Optical Devices
The optical device addresses the challenge of maintaining cell gap and adhesion in liquid crystal cells by controlling thickness and modulus relationships, achieving structural stability and uniformity.
Patent Information
- Application Number
- JP2023521486
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-29
- Filing Date
- 2021-10-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing methods for maintaining cell gap and adhesion between substrates in liquid crystal cells using flexible substrates are challenging due to the difficulty in controlling adhesive thickness and area, leading to potential contamination and structural instability under high temperature and pressure conditions.
The optical device includes specific thickness and modulus relationships between outer layers and the liquid crystal element, along with intermediate layers, to maintain cell gap and adhesion, minimizing defects and ensuring structural stability.
The solution effectively maintains cell gap and adhesion, reducing defects and ensuring uniformity and stability under high temperature and pressure conditions.
Smart Images

Figure 0007585578000001 
Figure 0007585578000002 
Figure 0007585578000003
Abstract
Description
[Technical field]
[0001] The present application relates to optical devices.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0142094, filed on October 29, 2020, and all contents disclosed in the documents of said Korean patent application are incorporated herein by reference. [Background technology]
[0003] For the long-term stability and large-area scalability of a liquid crystal cell using a flexible substrate, it is important to maintain a cell gap between the upper and lower substrates and to provide adhesive strength between the upper and lower substrates.
[0004] Non-Patent Document 1 ("Tight Bonding of Two Plastic Substrates for Flexible LCDs" SID Symposium Digest, 38, pp. 653-656 (2007)) discloses a technique of forming a columnar or wall-shaped organic film pattern with the height of the cell gap on one substrate and fixing it to the opposite substrate using an adhesive. However, this technique requires that the adhesive be located only on the columnar or wall surfaces, but the technique of micro-stamping the adhesive on the columnar or wall surfaces is highly difficult to process, difficult to control the thickness and area of the adhesive, and highly likely that the adhesive will be pushed out when the upper and lower substrates are bonded, which may contaminate the alignment film or the liquid crystal. Summary of the Invention [Problem to be solved by the invention]
[0005] In order to maintain the cell gap of the liquid crystal cell and ensure the adhesive strength between the upper and lower substrates, it is possible to form a spacer and an alignment film on the lower substrate, and then form an adhesive having both liquid crystal alignment and adhesive strength on the upper substrate, and then bond them together. However, this structure is vulnerable to external pressure due to the very low modulus of the adhesive layer, and it is difficult to obtain good quality in the high-temperature and high-pressure autoclave process. Specifically, if the structural stability of the liquid crystal cell is not ensured in the autoclave process, the cell gap may collapse and the liquid crystal may flow and / or concentrate poorly, which causes deterioration of the electro-optical properties and appearance uniformity of the liquid crystal cell.
[0006] The present application provides an optical device in which the cell gap of a liquid crystal cell is properly maintained, the upper and lower substrates have excellent adhesion, and defects such as pressing and concentration are minimized, thereby ensuring structural stability and good quality uniformity. [Means for solving the problem]
[0007] In the present specification, when the measurement temperature affects the results of the physical properties, the physical properties are measured at room temperature unless otherwise specified. The term "room temperature" refers to a natural temperature without heating or cooling, and is usually a temperature within a range of about 10°C to 30°C, or about 23°C or about 25°C. Furthermore, unless otherwise specified in the present specification, the unit of temperature is °C. In the present specification, when the measurement pressure affects the results of the physical properties, the physical properties are measured at normal pressure unless otherwise specified. The term "normal pressure" refers to a natural pressure without pressurization or depressurization, and normal pressure is usually about 1 atmosphere.
[0008] The present application relates to an optical device. FIG. 1 exemplarily illustrates the optical device of the present application. As shown in FIG. 1, the optical device may include a first outer substrate 100a, a second outer substrate 100b disposed opposite to the first outer substrate 100a, and a liquid crystal element 300 disposed between the first outer substrate 100a and the second outer substrate 100b. The optical device may include at least one intermediate layer disposed between the first outer substrate and the liquid crystal element and between the second outer substrate and the liquid crystal element. FIG. 1 exemplarily illustrates the optical device including intermediate layers 200a and 200b disposed between the first outer substrate 100a and the liquid crystal element 300 and between the second outer substrate 100b and the liquid crystal element 300, respectively.
[0009] The optical device may further include an outer layer 400 surrounding the side of the liquid crystal element 300. The optical device according to the present application can minimize pressing and / or concentration defects that may occur when the optical device and the outer substrate are bonded together by controlling the relationship between the thickness of the outer layer and the liquid crystal element or the relationship between the storage modulus of the outer layer and the adhesive layer.
[0010] In one example, the optical device of the present application can satisfy the following formula 1:
[0011] [Formula 1] -T2×0.4≦T1-T2≦T2×0.4
[0012] In formula 1, T1 is the thickness of the outer layer and T2 is the thickness of the liquid crystal element.
[0013] The thickness T1 of the outer layer may refer to the thickness of the layer or film when the outer layer is composed of a single layer or a single film. The thickness T1 of the outer layer may refer to the sum of the thicknesses of the layers or films when the outer layer is composed of multiple layers or multiple films. The thickness T2 of the liquid crystal element may refer to the sum of the thicknesses of the first base layer, the adhesive layer, the spacer, and the second base layer, for example.
[0014] If the thickness difference (T1-T2) between the outer layer and the liquid crystal element is too small, the liquid crystal element may be pressed and / or have poor concentration when the optical device is bonded, so the lower limit of the thickness difference (T1-T2) between the outer layer and the liquid crystal element is preferably -T2 x 0.4 or more. The lower limit of the thickness difference (T1-T2) may be specifically -T2 x 0.3 or more, -T2 x 0.2 or more, -T2 x 0.1 or more, -T2 x 0.08 or more, -T2 x 0.06 or more, -T2 x 0.04 or more, or -T2 x 0.02 or more.
[0015] If the thickness difference (T1-T2) between the outer layer and the liquid crystal element is too large, the outer substrate may be damaged during bonding of the optical device, so the upper limit of the thickness difference (T1-T2) between the outer layer and the liquid crystal element is preferably T2 x 0.4 or less. The upper limit of the thickness difference (T1-T2) may be specifically T2 x 0.35 or less, T2 x 0.3 or less, or T2 x 0.25 or less.
[0016] The thickness T1 of the outer layer and the thickness T2 of the liquid crystal element may be appropriately selected within a range that satisfies the formula 1. In one example, the thickness T1 of the outer layer may be within a range of 60 μm to 840 μm. In one example, the thickness T2 of the liquid crystal element may be within a range of 100 μm to 800 μm.
[0017] In one example, the optical device of the present application can satisfy the following formula 2:
[0018] [Formula 2] G1 ≧ G2
[0019] In formula 2, G1 is the storage modulus of the outer layer at 25° C., and G2 is the storage modulus of the pressure-sensitive adhesive layer at 25° C. The storage modulus may be a value measured at a frequency of 6 rad / sec.
[0020] If the storage modulus G1 of the outer layer is smaller than the storage modulus G2 of the adhesive layer, pressing and / or concentration problems may occur in the liquid crystal element when the optical device is attached, so the storage modulus G1 of the outer layer may be controlled to be the same as or greater than the storage modulus G2 of the adhesive layer.
[0021] The storage modulus G1 of the outer layer may refer to the storage modulus of the layer or film when the outer layer is composed of a single layer or a single film. When the outer layer is composed of multiple layers or multiple films, the storage modulus G1 of the outer layer may refer to the storage modulus of a laminate of multiple layers or multiple films, or may refer to the storage modulus of each layer or each film constituting the multiple layers or multiple films.
[0022] In one example, when the layer or film constituting the outer layer is measured so that the storage modulus value differs along the MD (Machine Direction) axis or the TD (Transverse direction) axis, either the storage modulus along the MD axis or the storage modulus along the TD axis may satisfy the above formula 2, or both the storage modulus along the MD axis and the storage modulus along the TD axis may satisfy the above formula 2. The MD axis and the TD axis may be perpendicular to each other.
[0023] The difference (G1-G2) between the storage modulus of the outer layer and the storage modulus of the adhesive layer may be, for example, 9999.99 MPa or less. If the difference (G1-G2) between the storage modulus of the outer layer and the storage modulus of the adhesive layer is too large, damage may occur when bonding with the outer substrate, so it may be advantageous to control it within the above range. The difference (G1-G2) between the storage modulus may be specifically 9,500 MPa or less, 9,000 MPa or less, 8,500 MPa or less, 8,000 MPa or less, 7,500 MPa or less, 7,000 MPa or less, or 6,500 MPa or less.
[0024] The difference (G1-G2) between the storage modulus of the outer layer and the storage modulus of the adhesive layer may be, for example, 0 MPa or more. If the difference (G1-G2) is too small, the liquid crystal holding and / or concentration failure may not be effectively improved, so it may be advantageous to control it within the above range. The difference (G1-G2) between the storage modulus may be specifically 1 MPa or more, 5 MPa or more, 10 MPa or more, 20 MPa or more, 40 MPa or more, 60 MPa or more, or 80 MPa or more.
