Phase shift mask blanks, their manufacturing method and phase shift mask

The silicon nitride-based phase shift mask blank addresses the challenges of KrF excimer lasers by optimizing film composition and thickness for improved wash and light resistance, enhancing pattern formation and efficiency.

JP7586216B2Active Publication Date: 2024-11-19SHIN ETSU CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023053683
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-14
Filing Date
2023-03-29
Publication Date
2024-11-19
Estimated Expiration
2040-02-17

AI Technical Summary

Technical Problem

Existing phase shift masks using molybdenum and silicon films for KrF excimer lasers face challenges in achieving high wash resistance, light resistance, and fine pattern formation due to film thickness and composition issues, leading to haze and pattern collapse.

Method used

A phase shift mask blank with a silicon nitride film composition optimized for KrF excimer lasers, featuring a refractive index of 2.55 to 2.7, extinction coefficient of 0.4 to 0.7, and a phase difference of 170 to 190°, with a transmittance of 4 to 8% and thickness of 85 nm or less, formed through reactive sputtering with controlled nitrogen gas flow rates.

Benefits of technology

The solution provides a thin phase shift film that enhances pattern formation and reduces three-dimensional effects, ensuring high efficiency and improved resistance to wash and light exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586216000001
    Figure 0007586216000001
  • Figure 0007586216000002
    Figure 0007586216000002
  • Figure 0007586216000003
    Figure 0007586216000003
Patent Text Reader

Abstract

A phase shift mask blank having a phase shift film formed on a transparent substrate from a material containing silicon and nitrogen but no transition metals, wherein the exposure light is KrF excimer laser light, and the phase shift film is composed of multiple layers including a surface oxide layer which is the outermost layer on the side separated from the transparent substrate, and a layer having a refractive index n of 2.5 or more and an extinction coefficient k of 0.4 to 1 with respect to the exposure light, or a layer having a nitrogen content (atomic %) of 0.43 to 0.53, N / (Si+N), which is the nitrogen content (atomic %) relative to the total content (atomic %) of silicon and nitrogen, and wherein the phase difference of the phase shift film with respect to the exposure light is 170 to 190°. [Effects] According to the present invention, it is possible to provide phase shift mask blanks and phase shift masks equipped with thin phase shift films that ensure the phase difference and transmittance required for a phase shift film when using a KrF excimer laser as exposure light, and that are advantageous in processing and exposing photomask patterns.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a phase shift mask blank used in the manufacture of semiconductor integrated circuits and the like, a method for manufacturing the same, and a phase shift mask. [Background technology]

[0002] In photolithography technology used in semiconductor technology, the phase shift method is used as one of the resolution improvement techniques. The phase shift method is, for example, a method using a photomask with a phase shift film formed on a substrate, and is a method of improving contrast by utilizing light interference by forming a phase shift film pattern on a substrate transparent to the exposure light, which is a photomask substrate, in which the phase difference between the light transmitted through the phase shift film and the light transmitted through the phase shift film is approximately 180° with respect to the exposure light transmitted through the portion where the phase shift film is not formed, that is, the exposure light transmitted through air of the same length as the thickness of the phase shift film. One photomask that applies this method is a halftone phase shift mask. The halftone phase shift mask is a mask pattern formed on a substrate transparent to the exposure light, such as quartz, with a phase difference of approximately 180° with the light transmitted through the portion where the phase shift film is not formed, and with a transmittance that does not substantially contribute to exposure. Until now, a film containing molybdenum and silicon has been mainly used as the phase shift film of a phase shift mask (JP Patent Publication No. 7-140635 (Patent Document 1)). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 7-140635 [Patent Document 2] JP 2007-33469 A [Patent Document 3] JP 2007-233179 A [Patent Document 4] JP 2007-241065 A Summary of the Invention [Problem to be solved by the invention]

[0004] In phase shift masks using films containing molybdenum and silicon, when the exposure light is a KrF excimer laser (wavelength 248 nm), a phase shift film with a transmittance of 6%, a phase difference of about 180°, and a film thickness of about 100 nm is generally used. In recent years, phase shift films using an ArF excimer laser (wavelength 193 nm) as the exposure light have come to use silicon nitride phase shift films in order to make the film thinner and improve its cleaning resistance and light resistance. Even when the exposure light is a KrF excimer laser, there is a demand for a phase shift film that is highly cleaning-resistant and light-resistant and does not easily generate haze, although not as much as when the exposure light is an ArF excimer laser.

[0005] When using silicon nitride with KrF excimer laser as exposure light, the composition ratio of nitrogen and silicon must be adjusted to match the wavelength of the KrF excimer laser in order to create a film that meets the required phase difference and transmittance. In addition, when considering the pattern collapse during processing into a phase shift mask and the cross-sectional shape of the pattern, a film that is as thin and as uniform in composition as possible is desired. When using ArF excimer laser as exposure light, the more nitrogen silicon nitride contains, the higher the refractive index n and the smaller the extinction coefficient k, so a phase shift film with as high a nitrogen content as possible has been proposed.

[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a phase shift mask blank having a thin phase shift film which is advantageous in pattern formation and reduction of three-dimensional effect while ensuring the necessary phase difference and transmittance as a phase shift film capable of handling fine patterns even when the exposure light is a KrF excimer laser with a wavelength of 248 nm, a method for manufacturing the same, and a phase shift mask. [Means for solving the problem]

[0007] As a result of extensive investigations to solve the above problems, the present inventors have found that, unlike ArF excimer lasers, when the exposure light is a KrF excimer laser, silicon nitride has the highest refractive index n when its composition ratio (atomic %) is around Si:N=53:47, and thinning of the film cannot be achieved simply by increasing the nitrogen content. For silicon nitride when the exposure light is a KrF excimer laser, phase shift mask blanks for KrF excimer laser exposure with a wavelength of 248 nm can have a phase shift film having a composition containing silicon and nitrogen but not containing a transition metal, and the refractive index n and extinction coefficient k are within predetermined ranges, or the ratio of silicon to nitrogen is within predetermined ranges, thereby resulting in phase shift mask blanks and phase shift masks having a thinner phase shift film with a phase difference (phase shift amount) of 170 to 190° relative to the exposure light, and in particular a transmittance of 4 to 8% and a film thickness of 85 nm or less. This has led to the completion of the present invention.

