Method for manufacturing semiconductor device

Electroless plating with a convex-then-smooth surface configuration addresses the limitations of vacuum film forming methods, enhancing semiconductor device reliability by preventing voids and corrosion, thus improving solderability and longevity.

JP7584620B2Active Publication Date: 2024-11-15MITSUBISHI ELECTRIC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023503858
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-02
Filing Date
2022-03-01
Publication Date
2024-11-15
Estimated Expiration
2042-03-01

AI Technical Summary

Technical Problem

Current methods for forming bonding electrode layers on semiconductor elements using vacuum film forming techniques, such as evaporation or sputtering, struggle to achieve thicknesses greater than 1.0 μm, leading to increased manufacturing costs and uneven surfaces that compromise the long-term reliability of semiconductor devices due to void formation and reduced adhesion.

Method used

A method involving electroless plating is employed to form a bonding electrode layer with a convex portion on the first bonding electrode and a smooth surface on the second bonding electrode, ensuring a smooth interface and preventing voids, thereby improving adhesion and reliability.

Benefits of technology

The electroless plating process results in a semiconductor device with enhanced long-term reliability by preventing local corrosion and void formation, ensuring improved solderability and extended operating life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584620000001
    Figure 0007584620000001
  • Figure 0007584620000002
    Figure 0007584620000002
  • Figure 0007584620000003
    Figure 0007584620000003
Patent Text Reader

Abstract

A semiconductor element according to the present invention comprises: a semiconductor chip (1); an electrode (4) provided on at least one main surface of the semiconductor chip (1); a first bonding electrode (6) provided on the electrode (4); and a second bonding electrode (7) provided on the first bonding electrode (6), wherein the electrode (4) has a raised part on a surface thereof which is located on the first bonding electrode (6) side, a surface of the first bonding electrode (6) which is located on the second bonding electrode (7) side is smooth, and a surface of the second bonding electrode (7) which is located on the opposite side from the first bonding electrode (6) is smooth.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a semiconductor device, a power conversion device, and a method for manufacturing a semiconductor device. [Background technology]

[0002] When mounting a front-back conductive semiconductor element (especially a power element for power conversion such as an IGBT or a diode) on a semiconductor substrate, the back side of the semiconductor element is joined to the semiconductor substrate by soldering, and on the front side of the semiconductor element, an electrode (front electrode) made of an aluminum alloy or the like is joined to a wiring circuit or the like by wire bonding of aluminum or the like.

[0003] However, currently, in order to shorten manufacturing time and reduce material costs, a mounting method in which electrodes made of aluminum alloy, copper, etc. are directly soldered to the front side of the semiconductor element, or a copper wire bond method is used. In order to relieve stress during soldering and prevent electrode wear, there is a demand for the ability to form a bonding electrode layer made of nickel, gold, copper, etc., thicker than about 1 μm on the electrode (front electrode) made of aluminum alloy, etc. on the surface of the semiconductor element.

[0004] However, when forming a bonding electrode layer on the front side of a semiconductor element by a vacuum film-forming method such as deposition or sputtering, it is difficult to form a patterned film only on the electrode of an aluminum alloy or the like. In addition, the thickness of the film formed by the vacuum film-forming method is usually about 1.0 μm or less, and if an attempt is made to increase the thickness of the bonding electrode layer, the film formation takes an order of magnitude longer than the plating method, resulting in increased manufacturing costs. For this reason, electroless plating, which can selectively form a bonding electrode layer on an electrode made of an aluminum alloy or the like and can form a bonding electrode layer thicker than about 1.0 μm at low cost and high speed, is attracting attention.

[0005] In Patent Document 1 (JP Patent Publication No. 2005-19829), a contact hole made of an interlayer insulating film is intentionally provided between a semiconductor substrate and an electrode, and the shape of the contact hole is utilized to uniformly form a recess of the same shape as the contact hole on the surface of the electrode. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-19829 A Summary of the Invention [Problem to be solved by the invention]

[0007] In addition, when unevenness is formed on the surface of an electrode using the method described in Patent Document 1, unevenness occurs on the surfaces of the nickel plating layer and the gold plating layer, which results in voids being generated when the nickel plating layer and the gold plating layer are joined, reducing the adhesion of the joint, making it difficult to improve the long-term reliability of the semiconductor element.

[0008] The present disclosure has been made to solve the above problems, and has an object to improve the long-term reliability of semiconductor elements. [Means for solving the problem]

[0009] A semiconductor chip; an electrode provided on at least one main surface of the semiconductor chip; a first bonding electrode provided on the electrode; A second bonding electrode provided on the first bonding electrode, The electrode has a convex portion on a surface facing the first bonding electrode, The first bonding electrode has a smooth surface on the side of the second bonding electrode, A semiconductor element, wherein the second bonding electrode has a smooth surface opposite to the first bonding electrode. Effect of the Invention

