Method for manufacturing non-aqueous lithium-type storage element

The manufacturing method for non-aqueous lithium type electricity storage elements addresses heat management and micro short circuits, enhancing energy density and durability by controlling voltage application sequences and promoting alkali metal ion doping.

JP7586729B2Active Publication Date: 2024-11-19ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021025357
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-11-19
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Existing power storage elements, such as lithium ion batteries and electric double layer capacitors, face challenges in achieving high energy density, high output characteristics, and durability, with lithium ion capacitors being a promising candidate but lacking effective methods to control heat generated during the manufacturing process, which can lead to micro short circuits.

Method used

A manufacturing method for non-aqueous lithium type electricity storage elements involves stacking positive and negative electrodes with a separator, injecting a non-aqueous electrolyte, and applying controlled voltages to groups of exterior bodies in a specific sequence to manage heat generation and promote alkali metal ion doping, thereby reducing micro short circuits and enhancing input/output characteristics.

Benefits of technology

The method effectively controls heat generation and promotes alkali metal ion doping, resulting in improved input/output characteristics and increased yield of non-aqueous lithium type electricity storage elements with enhanced energy density and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586729000001
    Figure 0007586729000001
  • Figure 0007586729000002
    Figure 0007586729000002
  • Figure 0007586729000003
    Figure 0007586729000003
Patent Text Reader

Abstract

To provide a manufacturing method which can suppress heat generation caused in decomposition of alkali metal compound included in a positive electrode precursor and suppress a fine short circuit in production to increase the yield.SOLUTION: Provided is a method for manufacturing a nonaqueous lithium-type power storage element, comprising a first voltage-applying step which includes: preparing a plurality of outer packaging bodies; setting, in each outer packaging body, a positive electrode, a negative electrode, a separator and a nonaqueous electrolyte solution, and electrically bonding them; dividing the plurality of outer packaging bodies to groups I and II; disposing the groups I and II in such a way that the outer packaging bodies belonging to the group II are not continuously adjacent to each other as far as possible; and then, applying a voltage to the group I.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a non-aqueous lithium-type storage element. [Background technology]

[0002] In recent years, from the perspective of protecting the global environment and effectively utilizing energy to conserve resources, power smoothing systems for wind power generation or late-night power storage systems, distributed home energy storage systems based on solar power generation technology, and energy storage systems for electric vehicles have been attracting attention.

[0003] The primary requirement for batteries used in these energy storage systems is a high energy density, and the development of lithium-ion batteries is being actively pursued as a promising candidate for a high-energy-density battery that can meet this requirement.

[0004] The second requirement is high output characteristics. For example, in a combination of a high-efficiency engine and a power storage system (e.g., a hybrid electric vehicle) or a combination of a fuel cell and a power storage system (e.g., a fuel cell electric vehicle), high output discharge characteristics are required in the power storage system during acceleration. Currently, electric double layer capacitors, nickel-metal hydride batteries, etc. are being developed as high-output power storage devices.

[0005] Among electric double layer capacitors, those that use activated carbon for the electrodes have output characteristics of approximately 0.5 to 1 kW / L. These electric double layer capacitors also have high durability (cycle characteristics and high-temperature storage characteristics), and have been considered the optimal device for the fields that require high output. However, their energy density is only approximately 1 to 5 Wh / L. Therefore, further improvement in energy density is necessary.

[0006] On the other hand, nickel-metal hydride batteries currently used in hybrid electric vehicles have high output equivalent to that of electric double-layer capacitors and an energy density of about 160 Wh / L. However, vigorous research is being conducted to further increase their energy density and output, as well as to improve their durability (especially their stability at high temperatures).

[0007] Research is also underway to increase the output of lithium-ion batteries. For example, lithium-ion batteries have been developed that can achieve high output of over 3 kW / L at a discharge depth of 50% (a value indicating the percentage of the discharge capacity of the storage element that has been discharged). However, their energy density is below 100 Wh / L, a design that deliberately suppresses the high energy density that is the greatest feature of lithium-ion batteries. Furthermore, their durability (cycle characteristics and high-temperature storage characteristics) is inferior to that of electric double-layer capacitors. Therefore, to ensure practical durability, they must be used within a discharge depth range narrower than 0 to 100%. Because the actual usable capacity is even smaller, vigorous research is being conducted to further improve durability.

[0008] As described above, there is a strong demand for practical application of energy storage elements that combine high energy density, high output characteristics, and durability. However, the existing energy storage elements described above each have their own advantages and disadvantages. Therefore, a new energy storage element that satisfies these technical requirements is required. As a promising candidate, an energy storage element called a lithium-ion capacitor has attracted attention and is being actively developed.

[0009] A lithium-ion capacitor is a type of energy storage element (non-aqueous alkali metal energy storage element) that uses a non-aqueous electrolyte containing lithium salt. At the positive electrode, at approximately 3 V or higher, a non-Faradic reaction occurs due to the adsorption and desorption of anions, similar to an electric double-layer capacitor, and at the negative electrode, a Faradic reaction occurs due to the absorption and release of lithium ions, similar to a lithium-ion battery.

[0010] To summarize the electrode materials and their characteristics, when materials such as activated carbon are used for the electrodes and charging and discharging is performed by the adsorption and desorption of ions on the surface of the activated carbon (non-Faradaic reaction), high output and durability are achieved, but the energy density is low (for example, 1x).On the other hand, when oxides or carbon materials are used for the electrodes and charging and discharging is performed by the Faradaic reaction, the energy density is high (for example, 10x that of non-Faradaic reactions using activated carbon), but there are issues with durability and output characteristics.

[0011] As a combination of these electrode materials, electric double layer capacitors use activated carbon (energy density 1x) for the positive and negative electrodes, and are characterized by charging and discharging through non-Faradic reactions at both the positive and negative electrodes.They have high output and high durability, but low energy density (positive electrode 1x x negative electrode 1x = 1).