[0008] Accordingly, the present invention provides the following phase shift mask blanks, a method for producing a phase shift mask blank, and a phase shift mask. 1. A photomask blank having a phase shift film formed on a transparent substrate from a material containing silicon and nitrogen and not containing a transition metal, The exposure light is KrF excimer laser light, The phase shift film is (A) a surface oxide layer which is the outermost layer on the side separated from the transparent substrate; (B) a layer having a refractive index n of 2.55 or more and an extinction coefficient k of 0.4 to 0.7 with respect to the exposure light; It is composed of multiple layers consisting of A phase shift mask blank, in which the phase shift film has a phase difference of 170 to 190°, a transmittance of 4 to 8% and a film thickness of 85 nm or less with respect to exposure light. 2. A phase shift mask blank in which the extinction coefficient k is 0.4 to 0.6. 3. A phase shift mask blank, wherein the transmittance of the phase shift film is 4.5 to 8%. 4. A phase shift mask blank in which the nitrogen content (atomic %) of layer (B) relative to the total content (atomic %) of silicon and nitrogen, N / (Si+N), is 0.43 or more and 0.53 or less. 5. A phase shift mask blank, wherein the layer (B) is formed from a material containing silicon and nitrogen. 6. A phase shift mask blank, wherein the phase shift film has a thickness of 79 nm or less. 7. A phase shift mask blank, wherein the oxygen content of the surface oxide layer is 20 atomic % or more. 8. A phase shift mask blank, wherein the phase shift film has a thickness of 50 nm or more. 9. A phase shift mask blank, wherein the thickness of the surface oxide layer is 1 nm or more and 10 nm or less. 10. A method for producing the above phase shift mask blank, comprising the steps of: forming the phase shift film by reactive sputtering using a silicon-containing target and nitrogen gas; A method for manufacturing a phase shift mask blank, characterized in that the nitrogen gas flow rate set in this process is constant or is changed continuously or stepwise within a range of -20% to +20% of the flow rate at which the refractive index n of the phase shift film to the exposure light is highest, obtained when the nitrogen gas flow rate is changed from a low flow rate to a high flow rate. 11 A phase shift mask formed using the above phase shift mask blank. Effect of the Invention

[0009] According to the present invention, it is possible to provide a phase shift mask blank and a phase shift mask having a thin phase shift film that ensures the necessary phase difference and transmittance as a phase shift film when KrF excimer laser is used as exposure light, and is advantageous in processing and exposing a photomask pattern. [Brief description of the drawings]

[0010] [Figure 1]1 is a cross-sectional view showing an example of a phase shift mask blank and a phase shift mask of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of a phase shift mask blank of the present invention. [Diagram 3] 1 is a graph plotting the refractive index n versus the nitrogen gas flow rate in Example 1. [Figure 4] 1 is a graph plotting the extinction coefficient k versus the nitrogen gas flow rate in Example 1. [Diagram 5] 1 is a graph plotting the refractive index n versus N / (Si+N) in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will now be described in further detail. The phase shift mask blank of the present invention has a phase shift film formed on a transparent substrate such as a quartz substrate. The phase shift mask of the present invention has a mask pattern (photomask pattern) of the phase shift film formed on a transparent substrate such as a quartz substrate.

[0012] In the present invention, the transparent substrate is preferably a transparent substrate called a 6025 substrate, which is defined in the SEMI standard as being 6 inches square and 0.25 inches thick, and when the SI system of units is used, this is usually expressed as a transparent substrate having a size of 152 mm square and a thickness of 6.35 mm.

[0013] Fig. 1(A) is a cross-sectional view showing an example of a phase shift mask blank of the present invention, and this phase shift mask blank 100 comprises a transparent substrate 10 and a phase shift film 1 formed on the transparent substrate 10. Also, Fig. 1(B) is a cross-sectional view showing an example of a phase shift mask of the present invention, and this phase shift mask 101 comprises a transparent substrate 10 and a phase shift film pattern 11 formed on the transparent substrate 10. A phase shift mask can be obtained by using a phase shift mask blank and forming a pattern of the phase shift film.

[0014] The phase shift film of the present invention is a film that, at a predetermined thickness, gives a predetermined phase difference (phase shift amount) and a predetermined transmittance to the exposure light of a KrF excimer laser (wavelength 248 nm). In the present invention, the phase shift film is formed of a material that contains silicon and nitrogen and does not contain transition metals. In order to improve the cleaning resistance of the film, it is effective to include oxygen in the phase shift film, so the material that contains silicon and nitrogen and does not contain transition metals may contain oxygen in addition to silicon and nitrogen, but the inclusion of oxygen reduces the refractive index n of the film, so the film tends to be thick. Therefore, the material that contains silicon and nitrogen and does not contain transition metals is preferably a material made of silicon and nitrogen (a material that is substantially composed of these two elements except for unavoidable impurities).

[0015] The phase shift film may be made of a single layer or multiple layers as long as it satisfies the phase difference and transmittance required for a phase shift film. In either case, each layer constituting the single layer or multiple layers may be a single composition layer (a layer whose composition does not change in the thickness direction) or a composition gradient layer (a layer whose composition changes in the thickness direction).

