Solid Oxide Fuel Cell

The solid oxide fuel cell design with a third oxide phase in the air electrode interface addresses thermal stress issues by enhancing bonding strength and maintaining power generation performance.

JP7585822B2Active Publication Date: 2024-11-19DENSO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021012176
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-28
Publication Date
2024-11-19
Estimated Expiration
2041-01-28

AI Technical Summary

Technical Problem

The challenge in solid oxide fuel cells is the decrease in strength of the air electrode due to thermal stress caused by differing linear thermal expansion coefficients of materials, which affects bonding properties and reduces power generation performance.

Method used

A solid oxide fuel cell design with an air electrode comprising first and second particles of different oxide materials, where a third oxide phase is unevenly distributed in the contact interface region, enhancing bonding strength and maintaining gas permeability.

Benefits of technology

The uneven distribution of the third oxide phase improves bonding between particles, reducing thermal stress and maintaining the strength of the air electrode while preserving power generation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585822000001
    Figure 0007585822000001
  • Figure 0007585822000002
    Figure 0007585822000002
  • Figure 0007585822000003
    Figure 0007585822000003
Patent Text Reader

Abstract

To provide a solid oxide fuel cell capable of suppressing a decrease in strength while maintaining the gas permeability of an air electrode by enhancing the bondability at the interface of different material particles that constitute the air electrode.SOLUTION: In a solid oxide fuel cell 1 in which an air electrode 2, a solid electrolyte layer 3, and a fuel electrode 4 are sequentially stacked, the air electrode 2 is a porous layer that includes first particles 21 made of a first oxide material having electronic conductivity, second particles 22 made of a second oxide material having oxide ion conductivity, and a third oxide phase 23. The third oxide phase 23 contains at least one of the constituent elements of the first oxide material excluding oxygen and at least one of the constituent elements of the second oxide material excluding oxygen, and is unevenly distributed in a contact interface region between the first particles 21 and the second particles 22.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid oxide fuel cell having a solid electrolyte layer, an air electrode, and a fuel electrode. [Background technology]

[0002] The basic component of a solid oxide fuel cell is a single cell that includes a solid electrolyte layer and an air electrode (cathode) and a fuel electrode (anode) formed on both sides of the solid electrolyte layer. To improve the power generation performance of a single cell, it is desirable to increase gas permeability by making the air electrode and the fuel electrode porous layers, while reducing the internal resistance and interface resistance of the electrodes to efficiently promote the electrode reaction.

[0003] In addition, since each layer constituting a single cell is a laminated structure of different materials, it is known that, for example, a layer for suppressing interlayer reactions or a layer for reducing interface resistance is inserted between the layers. It has also been proposed to make each layer a multi-layer structure or to construct it from a composite material. In either case, it is necessary to ensure not only the power generation performance of the single cell but also the mechanical strength.

[0004] For example, Patent Document 1 discloses that an anode support, which functions as a fuel electrode and also as a support for ensuring the mechanical strength of a single cell, is made of composite material particles. In general, an anode support is made of a mixed sintered body of an electron-conductive electrode material and an oxide-ion-conductive support material, and Patent Document 1 uses composite material particles in which these materials are integrated in advance as a raw material to improve the sintering property while maintaining the porosity of the porous anode support. The composite material particles have a particle structure in which high-strength zirconia particles with a large average particle size are used as mother particles, and highly active nickel oxide fine powder with a large specific surface area is fixed to the surface of the mother particles. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2012-146579 A Summary of the Invention [Problem to be solved by the invention]

[0006] On the other hand, the air electrode is composed of, for example, a transition metal perovskite oxide. Transition metal perovskite oxides are known to have good electronic conductivity and oxide ion conductivity. Some of them have an intermediate layer made of an oxide ion conductor between the air electrode and the solid electrolyte layer, and for example, the addition of an intermediate layer material to the air electrode material is being considered.

[0007] However, the linear thermal expansion coefficient of transition metal perovskite oxides is generally larger than that of the intermediate layer material. Therefore, when a porous layer serving as an air electrode is formed using these mixed raw materials, there is a concern that thermal stress will be applied to the particle interface of different materials due to thermal cycles during operation, resulting in a decrease in strength. In addition, the particle structure in which minute child particles are fixed to mother particles, as in Patent Document 1, not only requires a laborious granulation process, but also does not necessarily improve the bonding strength of the interface between the child particles and the mother particle, making it difficult to apply to air electrodes.

[0008] The present invention has been made in consideration of these problems, and aims to provide a solid oxide fuel cell that can suppress a decrease in strength while maintaining the gas permeability of the air electrode by improving the bonding at the interface between particles of different materials that make up the air electrode. [Means for solving the problem]

[0009] One aspect of the present invention is a solid oxide fuel cell (1) in which an air electrode (2), a solid electrolyte layer (3), and a fuel electrode (4) are stacked in this order, The air electrode is a porous layer including first particles (21) made of a first oxide material having electronic conductivity, second particles (22) made of a second oxide material having oxide ion conductivity, and a third oxide phase (23) including at least one of the constituent elements of the first oxide material, excluding oxygen, and at least one of the constituent elements of the second oxide material, excluding oxygen; The third oxide phase is unevenly distributed in the contact interface region between the first particles and the second particles. And, an abundance ratio of the third oxide phase in the contact interface region is 90 vol % or more with respect to the entire third oxide phase present in the interface region between the first particle and the second particle; The average thickness of the third oxide phase in the contact interface region is 15 nm or more and 150 nm or less. The present invention relates to a solid oxide fuel cell. Effect of the Invention

[0010] The cathode of the solid oxide fuel cell has the third oxide phase distributed unevenly in the contact interface region between the first and second particles, and therefore can strengthen the bond between the particles without impeding the electrode reaction on the surfaces of the first and second particles, thereby reducing the thermal stress generated at the interface between the first and second particles and suppressing a decrease in the strength of the cathode, which is a porous layer.

