Toner, toner storage unit, image forming apparatus and image forming method

A toner with crystalline and amorphous polyester resins, optimized for aspect ratio and center-to-center distance, addresses fixing and storage stability issues, enhancing low-temperature performance and cleaning efficiency.

JP7585687B2Active Publication Date: 2024-11-19RICOH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020162654
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-28
Publication Date
2024-11-19
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing toners with low-temperature fixing properties and heat-resistant storage properties face issues such as insufficient fixing performance, exposure of crystalline polyester resin on the surface leading to image quality deterioration, and reduced heat-resistant storage stability, along with inadequate cleaning performance.

Method used

A toner formulation containing crystalline and amorphous polyester resins with specific aspect ratios and shape indices, along with controlled center-to-center distances between crystalline polyester resin particles, ensures uniform plasticization and reduces adhesion, enhancing low-temperature fixing properties, heat-resistant storage stability, and cleaning performance.

Benefits of technology

The toner achieves superior low-temperature fixing properties, maintains image quality, and improves cleaning performance by uniformly dispersing crystalline polyester resin particles within the toner, preventing exposure on the surface and reducing adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585687000003
    Figure 0007585687000003
  • Figure 0007585687000004
    Figure 0007585687000004
  • Figure 0007585687000005
    Figure 0007585687000005
Patent Text Reader

Abstract

To provide a toner having better low temperature fixability, heat-resistant storage property, image quality, and cleaning performance.SOLUTION: A toner according to an embodiment is a toner including a crystalline polyester resin and an amorphous polyester resin. Toner particles have an aspect ratio of 1.5-5 and a shape index of 0.75 or more. The center-to-center distance L between particles of the crystalline polyester resin included in the toner particles is twice or more the maximum length D of a cross section of the particle of the crystalline polyester resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]

[0002] Image forming devices using toner, such as multi-function peripherals (MFPs) and printers, are widely used in various places, including offices. Toner is required to have low-temperature fixing property and heat-resistant storage property in order to reduce power consumption during fixing to save energy, and to improve resistance to high temperatures and high humidity during storage and transportation.

[0003] As a toner having low-temperature fixing property and heat-resistant storage stability, for example, a dry toner has been proposed which is obtained by removing the organic solvent from a dispersion liquid in which fine droplet particles containing an organic solvent, a binder resin, a colorant, and a wax are dispersed in an aqueous medium, and which has an average circularity of 0.900 to 0.960 and a spindle shape (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]

[0004] However, the dry toner described in Patent Document 1 does not sufficiently lower the fixability, and is insufficient to achieve low-temperature fixability. In addition, Patent Document 1 does not describe the use of crystalline polyester resin as a binder resin, so if the crystalline polyester resin is used in a finely divided form, the crystalline polyester resin is likely to be exposed on the toner surface, which may lead to a deterioration in the quality of the output image. In addition, the toner may be easily solidified due to heat generated in the image forming apparatus or heat during storage, and the heat-resistant storage stability may be reduced. Furthermore, Patent Document 1 does not describe cleaning properties, so there is a possibility that the toner attached to the carrier, photoconductor, blade, etc. may not be sufficiently removed.

[0005] An object of one aspect of the present invention is to provide a toner having superior low-temperature fixing property, heat-resistant storage stability, image quality and cleaning property. [Means for solving the problem]

[0006] One embodiment of the toner according to the present invention is a toner containing a crystalline polyester resin and a non-crystalline polyester resin, wherein the toner particles have an aspect ratio of 1.5 to 5 and a shape index of 0.75 or more, and the center-to-center distance L between particles of the crystalline polyester resin contained in the toner particles is at least twice the maximum length D of the cross section of the crystalline polyester resin particles. Effect of the Invention

[0007] One aspect of the present invention can provide a toner having superior low-temperature fixing property, heat-resistant storage stability, image quality and cleaning property. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a diagram illustrating an example of the inside of a toner according to an embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of a cross section of a crystalline polyester resin. [Diagram 3] FIG. 1 is a schematic configuration diagram illustrating an example of an image forming apparatus according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description, and can be modified as appropriate without departing from the gist of the present invention. In addition, in this specification, a tilde "~" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified.

[0010] <Toner> The toner according to the embodiment is a toner containing a crystalline polyester resin and a non-crystalline polyester resin, and the toner particles have an aspect ratio of 1.5 to 5 and a shape index of 0.75 or more, and the center-to-center distance L between the crystalline polyester resin particles (crystalline polyester resin particles) contained in the toner particles is two times or more the maximum length D of the cross section of the crystalline polyester resin particle.

[0011] FIG. 1 shows an example of the inside of a toner according to an embodiment, and FIG. 2 shows an example of a cross section of a crystalline polyester resin. As shown in FIG. 1, crystalline polyester resin particles are dispersed inside the toner. As shown in FIG. 2, when the crystalline polyester resin particle is formed in an elliptical shape, the length of the major axis of the cross section of the crystalline polyester resin particle is the maximum length. D The length of the minor axis is set as the minimum length, and the intersection of the major axis and the minor axis is set as the center point.

[0012] As a result of intensive research, the present inventors have focused on the aspect ratio and shape index of the toner, and the center-to-center distance and maximum length of the crystalline polyester resin particles. They have found that if the aspect ratio of the toner is 1.5 to 5, the shape index is 0.75 or more, and the center-to-center distance L of the cross section of the crystalline polyester resin particle is twice or more the maximum length D of the cross section of the crystalline polyester resin particle, the toner can simultaneously exhibit better low-temperature fixing property, heat-resistant storage stability, image quality, and cleaning property.

[0013] [Toner aspect ratio] The aspect ratio of the toner is preferably from 1.5 to 5, and more preferably from 2.0 to 4.0. When the aspect ratio of the toner is within the above preferred range, the toner particles do not roll in one direction, and blade cleaning properties can be maintained.

[0014] The aspect ratio of the toner can be calculated, for example, by dispersing the toner on a carbon tape, forming a metal or other vapor deposition film on the toner surface as necessary, observing the toner with a SEM, and taking an image of the toner surface with a Phenom ProX PREMIUM 2. The obtained images of 100 toner particles are analyzed using the particle analysis software "Particle Metric," and the aspect ratio can be calculated from the ratio of the maximum length to the minimum length of the toner particles.

[0015] The method for dispersing the toner sample on the carbon tape is not particularly limited and can be carried out by a conventional method, for example, using a dispersing device NEBLA that can disperse the toner on the carbon tape under vacuum.

[0016] The method for forming a metal or other vapor deposition film on the toner surface is not particularly limited, and can be carried out by a method generally used for the purpose. For example, it can be carried out using carbon, platinum, platinum vanadium, or the like, using a vacuum deposition apparatus.

[0017] [Toner shape index] The shape index of the toner is a value obtained by dividing a diameter D2 of a circle having an area equal to the area of ​​a toner particle by a diameter D1 of a circle having a perimeter equal to the perimeter of a toner particle. The shape index of the toner is preferably 0.75 to 0.84, more preferably 0.85 to 0.89, and further preferably 0.90 to 1.00.

[0018] The shape index is a measure of the unevenness of the surface of a toner particle. When the unevenness of the surface of a toner particle is small or absent, the shape index becomes large. When the concave portion of the surface of a toner particle is small or absent, the external additives contained in the toner are not concentrated and attached to the concave portion, and excessive stress from the outside can be reduced to be applied to the convex portion, so that the toner is less likely to deteriorate. The present inventors have found that the degree and speed of deterioration of the toner must be larger than that of other toners in order to match the degree and speed of deterioration of the toner with other toners.

[0019] The "shape index" can be measured, for example, using a desktop SEM: Phenom ProX PREMIUM2 and particle analysis software: Particle Metric (Phenom World). By using a desktop SEM: Phenom ProX PREMIUM2 and particle analysis software: Particle Metric (Phenom World), a shape index that takes into account the unevenness of the toner surface can be obtained. When using shape factors SF-1 and SF-2 as shape evaluation parameters, normal SEM image analysis only analyzes the contours of the toner particles, making it difficult to analyze recesses that are not included in the contours of the toner particles. By using the above particle analysis software for analysis, the true surface unevenness, not the projected image, can be quantified.

[0020] The shape index is calculated in the same way as the calculation of the toner aspect ratio described above, by capturing an image of the toner surface. The captured image of 100 toner particles is analyzed using the particle analysis software "Particle Metric," and the shape index can be calculated from the ratio of the diameter of a circle with an area equal to the area of ​​a toner particle to the diameter of a circle with a perimeter equal to the perimeter of a toner particle.

[0021] The method of dispersing the toner sample on the carbon tape and the method of depositing a metal or other vapor onto the toner surface can be performed in the same manner as in the calculation of the above-mentioned [toner aspect ratio], so details are omitted.

[0022] As a method for adjusting the shape index, for example, when the toner surface has minute irregularities, the toner surface is smoothed. Examples of methods for smoothing the toner surface include a method of applying a mechanical impact after powdering to remove corners or smooth the surface. More specifically, examples include a method of colliding powder particles with each other, a method of colliding powder particles with a collision plate, and a method of processing powder particles with a rotating toothed device. There is also a method of heating the toner in water or in an air current to a temperature above the softening temperature of the toner to melt the surface.

[0023] [Maximum length D of the cross section of crystalline polyester resin particle] The maximum length of the crystalline polyester resin in the toner is preferably 100 nm or more and less than 500 nm, and more preferably 210 nm to 500 nm. When the maximum length of the crystalline polyester resin is 100 nm or more and less than 500 nm, the crystalline polyester resin can efficiently plasticize the surrounding amorphous resin (melt the resin at low temperature). When the maximum length of the crystalline polyester resin is less than 100 nm, the crystalline polyester resin is too finely dispersed, and even when not heated, a part of the crystalline polyester resin is plasticized and becomes compatible with the amorphous polyester resin, which may cause a decrease in the fluidity of the toner powder as a whole and adversely affect image quality. On the other hand, when it is 500 nm or more, the crystalline polyester resin cannot efficiently plasticize with the amorphous polyester resin due to the contact area between the crystalline polyester resin and the amorphous polyester resin. Therefore, it is not preferable in that the function of the crystalline polyester resin cannot be fully exhibited and the low-temperature fixability cannot be fully exhibited.

[0024] The maximum length of the crystalline polyester resin particles in the toner can be measured by observing the cross section of an ultrathin slice of the toner with a transmission electron microscope (TEM) and measuring the maximum length of the crystalline polyester resin particles based on the observed image.

[0025] (TEM observation and measurement) The toner thus prepared is embedded in an epoxy resin and hardened. Ultrathin sections (approximately 100 nm thick) of the toner are prepared using an ultramicrotome (ULTRACUT UCT, manufactured by Leica, using a diamond knife).

[0026] The sample is exposed to gas using ruthenium tetroxide, osmium tetroxide, or another dye, etc., to distinguish and stain the crystalline polyester resin phase from the other parts. The exposure time is adjusted appropriately depending on the contrast during observation. Then, the sample is observed using a transmission electron microscope (JEM-2100, manufactured by JEOL) at an accelerating voltage of 100 kV. Depending on the composition of the crystalline polyester resin and the non-crystalline polyester resin, it may be possible to distinguish them without staining, in which case they are evaluated without staining. It is also possible to pretreat the sample by applying composition contrast using another method such as selective etching. After pretreatment, the crystalline polyester resin part may be evaluated by observing it using a transmission microscope.

[0027] The observed cross-sectional image is subjected to binarization processing using commercially available image processing software (e.g., Image-Pro Plus, etc.) to calculate the maximum length of the crystalline polyester resin portion. A plurality of (e.g., 20) toner cross sections are observed to determine the maximum length of each crystalline polyester resin particle. The average value is taken as the maximum length D of the cross section of the crystalline polyester resin particle. However, the crystalline polyester resin particles for which the maximum length is measured do not include crystalline polyester resin particles having a maximum length of 10 nm or less.

[0028] [Center-to-center distance L of crystalline polyester resin particles] The center-to-center distance L of the crystalline polyester resin particles is preferably at least twice, and more preferably at least three times, the maximum cross-sectional length D of the crystalline polyester resin particles. When the center-to-center distance L of the crystalline polyester resin particles is at least twice the maximum cross-sectional length D of the crystalline polyester resin particles, the toner can be uniformly melted, and the adhesive force between the toner particles can be reduced.

[0029] The center-to-center distance L is determined by identifying the smallest part in the same image as when determining the above [Maximum length D of the cross section of the crystalline polyester resin particle], and determining the intersection with the maximum length. The one with the shortest distance to the intersection of other crystalline polyester resin particles is selected, and that distance is determined. The average value of all center-to-center distances L is taken as the center-to-center distance L of the crystalline polyester resin particles of the selected toner particles. This is performed for the 20 toner particles for which the maximum length D was determined, and the average value is taken as the center-to-center distance L of the crystalline polyester resin particles. Note that the crystalline polyester resin particles for which the center-to-center distance L is measured do not include crystalline polyester resin particles whose maximum length is 10 nm or less.

[0030] [Coefficient of variation (CV value) of crystalline polyester resin particles] The coefficient of variation (CV value) of the crystalline polyester resin particles represents the ratio of the standard deviation of the center-to-center distance L of the crystalline polyester resin particles present in the toner particle to the average value, and indicates the distribution of the distance between the crystalline polyester resin particles. The CV value is obtained by dividing the standard deviation of the center-to-center distance L of the crystalline polyester resin particles present in the toner particle by the average value and multiplying the result by 100 (coefficient of variation = standard deviation / average value x 100 (%)). The CV value can be the average value of the CV values ​​of multiple (e.g., 20) toner particles.

[0031] If the CV value is 50% or less, the toner can be melted evenly and the adhesive force between the toner particles can be reduced. If the CV value is 30% or less, the distance between the crystalline polyester resin particles can be kept uniform, so the toner can be melted more evenly and the adhesive force between the toner particles can be further reduced.

[0032] The toner according to an embodiment contains, as described above, a crystalline polyester resin and a non-crystalline polyester resin as a binder resin. The toner according to an embodiment may contain a binder resin other than the non-crystalline polyester resin and the non-crystalline polyester resin, and may contain other components such as a colorant and a release agent as necessary.

[0033] [Crystalline polyester resin] The crystalline polyester resin is obtained from a polyhydric alcohol and a polycarboxylic acid such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, or a derivative thereof. Note that the crystalline polyester resin refers to a resin obtained by modifying a polyester resin, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, or a derivative thereof, as described above, and does not include a modified polyester resin obtained by crosslinking and / or elongating a modified polyester resin having a urethane bond and / or a urea bond, as described below, and a polymer (prepolymer) that can react with an active hydrogen group-containing compound.

[0034] (Polyhydric alcohol) The polyhydric alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diols and trihydric or higher alcohols.

[0035] Examples of the diol include saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred. If the saturated aliphatic diol is a branched type, the crystallinity of the crystalline polyester resin may decrease, resulting in a decrease in melting point. In addition, if the carbon number of the saturated aliphatic diol exceeds 12, it becomes difficult to obtain a practical material.

[0036] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosanedecanediol, etc. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred in terms of high crystallinity of the crystalline polyester resin and excellent sharp melt properties.

[0037] Examples of trihydric or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, etc. These may be used alone or in combination of two or more.

[0038] (Polycarboxylic Acid) The polyvalent carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids.

[0039] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid.Furthermore, anhydrides and lower (1 to 3 carbon atoms) alkyl esters of these may also be mentioned.

