Optical film and its manufacturing method

A cesium-tungsten composite oxide optical film addresses aesthetic and functional issues by ensuring transparency and radio wave penetration while minimizing near-infrared absorption, thus reducing thermal stress and energy consumption.

JP7585638B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020121550
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-15
Publication Date
2024-11-19
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

Existing window materials with heat ray shielding properties face issues such as aesthetic problems due to mirror-like reflections, interference with radio wave penetration, and thermal cracking from near-infrared absorption, making them unsuitable for widespread use.

Method used

A semi-reflective optical film composed of cesium-tungsten composite oxide with specific refractive index and extinction coefficient ranges is formed using a sputtering method, incorporating a surface layer and an inner layer to achieve transparency in the visible range and radio waves while minimizing near-infrared absorption.

Benefits of technology

The film provides a semi-reflective heat ray shielding solution that prevents thermal cracking and maintains radio wave transparency, reducing energy consumption by suppressing near-infrared absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585638000016
    Figure 0007585638000016
  • Figure 0007585638000017
    Figure 0007585638000017
  • Figure 0007585638000018
    Figure 0007585638000018
Patent Text Reader

Abstract

To provide a semi-reflective optical film which has a transmittance in a visible wavelength region and a radio wave transmittance, and whose absorptivity in a near-infrared wavelength region is suppressed, and to provide a manufacturing method therefor.SOLUTION: An optical film, which is formed on a base material 100 and composed of cesium-tungsten composite oxide, consists of: a surface layer 101 with a thickness of 20 to 60 nm located on the surface side, and an internal layer 102 located on the base material 100 side. A refractive index n and an extinction coefficient k of the surface layer 101 are set in a specific value range (a high extinction coefficient k in a near-infrared wavelength region) while the refractive index n and the extinction coefficient k of the internal layer 102 are set in a specific value range (a low extinction coefficient k in a near-infrared wavelength region). As a resulting effect, the base material 100 can be protected from heat cracks and the like by suppressing absorptivity in a near-infrared wavelength region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film that is transparent in the visible wavelength range, reflective in the near-infrared wavelength range, and radio wave transparent, and a manufacturing method thereof, and in particular to an optical film formed by a sputtering method and an improvement in the manufacturing method thereof. [Background technology]

[0002] In recent years, in order to reduce the energy consumption of air conditioners indoors and in vehicles such as cars during the summer, there has been progress in the development of heat shielding technology for window materials that let in outside light. Known technical means include attaching a colored film with heat shielding effect or a film with an optical film formed thereon (light-shielding material) to the window, coating the window with a substance with heat shielding effect, and using window materials on which an optical film with heat shielding effect is formed by sputtering.

[0003] For example, as the light-shielding member, Patent Document 1 describes a film (light-shielding member) having a mirror-like surface formed by vapor deposition of a metal film such as aluminum. However, when such a light-shielding member is used, the appearance becomes half-mirror-like, and the reflected light is too bright for outdoor use, which causes a problem in terms of scenery. In addition, metal films such as aluminum have high conductivity and therefore reflect radio waves (i.e., they interfere with radio wave transmission), which causes a problem that devices that use radio waves, such as mobile phones, smartphones, and devices using GPS (Global Positioning System), have difficulty connecting.

[0004] In addition, as the above-mentioned method of applying a substance having a heat ray shielding effect, the present applicant has proposed an infrared shielding microparticle dispersion having composite tungsten oxide microparticles described in Patent Document 2. Composite tungsten oxide microparticles efficiently absorb sunlight, particularly light in the near infrared region, and in addition have high transparency to visible light. The above-mentioned infrared shielding microparticle dispersion is prepared by dispersing composite tungsten oxide microparticles in an appropriate solvent to obtain a dispersion liquid, adding a medium resin to the obtained dispersion liquid, and then coating the surface of a substrate to form a thin film, and has both heat ray shielding properties and radio wave transmittance. However, the method described in Patent Document 2 has a problem that the light absorbed by the composite tungsten oxide microparticles is converted into heat to heat the substrate, since the composite tungsten oxide microparticles shield heat rays by absorbing light in the near infrared region. Furthermore, since the thin film is formed by a coating method, there is a problem that an advanced coating technique is required to control the film thickness and ensure the uniformity and flatness of the film thickness over a large area.

[0005] In the above method using a window material in which an optical film having a heat ray shielding effect is formed by a sputtering method, if the optical film contains a metal layer, it will hinder radio wave transmission. Therefore, a multilayer film having visible wavelength transmission, near-infrared wavelength blocking, and radio wave transmission can be designed by repeatedly stacking high refractive index films (TiO2, Ta2O5, Nb2O5) and low refractive index films (SiO2, MgF2, ZrO2) using only transparent dielectric materials (SiO2, MgF2, ZrO2, etc.). However, to achieve this, at least several tens to hundreds of film layers and accurate film thickness control are required. For example, Patent Document 3 discloses a technology related to an infrared cut filter for digital still cameras. However, it is difficult to adopt the method of Patent Document 3 for a window material that is not an optical component that constitutes an expensive optical device in terms of cost.

[0006] It is possible to significantly reduce the number of film layers by using a multilayer film having an optical constant with a small extinction coefficient in the visible wavelength range and a large extinction coefficient in the near-infrared wavelength range, instead of the multilayer film in which the high refractive index film (TiO2, Ta2O5, etc.) and the low refractive index film (SiO2, MgF2, etc.) are repeatedly laminated. However, when the multilayer film having an optical constant with a large extinction coefficient in the near-infrared wavelength range is used, there is a concern that the substrate (e.g., glass) may be heated by the heat rays absorbed by the multilayer film, causing thermal cracking of the substrate.

[0007] For this reason, there is a demand for the development of a semi-reflective heat ray shielding film that has transparency in the visible wavelength range and radio wave transparency while suppressing absorption in the near-infrared wavelength range. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 5-113085 [Patent Document 2] Patent No. 4096205 [Patent Document 3] JP 2016-070965 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in consideration of these problems, and an object of the present invention is to provide a semi-reflective optical film that has transparency in the visible wavelength range and radio wave transparency while suppressing absorption in the near-infrared wavelength range, and a method for manufacturing the same. [Means for solving the problem]

[0010] Therefore, in order to solve the above problems, the present inventors conducted intensive research and discovered that when an optical film formed on a substrate is made of a cesium tungsten composite oxide and the refractive index n and extinction coefficient k of at least the front surface side of the optical film are set within a specific numerical range (the extinction coefficient k in the near-infrared wavelength range is large), it is possible to achieve a semi-reflective heat ray shielding film that has radio wave transmittance and light transmittance in the visible wavelength range, and also has suppressed absorbance in the near-infrared wavelength range.

[0011] The present invention was completed based on these technical discoveries.