[0011] As described above, according to the above aspect, it is possible to provide a solid oxide fuel cell that can improve the bonding at the interface between the different material particles that make up the air electrode, thereby suppressing a decrease in strength while maintaining the gas permeability of the air electrode. In addition, the symbols in parentheses described in the claims and the means for solving the problems indicate a correspondence with the specific means described in the embodiments described below, and do not limit the technical scope of the present invention. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic structure of a main part of a fuel cell according to a first embodiment. [Diagram 2] FIG. 2 is an overall cross-sectional view showing a schematic view of a stacked structure of the fuel cell according to the first embodiment. [Diagram 3] An enlarged view of part A in FIG. [Figure 4]FIG. 2 is a cross-sectional view illustrating the structure of the air electrode in the first embodiment in comparison with other air electrode structures. [Diagram 5] FIG. 3 is an explanatory diagram of the function and effect of the air electrode structure in the first embodiment. [Figure 6] FIG. 4 is a graph showing concentration profiles of Ce and Co across the contact interface region by TEM-EDX in Example 1. [Figure 7] 4 is a cross-sectional TEM image of the air electrode in Example 1. [Figure 8] FIG. 2 shows a cross-sectional TEM image of the air electrode in Comparative Example 1 and concentration profiles of Ce and Co. [Figure 9] FIG. 13 shows a cross-sectional TEM image of the air electrode in Comparative Example 2 and concentration profiles of Ce and Co. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] (Embodiment 1) An embodiment of a solid oxide fuel cell will be described with reference to Figs. 1 to 3. A solid oxide fuel cell (hereinafter, abbreviated as fuel cell as appropriate) 1 is a fuel cell that uses solid oxide ceramics as a solid electrolyte (i.e., SOFC; Solid Oxide Fuel Cell). As shown in Fig. 2, the fuel cell 1 has a configuration in which an air electrode (cathode) 2, a solid electrolyte layer 3, and a fuel electrode (anode) 4 are laminated in this order. From the viewpoint of high power generation performance, the fuel cell 1 can have a flat plate type cell structure.

[0014] As shown in Fig. 1, the fuel cell 1 has an air electrode 2 on one side of a solid electrolyte layer 3. The air electrode 2 is configured as a porous layer including first particles 21 and second particles 22, with pores 24 formed between the particles. The first particles 21 are made of a first oxide material having electronic conductivity, preferably having electronic conductivity and oxide ion conductivity. The second particles 22 are made of a second oxide material having oxide ion conductivity. The air electrode 2 further includes a third oxide phase 23 (see, for example, Fig. 3).

[0015] 3, the third oxide phase 23 is unevenly distributed in the contact interface region (hereinafter, appropriately abbreviated as the contact interface region) between the first particle 21 and the second particle 22. The third oxide phase 23 contains at least one of the constituent elements of the first oxide material excluding oxygen, and at least one of the constituent elements of the second oxide material excluding oxygen.

[0016] Such a third oxide phase 23 is preferably configured as a reaction product phase that is generated by a reaction between the first oxide material and the second oxide material in the contact interface region between the first particle 21 and the second particle 22. In this case, the reaction product phase refers to a phase in which an oxide having a constant composition ratio of each constituent element is generated between the first particle 21 and the second particle 22. As a result, the first particle 21 and the second particle 22 are chemically bonded, and the bonding strength is improved compared to, for example, bonding by element diffusion.

[0017] Here, the contact interface region refers to a region where the particle interfaces of first particles 21 and second particles 22, which are particles of different materials, contact each other. In the air electrode 2, the third oxide phase 23 is biased toward this contact interface region. That is, the amount of the third oxide phase 23 present in the contact interface region is greater than the amount of the third oxide phase 23 present outside the contact interface region. This provides the effect of strengthening the bond between the different materials without inhibiting the electrode reaction.

[0018] Specifically, the abundance ratio of the third oxide phase 23 in the contact interface region is preferably 80% by volume or more with respect to the entire third oxide phase 23 present in the interface region between the first particle 21 and the second particle 22. In other words, the abundance ratio of the third oxide phase 23 present in interface regions other than the contact interface region between the first particle 21 and the second particle 22 is preferably less than 20% by volume. It is preferable that the third oxide phase 23 is unevenly distributed in the contact interface region and the abundance ratio is as large as possible, and the electrode reaction can be efficiently advanced at the two-phase interface between the oxidant gas introduced into the pores 24 and the first particle 21, or the three-phase interface between the oxidant gas and the first particle 21 and the second particle 22.

[0019] Here, the interface region of the first particle 21 and the second particle 22 refers to the entire region along the particle interface of the first particle 21 and the entire region along the particle interface of the second particle 22, and refers to the entire interface region including the contact interface region where the interfaces of the first particle 21 and the second particle 22 are in contact with each other, and the interface region of the first particle 21 and the second particle 22 other than the contact interface region. The interface region other than the contact interface region includes the interface between the first particle 21 or the second particle 22 and the pores 24, and the interface between the first particles 21 or between the second particles 22.