[0012] Lithium-ion secondary batteries use lithium transition metal oxides (10 times the energy density) for the positive electrode and carbon materials (10 times the energy density) for the negative electrode, and are characterized by charging and discharging via the Faraday reaction at both the positive and negative electrodes. While they have a high energy density (10 times the positive electrode x 10 times the negative electrode = 100), they have issues with output characteristics and durability. Furthermore, to meet the high durability required for hybrid electric vehicles and other applications, the depth of discharge must be limited, and lithium-ion secondary batteries can only use 10-50% of their energy.

[0013] Lithium-ion capacitors are a new asymmetric capacitor that combines the features of electric double-layer capacitors and lithium-ion secondary batteries. They use activated carbon (energy density 1x) for the positive electrode and carbon material (energy density 10x) for the negative electrode, and charge and discharge is carried out by a non-Faradic reaction at the positive electrode and a Faradic reaction at the negative electrode. They are characterized by high output and durability, as well as a high energy density (positive electrode 1x x negative electrode 10x = 10), and do not require limitations on the depth of discharge as with lithium-ion secondary batteries.

[0014] Lithium-ion capacitors are used in applications such as railways, construction machinery, and automotive energy storage. Capacitors used in these applications are constructed by connecting multiple capacitor cells (hereinafter, a single capacitor cell may be abbreviated as "cell") in series or parallel to form a pack that meets the required characteristics. Cells are required to have excellent input / output characteristics as well as a uniform self-discharge rate, and it is necessary to minimize manufacturing variations.

[0015] To meet these demands, there are known techniques for improving input / output characteristics and suppressing the occurrence of micro-short circuits by controlling parameters related to the cell in the doping process or aging process. For example, it has been proposed to pressurize and heat the cell in the doping process to control the voltage and current (Patent Document 1), and to store the nonaqueous alkali metal energy storage element precursor at a temperature of 45°C to 100°C in the aging process after adjusting the voltage to 4.03V to 5.0V (Patent Document 2).

[0016] However, neither of the documents considers a method for controlling heat generation due to decomposition of the alkali metal compound during the doping process. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] Patent No. 6669915 [Patent Document 2] Patent No. 6669914 Summary of the Invention [Problem to be solved by the invention]

[0018] The present invention has been made in view of the above-mentioned current situation, and therefore, an object of the present invention is to provide a production method that controls heat generated when an alkali metal compound contained in a positive electrode precursor is decomposed, thereby suppressing micro-short circuits during production and increasing yield. [Means for solving the problem]

[0019] The present invention has been made based on the above findings. That is, the present invention is as follows: <1> A method for producing a non-aqueous lithium-type storage element, comprising: The nonaqueous lithium-ion storage element includes a plurality of exterior housings, the plurality of exterior bodies each contain a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution, and are electrically connected to each other; The following steps: (1) a step of stacking a cathode precursor containing a cathode active material made of a carbon material and lithium carbonate, and a cathode containing a cathode active material capable of absorbing and releasing lithium ions, with the separator interposed therebetween, to obtain a laminate, and enclosing the laminate in each of the exterior bodies; (2) a liquid injection step of injecting the nonaqueous electrolyte solution containing lithium ions into each of the exterior bodies; (3) a storage element precursor formation step of electrically bonding the plurality of exterior bodies to obtain a non-aqueous lithium-based storage element precursor; (4) a first voltage application step of dividing the total number of the plurality of exterior bodies into an exterior body group I, which comprises 30% to 70% of the total number of the plurality of exterior bodies, and an exterior body group II, arranging the exterior body groups I and II so that the maximum number of consecutively adjacent exterior bodies belonging to the exterior body group II is 0% to 10% of the total number of the plurality of exterior bodies, and applying a voltage to the exterior body group I; and (5) a second voltage application step of applying a voltage to the exterior body group II after a predetermined delay time has elapsed since the first voltage application step; A method for producing a non-aqueous lithium-type storage element, comprising: <2> Item 2. The method for manufacturing a nonaqueous lithium-type storage element according to item 1, wherein in the first voltage application step, the maximum number of adjacent, consecutive exterior bodies belonging to the exterior body group II is 3 or less. <3> 3. The method for manufacturing a nonaqueous lithium-type storage element according to item 1 or 2, wherein in the first voltage application step, when the total number of exterior bodies belonging to exterior body group I and II is within a range of 10 to 50, the maximum number of consecutively adjacent exterior bodies belonging to exterior body group II is 3 or less. <4> Each of the plurality of exterior bodies has a front surface and a back surface, In the energy storage element precursor forming step, after one exterior body is arranged so that one of the front and rear surfaces thereof faces one of the front and rear surfaces of another exterior body, the plurality of exterior bodies are electrically coupled together; and 4. The method for manufacturing a nonaqueous lithium-type storage element according to any one of items 1 to 3, wherein in the first voltage application step, multiple exterior bodies belonging to both groups I and II are arranged such that the number of adjacent, face-to-face surfaces of multiple exterior bodies belonging to the same exterior body group is 0% to 50% of the total number of surfaces of the exterior bodies belonging to both groups, and a voltage is applied to exterior body group I. <5> 5. The method for producing a nonaqueous lithium-type storage element according to any one of items 1 to 4, wherein in the first voltage application step, the exterior bodies belonging to the exterior body group I are not adjacent to each other. <6> 6. The method for manufacturing a nonaqueous lithium-type storage element according to any one of items 1 to 5, wherein in the first voltage application step, exterior bodies belonging to exterior body group I and exterior bodies belonging to exterior body group II are arranged alternately. <7> When the delay time is X (min.) and the charging rate during voltage application is A, the first and second voltage application steps satisfy the following relational expression: (120 / A-10)≦X, and 1≦A≦8 7. The method for producing a nonaqueous lithium-ion storage element according to any one of items 1 to 6, wherein the above condition is satisfied. <8> 8. The method for producing a nonaqueous lithium-type storage element according to any one of items 1 to 7, wherein when the applied voltages in the first and second voltage application steps are in the range of 4.3 V to 4.5 V, the decomposition rate of the lithium carbonate per unit time is 4.5% / 0.1 V to 7.5% / 0.1 V. <9> When the temperature of the nonaqueous lithium-ion storage element precursor immediately after the start of the first and second voltage application steps is T1 (°C), and the maximum temperature of the nonaqueous lithium-ion storage element precursor during the first and second voltage application steps is T2 (°C), 9. The method for producing a nonaqueous lithium-type storage element according to any one of items 1 to 8, wherein 35≦T1≦50 and 0≦T2−T1≦10. <10> 10. The method for producing a nonaqueous lithium-type storage element according to any one of items 1 to 9, wherein the negative electrode included in the outer package belonging to group I and the negative electrode included in the outer package belonging to group II are doped with lithium ions sequentially. [Effects of the Invention]