[0040] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, as well as their anhydrides and lower (carbon number 1 to 3) alkyl esters, etc. These may be used alone or in combination of two or more.

[0041] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms, which provides high crystallinity and excellent sharp melting properties, and therefore can exhibit excellent low-temperature fixing properties.

[0042] In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method of designing and using a non-linear polyester obtained by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component or a trivalent or higher polycarboxylic acid such as trimellitic anhydride to the acid component during polyester synthesis and carrying out condensation polymerization.

[0043] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement of the solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc., but it can be easily confirmed by infrared absorption spectrum at 965±10cm -1 Or 990±10cm -1 Examples include those having absorption due to the δCH (out-of-plane bending vibration) of olefins.

[0044] Regarding the molecular weight, the viewpoint that a low molecular weight with a sharp molecular weight distribution is excellent in low temperature fixability, and that a large amount of low molecular weight components deteriorates heat resistance storage stability is taken into consideration. A molecular weight distribution diagram is used in which the horizontal axis is log (M) and the vertical axis is mass % for the molecular weight distribution of the soluble matter in o-dichlorobenzene by gel permeation chromatography (GPC). The peak position of the molecular weight distribution diagram is in the range of 3.5 to 4.0, and the half width of the peak is 1.5 or less. The weight average molecular weight (Mw) is preferably 3,000 to 30,000, and more preferably 5,000 to 15,000. The number average molecular weight (Mn) is preferably 1,000 to 10,000, and more preferably 2,000 to 10,000. The Mw / Mn is preferably 1.0 to 10, and more preferably 1.0 to 5.0.

[0045] The acid value of the crystalline polyester resin is preferably 5 mgKOH / g or more in order to achieve the desired low-temperature fixability from the viewpoint of the affinity between the paper and the resin, and more preferably 7 mgKOH / g or more in order to prepare fine particles by the phase inversion emulsification method, while the acid value of the crystalline polyester resin is preferably 45 mgKOH / g or less in order to improve the hot offset property.

[0046] The hydroxyl value of the crystalline polyester resin is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 50 mgKOH / g, in order to achieve a predetermined low-temperature fixability and good charging characteristics.

[0047] [Non-crystalline polyester resin] The non-crystalline polyester resin has sufficient flexibility even when it has a low molecular weight, and as a binder resin, it can have a function of sharply melting during fixing and smoothing the image surface.

[0048] Examples of the non-crystalline polyester resin include an unmodified polyester resin that does not have a urethane bond and / or a urea bond, and a modified polyester resin that has a urethane bond and / or a urea bond.

[0049] The amorphous polyester resin preferably contains a modified polyester resin having a urethane bond and / or a urea bond. By containing a modified polyester resin having a urethane bond and / or a urea bond, it is possible to ensure heat-resistant storage stability by crosslinking and to increase the latitude of low-temperature fixing design.

[0050] (Unmodified polyester resin having no urethane bond and / or urea bond) The unmodified polyester resin is a polyester resin obtained using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic anhydride, or a polycarboxylic ester, and is not modified with an isocyanate compound or the like.

[0051] The polyhydric alcohol includes, for example, diols.

[0052] Examples of diols include alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of bisphenol A such as polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol, propylene glycol; hydrogenated bisphenol A; and alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of hydrogenated bisphenol A. These may be used alone or in combination of two or more.

[0053] Examples of polycarboxylic acids include dicarboxylic acids.

[0054] Examples of dicarboxylic acids include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, and succinic acids substituted with an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, such as dodecenylsuccinic acid and octylsuccinic acid. In particular, from the viewpoint of heat-resistant storage stability, it is preferable to contain 50 mol % or more of terephthalic acid. These may be used alone or in combination of two or more.

[0055] Furthermore, the unmodified polyester resin may contain a trivalent or higher carboxylic acid and / or a trivalent or higher alcohol at the end of the resin chain in order to adjust the acid value and hydroxyl value.

[0056] Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, and acid anhydrides thereof.

[0057] Examples of trihydric or higher alcohols include glycerin, pentaerythritol, and trimethylolpropane.

[0058] The molecular weight of the unmodified polyester resin is not particularly limited and can be appropriately selected according to the purpose. If the molecular weight is too low, the heat-resistant storage stability of the toner and durability against stress such as stirring in a developing machine may decrease, and if the molecular weight is too high, the viscoelasticity of the toner when melted may increase, resulting in a decrease in low-temperature fixability. Therefore, in GPC measurement, the weight-average molecular weight (Mw) of the unmodified polyester resin is preferably 3,000 to 10,000, more preferably 4,000 to 7,000. The number-average molecular weight (Mn) is preferably 1,000 to 4,000, more preferably 1,500 to 3,000. The Mw / Mn is preferably 1.0 to 4.0, more preferably 1.0 to 3.5.

[0059] In addition, if the amount of the component having a molecular weight of 600 or less is too large, the toner may have poor heat-resistant storage stability and poor durability against stress such as stirring in a developing machine, whereas if the amount of the component having a molecular weight of 600 or less is too small, the toner may have poor low-temperature fixability. Therefore, the content of the component having a molecular weight of 600 or less is preferably 2% by mass to 10% by mass.

[0060] The unmodified polyester resin may be purified by extracting it with methanol to remove components having a molecular weight of 600 or less.

[0061] The acid value of the unmodified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 50 mgKOH / g, more preferably 5 to 30 mgKOH / g. When the acid value is 1 mgKOH / g or more, the toner tends to be negatively charged, and furthermore, the affinity between the paper and the toner is improved when fixed to the paper, and low-temperature fixability can be improved. On the other hand, when the acid value is 50 mgKOH / g or less, the problem of the charge stability, particularly the charge stability against environmental changes, decreasing can be effectively prevented.

[0062] The hydroxyl value of the unmodified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 mgKOH / g or more.

[0063] The glass transition point (also referred to as glass transition temperature) Tg of the unmodified polyester resin is preferably 40° C. to 80° C., more preferably 50° C. to 70° C. If the Tg is 40° C. or higher, the toner can be prevented from lowering in heat-resistant storage stability and durability against stress such as stirring in a developing machine, and from lowering in filming resistance. On the other hand, if the Tg is 80° C. or lower, the toner can be sufficiently deformed by heating and pressure during fixing, and can be sufficiently fixed at low temperatures.

[0064] (Modified polyester resin having urethane bonds and / or urea bonds) The modified polyester resin having a urethane bond and / or a urea bond is not particularly limited and can be appropriately selected depending on the purpose. The urethane bond or the urea bond behaves like a pseudo-crosslinking point, strengthens the rubber-like properties of the polyester resin, and can improve the heat-resistant storage stability of the toner, so that the resin can exhibit a function of improving adhesion to a recording medium such as paper.

[0065] The modified polyester resin having a urethane bond and / or a urea bond is preferably a resin that behaves like rubber in the temperature environment in which the toner is used, and therefore it is more preferable that the modified polyester resin having a urethane bond and / or a urea bond exhibits viscoelastic behavior such that it has a glass transition temperature Tg in a low temperature range of 20° C. or lower and has a rubber-like flat region in an environment of room temperature or higher.

[0066] The modified polyester resin having a urethane bond and / or a urea bond contains, as constituent components, a diol component and a crosslinking component, and preferably further contains a dicarboxylic acid component.

[0067] ((Diol component)) The diol component preferably has an odd number of carbon atoms in the main chain and has an alkyl group in the side chain, and preferably has a structure represented by the following general formula (1) similar to the linear saturated aliphatic diol having 3 to 10 carbon atoms. HO-(CR 1 R 2 ) n -OH (1) (In the above formula, R 1 and R 2 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms; n represents an odd number from 3 to 9. In the n repeating units, R 1 and R 2 may be the same or different.)

[0068] The diol component is not particularly limited and can be appropriately selected according to the purpose. Examples of the diol component include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetrafluoroethylene glycol. Examples of the diols include diols having an oxyalkylene group such as methylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols such as bisphenols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added. Among these, aliphatic diols having 4 to 12 carbon atoms are preferred. These diol components may be used alone or in combination of two or more.

[0069] ((Crosslinking component)) The crosslinking component contains a trihydric or higher aliphatic alcohol. The trihydric or higher aliphatic alcohol is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, dipentaerythritol, etc. Among these, it is preferable to contain a trihydric or tetrahydric aliphatic alcohol from the viewpoint of the gloss and image density of the fixed image. These trihydric or higher aliphatic alcohols may be used alone or in combination of two or more.

[0070] ((Dicarboxylic acid component)) The dicarboxylic acid component is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, etc. In addition, anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides of these may also be used.

[0071] Examples of the aliphatic dicarboxylic acid include succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid.

[0072] Examples of aromatic dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, etc. Among these, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred. These dicarboxylic acids may be used alone or in combination of two or more.

[0073] ((Modified polyester resin)) The modified polyester resin having a urethane bond and / or a urea bond preferably contains a modified polyester resin (adhesive substrate) as a constituent. The modified polyester resin can be appropriately selected according to the purpose, and examples thereof include a resin obtained by elongation reaction and / or crosslinking reaction of an active hydrogen group-containing compound and a polymer (hereinafter sometimes referred to as "prepolymer") that can react with the active hydrogen group-containing compound. The elongation reaction and / or crosslinking reaction may be terminated by a reaction terminator (diethylamine, dibutylamine, butylamine, laurylamine, a monoamine such as a ketimine compound, etc., which is blocked).

[0074] -Active hydrogen group-containing compounds- The active hydrogen group-containing compound can function as an elongation agent and a crosslinking agent when a prepolymer undergoes an elongation reaction and / or a crosslinking reaction in an aqueous medium (aqueous solvent) to produce a polyester resin.

[0075] The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds.

[0076] The active hydrogen group-containing compound is not particularly limited as long as it has an active hydrogen group, and can be appropriately selected according to the purpose. When the prepolymer is an isocyanate group-containing prepolymer described later, the active hydrogen group-containing compound is preferably an amine, since it can be made into a high molecular weight with the isocyanate group-containing prepolymer.

[0077] Examples of amines include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, and blocked amino groups of these. These may be used alone or in combination of two or more. Among these, diamines or mixtures of diamines and small amounts of trivalent or higher amines are preferred.

[0078] Examples of the diamine include aromatic diamines, alicyclic diamines, and aliphatic diamines. Examples of the aromatic diamines include phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane. Examples of the alicyclic diamines include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine. Examples of the aliphatic diamines include ethylenediamine, tetramethylenediamine, and hexamethylenediamine.

[0079] Examples of the trivalent or higher amine include diethylenetriamine and triethylenetetramine.

[0080] Examples of amino alcohols include ethanolamine and hydroxyethylaniline.

[0081] Examples of amino mercaptans include aminoethyl mercaptan and aminopropyl mercaptan.

[0082] Examples of the amino acid include aminopropionic acid and aminocaproic acid.

[0083] Examples of compounds in which the amino group is blocked include ketimine compounds and oxazoline compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.

[0084] -Polymers capable of reacting with compounds containing active hydrogen groups- The polymer (prepolymer) capable of reacting with the active hydrogen group-containing compound is not particularly limited as long as it is a polymer having at least a site capable of reacting with the active hydrogen group-containing compound, and can be appropriately selected according to the purpose, and examples thereof include polyol resin, polyacrylic resin, polyester resin, epoxy resin, and derivatives thereof. These may be used alone or in combination of two or more. Among these, polyester resin having an active hydrogen group is preferred in terms of high fluidity and transparency when melted.

[0085] An example of a polyester resin having an active hydrogen group is a polyester resin having a hydroxyl group.

[0086] The site of the prepolymer that can react with the active hydrogen group-containing compound includes an isocyanate group, an epoxy group, a carboxyl group, a functional group represented by -COCl, etc. These may be used alone or in combination of two or more. Among these, an isocyanate group is preferred.

[0087] In other words, the prepolymer is preferably a polyester resin having an isocyanate group capable of generating a urea bond, since it is easy to adjust the molecular weight of the polymer component and it has oil-less low-temperature fixing properties in a dry toner, and in particular, it is possible to ensure good releasability and fixing properties even when there is no mechanism for applying release oil to the heating medium for fixing.

[0088] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include diisocyanates and tri- or higher valent isocyanates.

[0089] Examples of diisocyanates include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactams, etc.

[0090] Examples of the aliphatic diisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate.

[0091] Examples of the alicyclic diisocyanate include isophorone diisocyanate and cyclohexylmethane diisocyanate.

[0092] Examples of aromatic diisocyanates include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, and 4,4'-diisocyanato-diphenyl ether.

[0093] Examples of the aromatic aliphatic diisocyanate include α,α,α',α'-tetramethylxylylene diisocyanate.

[0094] Examples of isocyanurates include tris(isocyanatoalkyl)isocyanurate, tris(isocyanatocycloalkyl)isocyanurate, and the like.

[0095] These diisocyanates may be used alone or in combination of two or more.

[0096] The molecular structure of amorphous polyester resins and the like can be confirmed by NMR measurement in solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 and 990±10cm -1 One method is to detect a resin that does not have absorption due to olefin δCH (out-of-plane bending vibration) as a non-crystalline polyester resin.

[0097] [Vinyl polymer modified polyester resin] The toner according to an embodiment preferably contains a vinyl polymer modified polyester resin. The vinyl polymer modified polyester resin is a polymer obtained by modifying a crystalline polyester resin with either or both of styrene and a (meth)acrylic compound.

[0098] The crystalline polyester resin has affinity for both the crystalline polyester resin and the non-crystalline polyester resin, which are present in the toner as a matrix. Since the toner according to one embodiment contains a vinyl polymer modified polyester resin, the crystalline polyester resin particles can be stabilized in the toner, and therefore the crystalline polyester resin particles can be uniformly dispersed inside the toner.

[0099] When a method is used in which a dispersion liquid containing a crystalline polyester resin (crystalline polyester resin dispersion liquid) is blended into an oil phase and then the oil phase is formed into oil droplets in water, it is presumed that this has the effect of causing the crystalline polyester resin particles to remain inside the oil droplets in water.

[0100] The vinyl polymer modified polyester resin can be produced, for example, by a method including a process of polycondensation reaction (polycondensation process) with raw material monomers for the polyester resin portion, and a process of addition polymerization reaction (addition polymerization process) with raw material monomers for the vinyl resin portion.

[0101] The polycondensation step may be carried out before the addition polymerization step, after the addition polymerization step, or simultaneously with the addition polymerization step. In addition, the polycondensation step and the addition polymerization step are preferably carried out in the same vessel.

[0102] Instead of carrying out a polycondensation reaction, a prepolymerized polycondensation resin may be used.

[0103] When the polycondensation step and the addition polymerization step are carried out in parallel, a mixture containing raw material monomers for the vinyl resin portion can be dropped into a mixture containing raw material monomers for the polyester resin portion to cause the reaction.

[0104] As the (meth)acrylic compound, a (meth)acrylic acid alkyl ester is preferable. As the (meth)acrylic acid alkyl ester, methyl (meth)acrylate, ethyl (meth)acrylate, (iso)propyl (meth)acrylate, (iso)butyl (meth)acrylate, etc. are exemplified. It is preferable to use one or more of these.

[0105] In this specification, "(iso)" means both the case where this group is present and the case where it is not present, and the case where this group is not present means that it is normal. In addition, "(meth)acrylic acid" means acrylic acid, methacrylic acid, or both.