[0020] The abundance ratio of the third oxide phase 23 refers to the ratio of the third oxide phase 23 present in the contact interface region to the entire third oxide phase 23 present in the entire interface region. The abundance ratio of the third oxide phase 23 can be quantitatively measured by analyzing the composition of the particle interface by a spectroscopic method and analyzing the obtained data by a statistical method. For example, the degree of uneven distribution of the third oxide phase 23 can be calculated as a volume ratio based on the result of elemental analysis of the interface region between the first particle 21 and the second particle 22 by observing the cross section of the sample using TEM-EDX (energy dispersive X-ray spectroscopy with a transmission electron microscope). Specifically, first, the number of required measurement points is determined statistically (for example, confidence interval 95%, allowable error 15%) from the result obtained by performing a preliminary line analysis (for example, number of samples: N=5). Then, based on the existence state of the third oxide phase 23 derived from the element distribution in the actual measurement data, the proportion (volume basis) of the third oxide phase 23 present in the contact interface region is calculated to obtain the abundance ratio. The calculated value indicates the average abundance ratio of the third oxide phase 23 in an arbitrarily selected measurement region, and can be used as an abundance ratio representative of the entire interface region.

[0021] The third oxide phase 23 may have an average thickness of, for example, 200 nm or less, preferably 150 nm or less, more preferably 100 nm or less, from the viewpoint of suppressing the decrease in electronic conductivity and ionic conductivity. The third oxide phase 23 may have a thickness capable of strengthening the bond between the first particle 21 and the second particle 22, and may be specifically greater than or equal to the thickness of a general particle interface, for example, 10 nm or more. Preferably, the third oxide phase 23 may be formed to have a thickness of 15 nm or more, more preferably 20 nm or more, from the viewpoint of improving the bondability of the interface. This allows the desired bond strength to be obtained, and the increase in electrical resistance in the electronic conduction path or ionic conduction path to be suppressed, thereby suppressing the decrease in power generation performance.

[0022] Here, the average thickness of the third oxide phase 23 can be calculated based on the results of line analysis including the contact interface region between the first particle 21 and the second particle 22, for example, by observing the cross section of the sample using TEM-EDX (energy dispersive X-ray spectroscopy with a transmission electron microscope). Specifically, line analysis is performed on arbitrarily selected contact interface regions of the cross section of the sample to calculate the thickness of the contact interface region at each measurement point, and the arithmetic average value is obtained to be the average thickness. In this case, as in the measurement of the abundance ratio, the average of the values ​​actually measured for a statistically derived number of measurement points can be adopted as a value representing the thickness of the third oxide phase 23 in the air electrode 2.

[0023] In this way, the cathode 2 has the third oxide phase 23 between the first particles 21 and the second particles 22, which strengthens the bond at the particle interface between the different materials. This reduces thermal stress caused by the difference in linear thermal expansion coefficient, and improves power generation performance while maintaining the strength of the cathode 2, which is a porous layer. A more specific configuration of the cathode 2 will be described later.

[0024] Next, the configuration of each part of the fuel cell 1 will be described in detail. 2, a single cell, which is a basic component of a fuel cell 1, has a flat laminate structure in which an air electrode 2, a solid electrolyte layer 3, and a fuel electrode 4 are laminated in this order. The single cell may be, for example, an anode-supported type in which the anode, which is the fuel electrode 4, serves as a support. In this case, the resistance of the solid electrolyte layer 3 can be reduced by making the solid electrolyte layer 3 thinner, and ion conductivity can be easily improved, compared to a free-standing membrane type in which the solid electrolyte layer 3 serves as a support.

[0025] The air electrode 2, which is the cathode, and the fuel electrode 4, which is the anode, are gas permeable porous electrode layers, and a solid electrolyte layer 3, which is a layer denser than these electrode layers, is disposed between the air electrode 2 and the fuel electrode 4. The air electrode 2 side of the solid electrolyte layer 3 is exposed to an oxidant gas atmosphere, and the fuel electrode 4 side of the solid electrolyte layer 3 is exposed to a fuel gas atmosphere. The oxidant gas is, for example, air containing oxygen, and the fuel gas is, for example, a gas containing hydrogen generated by steam reforming of a hydrocarbon or the like.

[0026] The solid electrolyte layer 3 is formed by absorbing oxide ions (O 2- ) is permeated and supplied to the fuel electrode 4 side. At the fuel electrode 4, hydrogen and oxide ions react to generate water and electrons (e - ) is released. The fuel cell 1 generates electricity through such an electrochemical reaction and extracts the resulting electrical energy to the outside. The fuel cell 1 can be configured as a cell stack in which a plurality of unit cells are stacked so as to obtain a desired power generation output, with gas supply passages, current collectors, and the like (not shown) being arranged on the outside of each electrode layer of the unit cells.

[0027] The material of the solid electrolyte layer 3 is not particularly limited, and a known solid oxide ceramic having oxide ion conductivity is used. Specific examples include zirconium oxide (ZrO2)-based oxides such as stabilized zirconia, cerium oxide (CeO2)-based oxides such as ceria-based solid solutions, and perovskite-type oxides. One or more of these may be used in combination.

[0028] Preferably, stabilized zirconia, which is excellent in strength and thermal stability, can be used as the solid electrolyte layer material. Stabilized zirconia is stabilized by dissolving an oxide containing an alkaline earth metal or a rare earth element in zirconia, and examples of such stabilized zirconia include yttria-stabilized zirconia (YSZ) and scandia-stabilized zirconia (ScSZ). Yttria-stabilized zirconia can be mainly used from the viewpoints of ion conductivity, mechanical stability, and chemical stability from air atmosphere to fuel gas atmosphere.