[0016] In the phase shift film of the present invention, the refractive index n of each layer constituting the single layer or multiple layers to the exposure light is preferably 2.5 or more, particularly 2.55 or more. The upper limit of the refractive index n is usually 2.7 or less. In addition, in the phase shift film of the present invention, the refractive index k of each layer constituting the single layer or multiple layers to the exposure light is preferably 0.4 or more, particularly 0.5 or more, and 1 or less, particularly 0.8 or less.

[0017] In the phase shift film of the present invention, when the phase shift film is composed of a single layer, at least a part of the single layer, particularly the entire single layer, and when the phase shift film is composed of multiple layers, at least a part of the layers constituting the multiple layers, particularly each layer (all layers), preferably have a nitrogen content (atomic %) to the total content (atomic %) of silicon and nitrogen, N / (Si+N), of 0.43 or more, particularly 0.45 or more, and 0.53 or less, particularly 0.5 or less. In addition, when the phase shift film is made into a composition gradient layer, it is preferable that the composition gradient range is within the above range. Note that when the single layer or each layer of the multiple layers contains oxygen, the oxygen content is preferably 30 atomic % or less, particularly 10 atomic % or less, especially 5 atomic % or less.

[0018] The phase difference of the phase shift film of the present invention with respect to the exposure light may be such that the exposure light passing through the boundary between the portion where the phase shift film is present (phase shift portion) and the portion where the phase shift film is not present interferes with each other to increase the contrast, and the phase difference may be 170° or more and 190° or less. On the other hand, the transmittance of the phase shift film of the present invention with respect to the exposure light may be 4% or more and 8% or less. In the case of the phase shift film of the present invention, the phase difference and transmittance with respect to the KrF excimer laser (wavelength 248 nm) may be within the above ranges.

[0019] The total thickness of the phase shift film of the present invention is set to 85 nm or less, preferably 80 nm or less, since the thinner the thickness, the easier it is to form a finer pattern. On the other hand, the lower limit of the thickness of the phase shift film is set within a range in which necessary optical characteristics can be obtained for the exposure light, and although there is no particular limit, it is generally 50 nm or more.

[0020] The phase shift film of the present invention can be formed by applying a known film forming method, but is preferably formed by a sputtering method that can easily obtain a film with excellent homogeneity. Either DC sputtering or RF sputtering can be used, but magnetron sputtering is more preferable. The target and sputtering gas are appropriately selected depending on the layer structure and composition. As the target, a target containing silicon, such as a silicon target, a silicon nitride target, or a target containing both silicon and silicon nitride, may be used. The nitrogen content can be adjusted by using nitrogen gas as a reactive gas in the sputtering gas and performing reactive sputtering by appropriately adjusting the amount of introduction. Furthermore, helium gas, neon gas, argon gas, etc. can also be used as a rare gas in the sputtering gas.

[0021] When the phase shift film of the present invention is formed by reactive sputtering using a silicon-containing target and nitrogen gas, the nitrogen gas flow rate is set within the range of -20% to +20% of the flow rate at which the refractive index n of the phase shift film to the exposure light is the highest, and in particular, it is preferable to form the phase shift film at the flow rate at which the refractive index n of the phase shift film to the exposure light is the highest. In this way, a phase shift film having a phase difference of 170 to 190° and a transmittance of 4 to 8% can be formed with a thinner film thickness. The flow rate at which the refractive index n of the phase shift film to the exposure light is the highest may be determined by confirming in advance the change in the refractive index n of silicon nitride obtained when the flow rate of nitrogen gas is changed from a low flow rate to a high flow rate. At this time, the sputtering conditions other than the flow rate of nitrogen gas (applied power to the target, flow rates of other sputtering gases, sputtering pressure, etc.) are fixed (constant). The flow rate set when the film is actually formed can be constant or can be changed continuously or stepwise.

[0022] When the phase shift film is made of multiple layers, a surface oxide layer can be provided as the outermost layer on the front side (the side separated from the transparent substrate) in order to suppress changes in the film quality of the phase shift film. The oxygen content of this surface oxide layer may be 20 atomic % or more, and may further be 50 atomic % or more. Specific methods for forming the surface oxide layer include oxidation by atmospheric oxidation (natural oxidation), as well as forced oxidation treatment methods, such as a method of treating a film formed by sputtering with ozone gas or ozone water, and a method of heating to 300°C or more in an oxygen-containing atmosphere such as an oxygen gas atmosphere by oven heating, lamp annealing, laser heating, etc. The thickness of this surface oxide layer is preferably 10 nm or less, particularly 5 nm or less, and especially 3 nm or less, and usually, an effect as an oxide layer is obtained with a thickness of 1 nm or more. The surface oxide layer can be formed by increasing the amount of oxygen in the sputtering process, but in order to obtain a layer with fewer defects, it is preferable to form it by the above-mentioned atmospheric oxidation or oxidation treatment.

[0023] A second layer consisting of a single layer or multiple layers can be provided on the phase shift film of the phase shift mask blank of the present invention. The second layer is usually provided adjacent to the phase shift film. Specific examples of this second layer include a light-shielding film, a combination of a light-shielding film and an anti-reflection film, and a processing auxiliary film that functions as a hard mask in the pattern formation of the phase shift film. In addition, when a third layer is provided as described below, this second layer can also be used as a processing auxiliary film (etching stopper film) that functions as an etching stopper in the pattern formation of the third layer. A material containing chromium is suitable as the material of the second layer.

[0024] A specific example of such a phase shift mask blank is shown in Fig. 2(A). Fig. 2(A) is a cross-sectional view showing an example of a phase shift mask blank of the present invention. This phase shift mask blank 100 includes a transparent substrate 10, a phase shift film 1 formed on the transparent substrate 10, and a second layer 2 formed on the phase shift film 1.

