Method for manufacturing a power semiconductor device

The method of hydrogen introduction, electron beam irradiation, and laser annealing addresses damage and interface issues in forming wide buffer layers for IGBTs and diodes, enhancing device performance by reducing damage and manufacturing time.

JP7584713B1Active Publication Date: 2024-11-15MITSUBISHI ELECTRIC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024539066
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-11-15
Estimated Expiration
2044-03-12

Smart Images

  • Figure 0007584713000001
    Figure 0007584713000001
  • Figure 0007584713000002
    Figure 0007584713000002
  • Figure 0007584713000003
    Figure 0007584713000003
Patent Text Reader

Abstract

The present disclosure aims to form a wide buffer layer with little damage accumulation and no interface. The method for manufacturing a power semiconductor device according to the present disclosure includes introducing hydrogen into a region of a silicon wafer (1) having a first main surface (S1) and a second main surface (S2) opposite to the first main surface (S1), including at least a first region that is a region from the second main surface (S2) to a predetermined depth, irradiating the silicon wafer (1) with an electron beam to penetrate the silicon wafer (1) to form defects in the first region and a second region between the first region and the first main surface, heat-treating the silicon wafer (1) to react the hydrogen with the defects to form donors, and performing laser annealing from the first main surface (S1) or the second main surface (S2) of the silicon wafer (1) to inactivate the donors in the second region and turn the first region into a buffer layer (11).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a power semiconductor device. [Background technology]

[0002] A vertical IGBT (Insulated Gate Bipolar Transistor) is composed of a region including, from the front side, a MOS (Metal Oxide Semiconductor) structure, an n-type drift layer, an n-type buffer layer, and a p-type collector layer. A vertical diode is composed of, from the front side, a p-type anode, an n-type drift layer, an n-type buffer layer, and an n-type cathode layer. Patent Document 1 discloses an IGBT having a vertical structure. Thinning the IGBT and diode is effective in reducing losses, but it also has the adverse effect of reducing the margin for voltage snap-off. As a countermeasure, a wide n-type buffer layer is adopted.

[0003] Patent Document 1 describes a method for manufacturing a buffer layer using proton (hydrogen ion) irradiation or implantation (hereinafter, both will be referred to as irradiation) and annealing. According to this method, the width of the buffer layer that can be made by one proton irradiation is limited. In order to form a buffer layer of the desired thickness on the back surface of the device, multiple irradiations with different proton irradiation ranges are required.

[0004] Patent documents 2 and 3 describe a method for producing a buffer layer without proton irradiation. Patent document 2 describes a method for bonding wafers with different concentrations. Patent document 3 describes a method for producing a buffer layer by multi-stage epitaxial growth. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6090329 [Patent Document 2] Patent No. 2878488 [Patent Document 3] Patent No. 3113156 Summary of the Invention [Problem to be solved by the invention]

[0006] When forming a wide n-type buffer layer in an IGBT or diode, the methods described in Patent Documents 1 to 3 have the following problems. In the multi-stage proton irradiation described in Patent Document 1, the number of irradiations is increased, so that excess damage accumulates in the silicon wafer. There is also a problem that an interface occurs between the regions where donors are formed by each irradiation. With the bonding described in Patent Document 2, there is a problem that a bonding interface inevitably occurs. The multi-stage epitaxial growth described in Patent Document 3 is vapor phase growth, so it essentially takes a long time to manufacture.