[0025] The storage modulus G1 of the outer layer and the storage modulus G2 of the pressure-sensitive adhesive layer may be appropriately selected within a range satisfying formula 2. In one example, the storage modulus G1 of the outer layer may be within a range of 0.1 MPa to 10,000 MPa. Specifically, the storage modulus G1 of the outer layer may be 1 MPa or more, 5 MPa or more, 10 MPa or more, 100 MPa or more, 500 MPa or more, 1,000 MPa or more, or 1,500 MPa or more, or 10,000 MPa or less, 9,000 MPa or less, 8,000 MPa or less, 7,000 MPa or less, 6,000 MPa or less, 5,000 MPa or less, 4,000 MPa or less, 3,000 MPa or less, 2,000 MPa or less, 1,000 MPa or less, 800 MPa or less, 600 MPa or less, 400 MPa or less, 200 MPa or less, or 100 MPa or less.
[0026] In one example, the storage modulus G2 of the pressure-sensitive adhesive layer may be within a range of 0.01 MPa to 1 MPa. Specifically, the storage modulus G2 of the pressure-sensitive adhesive layer may be 0.02 MPa or more, 0.04 MPa, 0.06 MPa, 0.08 MPa, or 0.1 MPa or more, and may be 0.8 MPa or less, 0.6 MPa or less, 0.4 MPa or less, or 0.2 MPa or less. If the storage modulus of the pressure-sensitive adhesive layer is too large, it becomes difficult to satisfy the above conditions, and if the storage modulus of the pressure-sensitive adhesive layer is too small, the pressure-sensitive adhesive may be pressed or pushed during bonding of the liquid crystal element, which may impair the electro-optical properties and the uniformity of the appearance, so it may be advantageous to control the storage modulus within the above range.
[0027] The optical device of the present application can satisfy both formulas 1 and 2. This can effectively minimize the pressing and / or concentration defects that may occur during bonding of the optical device.
[0028] The first outer substrate and the second outer substrate may be an inorganic substrate or a plastic substrate, respectively. The inorganic substrate is not particularly limited, and a known inorganic substrate may be used. For example, the inorganic substrate may be a glass substrate having excellent light transmittance. The glass substrate may be, but is not limited to, a soda lime glass substrate, a general reinforced glass substrate, a borosilicate glass substrate, or an alkali-free glass substrate. The polymer substrate may be a cellulose film such as TAC (triacetyl cellulose) or DAC (diacetyl cellulose), a cycloolefin copolymer film such as a norbornene derivative, an acrylic film such as PA (Polyacrylate) or PMMA (poly(methyl methacrylate), a PC (polycarbonate) film, a polyolefin film such as PE (polyethylene) or PP (polypropylene), a polyvinyl alcohol (PVA), or a cellulose ester film such as PEG (PEG), PEG (PEG), or a PEG (PEG) film. Examples of the film may include, but are not limited to, sulfone-based films such as alcohol film, PI (polyimide) film, PSF (polysulfone) film, PPS (polyphenylsulfone) film, or PES (polyethersulfone) film, polyester-based films such as PEEK (polyetheretherketon) film, PEI (polyetherimide) film, PEN (polyethylenenaphthalate) film, or PET (polyethyleneterephtalate) film, or fluororesin films. The first and second outer substrates may each have a functional layer such as a coating layer of gold, silver, or a silicon compound such as silicon dioxide or silicon monoxide, or an anti-reflection layer, if necessary.
[0029] In one example, the first outer substrate and / or the second outer substrate may be a glass substrate. In order to overcome the physical limitations of the liquid crystal device, in the automobile or window industry, glass substrates may be bonded to both sides of the liquid crystal device, or a glass substrate may be bonded to one side of the liquid crystal device and a film substrate may be bonded to the other side. Among these, in the automobile industry, it is required to bond glass substrates to both sides of the liquid crystal device via an adhesive layer. However, the liquid crystal device is vulnerable to external pressure due to the use of an adhesive layer, and defects such as collapse of the cell gap, flow or concentration of liquid crystal may occur during a glass bonding process such as a high-temperature and high-pressure autoclave. According to the present invention, the defects can be minimized by controlling the thicknesses of the first intermediate layer and the second intermediate layer as described below, and the structural stability and uniformity of the quality of the optical device can be ensured.
[0030] The thickness of the first outer substrate and the second outer substrate may each be about 0.3 mm or more. In other examples, the thickness may be about 0.5 mm or more, 1 mm or more, 1.5 mm or more, or about 2 mm or more, and may be about 10 mm or less, 9 mm or less, 8 mm or less, 7 mm or less, 6 mm or less, 5 mm or less, 4 mm or less, or about 3 mm or less.
[0031] The first outer substrate and the second outer substrate may be flat substrates or may have a curved shape. For example, the first outer substrate and the second outer substrate may be flat substrates at the same time, may have a curved shape at the same time, or one may be a flat substrate and the other may be a curved substrate. In addition, when the first outer substrate and the second outer substrate are curved at the same time, the curvature or the radius of curvature may be the same or different. In this specification, the curvature or the radius of curvature may be measured by a method known in the art, for example, using a non-contact device such as a 2D Profile Laser Sensor, a Chromatic confocal line sensor, or a 3D Measuring Confocal Microscopy. The method of measuring the curvature or the radius of curvature using such a device is well known.
[0032] Regarding the first outer substrate and the second outer substrate, for example, when the curvature or radius of curvature of the front surface and the rear surface are different, the curvature or radius of curvature of the opposing surface, i.e., in the case of the first outer substrate, the curvature or radius of curvature of the surface opposing the second outer substrate, and in the case of the second outer substrate, the curvature or radius of curvature of the surface opposing the first outer substrate, may be the reference. Also, when the curvature or radius of curvature of the surface is not constant and there are different portions, the maximum curvature or radius of curvature may be the reference, the minimum curvature or radius of curvature may be the reference, or the average curvature or radius of curvature may be the reference.
[0033] The difference between the curvature or radius of curvature of the first and second outer substrates may be within about 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, or about 1%. The difference between the curvature or radius of curvature is calculated as 100% x (CL-CS) / CS, where CL is the larger curvature or radius of curvature and CS is the smaller curvature or radius of curvature. The lower limit of the difference between the curvature or radius of curvature is not particularly limited. The difference between the curvature or radius of curvature of the first and second outer substrates may be the same, so the difference between the curvature or radius of curvature may be equal to or greater than about 0%. The control of the curvature or radius of curvature as described above is useful in a structure in which a liquid crystal element is in contact with an intermediate layer, such as the optical device of the present application. In other words, if the difference in curvature or radius of curvature exceeds 10%, when the outer substrate and the liquid crystal element are bonded to each other through an intermediate layer described below, the bonded outer substrates may widen due to a decrease in adhesive strength. However, if the difference is controlled to within 10%, the problem of the bonded outer substrates widening due to a decrease in adhesive strength can be effectively prevented.
[0034] The first outer substrate and the second outer substrate may have the same sign of curvature. In other words, the first and second outer substrates may be curved in the same direction. That is, in this case, the center of curvature of the first outer substrate and the center of curvature of the second outer substrate are located in the same portion among the upper and lower portions of the first and second outer substrates. When the first outer substrate and the second outer substrate are curved in the same direction, the first and second outer substrates can be bonded more efficiently by the intermediate layer, and the adhesion strength between the first and second outer substrates and the liquid crystal element film and / or the polarizer after bonding can be more efficiently prevented from decreasing.
[0035] The first outer substrate and the second outer substrate are not particularly limited in the specific range of the curvature or the radius of curvature. In one example, the first and second outer substrates may each have a radius of curvature of about 100R or more, 200R or more, 300R or more, 400R or more, 500R or more, 600R or more, 700R or more, 800R or more, or about 900R or more, or about 10,000R or less, 9,000R or less, 8,000R or less, 7,000R or less, 6,000R or less, 5,000R or less, 4,000R or less, 3,000R or less, 2,000R or less, 1,900R or less, 1,800R or less, 1,700R or less, 1,600R or less, 1,500R or less, 1,400R or less, 1,300R or less, 1,200R or less, 1,100R or less, or about 1,050R or less. In the above, R means the degree of curvature of a circle with a radius of 1 mm. Thus, for example, 100R is the degree of curvature of a circle with a radius of 100 mm, or the radius of curvature of the circle. The first and second outer substrates may have the same or different radii of curvature within the above range. In one example, when the curvatures of the first and second outer substrates are different from each other, the radius of curvature of the substrate with the larger curvature may be within the above range. In one example, when the curvatures of the first and second outer substrates are different from each other, the substrate with the larger curvature may be the substrate that is disposed in the direction of gravity when the optical device is used. If the curvatures or radii of curvature of the first and second substrates are controlled as described above, even if the adhesion force of the intermediate layer described later decreases, the resultant force, which is the sum of the restoring force and gravity, acts to prevent spreading.