[0012] That is, the first invention according to the present invention is: In an optical coating formed on a substrate and made of a cesium tungsten composite oxide containing cesium, tungsten, and oxygen, The optical film is composed of a surface layer having a thickness of 20 nm to 60 nm located on the surface side and an internal layer located on the substrate side, The above surface layer The refractive index n and extinction coefficient k are set within the numerical ranges in Table 1 below. And,

[0013] [Table 1] The refractive index n and extinction coefficient k of the inner layer are set within the numerical ranges shown in Table 2 below, [Table 2] In the table, "nm" means the wavelength, "n-min and n-max" mean the minimum and maximum values ​​of the refractive index n at each wavelength, and "k-min and k-max" mean the minimum and maximum values ​​of the extinction coefficient k at each wavelength (this also applies to other tables except Table 11). 、

[0014] The second invention is In the optical film according to the first aspect of the present invention, The optical film has a thickness of 300 nm to 560 nm, and has an average transmittance of 45% or more in the wavelength range of 400 nm to 550 nm, and a reflectance of 40% or more at a wavelength of 2000 nm. do .

[0016] Next, the first aspect of the present invention 3 The invention is No. 1 In the method for producing an optical film according to the present invention, a deposition process in which a sputtering target consisting of cesium atoms, tungsten atoms, and oxygen is used, and the oxygen partial pressure in the sputtering deposition atmosphere is feedback-controlled while controlling the heating temperature of the substrate to deposit a cesium tungsten composite oxide film on the substrate, the refractive index n and the extinction coefficient k of which are set within the numerical ranges shown in Table 3 below;

[0017] [Table 3]

[0018] an annealing process for annealing the formed cesium tungsten composite oxide film to form a surface layer on the surface side of the cesium tungsten composite oxide film, the refractive index n and extinction coefficient k of which are set within the numerical ranges shown in Table 4 below, and to make the substrate side portion of the cesium tungsten composite oxide film excluding the surface layer into an internal layer, the refractive index n and extinction coefficient k of which are set within the numerical ranges shown in Table 3 above; The present invention is characterized by comprising:

[0019] [Table 4]

[0020] The present invention also relates to the first 4 The invention is No. 3 In the method for producing an optical film according to the present invention, The annealing step is carried out at a temperature of 300° C. or higher in an oxygen-free atmosphere; No. 5 The invention is No. 3 The invention or 4 In the method for producing an optical film according to the present invention, The ratio of cesium atoms to tungsten atoms (Cs:W) of the sputtering target is 1:2 to 1:4; No. 6 The invention is No. 3 The invention or 4 In the method for producing an optical film according to the present invention, The film forming step is performed by a dual sputtering method using a cesium source sputtering target and a tungsten source sputtering target, and the oxygen partial pressure in the dual sputtering film forming atmosphere is feedback controlled to adjust the power or duty ratio applied to the sputtering cathode so that the ratio of cesium atoms to tungsten atoms (Cs:W) contained in the cesium tungsten composite oxide film is 1:2 to 1:4; No. 7 The invention is No. 3 Invention of 6 In any one of the above-mentioned methods for producing an optical film, The feedback control of the oxygen partial pressure is performed by an impedance controller that feedback controls an impedance change during the film formation, Also, 8 The invention is No. 3 Invention of 6 In any one of the above-mentioned methods for producing an optical film, The feedback control of the oxygen partial pressure is performed by a plasma emission monitor which measures the emission intensity of a specific wavelength during the film formation and feedback controls the oxygen partial pressure. Effect of the Invention

[0021] Optical film according to the present invention teeth , It is composed of a surface layer with a thickness of 20 nm to 60 nm located on the surface side and an internal layer located on the substrate side, and The refractive index n and the extinction coefficient k are set within the numerical ranges in Table 1 above. and the refractive index n and extinction coefficient k of the inner layer are set within the numerical ranges in Table 2 above. Therefore, it is possible to obtain a semi-reflective heat ray shielding film that has radio wave transmittance and light transmittance in the visible wavelength range, while suppressing absorption in the near-infrared wavelength range.

[0022] This has the effect of preventing thermal cracking of the base material on which the optical film is formed. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is a diagram illustrating the configuration of an optical film according to the present invention. [Diagram 2] FIG. 11 is a graph showing the spectral optical characteristics (wavelength and transmittance) of the optical film according to Example 5. [Diagram 3] FIG. 11 is a graph showing the spectral optical characteristics (wavelength and reflectance) of the optical film according to Example 5. [Figure 4] 13 is a graph showing the spectral optical characteristics (wavelength and reflectance) of the optical film according to Comparative Example 5. FIG. [Diagram 5] FIG. 5(A) is an explanatory diagram of a cesium tungsten composite oxide film formed on a substrate in the film formation step of the manufacturing method of the present invention, and FIG. 5(B) is an explanatory diagram of a surface layer and an internal layer formed in the cesium tungsten composite oxide film in the annealing step of the manufacturing method of the present invention. [Figure 6] FIG. [Figure 7] FIG. 1 is a schematic perspective view of a cylindrical target (rotary target). [Figure 8] FIG. 1 is a diagram illustrating the configuration of a sputtering apparatus equipped with a flat target. [Figure 9] FIG. 2 is an explanatory diagram showing the positional relationship between a substrate, which is an object to be coated, and a rotary target. [Figure 10] FIG. 2 is a diagram illustrating the configuration of a sputtering deposition unit A. [Figure 11] FIG. 2 is an explanatory diagram showing the positional relationship between a substrate and a rotary target in a dual-target sputtering method. [Figure 12] FIG. 2 is a diagram illustrating the configuration of a sputtering film-forming unit B for a dual-target sputtering method. [Figure 13] FIG. 2 is a diagram illustrating the configuration of a sputtering film-forming unit C according to a dual target sputtering method. [Figure 14] 1 is a graph showing the spectral optical characteristics (wavelength and transmittance) of the optical films according to Examples 4 to 6 and Comparative Example 5. FIG. [Figure 15]FIG. 1 is a graph showing the spectral optical characteristics (wavelength and reflectance) of the optical films according to Examples 4 to 6 and Comparative Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] Hereinafter, an embodiment of the present invention will be described in detail.

[0025] In the present invention, a composite tungsten oxide film containing cesium, tungsten, and oxygen and having a heat ray shielding effect is used, which makes it possible to significantly reduce the number of film layers compared to the case where a dielectric multilayer film that is transparent from the visible wavelength region to the near infrared wavelength region is used.

[0026] (1) optical film The optical film according to the present invention contains cesium (alkali metal), tungsten, and oxygen.

[0027] The applicant's technology for infrared shielding using composite tungsten oxide particles is shown in detail in the above Patent Document 2, and it is necessary to use a composite tungsten oxide in this composition range as the main component in order to obtain a film with high transparency in the visible wavelength range and absorption in the near-infrared wavelength range. The basic optical properties of the composite tungsten oxide film are derived from the theoretically calculated element M (M is one or more elements selected from H, He, alkali metals, alkaline earth metals, rare earth elements, Mg, Zr, Cr, Mn, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, Cd, Al, Ga, In, Tl, Si, Ge, Sn, Pb, Sb, B, F, P, S, Se, Br, Te, Ti, Nb, V, Mo, Ta, Re, Be, Hf, Os, Bi, and I), and the atomic arrangement of tungsten W and oxygen O. Specifically, when the composite tungsten oxide microparticles have a hexagonal crystal structure, the microparticles have improved transmission in the visible light region and improved absorption in the near infrared region. The composite tungsten oxide microparticles may be crystalline or amorphous.