[0007] The present disclosure has been made to solve the above problems, and has an object to form a wide buffer layer with little accumulation of damage and without an interface. [Means for solving the problem]

[0008] The method for manufacturing a power semiconductor device disclosed herein includes: introducing hydrogen into a region of a silicon wafer having a first main surface and a second main surface opposite the first main surface, the region including at least a first region being a region from the second main surface to a predetermined depth; irradiating the silicon wafer with a penetrating electron beam to form defects in the first region and a second region between the first region and the first main surface; heat-treating the silicon wafer to react the hydrogen with the defects to form donors; and performing laser annealing from the first main surface or the second main surface of the silicon wafer to inactivate the donors in the second region and turn the first region into a buffer layer. Effect of the Invention

[0009] According to the manufacturing method of the power semiconductor device of the present disclosure, the introduction of hydrogen, the penetrating irradiation of the electron beam, the heat treatment, and the laser annealing leave the donors only in the first region, and the first region can be formed as a buffer layer. Therefore, a wide buffer layer can be formed with little accumulation of damage and no interface. Objects, features, aspects, and advantages of the present disclosure will become more apparent from the following detailed description and the accompanying drawings. [Brief description of the drawings]

[0010] [Figure 1] 4 is a flowchart showing a method for manufacturing the power semiconductor device according to the first embodiment. [Diagram 2] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Diagram 3] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 4] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Diagram 5] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 6] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 7] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 8] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 9] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 10] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 11] 2A to 2C are cross-sectional views showing a manufacturing process of the power semiconductor device according to the first embodiment. [Figure 12] FIG. 13 is a graph showing the temperature dependence of the areal density of donors. [Figure 13] 5 is a diagram showing a hydrogen concentration distribution in the power semiconductor device according to the first embodiment. FIG. [Figure 14] It is a flowchart showing a method for manufacturing a power semiconductor device according to Embodiment 2. [Figure 15] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 16] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 17] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 18] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 19] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 20] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 2. [Figure 21] It is a diagram showing the hydrogen concentration distribution in the power semiconductor device according to Embodiment 2. [Figure 22] It is a flowchart showing a method for manufacturing a power semiconductor device according to Embodiment 3. [Figure 23] It is a cross-sectional view showing the manufacturing process of the power semiconductor device according to Embodiment 3.

Embodiments for Carrying Out the Invention

[0011] <A. Prerequisite Technology> First, as a prerequisite technology of the technology of the present disclosure, a method for forming a buffer layer by proton irradiation will be described.

[0012] Donors that contribute to the formation of the buffer layer are formed by recombining point defects and hydrogen present in the silicon wafer. Point defects are local disruptions in the crystal lattice and are classified into vacancy type and interstitial silicon type. Generally, when point defects and hydrogen recombine, the dangling bonds of the point defects are shielded by hydrogen and do not show mid-band levels. However, if the shielding effect of the dangling bonds is insufficient, shallow donor-type levels may be formed. By utilizing this physical phenomenon, it is possible to control the carrier concentration by controlling the donors formed in the silicon wafer and form a buffer layer in the power semiconductor device. As a result, the switching waveform of the power semiconductor device becomes soft, and snap-off or oscillation can be prevented. Generally, donors are formed in the silicon wafer using proton irradiation, but they can also be formed by combining a process of introducing helium ion irradiation and some kind of hydrogen.

[0013] When forming a buffer layer on a silicon wafer, an appropriate annealing process is required after proton irradiation. This is because by performing the annealing process, the donor generation region spreads to the back side of the silicon wafer, making it possible to form a buffer layer with a desired thickness on the back side of the device. If this spread width is small, a high-resistance region remains on the back side of the device, resulting in deterioration of the characteristics of the power semiconductor device. However, if multi-stage irradiation is performed to obtain a wide buffer layer, unnecessary damage accumulates in the silicon. Therefore, in the embodiments shown below, a method for forming a buffer layer with a desired width without using multi-stage irradiation will be described.

[0014] <B. Embodiment 1> FIG. 1 is a flowchart showing a method for manufacturing a power semiconductor device according to Embodiment 1. FIGS. 2 to 11 are cross-sectional views showing the manufacturing process of the power semiconductor device according to Embodiment 1. Hereinafter, with reference to these figures, a method for manufacturing a power semiconductor device according to Embodiment 1 will be described. Here, as an example, a method for manufacturing a vertical IGBT or a vertical diode from an n-type or n--type silicon wafer will be described.