[0106] It is preferable that the raw material monomer of the vinyl resin portion further contains a styrene compound from the viewpoint of adjusting the glass transition temperature Tg of the toner in order to ensure storage stability.

[0107] Examples of the styrene compound include styrene, α-methylstyrene, vinyltoluene, and other styrene derivatives.

[0108] The alcohol component of the crystalline polyester preferably contains an aliphatic diol having 6 to 12 carbon atoms.

[0109] Examples of the aliphatic diol having 6 to 12 carbon atoms include 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, and 1,12-dodecanediol.

[0110] From the viewpoint of low-temperature fixability, the carboxylic acid component of the crystalline polyester resin preferably contains an aliphatic dicarboxylic acid compound having 4 to 14 carbon atoms.

[0111] Examples of the aliphatic dicarboxylic acid compound having 4 to 14 carbon atoms include succinic acid (number of carbon atoms: 4), suberic acid (number of carbon atoms: 8), azelaic acid (number of carbon atoms: 9), sebacic acid (number of carbon atoms: 10), dodecanoic diacid (number of carbon atoms: 12), tetradecanoic diacid (number of carbon atoms: 14), succinic acid having an alkyl or alkenyl group on the side chain, anhydrides of these acids, and alkyl esters of these acids having 1 to 3 carbon atoms.

[0112] In this embodiment, the carboxylic acid compound includes not only free acids but also anhydrides that decompose during a reaction to generate acids, and alkyl esters having a carbon number of 1 to 3. However, the number of carbon atoms of the alkyl group in the alkyl ester moiety is not included in the number of carbon atoms of the aliphatic dicarboxylic acid compound.

[0113] [Relationship between crystalline polyester resin and non-crystalline polyester resin] The compounding ratio (A / C) of the amount (A) of the non-crystalline polyester resin (including modified polyester resin) to the amount (C) of the crystalline polyester resin is preferably 95 / 5 to 70 / 30, more preferably 95 / 5 to 85 / 15. When the compounding ratio (A / C) is 95 / 5 to 70 / 30, low-temperature fixability and heat-resistant storage stability can be achieved at the same time. When the compounding ratio (A / C) is 95 / 5 or more, low-temperature fixability can be maintained well. When the compounding ratio (A / C) is 70 / 30 or less, the amount of crystalline polyester resin present on the outermost surface of the toner can be reduced, so that the deterioration of image quality, the deterioration of developer fluidity, and the deterioration of image density due to contamination of the photoreceptor and other members can be suppressed. In addition, when the compounding ratio (A / C) is 70 / 30 or less, the surface properties of the toner deteriorate, causing contamination of the carrier, and sufficient chargeability can be maintained for a long period of time, and the deterioration of environmental stability can be effectively suppressed.

[0114] [Other binder resins] The toner according to an embodiment may contain other binder resin components in addition to the above-mentioned crystalline polyester resin and non-crystalline polyester resin. The other binder resins are not particularly limited, and examples thereof include known binder resins such as silicone resins, styrene-acrylic resins, styrene resins, acrylic resins, epoxy resins, diene resins, phenol resins, terpene resins, coumarin resins, amide-imide resins, butyral resins, urethane resins, and ethylene-vinyl acetate resins.

[0115] A method for calculating and analyzing the blending amounts of components contained in the toner according to an embodiment will be described.

[0116] [Methods for calculating and analyzing the amounts of components contained in toner] The content of the crystalline polyester resin in the toner can be calculated by a known method. Each component such as the crystalline polyester resin is separated from the toner by GPC or the like, and the mass ratio of the constituent components can be calculated by analyzing each of the separated components using the analysis method described below. It can also be calculated by quantifying the crystalline polyester resin components by gas chromatography mass spectrometry (GCMS).

[0117] Separation of each component by GPC can be carried out, for example, by the following method. First, in a GPC measurement using tetrahydrofuran (THF) as the mobile phase, the eluate is fractionated using a fraction collector or the like, and fractions corresponding to the desired molecular weight portion of the full integral of the elution curve are collected. The collected eluate is concentrated and dried using an evaporator or the like, and the solid content is dissolved in a heavy solvent such as deuterated chloroform or deuterated THF, 1 H-NMR measurement is performed, and the constituent monomer ratio of the resin in the eluted components is calculated from the integral ratio of each element. Another method is to concentrate the eluate, hydrolyze it with sodium hydroxide, etc., and then qualitatively and quantitatively analyze the decomposition products by high performance liquid chromatography (HPLC), etc. to calculate the constituent monomer ratio.

[0118] (Means for separating components in toner) An example of a method for separating each component when analyzing a toner is described in detail. First, 1 g of toner is put into 100 mL of THF, and the solution is obtained by dissolving the soluble portion while stirring for 30 minutes under the condition of 25°C. This is filtered through a membrane filter with an opening of 0.2 μm to obtain the THF-soluble portion in the toner. Next, this is dissolved in THF to prepare a sample for GPC measurement, and is injected into the GPC used to measure the molecular weight of each resin described above. Meanwhile, a fraction collector is placed at the eluate outlet of the GPC, and the eluate is fractionated at a predetermined count, and the eluate is obtained at 5% area ratios from the start of elution of the elution curve (the rise of the curve). Next, for each elution portion, 30 mg of a sample is dissolved in 1 mL of deuterated chloroform, and 0.05 vol. % of tetramethylsilane (TMS) is added as a reference substance. The solution is filled into a 5 mm diameter glass tube for NMR measurement, and a spectrum is obtained by integrating 128 times at a temperature of 23° C. to 25° C. using a nuclear magnetic resonance apparatus (JNM-AL400, manufactured by JEOL Ltd.). The monomer composition and composition ratio of the crystalline polyester resin and amorphous polyester resin contained in the toner are determined from the peak integral ratio of the obtained spectrum.

[0119] The solubility parameter values ​​(SP values) of crystalline polyester resin and non-crystalline polyester resin (unit: cal 1 / 2 / cm 3 / 2 ) may be adjusted. If the difference in SP value (ΔSP) between the crystalline polyester resin and the non-crystalline polyester resin is too small, the crystalline polyester resin will plasticize and become compatible with the non-crystalline polyester resin, causing crystal growth and preventing the crystalline polyester resin particles from maintaining their spherical shape. On the other hand, if ΔSP is too large, the crystalline polyester resin will not plasticize and will not be able to exhibit low-temperature fixability. Therefore, ΔSP should be set to 1.40 cal. 1 / 2 / cm 3 / 2 ~1.65cal 1 / 2 / cm 3 / 2 is preferred.

[0120] <Other characteristics of toner and their measurement methods> Other characteristics of the toner according to the embodiment and methods for measuring the same will be described below.

[0121] [Measurement of particle size of crystalline polyester resin particles in crystalline polyester resin dispersion] The particle size of the crystalline polyester resin particles in the crystalline polyester resin dispersion can be measured, for example, using a Nanotrack particle size distribution measuring device UPA-EX150 (Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). As a specific measuring method, the crystalline polyester resin dispersion is adjusted to a measuring concentration range and measured. At that time, background measurement is performed in advance using only the dispersion solvent of the crystalline polyester resin dispersion. By this measuring method, the particle size of the crystalline polyester resin particles can be measured from several tens of nm to several μm. The particle size of the crystalline polyester resin refers to the volume average particle size (volume average diameter).

[0122] In this embodiment, the particle size of the crystalline polyester resin in the crystalline polyester resin dispersion is preferably 100 nm to 500 nm, and more preferably 210 nm to 500 nm.

[0123] [Measuring method of melting point and glass transition temperature Tg] The melting point and glass transition temperature Tg of the toner can be measured, for example, using a DSC system (differential scanning calorimeter) ("Q-200", manufactured by TA Instruments Co., Ltd.) Specifically, the melting point and glass transition temperature Tg of the target sample can be measured by the following procedure.

[0124] First, about 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace. Next, in a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a heating rate of 10°C / min (first heating). After that, the sample is cooled from 150°C to -80°C at a heating rate of 10°C / min, and further heated to 150°C at a heating rate of 10°C / min (second heating). During each of the first and second heating, a DSC curve is measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments).

[0125] From the obtained DSC curves, the DSC curve at the first temperature rise can be selected using the analysis program in the Q-200 system, and the glass transition temperature at the first temperature rise of the target sample can be obtained. Similarly, the DSC curve at the second temperature rise can be selected, and the glass transition temperature at the second temperature rise of the target sample can be obtained.

[0126] Furthermore, from the obtained DSC curves, the analysis program in the Q-200 system can be used to select the DSC curve during the first heating and determine the endothermic peak top temperature during the first heating of the target sample as the melting point. Similarly, the DSC curve during the second heating can be selected and the endothermic peak top temperature during the second heating of the target sample as the melting point.

[0127] In this embodiment, unless otherwise specified, the melting points and Tg of the constituent components are the endothermic peak top temperature and Tg during the first temperature rise, respectively, of the target samples.

[0128] [Molecular weight] The molecular weight of the crystalline polyester resin, non-crystalline polyester resin, vinyl polymer modified polyester resin, etc., used can be measured by GPC under the following conditions, unless otherwise specified. Equipment: HLC-8220GPC (Tosoh Corporation) Column: TSKgel (registered trademark) SuperHZM-Mx3 (manufactured by Tosoh Corporation) ·Temperature: 40℃ Solvent: THF (tetrahydrofuran) ·Flow rate: 0.35mL / min Sample: 0.01mL of sample with a concentration of 0.05 to 0.6%

[0129] From the molecular weight distribution of the toner resin measured under the above conditions, the weight average molecular weight Mw is calculated using a molecular weight calibration curve prepared from a monodisperse polystyrene standard sample.

[0130] Ten monodisperse polystyrene standard samples were used: 5.8×100, 1.085×10000, 5.95×10000, 3.2×100000, 2.56×1000000, 2.93×1000, 2.85×10000, 1.48×100000, 8.417×100000, and 7.5×1000000.

[0131] [Other ingredients] The toner according to an embodiment may also contain other components such as a colorant, a release agent, resin fine particles, a charge control agent, inorganic fine particles, a flowability improver, a cleaning property improver, a magnetic material, and a metal soap.

[0132] (Coloring agent) The colorant is not particularly limited and can be appropriately selected from known dyes and pigments depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, Anthrazan Yellow BGL, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Nent Red F5R, Brilliant Carmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Celery Unblue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold,Examples of the pigments include acid green lake, malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone. These pigments may be used alone or in combination of two or more.

[0133] The content of the colorant in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1% by mass to 15% by mass, more preferably 3% by mass to 10% by mass. If the content of the colorant is 1% by mass or more, the decrease in the coloring power of the toner can be prevented, and if it is 15% by mass or less, the decrease in the coloring power and the decrease in the electrical properties of the toner due to poor dispersion of the pigment in the toner can be effectively prevented.

[0134] The colorant may be used as a master batch composited with a resin. The resin is not particularly limited and can be appropriately selected from known resins according to the purpose, and examples thereof include polyester, polymers of styrene or its substitutes, styrene-based copolymers, polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic hydrocarbon resins, alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, and paraffin wax. These may be used alone or in combination of two or more.

[0135] Examples of the polymer of styrene or its substitute include polyester resin, polystyrene, poly(p-chlorostyrene), polyvinyltoluene, etc. Examples of the styrene-based copolymer include styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α-methyl chloromethacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-acrylonitrile-indene copolymer, styrene-maleic acid copolymer, styrene-maleic acid ester copolymer, etc.

[0136] The master batch can be produced by mixing or kneading the master batch resin and the colorant under high shear force. In this case, it is preferable to add an organic solvent to enhance the interaction between the colorant and the resin. The so-called flushing method is also suitable in that the wet cake of the colorant can be used as is and does not need to be dried. The flushing method is a method in which an aqueous paste containing water of the colorant is mixed or kneaded with a resin and an organic solvent, and the colorant is transferred to the resin side to remove water and organic solvent components. For the mixing or kneading, a high shear dispersion device such as a three-roll mill is preferably used. It is well known that a colorant deteriorates the charging performance of the toner when it is present on the toner surface. Therefore, by improving the compatibility with the resin as a master batch, the charging performance of the toner (environmental stability, charge retention ability, charge amount, etc.) can be improved.

[0137] (Release agent) The release agent is not particularly limited and can be appropriately selected depending on the purpose, but a release agent having a low melting point of 50° C. to 120° C. is preferable. The release agent having a low melting point effectively acts as a release agent between the fixing roller and the toner interface by being dispersed in the resin, and as a result, the hot offset property is good even in an oil-less system (no release agent such as oil is applied to the fixing roller).

[0138] Suitable examples of the release agent include waxes. Examples of the waxes include vegetable waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusine; and natural waxes such as petroleum waxes such as paraffin, microcrystalline, and petrolatum. In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; synthetic waxes such as esters, ketones, and ethers; and the like. Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups on the side chains may be used. These may be used alone or in combination of two or more.

[0139] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50°C to 120°C, more preferably 60°C to 90°C. If the melting point is 50°C or higher, the wax can be prevented from adversely affecting the heat-resistant storage stability, and if the melting point is 120°C or lower, the problem of cold offset occurring during fixing at low temperatures can be effectively prevented. The melt viscosity of the release agent is preferably 5 cps to 1,000 cps, more preferably 10 cps to 100 cps, as measured at a temperature 20°C higher than the melting point of the release agent. If the melt viscosity is 5 cps or higher, the release property can be prevented from decreasing, and if it is 1,000 cps or lower, the effects of hot offset resistance and low-temperature fixing property can be sufficiently exhibited. The content of the release agent in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, more preferably 3% by mass to 30% by mass. If the content is 40% by mass or lower, the fluidity of the toner can be prevented from deteriorating.

[0140] (Resin fine particles) The resin of the resin microparticles is not particularly limited as long as it is a resin that can form an aqueous dispersion in an aqueous medium, and can be appropriately selected from known resins according to the purpose. The resin for the resin microparticles may be a thermoplastic resin or a thermosetting resin, and for example, vinyl resin, polyurethane resin, epoxy resin, polyester resin, polyamide resin, polyimide resin, silicon resin, phenol resin, melamine resin, urea resin, aniline resin, ionomer resin, polycarbonate resin, etc. can be used. These may be used alone or in combination of two or more. Among these, it is preferable to form at least one selected from vinyl resin, polyurethane resin, epoxy resin and polyester resin, in that it is easy to obtain an aqueous dispersion of fine spherical resin microparticles.

[0141] Incidentally, the vinyl resin is a polymer obtained by homopolymerizing or copolymerizing a vinyl monomer, and examples thereof include styrene-(meth)acrylic acid ester resin, styrene-butadiene copolymer, (meth)acrylic acid-acrylic acid ester polymer, styrene-acrylonitrile copolymer, styrene-maleic anhydride copolymer, and styrene-(meth)acrylic acid copolymer.

[0142] (Charge control agent) The charge control agent is not particularly limited and can be appropriately selected from known agents according to the purpose, and examples thereof include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus alone or its compounds, tungsten alone or its compounds, fluorine-based activators, metal salts of salicylic acid, metal salts of salicylic acid derivatives, etc. These may be used alone or in combination of two or more.