[0010] According to the present disclosure, it is possible to improve the long-term reliability of semiconductor elements. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a semiconductor device according to first and second embodiments. [Diagram 2] FIG. 2 is a flow diagram of a method for manufacturing a semiconductor device according to the first and second embodiments. [Diagram 3] FIG. 3 is a schematic cross-sectional view for illustrating a method for manufacturing the semiconductor device in the first and second embodiments. [Figure 4] FIG. 4 is a schematic cross-sectional view for illustrating a method for manufacturing the semiconductor device in the first and second embodiments. [Diagram 5] FIG. 5 is a schematic cross-sectional view for illustrating a method for manufacturing the semiconductor device in the first and second embodiments. [Figure 6] FIG. 6 is a flow diagram of electroless plating in the first and third embodiments. [Figure 7] FIG. 7 is a schematic cross-sectional view for illustrating a method for manufacturing the semiconductor element in the first embodiment. [Figure 8] FIG. 8 is a schematic cross-sectional view of a conventional semiconductor device according to the first and second embodiments. [Figure 9] FIG. 9 is a flow diagram of electroless plating in the second and fourth embodiments. [Figure 10] FIG. 10 is a schematic cross-sectional view for illustrating a method for manufacturing a semiconductor device in the second embodiment. [Figure 11] FIG. 11 is a schematic cross-sectional view of a semiconductor device according to the third and fourth embodiments. [Figure 12] FIG. 12 is a flow diagram of a method for manufacturing a semiconductor device in the third and fourth embodiments. [Figure 13] FIG. 13 is a schematic cross-sectional view of a conventional semiconductor device according to the third and fourth embodiments. [Figure 14] FIG. 14 is a schematic cross-sectional view of a semiconductor device according to the fifth embodiment. [Figure 15] FIG. 15 is a flow diagram of electroless plating in the fifth embodiment. [Figure 16] FIG. 16 is a schematic cross-sectional view of a conventional semiconductor device according to the fifth embodiment. [Figure 17] FIG. 17 is a block diagram showing a configuration of a power conversion system according to the sixth embodiment. As shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present disclosure will be described. In the drawings, dimensional relationships such as length, width, thickness, and depth are appropriately changed for clarity and simplification of the drawings, and do not represent actual dimensional relationships.

[0013] Embodiment 1 <Semiconductor element> Referring to FIG. 1, the semiconductor device of the present embodiment is A semiconductor chip 1, An electrode 4 (electrode layer) provided as a wiring layer on the front side (one main surface) of the semiconductor chip 1; A first bonding electrode 6 provided on the electrode 4 (on the surface opposite to the semiconductor chip 1); and a second bonding electrode 7 provided on the first bonding electrode 6 (on the surface opposite to the semiconductor chip 1).

[0014] The electrode 4 has a convex portion on the surface facing the first bonding electrode 6, The surface of the first bonding electrode 6 facing the second bonding electrode 7 is smooth, The surface of the second bonding electrode 7 opposite to the first bonding electrode 6 is smooth.

[0015] In FIG. 1, a back electrode 5 (back electrode layer) is provided on the back side of the semiconductor chip 1 (the surface opposite to the electrode 4).

[0016] The height of the convex portion of the electrode 4 is preferably 1.0 μm or more. The height of the convex portion of the electrode 4 can be calculated by the following method. That is, an arbitrary cross section obtained by irradiating a gallium ion beam using a focused ion beam device (FIB device) is observed at 5000 times magnification using a scanning electron microscope (SEM). The heights of 10 arbitrary points of the observed convex portions are measured, and the average value can be regarded as the height of the convex portion of the electrode 4.

[0017] The surface of the first bonding electrode 6 on the second bonding electrode 7 side and the surface of the second bonding electrode 7 on the opposite side to the first bonding electrode 6 are substantially smooth, but may not be completely smooth and may have some height difference. In this case, the height difference is preferably 0.5 μm or less.

[0018] The height difference can be calculated by the following method. That is, an arbitrary cross section obtained by irradiating a gallium ion beam using a focused ion beam device (FIB device) is observed at 5000 times magnification using a scanning electron microscope (SEM). Within a horizontal range of 20 μm on the observed surface, an arbitrarily determined measurement point is set as a reference point, and the difference between the highest point and the lowest point is measured, and the average value can be regarded as the height difference between the surface of the first bonding electrode 6 on the second bonding electrode 7 side and the surface of the second bonding electrode 7 on the opposite side to the first bonding electrode 6.

[0019] A gate oxide film 2 may be provided between the semiconductor chip 1 and the electrode 4, and a gate electrode 3 may be provided in the gate oxide film 2. In this case, the protruding portion of the electrode 4 is located above the gate oxide film 2.

[0020] The semiconductor chip 1 is made of, for example, silicon carbide. However, the material of the semiconductor chip 1 is not limited to silicon carbide, and may be silicon, gallium arsenide, gallium nitride, etc., or may be a front-back conductive semiconductor element such as an IGBT or a diode. Even in such a case, it is expected that the same effect can be obtained. The size of the semiconductor chip 1 is, for example, about 7 mm x 14 mm.

[0021] The electrode 4 preferably contains aluminum or an aluminum alloy. Examples of the aluminum alloy include aluminum alloys containing aluminum and silicon, silicon, copper, or the like.

[0022] The first bonding electrode 6 preferably contains nickel, nickel phosphorus, or nickel boron. An example of the first bonding electrode 6 is an electroless nickel plating layer.

[0023] The second bonding electrode 7 preferably contains gold or palladium. Examples of the second bonding electrode 7 include an electroless gold plating layer and an electroless palladium plating layer.

[0024] However, the first bonding electrode 6 and the second bonding electrode 7 are not limited to a nickel plating layer, a gold plating layer, and a palladium plating layer, and may be any plating layer that enables bonding of the electrode 4, the first bonding electrode 6, and the second bonding electrode 7. It is expected that the same effect can be obtained even if, for example, an electrolytic copper plating layer is used as such a plating layer.

[0025] The first bonding electrode 6 and the second bonding electrode 7 are preferably formed by electroless plating.

[0026] The gate oxide film 2 is made of an insulating material such as silicon oxide. The gate electrode 3 is made of a conductive material such as polysilicon.