[0015] Before starting the flow of Fig. 1, a silicon wafer 1 shown in Fig. 2 is prepared. The silicon wafer 1 is cut from an ingot and has a first main surface S1, which is the front surface, and a second main surface S2, which is the back surface opposite to the first main surface S1. The hydrogen concentration of the silicon wafer 1 is, for example, 1 × 10 13 cm -3 The thickness of the silicon wafer 1 at this stage is W1.

[0016] In step S101 of FIG. 1, a hydrogen introduction step is performed to control the hydrogen concentration in the silicon wafer 1. In the hydrogen introduction step, the silicon wafer 1 is annealed in either a hydrogen gas or hydrogen plasma atmosphere. For example, the silicon wafer 1 is exposed to a hydrogen atmosphere and annealed in a furnace such as a vertical furnace at a temperature range of 1000°C to 1300°C (627K to 1027K). For example, when annealing is performed at 1100°C for 5 hours, the penetration depth of hydrogen in silicon is 1.7cm. Therefore, hydrogen can be impregnated into the entire depth direction of the silicon wafer 1 for power semiconductors. FIG. 3 shows the silicon wafer 1 in this state, and the region into which hydrogen has been introduced is indicated by matte hatching.

[0017] In the silicon wafer 1, a region that will become a buffer layer in a later process is referred to as a first region, and a region that will become a drift layer and an anode layer or a MOS structure in a later process is referred to as a second region. In the above hydrogen introduction step, hydrogen is introduced into the entire depth direction of the silicon wafer 1, i.e., into both the first and second regions, but it is sufficient that hydrogen is introduced into at least the first region.

[0018] Next, in step S102 of Fig. 1, an electron beam irradiation step is performed in which an electron beam is irradiated from the second main surface S2 of the silicon wafer 1. Here, an accelerator is used to irradiate the second main surface S2 of the silicon wafer 1 with electrons accelerated from several hundreds KeV to several tens MeV. As a result, the electron beam penetrates the silicon wafer 1 for power semiconductor use, and point defects 2 are formed throughout the entire thickness direction of the silicon wafer 1, as shown in Fig. 4. That is, point defects 2 are formed in both the first region and the second region.

[0019] The dose of the electron beam depends on the amount of point defects to be formed. For example, it is 1×10 12 More than 1×10 16 cm -2 The second main surface S2 of the silicon wafer 1 may be irradiated with protons or helium ions instead of the electron beam to form point defects 2 in localized portions of the silicon wafer.

[0020] 1, a donor activation annealing step is performed to form donors 3. Specifically, the silicon wafer 1 is exposed to an inert gas atmosphere such as nitrogen, and annealed at 200° C. to 500° C. This process causes hydrogen and point defects 2 in the silicon wafer 1 to react with each other, and donors 3 are formed throughout the thickness of the silicon wafer 1, as shown in FIG.

[0021] Figure 12 shows the areal density of donors (cm -2 ) is shown. As shown in FIG. 12, annealing at a temperature lower than 200° C. is not preferred because the efficiency of donor formation decreases. Annealing at a temperature higher than 500° C. is also not preferred because the annihilation of donors becomes significant. Therefore, the annealing temperature for donor activation is preferably 200° C. or higher and 500° C. or lower. The concentration of donor 3 can also be adjusted by the annealing time.

[0022] Next, in step S104 of Fig. 1, a donor local inactivation annealing step is performed to locally inactivate the donor 3 formed in the second region of the silicon wafer 1. Specifically, as shown in Fig. 6, light in a wavelength band absorbed by silicon is irradiated onto the first main surface S1 of the silicon wafer 1. This causes a local increase in temperature near the first main surface S1 of the silicon wafer 1, and the heat is conducted in a direction from the first main surface S1 to the second main surface S2. As shown in Fig. 12, the donor 3 is inactivated in the region where the temperature of the silicon has increased to 500°C or higher.