[0025] In the phase shift mask blank of the present invention, an etching mask film that functions as a hard mask for forming a pattern on the light-shielding film or the phase shift film can be provided as a second layer on the phase shift film. In addition, a combination of a light-shielding film and an anti-reflection film can be provided as the second layer. By providing a second layer including a light-shielding film, a region that completely blocks exposure light can be provided on the phase shift mask. The light-shielding film and the anti-reflection film can also be used as a processing auxiliary film in etching. There are many reports on the film configuration and material of the light-shielding film and the anti-reflection film (for example, JP-A-2007-33469 (Patent Document 2), JP-A-2007-233179 (Patent Document 3), etc.), but a preferred film configuration of the combination of the light-shielding film and the anti-reflection film includes, for example, a light-shielding film made of a material containing chromium, and an anti-reflection film made of a material containing chromium that reduces reflection from the light-shielding film. Both the light-shielding film and the anti-reflection film may be configured as a single layer or multiple layers. Examples of chromium-containing materials for light-shielding films and anti-reflection films include chromium itself, and chromium compounds such as chromium oxide (CrO), chromium nitride (CrN), chromium carbide (CrC), chromium oxide nitride (CrON), chromium oxide carbide (CrOC), chromium nitride carbide (CrNC), and chromium oxide nitride carbide (CrONC). Note that the chemical formulas representing chromium-containing materials indicate the constituent elements, and do not mean the composition ratio of the constituent elements (the same applies to the following materials containing chromium).

[0026] When the second layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, the content of chromium in the chromium compound of the light-shielding film is preferably 40 atomic % or more, particularly 60 atomic % or more, and less than 100 atomic %, particularly 99 atomic % or less, and especially 90 atomic % or less. The content of oxygen is preferably 60 atomic % or less, particularly 40 atomic % or less, and more preferably 1 atomic % or more. The content of nitrogen is preferably 50 atomic % or less, particularly 40 atomic % or less, and more preferably 1 atomic % or more. The content of carbon is preferably 20 atomic % or less, particularly 10 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, and especially 100 atomic %.

[0027] In addition, when the second layer is a combination of a light-shielding film and an anti-reflection film, the anti-reflection film is preferably a chromium compound, and the chromium content in the chromium compound is preferably 30 atomic % or more, particularly 35 atomic % or more, and 70 atomic % or less, particularly 50 atomic % or less. The oxygen content is preferably 60 atomic % or less, more preferably 1 atomic % or more, particularly 20 atomic % or more. The nitrogen content is preferably 50 atomic % or less, particularly 30 atomic % or less, more preferably 1 atomic % or more, particularly 3 atomic % or more. The carbon content is preferably 20 atomic % or less, particularly 5 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, particularly 100 atomic %.

[0028] When the second layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, the thickness of the second layer is usually 20 to 100 nm, preferably 40 to 70 nm. The total optical density of the phase shift film and the second layer to the exposure light is preferably 2.0 or more, particularly 2.5 or more, and more particularly 3.0 or more.

[0029] A third layer consisting of a single layer or multiple layers can be provided on the second layer of the phase shift mask blank of the present invention. The third layer is usually provided adjacent to the second layer. Specific examples of this third layer include a processing auxiliary film that functions as a hard mask in the pattern formation of the second layer, a light-shielding film, and a combination of a light-shielding film and an anti-reflection film. As the material of the third layer, a material containing silicon is preferable, and in particular, a material not containing chromium is preferable.

[0030] A specific example of such a phase shift mask blank is shown in Fig. 2(B). Fig. 2(B) is a cross-sectional view showing an example of a phase shift mask blank of the present invention, and this phase shift mask blank 100 includes a transparent substrate 10, a phase shift film 1 formed on the transparent substrate 10, a second layer 2 formed on the phase shift film 1, and a third layer 3 formed on the second layer 2.

[0031] When the second layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, a processing auxiliary film (etching mask film) that functions as a hard mask in the pattern formation of the second layer can be provided as the third layer. When a fourth layer, which will be described later, is provided, this third layer can also be used as a processing auxiliary film (etching stopper film) that functions as an etching stopper in the pattern formation of the fourth layer. This processing auxiliary film is made of a material that has different etching characteristics from the second layer, for example, a material that is resistant to chlorine-based dry etching that is applied to etching materials containing chromium, specifically, SF 6 or CF 4 It is preferable to use a material containing silicon that can be etched with a fluorine-based gas such as fluorine-based gas such as fluorine-based gas, etc. Specific examples of the material containing silicon include silicon alone, a material containing silicon and either or both of nitrogen and oxygen, a material containing silicon and a transition metal, and a silicon compound such as a material containing silicon, either or both of nitrogen and oxygen, and a transition metal, and examples of the transition metal include molybdenum, tantalum, and zirconium.

[0032] When the third layer is a processing auxiliary film, the processing auxiliary film is preferably a silicon compound, and the silicon content in the silicon compound is preferably 20 atomic % or more, particularly 33 atomic % or more, and 95 atomic % or less, particularly 80 atomic % or less. The nitrogen content is preferably 50 atomic % or less, particularly 30 atomic % or less, and more preferably 1 atomic % or more. The oxygen content is preferably 70 atomic % or less, particularly 66 atomic % or less, and when the etching rate needs to be adjusted, it is more preferably 1 atomic % or more, and even more preferably 20 atomic % or more. A transition metal may or may not be contained, but when a transition metal is contained, its content is preferably 35 atomic % or less, particularly 20 atomic % or less. In this case, the total content of silicon, oxygen, nitrogen and transition metal is preferably 95 atomic % or more, particularly 99 atomic % or more, and especially 100 atomic %.