[0027] The back electrode 5 is composed of multiple metal layers. Since the back electrode 5 may be used for bonding, it is preferable to use an electrode formed by plating nickel or gold, which has excellent bonding properties, on an electrode made of nickel or a nickel alloy containing silicon, copper, etc., as the back electrode 5.

[0028] 1 is a front-back conductive type semiconductor element having a front electrode (electrode 4) and a back electrode 5. That is, the electrode 4 is the front electrode of the front-back conductive type semiconductor element.

[0029] In this embodiment, the electrode 4 has a convex portion on the surface facing the first bonding electrode 6, the surface of the first bonding electrode 6 facing the second bonding electrode 7 is smooth, and the surface of the second bonding electrode 7 opposite to the first bonding electrode 6 is smooth. This suppresses the generation of voids when bonding the first bonding electrode 6 and the second bonding electrode 7, improving the adhesion of the bonded portion. Therefore, the long-term reliability of the semiconductor element can be improved.

[0030] <Method of manufacturing semiconductor device> The method for manufacturing a semiconductor device according to the present embodiment includes the steps of: a first step (electrode formation step) of forming electrodes on at least one main surface of the semiconductor chip; A second step (first joining electrode forming step) of forming a first joining electrode on the electrode; and a third step (second bonding electrode forming step) of forming a second bonding electrode on the first bonding electrode.

[0031] In the first step, a convex portion is formed on the surface of the electrode on the side of the first bonding electrode. In the second step, the surface of the first joining electrode on the side of the second joining electrode is formed to be smooth.

[0032] In the third step, the surface of the second bonding electrode opposite to the first bonding electrode is formed to be smooth.

[0033] Hereinafter, an example of a method for manufacturing a semiconductor device according to this embodiment will be described with reference to FIG.

[0034] In the manufacturing method of a semiconductor element of this embodiment, the steps of forming an electrode 4 on a semiconductor chip 1 (first step), forming a back electrode 5, masking the back electrode 5, electroless plating (second and third steps), and removing the mask are mainly carried out in this order.

[0035] 3 to 5 are schematic cross-sectional views showing a manufacturing process flow of the semiconductor element shown in Fig. 1. Fig. 3 shows a cross-sectional structure of the semiconductor element before the electrode 4, the back electrode 5, the first bonding electrode 6, and the second bonding electrode 7 are formed in the first embodiment.

[0036] 1 will be described below with reference to Figures 2 to 5. Note that, in terms of manufacturing efficiency, it is preferable that all of the steps in the first embodiment are performed in wafer form.

[0037] (Formation of gate oxide film and gate electrode) 3, when the semiconductor element of the present embodiment includes a gate oxide film 2 and a gate electrode 3, the gate oxide film 2 containing the gate electrode 3 is formed by first depositing silicon oxide, which is an insulating material, as the gate oxide film 2 by a deposition method such as thermal oxidation or chemical vapor deposition, and then patterning the gate oxide film 2 by photolithography or etching, for example, to form a lower portion of the gate oxide film 2 (the semiconductor chip 1 side of the gate electrode 3 in FIG. 3). Next, polysilicon, which is a conductive material, is deposited as the gate electrode 3 by the above-mentioned method, and then patterned by the above-mentioned method to form the gate electrode 3. Then, silicon oxide is deposited by the above-mentioned method so as to cover the gate electrode 3, and then patterned by the above-mentioned method to form the gate oxide film 2.

[0038] The thickness of the gate oxide film 2 enclosing the gate electrode 3 is preferably, for example, not less than 1.0 μm and not more than 3.0 μm.

[0039] (1st step: electrode formation step) 4, in the electrode formation step (first step), for example, an aluminum alloy having low electrical resistance is patterned by sputtering, which is an easy process to control, in order to form an electrode with high adhesion on the semiconductor chip 1. When the semiconductor element of this embodiment includes a gate oxide film 2 and a gate electrode 3, the electrode 4 is formed while maintaining the unevenness caused by the gate oxide film 2 and the gate electrode 3, so that a convex portion is formed on the upper surface of the electrode 4. Depending on the application, a titanium compound such as titanium or titanium nitride may be formed as a barrier metal between the semiconductor chip 1 and the aluminum alloy, and between the gate oxide film 2 and the aluminum alloy.

[0040] The thickness of the electrode 4 is preferably, for example, 0.5 μm or more and 5.0 μm or less, and the height of the convex portion of the electrode 4 is preferably 1.0 μm or more. When the semiconductor chip 1 is made of silicon carbide, in order to further increase the adhesion with the semiconductor chip 1, for example, about 1 mass % of silicon, about 1 mass % of silicon, about 0.5 mass % of copper, or the like may be added to the electrode 4 in addition to aluminum, and the concentration thereof is preferably constant in the electrode.

[0041] (Back electrode formation) 5, in the process of forming the back electrode, in order to form the back electrode 5 composed of a plurality of metal layers on the surface of the semiconductor chip 1 opposite to the surface on which the electrode 4 is formed, for example, nickel is patterned by sputtering, which is easy to control the process, and then gold is patterned by sputtering, which is easy to control the process. Depending on the application, a barrier metal such as a titanium alloy or a nickel alloy may be formed between the semiconductor chip 1 and the nickel.

[0042] The thickness of the back electrode 5 is, for example, preferably 0.3 μm or more and 5.0 μm or less for the nickel layer, and preferably 0.01 μm or more and 0.2 μm or less for the gold layer.