[0023] For example, a laser annealing device or a lamp annealing device is used for the light irradiation in this process. The wavelength of the light, the power density, and the irradiation time are adjusted so that the donor 3 in the first region of the silicon wafer 1 is not inactivated. Only the donor 3 in the second region of the silicon wafer 1 is annealed out, and the first region where the donor 3 remains uninactivated becomes the buffer layer 11. This buffer layer 11 is also called the first buffer layer.

[0024] Next, in step S105 of Fig. 1, a surface structure forming step is performed to form a surface structure of a device on the first main surface S1 side of the silicon wafer 1. The surface structure is also referred to as a first main surface structure. When manufacturing a diode, in the surface structure forming step, as shown in Fig. 7, a p+ type anode layer 14 is formed on the first main surface S1 of the silicon wafer 1, and an anode electrode 15 is formed on the anode layer 14. When manufacturing an IGBT, a p-type base region is formed on the surface of the silicon wafer 1, an n-type source region is formed, the silicon wafer 1 is dry etched to form a trench gate, a gate oxide film is formed, a gate electrode such as polysilicon is formed, an interlayer insulating film such as TEOS is formed, and a source electrode is formed.

[0025] 1, a wafer grinding process is performed in which the second main surface S2 is ground to make the silicon wafer 1 have a desired thickness. For example, after protecting the first main surface structure, the second main surface S2 of the silicon wafer 1 is ground using a grinding means such as CMP (Chemical Mechanical Polish). Hereinafter, the silicon wafer 1 after grinding is referred to as a semiconductor region. The thickness of the silicon wafer 1 after grinding is W2.

[0026] 1, a second buffer layer formation step is performed to form a second buffer layer on the second main surface S2 of the silicon wafer 1. For example, as shown in FIG. 9, an n-type second buffer layer 12 is formed by implanting n-type dopant ions such as phosphorus into the second main surface S2. The second buffer layer 12 may be formed by multiple ion implantations. The second buffer layer 12 may be omitted by substituting the first buffer layer 11.

[0027] Next, in step S108 of FIG. 1, a back surface structure forming step is performed to form a back surface structure of the device on the second main surface S2 of the silicon wafer 1. Hereinafter, the back surface structure of the device is also referred to as the second main surface structure. When manufacturing a diode, in the back surface structure forming step, an n+ type cathode layer 16 is formed on the second main surface S2 of the silicon wafer 1 as shown in FIG. 10. When manufacturing an RFC (Relaxed Field of Cathode) diode, a p+ type cathode layer is partially formed in addition to the n+ type cathode layer. When manufacturing an IGBT, a p+ type collector layer is formed on the back surface of the silicon wafer 1. When manufacturing an RC (Revers Conductive) IGBT, an n+ cathode layer is partially formed in addition to the collector layer.

[0028] Next, in step S109 of Fig. 1, a back electrode is formed on the second main surface S2 of the silicon wafer 1. When a diode is manufactured, the back electrode is a cathode electrode 17 shown in Fig. 11. When an IGBT is manufactured, the back electrode is a collector electrode. This completes the method for manufacturing the power semiconductor device according to the first embodiment.

[0029] FIG. 13 schematically shows the hydrogen concentration distribution of the power semiconductor device according to Embodiment 1. The solid line indicates the hydrogen concentration when the annealing temperature is high or the annealing time is long in the range of 200° C. or higher and 500° C. or lower. The dashed line indicates the hydrogen concentration when the annealing temperature is lower or the annealing time is shorter than that of the solid line in the range of 200° C. or higher and 500° C. or lower.

[0030] According to the manufacturing method of the power semiconductor device according to Embodiment 1, a wide first buffer layer 11 having no interface inside can be formed in a short time on the silicon wafer 1 without accumulating damage by the hydrogen introduction step, the electron beam irradiation step, the donor activation annealing step, and the donor local inactivation annealing step.

