anti-reflective agent A", except that the operations of (2) and (4) were as follows. (2) Coating of resist A resist film with a thickness of 100 nm was formed over the entire wafer by spin-coating 0.2 to 0.25 g of resist A onto the pre-wetted wafer at 1000 rpm for 30 seconds, 3000 rpm for 5 seconds, and 2000 rpm for 5 seconds. (4) Baking process After the EBR process, the wafer was baked on a hot plate at 100° C. for 60 seconds and then cooled to room temperature.
[0058] [EBR processing test of resist B] The hump ratio after EBR treatment was calculated in the same manner as in the "EBR treatment test of anti-reflective agent A", except that the operations of (2) and (4) were as follows. (2) Coating of resist 0.2 to 0.25 g of resist B was spin-coated onto the pre-wetted wafer at 1000 rpm for 40 seconds, 3000 rpm for 5 seconds, and 2000 rpm for 5 seconds to form a resist film with a thickness of 90 nm over the entire wafer. (4) Baking process After the EBR process, the wafer was baked on a hot plate at 120° C. for 60 seconds and then cooled to room temperature.
[0059] 3. Pre-wetting test The solvent compositions in Table 1 were evaluated for their performance as pre-wet processing liquids by the following procedure. (1) Pre-wetting A 6-inch silicon wafer was set on the wafer holder (spin chuck) of a spin coater (ACT-300AIIS, manufactured by Active Corporation), and 1.5 g of the solvent composition shown in Table 1 was dispensed from a nozzle onto the center of the stationary wafer. The wafer was then rotated at 1000 rpm for 10.5 seconds to perform a pre-wet process in which the wafer surface was coated with the solvent composition. (2) Application of anti-reflective agent Antireflection agent D was spin-coated onto the pre-wetted wafer at 1250 rpm for 30 seconds and then at 700 rpm for 3 seconds to form an antireflection film with a thickness of 40 nm over the entire wafer. (3) Performance evaluation The amount of antireflection agent D required to coat the entire wafer was compared with the amount of antireflection agent D required to coat the entire wafer when the solvent composition of Comparative Example 5 was used as the prewet processing liquid, and the effect of reducing the amount of antireflection agent used was evaluated as follows: The composition of Comparative Example 5 (PGME:PGMEA=0.700:0.300 (mass ratio)) is known as OK-73 thinner, and is a composition generally used as a prewet processing liquid. Passed: The amount of anti-reflection agent used was less than that of Comparative Example 5. Failed: The amount of anti-reflection agent used was greater than in Comparative Example 5.
[0060] [Table 1-1] [Table 1-2]
Claims
1. A solvent composition comprising (a) a ketone compound having 5 or more carbon atoms and (b) a lactone compound, the content of (b) being more than 30% by mass and not more than 90% by mass, Further, the solvent composition contains (c) at least one member selected from the group consisting of alkylene glycol alkyl ethers and their carboxylates, represented by the following formula (1): R 1 O(C n H 2n O) x R 2 (1) (In formula (1), R 1 R represents an alkyl group selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. 2 is a hydrogen atom or -COCH 3 , -COC 2 H 5 , -COC 3 H 7 and -COC 4 H 9 wherein n is 2 or 3, and x is an integer from 1 to 4.
2. The solvent composition according to claim 1 , wherein the compound (a) is a cyclic ketone compound.
3. The solvent composition according to claim 2, wherein (a) is cyclohexanone.
4. The solvent composition according to any one of claims 1 to 3, wherein the (b) is γ-butyrolactone.
5. The solvent composition according to any one of claims 1 to 4, wherein the content of (a) is 5% by mass or more and less than 70% by mass.
6. The solvent composition according to any one of claims 1 to 5, wherein the content of (c) is 5% by mass or more and less than 70% by mass.
7. The content of the (a) is 5% by mass or more and less than 70% by mass, the content of the (b) is more than 30% by mass and 60% by mass or less, and the content of the (c) is 5% by mass or more and less than 70% by mass. The solvent composition according to any one of claims 1 to 5.
8. The solvent composition according to any one of claims 1 to 7, wherein the (c) is propylene glycol monomethyl ether.
9. The solvent composition according to any one of claims 1 to 7, wherein the (c) is propylene glycol monomethyl ether acetate.
10. The solvent composition according to any one of claims 1 to 7, wherein (c) contains both propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate.
11. The solvent composition according to any one of claims 1 to 10, which is used for removing an unnecessary coating film that is formed by applying a coating liquid to a substrate and adheres to an edge portion of the substrate.
12. The solvent composition according to claim 11, wherein the coating liquid is at least one selected from the group consisting of a resist and an antireflection agent.
13. The solvent composition according to any one of claims 1 to 12, which is used for pre-wetting a substrate.
14. An EBR treatment method, comprising removing an unnecessary coating film that is formed by applying a coating liquid to a substrate and adheres to an edge portion of the substrate, using the solvent composition according to any one of claims 1 to 10.
15. The EBR processing method according to claim 14, wherein the coating liquid is at least one selected from the group consisting of a resist and an anti-reflection agent.
16. A method of pre-wetting a substrate comprising pre-wetting the substrate with a solvent composition according to any one of claims 1 to 10.
Citation Information
Patent Citations
Solvent for cleaning and removing resist and manufacture of device for forming electronic parts
JP1999218933A
Improved edge bead removal composition for semiconductor stress buffer coatings and use thereof
JP2005524972A
Cleaning liquid for lithography and method for forming semiconductor base material using the same
JP2006189518A
Photosensitive composition removing liquid
JP2006251785A
Cleaning liquid for lithography
JP2007034066A