[0143] The charge control agent may be a commercially available product, and examples of the commercially available product include resins or compounds having an electron-donating functional group, azo dyes, and metal complexes of organic acids. Specifically, Nigrosine dyes such as Bontron 03, quaternary ammonium salts such as Bontron P-51, metal-containing azo dyes such as Bontron S-34, oxynaphthoic acid metal complexes such as E-82, salicylic acid metal complexes such as E-84, and phenol condensates such as E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), salicylic acid metal complexes such as TN-105, quaternary ammonium salt molybdenum complexes such as TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), quaternary ammonium salts such as Copy Charge PSY VP2038, triphenylmethane derivatives such as Copy Blue PR, quaternary ammonium salts such as Copy Charge NEG VP2036, and Copy Charge NX. Examples of suitable pigments include VP434 (all manufactured by Hoechst), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.

[0144] The charge control agent can be optionally contained in the resin phase of the toner particles by utilizing the difference in affinity to the resin in the toner particles. By selectively containing the charge control agent in the resin phase of the toner particles present in the inner layer, it is possible to suppress the charge control agent from being spent on other members such as the photoreceptor and the carrier. In the toner manufacturing method according to one embodiment, the arrangement of the charge control agent can be designed relatively freely, and an arbitrary arrangement can be adopted according to each image forming process.

[0145] (Inorganic fine particles) The inorganic fine particles are used as an external additive for imparting fluidity, developability, chargeability, etc. to the toner particles. The inorganic fine particles are not particularly limited and can be appropriately selected from known fine particles according to the purpose. For example, silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengala, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, silicon nitride, etc. can be used. These may be used alone or in combination of two or more.

[0146] As inorganic fine particles for aiding the fluidity, developability, and chargeability of toner particles, in addition to inorganic fine particles having a large particle size with a primary average particle size of 80 nm to 500 nm, inorganic fine particles having a small particle size can be preferably used. In particular, hydrophobic silica and hydrophobic titanium oxide are preferable. The primary average particle size of the inorganic fine particles is preferably 5 nm to 50 nm, and more preferably 10 nm to 30 nm. In addition, the specific surface area by the BET method is 20 m 2 / g~500m 2 The content of the inorganic fine particles in the toner is preferably 0.01% by mass to 5% by mass, and more preferably 0.01% by mass to 2.0% by mass.

[0147] (Flow improver) The flowability improver is an agent that improves hydrophobicity by surface treatment, and prevents the deterioration of flowability and charging properties even under high humidity.For example, it can be silane coupling agent, silylating agent, silane coupling agent with fluorinated alkyl group, organic titanate coupling agent, aluminum coupling agent, silicone oil, modified silicone oil, etc.It is particularly preferable that silica and titanium oxide are surface treated with such flowability improver and used as hydrophobic silica and hydrophobic titanium oxide.

[0148] (Cleaning improver) The cleaning improver is an agent added to the toner to remove the developer remaining on the photoconductor or primary transfer medium after transfer. Examples of the agent include zinc stearate, calcium stearate, fatty acid metal salts such as stearic acid, polymethyl methacrylate fine particles, polystyrene fine particles, and other polymer fine particles produced by soap-free emulsion polymerization. The polymer fine particles preferably have a relatively narrow particle size distribution, and the particle size is preferably 0.01 μm to 1 μm in volume average particle size.

[0149] (Magnetic material) The magnetic material is not particularly limited and can be appropriately selected from known materials depending on the purpose. For example, iron powder, magnetite, ferrite, etc. can be used. Among these, white materials are preferable in terms of color tone.

[0150] As described above, the toner according to one embodiment contains a crystalline polyester resin and a non-crystalline polyester resin, and the toner particles have an aspect ratio of 1.5 to 5 and a shape index of 0.75 or more, and are configured such that the center-to-center distance L between the cross-sections of the crystalline polyester resin particles contained in the toner particles is at least twice the maximum length D of the cross-section of the crystalline polyester resin particles.

[0151] In general, when crystalline polyester resin particles are present non-uniformly inside the toner, it is considered that the crystalline polyester resin particles are difficult to diffuse in the toner particles when melted, and plasticization is difficult to proceed. In addition, when multiple crystalline polyester resin particles approach each other, they tend to aggregate, so that when the crystalline polyester resin particles are exposed on the toner surface, they may spread on the toner surface and increase the adhesion of the toner. Furthermore, the crystalline polyester resin particles present near the surface of the toner tend to gather particularly easily on the convex parts of the toner particles.

[0152] Therefore, in order to plasticize the entire toner almost uniformly while preventing the crystalline polyester resin particles from being exposed on the toner surface, it is important to disperse the crystalline polyester resin particles inside the toner while preventing the crystalline polyester resin particles from being excessively close to each other inside the toner. It is also important to make the surface shape of the toner particles smooth by eliminating or reducing unevenness on the surface of the toner particles, and to make the toner particles have a shape with few contact points with the crystalline polyester resin particles.

[0153] Therefore, the center-to-center distance L of the crystalline polyester resin particles is set to a distance of at least twice the maximum cross-sectional length D of the crystalline polyester resin particles, and the crystalline polyester resin particles are dispersed as uniformly as possible inside the toner. If the crystalline polyester resin particles are dispersed uniformly inside the toner, the crystalline polyester resin particles dissolved during fixing can be diffused uniformly inside the toner, so that the entire toner can be plasticized uniformly. In addition, by dispersing the crystalline polyester resin particles inside the toner while maintaining a uniform distance, the crystalline polyester resin particles are less likely to be exposed on the surface of the toner, and the crystalline polyester resin particles can be prevented from spreading and overlapping when exposed on the toner surface, so that the adhesion force of the toner can be prevented from increasing.

[0154] By making the outer shape of the toner elliptical, which is distorted from a sphere, and by smoothing the surface shape of the toner particles, the number of contact points between the toner particles and the crystalline polyester resin particles present in the vicinity of the surfaces of the toner particles can be reduced, so that the plasticization of the entire toner and the reduction in the adhesive force of the toner can be more effectively achieved. Therefore, the toner according to one embodiment can improve low-temperature fixability and heat-resistant storage stability.

[0155] In addition, the crystalline polyester resin particles tend to spread on the contact surface due to mechanical pressure, and the toner particles tend to adhere to each other, resulting in transfer residue. By making the arrangement of the crystalline polyester resin particles uniform in the toner, it is possible to suppress image deterioration due to transfer omissions when the particles are packed by transfer pressure. Therefore, the toner according to one embodiment can improve image quality and cleaning properties.

[0156] Therefore, the toner according to one embodiment can have superior low-temperature fixing property, heat-resistant storage property, image quality and cleaning property.

[0157] The toner according to an embodiment can have a coefficient of variation (CV value) of crystalline polyester resin particles of 50% or less. As described above, the CV value represents the distribution of the distance between crystalline polyester resin particles. By making the CV value 50% or less, the variation in the center-to-center distance L of the crystalline polyester resin particles can be reduced, and the crystalline polyester resin particles can be more evenly dispersed inside the toner. Therefore, the toner according to an embodiment can plasticize the entire toner more evenly and can further reduce the adhesive force of the toner.

[0158] The toner according to an embodiment can have a standard deviation CV value of the center-to-center distance L of 30% or less. This can further reduce the variation in the center-to-center distance L of the crystalline polyester, and can disperse the crystalline polyester resin particles more evenly inside the toner. Therefore, the toner according to an embodiment can plasticize the entire toner more evenly and can further reduce the adhesive force of the toner.

[0159] The toner according to an embodiment may contain a vinyl polymer modified polyester resin. This allows each crystalline polyester resin particle to be stabilized in the toner. Therefore, the crystalline polyester resin particles can be uniformly dispersed and arranged inside the toner, so that the toner can further improve low-temperature fixability and heat-resistant storage stability.

[0160] <Toner manufacturing method> A toner manufacturing method according to one embodiment includes the steps of mixing a dispersion liquid containing a crystalline polyester (crystalline polyester dispersion liquid) with an oil phase containing a non-crystalline polyester resin to prepare a water-in-oil (W / O) emulsion in which the crystalline polyester is dispersed in the oil phase, and then mixing the water-in-oil (W / O) emulsion with an aqueous medium to prepare an oil-in-water (O / W) emulsion in which the crystalline polyester is dispersed in the aqueous medium, thereby producing toner base particles.

[0161] That is, the method for producing a toner according to an embodiment includes the following steps. A step of obtaining a solution by dissolving a crystalline polyester resin in an organic solvent (a step of producing a solution): A process of mixing the solution with an aqueous medium to generate crystalline polyester resin particles in the aqueous medium, and then removing the organic solvent to prepare a crystalline polyester resin dispersion containing the crystalline polyester resin particles in the aqueous medium (a process of preparing a crystalline polyester resin dispersion): A process for producing toner base particles by using a dissolution suspension method, by mixing a crystalline polyester resin dispersion with an oil phase to dissolve the crystalline polyester resin in the oil phase, and then mixing the mixture with an aqueous medium to disperse or emulsify the crystalline polyester resin in the aqueous medium (dissolution suspension process): A step of removing the organic solvent (organic solvent removal step):

[0162] Each step will be described below.

[0163] When an organic solvent, a neutralizing agent, and a surfactant are added to the crystalline polyester resin, a solution in which the crystalline polyester resin is dissolved in the organic solvent is obtained (solution generating step).

[0164] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include methanol, ethanol, propanol, IPA, butanol, ethyl acetate, MEK, and combinations thereof. Organic solvents having a boiling point of less than 150° C. are preferred because they are easily removed.

[0165] As the neutralizing agent, general acids and alkalis such as nitric acid, hydrochloric acid, sodium hydroxide, and ammonia can be used.

[0166] As the surfactant, one or more types of surfactants may be used. The surfactant may be selected from ionic surfactants and nonionic surfactants. Here, the term "ionic surfactant" is understood to include anionic surfactants and cationic surfactants.

[0167] Next, the solution is mixed with an aqueous medium to produce crystalline polyester resin particles in the aqueous medium, and then the organic solvent is removed to produce a crystalline polyester resin dispersion containing the crystalline polyester resin particles in the aqueous medium (crystalline polyester resin dispersion production process).

[0168] The crystalline polyester resin dispersion is preferably prepared by using a phase inversion emulsification method. The phase inversion emulsification method is a method in which an aqueous medium is dropped into a solution under stirring to obtain emulsified particles, and then an organic solvent is removed from a resin dispersion containing the solution and the aqueous medium to obtain an emulsion in which the crystalline polyester resin is dispersed or emulsified. In addition, heating is possible as necessary.

[0169] In addition, as a method for dispersing or emulsifying a crystalline polyester resin, for example, a method using a mechanical grinding device, a spray granulation method, a phase inversion emulsification method, etc. are available. When a mechanical grinding device is used, it is difficult to obtain fine particles with a narrow particle size distribution. When a phase inversion emulsification method is used, it is easy to control the particle size, and crystalline polyester resin particles with a narrow particle size distribution can be obtained. Therefore, as a method for dispersing or emulsifying a crystalline polyester resin in an aqueous medium, it is preferable to use a phase inversion emulsification method.

[0170] When the aqueous medium is mixed with the solution while stirring, crystalline polyester resin particles are produced in the aqueous medium as emulsified particles.

[0171] The method for removing the organic solvent contained in the resin dispersion containing the dissolving solution and the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. For example, a method of gradually increasing the temperature of the entire reaction system to evaporate the organic solvent in the oil droplets, a method of spraying the dispersion in a dry atmosphere to remove the organic solvent in the oil droplets, etc. can be mentioned.

[0172] The amount of the crystalline polyester resin particles added to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 parts by mass to 10 parts by mass with respect to 100 parts by mass of the aqueous medium.

[0173] The aqueous medium is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include water, a solvent miscible with water, and a mixture thereof. These may be used alone or in combination of two or more. Among these, water is preferred.

[0174] The water-miscible solvent can be appropriately selected depending on the purpose, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, and the like.

[0175] Examples of the alcohol include methanol, isopropanol, and ethylene glycol.

[0176] Examples of the lower ketones include acetone and methyl ethyl ketone.

[0177] Next, using a dissolution suspension method, the crystalline polyester resin dispersion is mixed into an oil phase and dissolved in the oil phase, and then mixed into an aqueous medium to disperse or emulsify the crystalline polyester resin in the aqueous medium, thereby producing toner base particles (dissolution suspension process).

[0178] Methods for introducing crystalline polyester resin particles produced by the phase inversion emulsification method into a toner include a pulverization method, an emulsion aggregation method, a dissolution suspension method, etc., but since the pulverization method and the emulsion aggregation method use heat in the process, it is difficult to maintain a spherical shape, and the crystalline polyester resin may be partially plasticized with the non-crystalline polyester resin due to heat. In contrast, the dissolution suspension method is a method in which a crystalline polyester resin or the like is dissolved in an organic solvent and dispersed or emulsified in an aqueous medium, and since it is easy to control the particle size and crystalline polyester resin particles with a narrow particle size distribution can be obtained, it is preferable to use the dissolution suspension method.

[0179] In addition, as described above, it is also important to adjust the SP value between the crystalline polyester resin and the non-crystalline polyester resin contained in the oil phase. If the difference in SP value (ΔSP) between the crystalline polyester resin and the non-crystalline polyester resin is too small, the crystalline polyester resin will plasticize and become compatible with the non-crystalline resin, so that the crystalline polyester resin will grow and the crystalline polyester resin will not be able to maintain a spherical shape. On the other hand, if ΔSP is too large, the plasticization of the crystalline polyester resin will not proceed, so that low-temperature fixability cannot be exhibited. In this embodiment, the dissolution suspension method is used to add an aqueous medium immediately after the oil phase is added to the crystalline polyester resin, thereby emulsifying or dispersing the crystalline polyester resin and the non-crystalline polyester resin, thereby suppressing the plasticization of the crystalline polyester resin and the non-crystalline polyester resin.

[0180] The dissolution and suspension process may include the following steps. A process (mixing process) of mixing the crystalline polyester resin dispersion with an oil phase in which a toner material containing a non-crystalline polyester resin is dissolved or dispersed to generate a water-in-oil (W / O type) emulsion in which the crystalline polyester resin particles are dispersed in the oil phase: A process for producing toner base particles by mixing a water-in-oil (W / O) emulsion with an aqueous medium to emulsify or disperse the emulsion to produce an oil-in-water (O / W) emulsion containing crystalline polyester particles dispersed in the aqueous medium (emulsification or dispersion process):

[0181] By mixing the crystalline polyester resin dispersion with an oil phase in which a toner material containing a non-crystalline polyester resin is dissolved or dispersed, a water-in-oil (W / O type) emulsion is generated in which the crystalline polyester resin particles are dispersed in the oil phase (mixing process).

[0182] The oil phase containing the toner materials can be prepared by dissolving or dispersing the toner materials containing the amorphous polyester resin in an organic solvent. The toner materials preferably contain a modified polyester resin having a urethane bond and / or a urea bond, a crystalline polyester resin, an active hydrogen group-containing compound, and a prepolymer, and may further contain a release agent, a colorant, etc.

[0183] The organic solvent can be appropriately selected depending on the purpose, but an organic solvent having a boiling point of less than 150° C. is preferable because it is easy to remove.

[0184] Examples of the organic solvent having a boiling point of less than 150° C. include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, and methyl isobutyl ketone. These may be used alone or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, and carbon tetrachloride are preferred, and ethyl acetate is more preferred.

[0185] Next, the water-in-oil (W / O) emulsion is mixed with an aqueous medium and emulsified or dispersed to produce an oil-in-water (O / W) emulsion containing crystalline polyester particles dispersed in the aqueous medium (emulsification or dispersion process).