[0036] In one example, the optical device may not include a polarizer between the first outer substrate and the liquid crystal element and between the second outer substrate and the liquid crystal element. FIG. 1 exemplarily illustrates an optical device that does not include a polarizer. In another example, the optical device may further include a polarizer at at least one of between the first outer substrate and the liquid crystal element and between the second outer substrate and the liquid crystal element. FIG. 2 exemplarily illustrates an optical device including a polarizer 500a positioned between the first outer substrate and the liquid crystal element and a second polarizer 500b positioned between the second outer substrate and the liquid crystal element. The optical device may include an intermediate layer 200a positioned between the first outer substrate and the first polarizer, an intermediate layer 200b positioned between the first polarizer and the liquid crystal element, an intermediate layer 200c positioned between the liquid crystal element and the second polarizer, and an intermediate layer 200d positioned between the second polarizer and the second outer substrate.
[0037] In this specification, the term polarizer means a film, sheet, or element having a polarizing function. A polarizer is a functional element that can extract light vibrating in one direction from incident light vibrating in various directions.
[0038] The polarizer may be an absorptive polarizer or a reflective polarizer. In this specification, the absorptive polarizer means an element that exhibits selective transmission and absorption characteristics for incident light. For example, the polarizer may transmit light that vibrates in one direction from incident light that vibrates in various directions, and absorb light that vibrates in the remaining directions. In this specification, the reflective polarizer means an element that exhibits selective transmission and reflection characteristics for incident light. For example, the polarizer may transmit light that vibrates in one direction from incident light that vibrates in various directions, and reflect light that vibrates in the remaining directions. According to one embodiment of the present application, the polarizer may be an absorptive polarizer.
[0039] The polarizer may be a linear polarizer. In this specification, a linear polarizer means that the selectively transmitted light is linearly polarized light that vibrates in one direction, and the selectively absorbed or reflected light is linearly polarized light that vibrates in a direction perpendicular to the vibration direction of the linearly polarized light. In the case of an absorptive linear polarizer, the light transmission axis and the light absorption axis may be perpendicular to each other. In the case of a reflective linear polarizer, the light transmission axis and the light reflection axis may be perpendicular to each other.
[0040] In one example, the polarizers may be polymer stretched films dyed with iodine or anisotropic dyes. The polymer stretched films include PVA (poly(vinyl alcohol)) stretched films. In another example, the first polarizer and the second polarizer may be guest-host polarizers in which a liquid crystal polymerized in an oriented state serves as a host and an anisotropic dye aligned by the orientation of the liquid crystal serves as a guest. In another example, the polarizers may be thermotropic liquid crystal films or lyotropic liquid crystal films.
[0041] A protective film, an anti-reflection film, a retardation film, an adhesive layer, an adhesive layer, a surface treatment layer, etc. may be further formed on one or both sides of the polarizer. The retardation film may be, for example, a quarter-wave plate or a half-wave plate. The quarter-wave plate may have an in-plane retardation value in the range of about 100 nm to 180 nm, 100 nm, or 150 nm for light with a wavelength of 550 nm. The half-wave plate may have an in-plane retardation value in the range of about 200 nm to 300 nm, or 250 nm to 300 nm for light with a wavelength of 550 nm. The retardation film may be, for example, a polymer stretched film or a liquid crystal polymerized film.
[0042] The transmittance of the polarizer for light having a wavelength of 550 nm may be within a range of 40% to 50%. The transmittance may refer to the single transmittance of the polarizer for light having a wavelength of 550 nm. The single transmittance of the polarizer may be measured, for example, using a spectrometer (V7100, manufactured by Jasco). For example, the air may be set as the baseline in a state where a polarizer sample (not including upper and lower protective films) is attached to the instrument, and the axis of the polarizer sample may be aligned vertically and horizontally with the axis of the reference polarizer to measure the respective transmittances, and then the single transmittance may be calculated.
[0043] Assuming that the blocking state is realized in a first orientation state of the liquid crystal element, the polarizer may be disposed in the optical device such that the angle between the average optical axis (vector sum of the optical axes) of the first orientation state and the light absorption axis of the polarizer is about 80 degrees to about 100 degrees, or about 85 degrees to about 95 degrees, or is almost perpendicular, or is 35 degrees to about 55 degrees, or about 40 degrees to about 50 degrees, or about 45 degrees.
[0044] Fig. 3 exemplarily illustrates a liquid crystal element. As shown in Fig. 3, the liquid crystal element may include a first base layer 10a, an adhesive layer 10c formed on the inner side of the first base layer, a second base layer 20a arranged opposite to the first base layer 10a, a spacer 20c formed on the inner side of the second base layer 20a, and a liquid crystal layer 30 located between the first base layer 10a and the second base layer 20a.
[0045] The first and second substrate layers may be, for example, inorganic films such as glass films, crystalline or amorphous silicon films, quartz or ITO (Indium Tin Oxide) films, or polymer films, and a polymer film may be used in terms of realizing a flexible element.
[0046] In one example, the first substrate layer and the second substrate layer may each be a polymer film. Examples of the polymer film that may be used include, but are not limited to, triacetyl cellulose (TAC), cycloolefin copolymer (COP) such as norbornene derivatives, poly(methyl methacrylate) (PMMA), polycarbonate (PC), polyethylene (PE), polypropylene (PP), polyvinyl alcohol (PVA), diacetyl cellulose (DAC), polyacrylate (PAC), polyether sulfone (PES), polyetheretherketone (PEEK), polyphenylsulfone (PPS), polyetherimide (PEI), polyethylenemaphthate (PEN), polyethyleneterephtalate (PET), polyimide (PI), polysulfone (PSF), polyarylate (PA), and amorphous fluororesin. The first and second substrate layers may have a coating layer of gold, silver, silicon compound such as silicon dioxide or silicon monoxide, or an anti-reflection layer, if necessary.
[0047] The first and second base layers may each have a thickness of about 10 μm to about 1,000 μm. As another example, the base layers may each have a thickness of about 20 μm or more, 40 μm or more, 60 μm or more, 80 μm or more, 100 μm or more, 120 μm or more, 140 μm or more, 160 μm or more, or about 180 μm or more, and may each be about 900 μm or less, 800 μm or less, 700 μm or less, 600 μm or less, 500 μm or less, or about 400 μm or less. When the thicknesses of the first and second base layers satisfy the above ranges, defects in appearance such as wrinkles can be reduced when the liquid crystal element is bonded to an outer substrate to manufacture an optical device.
[0048] The pressure-sensitive adhesive layer may be optically transparent, and may have an average transmittance of about 80% or more, 85% or more, 90% or more, or 95% or more in the visible light region, for example, in the wavelength range of 380 nm to 780 nm.
[0049] The adhesive layer may be a liquid crystal aligning adhesive layer. The adhesive layer may be, for example, a vertically aligning adhesive layer or a horizontally aligning adhesive layer. In this specification, the term "vertically aligning adhesive" may mean an adhesive having an adhesive force capable of imparting a vertical alignment force to adjacent liquid crystal compounds and bonding an upper substrate and a lower substrate. In this specification, the term "horizontally aligning adhesive" may mean an adhesive having an adhesive force capable of imparting a horizontal alignment force to adjacent liquid crystal compounds and bonding an upper substrate and a lower substrate. The pretilt angle of the adjacent liquid crystal compounds relative to the vertically aligning adhesive may be within a range of 80 degrees to 90 degrees, 85 degrees to 90 degrees, or about 87 degrees to 90 degrees, and the pretilt angle of the adjacent liquid crystal compounds relative to the horizontally aligning adhesive may be within a range of 0 degrees to 10 degrees, 0 degrees to 5 degrees, or 0 degrees to 3 degrees.
[0050] In this specification, the pretilt angle may refer to the angle that the director of the liquid crystal compound makes with respect to the liquid crystal alignment adhesive or alignment film and a plane horizontal thereto when no voltage is applied. In this specification, the director of the liquid crystal compound may refer to the optical axis or slow axis of the liquid crystal layer. Alternatively, the director of the liquid crystal compound may refer to the long axis direction when the liquid crystal compound is rod-shaped, and may refer to the axis parallel to the normal direction of the disc plane when the liquid crystal compound is discotic.
[0051] The thickness of the adhesive layer may be, for example, within a range of 3 μm to 15 μm. When the thickness of the adhesive layer is within this range, it may be advantageous in minimizing defects such as pressing or squeezing of the adhesive when used in manufacturing a liquid crystal element film while ensuring adhesion between the upper and lower substrates.
[0052] The adhesive layer may be made of various types of adhesives known in the industry as OCA (Optically Clear Adhesive). The adhesive may be different from OCR (Optically Clear Resin) type adhesives that are cured after the objects are bonded, in that the adhesive is cured before the objects are bonded. The adhesive may be, for example, an acrylic, silicone, epoxy, or urethane adhesive.
[0053] The adhesive layer may include a cured product of an adhesive resin. In one example, the adhesive layer may include a silicone-based adhesive. The silicone-based adhesive may include a cured product of a curable silicone compound as an adhesive resin.
[0054] The type of the curable silicone compound is not particularly limited, and for example, a heat-curable silicone compound or an ultraviolet-curable silicone compound may be used. The curable silicone compound may also be called an adhesive resin.
[0055] In one example, the curable silicone compound may be an addition-curable silicone compound.
[0056] Specifically, the addition curing silicone compound includes, but is not limited to, (1) an organopolysiloxane containing two or more alkenyl groups in the molecule and (2) an organopolysiloxane containing two or more silicon-bonded hydrogen atoms in the molecule. The silicone compound may form a cured product by addition reaction in the presence of a catalyst described later, for example.