[0043] (Masking the back electrode) Next, the rear electrode is masked to prevent the rear electrode 5 from being damaged during the subsequent film formation process of the first bonding electrode 6 and the second bonding electrode 7. This is done by attaching a film coated with an adhesive that can be peeled off by irradiating it with ultraviolet light.

[0044] (Electroless plating) Next, an electroless plating process is performed, which will be described separately below with reference to FIG.

[0045] (Removing the masking) Finally, the masking tape attached to the back electrode surface of the wafer is peeled off. Specifically, for example, a masking tape that peels off when irradiated with ultraviolet light is used, and the back surface of the wafer that has been subjected to the electroless plating process is irradiated with ultraviolet light to peel off the masking tape.

[0046] (Electroless plating process) The electroless plating process will now be described in detail.

[0047] 6, in the process of forming the first bonding electrode 6 and the second bonding electrode 7 on the electrode 4 on the wafer by electroless plating, degreasing, pickling, first zincate, zincate stripping, second zincate, electroless nickel plating, and electroless gold plating are performed in this order. At this time, it is necessary to secure a sufficient water rinsing time between each step and to take care not to carry over the processing solution or residue from the previous step to the next step.

[0048] Next, each step will be outlined. First, degreasing is performed to remove slight organic contamination, oil and grease, oxide film, etc. remaining on the surface of the electrode 4 and to impart wettability to the surface of the electrode 4. It is preferable to saponify the oil and grease residues using an alkaline chemical solution that has a strong etching power for aluminum alloys, etc.

[0049] Next, pickling is performed. The purpose of pickling is to neutralize the surface of the electrode 4, etch the surface of the electrode 4, increase the reactivity with a zincate solution described later, and improve the adhesion of the plating.

[0050] Next, a zincate treatment is carried out. The zincate treatment is a treatment in which an oxide film (e.g., an aluminum oxide film) is removed while etching the surface of an electrode (e.g., an aluminum alloy electrode), and a coating of zinc or the like is formed on the surface of the electrode. Generally, when an aluminum alloy is immersed in an aqueous solution in which zinc has dissolved as ions, the aluminum dissolves as ions because zinc has a more noble standard oxidation-reduction potential than aluminum, and the zinc ions receive electrons on the surface of the aluminum alloy due to the electrons generated at this time, and a zinc coating is formed on the surface of the aluminum.

[0051] After this, the zinc-coated aluminum alloy is immersed in nitric acid to dissolve the zinc. Then, the aluminum alloy is immersed again in a zincate solution to remove the aluminum oxide film and to uniformly coat the zinc. This operation makes the aluminum surface smooth. The more times the zincate treatment is performed, the more uniform the aluminum surface becomes and the better the plating layer will be, so the zincate treatment is performed at least two times, and preferably three times. If a uniform zinc coating is formed on the surface of the electrode 4 by this zincate treatment, a sound plating layer can be attached in the subsequent electroless plating treatment.

[0052] Next, electroless nickel plating will be described as an example of the second step (first bonding electrode forming step).

[0053] When an aluminum alloy coated with zinc is immersed in an electroless nickel plating solution, zinc and nickel are substituted for each other based on the difference in standard redox potential, and nickel is deposited on the aluminum alloy. After that, nickel is autocatalytically deposited on the nickel due to the action of the reducing agent contained in the plating solution.

[0054] During this autocatalytic deposition, the components of the reducing agent are incorporated into the plating layer, so the electroless nickel plating layer becomes an alloy. Generally, hypophosphorous acid is used as the reducing agent, and the phosphorus is incorporated into the plating layer, so the electroless nickel plating layer contains phosphorus.

[0055] At this time, in order to improve the degree of formation of unevenness (filling property) of the aluminum alloy, the initial nickel deposition rate is intentionally reduced. As shown in FIG. 7, when the nickel deposition rate is reduced, the reactivity at the convex part of the electrode 4 decreases due to the action of the stabilizer and complexing agent contained in the plating solution, but the electroless nickel plating layer is formed smoothly because the accelerator is concentrated in the concave part of the electrode 4 and the reactivity is higher than that of the convex part. In order to reduce the nickel deposition rate, it is effective to lower the temperature of the nickel plating bath or to suppress the supply of the nickel source and the reducing agent to the reaction surface. In this case, the nickel deposition rate is preferably 4.0 μm / hr or more and 10 μm / hr or less, and more preferably 6.0 μm / hr or more and 8.0 μm / hr or less. As described later, the electroless nickel plating layer is carried out at the speed until it becomes smooth.

[0056] On the other hand, if the nickel deposition rate is reduced by the above-mentioned method, not only will the productivity decrease, but the supply of nickel to the reaction surface will be biased, resulting in unevenness in the film thickness within the wafer surface. Therefore, after removing the unevenness of the electroless nickel plating layer by the initial deposition of nickel, the nickel deposition rate is increased by increasing the temperature of the nickel plating bath or promoting the diffusion of the nickel source and reducing agent to the reaction surface, thereby depositing a smooth electroless nickel plating layer on the aluminum alloy having uneven parts. In this case, the nickel deposition rate is preferably 10 μm / hr or more and 15 μm / hr or less, more preferably 11 μm / hr or more and 13 μm / hr or less.

[0057] The thickness of the electroless nickel plating layer is preferably, for example, 1.0 μm to 7.0 μm, and if there is a height difference on the surface of the electroless nickel plating layer, it is preferably 0.5 μm or less.

[0058] Then, finally, the third step (second bonding electrode forming step) is carried out. As an example of the third step, electroless gold plating will be described.