[0186] The amount of the aqueous medium used when emulsifying or dispersing the toner materials can be appropriately selected depending on the purpose, and is preferably 50 parts by mass to 2,000 parts by mass, more preferably 100 parts by mass to 1,000 parts by mass, relative to 100 parts by mass of the toner materials. If the amount of the aqueous medium used is 50 parts by mass or more, the dispersion state of the toner materials can be prevented from becoming poor, and toner base particles of a predetermined particle size can be obtained. If the amount of the aqueous medium used is 2,000 parts by mass or less, production costs can be reduced.

[0187] The oil phase preferably contains an active hydrogen group-containing compound and a prepolymer. When the active hydrogen group-containing compound and the prepolymer are contained in the oil phase and / or the aqueous medium, the active hydrogen group-containing compound and the prepolymer are subjected to an elongation reaction and / or a crosslinking reaction to produce a modified polyester resin (adhesive substrate) and form toner base particles.

[0188] The time when the adhesive base material is produced is not particularly limited and can be appropriately selected.

[0189] The adhesive substrate may be produced, for example, by emulsifying or dispersing an oil phase containing a polymer reactive with active hydrogen groups, such as a polyester resin having an isocyanate group, together with an active hydrogen group-containing compound, such as an amine, in an aqueous medium, and subjecting both to an elongation reaction and / or crosslinking reaction in the aqueous medium.

[0190] The adhesive substrate may also be produced by emulsifying or dispersing an oil phase containing a polymer reactive to active hydrogen groups in an aqueous medium to which an active hydrogen group-containing compound has been added in advance, and then subjecting both to an elongation reaction and / or crosslinking reaction in the aqueous medium.

[0191] Furthermore, the adhesive substrate may be produced by emulsifying or dispersing an oil phase containing a polymer reactive to active hydrogen groups in an aqueous medium, adding an active hydrogen group-containing compound, and causing an elongation reaction and / or crosslinking reaction between the two from the particle interface in the aqueous medium. When causing an elongation reaction and / or crosslinking reaction between the two from the particle interface, the modified polyester resin is preferentially formed on the surface of the toner produced, and a concentration gradient of the modified polyester resin can also be provided in the toner.

[0192] The reaction conditions (reaction time, reaction temperature) for producing the adhesive substrate can be appropriately selected depending on the combination of the active hydrogen group-containing compound and the prepolymer.

[0193] The reaction time is preferably from 10 minutes to 40 hours, more preferably from 2 hours to 24 hours.

[0194] The reaction temperature is preferably from 0°C to 150°C, more preferably from 40°C to 98°C.

[0195] A method for stably forming a dispersion liquid containing a prepolymer in an aqueous medium can be appropriately selected depending on the purpose. For example, there is a method in which an oil phase prepared by dissolving or dispersing a toner material in a solvent is added to an aqueous medium, and the oil phase is dispersed by shear force.

[0196] The dispersing machine for dispersion can be appropriately selected depending on the purpose, and examples thereof include a low-speed shearing dispersing machine, a high-speed shearing dispersing machine, a friction dispersing machine, a high-pressure jet dispersing machine, an ultrasonic dispersing machine, etc. Among these, a high-speed shearing dispersing machine is preferred because it can control the particle size of the dispersion (oil droplets) to 2 μm to 20 μm.

[0197] When a high-speed shear type dispersing machine is used, the conditions such as the rotation speed, dispersing time, and dispersing temperature can be appropriately selected depending on the purpose.

[0198] The rotation speed is preferably from 1,000 rpm to 30,000 rpm, and more preferably from 5,000 rpm to 20,000 rpm.

[0199] In the case of a batch method, the dispersion time is preferably 0.1 to 5 minutes.

[0200] The dispersion temperature under pressure is preferably 0° C. to 150° C., more preferably 40° C. to 98° C. Generally, the higher the dispersion temperature, the easier the dispersion.

[0201] When emulsifying or dispersing the oil phase containing the toner materials, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion such as oil droplets, forming a desired shape, and sharpening the particle size distribution.

[0202] The dispersant can be appropriately selected depending on the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.

[0203] The surfactant can be appropriately selected depending on the purpose. For example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used.

[0204] Examples of anionic surfactants include alkylbenzene sulfonates, α-olefin sulfonates, phosphates, etc. Among these, those having a fluoroalkyl group are preferred.

[0205] [Method of adjusting the aspect ratio of toner base particles] The aspect ratio of the toner base particles can be adjusted by deforming the toner base particles and fixing the deformed shape. As a method of deforming the toner base particles and fixing the deformed shape, for example, there is a method of adjusting the viscosity of the toner base particles in a medium such as an air flow or a liquid. It is important for the viscosity of the toner base particles to have hysteresis between the shear force and the deformation in order to maintain the deformation of the toner base particles.

[0206] As a method for deforming the toner base particles and fixing the deformed shape, there is a method for adjusting the viscosity of the medium to make it a non-Newtonian fluid or a highly viscous body. The viscosity of the medium can be adjusted by a method of adjusting the viscosity of the medium itself by selecting the medium, a method of adjusting the viscosity in water using a water-soluble polymer, a method of adjusting the temperature of the medium, a solvent concentration, etc.

[0207] As a method for deforming the toner base particles and fixing the deformed shape, there is a method in which a solid substance having a high aspect ratio and a planar, needle-like or spindle-like shape is included.

[0208] [Method of adjusting the shape index of toner base particles] The shape index of the toner base particles can be adjusted by moderating the factor for adjusting the aspect ratio of the toner base particles when carrying out the above-mentioned [Method for adjusting the aspect ratio of the toner base particles] in order to adjust the surface smoothness of the toner base particles. In particular, it is preferable to adjust the shape index of the toner base particles by gently deforming only the surface of the toner base particles in a medium (in an air stream or in a liquid) after carrying out the above-mentioned [Method for adjusting the aspect ratio of the toner base particles].

[0209] Furthermore, by making a solid substance exist on the surface of the toner base particle, the degree of surface shrinkage of the toner base particle can be adjusted, and thus the shape index of the toner base particle can be adjusted.

[0210] Furthermore, the shape index of the toner base particles can be adjusted by removing sharp edges of the toner base particles, for example, by contacting the toner base particles with each other in an air stream or by contacting the toner base particles with a container wall or the like.

[0211] Next, the organic solvent is removed from the oil-in-water (O / W) emulsion (organic solvent removal step).

[0212] The organic solvent is removed from the oil-in-water (O / W) emulsion, and the toner base particles are recovered.

[0213] The method for removing the organic solvent from the oil-in-water (O / W type) emulsion can be appropriately selected depending on the purpose. For example, there is a method in which the temperature of the entire reaction system is gradually increased to evaporate the organic solvent in the oil droplets, or a method in which the dispersion liquid is sprayed into a dry atmosphere to remove the organic solvent in the oil droplets.

[0214] The recovered toner base particles may be washed, dried, and further classified.

[0215] The classification may be carried out by removing fine particles in the liquid using a cyclone, decanter, centrifugal separation or the like, or the classification operation may be carried out after drying.

[0216] The obtained toner base particles may be mixed with particles of an external additive, a charge control agent, etc. In this case, by applying a mechanical impact force, it is possible to suppress the particles of the external additive, etc. from being detached from the surface of the toner base particles.

[0217] The method of applying the mechanical impact force can be appropriately selected depending on the purpose, and examples thereof include a method of applying an impact force to the mixture using a blade rotating at high speed, a method of introducing the mixture into a high-speed air current to accelerate it, and causing particles to collide with each other or against an appropriate collision plate, etc.

[0218] The device used in the method of applying a mechanical impact force can be appropriately selected depending on the purpose, and examples include an Angmill (manufactured by Hosokawa Micron Corporation), a device obtained by modifying an I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) to reduce the grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), an automatic mortar, and the like.

[0219] As described above, the toner manufacturing method according to the embodiment includes the steps of mixing a crystalline polyester resin dispersion with an oil phase to prepare a water-in-oil (W / O) emulsion in which crystalline polyester resin particles are dispersed in the oil phase, and then mixing the water-in-oil (W / O) emulsion with an aqueous medium to produce an oil-in-water (O / W) emulsion in which crystalline polyester particles are dispersed in the aqueous medium.Then, the aspect ratio and shape index of the toner base particles produced in the oil-in-water (O / W) emulsion produced in the above step are adjusted.This allows the toner according to the embodiment to be obtained.

[0220] In addition, the toner manufacturing method according to the embodiment includes the above-mentioned steps, so that the crystalline polyester resin can be introduced and dispersed inside the toner. In addition, since the crystalline polyester resin dispersion is not directly mixed into the aqueous medium, but is mixed into the aqueous medium via an oil phase, adhesion of the crystalline polyester resin to the surface of the toner can be reduced.

[0221] In addition, in the toner manufacturing method according to an embodiment, in the preparation step of the crystalline polyester resin dispersion, the crystalline polyester resin dispersion is prepared by phase inversion emulsification, so that spherical crystalline polyester resin with a good particle size distribution can be produced. Therefore, spherical crystalline polyester resin with a good particle size distribution can be introduced into the toner. Furthermore, in the mixing step and the emulsification or dispersion step, aggregation of the crystalline polyester resin is unlikely to occur, and there is no step of applying excessive heat, so that plasticization of the crystalline polyester resin can be suppressed. Therefore, the heat-resistant storage stability of the toner can be maintained, and deterioration of adhesion can be prevented.

[0222] In addition, in the toner manufacturing method according to an embodiment, in the mixing step, it is preferable to mix a vinyl polymer modified polyester resin as a dispersion aid into an oil phase containing a crystalline polyester resin and a non-crystalline polyester resin. This makes it easier for the crystalline polyester resin to be drawn into the toner, and the crystalline polyester resin can be contained in a dispersed state inside the toner. Therefore, the crystalline polyester resin particles can be kept inside the oil droplets in the aqueous medium, and the crystalline polyester resin can be easily and uniformly dispersed inside the toner. In addition, by using a dispersion aid, it is possible to suppress adhesion of the crystalline polyester resin to the toner surface.

[0223] In addition, in the toner manufacturing method according to an embodiment, the oil phase may contain an active hydrogen group-containing compound and a prepolymer in the mixing step, which allows the toner base particles to be formed while an adhesive base material is produced by an elongation reaction and / or a crosslinking reaction between the active hydrogen group-containing compound and the prepolymer.

[0224] <Developer> The developer according to an embodiment includes the toner according to an embodiment, and may include other appropriately selected components such as a carrier, etc., as necessary. This can ensure proper toner fluidity even in a high-temperature, high-humidity environment, and can perform proper development and transfer with little contamination of the developing member, thereby providing a developer with high environmental stability (reliability).

[0225] The developer may be a one-component developer or a two-component developer. However, when used in high-speed printers that correspond to the recent improvements in information processing speed, a two-component developer is preferable from the viewpoint of improving the developer life.

[0226] When the developer is used as a one-component developer, even if the toner is balanced, there is little variation in the particle size of the toner, there is little filming of the toner on the developing roller, and there is little melting of the toner to components such as blades that thin the toner layer, and good and stable developability and images can be obtained even with long-term stirring in the developing device.

[0227] When the developer is used as a two-component developer, even if the toner is balanced over a long period of time, the particle size of the toner does not vary much, and good and stable developability and images can be obtained even with long-term stirring in a developing device.

[0228] When the toner according to the embodiment is used in a two-component developer, it can be mixed with a carrier and used as a developer. The content of the carrier in the two-component developer can be appropriately selected depending on the purpose, but is preferably 90 parts by mass to 98 parts by mass, more preferably 93 parts by mass to 97 parts by mass, based on 100 parts by mass of the two-component developer.

[0229] The developer according to an embodiment can be suitably used for image formation by various known electrophotographic methods such as a magnetic one-component development method, a non-magnetic one-component development method, and a two-component development method.

[0230] [Career] The carrier is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer (coating layer) that coats the core material.

[0231] (Core material) The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium-based material of 50 emu / g to 90 emu / g, manganese-magnesium-based material of 50 emu / g to 90 emu / g, etc. can be mentioned. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more, magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g, because it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for high image quality. These materials may be used alone or in combination of two or more.

[0232] The volume average particle diameter of the core material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 10 μm to 150 μm, more preferably 40 μm to 100 μm. If the volume average particle diameter is 10 μm or more, the amount of fine powder in the carrier increases, and the magnetization per particle decreases, which can effectively prevent the problem of carrier scattering. On the other hand, if it is 150 μm or less, the specific surface area decreases, which can cause toner scattering, and in full color with many solid parts, the problem of poor reproduction of the solid parts can be effectively prevented.

[0233] (Resin layer) The material of the resin layer is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include amino resins, polyvinyl resins, polystyrene resins, polyhalogenated olefins, polyester resins, polycarbonate resins, polyethylene, polyvinyl fluoride, polyvinylidene fluoride, polytrifluoroethylene, polyhexafluoropropylene, copolymers of vinylidene fluoride and acrylic monomers, copolymers of vinylidene fluoride and vinyl fluoride, fluoro terpolymers such as copolymers of tetrafluoroethylene, vinylidene fluoride and monomers not having a fluoro group, silicone resins, etc. These may be used alone or in combination of two or more.

[0234] Examples of amino resins include urea-formaldehyde resins, melamine resins, benzoguanamine resins, urea resins, polyamide resins, and epoxy resins.

[0235] Examples of the polyvinyl resin include acrylic resin, polymethyl methacrylate, polyacrylonitrile, polyvinyl acetate, polyvinyl alcohol, and polyvinyl butyral.

[0236] Examples of polystyrene resins include polystyrene and styrene-acrylic copolymers.

[0237] An example of the polyhalogenated olefin is polyvinyl chloride.

[0238] Examples of polyester resins include polyethylene terephthalate and polybutylene terephthalate.

[0239] The resin layer may contain conductive powder, etc., if necessary. The conductive powder is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include metal powder, carbon black, titanium oxide, tin oxide, zinc oxide, etc. The average particle diameter of the conductive powder is preferably 1 μm or less. If the average particle diameter is 1 μm or less, it is advantageous in terms of controlling the electrical resistance.

[0240] Examples of methods for forming the resin layer include a method in which a coating liquid is prepared by dissolving a silicone resin or the like in a solvent, the coating liquid is applied to the surface of the core material, dried, and then baked.

[0241] The coating method is not particularly limited and can be appropriately selected depending on the purpose. Examples of the coating method include a dip coating method, a spray method, and a brush coating method.

[0242] The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, and butyl cellosolve acetate.

[0243] The baking may be performed by an external heating method or an internal heating method, and specific examples thereof include a method using a fixed electric furnace, a fluidized electric furnace, a rotary electric furnace, a burner furnace, or the like, and a method using microwaves.

[0244] The content of the resin layer in the carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 5.0% by mass. When the content is 0.01% by mass or more, a uniform resin layer can be formed on the surface of the core material. When the content is 5.0% by mass or less, the resin layer does not become too thick, and fusion between carrier particles is suppressed, thereby improving the uniformity of the carrier.

[0245] <Toner storage unit> The toner storage unit according to the embodiment can store the toner according to the embodiment. The toner storage unit according to the embodiment refers to a unit having a function of storing toner and storing the toner. Here, examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge.

[0246] The toner storage container refers to a container that stores toner.

[0247] The developing device has a means for containing toner and developing the toner.

[0248] The process cartridge is a cartridge that integrates at least an electrostatic latent image carrier (also called an image carrier) and a developing means, contains toner, and is detachable from an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, a cleaning means, etc.