[0057] More specific examples of the organopolysiloxane (1) that can be used in the present application include dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with trimethylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxane groups, dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, methylvinylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, dimethylsiloxane-methylvinylsiloxane-methylphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxane groups, R 1 2 SiO 1 / 2 The siloxane unit represented by R 1 2 R 2 SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 2 R 2 SiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 R 2 SiO 2 / 2 and a siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by R 2 SiO 3 / 2 and mixtures of two or more of the above. 1is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenethyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group. 2 is an alkenyl group, and specifically may be a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, or the like.
[0058] More specific examples of the organopolysiloxane (2) that can be used in the present application include methylhydrogenpolysiloxanes capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogen copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylsiloxane-methylhydrogensiloxane-methylphenylsiloxane copolymers capped with trimethylsiloxane groups at both molecular chain terminals, dimethylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, dimethylsiloxane-methylphenylsiloxane copolymers capped with dimethylhydrogensiloxane groups at both molecular chain terminals, methylphenylpolysiloxanes capped with dimethylhydrogensiloxane groups at both molecular chain terminals, R 1 3 SiO 1 / 2 The siloxane unit represented by R 1 2 HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 2 HSiO 1 / 2 The siloxane unit represented by the formula 4 / 2 Organopolysiloxane copolymers containing siloxane units represented by R 1 HSiO 2 / 2 The siloxane unit represented by R 1 SiO 3 / 2 Siloxane units represented by HSiO 3 / 2and mixtures of two or more of the above. 1 is a hydrocarbon group other than an alkenyl group, and specifically may be an alkyl group such as a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, or a heptyl group; an aryl group such as a phenyl group, a tolyl group, a xylyl group, or a naphthyl group; an aralkyl group such as a benzyl group or a phenentyl group; or a halogen-substituted alkyl group such as a chloromethyl group, a 3-chloropropyl group, or a 3,3,3-trifluoropropyl group.
[0059] When the adhesive layer is a vertically oriented adhesive layer, the surface energy may be 16 mN / m or less. The lower limit of the surface energy may be, for example, 5 mN / m or more. When the adhesive layer is a horizontally oriented adhesive layer, the surface energy may be more than 16 mN / m. The upper limit of the surface energy may be, for example, 50 mN / m or less. The surface energy may be measured using a Drop Shape Analyzer (DSA100 product of KRUSS). Specifically, deionized water with a known surface tension is dropped on the surface of the adhesive, the contact angle is measured, and the process is repeated five times to obtain the average value of the five contact angles obtained. Similarly, diiodomethane with a known surface tension is dropped on the surface of the adhesive, the contact angle is measured, and the process is repeated five times to obtain the average value of the five contact angles obtained. Then, the surface energy was calculated by substituting the value (Strom value) related to the surface tension of the solvent using the average contact angle for deionized water and diiodomethane obtained by the Owens-Wendt-Rabel-Kaelble method. The surface energy (γsurface) of the sample can be calculated by considering the dispersion force between nonpolar molecules and the interaction force between polar molecules (γsurface = γdispersion + γpolar), and the ratio of the polar term (γolar) in the surface energy γsurface can be defined as the polarity of the surface.
[0060] The upper and lower substrates of the liquid crystal element may be attached to each other by an adhesive layer. Specifically, the adhesive layer of the upper substrate may be attached to the spacer of the lower substrate. When an alignment film is formed on the spacer of the lower substrate, a region of the alignment film corresponding to the spacer may be attached to the adhesive layer of the upper substrate.
[0061] The liquid crystal layer may include a liquid crystal compound. As the liquid crystal compound, a liquid crystal compound whose alignment direction can be changed by application of an external action may be used. In this specification, the term "external action" may mean all external factors, such as an external voltage, that can affect the behavior of a substance contained in the liquid crystal layer. Therefore, a state without an external action may mean a state in which an external voltage or the like is not applied.
[0062] The type and properties of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. In one example, the liquid crystal compound may be a nematic liquid crystal or a smectic liquid crystal. Nematic liquid crystal refers to a liquid crystal in which rod-shaped liquid crystal molecules are arranged in parallel to the long axis direction of the liquid crystal molecules without any regularity in position, and smectic liquid crystal refers to a liquid crystal in which rod-shaped liquid crystal molecules are regularly arranged to form a layered structure and are regularly arranged in parallel to the long axis direction. According to one embodiment of the present application, the liquid crystal compound may be a nematic liquid crystal compound.
[0063] Nematic liquid crystal compounds may be selected, for example, to have a clearing point of about 40° C. or higher, 50° C. or higher, 60° C. or higher, 70° C. or higher, 80° C. or higher, 90° C. or higher, 100° C. or higher, or about 110° C. or higher, or a phase transition point within the above range, i.e., a phase transition point from a nematic phase to an isotropic phase. In one example, the clearing point or phase transition point may be about 160° C. or lower, 150° C. or lower, or about 140° C. or lower.
[0064] The liquid crystal compound may be a non-reactive liquid crystal compound. The non-reactive liquid crystal compound may mean a liquid crystal compound that does not have a polymerizable group. The polymerizable group may include, but is not limited to, an acryloyl group, an acryloyloxy group, a methacryloyl group, a methacryloyloxy group, a carboxyl group, a hydroxyl group, a vinyl group, or an epoxy group, and may include a known functional group known as a polymerizable group.
[0065] The liquid crystal compound may have a positive or negative dielectric anisotropy. The absolute value of the dielectric anisotropy of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. The term "dielectric anisotropy (Δε)" may mean the difference (ε / / -ε⊥) between the horizontal dielectric constant (ε / / ) and the vertical dielectric constant (ε⊥) of the liquid crystal. In this specification, the term horizontal dielectric constant (ε / / ) means a dielectric constant value measured along the direction of an electric field in a state where a voltage is applied so that the direction of the electric field caused by the applied voltage and the director of the liquid crystal compound are substantially horizontal, and the term vertical dielectric constant (ε⊥) means a dielectric constant value measured along the direction of an electric field in a state where a voltage is applied so that the direction of the electric field caused by the applied voltage and the director of the liquid crystal compound are substantially perpendicular.
[0066] The refractive index anisotropy of the liquid crystal compound may be appropriately selected in consideration of the object of the present application. In this specification, the term "refractive index anisotropy" may mean the difference between the extraordinary refractive index and the ordinary refractive index of the liquid crystal compound. The refractive index anisotropy of the liquid crystal compound may be, for example, 0.01 to 0.3. The refractive index anisotropy may be 0.01 or more, 0.05 or more, or 0.07 or more, and may be 0.3 or less, 0.2 or less, 0.15 or less, or 0.13 or less.
[0067] The liquid crystal layer may further include a dichroic dye. When the liquid crystal layer includes a dichroic dye, even if the liquid crystal element film includes an adhesive layer, there is little effect on the variation of the cell gap during the bonding process of the outer substrate, so that there is an advantage that the thickness of the intermediate layer for ensuring the structural stability and quality uniformity of the liquid crystal element can be relatively thin.
[0068] The dichroic dye can control the light transmittance variable property of the liquid crystal layer. In this specification, the term "dye" refers to a substance that can intensively absorb and / or transform light in at least a part or all of the visible light range, for example, a wavelength range of 400 nm to 700 nm, and the term "dichroic dye" refers to a substance that can anisotropically absorb light in at least a part or all of the visible light range.
[0069] The liquid crystal layer including the liquid crystal compound and the dichroic dye may be a GHLC layer (Guest Host Liquid Crystal Layer). In this specification, the term "GHLC layer (Guest Host Liquid Crystal Layer)" refers to a functional layer that is arranged with the dichroic dye by the arrangement of the liquid crystal compound and exhibits anisotropic light absorption characteristics in the alignment direction of the dichroic dye and in the direction perpendicular to the alignment direction. For example, the dichroic dye is a material whose light absorption rate changes depending on the polarization direction, and if it has a high absorption rate for light polarized in the long axis direction, it can be called a p-type dye, and if it has a high absorption rate for light polarized in the short axis direction, it can be called an n-type dye. In one example, when a p-type dye is used, polarized light vibrating in the long axis direction of the dye is absorbed, and polarized light vibrating in the short axis direction of the dye can be transmitted with little absorption. Hereinafter, unless otherwise specified, the dichroic dye is assumed to be a p-type dye.
[0070] As the dichroic dye, for example, a known dye that is known to have a property of being aligned according to the alignment state of the liquid crystal compound due to the so-called guest-host effect may be selected and used. Examples of such dichroic dyes include azo dyes, anthraquinone dyes, methine dyes, azomethine dyes, merocyanine dyes, naphthoquinone dyes, tetrazine dyes, phenylene dyes, chitalylene dyes, benzothiadiazole dyes, diketopyrrolopyrrole dyes, squaraine dyes, and pyromethene dyes, but the dyes applicable in the present application are not limited to the above.