[0020] According to the present invention, by suitably controlling the heat generated when the alkali metal compound contained in the positive electrode precursor is decomposed, it is possible to provide a method for manufacturing a nonaqueous lithium-type energy storage element that promotes doping of alkali metal ions into the negative electrode, thereby achieving excellent input / output characteristics and suppressing micro-short circuits during manufacturing. DETAILED DESCRIPTION OF THE INVENTION

[0021] Hereinafter, embodiments of the present invention will be described in detail. A nonaqueous lithium-type energy storage element generally has a positive electrode, a negative electrode, a separator, an electrolyte, and an exterior body as its main components. The electrolyte is an organic solvent in which a lithium salt is dissolved (hereinafter referred to as a nonaqueous electrolyte). In this specification, the positive electrode material before the doping process is referred to as a "positive electrode precursor," and the positive electrode material after the doping process is referred to as a "positive electrode."

[0022] <Positive electrode> The positive electrode has a positive electrode current collector and a positive electrode active material layer present on one or both sides thereof. The positive electrode is also characterized by including an alkali metal compound as a positive electrode precursor prior to the process of doping the alkali metal ions into the negative electrode. As described below, in this embodiment, it is preferable to pre-dope the negative electrode with alkali metal ions during the energy storage device assembly process. The pre-doping method is preferably to assemble the energy storage device using a positive electrode precursor containing an alkali metal compound, a negative electrode, a separator, an outer casing, and a non-aqueous electrolyte solution, and then apply a voltage between the positive electrode precursor and the negative electrode. The alkali metal compound is preferably contained in the positive electrode precursor, and more preferably in the positive electrode active material layer formed on the positive electrode current collector of the positive electrode precursor.

[0023] [Cathode active material layer] The positive electrode active material layer preferably contains a positive electrode active material containing a carbon material, and may further contain optional components such as a lithium transition metal oxide, a conductive filler, a binder, and a dispersion stabilizer, as necessary.

[0024] In this embodiment, an alkali metal compound such as lithium carbonate is preferably contained in the positive electrode active material layer of the positive electrode precursor or on the surface of the positive electrode active material layer.

[0025] [Cathode active material] The positive electrode active material preferably contains a carbon material. The carbon material is more preferably carbon nanotubes, graphene, graphene oxide, a conductive polymer, or a porous carbon material, and even more preferably activated carbon. The positive electrode active material may be a mixture of one or more materials, or may contain a material other than a carbon material (e.g., a composite oxide of lithium and a transition metal).

[0026] Preferably, the content of the carbon material with respect to the total amount of the positive electrode active material is 50% by mass or more, more preferably 60% by mass or more. The content of the carbon material can be 100% by mass, but from the viewpoint of obtaining good effects by using other materials in combination, for example, it is preferably 95% by mass or less, and may be 90% by mass or less. The upper and lower limits of the range of the content of the carbon material can be arbitrarily combined.

[0027] When using activated carbon as the positive electrode active material, there are no particular restrictions on the type of activated carbon and its raw materials. However, in order to achieve both high input / output characteristics and high energy density, it is preferable to optimally control the pores of the activated carbon. Specifically, the amount of mesopores derived from pores with a diameter of 20 Å (i.e., 20 × 10 -10 m) or more and 500 Å or less calculated by the BJH method is V1 (cm 3 / g), and the amount of micropores derived from pores with a diameter of less than 20 Å calculated by the MP method is V2 (cm 3 / g). Then, (1) For high input / output characteristics, activated carbon (hereinafter also referred to as activated carbon 1) that satisfies 0.3 < V1 ≤ 0.8, and 0.5 ≤ V2 ≤ 1.0, and has a specific surface area measured by the BET method of 1,500 m 2 / g or more and 3,000 m 2 / g or less is preferable. Also, (2) In order to obtain high energy density, activated carbon (hereinafter also referred to as activated carbon 2) that satisfies 0.8 < V1 ≤ 2.5, and 0.8 < V2 ≤ 3.0, and has a specific surface area measured by the BET method of 2,300 m 2 / g or more and 4,000 m 2 / g or less is preferable.

[0028] Hereinafter, (1) activated carbon 1 and (2) activated carbon 2 will be sequentially described individually.

[0029] [Activated Carbon 1] The amount of mesopores V1 of activated carbon 1 is 0.3 cm 3On the other hand, in order to prevent a decrease in the bulk density of the positive electrode, it is preferable that the value is 0.8 cm 3 / g or less. The V1 is more preferably 0.35 cm 3 / g or more 0.7cm 3 / g or less, more preferably 0.4 cm 3 / g or more 0.6cm 3 / g or less.

[0030] The micropore volume V2 of activated carbon 1 is 0.5 cm to increase the specific surface area of ​​activated carbon and increase the capacity. 3 On the other hand, in order to reduce the bulk of the activated carbon, increase the density as an electrode, and increase the capacity per unit volume, it is preferable that the activated carbon has a density of 1.0 cm 3 / g or less. The V2 is more preferably 0.6 cm 3 / g or more 1.0cm 3 / g or less, more preferably 0.8 cm 3 / g or more 1.0cm 3 / g or less.

