Manufacturing method for flexible substrate
By employing a chromium-containing metal layer with a higher chromium weight percentage in the first metal layer and a superheated steam treatment, the method enhances heat-resistant peel strength in flexible substrates while reducing manufacturing costs.
Patent Information
- Application Number
- JP2023083624
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2038-11-22
AI Technical Summary
Existing methods for manufacturing flexible substrates fail to adequately suppress the decrease in heat-resistant peel strength and are costly due to processes like plasma treatment.
A method involving a base metal layer with a chromium-containing metal layer and a copper conductor layer, where the weight percentage of chromium in the first metal layer is higher than in the second, combined with a superheated steam treatment to form a structure that suppresses copper diffusion, thereby maintaining heat-resistant peel strength while reducing manufacturing costs.
The method effectively maintains heat-resistant peel strength by preventing copper diffusion into the polyimide film, achieving nearly identical heat-resistant peel strength to initial peel strength at a lower cost.
Smart Images

Figure 0007586228000002 
Figure 0007586228000003 
Figure 0007586228000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a flexible substrate, and more particularly to a method for producing a flexible substrate having excellent heat resistance. [Background technology]
[0002] Many types of flexible wiring boards obtained by coating a metal film on a heat-resistant resin film are used in liquid crystal panels, notebook computers, digital cameras, mobile phones, etc. These flexible wiring boards often use resin films with metal film formed on one or both sides of a heat-resistant resin film. In this specification, these resin films with metal film may be referred to as "flexible substrates."
[0003] Known manufacturing methods for this type of flexible board include a method of attaching a metal foil to a resin film with an adhesive (a method of manufacturing a three-layer board), a method of coating a metal foil with a thermosetting resin solution and drying it (a casting method), a method of attaching a thermoplastic resin film to a metal foil and thermocompressing it (a lamination method), and a method of forming a metal film on a resin film by a vacuum film formation method or a combination of a vacuum film formation method and a wet plating method (a metallizing method), etc. Vacuum film formation methods for the metallizing method include vacuum deposition, sputtering, ion plating, ion beam sputtering, etc.
[0004] Here, among the vacuum film formation methods, the sputtering method generally has excellent adhesion, but it is known that the peel strength (hereinafter sometimes referred to as heat-resistant peel strength) measured after heating the substrate to 150°C in the atmosphere and holding it there for 168 hours decreases.
[0005] Regarding flexible boards that suppress the decrease in heat-resistant peel strength, Patent Document 1 discloses a metallizing method in which a chromium layer is sputtered on a polyimide insulating layer, and then copper is sputtered to form a conductor layer on the polyimide insulating layer. Patent Document 2 discloses a material for flexible circuit boards formed by laminating, in order, a first metal thin film formed by sputtering a copper-nickel alloy target on a polyimide film, and a second metal thin film formed by sputtering a copper target on a polyimide film. Patent Document 3 discloses a two-layer copper polyimide board in which the surface of a polyimide film is modified, and Patent Document 4 discloses a metal-coated polyimide resin board in which the surface of a polyimide resin film is modified. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2-98994 [Patent Document 2] Patent No. 3447070 [Patent Document 3] JP 2007-318177 A [Patent Document 4] International Publication No. 2010 / 098236 Summary of the Invention [Problem to be solved by the invention]
[0007] In Patent Documents 1 and 2, a metal layer of chromium or nickel copper is formed on the surface of a polyimide film by sputtering in order to suppress the decrease in heat-resistant peel strength. However, the flexible substrates obtained by these documents do not sufficiently suppress the decrease in heat-resistant peel strength. In Patent Documents 3 and 4, the surface of the polyimide film is modified before a metal layer is formed on the polyimide film to suppress the decrease in heat-resistant peel strength, but the suppression of the decrease in heat-resistant peel strength is not sufficient, and in addition, there is a problem that the process of plasma treatment or the like for modifying the surface of the polyimide film is costly.