[0071] The dichroic dye may have a dichroic ratio, i.e., the absorption of light polarized parallel to the long axis of the dichroic dye divided by the absorption of light polarized parallel to the direction perpendicular to the long axis, of 5 or more, 6 or more, or 7 or more. The dye may satisfy the dichroic ratio at least at some wavelengths or at any wavelength within the wavelength range of the visible light region, for example, within a wavelength range of about 380 nm to 700 nm or about 400 nm to 700 nm. The upper limit of the dichroic ratio may be, for example, about 20 or less, 18 or less, 16 or less, or 14 or less.
[0072] The content of the dichroic dye in the liquid crystal layer may be appropriately selected in consideration of the object of the present application. For example, the content of the dichroic dye in the liquid crystal layer may be 0.1 wt% or more, 0.25 wt% or more, 0.5 wt% or more, 0.75 wt% or more, 1 wt% or more, 1.25 wt% or more, or 1.5 wt% or more. The upper limit of the content of the dichroic dye in the liquid crystal layer may be, for example, 5.0 wt% or less, 4.0 wt% or less, 3.0 wt% or less, 2.75 wt% or less, 2.5 wt% or less, 2.25 wt% or less, 2.0 wt% or less, 1.75 wt% or less, or 1.5 wt% or less. When the content of the dichroic dye in the liquid crystal layer satisfies the above range, an optical device having excellent transmittance variable characteristics can be provided. In one example, the higher the content of the dichroic dye within the above range, the more excellent the transmittance variable characteristics can be provided.
[0073] The thickness of the liquid crystal layer is not particularly limited, and for example, the thickness of the liquid crystal layer may be about 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.5 μm or more, 1 μm or more, 1.5 μm or more, 2 μm or more, 2.5 μm or more, 3 μm or more, 3.5 μm or more, 4 μm or more, 4.5 μm or more, 5 μm or more, 5.5 μm or more, 6 μm or more, 6.5 μm or more, 7 μm or more, 7.5 μm or more, 8 μm or more, 8.5 μm or more, 9 μm or more, or 9.5 μm or more. The upper limit of the thickness of the liquid crystal layer is not particularly limited, and may generally be about 30 μm or less, 25 μm or less, 20 μm or less, or 15 μm or less.
[0074] The liquid crystal layer may be switched between a first alignment state and a second alignment state different from the first alignment state. The switching may be controlled by application of external energy such as a voltage. For example, the liquid crystal layer may be maintained in one of the first and second alignment states in the absence of an applied voltage, and may be switched to the other alignment state by application of a voltage.
[0075] Examples of the first alignment state and / or the second alignment state include a horizontal alignment state, a vertical alignment state, a twisted alignment state, an inclined alignment state, and a hybrid alignment state.
[0076] In this specification, the term "horizontal alignment state" refers to a state in which the directors of the liquid crystal compound in the liquid crystal layer are aligned approximately parallel to the plane of the liquid crystal layer, and for example, the angle that the directors of the liquid crystal compound make with respect to the plane of the liquid crystal layer can be, for example, within a range of approximately -10 degrees to 10 degrees or -5 degrees to 5 degrees, or can be approximately 0 degrees.
[0077] In this specification, the term "vertical alignment state" refers to a state in which the directors of the liquid crystal compound in the liquid crystal layer are aligned approximately perpendicular to the plane of the liquid crystal layer, and for example, the angle that the directors of the liquid crystal compound make with respect to the plane of the liquid crystal layer can be, for example, within a range of approximately 80 degrees to 100 degrees or 85 degrees to 95 degrees, or can be approximately 90 degrees.
[0078] In the present specification, the term "twisted alignment state" may refer to a helical structure in which directors of liquid crystal compounds are aligned in layers while twisting along a virtual helical axis in a liquid crystal layer. The twisted alignment state may be embodied as a vertical, horizontal, or tilted alignment state. That is, the vertical twist alignment mode is a state in which individual liquid crystal compounds are aligned vertically while twisting along a helical axis to form layers, the horizontal twist alignment mode is a state in which individual liquid crystal compounds are aligned horizontally while twisting along a helical axis to form layers, and the tilted twist alignment mode is a state in which individual liquid crystal compounds are aligned in a tilted state while twisting along a helical axis to form layers.
[0079] In the present specification, the term "inclined alignment state" may refer to an alignment state in which the tilt angle, which is the angle that the director of the liquid crystal compound in the liquid crystal layer makes with respect to the plane of the liquid crystal layer, deviates from the tilt angle of the horizontal alignment state and the tilt angle of the vertical alignment state. In the inclined alignment state, the tilt angle may be, for example, more than 10 degrees and less than 80 degrees. In the present specification, the term "hybrid alignment state" may refer to an alignment state in which the tilt angle, which is the angle that the director of the liquid crystal compound in the liquid crystal layer makes with respect to the plane of the liquid crystal layer, gradually increases or decreases along the thickness direction of the liquid crystal layer.
[0080] The liquid crystal element may further include a first electrode layer 10b formed on the inner surface of the first base layer 10a. In this case, the adhesive layer 10c may be present on the inner surface of the first electrode layer 10b. That is, the first electrode layer 10b may be present between the first base layer 10a and the adhesive layer 10c. The liquid crystal element may further include a second electrode layer 20b formed on the inner surface of the second base layer 20a. In this case, the spacer 20c may be present on the inner surface of the second electrode layer 20b. That is, the second electrode layer 20b may be present between the second base layer 20a and the spacer 20c.
[0081] The first electrode layer and the second electrode layer may serve to apply an external action, for example, application of an electric field, so that a material contained in the liquid crystal layer transmits or blocks incident light. In one example, the first electrode layer and / or the second electrode layer may include, but is not limited to, a conductive polymer, a conductive metal, a conductive nanowire, or a metal oxide such as ITO (Indium Tin Oxide). The upper and / or lower second electrode layers may be formed by depositing, for example, the conductive polymer, the conductive metal, the conductive nanowire, or a metal oxide such as ITO (Indium Tin Oxide).
[0082] The liquid crystal element may further include an alignment film 20d present on the inner surface of the second electrode layer 20b. The spacer 20c may be present between the second electrode layer 20b and the alignment film 20d. The alignment film may be formed on the spacer. That is, the upper surface and / or the side surface of the spacer may be in contact with the alignment film. The lower surface of the spacer may be in contact with the second electrode layer. Since the adhesive layer can have liquid crystal alignment properties, the inner surface of the first electrode layer may not include an alignment film.
[0083] In this specification, the combination of the first base layer, the first electrode layer, and the adhesive layer may be referred to as the upper substrate, and the combination of the second base layer, the second electrode layer, the spacer, and the alignment film may be referred to as the lower substrate. In the liquid crystal device, the upper substrate may not include a separate alignment film other than the adhesive layer, and the lower substrate may include an alignment film.
[0084] The alignment film and the liquid crystal layer may be in contact with each other. The alignment film may be a vertical alignment film or a horizontal alignment film. In this specification, the term "horizontal alignment film" may mean a layer containing an alignment material that imparts a horizontal alignment force to the liquid crystal compound present in the adjacent liquid crystal layer. In this specification, the term "vertical alignment film" may mean a layer containing an alignment material that imparts a vertical alignment force to the liquid crystal compound present in the adjacent liquid crystal layer. The pretilt angle of the adjacent liquid crystal compound relative to the vertical alignment film may be within a range of 80 degrees to 90 degrees, 85 degrees to 90 degrees, or about 87 degrees to 90 degrees, and the pretilt angle of the adjacent liquid crystal compound relative to the horizontal alignment film may be within a range of 0 degrees to 10 degrees, 0 degrees to 5 degrees, or 0 degrees to 3 degrees. Unlike the adhesive layer, the alignment film may not have an adhesive force that bonds the upper substrate and the lower substrate. In one example, the peel force of the alignment film relative to the upper substrate may be close to 0 in the state of the liquid crystal element of FIG. 2.
[0085] The alignment film may be a rubbing alignment film or a photo-alignment film. The alignment direction of the alignment film may be the rubbing direction in the case of a rubbing alignment film, and the direction of the irradiated polarized light in the case of a photo-alignment film, and such an alignment direction may be confirmed by a detection method using an absorbing linear polarizer. Specifically, the alignment direction may be confirmed by arranging an absorbing linear polarizer on one side of the liquid crystal layer in a state where the liquid crystal compound contained in the liquid crystal layer is horizontally aligned, and measuring the transmittance while rotating the polarizer 360 degrees. In the above state, when light is irradiated to the liquid crystal layer or the absorbing linear polarizer side and the brightness (transmittance) is measured on the other side, the transmittance tends to be low when the absorption axis or transmission axis coincides with the alignment direction of the liquid crystal alignment film, and the alignment direction may be confirmed through a simulation that reflects the refractive index anisotropy of the applied liquid crystal compound. A method for confirming the alignment direction depending on the mode of the liquid crystal layer is well known, and in this application, the alignment direction of the alignment film may be confirmed by such a well-known method.