[0031] The ratio of mesopore volume V1 to micropore volume V2 (V1 / V2) is preferably in the range of 0.3≦V1 / V2≦0.9. That is, from the viewpoint of increasing the ratio of mesopore volume to micropore volume to an extent that can suppress a decrease in output characteristics while maintaining high capacity, V1 / V2 is preferably 0.3 or more. On the other hand, from the viewpoint of increasing the ratio of micropore volume to mesopore volume to an extent that can suppress a decrease in capacity while maintaining high output characteristics, V1 / V2 is preferably 0.9 or less. A more preferable range for V1 / V2 is 0.4≦V1 / V2≦0.7, and an even more preferable range for V1 / V2 is 0.55≦V1 / V2≦0.7.

[0032] In order to maximize the output of the resulting electricity storage element, the average pore diameter of the activated carbon 1 is preferably 17 Å or more, more preferably 18 Å or more, and most preferably 20 Å or more. In order to maximize the capacity, the average pore diameter of the activated carbon 1 is preferably 25 Å or less.

[0033] The BET specific surface area of ​​activated carbon 1 is 1,500 m 2 / g or more 3,000m 2 / g or less, and 1,500m 2 / g or more 2,500m 2 / g or less is more preferable. 2 / g or more, a good energy density is easily obtained, while a BET specific surface area of ​​3,000 m 2 When the electrode has a porosity of 0.1g or less, it is not necessary to add a large amount of binder to maintain the strength of the electrode, and therefore the performance per volume of the electrode is improved.

[0034] The activated carbon 1 having the above-mentioned characteristics can be obtained, for example, using the raw materials and processing method described below.

[0035] In this embodiment, the carbon source used as the raw material for the activated carbon 1 is not particularly limited. Examples include plant-based raw materials such as wood, wood flour, coconut shells, pulp manufacturing by-products, bagasse, and blackstrap molasses; fossil-based raw materials such as peat, lignite, brown coal, bituminous coal, anthracite, petroleum distillation residue components, petroleum pitch, coke, and coal tar; various synthetic resins such as phenolic resins, vinyl chloride resins, vinyl acetate resins, melamine resins, urea resins, resorcinol resins, celluloid, epoxy resins, polyurethane resins, polyester resins, and polyamide resins; synthetic rubbers such as polybutylene, polybutadiene, and polychloroprene; other synthetic woods, synthetic pulps, and carbonized versions of these. Among these raw materials, plant-based raw materials such as coconut shells and wood flour, and carbonized versions of these, are preferred from the standpoints of mass production and cost, with coconut shell carbonized versions being particularly preferred.

[0036] As a method for carbonizing and activating these raw materials to convert them into the activated carbon 1, known methods such as a fixed bed method, a moving bed method, a fluidized bed method, a slurry method, a rotary kiln method, etc. can be used.

[0037] Examples of carbonization methods for these raw materials include a method of firing them at about 400 to 700°C (preferably 450 to 600°C) for about 30 minutes to 10 hours using an inert gas such as nitrogen, carbon dioxide, helium, argon, xenon, neon, carbon monoxide, or combustion exhaust gas, or a mixed gas containing these inert gases as the main component and other gases.

[0038] As a method for activating the carbonized material obtained by the carbonization method, a gas activation method is preferably used in which the carbonized material is fired using an activation gas such as water vapor, carbon dioxide, oxygen, etc. Among these, a method using water vapor or carbon dioxide as the activation gas is preferred.

[0039] In this activation method, it is preferable to activate the carbonized material by raising the temperature to 800 to 1,000°C over 3 to 12 hours (preferably 5 to 11 hours, more preferably 6 to 10 hours) while supplying an activation gas at a rate of 0.5 to 3.0 kg / h (preferably 0.7 to 2.0 kg / h).

[0040] Furthermore, prior to the activation treatment of the carbonized material, the carbonized material may be subjected to primary activation in advance. In this primary activation, a method of gas activation in which the carbon material is fired at a temperature of less than 900°C using an activation gas such as water vapor, carbon dioxide, or oxygen is preferably employed.

[0041] By appropriately combining the calcination temperature and calcination time in the carbonization method and the activation gas supply amount, temperature rise rate, and maximum activation temperature in the activation method, activated carbon 1 having the above-mentioned characteristics that can be used in this embodiment can be produced.

[0042] The average particle size of the activated carbon 1 is preferably 2 to 20 μm.

[0043] If the average particle diameter is 2 μm or more, the density of the active material layer is high, and therefore the capacity per electrode volume tends to be high. Here, a small average particle diameter may result in the drawback of low durability, but if the average particle diameter is 2 μm or more, such a drawback is unlikely to occur. On the other hand, if the average particle diameter is 20 μm or less, the battery tends to be more suitable for high-speed charge and discharge. The average particle diameter is more preferably 2 to 15 μm, and even more preferably 3 to 10 μm.

[0044] [Activated carbon 2] The mesopore volume V1 of activated carbon 2 is set to 0.8 cm from the viewpoint of increasing the output characteristics when the positive electrode material is incorporated into an energy storage element. 3 / g, while a value greater than 2.5 cm 3 / g or less. The V1 is more preferably 1.00 cm 3 / g or more 2.0cm 3 / g or less, more preferably 1.2 cm 3 / g or more 1.8cm 3 / g or less.

[0045] On the other hand, the micropore volume V2 of activated carbon 2 is set to 0.8 cm in order to increase the specific surface area of ​​the activated carbon and increase the capacity. 3 / g is preferable, while from the viewpoint of increasing the density of the activated carbon as an electrode and increasing the capacity per unit volume, it is preferable to use a value of 3.0 cm 3 / g or less. The V2 is more preferably 1.0 cm 3 / g or greater than 2.5cm 3 / g or less, more preferably 1.5 cm 3 / g or more 2.5cm 3 / g or less.