[0033] When the second layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film and the third layer is a processing auxiliary film, the thickness of the second layer is usually 20 to 100 nm, preferably 40 to 70 nm, and the thickness of the third layer is usually 1 to 30 nm, preferably 2 to 15 nm. In addition, it is preferable that the total optical density of the phase shift film and the second layer with respect to the exposure light is 2.0 or more, particularly 2.5 or more, and especially 3.0 or more.

[0034] In addition, when the second layer is a processing auxiliary film, a light-shielding film can be provided as the third layer. In addition, a combination of a light-shielding film and an anti-reflection film can be provided as the third layer. In this case, the second layer is a processing auxiliary film (etching mask film) that functions as a hard mask in the pattern formation of the phase shift film, and can also be used as a processing auxiliary film (etching stopper film) that functions as an etching stopper in the pattern formation of the third layer. An example of the processing auxiliary film is a film made of a material containing chromium as shown in JP-A-2007-241065 (Patent Document 4). The processing auxiliary film may be made of a single layer or multiple layers. Examples of the chromium-containing material of the processing auxiliary film include chromium alone, chromium oxide (CrO), chromium nitride (CrN), chromium carbide (CrC), chromium oxide nitride (CrON), chromium oxide carbide (CrOC), chromium nitride carbide (CrNC), chromium oxide nitride carbide (CrONC), and other chromium compounds.

[0035] When the second layer is a processing aid film, the chromium content in the chromium compound of the second layer is preferably 40 atomic % or more, particularly 50 atomic % or more, and 100 atomic % or less, particularly 99 atomic % or less, and especially 90 atomic % or less. The oxygen content is preferably 60 atomic % or less, particularly 55 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. The nitrogen content is preferably 50 atomic % or less, particularly 40 atomic % or less, and more preferably 1 atomic % or more. The carbon content is preferably 20 atomic % or less, particularly 10 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, and especially 100 atomic %.

[0036] On the other hand, the light-shielding film and anti-reflection film of the third layer are made of a material having etching characteristics different from those of the second layer, for example, a material having resistance to chlorine-based dry etching applied to etching of materials containing chromium, specifically, SF 6 or CF 4It is preferable to use a material containing silicon that can be etched with a fluorine-based gas such as fluorine-based gas such as fluorine-based gas, etc. Specific examples of the material containing silicon include silicon alone, a material containing silicon and either or both of nitrogen and oxygen, a material containing silicon and a transition metal, and a silicon compound such as a material containing silicon, either or both of nitrogen and oxygen, and a transition metal, and examples of the transition metal include molybdenum, tantalum, and zirconium.

[0037] When the third layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, the light-shielding film and the anti-reflection film are preferably silicon compounds, and the content of silicon in the silicon compound is preferably 10 atomic % or more, particularly 30 atomic % or more, and less than 100 atomic %, particularly 95 atomic % or less. The content of nitrogen is preferably 50 atomic % or less, particularly 40 atomic % or less, and particularly 20 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. The content of oxygen is preferably 60 atomic % or less, particularly 30 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. The content of transition metal is preferably 35 atomic % or less, particularly 20 atomic % or less, and more preferably 1 atomic % or more. In this case, the total content of silicon, oxygen, nitrogen and transition metal is preferably 95 atomic % or more, particularly 99 atomic % or more, and particularly 100 atomic %.

[0038] When the second layer is a processing auxiliary film and the third layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, the thickness of the second layer is usually 1 to 20 nm, preferably 2 to 10 nm, and the thickness of the third layer is usually 20 to 100 nm, preferably 30 to 70 nm. In addition, it is preferable that the total optical density of the phase shift film, the second layer and the third layer with respect to the exposure light is 2.0 or more, particularly 2.5 or more, and especially 3.0 or more.

[0039] A fourth layer consisting of a single layer or multiple layers can be provided on the third layer of the phase shift mask blank of the present invention. The fourth layer is usually provided adjacent to the third layer. Specific examples of this fourth layer include a processing auxiliary film that functions as a hard mask in patterning the third layer. A material containing chromium is suitable as the material of the fourth layer.

[0040] A specific example of such a phase shift mask blank is shown in Fig. 2(C). Fig. 2(C) is a cross-sectional view showing an example of a phase shift mask blank of the present invention, and this phase shift mask blank 100 includes a transparent substrate 10, a phase shift film 1 formed on the transparent substrate 10, a second layer 2 formed on the phase shift film 1, a third layer 3 formed on the second layer 2, and a fourth layer 4 formed on the third layer 3.

[0041] When the third layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, a processing auxiliary film (etching mask film) that functions as a hard mask in the pattern formation of the third layer can be provided as the fourth layer. This processing auxiliary film is preferably made of a material having different etching characteristics from the third layer, for example, a material having resistance to fluorine-based dry etching applied to etching of materials containing silicon, specifically, a material containing chromium that can be etched with a chlorine-based gas containing oxygen. Specific examples of materials containing chromium include chromium alone, chromium oxide (CrO), chromium nitride (CrN), chromium carbide (CrC), chromium oxide nitride (CrON), chromium oxide carbide (CrOC), chromium nitride carbide (CrNC), chromium oxide nitride carbide (CrONC), and other chromium compounds.

[0042] When the fourth layer is a processing auxiliary film, the chromium content in the fourth layer is preferably 40 atomic % or more, particularly 50 atomic % or more, and 100 atomic % or less, particularly 99 atomic % or less, particularly 90 atomic % or less. The oxygen content is preferably 60 atomic % or less, particularly 40 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. The nitrogen content is preferably 50 atomic % or less, particularly 40 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. The carbon content is preferably 20 atomic % or less, particularly 10 atomic % or less, and more preferably 1 atomic % or more when the etching rate needs to be adjusted. In this case, the total content of chromium, oxygen, nitrogen and carbon is preferably 95 atomic % or more, particularly 99 atomic % or more, and more preferably 100 atomic %.