[0029] The air electrode 2 and the solid electrolyte layer 3 may be in direct contact with each other, but when a zirconium oxide-based oxide is used as the solid electrolyte layer material, it is preferable to form an intermediate layer 5, which mainly functions as a reaction suppression layer, between the air electrode 2 and the solid electrolyte layer 3, as exemplified in Fig. 2. The material for the intermediate layer 5 is a solid oxide that has oxide ion conductivity, is interposed between the air electrode 2 and the solid electrolyte layer 3, and can suppress the reaction between the first oxide material contained in the air electrode material constituting the air electrode 2 and the solid electrolyte layer material.

[0030] The fuel electrode 4 may be composed of a single layer or multiple layers. Fig. 2 shows an example composed of multiple layers, in which case the fuel electrode 4 can be configured to include an active layer 41 arranged on the solid electrolyte layer 3 side and a diffusion layer 42 arranged on the opposite side of the active layer 41 from the solid electrolyte layer 3 side. The active layer 41 is a layer that mainly enhances the electrochemical reaction on the fuel electrode 4 side, and the diffusion layer 42 is a layer that can diffuse the supplied fuel gas into the layer plane.

[0031] The material of the fuel electrode 4 may be, for example, a mixture of an electron conductive material and an oxide ion conductive material. Examples of the electron conductive material include metals having catalytic action or their oxides, such as metallic nickel (Ni) and nickel oxide (NiO), and examples of the oxide ion conductive material include the above-mentioned zirconium oxide-based oxides. Note that NiO becomes Ni in a reducing atmosphere during power generation. Specifically, a mixture of Ni or NiO and yttria-stabilized zirconia may be used.

[0032] 1, the air electrode 2 is composed of first particles 21 and second particles 22 having different compositions. The first particles 21 are the main electrode material and are composed of a first oxide material having electronic conductivity. The second particles 22 are composed of a second oxide material having oxide ion conductivity and can be the same as or the same as the intermediate layer material constituting the intermediate layer 5.

[0033] As the first oxide material constituting the first particle 21, an oxide having a catalytic effect on the reaction in the air electrode 2 and at least electronic conductivity in an oxidizing atmosphere can be used. Specifically, an oxide having mixed conductivity of electrons and oxide ions, such as a perovskite-type oxide containing a transition metal element (hereinafter referred to as a transition metal perovskite oxide), is used. The transition metal perovskite oxide is a composite oxide having a perovskite structure represented by the general formula ABO3 and containing at least one transition metal element (e.g., Mn, Fe, Co, Ni, Cu, etc.). Specifically, there can be mentioned a structural oxide containing a lanthanoid element (e.g., La, Sm, etc.) in the A site of the general formula ABO3 and a transition metal element in the B site, with some of these elements being replaced with an alkaline earth metal element or a rare earth element.

[0034] Preferably, such transition metal perovskite oxides are (La,M1)(Co,M2)O3-based oxides or (La,M1)(Gd,Mg,M2)O3-based oxides, where M1 and M2 represent at least one selected from the following metal elements: M1: Sr, Ca, Ba M2: Ni, Co, Mn, Fe, Cu

[0035] As the first oxide material, from the viewpoint of enhancing the reactivity of the three-phase interface in the air electrode 2, a perovskite-type cobalt oxide such as lanthanum strontium cobaltite (La x Sr 1-x CoO3)-type oxide, and at least one of lanthanum strontium cobalt ferrite (La x Sr 1-x Co y Fe 1-y O3)-type oxide is more preferably contained. However, in the formula, 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1.

[0036] As the second oxide material constituting the second particles 22, a solid oxide having oxide ion conductivity, capable of expanding the three-phase interface in the air electrode 2, and having low reactivity with the first oxide material in the use environment, such as ceria or a ceria-based solid solution, etc., a cerium oxide-based oxide, a perovskite-type oxide, etc. are used. Also, it is preferable that the linear thermal expansion coefficient is smaller than that of the first oxide material and the difference in the linear thermal expansion coefficient from the constituent material of the adjacent layer is small. When the layer adjacent to the air electrode 2 is the intermediate layer 5, by configuring the second oxide material and the intermediate layer material with the same material, the difference in the linear thermal expansion coefficient can be made extremely small, and the bonding property at the interface can be improved.

[0037] Specific examples of the ceria-based solid solution include, for example, doped ceria doped with one or more elements selected from alkaline earth metal elements (such as Mg, Ca, Sr, Ba, etc.), rare earth elements (such as Sc, Y, La, Nd, Sm, Gd, Ho, Yb, etc.), and other elements (such as Ti, Zr, Nb, etc.). Perovskite-type oxides include those containing one or more elements selected from alkaline earth metal elements, rare earth elements, etc. in each of the A-site and B-site.

[0038] Preferably, as the second oxide material, ceria, gadolinium-doped ceria (GDC), samarium-doped ceria (SDC), etc. are mainly used from the viewpoints of ion conductivity, reactivity with the first oxide material, etc.

[0039] The intermediate layer 5 is made of a material similar to the second oxide material. Preferably, from the viewpoints of ion conductivity and suppressing the reactivity between the solid electrolyte layer material and the first oxide material, ceria, gadolinium-doped ceria (GDC), samarium-doped ceria (SDC), etc. are mainly used, which can improve the bond with the air electrode 2 and reduce the interface resistance.