[0008] In view of the above circumstances, an object of the present invention is to provide a method for manufacturing a flexible substrate that can suppress a decrease in heat resistant peel strength and can reduce the overall manufacturing costs of the flexible substrate. [Means for solving the problem]
[0009] A method for producing a flexible substrate according to a first aspect of the present invention includes the steps of: forming an undercoat metal layer on a surface of a polyimide film, the undercoat metal layer including a chromium-containing metal layer in contact with the polyimide film; forming a copper conductor layer on the undercoat metal layer by superposing the copper conductor layer; and applying heat to the polyimide film, the undercoat metal layer, and the copper conductor layer by a predetermined heating method to form the chromium-containing metal layer into a first metal layer in contact with the polyimide film and a second metal layer positioned so as to superpose the first metal layer. The heating method is a superheated steam treatment in which superheated steam is sprayed onto the polyimide film, the base metal layer, and the copper conductor layer. It is characterized by: Effect of the Invention
[0010] According to the first invention, the base metal layer formed on the surface of the polyimide film includes a chromium-containing metal layer, and the weight percentage of chromium in the first metal layer in contact with the polyimide film is greater than the weight percentage of chromium in the second metal layer, thereby suppressing the diffusion of copper into the first metal layer. Since the heat-resistant peel strength decreases when the polyimide film is decomposed by copper, the reduction in the heat-resistant peel strength can be suppressed by suppressing the diffusion of copper into the first metal layer. In addition, it is relatively easy to make the weight percentage of chromium in the first metal layer greater than the weight percentage of chromium in the second metal layer, so that the reduction in the heat-resistant peel strength can be suppressed while suppressing the manufacturing cost of the flexible substrate. [Brief description of the drawings]
[0011] [Figure 1] 1 is an enlarged partial cross-sectional view of a flexible substrate according to a first embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of a flexible substrate according to a first embodiment of the present invention. [Diagram 3] FIG. 1 shows element mapping measurements by TEM of a flexible substrate according to a first embodiment of the present invention. (A) is a diagram showing the distribution state of Cr elements after superheated steam treatment. (B) is a diagram showing the distribution state of Cr elements before superheated steam treatment. (C) is a diagram showing the distribution state of Cu elements after superheated steam treatment. (D) is a diagram showing the distribution state of Cu elements before superheated steam treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Next, an embodiment of the present invention will be described with reference to the drawings. However, the embodiment shown below is an example of a flexible substrate 10 for embodying the technical concept of the present invention, and the present invention does not limit the flexible substrate 10 to the following. Note that the size or positional relationship of the components shown in each drawing may be exaggerated for clarity of explanation.
[0013] (First embodiment) FIG. 2 shows a cross-sectional view of a flexible substrate 10 according to a first embodiment of the present invention. As shown in FIG. 2, the flexible substrate 10 according to the present invention includes a polyimide film 11, a base metal layer 12 formed on the surface of the polyimide film 11, and a copper conductor layer 13 formed so as to be superimposed on the base metal layer 12. The base metal layer 12 is, for example, composed of a chromium-containing metal layer 14 and a base copper layer 15 provided on the polyimide film 11 side. In this embodiment, the base metal layer 12 and the like are formed on one side of the polyimide film 11, but this is not particularly limited, and a substrate in which the base metal layer 12 and the like are formed on both sides of the polyimide film 11 also corresponds to the flexible substrate 10 according to the present invention.
[0014] Fig. 1 shows an enlarged view of the circled portion in Fig. 2. In this embodiment, the chromium-containing metal layer 14 of the base metal layer 12 has a first metal layer 14a in contact with the polyimide film 11 and a second metal layer 14b positioned so as to overlap the first metal layer 14a. The flexible substrate 10 according to the present invention is characterized in that the weight percentage of chromium in the first metal layer 14a is greater than the weight percentage of chromium in the second metal layer 14b.