[0046] The activated carbon 2 having the above-described mesopores and micropores has a higher BET specific surface area than activated carbons used in conventional electric double layer capacitors or lithium ion capacitors. The specific value of the BET specific surface area of ​​the activated carbon 2 is 3,000 m 2 / g or more 4,000m 2 / g or less, and 3,200m 2 / g or more 3,800m 2 / g or less is more preferable. 2 / g or more, a good energy density is easily obtained, while a BET specific surface area of ​​4,000 m 2 When the electrode has a porosity of 0.1g or less, it is not necessary to add a large amount of binder to maintain the strength of the electrode, and therefore the performance per volume of the electrode is improved.

[0047] The activated carbon 2 having the above-mentioned characteristics can be obtained, for example, using the raw materials and processing methods described below.

[0048] The carbonaceous material used as the raw material for the activated carbon 2 is not particularly limited as long as it is a carbon source typically used as a raw material for activated carbon, and examples thereof include plant-based raw materials such as wood, wood flour, and coconut shells; fossil-based raw materials such as petroleum pitch and coke; and various synthetic resins such as phenolic resin, furan resin, vinyl chloride resin, vinyl acetate resin, melamine resin, urea resin, and resorcinol resin. Among these raw materials, phenolic resin and furan resin are particularly preferred because they are suitable for producing activated carbon with a high specific surface area.

[0049] Methods for carbonizing these raw materials or heating methods during activation treatment include known methods such as fixed bed, moving bed, fluidized bed, slurry, and rotary kiln. The atmosphere used during heating is an inert gas such as nitrogen, carbon dioxide, helium, or argon, or a gas mixture containing these inert gases as the main component with other gases. Carbonization is generally performed at a temperature of about 400 to 700°C for about 0.5 to 10 hours.

[0050] Methods for activating carbides include gas activation, in which the carbide is fired using an activation gas such as steam, carbon dioxide, or oxygen, and alkali metal activation, in which the carbide is mixed with an alkali metal compound and then heated. However, the alkali metal activation method is preferred for producing activated carbon with a high specific surface area.

[0051] In this activation method, carbide is mixed with an alkali metal compound such as KOH or NaOH in a mass ratio of 1:1 or more (the amount of alkali metal compound is equal to or greater than the amount of carbide), and then heated in an inert gas atmosphere at a temperature in the range of 600 to 900°C for 0.5 to 5 hours. Thereafter, the alkali metal compound is removed by washing with acid and water, and the mixture is then dried.

[0052] To increase the micropore volume without increasing the mesopore volume, it is recommended to mix a larger amount of carbide with KOH during activation. To increase both the micropore volume and the mesopore volume, it is recommended to use a larger amount of KOH. Furthermore, to mainly increase the mesopore volume, it is preferable to perform steam activation after alkali activation treatment.

[0053] The average particle size of the activated carbon 2 is preferably 2 μm or more and 20 μm or less, and more preferably 3 μm or more and 10 μm or less.

[0054] [Use of activated carbon] Each of activated carbons 1 and 2 may be a single type of activated carbon, or may be a mixture of two or more types of activated carbon, with the mixture as a whole exhibiting the above-mentioned characteristic values ​​for each of them.

[0055] The activated carbons 1 and 2 may be used either alone or in combination.

[0056] The positive electrode active material may contain a material other than activated carbons 1 and 2 (for example, activated carbon not having the specific V1 and / or V2, or a material other than activated carbon (for example, a composite oxide of lithium and a transition metal)). In an exemplary embodiment, the content of activated carbon 1, the content of activated carbon 2, or the total content of activated carbons 1 and 2 is preferably more than 50 mass% of the total positive electrode active material, more preferably 70 mass% or more, even more preferably 90 mass% or more, and most preferably 100 mass%.

[0057] [Lithium transition metal oxide] The lithium transition metal oxide contains a transition metal oxide capable of occluding and releasing lithium. There is no particular limitation on the transition metal oxide used as the positive electrode active material. Examples of the transition metal oxide include oxides containing at least one element selected from the group consisting of cobalt, nickel, manganese, iron, vanadium, and chromium. Specifically, the transition metal oxide has the following formula: Li x CoO2{where x satisfies 0 ≦ x ≦ 1.}, Li x NiO2{where x satisfies 0 ≦ x ≦ 1.}, Li x Ni y M (1-y) O2{where M is at least one element selected from the group consisting of Co, Mn, Al, Fe, Mg, and Ti, x satisfies 0 ≦ x ≦ 1, and y satisfies 0.02 < y < 0.97.}, Li x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O2{where x satisfies 0 ≦ x ≦ 1.}, Li x MnO2{where x satisfies 0 ≦ x ≦ 1.}, α-Li x FeO2{where x satisfies 0 ≦ x ≦ 1.}, Li x VO2{where x satisfies 0 ≦ x ≦ 1.}, Li x CrO2{where x satisfies 0 ≦ x ≦ 1.}, Li x FePO4{where x satisfies 0 ≦ x ≦ 1.}, Li x MnPO4{where x satisfies 0 ≦ x ≦ 1.}, Li z V2(PO4)3{where z satisfies 0 ≦ z ≦ 3.}, Li x Mn2O4{where x satisfies 0 ≦ x ≦ 1.}, Li x M y Mn (2-y)O4{In the formula, M is at least one element selected from the group consisting of Co, Mn, Al, Fe, Mg, and Ti, x satisfies 0 ≦ x ≦ 1, and y satisfies 0.02 < y < 0.97.}, Li x Ni a Co b Al (1-a-b) O2{In the formula, x satisfies 0 ≦ x ≦ 1, and a and b satisfy 0.02 < a < 0.97 and 0.02 < b < 0.97.}, Li x Ni c Co d Mn (1-c-d) O2{In the formula, x satisfies 0 ≦ x ≦ 1, and c and d satisfy 0.02 < c < 0.97 and 0.02 < d < 0.97.} Compounds represented by etc. are exemplified. Among these, from the viewpoints of high capacity, low resistance, cycle characteristics, decomposition of alkali metal compounds, and suppression of the lack of positive electrode active material during pre-doping, the above formula Li x Ni a Co b Al (1-a-b) O2, Li x Ni c Co d Mn (1-c-d) O2, Li x CoO2, Li x Mn2O4, Li x FePO4, Li x MnPO4, or Li z Compounds represented by V2(PO4)3 are preferred.