[0031] In the present embodiment, in the surface structure forming step, the wafer grinding step, the second buffer forming step, the back surface structure forming step, and the back surface electrode forming step, not limited to the above examples, other general manufacturing methods of IGBTs or diodes are applicable.

[0032] <C. Embodiment 2> In Embodiment 1, the first buffer layer (from step S101 to step S104 in FIG. 1) was formed prior to the device structure (from step S105 to step S109 in FIG. 1).

[0033] In contrast, in Embodiment 2, the forming step of the first buffer layer is formed after the device structure. By the way, when the device structure is formed on the silicon wafer 1, the annealing temperature and annealing time are restricted by the device structure thereafter. Also, since a metal electrode is generally used for the surface electrode of the power device, heat cannot be introduced into the silicon wafer 1 by irradiating light from the surface side after the formation of the surface structure. Therefore, in the manufacturing method of the power semiconductor device according to Embodiment 2, heat is introduced into the silicon wafer 1 by irradiating light from the back surface side.

[0034] Fig. 14 is a flowchart showing a method for manufacturing a power semiconductor device according to embodiment 2. The method for manufacturing a power semiconductor device according to embodiment 2 will be described below with reference to the flow of Fig. 14. Note that, as an example, a method for manufacturing a vertical IGBT or a vertical diode from an n-type or n-type silicon wafer will be described here.

[0035] Before starting the flow of FIG. 14, a silicon wafer 1 having a thickness W1 is prepared as in the first embodiment. Then, in step S201 of FIG. 14, a surface structure of a device is formed on the first main surface S1 of the silicon wafer 1. When manufacturing a diode, in the surface structure formation step, as shown in FIG. 15, a p+ type anode layer 14 is formed on the first main surface S1 of the silicon wafer 1, and an anode electrode 15 is formed on the anode layer 14. The region of the silicon wafer 1 other than the anode layer 14 is made into a drift layer 13. This step is similar to step S105 of FIG. 1.

[0036] Next, in step S202, a wafer grinding step is performed in which the second main surface S2 is ground to make the silicon wafer 1 have a desired thickness. This step is similar to step S106 in Fig. 1. Through this step, the silicon wafer 1 has a thickness W2.

[0037] Thereafter, in step S203, a second buffer layer formation step is performed in which a second buffer layer 12 is formed on the second main surface S2 of the silicon wafer 1. This step is similar to step S107 in FIG.

[0038] Next, in step S204, a back surface structure forming step is performed to form a back surface structure of a device on the second main surface S2 of the silicon wafer 1. When manufacturing a diode, in the back surface structure forming step, an n+ type cathode layer 16 is formed on the second main surface S2 of the silicon wafer 1 as shown in Fig. 17. This step is similar to step S108 in Fig. 1.

[0039] Thereafter, in step S205, a hydrogen introduction step is performed to control the hydrogen concentration in the silicon wafer 1. This step is similar to step S101 in Fig. 1, but the upper limit of the annealing temperature is set so that the surface structure is not destroyed, for example, 500°C or less. In this step, hydrogen should be introduced into at least the first region of the silicon wafer 1.

[0040] Next, in step S206, an electron beam irradiation process is performed in which an electron beam is irradiated from the second main surface S2 of the silicon wafer 1 to form point defects 2. This step is similar to step S102 in Fig. 1. Fig. 18 shows the silicon wafer 1 in which point defects 2 have been formed by this process.

[0041] Thereafter, in step S207, a donor activation annealing step is performed to form donors 3. This step is similar to step S103 in Fig. 1. Fig. 19 shows the silicon wafer 1 in a state in which donors 3 have been formed by this step.