[0028] When the composite tungsten oxide fine particles having a hexagonal crystal structure have a uniform crystal structure, the amount of the additive element M is preferably 0.2 to 0.5, more preferably 0.33, relative to 1 tungsten. 0.33 It is believed that by forming WO3, the added element M is placed in all of the hexagonal voids.

[0029] However, when the composite tungsten oxide film described in Patent Document 2, which has absorptivity in the near-infrared wavelength range, or a multilayer film having an optical constant with a large extinction coefficient in the near-infrared wavelength range is used, there is a problem that the light absorbed by these films is converted into heat, heating the substrate.

[0030] Therefore, an object of the present invention is to provide a semi-reflective optical film that has transparency in the visible wavelength range and radio wave transparency while suppressing absorption in the near-infrared wavelength range, and a method for manufacturing the same.

[0031] That is, the present invention provides In an optical coating formed on a substrate and made of a cesium tungsten composite oxide containing cesium, tungsten, and oxygen, The optical film is composed of a surface layer having a thickness of 20 nm to 60 nm located on the surface side and an internal layer located on the substrate side, the above surface layer The refractive index n and extinction coefficient k are within the numerical ranges in Table 5 below. It is set,

[0032] [Table 5] In addition, the refractive index n and extinction coefficient k of the inner layer are set within the numerical ranges shown in Table 6 below.

[0033] According to the optical film of the present invention, The above surface layer Since the refractive index n and the extinction coefficient k are set within the numerical ranges shown in Table 5, it is possible to form a semi-reflective heat-shielding film that has radio wave transmittance and light transmittance in the visible wavelength range, and also has reduced absorbance in the near-infrared wavelength range.

[0035] (1B) Optical film with a thickness of 300nm to 560nm, consisting of a surface layer and an internal layer Optical film according to the present invention teeth The refractive index n and extinction coefficient k of the surface layer 101 are set within the numerical ranges shown in Table 5 above, and the refractive index n and extinction coefficient k of the internal layer 102 are set within the numerical ranges shown in Table 6 below. For The thickness of the surface layer 101 is such that it has optical transparency in the visible wavelength range and suppresses heat generation associated with absorption in the near-infrared wavelength range, and at the same time, a part of the light in the near-infrared wavelength range is reflected at the interface between the surface layer 101 and the inner layer 102, so that a semi-reflective heat ray shielding film can be formed, and radio wave transparency [sheet resistance is 10 4 It is also possible to provide a resistance of Ω / □ (ohms per square) or more.

[0036] [Table 6]

[0037] The surface layer 101 and internal layer 102 of the optical film shown in FIG. 1 are optically different, and ellipsometer analysis of the optical film in the depth direction has revealed that the optical constants of the refractive index n and extinction coefficient k of the surface layer 101 and the internal layer 102 are different (the refractive index n and extinction coefficient k of the surface layer 101 are set within the numerical ranges in Table 5 above, and the refractive index n and extinction coefficient k of the internal layer 102 are set within the numerical ranges in Table 6 above).

[0038] The reason why the optical constants of the surface layer 101 and the internal layer 102 of the optical film are different is due to the manufacturing method of the optical film according to the present invention. That is, the reduction of the surface layer 101 and the like progresses during the annealing treatment after the formation of the cesium tungsten composite oxide film on the substrate, and the chemical state of the surface layer 101 changes.

[0039] If the annealing time is long, the reduction progresses to the inside, and the thickness of the surface layer 101 becomes thick. If the thickness of the surface layer 101 is less than 20 nm, the annealing process for obtaining the optical film according to the present invention is insufficient, and it becomes difficult to set the refractive index n and extinction coefficient k of the surface layer 101 within the numerical ranges in Table 5 above. On the other hand, if the thickness of the surface layer 101 exceeds 60 nm, the transmittance in the visible light region decreases. For this reason, the thickness of the surface layer 101 is preferably 20 nm to 60 nm.

[0040] The graphs in Figures 2 and 3 show the spectral optical characteristics (wavelength and transmittance) and the spectral optical characteristics (wavelength and reflectance) of the optical film of Example 5 having a thickness of 440 nm and consisting of a surface layer having a thickness of 40 nm and an internal layer having a thickness of 400 nm. From the graphs in Figures 2 and 3, it is confirmed that a semi-reflective heat ray shielding film is formed, with an average transmittance of 45% or more in the wavelength range of 400 nm to 550 nm and a reflectance of 40% or more at a wavelength of 2000 nm.

[0041] (1C) Method for manufacturing optical film The method for producing an optical film according to the present invention, which is composed of a surface layer and an internal layer, comprises the steps of: a deposition process in which a sputtering target consisting of cesium atoms, tungsten atoms, and oxygen is used, and the oxygen partial pressure in the sputtering deposition atmosphere is feedback-controlled while controlling the heating temperature of the substrate to deposit a cesium tungsten composite oxide film on the substrate, the refractive index n and the extinction coefficient k of which are set within the numerical ranges shown in Table 7 below;

[0042] [Table 7]

[0043] An annealing process of annealing the formed cesium tungsten composite oxide film to form a surface layer on the surface side of the cesium tungsten composite oxide film, the refractive index n and the extinction coefficient k of which are set within the numerical ranges in Table 8 below, and to make the substrate side portion of the cesium tungsten composite oxide film excluding the surface layer into an internal layer, the refractive index n and the extinction coefficient k of which are set within the numerical ranges in Table 7 above; The present invention is characterized in that it comprises:

[0044] [Table 8]

[0045] The annealing treatment is preferably performed at a temperature of 300°C or higher in an oxygen-free atmosphere that does not contain oxygen, and the annealing treatment can be performed using an electric furnace or the like that can control the atmosphere and temperature. Figure 5 shows the manufacturing process of the optical film according to the present invention, and in the film formation process using a sputtering device, a cesium tungsten composite oxide film 108 having a refractive index n and an extinction coefficient k set within the numerical ranges of Table 7 as shown in Figure 5(A) is formed on a substrate 100, and in the annealing process using an electric furnace or the like, a surface layer 101 having a refractive index n and an extinction coefficient k set within the numerical ranges of Table 8 as shown in Figure 5(B) is formed on the surface side of the cesium tungsten composite oxide film 108, and the substrate 100 side portion of the cesium tungsten composite oxide film 108 excluding the surface layer 101 can be an internal layer 102 having a refractive index n and an extinction coefficient k set within the numerical ranges of Table 7.