[0058] In the present embodiment, if an alkali metal compound different from the positive electrode active material is contained in the positive electrode coating liquid, the alkali metal compound can serve as a dopant source of alkali metal during pre-doping and can be pre-doped into the negative electrode. Therefore, even if lithium ions are not contained in the transition metal compound in advance (that is, even if x = 0 or z = 0 in the above formula), electrochemical charge and discharge can be performed as a non-aqueous lithium-type energy storage device.

[0059] The average particle size of the lithium transition metal oxide is preferably 0.1 to 20 μm, more preferably 0.5 to 15 μm, and even more preferably 1 to 10 μm. When the average particle size of the lithium transition metal oxide is 0.1 μm or more, the density of the active material layer is high, and therefore the capacity per electrode volume tends to be high. Here, a small average particle size may result in the drawback of low durability, but an average particle size of 0.1 μm or more is less likely to cause such a drawback. On the other hand, when the average particle size of the lithium transition metal oxide is 20 μm or less, it tends to be more suitable for high-speed charge and discharge. The average particle size of the lithium transition metal oxide is preferably smaller than the average particle size of the carbon material. When the average particle size of the lithium transition metal oxide is small, the lithium transition metal oxide is arranged in the voids formed by the carbon material with a large average particle size, thereby reducing resistance.

[0060] The lithium transition metal oxide may be used singly or may be a mixture of two or more materials, each of which exhibits the above-mentioned characteristic values ​​as a whole mixture.

[0061] The positive electrode active material may contain a material other than the lithium transition metal oxide, for example, a conductive polymer, etc. When the content of the lithium transition metal oxide in the total solid content of the positive electrode coating liquid is A2, A2 is preferably 5% by mass or more and 35% by mass or less, and more preferably 10% by mass or more and 30% by mass or less.

[0062] The ratio A2 / A1 of the content A2 of the lithium transition metal oxide to the content A1 of the carbon material is preferably 0.1 or more and 10.0 or less, more preferably 0.2 or more and 5.0 or less. If A2 / A1 is 0.1 or more, the bulk density of the positive electrode active material layer can be increased, resulting in a high capacity. If A2 / A1 is 10.0 or less, the electronic conduction between the activated carbon is increased, resulting in a low resistance, and the contact area between the activated carbon and the alkali metal compound is increased, resulting in a promotion of decomposition of the alkali metal compound.

[0063] [Alkali metal compounds] In this embodiment, the alkali metal compound may be at least one compound selected from the group consisting of lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate, lithium oxide, and lithium hydroxide. Because the alkali metal compound is decomposed in the positive electrode precursor to release cations and then reduced at the negative electrode to allow pre-doping, at least one compound selected from the group consisting of lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, and cesium carbonate is preferred, and at least one compound selected from the group consisting of lithium carbonate, sodium carbonate, and potassium carbonate is more preferred. Among these, lithium carbonate is preferred from the viewpoint of high capacity per unit weight. The alkali metal compound contained in the positive electrode coating solution may be one type, or may contain two or more types of alkali metal compounds.

[0064] In this embodiment, the composition may contain at least one alkali metal compound, where M is at least one selected from Li, Na, K, Rb, and Cs, and may include at least one oxide such as MO, hydroxide such as MOH, halide such as MF or MCl, or carboxylate such as RCOOM (where R represents H, an alkyl group, or an aryl group). In this embodiment, the composition may also contain at least one alkaline earth metal carbonate selected from the group consisting of BeCO, MgCO, CaCO, SrCO, and BaCO. In this embodiment, the composition may also contain at least one alkaline earth metal oxide, alkaline earth metal hydroxide, alkaline earth metal halide, or alkaline earth metal carboxylate.

[0065] The weight ratio A3 of the alkali metal compound in the positive electrode active material layer of the positive electrode precursor is preferably 10% by mass or more and 50% by mass or less. If A3 is 10% by mass or more, a sufficient amount of alkali metal ions can be pre-doped into the negative electrode, thereby increasing the capacity of the nonaqueous lithium-type storage element. If A3 is 50% or less, electronic conductivity in the positive electrode precursor can be increased, thereby efficiently decomposing the alkali metal compound.

[0066] When the positive electrode precursor contains two or more of the above alkali metal compounds or alkaline earth metal compounds in addition to the alkali metal compound, the positive electrode precursor is preferably produced so that the total amount of the alkali metal compounds and alkaline earth metal compounds is 10% by mass or more and 50% by mass or less relative to the positive electrode active material layer of the positive electrode precursor.

[0067] [Optional components of the positive electrode active material layer] The positive electrode active material layer of the positive electrode precursor in this embodiment may contain optional components such as a conductive filler, a binder, a dispersion stabilizer, and a pH adjuster, in addition to the positive electrode active material and the alkali metal compound, as needed.

[0068] The conductive filler may be a conductive carbonaceous material having higher conductivity than the positive electrode active material, such as ketjen black, acetylene black, vapor-grown carbon fiber, graphite, flake graphite, carbon nanotubes, graphene, graphene oxide, or a mixture thereof.

[0069] The amount of conductive filler mixed in the positive electrode active material layer of the positive electrode precursor is preferably 0 to 20 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the positive electrode active material. Mixing a conductive filler is preferable from the viewpoint of high input power. However, if the amount mixed exceeds 20 parts by mass, the content of the positive electrode active material in the positive electrode active material layer decreases, which is undesirable because it reduces the energy density per volume of the positive electrode active material layer.