[0042] Next, in step S208, a donor local inactivation annealing process is performed to locally inactivate the donor 3 formed in the second region of the silicon wafer 1. In the first embodiment, the first main surface S1 is irradiated with light in a wavelength band absorbed by silicon, but in the present embodiment, the second main surface S2 is irradiated with pulsed laser light in a wavelength band not absorbed by silicon. At this time, if the optical power is strong, local light absorption can be generated only at the focal position of the incident light due to a nonlinear optical effect. That is, only the deep part can be raised to 500° C. or more without heating the second main surface S2 of the silicon wafer 1. In this way, a part of the donor 3 generated in the donor activation annealing process is inactivated. By scanning the focus of the pulsed laser from the first main surface S1 to the bottom of the second region, the donor 3 in the second region can be inactivated. In this way, as shown in FIG. 20, the region of the drift layer 13 where the donor 3 remains becomes the buffer layer 11.

[0043] Thereafter, in step S209, a back surface electrode is formed on the second main surface S2 of the silicon wafer 1. This step is the same as step S109 in FIG. 1. The above is the manufacturing method of the power semiconductor device according to Embodiment 2.

[0044] FIG. 21 schematically shows the hydrogen concentration distribution of the power semiconductor device according to Embodiment 2. In FIG. 21, W3 is the total thickness of the first buffer layer 11, the second buffer layer 12, and the back surface structure. FIG. 21 shows the case where hydrogen is mainly introduced into the first region of the silicon wafer 1 in step S205.

[0045] According to the manufacturing method of the power semiconductor device according to Embodiment 2, a wide first buffer layer 11 having no interface inside can be formed in a short time on the silicon wafer 1 without accumulating damage by the hydrogen introduction step, the electron beam irradiation step, the donor activation annealing step, and the donor local deactivation annealing step.

[0046] In the present embodiment, in the surface structure formation step, the wafer grinding step, the second buffer formation step, the back surface structure formation step, and the back surface electrode formation step, not limited to the above examples, other general manufacturing methods of IGBTs or diodes are applicable.

[0047] <D. Embodiment 3> In the manufacturing method of the power semiconductor device according to Embodiment 3, after forming donors 3 in the first region and the second region of the silicon wafer 1, the donors 3 are locally deactivated in the second region, so that donors 3 are formed only in the first region.

[0048] On the other hand, in the manufacturing method of the power semiconductor device according to Embodiment 3, donors 3 are locally formed in the first region of the silicon wafer 1 by annealing using light.

[0049] Fig. 22 is a flowchart showing a method for manufacturing a power semiconductor device according to embodiment 3. The method for manufacturing a power semiconductor device according to embodiment 3 will be described below along the flow of Fig. 22. Note that, as an example, a method for manufacturing a vertical IGBT or a vertical diode from an n-type or n-type silicon wafer will be described here.

[0050] Before starting the flow of Fig. 22, a silicon wafer 1 having a thickness W1 is prepared as in the first and second embodiments. The subsequent processes from step S301 to step S306 are similar to steps S201 to S206 in Fig. 14, and the processes shown in Fig. 15 to Fig. 18 are performed.

[0051] After step S306, in step S307, a donor local activation annealing step is performed to locally convert point defects 2 in the semiconductor region into donors. For example, as shown in Fig. 23, an annealing process is performed in which light such as laser annealing or lamp annealing is irradiated onto the second main surface S2 of the silicon wafer 1. As a result, the temperature of the first region of the silicon wafer 1 is raised to a donor formation temperature or higher, for example, 200°C or higher, and donors 3 are formed locally in the first region.

[0052] If the annealing temperature is less than 200°C, the efficiency of donor formation decreases as shown in FIG. 12. If the annealing temperature is higher than 500°C, the annihilation of donors becomes significant. Therefore, the annealing temperature in this process is preferably 200°C or higher and 500°C or lower. The light intensity and irradiation time are adjusted so that the donor concentration becomes a desired value. In this process, of the point defects 2 formed in the silicon wafer 1 by electron beam irradiation, only the point defects 2 present in the first region are converted into donors 3, and the first region becomes a first buffer layer 11.

