Photocatalyst
A NiCrFe oxide-supported photocatalyst on titanium oxide addresses the cost and environmental issues of rare metal-based systems by achieving high hydrogen production efficiency.
Patent Information
- Application Number
- JP2022016878
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-02-07
AI Technical Summary
Existing photocatalysts using rare metals like ruthenium oxide and iridium oxide are costly and environmentally unfavorable for hydrogen production.
A photocatalyst comprising NiCrFe oxide supported on titanium oxide, with specific atomic ratios of Cr, Ni, and Fe, is developed to enhance water decomposition activity without using rare metals.
The NiCrFe oxide-based photocatalyst achieves high water decomposition activity, generating a significant amount of hydrogen, thus overcoming the cost and environmental concerns of rare metal-based systems.
Smart Images

Figure 0007586107000001 
Figure 0007586107000002 
Figure 0007586107000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocatalyst. [Background technology]
[0002] In recent years, research has been conducted into photocatalysts that are used to split water using light energy to obtain hydrogen. In order to obtain a larger amount of hydrogen, it is preferable that the photocatalyst has high water splitting activity.
[0003] Patent Document 1 describes a photocatalyst in which a barium titanate salt incorporating any one of rare earth elements, alkaline earth metal elements, and titanium group elements is supported with a single oxide of ruthenium oxide, iridium oxide, or tantalum oxide, or a mixture of at least two of the above oxides, for the purpose of increasing water decomposition activity. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 7-88370 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the photocatalyst described in Patent Document 1 uses rare metals such as ruthenium oxide and iridium oxide, which is costly and undesirable from the standpoint of environmental conservation.
[0006] The present invention is devised to solve the above-mentioned problems, and has an object to provide a photocatalyst that has high water splitting activity without using rare metals. [Means for solving the problem]
[0007] The photocatalyst of the present invention has NiCrFe oxide supported on titanium oxide, the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.40 or less; the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.75 or less; The NiCrFe oxide is characterized in that the atomic ratio Fe / (Ni+Cr+Fe) of the content of Fe to the total content of Ni, Cr, and Fe is 0.10 or more and 0.65 or less. Effect of the Invention
[0008] The photocatalyst of the present invention does not contain rare metals but has high activity, and therefore can generate a large amount of hydrogen by decomposing water. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a diagram showing a schematic structure of a photocatalyst of the present invention. [Diagram 2] FIG. 1 is a diagram showing a schematic configuration of an apparatus used for evaluating the activity of a photocatalyst. [Diagram 3] FIG. 1 is a diagram showing the relationship between the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in NiCrFe oxide, which is a promoter for the photocatalyst in the first embodiment, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe, and the proportion of hydrogen in a mixed gas. [Figure 4]3 , where Cr / (Ni+Cr+Fe) is from 0.15 to 0.35, Ni / (Ni+Cr+Fe) is from 0.15 to 0.75, and Fe / (Ni+Cr+Fe) is from 0.10 to 0.55; (b) is a diagram showing ranges of Cr / (Ni+Cr+Fe) from 0.15 to 0.30, Ni / (Ni+Cr+Fe) is from 0.30 to 0.70, and Fe / (Ni+Cr+Fe) is from 0.10 to 0.50; and (c) is a diagram showing ranges of Cr / (Ni+Cr+Fe) from 0.15 to 0.25, Ni / (Ni+Cr+Fe) is from 0.30 to 0.65, and Fe / (Ni+Cr+Fe) is from 0.15 to 0.50. [Diagram 5] FIG. 13 is a diagram showing the relationship between the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in NiCrFe oxide, which is a promoter for a photocatalyst in a second embodiment, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe, and the proportion of hydrogen in a mixed gas. [Figure 6] 5, (a) is a diagram showing ranges of the atomic ratio Cr / (Ni+Cr+Fe) of 0.15 or more and 0.35 or less, the atomic ratio Ni / (Ni+Cr+Fe) of 0.15 or more and 0.75 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of 0.10 or more and 0.55 or less, (b) is a diagram showing ranges of the atomic ratio Cr / (Ni+Cr+Fe) of 0.15 or more and 0.30 or less, the atomic ratio Ni / (Ni+Cr+Fe) of 0.30 or more and 0.70 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of 0.10 or more and 0.50 or less, and (c) is a diagram showing ranges of the atomic ratio Cr / (Ni+Cr+Fe) of 0.15 or more and 0.25 or less, the atomic ratio Ni / (Ni+Cr+Fe) of 0.30 or more and 0.65 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of 0.15 or more and 0.50 or less. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] 1 is a diagram showing a schematic structure of a photocatalyst 10 of the present invention. The photocatalyst 10 of the present invention has a structure in which a NiCrFe oxide 12 is supported on a titanium oxide 11, and does not contain rare metals such as ruthenium oxide or iridium oxide. The atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide 12 is 0.15 or more and 0.40 or less, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide 12 is 0.15 or more and 0.75 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide 12 is 0.10 or more and 0.65 or less.