[0040] Here, the first oxide material and the second oxide material usually have a large difference in linear thermal expansion coefficient. For example, the linear thermal expansion coefficient of (La,Sr)CoO3 used as the first oxide material is 15×10 -6 / K~22×10 -6 / K, which varies with temperature (for example, 18×10 -6 / K, 900℃ 20×10 -6 / K). The linear thermal expansion coefficient of (La,Sr)(Co,Fe)O3 is smaller than that of (La,Sr)CoO3. The linear thermal expansion coefficient is measured in the temperature range of 25°C to 900°C in accordance with JIS R1618:2002. The same applies to the linear thermal expansion coefficient described below.

[0041] In contrast, the linear thermal expansion coefficient of gadolinium-doped ceria used as the second oxide material is about 9.3 ppm / K. Therefore, the bond between the first particles 21 and the second particles 22 is likely to deteriorate due to the difference in the linear thermal expansion coefficient between the two materials caused by thermal cycles during operation of the fuel cell 1. In such a case, the strength of the air electrode 2 is reduced due to a decrease in the bond strength between the particles, and the electrode reaction resistance in the air electrode 2 is likely to increase, leading to a decrease in power generation performance.

[0042] Thus, in the air electrode 2, a third oxide phase 23 is formed in the contact interface region between the first particle 21 and the second particle 22. As described above, the first oxide material constituting the first particle 21 and the second oxide material constituting the second particle 22 have different compositions, and the third oxide phase 23 is formed by the reaction of these materials in the contact interface region. The third oxide phase 23 is a reaction product phase and has a composition independent of the first oxide material or the second oxide material. Specifically, the third oxide phase 23 is composed of one or more of the constituent elements (excluding oxygen) of the first oxide material and the second oxide material.

[0043] When the first oxide material is a lanthanum cobaltite-based oxide and the second oxide material is a ceria-based solid solution, the third oxide phase 23 is composed of an oxide containing cerium and at least one of lanthanum and cobalt. Preferably, the third oxide phase 23 is an oxide containing lanthanum, cobalt, and cerium.

[0044] 3, in the air electrode 2, constituent particles including first particles 21 and second particles 22 are bonded to each other to form a porous layer capable of electronic or ion conductivity, and a large number of pores 24 (see, for example, FIG. 1) are formed between the constituent particles, which communicate with each other and allow the oxidant gas to pass through. A third oxide phase 23 is formed in the contact interface region between the first particles 21 and the second particles 22.

[0045] The third oxide phase 23 is mainly formed along the interface where the first particle 21 and the second particle 22 contact each other. The third oxide phase 23 is hardly formed on the surface of the first particle 21 or the second particle 22 facing the pores 24. As described above, the abundance ratio of the third oxide phase 23 in the contact interface region is preferably 80% by volume or more, and more preferably 90% by volume or more, relative to the entire third oxide phase 23 present in the interface region between the first particle 21 and the second particle 22. This allows both the bonding strength and the power generation performance to be achieved. The abundance ratio of the third oxide phase 23 can be adjusted by the sintering conditions of the air electrode 2, as described later.

[0046] 4, when the fuel cell 1 is cooled after being heated to an operating temperature, compressive stress occurs in the second particles 22 made of the second oxide material with a small linear thermal expansion coefficient near the contact interface region between the first particles 21 and the second particles 22, and tensile stress occurs in the first particles 21 made of the first oxide material with a large linear thermal expansion coefficient. Even in this case, the third oxide phase 23 formed in the contact interface region improves the bonding strength at the interface between the first particles 21 and the second particles 22, and an effect of suppressing destruction of the interface due to the generated stress is obtained.

[0047] In the case where the third oxide phase 23 is not formed in the contact interface region between the first particle 21 and the second particle 22 as shown in the left diagram of Fig. 5 in the configuration having the third oxide phase 23, the bonding strength between the first particle 21 and the second particle 22 becomes insufficient, and there is a risk of interface destruction or the like occurring due to thermal cycles during operation. In addition, as shown in the right diagram of Fig. 5, when the third oxide phase 23 is formed not only in the contact interface region between the first particle 21 and the second particle 22 but also on the surface of the first particle 21 or the second particle 22 facing the pores 24, the number of two-phase interfaces and three-phase interfaces contributing to the electrode reaction decreases, and power generation performance decreases.

[0048] The porosity of the porous layer constituting the air electrode 2 can be, for example, in the range of 20% to 50%. By improving the bonding between the first particles 21 and the second particles 22, the strength of the air electrode 2 can be maintained even if the porosity is increased. The porosity of the solid electrolyte layer 3 or the intermediate layer 5 is 20% or less, and the porosity of the fuel electrode 4 can be in the range of 20% to 50%. The porosity of the porous layer constituting the air electrode 2 is preferably higher than that of the intermediate layer 5. The porosity mentioned above is a value calculated by calculating the apparent density and bulk density by Archimedes' method, and then calculating {1-(bulk density / apparent density)}×100.

[0049] The fuel cell 1 of this embodiment can be manufactured, for example, as follows. First, a ceramic substrate is prepared in which the fuel electrode 4, the solid electrolyte layer 3, and the intermediate layer 5 are laminated in this order. The ceramic substrate can be prepared, for example, by using a sheet forming process.