[0249] The toner storage unit according to the embodiment stores the toner according to the embodiment. By mounting the toner storage unit according to the embodiment on an image forming apparatus and forming an image, the toner according to the embodiment is used to form an image, so that a toner having superior low-temperature fixing property, heat-resistant storage stability, image quality, and cleaning property can be obtained.

[0250] [Image forming device] An image forming apparatus according to one embodiment has an electrostatic latent image carrier, an electrostatic latent image forming unit that forms an electrostatic latent image on the electrostatic latent image carrier, and a developing unit that develops the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, and may further have other components as necessary.

[0251] More preferably, the image forming apparatus according to one embodiment includes, in addition to the electrostatic latent image carrier, electrostatic latent image forming unit, and developing unit described above, a transfer unit that transfers the toner image onto a recording medium, and a fixing unit that fixes the transferred image onto the surface of the recording medium.

[0252] In the developing section, a toner according to an embodiment is used. Preferably, a developer containing the toner according to an embodiment and, if necessary, other components such as a carrier may be used to form a toner image.

[0253] (Electrostatic latent image carrier) The material, shape, structure, size, etc. of the electrostatic latent image carrier (sometimes called "electrophotographic photoreceptor" or "photoreceptor") are not particularly limited and can be appropriately selected from known materials. Examples of materials for the electrostatic latent image carrier include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors (OPC) such as polysilane and phthalopolymethine. Among these, organic photoreceptors (OPC) are preferred because they can provide higher resolution images. A preferred shape of the electrostatic latent image carrier is a drum shape.

[0254] (Electrostatic latent image forming section) The electrostatic latent image forming unit is not particularly limited as long as it is a means for forming an electrostatic latent image on an electrostatic latent image carrier, and can be appropriately selected according to the purpose. The electrostatic latent image forming unit includes, for example, a charging member (charger) for uniformly charging the surface of the electrostatic latent image carrier, and an exposure member (exposure device) for imagewise exposing the surface of the electrostatic latent image carrier.

[0255] The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger equipped with a conductive or semiconductive roll, brush, film, rubber blade, etc., and a non-contact charger that utilizes corona discharge such as a corotron or scorotron.

[0256] The charger is preferably one that is arranged in contact or non-contact with the electrostatic latent image carrier and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the electrostatic latent image carrier. Also, the charger is preferably a charging roller that is arranged in close proximity to the electrostatic latent image carrier in a non-contact manner via a gap tape and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the charging roller.

[0257] The exposure device is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charger in an image to be formed, and can be appropriately selected depending on the purpose, and examples thereof include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, a liquid crystal shutter optical system, etc. Note that a light back system in which exposure is performed in an image from the back side of the electrostatic latent image carrier may be adopted.

[0258] (Developing section) The developing unit is not particularly limited as long as it can develop the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, and can be appropriately selected according to the purpose. For example, the developing unit can be suitably used one that contains toner and has a developing device that can apply the toner to the electrostatic latent image in a contact or non-contact manner, and a developing device equipped with a toner container is preferable.

[0259] The developing device may be a single-color developing device or a multi-color developing device, and a suitable example is one having an agitator that charges the toner by friction and agitation, and a rotatable magnetic roller.

[0260] (Transfer section) The transfer section preferably has a first transfer section that transfers a visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer section that transfers the composite transfer image onto a recording medium. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose, and a transfer belt or the like is preferably used.

[0261] The transfer section (first transfer means and second transfer section) preferably has at least a transfer device that peels and charges a visible image formed on an electrostatic latent image carrier (photoconductor) onto a recording medium. The number of transfer sections may be one or more.

[0262] Examples of the transfer device include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, an adhesive transfer device, etc. The recording medium is not particularly limited and can be appropriately selected from known recording media (recording paper).

[0263] (Fixing part) The fixing unit is not particularly limited and can be appropriately selected depending on the purpose, but a known heating and pressing unit is suitable. Examples of the heating and pressing unit include a combination of a heating roller and a pressure roller, and a combination of a heating roller, a pressure roller, and an endless belt.

[0264] The fixing section is preferably a heating and pressing section having a heating body having a heating element, a film in contact with the heating body, and a pressure member in pressure contact with the heating body through the film, and capable of passing a recording medium on which an unfixed image has been formed between the film and the pressure member to perform heat fixing. Heating in the heating and pressing section is usually preferably 80°C to 200°C. In this embodiment, for example, a known optical fixing device may be used together with or instead of the fixing section depending on the purpose.

[0265] (others) The image forming apparatus according to the first embodiment may further include, for example, a static eliminator, a recycle unit, a controller, and the like.

[0266] ((Static charge removal section)) The charge removing section is not particularly limited as long as it can apply a charge removing bias to the electrostatic latent image bearing member, and can be appropriately selected from among known charge removers. For example, a charge removing lamp or the like is preferably used.

[0267] (Cleaning Department) The cleaning unit may be any type capable of removing the toner remaining on the electrostatic latent image carrier, and may be appropriately selected from among known cleaners. Examples of the cleaning unit include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, and a web cleaner.

[0268] As described above, since the toner according to the primary embodiment has excellent cleaning properties, it is preferable that the image forming apparatus according to the embodiment has a cleaning unit. By applying the toner to an image forming apparatus having a cleaning unit, the cleaning properties can be improved. That is, by controlling the adhesion between toner particles, the fluidity of the toner can be controlled, and the cleaning properties can be improved. In addition, by controlling the characteristics of the toner after deterioration, it is possible to maintain excellent cleaning quality even under severe conditions such as long life and high temperature and humidity. Furthermore, since the external additive can be sufficiently liberated from the toner on the photoreceptor, a deposition layer (dam layer) of the external additive in the cleaning blade nip can be formed, thereby achieving high cleaning properties.

[0269] (Recycling Department) The recycling section is not particularly limited, and examples thereof include known conveying means.

[0270] ((Control Unit)) The control unit can control the movement of each of the above-mentioned parts. The control unit is not particularly limited as long as it can control the movement of each of the above-mentioned parts, and can be appropriately selected depending on the purpose. For example, the control unit can be a control device such as a sequencer or a computer.

[0271] The image forming apparatus according to an embodiment can form images using the toner according to an embodiment, and therefore can reduce power consumption and stably provide high-quality images.

[0272] <Image forming method> An image forming method according to an embodiment includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, and a developing step of developing the electrostatic latent image with toner to form a toner image, and may further include other steps as necessary. The image forming method can be suitably performed by the image forming apparatus, the electrostatic latent image forming step can be suitably performed by the electrostatic latent image forming unit, the developing step can be suitably performed by the developing unit, and the other steps can be suitably performed by the other units.

[0273] Furthermore, the image forming method according to one embodiment more preferably includes, in addition to the electrostatic latent image forming process and the developing process described above, a transfer process of transferring the toner image onto a recording medium, and a fixing process of fixing the transferred image onto the surface of the recording medium.

[0274] In the developing step, the toner according to an embodiment is used. Preferably, a developer containing the toner according to an embodiment and, if necessary, other components such as a carrier may be used to form a toner image.

[0275] The electrostatic latent image forming process is a process of forming an electrostatic latent image on an electrostatic latent image carrier, and includes a charging process of charging the surface of the electrostatic latent image carrier and an exposure process of exposing the charged surface of the electrostatic latent image carrier to light to form an electrostatic latent image. Charging can be performed, for example, by applying a voltage to the surface of the electrostatic latent image carrier using a charger. Exposure can be performed, for example, by exposing the surface of the electrostatic latent image carrier to light in an imagewise manner using the exposure device. The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image carrier and then exposing it to light in an imagewise manner, and can be performed by an electrostatic latent image forming unit.

[0276] The developing step is a step of sequentially developing the electrostatic latent image with toners of multiple colors to form a visible image. The visible image can be formed, for example, by developing the electrostatic latent image with the toners, using a developing device.

[0277] In the developing device, for example, toner and carrier are mixed and stirred, and the toner becomes charged by friction during this process and is held in a standing state on the surface of the rotating magnet roller, forming a magnetic brush. Since the magnet roller is disposed near an electrostatic latent image carrier (photoconductor), a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier (photoconductor) by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image made of the toner is formed on the surface of the electrostatic latent image carrier (photoconductor).

[0278] The transfer step is a step of transferring a visible image to a recording medium. The transfer step is preferably performed using an intermediate transfer body, and after the visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. The transfer step is more preferably performed using toner of two or more colors, preferably full-color toner, and includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto the recording medium. The transfer can be performed, for example, by charging an electrostatic latent image carrier (photoconductor) with a transfer charger, and can be performed by a transfer section.

[0279] The fixing process is a process in which the visible image transferred to the recording medium is fixed using a fixing device, and may be performed for each color developer each time it is transferred to the recording medium, or may be performed simultaneously for each color developer in a stacked state.

[0280] The image forming method according to the first embodiment may further include other steps appropriately selected as necessary, such as a static elimination step, a cleaning step, a recycling step, and the like.

[0281] The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by the charge removing unit.

[0282] The cleaning step is a step of removing the toner remaining on the electrostatic latent image bearing member, and can be suitably performed by a cleaning unit.

[0283] The recycling step is a step in which the toner removed in the cleaning step is recycled to the developing unit, and can be suitably carried out by the recycling unit.

[0284] The image forming method according to an embodiment can form an image using the toner according to an embodiment, and therefore can reduce power consumption and stably provide high-quality images.

[0285] [One embodiment of the image forming apparatus] Next, one aspect of an image forming apparatus according to an embodiment will be described with reference to Fig. 3. Fig. 3 is a schematic diagram showing an example of an image forming apparatus according to an embodiment. As shown in Fig. 3, the color image forming apparatus 1 includes a photoconductor drum 10 which is an electrostatic latent image carrier, a charging roller 20 which is a charging section, an exposure device 30 which is an exposure section, a developing device 40 which is a developing section, an intermediate transfer body (intermediate transfer belt) 50, a cleaning device 60 which is a cleaning section, a transfer roller 70 which is a transfer section, a static elimination lamp 80 which is a static elimination section, and an intermediate transfer body cleaning device 90.

[0286] The intermediate transfer body 50 is an endless belt stretched by three rollers 51 arranged inside, and is designed to be movable in the direction of the arrow by the three rollers 51. Some of the three rollers 51 also function as transfer bias rollers that can apply a predetermined transfer bias (primary transfer bias) to the intermediate transfer body 50. An intermediate transfer body cleaning device 90 is arranged near the intermediate transfer body 50. Furthermore, a transfer roller 70 is arranged facing the intermediate transfer body 50 near the intermediate transfer body 50, and can apply a transfer bias (secondary transfer bias) for transferring (secondary transfer) a developed image (toner image) to a transfer paper P as a recording medium. Around the intermediate transfer body 50, a corona charger 52 for applying a charge to the toner image on the intermediate transfer body 50 is arranged between the contact portion between the photosensitive drum 10 and the intermediate transfer body 50 and the contact portion between the intermediate transfer body 50 and the transfer paper P with respect to the rotation direction of the intermediate transfer body 50.

[0287] The developing device 40 is composed of a developing belt 41 which is a developer carrier, and a black (Bk) developing unit 42K, a yellow (Y) developing unit 42Y, a magenta (M) developing unit 42M, and a cyan (C) developing unit 42C which are arranged around the developing belt 41.

[0288] The developing belt 41 is an endless belt that is stretched around a plurality of belt rollers and can move in the direction of the arrow in the figure. Furthermore, a part of the developing belt 41 is in contact with the photoconductor drum 10.

[0289] The black developing unit 42K includes a developer container 421K, a developer supply roller 422K, and a developing roller (developer carrier) 423K. The yellow developing unit 42Y includes a developer container 421Y, a developer supply roller 422Y, and a developing roller 423Y. The magenta developing unit 42M includes a developer container 421M, a developer supply roller 422M, and a developing roller 423M. The cyan developing unit 42C includes a developer container 421C, a developer supply roller 422C, and a developing roller 423C.

[0290] Next, a method of forming an image using the image forming apparatus 1 will be described. First, the surface of the photosensitive drum 10 is uniformly charged using the charging roller 20, and then the photosensitive drum 10 is exposed to exposure light L using the exposure device 30 to form an electrostatic latent image. Next, the electrostatic latent image formed on the photosensitive drum 10 is developed with toner supplied from the developing device 40 to form a toner image. Furthermore, the toner image formed on the photosensitive drum 10 is transferred (primary transfer) onto the intermediate transfer body 50 by the transfer bias applied from the roller 51, and then transferred (secondary transfer) onto the transfer paper P fed by a paper feed unit (not shown) by the transfer bias applied from the transfer roller 70. Meanwhile, the photosensitive drum 10 on which the toner image has been transferred to the intermediate transfer body 50 has the toner remaining on its surface removed by the cleaning device 60, and is then discharged by the discharge lamp 80. The residual toner on the intermediate transfer body 50 after the image transfer is removed by the intermediate transfer body cleaning device 90.

[0291] After the transfer process is completed, the transfer paper P is transported to a fixing unit, where the transferred toner image is fixed onto the transfer paper P. EXAMPLES

[0292] The embodiments will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to these examples and comparative examples.

[0293] <Synthesis of crystalline polyester resin A-1> In a 5L four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, 1,10-decanediol and dodecanedioic acid were charged so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. The reaction was carried out while discharging water together with 500 ppm of titanium tetraisopropoxide relative to the mass of the charged raw materials, and the temperature was finally raised to 235°C and the reaction was carried out for 1 hour. Then, the reaction was carried out for 6 hours under a reduced pressure of 10 mmHg or less. Then, the temperature was set to 185°C, trimellitic anhydride was added so that the molar ratio with the COOH groups was 0.053, and the reaction was carried out for 2 hours while stirring. As a result, crystalline polyester resin A-1 was obtained. The acid value (AV) of the obtained crystalline polyester resin A-1 was 18 mgKOH / g, the melting point (Tm) was 78°C, and the weight average molecular weight (Mw) was 10,500. 。

[0294] <Preparation of Crystalline Polyester Resin Dispersion> [Preparation of crystalline polyester resin dispersion A-1a] A four-neck flask was charged with crystalline polyester resin A-1 (40 parts by mass), methyl ethyl ketone (24 parts by mass), and 2-propyl alcohol (4 parts by mass). The mixture was then heated and stirred at the melting point temperature of the crystalline polyester resin A-1 to dissolve the crystalline polyester resin. A 10% by mass aqueous ammonia solution was then added so that the neutralization rate was 150%. The neutralization rate was calculated from the acid value of the crystalline polyester resin. Ion-exchanged water (160 parts by mass) was then gradually added to carry out phase inversion emulsification, followed by desolvation. Ion-exchanged water was then added to adjust the solid content concentration (concentration of the crystalline polyester resin) to 25% by mass, thereby obtaining crystalline polyester resin dispersion A-1a, which is a binder resin dispersion for toner. The particle size of the particulate crystalline polyester resin in the crystalline polyester resin dispersion A-1a was 250 nm. 。

[0295] [Preparation of crystalline polyester resin dispersion A-1b] A four-neck flask was charged with crystalline polyester resin A-1 (40 parts by mass) and tetrahydrofuran (40 parts by mass). Then, the mixture was heated and stirred at the melting point temperature of the crystalline polyester resin A-1 to dissolve the crystalline polyester resin. Then, a 10% by mass aqueous triethylamine solution was added so that the neutralization rate was 200%. The neutralization rate was calculated from the acid value of the crystalline polyester resin. Further, ion-exchanged water (120 parts by mass) was gradually added to carry out phase inversion emulsification, and then the solvent was removed. Then, ion-exchanged water was added to adjust the solid content concentration (concentration of the crystalline polyester resin) to 25% by mass, and a crystalline polyester resin dispersion A-1b, which is a binder resin dispersion for toner, was obtained. The particle size of the particulate crystalline polyester resin in the crystalline polyester resin dispersion A-1b was 150 nm.