[0011] The features of the present invention will be described in detail below with reference to embodiments of the present invention.
[0012] <First embodiment> In the photocatalyst 10 of the first embodiment, the titanium oxide 11 contains TiO2 as a main component. "Containing TiO2 as a main component" means that 50% or more of the component in terms of molar ratio is TiO2, and may contain components other than TiO2.
[0013] The NiCrFe oxide 12 serving as the promoter is an oxide containing Ni, Cr and Fe as main components.
[0014] Example 1 The raw powder of TiO2 was immersed in an aqueous solution of Ni nitrate, Cr nitrate, and Fe nitrate in the desired composition ratio and amount, and then heated on a hot plate set at 150°C to obtain a dried product. The dried product was then heat-treated in air at 500°C to volatilize the nitric acid and crystallize the NiCrFe oxide, producing a photocatalyst powder in which the co-catalyst NiCrFe oxide is supported on the titanium oxide TiO2.
[0015] The activity of the prepared photocatalyst was evaluated by the following method.
[0016] 2 is a schematic diagram showing the configuration of an apparatus used to evaluate the activity of a photocatalyst. A slurry obtained by mixing 0.3 g of the prepared photocatalyst powder with 1 g of pure water was placed in a petri dish 21. The petri dish 21 was then placed in a sealed container 22, which was then sealed with a lid 23 made of quartz glass. The lid 23 made of quartz glass is transparent to ultraviolet light.
[0017] Next, argon gas was sent out from pack 24 filled with 1 liter of argon gas using blower pump 25, and argon gas was circulated at a rate of 1 cc / min. That is, the argon gas in pack 24 was circulated so as to pass through sealed container 22 and return to pack 24. The argon gas was introduced into sealed container 22 in order to prevent hydrogen generated by decomposition of water from reacting with oxygen, etc.
[0018] Next, the slurry in the petri dish 21 was irradiated with ultraviolet light through the quartz glass cover 23. By irradiating the slurry with ultraviolet light, water was decomposed and hydrogen was generated. This state was continued for one hour, and the hydrogen content in the mixed gas after one hour was determined by gas chromatography. The hydrogen content in the mixed gas means the hydrogen content in the mixed gas of argon and hydrogen.
[0019] A 200 W mercury xenon lamp was used as the ultraviolet irradiation source. This mercury xenon lamp can irradiate ultraviolet rays uniformly over an area of 4 cm square, so it is possible to irradiate ultraviolet rays over the entire circular petri dish 21 with a diameter of 3 cm in plan view.
[0020] Here, we investigated the amount of hydrogen generated when changing the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in NiCrFe oxide, which is the co-catalyst for the photocatalyst, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in NiCrFe oxide. The relationship between the atomic ratios Cr / (Ni+Cr+Fe) and Fe / (Ni+Cr+Fe) and the proportion of hydrogen in the mixed gas is shown in Figure 3.
[0021] In addition, Fig. 3 does not show the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide, but if the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe are known, it can be calculated. For example, in Fig. 3, if the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe is 0.20 and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.30, the atomic ratio of the Ni content to the total content of Ni, Cr, and Fe is 0.50 (=1-0.20-0.30).