[0015] Of the base metal layer 12 formed on the surface of polyimide film 11, the weight percentage of chromium in first metal layer 14a in contact with polyimide film 11 is greater than the weight percentage of chromium in second metal layer 14b, thereby suppressing diffusion of copper into first metal layer 14a, as described below.
[0016] One of the causes of the decrease in the heat-resistant peel strength of the flexible substrate 10 is the decomposition of the polyimide film 11 by copper. In other words, if it is possible to prevent copper, which has high electrical conductivity, from coming into direct contact with the polyimide film 11, the heat-resistant peel strength will be increased. In this embodiment, at least a part of the base metal layer 12 is a chromium-containing metal layer 14, specifically a nickel-chromium alloy layer, so that it is possible to prevent copper from coming into contact with the polyimide film 11. However, if the chromium-containing metal layer 14 is merely formed, as the temperature of the flexible substrate 10 increases, copper will gradually diffuse in the chromium-containing metal layer 14 and come into contact with the polyimide film 11.
[0017] For this reason, a layer with a high chromium content, i.e., first metal layer 14a, is provided in a portion of chromium-containing metal layer 14. When flexible substrate 10 is heated to a high temperature, copper binds with oxygen in chromium-containing metal layer 14 and diffuses into chromium-containing metal layer 14. When a layer in which this oxygen is bound to chromium, i.e., first metal layer 14a with a high chromium content, is present, this first metal layer 14a suppresses copper diffusion even when the temperature of flexible substrate 10 is raised, and a decrease in heat-resistant peel strength can be suppressed.
[0018] A method for making the weight percentage of chromium in the first metal layer 14a greater than the weight percentage of chromium in the second metal layer 14b will be described later. This method is relatively easy to implement, and therefore makes it possible to suppress a decrease in heat-resistant peel strength while keeping the manufacturing costs of the flexible substrate 10 low.
[0019] In the flexible substrate 10 according to the present invention, the base metal layer 12 preferably includes a chromium-containing metal layer 14, i.e., a nickel-chromium alloy layer, and this nickel-chromium alloy layer is preferably composed of a first metal layer 14a and a second metal layer 14b. Nickel-chromium alloys are easily available, so they can prevent a decrease in heat-resistant peel strength at a lower cost.
[0020] (Polyimide film 11) The polyimide film 11 used in the flexible substrate 10 according to this embodiment is a film-like insulator, such as Kapton (registered trademark) 100EN film manufactured by DuPont Toray, or Upilex (registered trademark) 25SGA manufactured by Ube Industries.
[0021] (Base metal layer 12) The base metal layer 12 constituting the flexible substrate 10 according to this embodiment is formed directly on the surface of the polyimide film 11. The base metal layer 12 is preferably formed to include a chromium-containing metal layer 14 and a base copper layer 15. In this embodiment, the chromium-containing metal layer 14 is a nickel-chromium alloy, but it is also possible to use at least one selected from chromium and chromium oxide. These base metal layers 12 are preferably formed by sputtering, which is a dry plating method. The base metal layer 12 may also be formed by vacuum deposition or ion plating.
[0022] The chromium-containing metal layer 14 has relatively good adhesion to the synthetic resin that is the constituent material of the polyimide film 11. The underlying copper layer 15 has high conductivity. Since the underlying metal layer 12 is thus configured as two layers, the adhesion between the underlying metal layer 12 and the polyimide film 11 is improved and the conductivity is also increased, so that the copper conductor layer 13 superimposed on the underlying metal layer 12 can be easily wet-plated.
[0023] The thickness of the chromium-containing metal layer 14 is preferably 50 angstroms or more and 500 angstroms or less, and the thickness of the underlying copper layer 15 is preferably 500 angstroms or more and 5000 angstroms or less.