[0059] The electroless gold plating used here is generally of the substitution type, where gold plating is deposited through the substitution of nickel with gold. Substitution type electroless gold plating is applied on top of an electroless nickel plating layer, and utilizes the action of the complexing agent contained in the plating solution, which causes nickel to substitute for gold. Because it is a substitution type, the reaction stops once the nickel surface is covered with gold, making it difficult to make the plating layer thick, and it is generally often around 0.05 μm thick.

[0060] In addition, if the surface of the electroless nickel plating layer is uneven, electroless gold plating will cause nickel to corrode locally in the recesses and become phosphorus-rich, which will reduce the bonding strength and bonding reliability. Therefore, it is preferable that the electroless nickel plating layer as the base is smooth.

[0061] Using the process flow described above, a semiconductor element can be obtained by depositing a smooth first bonding electrode 6 (nickel plating layer) and a smooth second bonding electrode 7 (gold plating layer) on the surface of an electrode 4 having a convex portion by electroless plating.

[0062] The obtained semiconductor element has less localized corrosion than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 8. Also, the obtained semiconductor element has less voids in the recesses during soldering than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 8. Therefore, the semiconductor element of this embodiment is expected to have an effect of extending the operating life even in a power cycle test when incorporated into a power module.

[0063] As described above, in this embodiment, even if the electrode 4 has unevenness, the surfaces of the first joining electrode 6 and the second joining electrode 7 are formed smoothly, thereby suppressing local nickel corrosion and the occurrence of voids, thereby improving solderability and ensuring the long-term reliability of the semiconductor element.

[0064] Embodiment 2 In the second embodiment, CMP (Chemical Mechanical Polishing) is additionally performed in the electroless plating process of the manufacturing method shown in the first embodiment. The components of the semiconductor element of the present embodiment are explained in the first embodiment, so the overlapping explanation will be omitted.

[0065] The electroless nickel plating and CMP will be described below, but since the other steps are the same as those in the first embodiment, duplicated descriptions will be omitted.

[0066] 9 is a flow diagram of the first joining electrode forming step (second step) in the second embodiment. In the second embodiment, the procedure is the same as that in the first embodiment up to the second zincate treatment, but thereafter, electroless nickel plating and CMP are performed in this order. First, the electroless nickel plating will be described.

[0067] When an aluminum alloy coated with zinc is immersed in an electroless nickel plating solution, zinc and nickel are substituted for each other based on the difference in standard redox potential, and nickel is deposited on the aluminum alloy. After that, nickel is autocatalytically deposited on the nickel due to the action of the reducing agent contained in the plating solution.

[0068] During this autocatalytic deposition, the components of the reducing agent are incorporated into the plating layer, so the electroless nickel plating layer becomes an alloy. Generally, hypophosphorous acid is used as the reducing agent, and the phosphorus is incorporated into the plating layer, so the electroless nickel plating layer contains phosphorus.

[0069] At this time, the nickel plating layer is affected by the uneven surface of the aluminum alloy, so the upper surface of the electroless nickel plating layer becomes uneven, as shown in Fig. 10. Considering that the electroless nickel plating layer will be reduced by 1.0 µm by CMP in the following process, it is preferable to form the electroless nickel plating layer thicker than the final desired electroless nickel plating layer.

[0070] Next, CMP is performed. CMP means a process for flattening unevenness by improving mechanical polishing performance by the surface chemical action of the slurry. When CMP is performed on the electroless nickel plating layer, the slurry collides with the steps of the uneven surface, generating thermal energy, and thus promoting chemical reactions at the steps. Therefore, the convex parts are selectively etched to eliminate the steps, and the electroless nickel plating layer is flattened. In this embodiment, a smooth surface shape can be obtained by polishing the electroless nickel plating layer of the convex parts by 1.0 μm by CMP. Then, as in the first embodiment, a smooth electroless gold plating layer is formed by electroless gold plating. Note that, as in the first embodiment, the second joining electrode being an electroless gold plating layer is just an example, and the second joining electrode may be, for example, an electroless palladium plating layer.

[0071] According to the process flow described above, a semiconductor element can be obtained in which a smooth first bonding electrode (nickel plating layer) and a smooth second bonding electrode (gold plating layer) are deposited by electroless plating.

[0072] The obtained semiconductor element has less localized corrosion than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 8. Also, the obtained semiconductor element has less voids in the recesses during soldering than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 8. Therefore, the semiconductor element of this embodiment is expected to have an effect of extending the operating life even in a power cycle test when incorporated into a power module.

[0073] As described above, in this embodiment, even if the electrodes are uneven, the surfaces of the first joining electrode 6 and the second joining electrode 7 are formed smoothly, thereby suppressing local nickel corrosion and the occurrence of voids, thereby improving solderability and ensuring the long-term reliability of the semiconductor element.

[0074] Embodiment 3 11, in the semiconductor element of the present embodiment, a first bonding electrode 61 and a second bonding electrode 71 are also formed on the back electrode 5 (opposite side of the semiconductor chip 1) in the same manner as the electrode 4 (front electrode) in the first embodiment. The other components have been described in the first embodiment, so duplicated description will be omitted.

[0075] In this embodiment, the back electrode 5 is made of, for example, aluminum (the same material as the electrode 4) or an aluminum alloy containing silicon, silicon, copper, or the like, so that it can be plated by electroless plating.

[0076] 12, in the method for manufacturing a semiconductor element according to the present embodiment, mainly, formation of an electrode 4 on a semiconductor chip 1, formation of a back electrode 5, and electroless plating are carried out in this order.