[0046] The optical constants of the cesium tungsten composite oxide film after sputtering are within the numerical ranges shown in Table 7. As can be seen from the graph of Fig. 4 showing the spectroscopic optical characteristics (wavelength and reflectance) of the optical film according to Comparative Example 5, the cesium tungsten composite oxide film (optical film) after sputtering without a surface layer has a slight light reflection in the near infrared region, and the reflectance at a wavelength of 2000 nm is confirmed to be about 20%.

[0047] In addition, the optical constants (refractive index n and extinction coefficient k) of the surface layer after the annealing process are set within the numerical ranges of Table 8 above. As can be seen from the graph of FIG. 3 showing the spectroscopic optical characteristics (wavelength and transmittance) of the optical film of Example 5, the optical film having a surface layer has significant light reflection in the near-infrared region, and it is confirmed that the reflectance at a wavelength of 2000 nm is approximately 60%.

[0048] In addition, for an optical film having a thickness of 300 nm to 560 nm, if the optical constants (refractive index n and extinction coefficient k) of the optical film after sputtering deposition are set within the numerical ranges of Table 8 above by appropriately controlling the atmosphere during sputtering deposition, the temperature of the substrate, etc., then annealing treatment after the deposition process is not required.

[0049] (2) Sputtering Targets The optical film containing cesium, tungsten, and oxygen, and having a refractive index n and an extinction coefficient k set within the numerical ranges of Table 5 or Table 6, respectively, requires that the ratio of cesium atoms to tungsten atoms (Cs:W) is set within a specific range, and can be formed by a sputtering method. The sputtering target used in forming the film includes a target containing cesium atoms and tungsten atoms (i.e., a target composed of a mixture of a cesium source compound and a tungsten source compound), and may also be a target composed of a cesium source and a tungsten source separately (i.e., a cesium source sputtering target and a tungsten source sputtering target).

[0050] Hereinafter, sputtering film formation using a target containing cesium atoms and tungsten atoms will be described.

[0051] To obtain an optical film in which the refractive index n and extinction coefficient k are set within the numerical ranges of Table 5 or Table 6, a sputtering target in which the ratio of cesium atoms to tungsten atoms (Cs:W) is set in the range of 1:2 to 1:4 may be used, and the ratio (Cs:W) is preferably 1:2.5 to 1:4, and most preferably 1:2.8 to 1:4. The ratio of cesium atoms to tungsten atoms in the sputtering target approximately matches the ratio of cesium atoms to tungsten atoms in the optical film.

[0052] In addition, even if the target itself does not contain an appropriate amount of oxygen, the amount of oxygen that is incorporated into the film can be adjusted by reactive sputtering.Furthermore, the target may contain components such as carbon that are exhausted during sputtering.That is, the target does not need to be a cesium tungsten composite oxide, and may be a precursor of a cesium tungsten composite oxide that has the atomic ratio of cesium and tungsten of the optical film according to the present invention.

[0053] Furthermore, when forming the optical film according to the present invention by a two-target sputtering method, a sputtering target serving as a cesium source or a sputtering target consisting of a compound of cesium and tungsten containing more cesium than the optical film according to the present invention may be mounted on one sputtering cathode, and a sputtering target serving as a tungsten source or a sputtering target consisting of a compound of cesium and tungsten containing more tungsten than the optical film according to the present invention may be mounted on the other sputtering cathode. The atomic ratio of cesium to tungsten in the optical film obtained by the two-target sputtering method can be set by adjusting the power or duty ratio applied to each sputtering cathode.

[0054] The cesium source can be a metal, an oxide, or a carbonate. Cesium oxides include Cs2O, Cs2O2, CsO2, Cs2O3, and Cs 11 Examples include O3, Cs4O, and Cs7O.

[0055] The tungsten source may be a metal, an oxide, or a carbide. The oxides of tungsten include WO, WO, and W. 20 O 58 , WO3 can be used.

[0056] Next, there are two types of sputtering targets: a planar target shown in FIG. 6 and a cylindrical target shown in FIG. 7. The planar target has a structure in which a sputtering target 104 is fixed to the surface of a backing plate 103 with a bonding material such as indium. The planar sputtering target 104 is obtained by producing a molded body by pressure molding using a cold isostatic pressing method and sintering the resulting molded body. Although the planar target can be produced relatively easily, the entire surface is not sputtered, and foreign matter accumulates in the non-erosion portion that is not sputtered, and this foreign matter may cause abnormal discharge, and further, this foreign matter may adhere to the product. In recent years, cylindrical targets (rotary targets) shown in FIG. 7 have become mainstream for large targets. Although it is difficult to produce, the entire surface is sputtered, so there are no disadvantages like planar targets, and furthermore, the usage efficiency is nearly three times that of planar targets.

[0057] The cylindrical target (rotary target) 2 shown in Fig. 7 is mainly manufactured by two methods. The first method is a method in which, like the flat target, a molded body is manufactured by pressure molding using a cold isostatic pressing method, and the obtained molded body is sintered and cylindrically ground, and then inserted into the backing tube 1 shown in Fig. 7 and bonded with a bonding material such as indium. The second method is a method in which powder is directly sprayed onto the backing tube 1.

[0058] A cylindrical target (rotary target) manufactured by thermal spraying is formed by forming a base layer selected from an alloy such as a nickel-aluminum alloy, nickel-chromium alloy, copper-aluminum alloy, or copper-zinc alloy by thermal spraying on a backing tube 1 made of a metal such as copper or a copper alloy and having a surface roughened by blasting, and then directly spraying powder (cesium source powder and tungsten source powder) to form a thermal sprayed film (target film) with a thickness of 5 mm to 20 mm, and then polishing the thermal sprayed film (target film) to finish it into a rotary target.

[0059] Here, plasma spraying can be used for the thermal spraying, and an AC / DC arc plasma torch or an inductively coupled plasma torch or the like can be used, and the atmosphere during the thermal spraying may be an inert gas or the like.

[0060] When manufacturing a sputtering target by the thermal spraying method, it is necessary to note that depending on the temperature, the cesium source Cs2O may undergo a disproportionation reaction to become Cs2O2, which will affect the sputtering rate of the obtained target (fluctuations in the sputtering rate).

[0061] (3) Sputtering Equipment By using the above target and performing reactive sputtering with oxygen, an optical film composed of CsαWβOγCδ can be obtained. α and β directly reflect the target composition ratio, and γ can be adjusted by the amount of oxygen introduced during reactive sputtering. Carbon C released from the target (for example, when the tungsten source is composed of carbide) combines with oxygen O released from the target or oxygen O introduced to perform reactive sputtering, and becomes CO2 and is exhausted, so it hardly remains in the optical film.