[0043] When the second layer is a processing auxiliary film, the third layer is a light-shielding film or a combination of a light-shielding film and an anti-reflection film, and the fourth layer is a processing auxiliary film, the thickness of the second layer is usually 1 to 20 nm, preferably 2 to 10 nm, the thickness of the third layer is usually 20 to 100 nm, preferably 30 to 70 nm, and the thickness of the fourth layer is usually 1 to 30 nm, preferably 2 to 20 nm. In addition, it is preferable that the total optical density of the phase shift film, the second layer, and the third layer with respect to the exposure light is 2.0 or more, particularly 2.5 or more, and especially 3.0 or more.

[0044] The second and fourth layers made of a material containing chromium can be formed by reactive sputtering using a chromium target, a target in which chromium has been doped with one or more elements selected from oxygen, nitrogen, and carbon, or the like, and a sputtering gas in which a rare gas such as Ar, He, or Ne has been appropriately doped with a reactive gas selected from an oxygen-containing gas, a nitrogen-containing gas, a carbon-containing gas, or the like, depending on the composition of the film to be formed.

[0045] On the other hand, a film composed of a silicon-containing material of the third layer can be formed by reactive sputtering using a silicon target, a silicon nitride target, a target containing both silicon and silicon nitride, a transition metal target, a composite target of silicon and a transition metal, etc., and a sputtering gas composed of a rare gas such as Ar, He, or Ne to which a reactive gas selected from an oxygen-containing gas, a nitrogen-containing gas, a carbon-containing gas, etc., has been appropriately added depending on the composition of the film to be formed.

[0046] The phase shift mask of the present invention can be manufactured from a phase shift mask blank by a conventional method. For example, in the case of a phase shift mask blank having a chromium-containing material film formed as a second layer on a phase shift film, the phase shift mask can be manufactured by the following steps.

[0047] First, an electron beam resist film is formed on the second layer of the phase shift mask blank, and a pattern is drawn by an electron beam, followed by a predetermined developing operation to obtain a resist pattern. Next, the obtained resist pattern is used as an etching mask, and the resist pattern is transferred to the second layer by oxygen-containing chlorine-based dry etching to obtain a pattern of the second layer. Next, the obtained pattern of the second layer is used as an etching mask, and the pattern of the second layer is transferred to the phase shift film by fluorine-based dry etching to obtain a phase shift film pattern. Here, if it is necessary to leave a part of the second layer, a resist pattern that protects that part is formed on the second layer, and then the part of the second layer that is not protected by the resist pattern is removed by oxygen-containing chlorine-based dry etching. Then, the resist pattern is removed by a conventional method to obtain a phase shift mask.

[0048] In addition, in a phase shift mask blank in which a light-shielding film made of a material containing chromium or a combination of a light-shielding film and an anti-reflective film is formed as a second layer on the phase shift film, and a processing auxiliary film made of a material containing silicon is formed as a third layer on the second layer, a phase shift mask can be manufactured, for example, by the following process.

[0049] First, an electron beam resist film is formed on the third layer of the phase shift mask blank, and a pattern is drawn by an electron beam, followed by a predetermined developing operation to obtain a resist pattern. Next, the obtained resist pattern is used as an etching mask to transfer the resist pattern to the third layer by fluorine-based dry etching to obtain a pattern of the third layer. Next, the obtained pattern of the third layer is used as an etching mask to transfer the pattern of the third layer to the second layer by oxygen-containing chlorine-based dry etching to obtain a pattern of the second layer. Next, after removing the resist pattern, the obtained pattern of the second layer is used as an etching mask to transfer the pattern of the second layer to the phase shift film by fluorine-based dry etching to obtain a phase shift film pattern, and at the same time, the pattern of the third layer is removed. Next, a resist pattern that protects the portion of the second layer that is to remain is formed on the second layer, and then the portion of the second layer that is not protected by the resist pattern is removed by oxygen-containing chlorine-based dry etching. Then, the resist pattern is removed by a conventional method to obtain a phase shift mask.

[0050] On the other hand, in a phase shift mask blank in which a processing auxiliary film made of a material containing chromium is formed as a second layer on a phase shift film, and a light-shielding film made of a material containing silicon, or a combination of a light-shielding film and an anti-reflection film is formed as a third layer on the second layer, a phase shift mask can be manufactured, for example, by the following process.

[0051] First, an electron beam resist film is formed on the third layer of the phase shift mask blank, and a pattern is drawn by an electron beam, followed by a predetermined developing operation to obtain a resist pattern. Next, the obtained resist pattern is used as an etching mask, and the resist pattern is transferred to the third layer by fluorine-based dry etching to obtain a pattern of the third layer. Next, the obtained third layer pattern is used as an etching mask, and the third layer pattern is transferred to the second layer by oxygen-containing chlorine-based dry etching to obtain a pattern of the second layer in which the second layer in the portion where the phase shift film is to be removed is removed. Next, the resist pattern is removed, and a resist pattern that protects the portion where the third layer is to be left is formed on the third layer, and then the obtained second layer pattern is used as an etching mask, and the second layer pattern is transferred to the phase shift film by fluorine-based dry etching to obtain a phase shift film pattern, and at the same time, the third layer in the portion not protected by the resist pattern is removed. Next, the resist pattern is removed by a conventional method. Then, the second layer in the portion where the third layer is removed is removed by oxygen-containing chlorine-based dry etching to obtain a phase shift mask.