[0077] In this embodiment, by performing the electroless nickel plating shown in the first embodiment, a smooth electroless nickel plating layer is simultaneously deposited on the electrode 4 having the uneven portion and the smooth back electrode 5. Then, by performing electroless gold plating, a smooth electroless gold plating layer is simultaneously deposited on the electroless nickel plating layer on the electrode 4 and the electroless nickel plating layer on the back electrode 5. As in the first embodiment, the second joining electrode being an electroless gold plating layer is just an example, and the second joining electrode may be, for example, an electroless palladium plating layer.

[0078] According to the process flow described above, a semiconductor element in which the first bonding electrodes 6, 61 and the second bonding electrodes 7, 71 are formed on both the front and back surfaces of the semiconductor chip 1 by electroless plating can be obtained.

[0079] The obtained semiconductor element has less localized corrosion than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 13. Also, the obtained semiconductor element has less voids in the recesses during soldering than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 13. Therefore, the semiconductor element of this embodiment is expected to have an effect of extending the operating life even in a power cycle test when incorporated into a power module.

[0080] As described above, in this embodiment, even if the electrodes are uneven, the surfaces of the first joining electrode and the second joining electrode are formed smoothly, thereby suppressing localized nickel corrosion and the occurrence of voids, thereby improving solderability and ensuring the long-term reliability of the semiconductor element.

[0081] Embodiment 4 In the fourth embodiment, a semiconductor element having the configuration shown in the third embodiment is formed, but the first bonding electrode 6 is formed on the electrode 4 by the manufacturing method shown in the second embodiment, and the first bonding electrode 61 is formed on the back electrode 5 by the manufacturing method shown in the second embodiment, except that CMP is not performed. The other components are described in the first and third embodiments, so duplicated descriptions will be omitted.

[0082] In this embodiment, the back electrode 5 is made of, for example, aluminum (the same material as the electrode 4) or an aluminum alloy containing silicon, silicon, copper, or the like, so that it can be plated by electroless plating.

[0083] 12, in the method for manufacturing a semiconductor element according to the present embodiment, mainly, formation of an electrode 4 on a semiconductor chip 1, formation of a back electrode 5, and electroless plating are carried out in this order.

[0084] In this embodiment, a smooth electroless nickel plating layer is deposited on the electrode 4 having the uneven portion by performing the electroless nickel plating and CMP shown in the second embodiment, and a smooth electroless nickel plating layer is deposited on the smooth back electrode 5 by performing electroless nickel plating without performing the CMP shown in the second embodiment. Then, a smooth electroless gold plating layer is simultaneously deposited on the electroless nickel plating layer on the electrode 4 and the electroless nickel plating layer on the back electrode 5 by performing electroless gold plating. As in the first embodiment, the second joining electrode being an electroless gold plating layer is just an example, and the second joining electrode may be, for example, an electroless palladium plating layer.

[0085] According to the process flow described above, a semiconductor element in which the first bonding electrodes 6, 61 and the second bonding electrodes 7, 71 are formed on both the front and back surfaces of the semiconductor chip 1 by electroless plating can be obtained.

[0086] The obtained semiconductor element has less localized corrosion than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 13. Also, the obtained semiconductor element has less voids in the recesses during soldering than when the electroless nickel plating layer and the electroless gold plating layer have uneven surfaces as shown in Fig. 13. Therefore, the semiconductor element of this embodiment is expected to have an effect of extending the operating life even in a power cycle test when incorporated into a power module.

[0087] As described above, in this embodiment, even if the electrodes are uneven, the surfaces of the first joining electrode and the second joining electrode are formed smoothly, thereby suppressing localized nickel corrosion and the occurrence of voids, thereby improving solderability and ensuring the long-term reliability of the semiconductor element.

[0088] Embodiment 5. In the fifth embodiment, the second bonding electrode 7 is made of multiple layers in any of the semiconductor elements according to the first to fourth embodiments. The other components are the same as those described in the first to fourth embodiments, and therefore will not be described again.

[0089] 14, in the semiconductor element of the present embodiment, the second bonding electrode has a two-layer structure consisting of a first layer 7a and a second layer 7b. The first layer 7a preferably contains palladium, palladium phosphorus, or a palladium alloy. An example of the first layer 7a is an electroless palladium plating layer. The second layer 7b preferably contains gold. An example of the second layer 7b is an electroless gold plating layer.

[0090] However, the first layer 7a and the second layer 7b are not limited to a palladium plating layer and a gold plating layer, and may be any plating layer that enables bonding of the first bonding electrode 6, the first layer 7a, and the second layer 7b. It is expected that the same effect can be obtained even if, for example, an electrolytic copper plating layer is used as such a plating layer.

[0091] The first layer 7a and the second layer 7b are preferably formed by electroless plating.

[0092] 15 is a flow diagram of electroless plating in this embodiment. In this embodiment, the procedure is the same as in embodiment 1 up to electroless nickel plating, but then electroless palladium plating and electroless gold plating are performed in this order. Below, electroless palladium plating and electroless gold plating will be explained, but since the other steps have been explained in embodiments 1 to 4, overlapping explanations will be omitted.

[0093] The electroless palladium plating used here is generally of the substitution type, in which nickel and palladium are substituted to deposit palladium. Formic acid or hypophosphorous acid is used as the reducing agent. The thickness of the first layer 7a is preferably, for example, 0.1 μm or more and 1.0 μm or less.