[0062] FIG. 8 is a diagram illustrating the configuration of a sputtering apparatus (film forming apparatus) 105 equipped with a flat target. In the film forming chamber, a substrate holding member 107 is disposed so as to face a magnetron sputtering cathode 106. The sputtering target 104 is attached to the sputtering cathode 106, and the substrate holding member 107 holds the substrate 10 on which a film is to be formed by sputtering. The substrate holding member 107 may be equipped with a heater. As the heater (not shown), a near-infrared heater, a carbon heater, a sheath heater, or the like can be used. A power source is connected to the sputtering cathode 106. It is difficult to sputter a non-conductive target using a DC power source. For this reason, a medium frequency power source (20 kHz to 200 kHz) is connected. Furthermore, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used.

[0063] 9 is an explanatory diagram showing a film formation method using a cylindrical target (rotary target), that is, the positional relationship between the substrate and the rotary target. This film formation method generally uses a dual magnetron sputtering method in which power is alternately applied to two rotary targets 11, 12, 13, and 14 arranged in parallel with a substrate 10 moving in the direction of the arrow, using a medium frequency power source (20 kHz to 200 kHz), and furthermore, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used.

[0064] A sputtering apparatus using the dual magnetron sputtering method will be described below.

[0065] (3A) Sputtering film formation unit A and film formation method The sputtering deposition unit A in which a film is formed by the dual magnetron sputtering method is composed of the connection chambers 20, 22 and the deposition chamber 21 as shown in FIG. 10. The transfer rollers 24 for transferring the substrate 23 are arranged in series in the connection chambers 20, 22 and the deposition chamber 21, and the deposition chamber 21 is provided with the dual magnetron cathode units 33, 34 for maintaining the deposition gas pressure. The substrate 23 is preheated to 400° C. or higher in the connection chamber 20. The substrate 23, which is the substrate to be deposited, is heated by heating the connection chamber 20. A near-infrared heater, a carbon heater, a sheath heater, or the like can be used as the heater for the connection chamber 20. The substrate 23 can be supplied to the connection chamber 20 from a substrate stocker (not shown). It is preferable to further arrange a pretreatment chamber (not shown) between the connection chamber 20 and the substrate stocker, and treat (clean, etch) the surface of the substrate 23 with plasma or an ion beam, or the like.

[0066] In addition, the dual magnetron cathode units 33 and 34 are provided with rotary magnetron cathodes (not shown) on which a set of rotary targets 25, 26, 27, and 28 are mounted, and the rotary targets 25, 26 and the rotary targets 27, 28 are connected to a medium frequency power source, so that power is applied alternately. Specifically, dual magnetron sputtering can be performed by alternately applying power to the medium frequency power source using a power source of 20 kHz to 200 kHz, and further, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used. In addition, the rotary magnetron cathode (not shown) is provided with magnets (not shown) that generate sputtering 29, 30, 31, and 32 only on the substrate 23 side of the rotary targets 25, 26, 27, and 28, so that most of the target particles from the rotary targets 25, 26, 27, and 28 fly toward the substrate 23 side, and the deposition efficiency is about 90%.

[0067] Oxygen gas for reactive sputtering is introduced into each of the dual magnetron cathode units 33, 34, and the amount of oxygen introduced into the dual magnetron cathode units 33, 34 can be controlled, for example, by "impedance control," which controls the impedance change of the sputtering power supply to a set value, or by plasma emission monitor (PEM) control, which controls the plasma emission intensity of a specific wavelength to a set value.

[0068] In the sputtering deposition unit A shown in Figure 10, in which two pairs of dual magnetron cathode units 33, 34 are arranged in the deposition chamber 21, it is possible to deposit up to two types of optical films, and if the same rotary target is incorporated in the two pairs of dual magnetron cathode units 33, 34, it is possible to deposit one type of optical film with twice the thickness.

[0069] Next, in the film formation method using the dual sputtering method, a sputtering target serving as a cesium source and a sputtering target serving as a tungsten source are prepared, and each sputtering target is attached to a different rotary magnetron cathode for sputtering.

[0070] A CsxWyOz film can be obtained by reactive sputtering with oxygen. The sputtering rates of the sputtering targets serving as the cesium source and the tungsten source must be adjusted to x and y.

[0071] There are several methods for adjusting the sputtering rate by mounting a sputtering target serving as a cesium source and a sputtering target serving as a tungsten source on different rotary magnetron cathodes. (i) A method of connecting separate pulse power supplies to both rotary magnetron cathodes and simultaneously applying sputtering powers with equal co-pulse times and different peak powers to both rotary magnetron cathodes. (ii) A method of adjusting the sputtering power by connecting one dual magnetron power supply to both rotary magnetron cathodes and alternately applying sputtering power with equal peak power but different duty ratios to both rotary magnetron cathodes. (iii) The composition ratio of both targets can be adjusted by the above method (i) or (ii).

[0072] Moreover, z in the CsxWyOz film can be adjusted by the amount of oxygen introduced during reactive sputtering.

[0073] As mentioned above, it is difficult to sputter non-conductive targets using a DC power source, so a dual magnetron sputtering method is generally used in which targets 111, 113 mainly composed of a cesium source and targets 112, 114 mainly composed of a tungsten source are arranged in parallel to a substrate 10 moving in the direction of the arrow as shown in Figure 11, and power is alternately applied using a medium frequency power source (20 kHz to 200 kHz).In addition, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used.

[0074] Furthermore, the temperature of the substrate 10 (23) also affects the optical properties of the optical film. An optical film having the optical properties (refractive index n and extinction coefficient k) shown in Table 5 or Table 6 above can be obtained by appropriately adjusting the sputtering gas, sputtering power, and substrate temperature depending on the sputtering deposition unit used.

[0075] (3B) Sputtering film formation unit B and film formation method The sputtering deposition unit B in which deposition is performed by the dual magnetron sputtering method is composed of connecting chambers 120, 122 and a deposition chamber 121 as shown in Fig. 12. Transport rollers 124 for transporting the substrate 23 are continuously arranged in the connecting chambers 120, 122 and the deposition chamber 121, and dual magnetron cathode units 133, 134 for maintaining deposition gas pressure are provided in the deposition chamber 121. The substrate 23 is preheated to 400°C or higher in the connecting chamber 120. Further, the two sets of dual magnetron cathode units 133 and 134 are provided with rotary magnetron cathodes (not shown) on which rotary targets 125 and 127 mainly made of a cesium source and rotary targets 126 and 128 mainly made of a tungsten source are mounted, and the rotary targets 125 and 126 and the rotary targets 127 and 128 are connected to medium frequency power sources, respectively, so that power is applied alternately. Specifically, dual magnetron sputtering can be performed by alternately supplying power to the medium frequency power source using a power source of 20 kHz to 200 kHz, and furthermore, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used. In addition, a magnet (not shown) is arranged in the rotary magnetron cathode (not shown) to cause sputtering 129, 130, 131, 132 only on the substrate 23 side of the rotary targets 125, 126, 127, 128. As a result, most of the target particles from the rotary targets 125, 126, 127, 128 fly in the direction of the substrate 23 side, and the deposition efficiency is about 90%.