[0053] Next, in step S308, a back surface structure forming process is performed to form a back surface structure of the device on the second main surface S2 of the silicon wafer 1. This step is similar to step S108 in Fig. 1 and step S204 in Fig. 14. This completes the method for manufacturing the power semiconductor device according to the third embodiment.

[0054] The hydrogen concentration distribution of the power semiconductor device according to Embodiment 3 is as shown in FIG. 21.

[0055] According to the manufacturing method of the power semiconductor device according to Embodiment 3, by the hydrogen introduction step, the electron beam irradiation step, and the donor local activation annealing step, a wide first buffer layer 11 having no interface inside can be formed on the silicon wafer 1 in a short time without accumulating damage.

[0056] In the present embodiment, in the surface structure formation step, the wafer grinding step, the second buffer formation step, the back surface structure formation step, and the back surface electrode formation step, not limited to the above examples, other general manufacturing methods of IGBTs or diodes can be applied.

[0057] <E. Modification Example> In Embodiments 1, 2, and 3, the electron beam irradiation step was performed. However, when point defects originally exist in the silicon wafer 1, the electron beam irradiation step is not essential.

[0058] In Embodiment 1, the hydrogen introduction step, the electron beam irradiation step, the donor activation annealing step, and the donor local deactivation annealing step were performed before the surface structure formation step. By performing the hydrogen introduction step before the surface structure formation step, there is an advantage that the processing temperature of the hydrogen introduction step can be increased. However, the hydrogen introduction step, the electron beam irradiation step, the donor activation annealing step, and the donor local deactivation annealing step may be appropriately incorporated after the surface structure formation step. Also, the order of the hydrogen introduction step and the electron beam irradiation step may be interchanged. That is, after performing the hydrogen introduction step and the electron beam irradiation step, the donor activation annealing step and the donor local deactivation annealing step are performed in order, and then, if the silicon does not become hotter than 500°C (more preferably 400°C), the order of each step can be appropriately changed.

[0059] Similarly, in the second embodiment, the hydrogen introduction step, the electron beam irradiation step, the donor activation annealing step, and the donor local passivation annealing step are performed after the back surface structure formation step, but these steps may be appropriately incorporated after the front surface structure formation step and before the back surface structure formation step. The order of the hydrogen introduction step and the electron beam irradiation step may also be interchanged. That is, after the hydrogen introduction step and the electron beam irradiation step are performed, the donor activation annealing step and the donor local passivation annealing step are performed in that order, and the order of each step can be appropriately changed as long as the silicon does not become hotter than 500°C (more preferably 400°C) thereafter.

[0060] Similarly, in the third embodiment, the hydrogen introduction step, the electron beam irradiation step, and the donor local activation annealing step are performed after the back surface structure formation step, but these steps may be appropriately inserted after the front surface structure formation step and before the back surface structure formation step. The order of the hydrogen introduction step and the electron beam irradiation step may also be interchanged. That is, the order of each step can be appropriately changed as long as the donor local activation annealing step is performed after the hydrogen introduction step and the electron beam irradiation step, and the silicon temperature does not become higher than 500°C (more preferably 400°C) thereafter.

[0061] In addition, in the first, second and third embodiments, the hydrogen introduction step is performed on the surface of the silicon wafer, but the hydrogen introduction step may be performed on the side surface as well as the surface.

[0062] In the first, second and third embodiments, the hydrogen introduction step is described as annealing the silicon wafer 1 in either a hydrogen gas or hydrogen plasma atmosphere. However, hydrogen can also be introduced into the silicon wafer 1 by annealing the silicon wafer 1 in a state in which a hydrogen-containing film is deposited on the silicon wafer 1, or by immersing the silicon wafer 1 in a chemical solution containing hydrogen, i.e., an acidic liquid.

[0063] In addition, the above description does not specifically describe the electrode material, the film formation method, the concentration of each p-type or n-type region, etc. For these, general power semiconductor device design conditions may be applied according to the application.