[0024] If the thickness of the chromium-containing metal layer 14 is less than 50 angstroms, adhesion problems are likely to occur during each subsequent processing step. If the thickness is greater than 500 angstroms, it becomes difficult to remove nickel or chromium during wiring processing, and cracks or warping is likely to occur in the chromium-containing metal layer 14, which is likely to cause adhesion problems between the polyimide film 11 and the underlying metal layer 12. If the thickness of the underlying copper layer 15 is less than 500 angstroms, the effect of reducing defects due to pinholes is reduced, and there is a possibility of causing electrical conductivity failure during subsequent wet plating. If the thickness exceeds 5,000 angstroms, cracks or warping is likely to occur in the underlying copper layer 15, which is likely to cause adhesion problems between the polyimide film 11 and the underlying metal layer 12.
[0025] The weight percentage of chromium in the chromium-containing metal layer 14 is preferably 12 percent or more and 50 percent or less. With such a configuration, it is possible to increase the certainty of suppressing the diffusion of copper into the first metal layer 14a.
[0026] A chromium weight percentage less than 12 percent does not migrate enough into the first metal layer 14a to inhibit copper migration, and a chromium weight percentage greater than 50% increases the cost of sputtering.
[0027] (Copper conductor layer 13) The copper conductor layer 13 constituting the flexible substrate 10 according to this embodiment is formed directly on the surface of the base metal layer 12. When the flexible substrate 10 according to this embodiment is made into a flexible wiring substrate by a semi-additive method, the thickness of the copper conductor layer 13 is about 2 μm. This is because the flexible substrate 10 has good handleability. When the flexible substrate 10 according to this embodiment is made into a flexible wiring substrate by a subtractive method, the thickness of the copper conductor layer 13 is about 8 μm. The flexible substrate 10 according to the present invention is not limited to these thicknesses. The wet plating carried out in the method for producing the flexible substrate 10 according to this embodiment is known electroplating.
[0028] (Superheated steam treatment) After the copper conductor layer 13 is formed on the flexible substrate 10 according to this embodiment, a superheated steam treatment is performed in which superheated steam is sprayed onto the flexible substrate 10. By performing this superheated steam treatment, the chromium-containing metal layer 14 constituting the base metal layer 12 has a configuration in which the chromium weight percentage is higher than that of the second metal layer 14b. In this embodiment, the chromium-containing metal layer 14 has a configuration in which the first metal layer 14a has a higher chromium content by the superheated steam treatment, but it is also possible to have a configuration in which the first metal layer 14a has a higher oxygen content by heating in a vacuum furnace, for example.
[0029] The temperature of the superheated steam is preferably 200° C. or more and 450° C. or less. If the temperature is lower than 200° C., the chromium concentration in the two metal layers of the chromium-containing metal layer 14 does not change, and the decrease in heat-resistant peel strength cannot be suppressed. In addition, superheated steam with a temperature higher than 450° C. is difficult to handle, and the superheated steam treatment is too time-consuming.
[0030] The time for spraying the superheated steam is preferably 60 seconds or more and 180 seconds or less. If the time is shorter than 60 seconds, the chromium concentration of the two metal layers of the chromium-containing metal layer 14 does not change, and the decrease in heat-resistant peel strength cannot be suppressed. If the time is longer than 180 seconds, the productivity of the flexible substrate 10 decreases.
[0031] FIG. 3 shows element mapping measurements of the flexible substrate 10 by TEM before and after superheated steam treatment. The figures in the circles in each figure represent the contents of the circles in FIG. 2, and the width of the hatched lines represents the shade of each element. That is, the narrower the width of the hatched lines, the more elements there are, i.e., the higher the volume percentage of the elements is. FIG. 3(A) and FIG. 3(B) show the distribution of chromium elements before and after superheated steam treatment, and FIG. 3(C) and FIG. 3(D) show the distribution of copper elements before and after superheated steam treatment.
[0032] 3(B), before the superheated steam treatment, chromium elements are uniformly distributed in the chromium-containing metal layer 14. After the superheated steam treatment, a large amount of chromium elements is present in the first metal layer 14a of the chromium-containing metal layer 14, and less chromium elements are present in the second metal layer 14b than in the first metal layer 14a.