[0022] As shown in Fig. 3, when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.40, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.65, the proportion of hydrogen in the mixed gas is 0.016% or more. In Fig. 3, the ranges where the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.40, the atomic ratio Ni / (Ni+Cr+Fe) is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.65 are surrounded by thick lines.
[0023] That is, the photocatalyst in the first embodiment in which NiCrFe oxide is supported on titanium oxide TiO2, the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr and Fe contained in the NiCrFe oxide is 0.15 or more and 0.40 or less, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr and Fe is 0.15 or more and 0.75 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr and Fe is 0.10 or more and 0.65 or less, has high catalytic activity and generates a large amount of hydrogen by decomposition of water.
[0024] 3 and 4(a), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.35, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.55, the proportion of hydrogen in the mixed gas is 0.019% or more, which is even higher. Therefore, in the photocatalyst in the first embodiment, it is preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.35, the atomic ratio Ni / (Ni+Cr+Fe) is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.55.
[0025] 3 and 4(b), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.30, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.30 to 0.70, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.50, the proportion of hydrogen in the mixed gas is 0.021% or more, which is even higher. Therefore, in the photocatalyst in the first embodiment, it is more preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.30, the atomic ratio Ni / (Ni+Cr+Fe) is 0.30 to 0.70, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.50.
[0026] 3 and 4(c), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.25, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.30 to 0.65, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.15 to 0.50, the proportion of hydrogen in the mixed gas is 0.025% or more, which is even higher. Therefore, in the photocatalyst in the first embodiment, it is more preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.25, the atomic ratio Ni / (Ni+Cr+Fe) is 0.30 to 0.65, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.15 to 0.50.
[0027] <Second embodiment> The photocatalyst 10 in the second embodiment also has a structure in which the titanium oxide 11 supports the NiCrFe oxide 12 as a promoter. In this embodiment, the titanium oxide 11 contains BaTi4O9 as a main component. "Containing BaTi4O9 as a main component" means that 50% or more of the component in terms of molar ratio is BaTi4O9, and may contain components other than BaTi4O9. The titanium oxide 11 may also contain barium titanate with a composition ratio different from that of BaTi4O9.
[0028] Example 2 The raw powders of BaCO3 and TiO2 were mixed in a molar ratio of BaCO3:TiO2 = 1:4, placed in a pot mill together with water and zirconia beads, mixed for 5 hours, dried, and then heat-treated at 1100°C in air to obtain BaTi4O9 powder.
[0029] Next, the BaTi4O9 powder was immersed in an aqueous solution of Ni nitrate, Cr nitrate, and Fe nitrate in the desired composition ratio and amount, and then heated on a hot plate set at 150°C to obtain a dried product. The dried product was then heat-treated in air at 500°C to volatilize the nitric acid and crystallize the NiCrFe oxide, producing a photocatalyst powder in which the titanium oxide BaTi4O9 supports the co-catalyst NiCrFe oxide.
[0030] The activity of the photocatalyst prepared in Example 2 was evaluated by the same method as that used to evaluate the activity of the photocatalyst in Example 1. The relationship between the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide of the photocatalyst in Example 2, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide of the photocatalyst in Example 2, and the proportion of hydrogen in the mixed gas is shown in FIG.
[0031] As shown in Fig. 5, when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.40, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.65, the proportion of hydrogen in the mixed gas is 0.054% or more. In Fig. 5, the ranges where the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.40, the atomic ratio Ni / (Ni+Cr+Fe) is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.65 are surrounded by thick lines.
[0032] That is, the photocatalyst in the second embodiment in which NiCrFe oxide is supported on BaTi4O9 which is a titanium oxide, and the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr and Fe contained in the NiCrFe oxide is 0.15 or more and 0.40 or less, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr and Fe is 0.15 or more and 0.75 or less, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr and Fe is 0.10 or more and 0.65 or less, has high catalytic activity and generates a large amount of hydrogen by decomposition of water.
[0033] 5 and 6(a), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.35, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.55, the proportion of hydrogen in the mixed gas is 0.064% or more, which is even higher. Therefore, in the photocatalyst in the second embodiment, it is preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.35, the atomic ratio Ni / (Ni+Cr+Fe) is 0.15 to 0.75, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.55.