[0076] Oxygen gas for reactive sputtering is introduced into each of the dual magnetron cathode units 133, 134, and the amount of oxygen introduced into the dual magnetron cathode units 133, 134 can be controlled, for example, by "impedance control," which controls the impedance change of the sputtering power supply to a set value, or by plasma emission monitor (PEM) control, which controls the plasma emission intensity of a specific wavelength to a set value.

[0077] 12 in which two pairs of dual magnetron cathode units 133, 134 are arranged in the film formation chamber 121, it is possible to form up to two types of optical films, and when the same rotary target is incorporated in the two pairs of dual magnetron cathode units 133, 134, it is possible to form one type of optical film with twice the thickness. However, with the cathode arrangement as in FIG. 12, a film mainly composed of cesium oxide and a film mainly composed of tungsten oxide are laminated on top of each other.

[0078] Furthermore, a compound of cesium and tungsten, such as cesium tungstate, can be used for the rotary target mainly composed of a cesium source. By using this rotary target mainly composed of a tungsten source in combination with a dual magnetron cathode unit and adjusting the sputtering rate of each, an optical film with an adjusted ratio of cesium to tungsten can be obtained.

[0079] Incidentally, in order to form an optical film by controlling the atmospheric oxygen partial pressure during film formation using a dual sputtering method employing a rotary target mainly made of a cesium source and a rotary target mainly made of a tungsten source, and to obtain a film in which the molar ratio of cesium to tungsten contained in the optical film is 1:2 to 1:4, it is sufficient to arrange the magnet bar (not shown) inside the rotary magnetron cathode so as to be tilted in the direction of rotation as shown in Fig. 13, so that the sputtering film formation areas overlap as shown in Fig. 13. It is also possible to subtly swing the magnet bar in the direction of rotation.

[0080] Furthermore, the temperature of the substrate 23 also affects the optical properties of the optical film. An optical film having the optical properties shown in Table 5 or Table 6 above can be obtained by appropriately adjusting the sputtering gas, sputtering power, and substrate temperature depending on the sputtering deposition unit used.

[0081] (3C) Sputtering film formation unit C and film formation method The sputtering deposition unit C, which deposits films so that the sputter deposition areas overlap, is composed of connecting chambers 140, 142 and a deposition chamber 141 as shown in Fig. 13, and transport rollers 144 for transporting a substrate 143 are continuously arranged in the connecting chambers 140, 142 and the deposition chamber 141, and dual magnetron cathode units 153, 154 for maintaining deposition gas pressure are provided in the deposition chamber 141. The substrate 143 is preheated to 400°C or higher in the connecting chamber 140. In addition, the two sets of dual magnetron cathode units 153 and 154 are provided with rotary magnetron cathodes (not shown) on which rotary targets 145 and 147 mainly made of cesium oxide powder and rotary targets 146 and 148 mainly made of tungsten oxide powder are mounted, and the rotary targets 145 and 146 and the rotary targets 147 and 148 are connected to medium frequency power sources, respectively, so that power is applied alternately. Specifically, dual magnetron sputtering can be performed by alternately applying power to the medium frequency power source using a power source of 20 kHz to 200 kHz, and further, a normal pulse power source or a high voltage pulse power source (HiPMS) can also be used. In addition, a magnet (not shown) is arranged in the rotary magnetron cathode (not shown) to cause sputtering 149, 150, 151, 152 only on the substrate 143 side of the rotary targets 145, 146, 147, 148. As a result, most of the target particles from the rotary targets 145, 146, 147, 148 fly in the direction of the substrate 143 side, and the deposition efficiency is about 90%.

[0082] Oxygen gas for reactive sputtering is introduced into each of the dual magnetron cathode units 153, 154, and the amount of oxygen introduced into the dual magnetron cathode units 153, 154 can be controlled, for example, by "impedance control," which controls the impedance change of the sputtering power supply to a set value, or by plasma emission monitor (PEM) control, which controls the plasma emission intensity of a specific wavelength to a set value.

[0083] In addition, when using the sputtering film formation unit C, the ratio of cesium atoms and tungsten atoms in one of the rotary targets arranged in the dual magnetron cathode units 153 and 154 can be shifted from the ratio of cesium atoms and tungsten atoms in the desired optical film, so that the other rotary target can be made to contain the cesium or tungsten that is lacking in the other rotary target. For example, the rotary targets 145 and 147 can be made of Cs2WO4, and the rotary targets 146 and 148 can be made of a tungsten source.

[0084] Furthermore, the temperature of the base material 143 also affects the optical properties of the optical film. An optical film having the optical properties shown in Table 5 or Table 6 above can be obtained by appropriately adjusting the sputtering gas, sputtering power, and base material temperature depending on the sputtering deposition unit used. EXAMPLES

[0085] Examples of the present invention will be specifically described below with reference to comparative examples.

[0086] The ellipsometer used was a JA Woollam "RC2-XNIR" model, the optical properties (transmittance and reflectance) of the optical film were measured using a JASCO "V-670" model, and the surface resistance of the optical film was measured using a Mitsubishi Chemical "Loresta-GX" model.

[0087] The sputtering target was prepared by forming a cesium tungsten composite oxide powder manufactured by Sumitomo Metal Mining Co., Ltd. into an 8-inch circular shape, placing the resulting molded body in a hot press device, and subjecting it to a vacuum atmosphere at a temperature of 950°C and a pressure of 250 kgf / cm. 2 The powder could be sintered under the above conditions.

[0088] The obtained sputtering target having an outer diameter of 8 inches was bonded to a copper backing plate with indium, and the sputtering target fixed to the backing plate was placed in the sputtering apparatus (film formation apparatus) shown in FIG.

[0089] A high frequency power source (13 MHz) was used as the power source for this sputtering device (film formation device), oxygen was introduced from the sputtering cathode 106, and the distance between the sputtering target 104 and the substrate 10 was set to 100 mm.

[0090] A synthetic quartz wafer having a diameter of 8 inches was used as the substrate 10. The substrate 10 was heated to 400° C. or higher using a near-infrared heater.

[0091] [Comparative Examples 1 to 4, Examples 1 to 3] The deposition chamber of the sputtering equipment (deposition equipment) shown in Figure 8 is 5 × 10 -4 After evacuation to a pressure of less than 1 Pa, argon gas mixed with oxygen was introduced at 800 sccm.

[0092] Argon gas mixed with gas having an oxygen concentration of 3% was introduced, and the deposition rate was set to approximately 1 nm / sec. Optical films having thicknesses of 300 nm (Comparative Example 1), 320 nm (Comparative Example 2), 340 nm (Comparative Example 3), and 360 nm (Comparative Example 4) were deposited on the substrate 10.

[0093] The optical films of Comparative Examples 1 to 4 were measured using the above-mentioned JASCO V-670 model. As shown in Table 11 below, the films had the characteristics of a heat ray shielding film, having a high average transmittance in the visible wavelength range (wavelength 400 nm to 550 nm) and a low reflectance in the near infrared range (wavelength 2000 nm).