[0070] The binder is not particularly limited, and examples thereof include PVdF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), polyimide, latex, styrene-butadiene copolymer, fluororubber, acrylic copolymer, polyacrylic acid, and polyglutamic acid. The amount of binder used is preferably 1 to 30 parts by mass per 100 parts by mass of the positive electrode active material. More preferably, it is 3 to 27 parts by mass, and even more preferably, it is 5 to 25 parts by mass. When the amount of binder is 1% by mass or more, sufficient electrode strength is achieved. On the other hand, when the amount of binder is 30 parts by mass or less, the ingress and egress of ions into and diffusion from the positive electrode active material are not hindered, and high input / output characteristics are achieved.

[0071] The dispersion stabilizer is not particularly limited, and examples thereof include PVP (polyvinylpyrrolidone), PVA (polyvinyl alcohol), and cellulose derivatives. The amount of the dispersion stabilizer used is preferably 0 to 10 parts by mass relative to 100 parts by mass of the positive electrode active material. When the amount of the dispersion stabilizer is 10 parts by mass or less, the ingress and egress of ions into and diffusion from the positive electrode active material are not inhibited, and high input / output characteristics are achieved.

[0072] When water is used as the solvent for the coating liquid, the addition of an alkali metal compound may make the coating liquid alkaline, so a pH adjuster may be added to the coating liquid as needed. The pH adjuster is not particularly limited, but examples thereof include hydrogen halides such as hydrogen fluoride, hydrogen chloride, and hydrogen bromide, halogen oxo acids such as hypochlorous acid, chlorous acid, and chloric acid, carboxylic acids such as formic acid, acetic acid, citric acid, oxalic acid, lactic acid, maleic acid, and fumaric acid, sulfonic acids such as methanesulfonic acid, benzenesulfonic acid, and p-toluenesulfonic acid, and acids such as nitric acid, sulfuric acid, phosphoric acid, boric acid, and carbon dioxide.

[0073] [Positive electrode current collector] The material for the positive electrode current collector according to this embodiment is not particularly limited as long as it has high electronic conductivity and is not susceptible to deterioration due to elution in the electrolytic solution or reaction with the electrolyte or ions, but metal foil is preferred. Aluminum foil is more preferred as the positive electrode current collector in the nonaqueous lithium-ion storage element according to this embodiment.

[0074] The metal foil may be a normal metal foil without irregularities or through holes, or may be a metal foil with irregularities that has been subjected to embossing, chemical etching, electrolytic deposition, blasting, or the like, or may be a metal foil with through holes such as expanded metal, punched metal, or etched foil. From the viewpoint of the pro-dope treatment described below, non-porous aluminum foil is more preferred, and it is particularly preferred that the surface of the aluminum foil is roughened.

[0075] The thickness of the positive electrode current collector is not particularly limited as long as it can sufficiently maintain the shape and strength of the positive electrode, but is preferably 1 to 100 μm, for example.

[0076] It is also preferable to provide an anchor layer containing a conductive material such as graphite, flake graphite, carbon nanotubes, graphene, ketjen black, acetylene black, or vapor-grown carbon fiber on the surface of the metal foil. By providing the anchor layer, electrical conduction between the positive electrode current collector and the positive electrode active material layer can be improved, resulting in lower resistance. The thickness of the anchor layer is preferably 0.1 μm or more and 5 μm or less per side of the positive electrode current collector.

[0077] [Production of positive electrode precursor] In this embodiment, the positive electrode precursor serving as the positive electrode of the nonaqueous lithium-ion battery element can be manufactured using known electrode manufacturing techniques for lithium-ion batteries, electric double layer capacitors, and the like. For example, a positive electrode active material, an alkali metal compound, and other optional components used as needed are dispersed or dissolved in water or an organic solvent to prepare a slurry coating solution, which is then applied to one or both sides of a positive electrode current collector to form a coating film, which is then dried to obtain a positive electrode precursor. The resulting positive electrode precursor may then be pressed to adjust the film thickness or bulk density of the positive electrode active material layer. Alternatively, a method is also possible in which the positive electrode active material, the alkali metal compound, and other optional components used as needed are dry-mixed without using a solvent, the resulting mixture is press-molded, and then attached to the positive electrode current collector using a conductive adhesive. Alternatively, the resulting mixture is hot-pressed onto the positive electrode current collector to form a positive electrode active material layer.

[0078] The coating solution for the positive electrode precursor may be prepared by dry-blending some or all of various material powders, including the positive electrode active material, followed by the addition of water or an organic solvent, and / or a liquid or slurry-like substance in which a binder, a dispersion stabilizer, or a pH adjuster is dissolved or dispersed therein. Alternatively, the coating solution may be prepared by adding various material powders, including the positive electrode active material, to a liquid or slurry-like substance in which a binder, a dispersion stabilizer, or a pH adjuster is dissolved or dispersed in water or an organic solvent. As a dry-blending method, for example, a ball mill may be used to premix the positive electrode active material and the alkali metal compound, and optionally a conductive filler, to coat the low-conductivity alkali metal compound with the conductive material. This facilitates decomposition of the alkali metal compound in the positive electrode precursor during the pre-doping step described below.

[0079] The preparation of the coating solution for the positive electrode precursor is not particularly limited, but preferably a disperser such as a homodisper, a multi-axis disperser, a planetary mixer, or a thin film rotary high-speed mixer can be used. To obtain a coating solution in a well-dispersed state, the coating solution is preferably dispersed at a peripheral speed of 1 m / s or more and 50 m / s or less. A peripheral speed of 1 m / s or more is preferred because various materials are well dissolved or dispersed. Furthermore, a peripheral speed of 50 m / s or less is preferred because various materials are not destroyed by heat or shear force due to dispersion, and re-aggregation does not occur.

[0080] The degree of dispersion of the coating liquid is preferably 0.1 μm or more and 100 μm or less, as measured with a particle gauge. The upper limit of the degree of dispersion is more preferably 80 μm or less, and even more preferably 50 μm or less. A particle size of 0.1 μm or less is less than the particle size of the powders of various materials, including the positive electrode active material, and is therefore undesirable because the materials are crushed during preparation of the coating liquid. Furthermore, a particle size of 100 μm or less allows stable coating without clogging during discharge of the coating liquid or streaks in the coating film.