[0052] In addition, in a phase shift mask blank in which a processing auxiliary film made of a material containing chromium is formed as a second layer on the phase shift film, a light-shielding film made of a material containing silicon or a combination of a light-shielding film and an anti-reflection film is formed as a third layer on the second layer, and further, a processing auxiliary film made of a material containing chromium is formed as a fourth layer on the third layer, a phase shift mask can be manufactured, for example, by the following process.

[0053] First, an electron beam resist film is formed on the fourth layer of the phase shift mask blank, and a pattern is drawn by an electron beam, followed by a predetermined developing operation to obtain a resist pattern. Next, the obtained resist pattern is used as an etching mask, and the resist pattern is transferred to the fourth layer by oxygen-containing chlorine-based dry etching to obtain a fourth layer pattern. Next, the obtained fourth layer pattern is used as an etching mask, and the fourth layer pattern is transferred to the third layer by fluorine-based dry etching to obtain a third layer pattern. Next, the resist pattern is removed, and a resist pattern that protects the portion where the third layer is to be left is formed on the fourth layer, and then, the obtained third layer pattern is used as an etching mask, and the third layer pattern is transferred to the second layer by oxygen-containing chlorine-based dry etching to obtain a second layer pattern, and at the same time, the fourth layer in the portion not protected by the resist pattern is removed. Next, the second layer pattern is used as an etching mask, and the second layer pattern is transferred to the phase shift film by fluorine-based dry etching to obtain a phase shift film pattern, and at the same time, the third layer in the portion not protected by the resist pattern is removed. Next, the resist pattern is removed by a conventional method, and then the second layer in the area where the third layer has been removed and the fourth layer in the area where the resist pattern has been removed are removed by chlorine-based dry etching containing oxygen, to obtain a phase shift mask. EXAMPLES

[0054] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0055] [Example 1] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering device, and a silicon target was used as the sputtering target, with argon gas and nitrogen gas used as the sputtering gas. The discharge power was 1.9 kW, the argon gas flow rate was set to 28 sccm (fixed), and the nitrogen gas flow rate was set to between 19 and 40 sccm. Eight types of single-layer phase shift films made of SiN and with different compositions were deposited.

[0056] The optical constants of these films for a KrF excimer laser (wavelength 248 nm), the refractive index n and extinction coefficient k, were determined. Graphs plotting the values ​​of the refractive index n and extinction coefficient k versus the nitrogen gas flow rate are shown in Figures 3 and 4, respectively. The composition of these films was also measured by XPS (X-ray photoelectron spectroscopy, the same applies below). Figure 5 shows a graph plotting the values ​​of the refractive index n versus the value of N / (Si+N) (atomic ratio). From Figure 5, it was found that the flow rate at which the refractive index n was highest was when the value of N / (Si+N) was around 0.47.

[0057] Next, a 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus, and a silicon target was used as the sputtering target, and argon gas and nitrogen gas were used as the sputtering gas. The discharge power was set to 1.9 kW, the argon gas flow rate to 28 sccm, and the nitrogen gas flow rate to 27 sccm, to deposit a single-layer phase shift film made of SiN.

[0058] The refractive index n of this phase shift film for a KrF excimer laser (wavelength 248 nm) was 2.60, the extinction coefficient k was 0.70, the phase difference was 177°, the transmittance was 4.5%, and the thickness was 79 nm. When the composition of this film was measured by XPS, the value of N / (Si+N) (atomic ratio) was 0.49.

[0059] [Example 2] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering device, and a silicon target was used as the sputtering target, with argon gas and nitrogen gas used as the sputtering gas. The discharge power was 1.9 kW, the argon gas flow rate was set to 17 sccm (fixed), and the nitrogen gas flow rate was set to between 10 and 30 sccm. Eight types of single-layer phase shift films made of SiN and with different compositions were deposited.

[0060] The optical constants of these films for a KrF excimer laser (wavelength 248 nm), that is, the refractive index n and the extinction coefficient k, were obtained, and the compositions of these films were measured by XPS and confirmed in the same manner as in Example 1. It was found that the flow rate at which the refractive index n became highest was the value of N / (Si+N) of around 0.47.

[0061] Next, a 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus, and a silicon target was used as the sputtering target, and argon gas and nitrogen gas were used as the sputtering gas. The discharge power was set to 1.9 kW, the argon gas flow rate to 17 sccm, and the nitrogen gas flow rate to 27 sccm, to deposit a single-layer phase shift film made of SiN.

[0062] The refractive index n of this phase shift film for a KrF excimer laser (wavelength 248 nm) was 2.60, the extinction coefficient k was 0.60, the phase difference was 179°, the transmittance was 6.7%, and the thickness was 80 nm. When the composition of this film was measured by XPS, the value of N / (Si+N) (atomic ratio) was 0.50.

[0063] [Example 3] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus. A silicon target was used as the sputtering target, and argon gas, nitrogen gas, and oxygen gas were used as the sputtering gas. The discharge power was set to 1.9 kW, the argon gas flow rate to 28 sccm, the nitrogen gas flow rate to 26 sccm, and the oxygen gas flow rate to 1.5 sccm, to deposit a single-layer phase shift film made of SiON.

[0064] The refractive index n of this phase shift film for a KrF excimer laser (wavelength 248 nm) was 2.52, the extinction coefficient k was 0.56, the phase difference was 178°, the transmittance was 7.3%, and the thickness was 83 nm. When the composition of this film was measured by XPS, the value (atomic ratio) of N / (Si+N) was 0.49, and the oxygen content was 2 atomic %.

[0065] [Comparative Example 1] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus. A silicon target was used as the sputtering target, and argon gas and nitrogen gas were used as the sputtering gas. The discharge power was set to 1.9 kW, the argon gas flow rate to 28 sccm, and the nitrogen gas flow rate to 19 sccm to deposit a phase shift film consisting of two layers: a lower layer (thickness 27 nm) made of SiN, and an upper layer (thickness 64 nm) made of SiN, with the nitrogen gas flow rate set to 35 sccm.