[0086] The alignment film may be a known material that exhibits alignment ability by rubbing alignment, such as a polyimide compound, a poly(vinyl alcohol) compound, a poly(amic acid) compound, a polystyrene compound, a polyamide compound, or a polyoxyethylene compound; or a polyimide compound, a polyamic acid compound, a polynorbornene compound, a phenylmaleimide copolymer compound, a polyvinylcinamate compound, a polyazobenzene compound, a polyethyleneimide compound, a polyvinylalcohol compound, a polyamide compound, a polyethylene compound, a polystyrene compound, a polyphenylenephthalamide compound, a polyester compound, a CMPI (chloromethylated The material may include, but is not limited to, one or more selected from the group consisting of known substances that can exhibit alignment ability upon light irradiation, such as a polyimide compound, a PVCI (polyvinylcinnamate) compound, and a polymethylmethacrylate compound.
[0087] The spacers 20c may maintain the distance between the upper and lower substrates. A liquid crystal layer may be present between the upper and lower substrates in the areas where there are no spacers.
[0088] The spacer may be a patterned spacer. The spacer may have a column shape or a partition wall shape. The partition wall may divide the space between the lower substrate and the upper substrate into two or more spaces. In the area where the spacer is not present, other films or other layers present thereunder may be exposed. For example, the second electrode layer may be exposed in the area where the spacer is not present. The alignment film may cover the spacer and the second electrode layer exposed in the area where the spacer is not present. In a liquid crystal device in which the upper substrate and the lower substrate are bonded together, the alignment film present on the spacer of the lower substrate and the adhesive layer of the upper substrate may be in contact with each other.
[0089] In the region between the upper and lower substrates where no spacer is present, the liquid crystal compound and the above-mentioned additives, for example, dichroic dyes, chiral agents, etc., may be present. The shape of the spacer is not particularly limited, and may be applied without limitation to have multiple faces such as a circle, an ellipse, or other polygonal shapes.
[0090] The spacer may include a curable resin. The type of the curable resin is not particularly limited, and may be, for example, a thermosetting resin or a photocurable resin, such as an ultraviolet curable resin. As the thermosetting resin, for example, a silicone resin, a silicon resin, a furan resin, a polyurethane resin, an epoxy resin, an amino resin, a phenol resin, a urea resin, a polyester resin, or a melamine resin may be used, but is not limited thereto. As the ultraviolet curable resin, a representative acrylic polymer, for example, a polyester acrylate polymer, a polystyrene acrylate polymer, an epoxy acrylate polymer, a polyurethane acrylate polymer, or a polybutadiene acrylate polymer, a silicone acrylate polymer, or an alkyl acrylate polymer may be used, but is not limited thereto.
[0091] The spacer may be formed by a patterning process. For example, the spacer may be formed by a photolithography process. The photolithography process may include a process of applying a curable resin composition onto a substrate layer or an electrode layer, and then irradiating the curable resin composition with ultraviolet light through a pattern mask. The pattern mask may be patterned into an ultraviolet light transmitting region and an ultraviolet light blocking region. The photolithography process may further include a process of washing the curable resin composition irradiated with ultraviolet light. The region irradiated with ultraviolet light is cured, and the region not irradiated with ultraviolet light remains in a liquid state, so that the region is removed through a washing process to perform patterning into a partition wall shape. In the photolithography process, in order to easily separate the resin composition from the pattern mask after ultraviolet light irradiation, a release treatment may be performed on the pattern mask, or a release paper may be placed between the layer of the resin composition and the pattern mask.
[0092] The width (line width), interval (pitch), thickness, and area of the spacer may be appropriately selected within a range that does not impair the object of the present application. For example, the width (line width) of the spacer may be in the range of 10 μm to 500 μm, or in the range of 10 μm to 50 μm. The interval (pitch) of the spacer may be in the range of 10 μm to 1000 μm, or in the range of 100 μm to 1000 μm. The area of the spacer may be about 5% or more, or 50% or less, with respect to 100% of the total area of the second base layer. When the area of the spacer is within the above range, it can be advantageous to ensure excellent electro-optical characteristics while appropriately ensuring the adhesion between the upper substrate and the lower substrate. The thickness of the spacer may be, for example, in the range of 1 μm to 30 μm or 3 μm to 20 μm.
[0093] The optical device may include at least one intermediate layer located between the first outer substrate and the liquid crystal element, and may include at least one intermediate layer located between the second outer substrate and the liquid crystal element. Thus, the optical device may include at least two intermediate layers. One side of the first outer substrate and one side of the second outer substrate may be in contact with the adjacent intermediate layer, respectively. Both sides of the liquid crystal element may be in contact with the adjacent intermediate layer, respectively.
[0094] The number of intermediate layers in the optical device may be determined depending on whether the optical device further includes other elements other than the first outer substrate, the second outer substrate, and the liquid crystal element, such as a polarizer.
[0095] In one example, the optical device may further include other elements, such as a polarizer, in addition to the liquid crystal element between the first outer substrate and the second outer substrate. In this case, in one embodiment, the optical device may have a structure in which the first outer substrate, an intermediate layer, a liquid crystal element, an intermediate layer, a polarizer, an intermediate layer, and a second outer substrate are stacked in this order. In another embodiment, the optical device may have a structure in which the first outer substrate, an intermediate layer, a polarizer, an intermediate layer, a liquid crystal element, an intermediate layer, and a second outer substrate are stacked in this order. In yet another embodiment, the optical device may have a structure in which the first outer substrate, an intermediate layer, a polarizer, an intermediate layer, a liquid crystal element, an intermediate layer, a polarizer, an intermediate layer, and a second outer substrate are stacked in this order.
[0096] In another example, the optical device may not include any other elements, such as a polarizer, between the first outer substrate and the second outer substrate other than the liquid crystal element. In this case, the optical device may have a structure in which the first outer substrate, an intermediate layer, the liquid crystal element, an intermediate layer, and the second outer substrate are stacked in this order.
[0097] In order to overcome the physical limitations of the liquid crystal element, outer substrates can be bonded to both sides of the liquid crystal element via an intermediate layer, but due to the low modulus of the adhesive layer, it is vulnerable to external pressure, and defects such as cell gap collapse, liquid crystal flow, and concentration can occur during the bonding process. By controlling the thickness of the intermediate layer included in the optical device, the above defects can be minimized, and the structural stability and uniform appearance characteristics of the optical device can be ensured.
[0098] As an example, the at least one intermediate layer may have a sum of total thicknesses of 800 μm or more. The sum of total thicknesses of the at least one intermediate layer refers to the sum of thicknesses of all intermediate layers present between the first outer substrate and the liquid crystal element and between the second outer substrate and the liquid crystal element. When the total thickness of the intermediate layers is within the above range, defects during the bonding process of the outer substrates can be minimized, thereby ensuring structural stability and uniform appearance characteristics of the optical device. The sum of the total thicknesses of the at least one intermediate layer may be specifically 900 μm or more, 1,000 μm or more, 1,100 μm or more, 1,200 μm or more, 1,300 μm or more, 1,400 μm or more, 1,500 μm or more, 1,600 μm or more, 1,650 μm or more, 1,700 μm or more, 1,750 μm or more, 1,800 μm or more, 1,850 μm or more, 1,900 μm or more, 1,950 μm or more, 2,000 μm or more, 2,100 μm or more, 2,150 μm or more, or about 2,200 μm or more. The sum of the total thicknesses of the at least one or more intermediate layers may be, for example, about 6,000 μm or less, 5,900 μm or less, 5,800 μm or less, 5,700 μm or less, 5,600 μm or less, 5,500 μm or less, 5,400 μm or less, 5,300 μm or less, 5,200 μm or less, 5,100 μm or less, or about 5,000 μm or less. If the sum of the total thicknesses of the at least one or more intermediate layers is too thick, it may degrade electro-optical properties such as transmittance properties of an optical device, so it may be advantageous for it to be within the above range.
[0099] Each of the at least one intermediate layer may have a single layer structure of one intermediate layer, or may be a laminate of two or more sub-intermediate layers. The thickness and number of the sub-intermediate layers may be controlled in consideration of the desired thickness of the intermediate layer. In one example, the thickness of the sub-intermediate layer may be in the range of 100 μm to 500 μm or 300 μm to 400 μm.
[0100] For example, the total thickness Ta of the at least one intermediate layer between the first outer substrate and the liquid crystal element and the total thickness Tb of the at least one intermediate layer between the second outer substrate and the liquid crystal element may be about 400 μm or more, 500 μm or more, 600 μm or more, 700 μm or more, 800 μm or more, 900 μm or more, 1,000 μm or more, or about 3,000 μm or less, 2,900 μm or less, 2,800 μm or less, 2,700 μm or less, about 2,600 μm or less, about 2,500 μm or less, about 2,400 μm or less, or about 2,300 μm or less. When the thicknesses Ta and Tb are within the above ranges, it may be advantageous to ensure structural stability and uniform appearance characteristics without defects during the bonding process of the outer substrate without impairing the electro-optical characteristics of the optical device. The sum of the total thickness Ta of the at least one intermediate layer between the first outer substrate and the liquid crystal element means the sum of the thicknesses of all the intermediate layers between the first outer substrate and the liquid crystal element, and the sum of the total thickness Tb of the at least one intermediate layer between the second outer substrate and the liquid crystal element means the sum of the thicknesses of all the intermediate layers between the second outer substrate and the liquid crystal element.