[0034] 5 and 6(b), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.30, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.30 to 0.70, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.10 to 0.50, the proportion of hydrogen in the mixed gas is 0.072% or more, which is even higher. Therefore, in the photocatalyst in the second embodiment, it is more preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.30, the atomic ratio Ni / (Ni+Cr+Fe) is 0.30 to 0.70, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.10 to 0.50.
[0035] 5 and 6(c), when the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 to 0.25, the atomic ratio Ni / (Ni+Cr+Fe) of the Ni content to the total content of Ni, Cr, and Fe is 0.30 to 0.65, and the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe is 0.15 to 0.50, the proportion of hydrogen in the mixed gas is 0.082% or more, which is even higher. Therefore, in the photocatalyst in the second embodiment, it is more preferable that the atomic ratio Cr / (Ni+Cr+Fe) is 0.15 to 0.25, the atomic ratio Ni / (Ni+Cr+Fe) is 0.30 to 0.65, and the atomic ratio Fe / (Ni+Cr+Fe) is 0.15 to 0.50.
[0036] When the photocatalyst 10 in the first embodiment and the photocatalyst 10 in the second embodiment are compared under the same conditions, the photocatalyst 10 in the second embodiment generates a larger amount of hydrogen by decomposition of water than the photocatalyst 10 in the first embodiment. Therefore, it is preferable that the titanium oxide 11 contains BaTi4O9 as a main component. The same conditions are conditions in which the atomic ratios Cr / (Ni+Cr+Fe), Ni / (Ni+Cr+Fe), and Fe / (Ni+Cr+Fe) are the same in the photocatalyst 10 in the first embodiment and the photocatalyst 10 in the second embodiment.
[0037] The present invention is not limited to the above embodiment, and various applications and modifications can be made within the scope of the present invention. For example, the titanium oxide 11 is exemplified by those containing TiO2 as a main component and those containing BaTi4O9 as a main component, but the titanium oxide 11 is not limited thereto. For example, the titanium oxide 11 may be one containing barium titanate with a composition ratio different from BaTi4O9 as a main component, or one containing strontium titanate as a main component. [Explanation of symbols]
[0038] 10 Photocatalyst 11 Titanium oxide 12 CuCr oxide 21 Petri dish 22 Sealed container 23 Lid 24 Pack 25 Blower Pump
Claims
1. The titanium oxide supports NiCrFe oxide, The titanium oxide contains BaTi 4 O 9 as a main component, the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.40 or less; the atomic ratio Ni / (Ni+Cr+Fe) of the content of Ni to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.75 or less; A photocatalyst characterized in that the atomic ratio Fe / (Ni+Cr+Fe) of the content of Fe to the total content of Ni, Cr and Fe contained in the NiCrFe oxide is 0.10 or more and 0.65 or less.
2. the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.35 or less; the atomic ratio Ni / (Ni+Cr+Fe) of the content of Ni to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.75 or less; 2. The photocatalyst according to claim 1, wherein the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.10 or more and 0.55 or less.
3. the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.30 or less; the atomic ratio Ni / (Ni+Cr+Fe) of the content of Ni to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.30 or more and 0.70 or less; 3. The photocatalyst according to claim 1, wherein the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.10 or more and 0.50 or less.
4. the atomic ratio Cr / (Ni+Cr+Fe) of the Cr content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.25 or less; the atomic ratio Ni / (Ni+Cr+Fe) of the content of Ni to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.30 or more and 0.65 or less; The photocatalyst according to any one of claims 1 to 3, characterized in that the atomic ratio Fe / (Ni+Cr+Fe) of the Fe content to the total content of Ni, Cr, and Fe contained in the NiCrFe oxide is 0.15 or more and 0.50 or less.
Citation Information
Patent Citations
Photocatalyst and production of photocatalyst
JP1995088370A
Photocatalyst
JP2001246264A
Method for photocatalytic water purification
JP2012530599A
Photocatalyst for water decomposition
JP2014000502A
Visible light-responsive catalyst body and water decomposition method utilizing the same
JP2015112501A