[0050] Next, the paste for forming an air electrode is applied in a layer shape on the surface of the intermediate layer 5 of the ceramic substrate by screen printing or the like, and baked by firing. The paste for forming an air electrode can be prepared in a paste shape, for example, by mixing the first oxide material and the second oxide material in a predetermined ratio, and adding a binder, a solvent, or the like. The mixing ratio of the first oxide material and the second oxide material can be appropriately set in terms of power generation performance, bonding with the intermediate layer 5, and the like, within a range of, for example, 25:75 to 50:50 in volume ratio. Specifically, the mixing ratio of the first oxide material and the second oxide material can be, for example, 30:70 in volume ratio.

[0051] The firing temperature is equal to or higher than the decomposition temperature or reaction temperature of the first oxide material or the second oxide material, and is selected so that the third oxide phase 23 can be generated by the reaction between the first oxide material and the second oxide material, and the third oxide phase 23 can be unevenly distributed in the contact interface region between different particles. The firing time can be appropriately adjusted depending on the thickness, the amount of binder, etc., but is selected as a relatively short time so that the reaction does not proceed outside the contact interface region. For example, the firing temperature is adjusted to a temperature higher than 1000°C, preferably 1100°C or higher, and lower than 1200°C, preferably 1150°C or lower, and the firing time can be adjusted to a range of 30 minutes or less. Specifically, firing can be performed at a temperature of about 1125°C for about 10 minutes, and by performing firing for a short time at a high temperature, the third oxide phase 23 can be mainly formed in the contact interface region between the first particle 21 and the second particle 22.

[0052] In this manner, the solid oxide fuel cell 1 can be manufactured. In the air electrode 2 after firing, the average particle diameter D50 of the first particles 21 can be 0.1 μm to 10 μm, preferably 0.5 to 5 μm. The average particle diameter D50 of the second particles 22 can be 0.1 μm to 10 μm, preferably 0.5 to 5 μm. In this range, the particle interface is prevented from impairing the conductivity in the electron conduction path or ion conduction path, while the decrease in reaction sites at the three-phase interface is suppressed, allowing the electrode reaction to proceed.

[0053] The average particle size of the sintered grains in the air electrode 2 is calculated by measuring the particle sizes of, for example, 100 random sintered grains through cross-sectional observation using a scanning electron microscope, and calculating the arithmetic mean value. The scanning electron microscope used is SU8200 manufactured by Japan High-Technologies Corporation, and the average particle size is determined from SEM images at a magnification of 300 to 5000 times.

[0054] In the fuel cell 1, the thickness of the solid electrolyte layer 3 may be preferably 3 to 20 μm, more preferably 5 to 15 μm, from the viewpoint of reducing ohmic resistance. The thickness of the fuel electrode 4 may be, for example, preferably 100 to 1000 μm, more preferably 200 to 700 μm, from the viewpoints of gas diffusion, electrical resistance, strength, etc. The thickness of the air electrode 2 may be preferably 20 to 100 μm, more preferably 30 to 80 μm, from the viewpoints of gas diffusion, electrode reaction resistance, current collection, etc. The thickness of the intermediate layer 5 may be preferably 1 to 20 μm, more preferably 5 to 15 μm, from the viewpoints of reducing ohmic resistance, suppressing element diffusion from the air electrode 2, etc. EXAMPLES

[0055] Example 1 A fuel cell 1 having the same configuration as that of the above-mentioned embodiment 1 was fabricated as follows, and the state of formation of the third oxide phase 23 in the interface region between the first particle 21 and the second particle 22 of the air electrode 2 was confirmed. In addition, a comparison was made of the state of formation of the third oxide phase 23 in the interface region when the firing temperature in forming the air electrode 2 was changed (Comparative Example 1 and Comparative Example 2). <Material preparation>

[0056] NiO powder, yttria-stabilized zirconia powder containing 8 mol% Y2O3, carbon as a pore former, polyvinyl butyral as a binder, and isoamyl acetate, 2-butanol, and ethanol as a mixed solvent were mixed in a ball mill to prepare a slurry. Hereinafter, yttria-stabilized zirconia containing 8 mol% Y2O3 is referred to as "8YSZ". The average particle diameter of the NiO powder is 1.0 μm, and the average particle diameter of the 8YSZ powder is 0.8 μm. The mass ratio of the NiO powder to the YSZ powder was 60:40. The above slurry was applied in a layer on a plastic substrate using a doctor blade method, and dried to prepare a sheet for forming an anode.

[0057] The average particle size of a powder is the particle size d50 at which the cumulative frequency distribution on a volume basis measured by a laser diffraction / scattering method is 50%. The particle size is specifically the diameter, and the same applies to the average particle size of powders described below.

[0058] A slurry was prepared by mixing 8YSZ powder with an average particle size of 0.8 μm, polyvinyl butyral as a binder, and isoamyl acetate, 2-butanol, and ethanol as a mixed solvent in a ball mill. This slurry was applied in a layer on a plastic substrate by a doctor blade method and dried to prepare a sheet for forming a solid electrolyte layer.

[0059] 10mol% Gd-doped ceria (Ce 0.9 Gd 0.1 O 1.95 A slurry was prepared by mixing the powder of Gd, polyvinyl butyral as a binder, and isoamyl acetate, 2-butanol, and ethanol as a mixed solvent in a ball mill. 10 mol % Gd-doped ceria is hereinafter referred to as "10GDC". The average particle size of the 10GDC powder is 0.8 μm. This slurry was applied in a layer on a plastic substrate using a doctor blade method and dried to prepare a sheet for forming an intermediate layer.