[0094] By providing this electroless palladium plating layer between the electroless nickel plating layer and the electroless gold plating layer, it is possible to suppress nickel from diffusing into the surface of the gold plating layer due to heat.

[0095] Next, electroless gold plating is carried out. As described above, electroless gold plating is generally of the substitution type, but may be of the substitution reduction type, or the substitution and reduction types may be carried out successively.

[0096] On the other hand, regardless of the method used for electroless gold plating, the electroless gold plating layer locally corrodes the electroless nickel plating layer through the electroless palladium plating layer. If the surface of the electroless nickel plating layer is uneven, the presence of the electroless palladium plating layer will promote local corrosion of the recesses due to galvanic action. Therefore, if there is an electroless palladium plating layer, it is preferable that the underlying electroless nickel plating layer is smooth.

[0097] Using the process flow described above, a semiconductor element can be obtained by depositing a smooth first bonding electrode 6 (nickel plating layer) and a smooth second bonding electrode 7 made up of a first layer 7a (palladium plating layer) and a second layer 7b (gold plating layer) on the surface of an electrode 4 having a convex portion by electroless plating.

[0098] The configuration of the second bonding electrode 7 is not limited to two layers, and may be three or more layers. In this case, in the second bonding electrode 7, the layer in contact with the first bonding electrode 6, i.e., the bottom layer, preferably contains palladium, palladium phosphorus, or a palladium alloy, and the layer farthest from the first bonding electrode 6, i.e., the top layer, preferably contains gold. For example, when the second bonding electrode 7 is made of three layers, the bottom layer may be an electroless palladium plating layer, the top layer may be a reduction-type electroless gold plating layer, and the layer between the top layer and the bottom layer, i.e., the intermediate layer, may be a substitution-type electroless gold plating layer.

[0099] The obtained semiconductor element has less localized corrosion than when the electroless nickel plating layer, the electroless palladium plating layer, and the electroless gold plating layer have uneven surfaces as shown in FIG. 16. In addition, the smoothness of the electroless palladium plating layer prevents nickel from diffusing into the surface of the electroless gold plating layer, improving the bonding strength with the solder. Furthermore, the obtained semiconductor element has less voids in the recesses during solder bonding than when the electroless nickel plating layer, the electroless palladium plating layer, and the electroless gold plating layer have uneven surfaces as shown in FIG. 16. Therefore, the semiconductor element of this embodiment is expected to have a longer operating life even in a power cycle test when incorporated into a power module.

[0100] As described above, in the present embodiment, even if the electrodes are uneven, the surfaces of the first joining electrode and the first and second layers which are the second joining electrode are formed smoothly, thereby suppressing localized nickel corrosion and the occurrence of voids, thereby improving solderability and ensuring the long-term reliability of the semiconductor element.

[0101] Embodiment 6 In this embodiment, any one of the semiconductor elements according to the above-mentioned embodiments 1 to 5 is applied to a power conversion device. Although the present disclosure is not limited to a specific power conversion device, the following will describe a case where the present disclosure is applied to a three-phase inverter as embodiment 6.

[0102] FIG. 17 is a block diagram showing a configuration of a power conversion system to which the power conversion device according to this embodiment is applied.

[0103] The power conversion system shown in Fig. 17 is composed of a power source 100, a power conversion device 200, and a load 300. The power source 100 is a DC power source and supplies DC power to the power conversion device 200. The power source 100 can be composed of various things, for example, a DC system, a solar cell, or a storage battery, or it may be composed of a rectifier circuit connected to an AC system or an AC / DC converter. The power source 100 may also be composed of a DC / DC converter that converts DC power output from a DC system into a predetermined power.

[0104] The power conversion device 200 is a three-phase inverter connected between the power source 100 and the load 300, converts DC power supplied from the power source 100 into AC power, and supplies the AC power to the load 300. As shown in Fig. 17, the power conversion device 200 includes a main conversion circuit 201 that converts DC power into AC power and outputs it, and a control circuit 203 that outputs a control signal for controlling the main conversion circuit 201 to the main conversion circuit 201.

[0105] The load 300 is a three-phase motor driven by AC power supplied from the power conversion device 200. The load 300 is not limited to a specific application, but is a motor mounted on various electric devices, and is used as, for example, a motor for a hybrid vehicle, an electric vehicle, a railroad car, an elevator, or an air conditioner.

[0106] The power conversion device 200 will be described in detail below. The main conversion circuit 201 includes a switching element (not shown) and a freewheeling diode (not shown), and converts DC power supplied from the power source 100 into AC power by switching the switching element, and supplies the AC power to the load 300. There are various specific circuit configurations of the main conversion circuit 201, but the main conversion circuit 201 according to this embodiment is a two-level three-phase full bridge circuit, and can be configured with six switching elements and six freewheeling diodes connected in reverse parallel to each switching element. At least one of the switching elements and freewheeling diodes of the main conversion circuit 201 is a switching element or freewheeling diode of the semiconductor device 202 corresponding to any of the semiconductor elements of the above-mentioned embodiments 1 to 5. The six switching elements are connected in series with every two switching elements to form upper and lower arms, and each upper and lower arm forms each phase (U phase, V phase, W phase) of the full bridge circuit. The output terminals of each upper and lower arm, i.e., the three output terminals of the main conversion circuit 201, are connected to the load 300.