[0094] The optical constants (refractive index n and extinction coefficient k) of the optical films according to Comparative Examples 1 to 4 having such characteristics were measured using the above-mentioned ellipsometer "RC2-XNIR type," and the refractive indexes and extinction coefficients were as shown in Table 9 below.

[0095] [Table 9]

[0096] Next, the optical films having thicknesses of 320 nm (Comparative Example 2), 340 nm (Comparative Example 3), and 360 nm (Comparative Example 4) were subjected to an annealing treatment in a nitrogen atmosphere at about 700° C. to reduce the surface of each optical film.

[0097] The reduction depth from the optical film surface is thought to depend on the annealing time, and three annealing times were performed: 2 minutes, 4 minutes, and 6 minutes. The optical constants (refractive index n and extinction coefficient k) of the surface side of the optical film reduced by annealing were also measured in the same manner using the above-mentioned ellipsometer "RC2-XNIR type," resulting in the refractive index and extinction coefficients shown in Table 10 below. Furthermore, the depth of the surface side of the optical film reduced by annealing can also be estimated from the change in the optical constants in the depth direction by ellipsometer analysis of the optical film. The results are also shown in Table 11 below.

[0098] [Table 10]

[0099] An optical film having an optical film thickness of 320 nm and a reduced surface depth of 20 nm (i.e., annealing time is 2 minutes: surface layer thickness is 20 nm, internal layer thickness is 300 nm) was designated as Example 1, an optical film having an optical film thickness of 340 nm and a reduced surface depth of 40 nm (i.e., annealing time is 4 minutes: surface layer thickness is 40 nm, internal layer thickness is 300 nm) was designated as Example 2, and an optical film having an optical film thickness of 360 nm and a reduced surface depth of 60 nm (i.e., annealing time is 6 minutes: surface layer thickness is 60 nm, internal layer thickness is 300 nm) was designated as Example 3. As in the comparative example, the optical films according to Examples 1 to 3 were measured using the above-mentioned JASCO "V-670 type". As shown in Table 11 below, the average transmittance in the visible wavelength region (wavelength 400 nm to 550 nm) was slightly reduced, but the film had the characteristics of a heat ray shielding film with high reflectance in the near infrared region (wavelength 2000 nm).

[0100] As can be seen from Table 11 below, in Examples 1 to 3, light in the near infrared range incident on each optical film is reflected on the surface side, which is expected to have the effect of suppressing heat generation in the base material due to heat ray absorption.

[0101] It can be easily assumed that the spectral optical characteristics will be the same even if a film (surface-side layer) having the same optical constants as the film subjected to reduction annealing instead of annealing is directly sputtered on the substrate-side layer.

[0102] [Table 11]

[0103] [Comparative Examples 5 to 8, Examples 4 to 6] As described above, argon gas mixed with gas having an oxygen concentration of 3% was introduced, and the deposition rate was set to approximately 1 nm / sec. Optical films having thicknesses of 400 nm (Comparative Example 5), 420 nm (Comparative Example 6), 440 nm (Comparative Example 7), and 460 nm (Comparative Example 8) were deposited on the substrate 10.

[0104] The optical films of Comparative Examples 5 to 8 were measured using a JASCO V-670 model. As shown in Table 11 above, the films had the characteristics of a heat-shielding film, having a high average transmittance in the visible wavelength range (wavelength 400 nm to 550 nm) and a low reflectance in the near-infrared range (wavelength 2000 nm).

[0105] The optical constants (refractive index n and extinction coefficient k) of the optical films according to Comparative Examples 5 to 8 having such characteristics were measured using an ellipsometer "RC2-XNIR type," and the refractive index and extinction coefficient were as shown in Table 9 above.

[0106] Next, the optical films having thicknesses of 420 nm (Comparative Example 6), 440 nm (Comparative Example 7), and 460 nm (Comparative Example 8) were subjected to an annealing treatment in a nitrogen atmosphere at approximately 700°C for three stages of annealing times of 2 minutes, 4 minutes, and 6 minutes to reduce the surface of each optical film.

[0107] The optical constants (refractive index n and extinction coefficient k) of the surface side of the optical film reduced by annealing were also measured in the same manner using the ellipsometer "RC2-XNIR type" described above, and the refractive index and extinction coefficient were as shown in Table 10 above. Furthermore, the depth of the surface side of the optical film reduced by annealing was estimated from the change in the optical constants in the depth direction by ellipsometer analysis of the optical film. The results are also shown in Table 11 above.

[0108] An optical film having an optical film thickness of 420 nm and a reduced surface depth of 20 nm (i.e., a surface layer thickness of 20 nm and an internal layer thickness of 400 nm) was used as Example 4, an optical film having an optical film thickness of 440 nm and a reduced surface depth of 40 nm (i.e., a surface layer thickness of 40 nm and an internal layer thickness of 400 nm) was used as Example 5, and an optical film having an optical film thickness of 460 nm and a reduced surface depth of 60 nm (i.e., a surface layer thickness of 60 nm and an internal layer thickness of 400 nm) was used as Example 6. As in the comparative example, the optical films according to Examples 4 to 6 were measured using the above-mentioned JASCO Corporation "V-670 type". As shown in Table 11 above, the average transmittance in the visible wavelength range (wavelength 400 nm to 550 nm) was slightly reduced, but the film had the characteristics of a heat ray shielding film with high reflectance in the near infrared range (wavelength 2000 nm).

[0109] The spectral optical characteristics (wavelength and transmittance) of the optical films of Examples 4 to 6 and Comparative Example 5 are shown in FIG. 14, and the spectral optical characteristics (wavelength and reflectance) of the optical films of Examples 4 to 6 and Comparative Example 5 are shown in FIG. 15.

[0110] As can be seen from Table 11 above and the graphs in Figures 14 and 15, in Examples 4 to 6 as well, near-infrared light incident on each optical film is reflected on the surface side, which is expected to have the effect of suppressing heat generation in the substrate due to heat ray absorption.

[0111] [Comparative Examples 9 to 12, Examples 7 to 9] As described above, argon gas mixed with gas having an oxygen concentration of 3% was introduced, and the deposition rate was set to approximately 1 nm / sec. Optical films having thicknesses of 500 nm (Comparative Example 9), 520 nm (Comparative Example 10), 540 nm (Comparative Example 11), and 560 nm (Comparative Example 12) were deposited on the substrate 10.

[0112] The optical films of Comparative Examples 9 to 12 were measured using a JASCO V-670 model. As shown in Table 11 above, the films had the characteristics of a heat-shielding film, having a high average transmittance in the visible wavelength range (wavelength 400 nm to 550 nm) and a low reflectance in the near-infrared range (wavelength 2000 nm).

[0113] The optical constants (refractive index n and extinction coefficient k) of the optical films according to Comparative Examples 9 to 12 having such characteristics were measured using an ellipsometer "RC2-XNIR type," and the refractive index and extinction coefficient were as shown in Table 9 above.