[0060] The first and second oxide materials constituting the air electrode 2 are lanthanum strontium cobaltite (La 0.6 Sr 0.4 CoO3) powder and 10GDC powder with an average particle size of 0.8 μm were prepared. Lanthanum strontium cobaltite is hereinafter referred to as "LSC". The average particle size of the LSC powder is 1.5 μm. The LSC powder constituting the first particles 21 and the 10GDC powder constituting the second particles 22 were mixed together. Volume ratio The mixture was mixed in a ratio of 30:70, and ethyl cellulose as a binder and terpineol as a solvent were mixed in a ball mill to prepare a paste for forming an air electrode.

[0061] <Fuel cell construction> The fuel electrode forming sheet, the solid electrolyte layer forming sheet, and the intermediate layer forming sheet were laminated in this order to obtain a laminate. The obtained laminate was pressed and degreased using a hydrostatic press molding method. Hydrostatic press is also called CIP. The CIP molding conditions were a temperature of 80°C, a pressure of 50 MPa, and a pressurizing time of 10 minutes.

[0062] The laminate was fired for 2 hours at 1350° C. This produced a sintered body that would become a ceramic substrate in which a 500 μm-thick fuel electrode, a 10 μm-thick solid electrolyte layer, and a 10 μm-thick intermediate layer were laminated in this order.

[0063] Next, the paste for forming an air electrode was applied to the surface of the intermediate layer 5 of the ceramic substrate by screen printing and fired at 1125°C for 10 minutes to form an air electrode 2 with a thickness of 50 μm. The average particle diameter of the sintered grains of the air electrode 2 was 1.5 μm for the first particles 21 and 1.5 μm for the second particles 22.

[0064] In this manner, the fuel cell 1 in which the fuel electrode 4, the solid electrolyte layer 3, the intermediate layer 5, and the air electrode 2 were laminated in this order and joined together was obtained.

[0065] For comparison, the firing temperature in forming the air electrode 2 was changed to 1000°C as Comparative Example 1, and the firing temperature was changed to 1200°C as Comparative Example 2.

[0066] <Evaluation method> For the fuel cell 1 of Example 1, a cross-sectional sample of the air electrode 2 for evaluation was prepared, and interface observation and elemental analysis were performed using TEM-EDX (JEM-ARM300F manufactured by JEOL Ltd.; acceleration voltage 300 kV). As shown in Figs. 6 and 7 as an example, elemental analysis was performed on the main constituent elements of the first particle 21 and the second particle 22, and a line analysis was performed across the contact interface region between the first particle 21 and the second particle 22 to obtain a concentration profile. Here, Co contained in the LSC constituting the first particle 21 and Ce contained in the GDC constituting the second particle 22 were measured from the second particle 22 side to the first particle 21 side as shown by the arrow in Fig. 7, and the results are shown in Fig. 6.

[0067] As shown in Fig. 6, as the measurement position moves from the GDC side to the LSC side, the signal intensity of Ce decreases, while the signal intensity of Co increases. In addition, between the first particle 21 and the second particle 22, the signal intensity of Ce and Co changes stepwise, and a reaction product phase having a composition different from either the first oxide material or the second oxide material was confirmed at the particle interface. Although not shown in Fig. 6, a similar elemental analysis confirmed that the third oxide phase 23 formed between the first particle 21 and the second particle 22 contains La, which is a constituent element of LSC, in addition to Ce and Co.

[0068] 6, the signal intensity of Ce or Co changes from a substantially constant region through a gradient composition region in which it decreases or increases, to a step-like region, and then changes again through a gradient composition region to a substantially constant region. At this time, the interfaces between the third oxide phase 23 and the first particle 21 and the second particle 22 can be located at the middle positions of the two gradient composition regions sandwiching the step-like region. The thickness of the third oxide phase 23 can be represented by the distance between the middle positions of the two gradient composition regions.

[0069] Specifically, the concentration profiles of the constituent elements of the first particle 21 and the second particle 22 whose contents are 1 mass % or more are obtained, and the thickness is defined based on the element (e.g., Ce) that shows the strongest signal. In this case, for example, the parameters A1, A2, B1, B2, C1, and C2 are optimized by the least squares method using the function f(x) shown below, and the absolute value of the difference between the obtained C1 and C2, |C1-C2|, can be defined as the thickness of the third oxide phase 23. f(x)=A1 / (EXP(-B1*(x-C1))+1)+A2 / (EXP(-B2*(x-C2))+1)+y0 However, A1, A2>0

[0070] The thickness of the third oxide phase 23 calculated in this manner for the measurement points shown in FIG. 6 was 89 nm. Furthermore, measurements were performed in the same manner for arbitrarily selected measurement points on the same cross-sectional sample for evaluation. The number of measurement points in this case was statistically determined in advance, and a line analysis was performed at one location for one contact interface region to calculate the thickness of each of the third oxide phases 23. As a result, the calculated thicknesses of the third oxide phase 23 were all in the range of 20 nm to 100 nm, and the average thickness, which was the arithmetic mean value thereof, was 40.9 nm.

[0071] In this way, as shown in Fig. 7, it was confirmed that a phase that would become the third oxide phase 23 was formed in the contact interface region between the first particles 21 (gray particles in the figure) and the second particles 22 (white particles in the figure) in the air electrode 2 of Example 1. Note that Fig. 7 is an enlarged view of a portion of the cross-sectional sample for evaluation.