[0033] 3(D), before the superheated steam treatment, copper elements are uniformly present in the underlying copper layer 15 and the copper conductor layer 13. After the superheated steam treatment, copper elements are diffused into the second metal layer 14b, but copper is not diffused into the first metal layer 14a.
[0034] By performing superheated steam treatment, the weight percentage of chromium in the first metal layer 14a is higher than that in the second metal layer 14b, as described above, thereby suppressing the diffusion of copper elements and preventing a decrease in heat-resistant peel strength.
[0035] The thickness of the first metal layer 14a (the distance from top to bottom on the paper surface of FIG. 1) is determined by the temperature and time of the superheated steam treatment. For example, if it is 20 angstroms or more, the diffusion of copper elements can be suppressed.
[0036] (Example) EXAMPLES The present invention will be described below with reference to examples and comparative examples. Note that the flexible substrate 10 according to the present invention is not limited to the following examples.
[0037] Example 1 A Kapton (registered trademark) 100EN film manufactured by DuPont Toray was used as the polyimide film 11. A chromium-containing metal layer 14 of 150 angstroms was formed on both sides of the polyimide film 11 by sputtering, and a 200 nm undercoat copper layer 15 was formed superimposed on the chromium-containing metal layer 14. The chromium-containing metal layer 14 and undercoat copper layer 15 form an undercoat metal layer 12. In Example 1, the proportion of chromium in the chromium-containing metal was 20 weight percent, and most of the other metals were nickel. A copper conductor layer 13 of 8 μm was formed superimposed on the undercoat metal layer 12 by electrolytic copper plating. After that, 300° C. superheated steam was sprayed on the substrate for about 120 seconds, and the substrate was cooled to room temperature to obtain a flexible substrate 10.
[0038] The thickness of the first metal layer 14a of this flexible substrate 10 was measured. A 1 mm wide pattern for measuring peel strength was also created from this flexible substrate 10 using a ferric chloride etching solution. The initial peel strength of the flexible substrate 10 was then measured. In addition, the flexible substrate 10 was heated and held at 150°C in the atmosphere for 168 hours, and then the heat resistant peel strength was measured. It was determined that the heat resistant peel strength was satisfactory if it was 75% of the initial peel strength. The results are shown in Table 1.
[0039] In Example 1, the initial peel strength was 510 N / m, the heat-resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0040] Example 2 The conditions were the same as in Example 1, except that the chromium content of the chromium-containing metal layer 14 was 40 weight percent. The measurement results are shown in Table 1.
[0041] In Example 2, the initial peel strength was 510 N / m, the heat-resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0042] Example 3 The conditions were the same as in Example 1, except that the chromium content of the chromium-containing metal layer 14 was 100 weight percent. The measurement results are shown in Table 1.
[0043] In Example 3, the initial peel strength was 510 N / m, the heat-resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0044] Example 4 The conditions were the same as in Example 1, except that the thickness of the chromium-containing metal layer 14 was 75 angstroms. The measurement results are shown in Table 1.
[0045] In Example 4, the initial peel strength was 510 N / m, the heat-resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0046] Example 5 The conditions were the same as in Example 1, except that the thickness of the chromium-containing metal layer 14 was 300 angstroms. The measurement results are shown in Table 1.
[0047] In Example 5, the initial peel strength was 510 N / m, the heat resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. The heat resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0048] Example 6 The conditions were the same as in Example 1, except that the temperature of the superheated steam was 200° C. The measurement results are shown in Table 1.
[0049] In Example 6, the initial peel strength was 510 N / m, the heat-resistant peel strength was 400 N / m, and the strength retention rate was 78.4%. That is, although the heat-resistant peel strength decreased, it was about 78% of the initial peel strength, and a good result was obtained.
[0050] Example 7 The conditions were the same as in Example 1, except that the temperature of the superheated steam was 350° C. The measurement results are shown in Table 1.