[0296] [Preparation of crystalline polyester resin dispersion A-1c] Crystalline polyester resin A-1 (100 g), non-crystalline polyester resin B (100 g), and ethyl acetate (400 g) were added to a 2 L metal container. The mixture was then heated at 77°C to dissolve the crystalline polyester resin A-1, and then rapidly cooled in an ice water bath at a rate of 27°C / min. 500 mL of glass beads (3 mmφ) were added thereto, and the mixture was ground for 12 hours using a batch-type sand mill (manufactured by Kampe Hapio Co., Ltd.) to obtain a crystalline polyester dispersion A-1c having a volume average particle size of 0.3 μm. The obtained crystalline polyester dispersion A-1c was diluted with ethyl acetate to adjust the solid content concentration (concentration of the crystalline polyester resin) to 25 mass%, thereby obtaining a crystalline polyester resin dispersion A-1c, which is a binder resin dispersion for toner. The particle size of the particulate crystalline polyester resin in the crystalline polyester resin dispersion A-1c was 330 nm.

[0297] <Synthesis of non-crystalline polyester resin B> A four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple was charged with 2-mol ethylene oxide adduct of bisphenol A (BisA-EO), 3-mol propylene oxide adduct of bisphenol A (BisA-PO), trimethylolpropane (TMP), terephthalic acid, and adipic acid. The molar ratio of 2-mol ethylene oxide adduct of bisphenol A, 3-mol propylene oxide adduct of bisphenol A, and trimethylolpropane (2-mol ethylene oxide adduct of bisphenol A / 3-mol propylene oxide adduct of bisphenol A / trimethylolpropane) was 38.6 / 57.9 / 3.5. The molar ratio of terephthalic acid and adipic acid (terephthalic acid / adipic acid) was 80 / 20. The molar ratio of OH / COOH, which is the molar ratio of hydroxyl groups to carboxyl groups, was 1.2. The mixture was reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at normal pressure for 8 hours at 230°C. After further reacting for 4 hours at a reduced pressure of 10 mmHg to 15 mmHg, trimellitic anhydride was added to the reaction vessel so that the amount was 1 mol% relative to the total resin components, and the mixture was reacted at 180°C and normal pressure for 3 hours. As a result, amorphous polyester resin B was obtained. The solubility parameter value (SP value) of amorphous polyester resin B was 11.2 cal1 / 2 / cm 3 / 2 The glass transition temperature Tg was 57.6° C., the weight average molecular weight Mw was 10,000, and the acid value Av was 20.

[0298] <Synthesis of prepolymer C> In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 97 mol% of 3-methyl-1,5-pentanediol and 3 mol% of trimethylolpropane (TMP) were charged as alcohol components, and 50 mol% of adipic acid and 50 mol% of terephthalic acid were charged as acid components. At that time, OH / COOH was set to 1.1. Furthermore, titanium tetraisopropoxide (300 ppm to resin component) was also charged. After that, the temperature was raised to 200°C in about 4 hours, and then to 230°C in 2 hours, and the reaction was continued until no water was discharged. After that, the reaction was continued for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg. As a result, intermediate polyester C-1 was obtained.

[0299] Next, intermediate polyester B-1 and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate group of IPDI / hydroxyl group of intermediate polyester) of 1.8. After diluting with ethyl acetate to a 48% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain a nonlinear polyester resin C (prepolymer C) having reactive groups. The glass transition temperature Tg of prepolymer C was -38.5°C, the weight average molecular weight Mw was 12,000, and the acid value Av was 0.14.

[0300] <Synthesis of vinyl polymer modified polyester resin D> As raw material monomers of the condensation polymerization resin, 1,225g of polyoxypropylene (2.2)-2,2-(4-hydroxyphenyl)propane, 485g of polyoxyethylene (2.0)-2,2-(4-hydroxyphenyl)propane, 345g of terephthalic acid, 250g of isododecenyl succinic acid, and 5g of dibutyltin oxide as an esterification catalyst were condensed and polymerized at 230°C for 6 hours under a nitrogen atmosphere. Then, it was cooled to 150°C. 175g of trimellitic acid was added to the reaction vessel. Then, a mixture of 400g of styrene as raw material monomers of the addition polymerization resin, 55g of 2-ethylhexyl acrylate, 35g of acrylic acid as a bireactive compound, and 25g of dicumyl peroxide as a polymerization initiator was added dropwise over 1 hour while stirring at 160°C. The same temperature was maintained for another hour to carry out an addition polymerization reaction, and then the temperature was raised to 200°C to carry out a condensation polymerization reaction, yielding a vinyl polymer modified polyester resin D, which is a hybrid resin of styrene acrylic and polyester resin. The glass transition temperature of vinyl polymer modified polyester resin D was 60°C, and the acid value was 21 mgKOH / g.

[0301] <Synthesis of Sulfonic Group-Containing Vinyl Polymer Modified Polyester Resin E> As raw material monomers of the condensation polymerization resin, 1,225g of polyoxypropylene (2.2)-2,2-(4-hydroxyphenyl)propane, 485g of polyoxyethylene (2.0)-2,2-(4-hydroxyphenyl)propane, 345g of terephthalic acid, 250g of isododecenyl succinic acid, and 5g of dibutyltin oxide as an esterification catalyst were condensed and polymerized at 230°C for 6 hours under a nitrogen atmosphere. Then, it was cooled to 150°C. 175g of trimellitic acid was added to the reaction vessel. Then, a mixture of 200g of methyl methacrylate, 50g of t-butylacrylamidosulfonic acid, 55g of 2-ethylhexyl acrylate as raw material monomers of the addition polymerization resin, 100g of 2-hydroxyethyl methacrylate as a bireactive compound, and 25g of dicumyl peroxide as a polymerization initiator was added dropwise over 1 hour while stirring at 160°C. The same temperature was maintained for another hour to carry out an addition polymerization reaction, and then the temperature was raised to 200°C to carry out a condensation polymerization reaction, yielding a sulfone group-containing vinyl polymer-modified polyester resin E, which is a hybrid resin of styrene acrylic containing sulfone groups and polyester resin. The glass transition temperature Tg of the sulfone group-containing vinyl polymer-modified polyester resin E was 65°C, and the acid value Av was 35 mgKOH / g.

[0302] <Example 1> [Toner manufacturing] (Masterbatch (MB) adjustment) 600 parts by mass of water, 500 parts by mass of carbon black (Nipex 60, manufactured by Dexa), and 500 parts by mass of non-crystalline polyester resin B were added and mixed in a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). The mixture was kneaded using two rolls at 150°C for 30 minutes, then rolled and cooled, and pulverized in a pulverizer to obtain a master batch.

[0303] (Synthesis of organic fine particle emulsion (fine particle dispersion)) In a reaction vessel equipped with a stirring rod and a thermometer, 683 parts by mass of water, 11 parts by mass of sodium salt of methacrylic acid ethylene oxide adduct sulfate (Eleminol RS-30: manufactured by Sanyo Chemical Industries, Ltd.), 138 parts by mass of styrene, 138 parts by mass of methacrylic acid, and 1 part by mass of ammonium persulfate were charged. After stirring for 15 minutes at 400 rpm, a white emulsion was obtained. The emulsion was heated to an internal temperature of 75°C and reacted for 5 hours. Further, 30 parts by mass of a 1% aqueous ammonium persulfate solution was added, and the mixture was aged at 75°C for 5 hours to obtain an aqueous dispersion (fine particle dispersion) of a vinyl resin (a copolymer of styrene-methacrylic acid-sodium salt of methacrylic acid ethylene oxide adduct sulfate). The fine particle dispersion was adjusted to a solid content of 30%. The volume average particle diameter of the fine particle dispersion measured with an LA-920 (manufactured by HORIBA) was 0.14 μm.

[0304] (Preparation of aqueous phase) 930 parts by mass of water, 67 parts by mass of the microparticle dispersion, 103 parts by mass of a 48.5% aqueous solution of sodium dodecyldiphenyletherdisulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.), and 80 parts by mass of ethyl acetate were mixed and stirred to obtain a milky white liquid, which was used as the aqueous phase.

[0305] (Preparation of wax dispersion) A container equipped with a stirring rod and a thermometer was charged with 100 parts by mass of ester wax (NOF Corp., WEP-3, melting point 70°C, acid value 0.1mgKOH / g) as a release agent and 400 parts by mass of ethyl acetate. The mixture was heated to 80°C while stirring, and held at 80°C for 5 hours, then cooled to 20°C in 1 hour. Dispersion was performed using a bead mill (Ultraviscomill, Imex Corp.) under conditions of a liquid delivery rate of 1kg / hr, a disk peripheral speed of 6m / sec, 80% by volume of 0.5mm zirconia beads, and 3 passes to obtain a wax dispersion. The wax dispersion was adjusted to a solid content of 20%.

[0306] (Preparation of oil phase) Ethyl acetate, wax dispersion, non-crystalline polyester resin B and master batch were placed in a container in the amounts shown below, and mixed and dispersed for 1 hour at 5,000 rpm with a TK homomixer (manufactured by Tokushu Kika) while maintaining the internal temperature at 25°C. Furthermore, crystalline polyester resin dispersion A-1a was gradually added over 1 hour while mixing at 5,000 rpm in the amounts shown below. After the entire amount was added, the oil phase was observed to have formed a W / O emulsion in which fine water droplets existed in the colored oil phase. It was presumed that the crystalline polyester resin particles existed in the water droplets. Then, the ethyl acetate solution of prepolymer C and isophorone diamine (IPDA) as an active hydrogen group-containing compound were added in the amounts shown below, and mixed for 1 minute at 5,000 rpm with a TK homomixer (manufactured by Tokushu Kika) to obtain an oil phase. ((Amount)) Ethyl acetate: 110 parts by weight Wax dispersion: 90 parts by weight Amorphous polyester resin B: 192 parts by weight Masterbatch: 30 parts by weight Crystalline polyester resin dispersion A-1a: 90 parts by weight Ethyl acetate solution of prepolymer C: 58 parts by weight Active hydrogen group-containing compound (isophoronediamine (IPDA)): 0.3 parts by weight

[0307] (Emulsification and aspect ratio adjustment) The oil phase was added to a vessel containing 1,000 parts by weight of the aqueous phase, and mixed for 3 minutes at 13,000 rpm using a TK homomixer to obtain an emulsified slurry. The resulting emulsified slurry was transferred to a flask, and the bath temperature was kept at 25°C using an evaporator, and the solvent was removed under reduced pressure while measuring the weight of the flask. The solvent removal was stopped when 30% of the weight of the ethyl acetate had evaporated. The slurry was then transferred to a flask equipped with a sealed paddle-type stirring blade, and 10 parts by weight of carboxymethylcellulose (a grade with a viscosity of 10,000 mPa·s at 25°C for a 1% aqueous solution) was added and dissolved by stirring. Stirring was continued for 30 minutes at 300 rpm and at 25°C, and deformation of the spherical particles was observed.

[0308] (Desolvation and surface adjustment) The slurry containing the deformed particles was again desolvated in an evaporator until the ethyl acetate was 10 ppm or less. The obtained slurry was then centrifuged, solid-liquid separated, the supernatant was discarded, and the slurry was reslurried with ion-exchanged water three times to obtain a slurry with a solid content of 20%. This slurry was returned to a flask equipped with a paddle-type stirring blade, immersed in a bath with an internal temperature of 60°C, and heat-treated for 2 hours while stirring at a rotation speed of 200 rpm. The volume average particle size after treatment was 5.5 μm. The slurry was left to stand at 45°C for 12 hours for aging, and a dispersion slurry was obtained.

[0309] (Washing and drying) 100 parts by mass of the dispersed slurry was filtered under reduced pressure, and the following operations (1) to (4) were carried out twice to obtain a filter cake. (1): 100 parts by mass of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 100 parts by mass of a 10% aqueous sodium hydroxide solution was added to the filter cake of (1), mixed with a TK homomixer (at 12,000 rpm for 30 minutes), and then filtered under reduced pressure. (3): 100 parts by mass of 10% hydrochloric acid was added to the filter cake of (2), and the mixture was mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered. (4): 300 parts by mass of ion-exchanged water was added to the filter cake of (3) and mixed with a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes).

[0310] The resulting filter cake was then dried at 45° C. for 48 hours using a circulating air dryer, and sieved through a mesh with 75 μm openings to obtain toner base particles.

[0311] (External Addition Treatment) The toner base particles, hydrophobic silica (X24, manufactured by Shin-Etsu Chemical Co., Ltd.) having an average particle size of 100 nm, titanium oxide (MT-150AI, manufactured by Titan Kogyo Co., Ltd.) having an average particle size of 20 nm, and hydrophobic silica fine powder (AEROSIL R812, manufactured by Nippon Aerosil Co., Ltd.) having an average particle size of 30 nm were mixed in the amounts shown below using a Henschel mixer to obtain a toner. ((Amount)) Toner base particles: 100 parts by weight Hydrophobic silica with an average particle size of 100 nm: 0.6 parts by weight Titanium oxide with an average particle size of 20 nm: 1.0 part by weight Hydrophobic silica fine powder with an average particle size of 15 nm: 0.8 parts by weight

[0312] The aspect ratio and CV value of the obtained toner, and the shape index, center-to-center distance L, maximum length D, and center-to-center distance L / maximum length D of the crystalline polyester resin were measured as shown below.

[0313] [Toner aspect ratio] The toner was dispersed on carbon tape, a vapor deposition film was formed on the toner surface, the toner was observed using a SEM, and the image of the toner surface was taken using a Phenom ProX PREMIUM 2. The 100 toner images obtained were analyzed using the particle analysis software "Particle Metric," and the aspect ratio of the toner was calculated from the ratio of the maximum length to the minimum length of the toner.

[0314] [Toner shape index] The shape index of the toner was measured using a desktop SEM: Phenom ProX PREMIUM2 and particle analysis software: Particle Metric (Phenom World). The shape index was calculated in the same manner as in the calculation of the toner aspect ratio described above. First, an image of the toner surface was captured using a desktop SEM "Phenom ProX PREMIUM2". Then, 100 toner images from the obtained images were analyzed using particle analysis software "Particle Metric", and the shape index was calculated from the ratio of the diameter of a circle with an area equal to the toner area to the diameter of a circle with a perimeter equal to the perimeter of the toner.

[0315] [CV value of center distance L of crystalline polyester resin A-1] The coefficient of variation (CV value) of the center-to-center distance L of the crystalline polyester resin A-1 was calculated by dividing the standard deviation of the center-to-center distance L of the crystalline polyester resin particles A-1 present in the toner by the average value and multiplying the result by 100 (coefficient of variation = standard deviation / average value x 100 (%)). The CV value was taken as the average value of the CV values ​​of the 20 toner particles. The CV value of the center-to-center distance L of the crystalline polyester resin particles A-1 represents the proportion of the standard deviation of the center-to-center distance L of the crystalline polyester resin particles present in the toner to the average value, and indicates the distribution of the distance between the crystalline polyester resin particles A-1.