[0114] Next, optical films having thicknesses of 520 nm (Comparative Example 10), 540 nm (Comparative Example 11), and 560 nm (Comparative Example 12) were subjected to an annealing treatment in a nitrogen atmosphere at approximately 700°C for three stages of annealing times of 2 minutes, 4 minutes, and 6 minutes to reduce the surface of each optical film.

[0115] The optical constants (refractive index n and extinction coefficient k) of the surface side of the optical film reduced by annealing were also measured in the same manner using the ellipsometer "RC2-XNIR type" described above, and the refractive index and extinction coefficient were as shown in Table 10 above. Furthermore, the depth of the surface side of the optical film reduced by annealing was estimated from the change in the optical constants in the depth direction by ellipsometer analysis of the optical film. The results are also shown in Table 11 above.

[0116] An optical film having a thickness of 520 nm and a reduced surface depth of 20 nm (i.e., a surface layer thickness of 20 nm and an internal layer thickness of 500 nm) was used as Example 7, an optical film having a thickness of 540 nm and a reduced surface depth of 40 nm (i.e., a surface layer thickness of 40 nm and an internal layer thickness of 500 nm) was used as Example 8, and an optical film having a thickness of 560 nm and a reduced surface depth of 60 nm (i.e., a surface layer thickness of 60 nm and an internal layer thickness of 500 nm) was used as Example 9. As in the comparative example, the optical films according to Examples 7 to 9 were measured using the above-mentioned JASCO Corporation "V-670 type". As shown in Table 11 above, the average transmittance in the visible wavelength range (wavelength 400 nm to 550 nm) was slightly reduced, but the film had the characteristics of a heat ray shielding film with high reflectance in the near infrared range (wavelength 2000 nm).

[0117] As can be seen from Table 11 above, in Examples 7 to 9, near-infrared light incident on each optical film is reflected on the surface side, which is expected to have the effect of suppressing heat generation in the base material due to heat ray absorption. [Industrial Applicability]

[0118] The optical film according to the present invention can be a semi-reflective heat ray shielding film that has radio wave transparency and light transparency in the visible wavelength range, while suppressing absorption in the near-infrared wavelength range, and therefore has industrial applicability for use in window glass and the like that reduces energy consumption of air conditioners in the summer. [Explanation of symbols]

[0119] 1 Backing Tube 2. Cylindrical targets (rotary targets) 10 Base material 11, 12, 13, 14 Rotary Target 20, 22 Connecting rooms 21 Deposition chamber 23 Substrate (glass substrate) 24 Transport roller 25, 26, 27, 28 Rotary Target 29, 30, 31, 32 Sputtering 33, 34 Dual magnetron cathode unit 60, 68 Substrate stocker room 62, 64, 66 Sputtering deposition unit 61, 63, 65, 67 Connecting rooms 100 Base material 101 Surface layer 102 Inner layer 103 Backing Plate 104 Sputtering Target 105 Sputtering equipment (film deposition equipment) 106 Sputtering cathode 107 Substrate holding member 108 Cesium-tungsten composite oxide film 111, 112, 113, 114 Target 120, 122 Connecting rooms 121 Deposition chamber 124 Transport roller 125, 126, 127, 128 Rotary Target 129, 130, 131, 132 Sputtering 133, 134 Dual magnetron cathode unit 140, 142 Connecting rooms 141 Deposition chamber 143 Base material 144 Transport roller 145, 146, 147, 148 Rotary Target 149, 150, 151, 152 Sputtering 153, 154 Dual magnetron cathode unit

Claims

1. In an optical coating formed on a substrate and made of a cesium tungsten composite oxide containing cesium, tungsten, and oxygen, The optical film is composed of a surface layer having a thickness of 20 nm to 60 nm located on the surface side and an internal layer located on the substrate side, The refractive index n and extinction coefficient k of the surface layer are set within the numerical ranges of Table 12 below, [Table 12] The optical film is characterized in that the refractive index n and extinction coefficient k of the inner layer are set within the numerical ranges shown in Table 13 below. [Table 13] In the table, "nm" refers to the wavelength, "n-min and n-max" refer to the minimum and maximum values ​​of the refractive index n at each wavelength, and "k-min and k-max" refer to the minimum and maximum values ​​of the extinction coefficient k at each wavelength (the same applies to other tables except for Table 11).

2. 2. The optical film according to claim 1, wherein the optical film has a thickness of 300 nm to 560 nm, and has an average transmittance of 45% or more in the wavelength range of 400 nm to 550 nm, and a reflectance of 40% or more at a wavelength of 2000 nm.

3. 2. The method for producing an optical film according to claim 1 , a film formation process in which a sputtering target consisting of cesium atoms, tungsten atoms, and oxygen is used, and the oxygen partial pressure in the sputtering film formation atmosphere is feedback-controlled while controlling the heating temperature of the substrate to form a cesium tungsten composite oxide film on the substrate, the refractive index n and the extinction coefficient k of which are set within the numerical ranges shown in Table 14 below; [Table 14] An annealing process of annealing the formed cesium tungsten composite oxide film to form a surface layer on the surface side of the cesium tungsten composite oxide film, the refractive index n and the extinction coefficient k of which are set within the numerical ranges shown in Table 15 below, and to make the substrate side portion of the cesium tungsten composite oxide film excluding the surface layer into an internal layer, the refractive index n and the extinction coefficient k of which are set within the numerical ranges shown in Table 14 above; A method for producing an optical film, comprising: [Table 15]

4. The method for manufacturing an optical film according to claim 3 , wherein the annealing step is performed in an oxygen-free atmosphere at a temperature of 300° C. or higher.

5. 5. The method for producing an optical coating according to claim 3, wherein the ratio of cesium atoms to tungsten atoms (Cs:W) in the sputtering target is 1:2 to 1:

4.

6. The method for producing the optical film according to claim 3 or 4, characterized in that the film forming process is carried out by a dual sputtering method using a sputtering target of a cesium source and a sputtering target of a tungsten source, and the oxygen partial pressure of the dual sputtering film forming atmosphere is feedback controlled, so that the ratio (Cs:W) of cesium atoms and tungsten atoms contained in the cesium tungsten composite oxide film is 1:2 to 1:4, and the power or duty ratio applied to the sputtering cathode is adjusted.

7. The method for manufacturing an optical film according to any one of claims 3 to 6, characterized in that the feedback control of the oxygen partial pressure is performed by an impedance controller that feedback controls a change in impedance during film formation.

8. The method for manufacturing an optical film described in any one of claims 3 to 6, characterized in that the feedback control of the oxygen partial pressure is performed by a plasma emission monitor that measures the emission intensity of a specific wavelength during film formation and feedback controls the oxygen partial pressure.

Citation Information

Patent Citations

  • Lightproof film

    JP1993113085A

  • Absorption-type multilayer film nd filter and manufacturing method therefor

    JP2010224350A

  • laminate

    JP2012214016A

  • Near-infrared cut filter