[0051] In Example 7, the initial peel strength was 510 N / m, the heat-resistant peel strength was 500 N / m, and the strength retention rate was 98.0%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0052] Example 8 The conditions were the same as in Example 1, except that the temperature of the superheated steam was 450° C. The measurement results are shown in Table 1.
[0053] In Example 8, the initial peel strength was 510 N / m, the heat-resistant peel strength was 510 N / m, and the strength retention rate was 100.0%. That is, the heat-resistant peel strength was the same as the initial peel strength, and good results were obtained.
[0054] Example 9 The conditions were the same as in Example 1, except that the polyimide film 11 was Upilex (registered trademark) 25SGA manufactured by Ube Industries, Ltd. The measurement results are shown in Table 1.
[0055] In Example 9, the initial peel strength was 550 N / m, the heat-resistant peel strength was 450 N / m, and the strength retention rate was 81.8%. That is, the heat-resistant peel strength was almost the same as the initial peel strength, and good results were obtained.
[0056] Comparative Example 1 Except for not carrying out the superheated steam treatment, the conditions were the same as in Example 1. The measurement results are shown in Table 1.
[0057] In Comparative Example 1, the initial peel strength was 510 N / m, the heat resistant peel strength was 350 N / m, and the strength retention rate was 68.6%. That is, the heat resistant peel strength was lower than the initial peel strength.
[0058] Comparative Example 2 The conditions were the same as in Example 1, except that the chromium content of the chromium-containing metal layer 14 was 7 weight percent. The measurement results are shown in Table 1.
[0059] In Comparative Example 2, the initial peel strength was 510 N / m, the heat resistant peel strength was 300 N / m, and the strength retention rate was 58.8%. That is, the heat resistant peel strength was lower than the initial peel strength.
[0060] Comparative Example 3 The conditions were the same as in Example 1, except that the thickness of the chromium-containing metal layer 14 was 30 angstroms. The measurement results are shown in Table 1.
[0061] In Comparative Example 3, the initial peel strength was 510 N / m, the heat resistant peel strength was 200 N / m, and the strength retention rate was 39.2%. That is, the heat resistant peel strength was lower than the initial peel strength.
[0062] Comparative Example 4 The conditions were the same as in Example 1, except that the polyimide film 11 was Upilex (registered trademark) 25SGA manufactured by Ube Industries, Ltd., and the superheated steam treatment was not performed. The measurement results are shown in Table 1.
[0063] In Comparative Example 4, the initial peel strength was 600 N / m, the heat resistant peel strength was 300 N / m, and the strength retention rate was 50.0%. That is, the heat resistant peel strength was lower than the initial peel strength.
[0064] [Table 1] [Explanation of symbols]
[0065] 10 Flexible substrate 11 Polyimide film 12 Undercoat metal layer 13 Copper conductor layer 14 Chromium-containing metal layer 14a 1st metal layer 14b 2nd metal layer
Claims
[Claim 1] A chromium-containing metal layer is provided on the surface of the polyimide film and is in contact with the polyimide film. forming a base metal layer; forming a copper conductor layer on the base metal layer; The polyimide film, the base metal layer, and the copper conductor layer are Heat is applied by the heating method described above to bond the chromium-containing metal layer to the polyimide film. a first metal layer overlapping the first metal layer; and a second metal layer positioned so as to overlap the first metal layer. and The weight percent of chromium in the first metal layer is More than a percent of the amount The heating method includes heating the polyimide film, the base metal layer, and the copper film by applying superheated steam to the polyimide film, the base metal layer, and the copper film. This is a process in which superheated steam is sprayed onto the conductor layer. A method for manufacturing a flexible substrate comprising the steps of:
Citation Information
Patent Citations
Formation of conductor layer on polyimide insulation layer
JP1990098994A
Flexible printed wiring board
JP2003318533A
Double layer copper polyimide substrate
JP2007318177A
Copper foil for printed circuit board
JP2010258398A
Copper foil for printed circuit board
JP2011014642A