[0316] [Maximum length D of crystalline polyester resin A-1] The toner thus prepared was embedded in an epoxy resin and cured, and then an ultrathin section (approximately 100 nm thick) of the toner was prepared using an ultramicrotome (ULTRACUT UCT, manufactured by Leica, using a diamond knife). The sample was then exposed to gas using a dye (ruthenium tetroxide, manufactured by Filgen Co., Ltd.) to differentiate the crystalline polyester resin phase from the other parts. The cross section of the ultrathin section of the toner was then observed using a TEM (JEM-2100, manufactured by JEOL Co., Ltd.). The observed cross-sectional image was binarized using a commercially available image processing software (e.g., Image-Pro Plus, etc.) to calculate the maximum length D of the crystalline polyester resin A-1. The cross sections of 20 toner particles were observed, and the maximum length D of each crystalline polyester resin A-1 was determined, and the average value was taken as the maximum length D of the cross section of the crystalline polyester resin particle.

[0317] [Center distance L of crystalline polyester resin A-1] The center-to-center distance L of the crystalline polyester resin A-1 was determined by identifying the minimum length part in the same image as when determining the above [maximum length D of the cross section of the crystalline polyester resin particle], and determining the intersection with the maximum length. The one with the shortest distance to the intersection of the other crystalline polyester resin particles A-1 was selected, and the distance was determined. The average value of all center-to-center distances L was taken as the center-to-center distance L of the crystalline polyester resin particles A-1 of the selected toner particles. This was performed for the 20 toners for which the maximum length D was determined, and the average value was taken as the maximum length D of the crystalline polyester resin A-1. The crystalline polyester resin A-1 for which the center-to-center distance L was measured did not include crystalline polyester resin A-1 whose maximum length D was 10 nm or less.

[0318] [Center distance L / Maximum length D] Using the center-to-center distance L and maximum length D obtained above, the center-to-center distance L / maximum length D was calculated.

[0319] The results of these measurements are shown in Table 1.

[0320] [Table 1]

[0321] <Example 2> In Example 1, the paddle-type stirring blade used in Example 1 (adjustment of emulsification and aspect ratio) was changed to a helical ribbon-type stirring blade, 10 parts by mass of carboxymethyl cellulose (grade with a viscosity of 10,000 mPa s for a 1% aqueous solution at 25°C) was changed to 20 parts by mass of carboxymethyl cellulose (grade with a viscosity of 10,000 mPa s for a 1% aqueous solution at 25°C), and the rotation speed was changed from 300 rpm to 200 rpm. A toner was produced in the same manner as in Example 1 except for the above.

[0322] <Example 3> A toner was produced in the same manner as in Example 2, except that the rotation speed when stirring the slurry during (emulsification and adjustment of the aspect ratio) was changed to 300 rpm.

[0323] <Example 4> A toner was produced in the same manner as in Example 2, except that the content of carboxymethyl cellulose used when carrying out (emulsification and aspect ratio adjustment) in Example 2 was changed to 30 parts by mass, and the rotation speed when stirring the slurry was changed to 500 rpm.

[0324] <Example 5> A toner was produced in the same manner as in Example 1, except that, when performing (removal of the solvent and adjustment of the surface properties) in Example 1, the internal temperature of the bath in which the flask containing the slurry with a solid content of 20% was immersed was changed to 70°C.

[0325] <Example 6> In Example 1, when performing (preparation of oil phase), the amorphous polyester resin B was replaced with the amorphous polyester resin A (192 parts by mass). The rotation speed when the crystalline polyester resin dispersion A-1a was mixed with the mixed liquid containing ethyl acetate, wax dispersion, amorphous polyester resin B and master batch was changed to 10,000 rpm. When the oil phase was observed after the entire amount of the crystalline polyester resin was added, it was confirmed that the presence of fine water droplets in the colored oil phase was too large to be confirmed by optical microscope. The rest was the same as in Example 1 to prepare a toner. The blending amounts of each component used in the preparation of the oil phase are as follows. ((Amount)) Ethyl acetate: 110 parts by weight Wax dispersion: 90 parts by weight Amorphous polyester resin A: 192 parts by weight Masterbatch: 30 parts by weight Crystalline polyester resin dispersion A-1a: 90 parts by weight Ethyl acetate solution of prepolymer C: 58 parts by weight Active hydrogen group-containing compound (isophoronediamine (IPDA)): 0.3 parts by weight

[0326] <Example 7> In Example 2, when performing (removal of solvent and adjustment of surface properties), the internal temperature of the bath in which the flask containing the slurry with a solid content of 20% was immersed was changed to 70° C., and the heat treatment was performed. A toner was produced in the same manner as in Example 2 except for the above.

[0327] <Example 8> A toner was produced in the same manner as in Example 6, except that in the step of removing the solvent and adjusting the surface properties in Example 6, the internal temperature of the bath in which the flask containing the slurry with a solid content of 20% was immersed was changed to 70°C and the heat treatment was performed.

[0328] <Example 9> A toner was produced in the same manner as in Example 8, except that the crystalline polyester resin dispersion A-1a used in (preparation of the oil phase) in Example 8 was changed to crystalline polyester resin dispersion A-1b.

[0329] <Example 10> In Example 9, when performing (preparation of oil phase), in addition to ethyl acetate, wax dispersion, non-crystalline polyester resin B and master batch, vinyl polymer modified polyester resin was added, and the content of non-crystalline polyester resin B was changed from 192 parts by mass to 162 parts by mass. Crystalline polyester resin dispersion A-1b was used instead of crystalline polyester resin dispersion A-1a, and the rotation speed when mixing crystalline polyester resin dispersion A-1b was changed to 10000 rpm. After the entire amount was added, when the oil phase was observed, it was confirmed that the presence of fine water droplets in the colored oil phase had become too large to be confirmed by optical microscope. Other than that, the same procedure as in Example 9 was carried out to prepare a toner. ((Amount)) Ethyl acetate: 110 parts by weight Wax dispersion: 90 parts by weight Vinyl polymer modified polyester resin D: 30 parts by weight Amorphous polyester resin B: 162 parts by weight Masterbatch: 30 parts by weight Crystalline polyester resin dispersion A-1a: 90 parts by weight Ethyl acetate solution of prepolymer C: 58 parts by weight Active hydrogen group-containing compound (isophoronediamine (IPDA)): 0.3 parts by weight

[0330] <Example 11> A toner was prepared in the same manner as in Example 10, except that in the preparation of the oil phase, vinyl polymer modified polyester resin D was changed to sulfonic group-containing vinyl polymer modified polyester resin E.

[0331] <Comparative Example 1> In Example 1, when performing (removal of the solvent and adjustment of the surface properties), a dispersion slurry was obtained without performing a heat treatment on a slurry having a solid content concentration of 20%. A toner was produced in the same manner as in Example 1 except for the above.

[0332] <Comparative Example 2> A toner was produced in the same manner as in Example 2, except that the content of carboxymethyl cellulose used when performing (emulsification and aspect ratio adjustment) in Example 2 was changed to 30 parts by mass, and the rotation speed when stirring the slurry was changed to 750 rpm.

[0333] <Comparative Example 3> In Example 1, when performing (desolvation and adjustment of surface properties), the slurry containing the deformed particles was again desolvated in an evaporator until the ethyl acetate was 10 ppm or less, and then the slurry was left to stand for 12 hours at 45°C for aging without being reslurried or heated, and a toner was produced in the same manner as in Example 1.

[0334] <Comparative Example 4> A toner was produced in the same manner as in Example 1, except that the crystalline polyester resin dispersion A-1c was used instead of the crystalline polyester resin dispersion A-1a in Example 1.

[0335] [Creating the carrier] 100 parts by mass of silicone resin (organo straight silicone), 5 parts by mass of γ-(2-aminoethyl)aminopropyltrimethoxysilane, and 10 parts by mass of carbon black were added to 100 parts by mass of toluene, and dispersed for 20 minutes with a homomixer to prepare a resin layer coating liquid. Using a fluidized bed type coating device, the resin layer coating liquid was applied to the surface of 1,000 parts by mass of spherical magnetite with an average particle size of 50 μm to prepare a carrier.

[0336] [Preparation of developer] 5 parts by weight of each toner and 95 parts by weight of the carrier were mixed in a ball mill to prepare a developer.

[0337] <Toner characteristic evaluation> Using each toner or developer, various characteristics were evaluated as follows.

[0338] [Low temperature fixability] After putting each developer into the unit of the imagio MP C4300 (manufactured by Ricoh Co., Ltd.), a rectangular solid image of 2 cm x 15 cm was printed on PPC paper type 6000<70W>A4 T (manufactured by Ricoh Co., Ltd.) with a toner adhesion of 0.40 mg / cm 2 At this time, the surface temperature of the fixing roller was changed to determine the cold offset temperature (lowest limit fixing temperature) at which an offset occurred in which a residual image of a solid image was fixed in a place other than the desired place, and the low-temperature fixing property was evaluated based on the following evaluation criteria. (Evaluation Criteria) ◎◎: The minimum fixing temperature is less than 100℃ ◎: The minimum fixing temperature is 100℃ or higher and less than 110℃ ○: The minimum fixing temperature is 110℃ or higher and less than 120℃ △: The minimum fixing temperature is 120℃ or higher and less than 130℃ ×: The minimum fixing temperature is 130°C or higher

[0339] [Heat-resistant storage stability] A 50 mL glass container was filled with 10 g of toner, tapped thoroughly until there was no change in the apparent density of the resulting toner powder, and the container was then capped. The toner was left in a thermostatic chamber at 50° C. for 24 hours, and then cooled to 24° C. Thereafter, the penetration (unit: mm) was measured using a penetration test (JIS K2235-1991), and the heat-resistant storage stability was evaluated based on the following evaluation criteria. Note that a larger penetration indicates better heat-resistant storage stability. A penetration of less than 10 mm is likely to cause problems in use. (Evaluation Criteria) ◎◎: Penetration ◎: Penetration is 20mm or more ○: Penetration is 15mm or more and less than 20mm △: Penetration is 10mm or more and less than 15mm ×: Penetration is less than 10 mm

[0340] [Image quality (transferability)] Using a RICOH Pro C7210S (manufactured by Ricoh Co., Ltd.), a 400 dpi standard line chart image (output image) for evaluation was formed on coated paper (POD gloss coated paper, manufactured by Oji Paper Co., Ltd.). The output image was formed so that a line image of a solid black image was created. The formed thin line portion was compared with the original file image, and reproducibility was evaluated according to the following evaluation criteria. An evaluation result of "○" or higher is at a level that can be used practically. [Evaluation Criteria] .circle.: Even when the image of the continuous lines in the original image is observed with a magnifying glass, there are no missing parts of the high luminance lines and they are reproduced. ○: When observed with a loupe at 100x magnification, partial loss of the line image is observed. △: Partial loss of the line image is visually observed. ×: Continuous missing portions of the line image are clearly visible to the naked eye.

[0341] [Cleaning ability] Under the same image forming conditions as those for image quality (transferability), 10 solid images were output using a cleaning blade that had been used to output approximately 100,000 images. However, no transfer bias was applied for the secondary transfer, and almost all of the untransferred toner was deposited on the cleaning blade. After that, a normal solid image was output, and then a blank image was created. The stains on the resulting blank image were evaluated according to the following evaluation criteria. Evaluation results of "good" or higher are at a level that can be used practically. (Evaluation Criteria) ⊚: No toner was observed on the white paper. ○: When observed on a blank sheet of paper, slight vertical lines can be seen with a magnifying glass. △: When observed on a white sheet of paper, one or two slight vertical lines are visible to the naked eye. ×: When observed on a white sheet of paper, three or more clear vertical streaks are visible in succession.

[0342] [comprehensive evaluation] The overall evaluation was performed according to the following evaluation criteria: A product with all evaluation items being ○, ◎, or ◎◎ was rated as ◎, a product with one or more △ but no problem in use was rated as ○, a product with two or more △ but no problem in use was rated as △, and a product with one or more × was rated as ×. (Evaluation Criteria) ◎:Excellent ○:Excellent △: Practical ×: Not practical

[0343] The evaluation results are shown in Table 2.

[0344] [Table 2]

[0345] From Table 2, it was confirmed that the toners of Examples 1 to 11 satisfied the conditions for use in terms of low fixing property, heat-resistant storage stability, image quality, and cleaning property. In contrast, it was confirmed that the toners obtained in Comparative Examples 1 to 4 did not satisfy the conditions for use in terms of at least one of low fixing property, heat-resistant storage stability, image quality, and cleaning property, and thus had practical problems.

[0346] Therefore, the toners of Examples 1 to 11 differ from the toners of Comparative Examples 1 to 4 in that at least the toner particles have an aspect ratio of 1.55 to 4.8 and a shape index of 0.76 or more, and the center-to-center distance L of the cross-sections of the crystalline polyester resin particles contained in the toner particles is 2.3 times or more the maximum length D of the cross-sections of the crystalline polyester resin particles, and therefore can be said to be high-quality toners with excellent low-temperature fixing properties, heat-resistant storage properties, image quality and cleanability.

[0347] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]

[0348] 1. Color image forming device [Prior art documents] [Patent documents]

[0349] [Patent Document 1] JP 2005-196056 A

Claims

1. A toner comprising a crystalline polyester resin and a non-crystalline polyester resin, The toner particles have an aspect ratio of 1.5 to 5 and a shape index of 0.75 or more; The toner, wherein the center-to-center distance L between the particles of the crystalline polyester resin contained in the toner particles is at least twice the maximum length D of a cross section of the particle of the crystalline polyester resin.

2. 2. The toner according to claim 1, wherein the coefficient of variation CV of the center-to-center distance L is 50% or less.

3. A toner as described in claim 1 or 2, wherein the crystalline polyester resin is synthesized from a linear saturated aliphatic diol and a linear saturated aliphatic dicarboxylic acid.

4. 4. The toner according to claim 1, comprising a vinyl polymer modified polyester resin obtained by modifying a polyester resin with either or both of styrene and a (meth)acrylic compound.

5. the step of mixing a dispersion liquid containing a crystalline polyester resin with an oil phase containing a non-crystalline polyester resin to prepare a water-in-oil (W / O) emulsion in which the crystalline polyester resin is dispersed in the oil phase, and then mixing the water-in-oil (W / O) emulsion with an aqueous medium to prepare an oil-in-water (O / W) emulsion in which the crystalline polyester resin is dispersed in the aqueous medium; The method for producing the toner according to any one of claims 1 to 4, further comprising adjusting an aspect ratio and a shape index of the toner produced in the oil-in-water (O / W) emulsion.

6. A toner storage unit containing the toner according to any one of claims 1 to 4.

7. An electrostatic latent image carrier; an electrostatic latent image forming unit for forming an electrostatic latent image on the electrostatic latent image carrier; a developing section for developing the electrostatic latent image with toner to form a visible image; a transfer section for transferring the visible image onto a recording medium; a fixing unit that fixes the transferred image on the recording medium, 5. An image forming apparatus, wherein the toner is the toner according to claim 1.

8. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; A fixing step of fixing the transferred image transferred onto the recording medium, An image forming method, wherein the toner is the toner according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Toner, parent particle for toner, developer, developing device, process cartridge, and image forming apparatus

    JP2005173578A

  • Toner, developer, image forming apparatus, and process cartridge

    JP2005196056A

  • Toner and developer, toner-containing vessel, process cartridge, and image forming apparatus and method

    JP2006085095A

  • Toner for developing electrostatic charge image, developer, image forming method, and image forming apparatus

    JP2011018029A

  • Toner, image forming apparatus, image forming method, process cartridge, and developer

    JP2015072445A