[0107] The main conversion circuit 201 also includes a drive circuit (not shown) for driving each switching element, but the drive circuit may be built in the semiconductor device 202, or the semiconductor device 202 may include a drive circuit separately. The drive circuit generates drive signals for driving the switching elements of the main conversion circuit 201 and supplies them to the control electrodes of the switching elements of the main conversion circuit 201. Specifically, in accordance with a control signal from a control circuit 203 (described later), the drive circuit outputs to the control electrodes of each switching element a drive signal for turning the switching element on and a drive signal for turning the switching element off. When maintaining a switching element in the on state, the drive signal is a voltage signal (on signal) equal to or higher than the threshold voltage of the switching element, and when maintaining a switching element in the off state, the drive signal is a voltage signal (off signal) equal to or lower than the threshold voltage of the switching element.

[0108] The control circuit 203 controls the switching elements of the main conversion circuit 201 so that a desired power is supplied to the load 300. Specifically, the control circuit 203 calculates the time (on time) for each switching element of the main conversion circuit 201 to be in the on state based on the power to be supplied to the load 300. For example, the main conversion circuit 201 can be controlled by PWM control that modulates the on time of the switching elements according to the voltage to be output. Then, a control command (control signal) is output to a drive circuit provided in the main conversion circuit 201 so that an on signal is output to a switching element that should be in the on state at each time point, and an off signal is output to a switching element that should be in the off state. The drive circuit outputs an on signal or an off signal as a drive signal to the control electrode of each switching element according to this control signal.

[0109] In the power conversion device 200 according to this embodiment, any one of the semiconductor elements according to the first to fifth embodiments is applied as the semiconductor device 202 constituting the main conversion circuit 201, so that the power conversion device 200 according to this embodiment can achieve improved long-term reliability.

[0110] In the present embodiment, an example of applying the present disclosure to a two-level three-phase inverter has been described, but the present disclosure is not limited thereto and can be applied to various power conversion devices. In the present embodiment, a two-level power conversion device is described, but a three-level or multi-level power conversion device may be used, and the present disclosure may be applied to a single-phase inverter when supplying power to a single-phase load. In addition, the present disclosure may be applied to a DC / DC converter or an AC / DC converter when supplying power to a DC load or the like.

[0111] Furthermore, the power conversion device to which the present disclosure is applied is not limited to the case where the above-mentioned load is an electric motor, but can also be used, for example, as a power supply device for an electric discharge machine or laser processing machine, or an induction heating cooker or a non-contact power supply system, and can also be used as a power conditioner for a solar power generation system or a power storage system, etc.

[0112] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Explanation of symbols]

[0113] 1 semiconductor chip, 2 gate oxide film, 3 gate electrode, 4 electrode, 5 back electrode, 6, 61 first junction electrode, 7, 71 second junction electrode, 7a first layer, 7b second layer, 100 power supply, 200 power conversion device, 201 main conversion circuit, 202 semiconductor device, 203 control circuit, 300 load.

Claims

1. A method for manufacturing a semiconductor device, comprising the steps of: a first step of forming an electrode on at least one main surface of a semiconductor chip; a second step of forming a first joining electrode on the electrode; and a third step of forming a second joining electrode on the first joining electrode, In the first step, a convex portion is formed on a surface of the electrode on the side of the first joining electrode, In the second step, a surface of the first joining electrode on the side of the second joining electrode is formed to be smooth; In the third step, a surface of the second joining electrode opposite to the first joining electrode is formed to be smooth, The first bonding electrode is formed by electroless nickel plating, The electroless nickel plating method includes a first electroless nickel plating process in which electroless nickel plating is performed at a nickel deposition rate of 4.0 μm / hr or more and 10 μm / hr or less, and a second electroless nickel plating process in which electroless nickel plating is performed at a nickel deposition rate of more than 10 μm / hr and 15 μm / hr or less, The electroless nickel plating is carried out until the surface on the second bonding electrode side becomes smooth.

2. the electrode comprises aluminum or an aluminum alloy; the first bonding electrode contains nickel, nickel phosphorus, or nickel boron; The method according to claim 1 , wherein the second bonding electrode includes gold.

3. The manufacturing method according to claim 1 , wherein the second bonding electrode is made of multiple layers.

4. the bottom layer of the second bonding electrode contains palladium, palladium phosphorus, or a palladium alloy; The method of claim 3 , wherein the uppermost layer of the second bonding electrode comprises gold.

5. the semiconductor element is a front-back conductive type semiconductor element having a front electrode and a back electrode, The method according to claim 1 , wherein the electrodes include the front electrode.

6. The manufacturing method according to claim 5 , wherein the first bonding electrode and the second bonding electrode are also formed on the back electrode.

7. The manufacturing method according to any one of claims 1 to 6, wherein the first bonding electrode is formed by carrying out the electroless nickel plating method and the CMP method in this order.

8. A method for manufacturing a semiconductor device, comprising the steps of: a first step of forming an electrode on at least one main surface of a semiconductor chip; a second step of forming a first joining electrode on the electrode; and a third step of forming a second joining electrode on the first joining electrode, In the first step, a convex portion is formed on a surface of the electrode on the side of the first joining electrode, In the second step, a surface of the first joining electrode on the side of the second joining electrode is formed to be smooth; In the third step, a surface of the second joining electrode opposite to the first joining electrode is formed to be smooth, The manufacturing method, wherein the first bonding electrode is formed by performing an electroless nickel plating method and a CMP method in this order.

Citation Information

Patent Citations

  • Vertical semiconductor device, and manufacturing method thereof

    JP2001177096A

  • Semiconductor device

    JP2005019829A

  • Method of manufacturing semiconductor device

    JP2010251719A

  • Semiconductor device and method of manufacturing the same