[0066] The refractive index n of this phase shift film for a KrF excimer laser (wavelength 248 nm) was 2.45 for the lower layer and 2.38 for the upper layer, the extinction coefficient k was 1.5 for the lower layer and 0.07 for the upper layer, the phase difference was 177°, the transmittance was 6.2%, but the thickness was as thick as 91 nm. When the composition of this film was measured by XPS, the value (atomic ratio) of N / (Si+N) was 0.40 for the lower layer and 0.53 for the upper layer.

[0067] [Comparative Example 2] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus. A silicon target was used as the sputtering target, and argon gas and nitrogen gas were used as the sputtering gas. The discharge power was set to 1.9 kW, the argon gas flow rate was set to 28 sccm, and the nitrogen gas flow rate was continuously changed from 19 to 45 sccm to deposit a single-layer phase shift film consisting of SiN whose composition changes continuously in the thickness direction and which is a compositionally graded layer whose optical properties change continuously in the thickness direction.

[0068] The refractive index n of this phase shift film for KrF excimer laser (wavelength 248 nm) was 2.45 at the bottom surface in contact with the quartz substrate and 2.33 at the top surface away from the quartz substrate, the extinction coefficient k was 1.5 at the bottom surface in contact with the quartz substrate and 0.05 at the bottom surface in contact with the quartz substrate, the phase difference was 177°, the transmittance was 6.0%, but the thickness was as thick as 87 nm. In addition, when the composition of this film was measured by XPS, the value of N / (Si+N) (atomic ratio) was 0.40 at the bottom surface in contact with the quartz substrate and 0.53 at the top surface away from the quartz substrate.

[0069] [Comparative Example 3] A 6025 quartz substrate measuring 152 mm square and 6.35 mm thick was placed in the chamber of the sputtering apparatus. A molybdenum silicon (MoSi) target and a silicon target were used as sputtering targets, and argon gas, nitrogen gas, and oxygen gas were used as sputtering gases. The discharge power of the MoSi target was 1.2 kW, the discharge power of the silicon target was 8 kW, the argon gas flow rate was 5 sccm, the nitrogen gas flow rate was 65 sccm, and the oxygen gas flow rate was 2.5 sccm, to form a single-layer phase shift film made of MoSiON.

[0070] The refractive index n of this phase shift film for a KrF excimer laser (wavelength 248 nm) was 2.25, the extinction coefficient k was 0.52, the phase difference was 175°, and the transmittance was 6.2%, but the thickness was as thick as 99 nm. When the composition of this film was measured by XPS, it was found to contain 14 atomic % of molybdenum, and the value of N / (Si+N) (atomic ratio) was 0.56. [Explanation of symbols]

[0071] 1 Phase shift film 2. Second Layer 3. The third layer 4. The Fourth Layer 10 Transparent substrate 11 Phase shift film pattern 100 Phase Shift Mask Blanks 101 Phase shift mask

Claims

1. A photomask blank having a phase shift film formed on a transparent substrate, the phase shift film being made of a material containing silicon and nitrogen and not containing a transition metal, The exposure light is KrF excimer laser light, The phase shift film is (A) a surface oxide layer which is the outermost layer on the side separated from the transparent substrate; (B) a layer having a refractive index n of 2.55 or more and an extinction coefficient k of 0.4 to 0.7 with respect to the exposure light; It is composed of multiple layers consisting of The phase shift mask blank is characterized in that the phase shift film has a phase difference of 170 to 190°, a transmittance of 4 to 8% with respect to exposure light, and a film thickness of 85 nm or less.

2. 2. The phase shift mask blank according to claim 1, wherein the extinction coefficient k is 0.4 to 0.

6.

3. 3. The phase shift mask blank according to claim 1, wherein the transmittance of the phase shift film is 4.5 to 8%.

4. A phase shift mask blank according to any one of claims 1 to 3, characterized in that the nitrogen content (atomic %) of the (B) layer relative to the total content (atomic %) of silicon and nitrogen, N / (Si+N), is 0.43 or more and 0.53 or less.

5. 5. The phase shift mask blank according to claim 1, wherein the layer (B) is made of a material containing silicon and nitrogen.

6. 6. The phase shift mask blank according to claim 1, wherein the phase shift film has a thickness of 79 nm or less.

7. 7. The phase shift mask blank according to claim 1, wherein the surface oxide layer has an oxygen content of 20 atomic % or more.

8. 8. The phase shift mask blank according to claim 1, wherein the phase shift film has a thickness of 50 nm or more.

9. 9. The phase shift mask blank according to claim 1, wherein the surface oxide layer has a thickness of 1 nm or more and 10 nm or less.

10. A method for producing a phase shift mask blank according to any one of claims 1 to 9, comprising the steps of: forming the phase shift film by reactive sputtering using a silicon-containing target and nitrogen gas; The method for producing a phase shift mask blank is characterized in that the nitrogen gas flow rate set in the process is constant or is changed continuously or stepwise within a range of -20% to +20% of the flow rate at which the refractive index n of the phase shift film to the exposure light is maximized when the nitrogen gas flow rate is changed from a low flow rate to a high flow rate.

11. 10. A phase shift mask formed by using the phase shift mask blank according to claim 1.

Citation Information

Patent Citations

  • Mask for exposing and pattern forming method

    JP1995134392A

  • Phase shift mask and its production and exposure method using the phase shift mask

    JP1995140635A

  • Method for designing translucent film

    JP1995239546A

  • Mask for exposure, resist pattern forming method and method for producing substrate for the mask

    JP2002040625A

  • Mask for exposure, method for producing the same and exposure method using the same