[0064] In the above description, a diode or an IGBT is given as an example of a power semiconductor device manufactured by the manufacturing method according to each embodiment, but a MOSFET (Metal Oxide Semiconductor Field Effect Transistor), an SBD (Schottky Barrier Diode), a Thyristor, etc. may also be formed.

[0065] In addition, each embodiment can be freely combined, and each embodiment can be appropriately modified or omitted. The above description is an example in all respects. It is understood that countless modified examples not illustrated can be assumed. [Explanation of symbols]

[0066] 1 silicon wafer, 2 point defect, 3 donor, 11 first buffer layer, 12 second buffer layer, 13 drift layer, 14 anode layer, 15 anode electrode, 16 cathode layer, 17 cathode electrode, S1 first main surface, S2 second main surface.

Claims

1. introducing hydrogen into a region of a silicon wafer having a first main surface and a second main surface opposite to the first main surface, the first region being a region from the second main surface to a predetermined depth; forming defects in the first region and in a second region between the first region and the first main surface by penetrating the silicon wafer with an electron beam; heat-treating the silicon wafer to react the hydrogen with the defects to form donors; performing laser annealing from the first main surface or the second main surface of the silicon wafer, thereby inactivating the donors in the second region and making the first region into a buffer layer; A method for manufacturing a power semiconductor device.

2. The introduction of hydrogen is annealing the silicon wafer in a hydrogen atmosphere; annealing the silicon wafer in a hydrogen plasma; annealing the silicon wafer with a hydrogen-containing film deposited on the silicon wafer; or immersing the silicon wafer in an acidic liquid; Either of the following: The method for manufacturing a power semiconductor device according to claim 1 .

3. The laser annealing is a process of locally heating the second region by irradiating the first principal surface with light in a wavelength band that is absorbed by silicon. The method for manufacturing a power semiconductor device according to claim 1 or 2.

4. The laser annealing is a process of irradiating the second main surface with light of a wavelength band that is not absorbed by silicon, and scanning a focal point in a depth direction from the first main surface of the silicon wafer to a bottom of the second region, thereby locally heating the second region. The method for manufacturing a power semiconductor device according to claim 1 or 2.

5. The second region is heated to 500° C. or higher by the laser annealing. The method for manufacturing a power semiconductor device according to claim 1 or 2.

6. The second region is heated to 500°C or higher by the laser annealing. The method for manufacturing a power semiconductor device according to claim 3 .

7. The second region is heated to 500°C or higher by the laser annealing. The method for manufacturing a power semiconductor device according to claim 4 .

8. introducing hydrogen into a region of a silicon wafer having a first main surface and a second main surface opposite to the first main surface, the first region being a region from the second main surface to a predetermined depth; forming defects in the first region and in a second region between the first region and the first main surface by penetrating the silicon wafer with an electron beam; laser annealing the silicon wafer from the second main surface to locally react the hydrogen with the defects in the first region to form donors; The introduction of hydrogen is annealing the silicon wafer in a hydrogen atmosphere; annealing the silicon wafer in a hydrogen plasma; annealing the silicon wafer with a hydrogen-containing film deposited on the silicon wafer; or immersing the silicon wafer in an acidic liquid; Either of the following: A method for manufacturing a power semiconductor device.

9. The laser annealing is a process of locally heating the first region by irradiating the second principal surface with light in a wavelength band that is absorbed by silicon. The method for manufacturing a power semiconductor device according to claim 8 .

10. The first region is heated to 250° C. or higher by the laser annealing. The method for manufacturing a power semiconductor device according to claim 8 or 9.

Citation Information

Patent Citations

  • Semiconductor device and method for manufacturing semiconductor device

    JP2022035157A

  • Semiconductor device and method for manufacturing semiconductor device

    JP2023062606A

  • Semiconductor device and semiconductor device manufacturing method

    WO2016051973A1

  • Variable magnification slit exposing method in electronic copying machine

    JP1985090329A

  • Manufacturing method of semiconductor substrate

    JP2878488B2