[0101] As an example, a thickness ratio Ta / Tb of a total thickness Tb of at least one intermediate layer located between the second outer substrate and the liquid crystal element to a total thickness Ta of at least one intermediate layer located between the first outer substrate and the liquid crystal element may be within a range of 0.1 to 10. As another example, the thickness ratio Ta / Tb may be about 0.12 or more, about 0.13 or more, or about 0.14 or more, and may be about 9.5 or less, 9.0 or less, 8.5 or less, 8.0 or less, 7.5 or less, or about 7.0 or less. When the thickness ratio is within a range of 0.1 to 10, the appearance defect of the liquid crystal element can be improved more effectively.
[0102] As an example, the storage modulus of at least one intermediate layer may be 1 MPa or more. If the storage modulus of the intermediate layer is low, the substrate layer may not be able to withstand the stress of contraction or expansion in a high-temperature durability test or a cycle test, and the liquid crystal element may be damaged. The storage modulus of the intermediate layer may be 2 MPa or more or 4 MPa or more, or may be 100 MPa or less, 80 MPa or less, 60 MPa or less, 40 MPa or less, 20 MPa or less, 10 MPa or less, or 5 MPa or less. The storage modulus may be a value measured at a temperature of 25° C. and a frequency of 6 rad / sec.
[0103] For example, the at least one intermediate layer may have a Young's modulus (E) in the range of 0.1 MPa to 100 MPa. For another example, the Young's modulus E of the intermediate layer may be about 0.2 MPa or more, 0.4 MPa or more, 0.6 MPa or more, 0.8 MPa or more, 1 MPa or more, 5 MPa or more, or about 10 MPa or more, and may be about 95 MPa or less, 80 MPa or less, 75 MPa or less, 70 MPa or less, 65 MPa or less, 60 MPa or less, 55 MPa or less, or about 50 MPa or less. The Young's modulus E may be measured, for example, by a method specified in ASTM D882, and may be measured by cutting the film in a form provided in the standard and using equipment capable of measuring a stress-strain curve (capable of simultaneously measuring force and length), for example, a universal testing machine (UTM). When the Young's modulus of the intermediate layer included in the optical device is within the above range, it may be more advantageous to ensure excellent durability of the optical device. When the intermediate layer is a laminate of at least two or more sub-intermediate layers, each of the sub-intermediate layers can satisfy the above range of Young's modulus.
[0104] As an example, at least one or more intermediate layers may each have a coefficient of thermal expansion of 2,000 ppm / K or less, which in other examples may be about 1,900 ppm / K or less, 1,700 ppm / K or less, 1,600 ppm / K or less, or about 1,500 ppm / K or less, or about 10 ppm / K or more, 20 ppm / K or more, 30 ppm / K or more, 40 ppm / K or more, 50 ppm / K or more, 60 ppm / K or more, 70 ppm / K or more, 80 ppm / K or more, 90 ppm / K or more, 100 ppm / K or more, 200 ppm / K or more, 300 ppm / K or more, 400 ppm / K or more, 500 ppm / K or more, 600 ppm / K or more, 700 ppm / K or more, or about 800 ppm / K or more. The thermal expansion coefficient of the intermediate layer can be measured, for example, according to the ASTM D696 standard, by cutting into a shape provided in the standard, measuring the change in length per unit temperature, and calculating the thermal expansion coefficient, which can be measured by a known method such as TMA (ThermoMechanic Analysis). If the thermal expansion coefficient of the intermediate layer included in the optical device is within the above range, it can be more advantageous in ensuring excellent durability of the optical device. If the intermediate layer is a laminate of at least two or more sub-intermediate layers, each of the sub-intermediate layers can satisfy the above range of thermal expansion coefficient.
[0105] The at least one or more intermediate layers may be a thermoplastic polyurethane (TPU) adhesive layer, a polyamide adhesive layer, a polyester adhesive layer, an EVA (Ethylene Vinyl Acetate) adhesive layer, an acrylic adhesive layer, a silicone adhesive layer, or a polyolefin adhesive layer. According to one embodiment of the present application, the at least one or more intermediate layers may be a thermoplastic polyurethane.
[0106] In the optical device, the outer layer may surround the side of the liquid crystal element. In the optical device, the upper area of the liquid crystal element may be smaller than the upper area of the first outer substrate or the second outer substrate. Also, the upper area of the liquid crystal element may be smaller than the upper area of at least one intermediate layer included in the optical device. In one example, the liquid crystal element may be encapsulated by an intermediate layer located between the first outer substrate and the liquid crystal element, an intermediate layer located between the second outer substrate and the liquid crystal element, and the outer shell layer. In this specification, the term "encapsulation" may mean covering the entire surface of the liquid crystal element with the intermediate layer and the outer shell layer. Depending on the desired structure, for example, the encapsulation structure can be realized by a method of vacuum-pressing a laminate including a first outer substrate, an intermediate layer, a liquid crystal element, an intermediate layer, and a second outer substrate in sequence, and an outer shell layer surrounding the side of the liquid crystal element. Such an encapsulation structure significantly improves the durability and weather resistance of the optical device, and as a result, it can be stably applied to outdoor applications such as sunroofs.
[0107] The outer layer may include, for example, a polymer film. In one example, the outer layer may be composed of one polymer film. In another example, the outer layer may be a laminate of two or more polymer films. In the case of a laminate of two or more polymer films, it may further include an adhesive layer to which the two or more polymer films are attached. The structure of the outer layer may be appropriately selected within a range that can ensure the desired thickness and storage modulus.
[0108] As the polymer film, an appropriate polymer film may be used within a range that satisfies the storage modulus of formula 1. As the polymer film, for example, a PC (polycarbonate) film, a PE (polyethylene) film, a TPU (thermoplastic polyurethane), a COP (cycloolefin copolymer) film, a POE (polyolefin, elastomer) film, an EVA (ethylene vinyl acetate) film, etc. may be used.
[0109] The present application further relates to a method for manufacturing an optical device. The method for manufacturing the optical device may include the steps of preparing a laminate including, in order, a first outer substrate, at least one intermediate layer, a liquid crystal element, at least one intermediate layer, and a second outer substrate, and autoclaving the laminate. Unless otherwise specified, the same applies to the method for manufacturing the optical device.
[0110] The laminate may further include an outer layer surrounding a side surface of the liquid crystal element.
[0111] When the optical device further includes an element other than the liquid crystal element, for example a polarizer, the laminate may further include the element other than the liquid crystal element at a desired position.
[0112] The autoclaving step may be performed by applying heat and / or pressure to the laminate formed after the lamination step.
[0113] The conditions of the autoclave process are not particularly limited, and may be performed under appropriate temperature and pressure depending on the type of intermediate layer applied. The temperature of the typical autoclave process is about 80°C or more, 90°C or more, or 100°C or more, and the pressure is 2 atm or more, but is not limited thereto. The upper limit of the process temperature may be about 200°C or less, 190°C or less, 180°C or less, or 170°C or less, and the upper limit of the process pressure may be about 10 atm or less, 9 atm or less, 8 atm or less, 7 atm or less, or 6 atm or less.
[0114] The optical device may be used for various purposes, for example, in eyewear such as sunglasses, AR (Argumented Reality) or VR (Virtual Reality) eyewear, building exterior walls, vehicle sunroofs, etc. In one example, the optical device may be a vehicle sunroof itself. For example, the optical device or vehicle sunroof may be attached to at least one opening in an automobile including a body having the opening. Effect of the Invention
[0115] The optical device of the present application can properly maintain the cell gap of the liquid crystal element, have excellent adhesion between the upper and lower substrates, minimize defects such as pressing and concentration, and ensure structural stability and good quality uniformity. [Brief description of the drawings]
[0116] [Figure 1] 1 is a cross-sectional view of an exemplary optical device of the present application. [Diagram 2] 1 is a cross-sectional view of an exemplary optical device of the present application. [Diagram 3] FIG. 2 is a cross-sectional view of an exemplary liquid crystal element of the present application. [Figure 4] 1 is a photograph of the optical device of Comparative Example 1. [Figure 5(A)] 1 is a microscope image of Comparative Example 1. [Figure 5(B)] 1 is a microscope image of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0117] Hereinafter, the present application will be described in detail with reference to examples, but the scope of the present application is not limited to the following examples.
[0118] Measurement example 1. Storage modulus measurement The storage modulus was measured using a DMA Q800 manufactured by TA Corp. Specifically, the storage modulus was recorded in Multi-Frequency-Strain mode under the conditions of a temperature of 25°C, a frequency of 6rad / sec, a force of 0.01N, and a ramp rate of 3° / min.
[0119] Example 1 Liquid crystal element manufacturing A PET film with a thickness of about 145 μm and a horizontal x vertical area of 900 mm x 600 mm was prepared as the first base layer. ITO (indium-tin-oxide) was evaporated to a thickness of 50 nm on the first base layer to form a first electrode layer. An adhesive composition (KR-3700, Shin-Etsu) was bar-coated on the first electrode layer, and then dried at about 150° C. for about 5 minutes to form an adhesive layer with a thickness of about 10 μm. The storage modulus of the adhesive layer was about 0.1 MPa. The combination of the first base layer, the first electrode layer, and the adhesive layer is called the upper substrate.