[0072] In contrast, the air electrodes 2 of Comparative Examples 1 and 2 were observed and analyzed in the interface region by the same method. No different phase was found in the air electrode 2 of Comparative Example 1, and a different phase was found in the interface region other than the contact interface region between the first particle 21 and the second particle 22 in the air electrode 2 of Comparative Example 2. In Comparative Example 1, as shown in the left diagram of FIG. 8, the measurement was performed from the second particle 22 side to the first particle 21 side. In the line analysis results shown in the right diagram of FIG. 8, when moving from the region with a lot of Ce on the second particle 22 side to the region with a lot of Co on the first particle 21 side, Ce rapidly decreases and Co rapidly increases. In other words, the third oxide phase 23 is not formed between the first particle 21 and the second particle 22. On the other hand, in Comparative Example 2, as shown in the left diagram of FIG. 9, the measurement was performed on the contact interface between the second particles 22. As shown in the line analysis results in the right diagram of FIG. 9, Ce gradually decreases and Co gradually increases between the regions with a lot of Ce on both sides. That is, a reaction product phase of Ce and Co is formed in areas other than the contact interface region between the first particle 21 and the second particle 22.

[0073] Furthermore, in the air electrode 2 of Example 1, a two-dimensional elemental analysis was performed on the interface region between the first particle 21 and the second particle 22, and the presence ratio of the third oxide phase 23 in the contact interface region was calculated among the third oxide phase 23 present in the entire interface region including the contact interface region between the first particle 21 and the second particle 22. Specifically, for example, a line analysis was performed at a plurality of measurement points arbitrarily selected for the contact interface region between the first particle 21 and the second particle 22, each interface region along the interface between the first particle 21 or the second particle 22 and the pores 24, and each interface region along the interface of the first particle 21 or the second particle 22 other than those, and the average thickness of the third oxide phase 23 in each interface region was determined from the arithmetic average value. Furthermore, the volume of the third oxide phase 23 in the entire interface region and the volume of the third oxide phase 23 in the contact interface region between the first particle 21 and the second particle 22 were calculated from the interface length of each interface region and the average thickness calculated above. Then, the ratio of the latter to the former was calculated, and this was taken as the abundance ratio (unit: volume %) of the third oxide phase 23 in the contact interface region.

[0074] At this time, the number of measurement points in each interface region can be statistically determined in advance as described above. In this way, the existence ratio of the third oxide phase 23 calculated was 95 volume %, and it was confirmed that the third oxide phase 23 was unevenly distributed in the contact interface region between the first particle 21 and the second particle 22.

[0075] In addition, in this example, LSC powder and 10GDC powder were used, but if lanthanum cobaltite and ceria are used as the first particles 21 and the second particles 22 instead of these materials, a third oxide phase 23 containing La, Co and Ce is similarly formed.

[0076] In this way, it was confirmed that the third oxide phase 23 was formed unevenly in the contact interface region between the first particles 21 and the second particles 22 in the air electrode 2. This makes it possible to strengthen the bonds between the particles of different materials while suppressing the effect on the electrode reaction, thereby improving the power generation performance.

[0077] The present invention is not limited to the above-described embodiments, and can be applied to various embodiments without departing from the gist of the present invention. [Explanation of symbols]

[0078] 1 Solid oxide fuel cell 2 Air electrode 3 Solid electrolyte layer 4 Fuel electrode 5. Middle Tier 21 1st particle 22 2nd particle 23 Third oxide phase 24 Stoma

Claims

1. A solid oxide fuel cell (1) in which an air electrode (2), a solid electrolyte layer (3), and a fuel electrode (4) are sequentially stacked, The air electrode is a porous layer including first particles (21) made of a first oxide material having electronic conductivity, second particles (22) made of a second oxide material having oxide ion conductivity, and a third oxide phase (23) including at least one of the constituent elements of the first oxide material, excluding oxygen, and at least one of the constituent elements of the second oxide material, excluding oxygen; the third oxide phase is unevenly distributed in a contact interface region between the first particle and the second particle, an abundance ratio of the third oxide phase in the contact interface region is 90 vol % or more with respect to the entire third oxide phase present in the interface region between the first particle and the second particle; A solid oxide fuel cell, wherein the average thickness of the third oxide phase in the contact interface region is 15 nm or more and 150 nm or less.

2. The solid oxide fuel cell according to claim 1 , wherein the third oxide phase is a reaction product phase of the first oxide material and the second oxide material.

3. 3. The solid oxide fuel cell according to claim 1, wherein the presence ratio of the third oxide phase in the contact interface region between the first particle and the second particle is 95 volume % or more with respect to the entire third oxide phase present in the interface region between the first particle and the second particle.

4. 4. The solid oxide fuel cell according to claim 1, wherein the third oxide phase has an average thickness of 20 nm or more and 100 nm or less.

5. 5. The solid oxide fuel cell according to claim 1, further comprising an intermediate layer (5) made of the second oxide material between the air electrode and the solid electrolyte layer.

6. the first oxide material is a perovskite-type oxide containing a transition metal element, and the second oxide material is a cerium oxide-based oxide; 6. The solid oxide fuel cell according to claim 1, wherein a mixing ratio of the first oxide material to the second oxide material is in a range of 25:75 to 50:50 in terms of volume ratio.

7. the first oxide material is a lanthanum cobaltite-based oxide; 7. The solid oxide fuel cell of claim 6, wherein the third oxide phase comprises lanthanum, cobalt and cerium.

Citation Information

Patent Citations

  • Material for anode support, and method for manufacturing anode support

    JP2012146579A

  • Electrochemical reaction single cell, interconnector-electrochemical reaction single cell composite body, and electrochemical reaction cell stack

    JP2017130327A

  • Porous sintered body

    JP2019196291A