[0120] As the second base layer, a PET film with a thickness of about 145 μm and a horizontal x vertical area of 900 mm x 600 mm was prepared. ITO (indium-tin-oxide) was vapor-deposited on the second base layer to a thickness of 50 nm to form a second electrode layer. An acrylic resin composition (KAD-03, Minutec) was coated on the second electrode layer, and then a honeycomb-type spacer (partition-type spacer) was formed by photolithography. The regular hexagons (closed hexagons) constituting the honeycomb had a pitch of about 450 μm, a height of about 6 μm, and a line width of about 30 μm. The area of the closed hexagons (regular hexagons) formed by the partition-type spacers was about 2.14 mm 2 A vertical alignment film (5661, Nissan Chemical) was coated on the spacer to a thickness of about 300 nm, and then rubbed in one direction. The combination of the second base layer, the second electrode layer, the spacer, and the vertical alignment film was called the lower substrate.
[0121] A liquid crystal composition was coated on the vertical alignment film of the lower substrate to form a liquid crystal layer, and then the adhesive layer of the upper substrate was laminated facing the liquid crystal composition coating surface. The liquid crystal composition contained a liquid crystal compound (T12, JNC) and a chiral dopant (S811, HCCH), and the pitch p of the formed liquid crystal layer was about 20 μm, and the ratio d / p of the cell gap d to the pitch p was about 0.3. The liquid crystal element was an RTN mode liquid crystal cell that was in a vertical alignment state when no voltage was applied. The total thickness of the liquid crystal element was about 306 μm.
[0122] Optical Device Manufacturing A laminate including an outer layer surrounding the side of the liquid crystal element was prepared, which sequentially included a first outer substrate, a first intermediate layer, a first polarizer, a second intermediate layer, the manufactured liquid crystal element, a third intermediate layer, a second polarizer, a fourth intermediate layer, and a second outer substrate. The second outer substrate was disposed in the direction of gravity relative to the first outer substrate.
[0123] The first outer substrate was a glass substrate having a thickness of about 3 mm, an area of 1100 mm x 800 mm, and a radius of curvature of about 2,470R. The second outer substrate was a glass substrate having a thickness of about 3 mm, an area of 1100 mm x 800 mm, and a radius of curvature of about 2,400R. The first polarizer and the second polarizer were PVA polarizers, and the light transmission axis of the first polarizer and the light transmission axis of the second polarizer were arranged to form an angle of about 90 degrees. The first intermediate layer and the fourth intermediate layer were each a single layer of TPU layer (Argotec) with a thickness of 380 μm. The second intermediate layer and the third intermediate layer were each a laminate of three TPU layers (Argotec) with a thickness of 380 μm. The thermal expansion coefficient of the TPU layer (Argotec) used to form the first to fourth intermediate layers was 307 ppm / K and the storage modulus was 2.18 MPa. As the outer layer, a PC film (Keiwa) with a storage modulus of 2000 MPa and a thickness of 300 μm was used.
[0124] The laminate was subjected to an autoclave process at a temperature of about 110° C. and a pressure of about 2 atm to manufacture an optical device having the structure shown in FIG.
[0125] Example 2 An optical device was manufactured by carrying out the same process as in Example 1, except that a laminate was used in which two PET films, each having a storage modulus in the MD direction of about 6,000 MPa and a storage modulus in the TD direction of about 3,000 MPa and a thickness of 145 μm, were attached via a pressure-sensitive adhesive layer (KR-3700, Shin-Etsu Co., Ltd.) having a storage modulus of about 0.1 MPa and a thickness of 10 μm, for the outer layer. In Example 2, the total thickness of the outer layer was about 300 μm.
[0126] Example 3 An optical device was manufactured by carrying out the same process as in Example 1, except that a TPU film (Argotec) having a storage modulus of about 100 MPa and a thickness of about 380 μm was used for the outer layer.
[0127] Comparative Example 1 An optical device was manufactured by carrying out the same process as in Example 1, except that a TPU film (Argotec) having a storage modulus of about 100 MPa and a thickness of about 150 μm was used for the outer layer.
[0128] Comparative Example 2 An optical device was manufactured by carrying out the same process as in Example 1, except that a laminate of a TPU film (Argotec) having a storage modulus of about 100 MPa and a thickness of about 380 μm and a TPU film (Argotec) having a storage modulus of about 100 MPa and a thickness of about 150 μm was used for the outer layer. In Comparative Example 2, the total thickness of the outer layer was about 530 μm.
[0129] Evaluation example 1. Evaluation of defective bonding process The optical devices manufactured in Example 1 and Comparative Example 1 were observed to see whether or not pressing and concentration defects occurred when no voltage was applied. In Example 1, pressing and concentration defects were not observed, but pressing and concentration defects were observed in Comparative Example 1 as shown in Figs. 4 and 5. Fig. 4 is a camera photograph of the optical device of Comparative Example 1, and Fig. 5 is a microscope image of the optical device of Comparative Example 1. As shown in red in Fig. 4 (left side), in the case of the concentration defect area, the concentration of the dichroic dye is higher than that of the surrounding area, so it appears darker than the surrounding area, and as shown in green in Fig. 4 (right side), in the case of the pressing defect area, the concentration of the dichroic dye is lower than that of the surrounding area, so it appears brighter than the surrounding area. In Comparative Example 2, the glass substrate was damaged during the bonding process. Fig. 5(A) shows pressing defects in Comparative Example 1, and Fig. 5(B) shows concentration defects in Comparative Example 1. [Explanation of symbols]
[0130] 100a: First outer substrate 100b: second outer substrate 200a, 200b, 200c, 200d: Middle layer 300: Liquid crystal element 400: Outer layer 500a: First polarizer 500b: Second polarizer 10a: First base layer 10b: First electrode layer 10c:Adhesive layer 20a: second substrate layer 20b: second electrode layer 20c: Spacer 20d: Alignment film
Claims
1. A liquid crystal display device comprising a first outer substrate, a second outer substrate arranged opposite the first outer substrate, a liquid crystal element between the first outer substrate and the second outer substrate, an outer layer surrounding a side surface of the liquid crystal element, and at least one intermediate layer located between the first outer substrate and the liquid crystal element and between the liquid crystal element and the second outer substrate, The liquid crystal element includes a first base material layer, a first electrode layer formed on an inner surface of the first base material layer, a pressure-sensitive adhesive layer present on the inner surface of the first base material layer, a second base material layer disposed opposite to the first base material layer, a second electrode layer formed on the inner surface of the second base material layer, a spacer present on the inner surface of the second base material layer, and a liquid crystal layer located between the first base material layer and the second base material layer, Satisfying the following formula 1 and the following formula 2, [Formula 1] −T2×0.4≦T1−T2≦T2×0.4 In Equation 1, T1 is the thickness of the outer layer, and T2 is the thickness of the liquid crystal element; [Formula 2] G1 ≧ G2 In Equation 2, G1 is the storage modulus of the outer layer at a temperature of 25° C. and a frequency of 6 rad / sec, and G2 is the storage modulus of the pressure-sensitive adhesive layer at a temperature of 25° C. and a frequency of 6 rad / sec.
2. The optical device according to claim 1 , wherein the thickness T1 of the outer layer is in the range of 60 μm to 840 μm.
3. 3. The optical device according to claim 1, wherein the difference (G1-G2) between the storage modulus G1 of the outer layer and the storage modulus G2 of the adhesive layer is in the range of 0 MPa to 9999.99 MPa.
4. 4. The optical device according to claim 1, wherein the outer layer has a storage modulus G1 at 25° C. in the range of 0.1 MPa to 10,000 MPa.
5. The optical device of claim 1 , wherein the outer layer comprises a polymer film.
6. The optical device according to claim 1 , wherein the liquid crystal layer is switched between a first alignment state and an alignment state different from the first alignment state through application of external energy.
7. The optical device of claim 1 , wherein the spacer is a patterned spacer that maintains a spacing between the first and second substrate layers.
8. 8. The optical device according to claim 1, wherein a ratio B / A of an area B of the spacer to an area A of the second base layer is within a range of 5% to 50%.
9. The optical device according to claim 1 , wherein the liquid crystal element further includes an alignment film present on an inner surface of the second electrode layer, and the inner surface of the first base material layer does not include an alignment film.
10. 10. The optical device of claim 1, wherein the liquid crystal element is encapsulated by the intermediate layer and the outer layer.
11. The optical device according to claim 1 , wherein the sum of the total thicknesses of the at least one intermediate layer is 800 μm or more.
12. 12. The optical device of claim 1, wherein the at least one or more intermediate layers are a thermoplastic polyurethane adhesive layer, a polyamide adhesive layer, a polyester adhesive layer, an EVA (Ethylene Vinyl Acetate) adhesive layer, an acrylic adhesive layer, a silicone adhesive layer, or a polyolefin adhesive layer.
13. 13. A motor vehicle comprising a body having one or more openings formed therein, and an optical device according to any one of claims 1 to 12 attached to said openings.
Citation Information
Patent Citations
Liquid crystal element and its production
JP1995020479A
Liquid crystal display element and its production
JP1998301115A
display element
JP2018507443A
Method for production of glass laminate
JP2020007182A