[0081] The viscosity (ηb) of the coating solution for the positive electrode precursor is preferably 100 mPa·s or more and 10,000 mPa·s or less, more preferably 500 mPa·s or more and 7,000 mPa·s or less, and even more preferably 1,000 mPa·s or more and 4,000 mPa·s or less. A viscosity (ηb) of 100 mPa·s or more suppresses dripping during coating film formation, allowing for good control of the coating film width and thickness. Furthermore, a viscosity of 10,000 mPa·s or less allows for stable coating with minimal pressure loss in the coating solution flow path when using a coating machine, and also allows for control of the coating film thickness to the desired level.

[0082] The TI value (thixotropy index value) of the coating liquid is preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.5 or more. If the TI value is 1.1 or more, the width and thickness of the coating film can be well controlled.

[0083] The coating film of the positive electrode precursor is not particularly limited, but a coating machine such as a die coater, comma coater, knife coater, or gravure coater can be suitably used. The coating film may be formed by single-layer coating or multi-layer coating. In the case of multi-layer coating, the coating liquid composition may be adjusted so that the content of the alkali metal compound in each layer of the coating film is different. When applying the coating film to the positive electrode current collector, multi-line coating, intermittent coating, or multi-line intermittent coating may be used. In addition, sequential coating may be performed by coating one side of the positive electrode current collector and drying, and then coating the other side and drying, or simultaneous double-sided coating may be performed by simultaneously coating both sides of the positive electrode current collector with the coating liquid and drying.

[0084] The coating speed is preferably 0.1 m / min or more and 100 m / min or less, more preferably 0.5 m / min or more and 70 m / min or less, and even more preferably 1 m / min or more and 50 m / min or less. If the coating speed is 0.1 m / min or more, stable coating can be achieved. On the other hand, if the coating speed is 100 m / min or less, sufficient coating accuracy can be ensured.

[0085] The coating film of the positive electrode precursor is preferably dried using a drying method such as hot air drying or infrared (IR) drying, more preferably using far infrared rays, near infrared rays, or hot air at 80°C or higher. The coating film may be dried at a single temperature or by varying the temperature in multiple stages. Alternatively, a combination of multiple drying methods may be used. The drying temperature is preferably 25°C or higher and 200°C or lower, more preferably 40°C or higher and 180°C or lower, and even more preferably 50°C or higher and 160°C or lower. A drying temperature of 25°C or higher can sufficiently volatilize the solvent in the coating film. On the other hand, a drying temperature of 200°C or lower can suppress cracking of the coating film due to rapid solvent evaporation, uneven distribution of the binder due to migration, and oxidation of the positive electrode current collector or positive electrode active material layer.

[0086] A hydraulic press, vacuum press, or other press can be suitably used to press the positive electrode precursor. The thickness, bulk density, and electrode strength of the positive electrode active material layer can be adjusted by the press pressure, the gap between the press rolls, and the surface temperature of the press unit, as described below. The press pressure is preferably 0.5 kN / cm or more and 20 kN / cm or less, more preferably 1 kN / cm or more and 10 kN / cm or less, and even more preferably 2 kN / cm or more and 7 kN / cm or less. A press pressure of 0.5 kN / cm or more can sufficiently increase the electrode strength. On the other hand, a press pressure of 20 kN / cm or less can be adjusted to the desired thickness or bulk density of the positive electrode active material layer without causing bending or wrinkling in the positive electrode precursor. The gap between the press rolls can be set to any value depending on the thickness of the positive electrode precursor after drying to achieve the desired thickness or bulk density of the positive electrode active material layer. Furthermore, the press speed can be set to any speed that does not cause bending or wrinkling in the positive electrode precursor. The surface temperature of the press unit can be room temperature, or it can be heated as necessary. The lower limit of the surface temperature of the press part when heated is preferably at least 60°C below the melting point of the binder used, more preferably at least 45°C below the melting point of the binder, and even more preferably at least 30°C below the melting point of the binder. On the other hand, the upper limit of the surface temperature of the press part when heated is preferably at most 50°C above the melting point of the binder used, more preferably at most 30°C above the melting point of the binder, and even more preferably at most 20°C above the melting point of the binder. For example, when PVdF (polyvinylidene fluoride: melting point 150°C) is used as the binder, heating is preferably from 90°C to 200°C, more preferably from 105°C to 180°C, and even more preferably from 120°C to 170°C. Furthermore, when a styrene-butadiene copolymer (melting point 100°C) is used as the binder, it is preferable to heat the mixture to a temperature of 40°C or higher and 150°C or lower, more preferably 55°C or higher and 130°C or lower, and even more preferably 70°C or higher and 120°C or lower.

[0087] The melting point of the binder can be determined from the endothermic peak position in DSC (Differential Scanning Calorimetry). For example, using a PerkinElmer DSC7 differential scanning calorimeter, 10 mg of sample resin is placed in the measurement cell, and the temperature is raised from 30°C to 250°C at a rate of 10°C / min in a nitrogen gas atmosphere. The endothermic peak temperature during the temperature rise is the melting point.

[0088] Pressing may be performed multiple times while changing the conditions of the press pressure, gap, speed, and surface temperature of the press part.

[0089] When the positive electrode precursor is multi-line coated, it is preferable to slit it before pressing. If the multi-line coated positive electrode precursor is pressed without slitting, stress is applied to the current collector portion not coated with the positive electrode active material layer, causing wrinkles. Alternatively, the positive electrode precursor can be slit again after pressing.

[0090] The thickness of the positive electrode active material layer according to this embodiment is preferably 10 μm to 200 μm per side of the positive electrode current collector. The thickness of the positive electrode active material layer is more preferably 20 μm to 100 μm per side, and even more preferably 30 μm to 80 μm per side. A thickness of 10 μm or more can achieve sufficient charge / discharge capacity. On the other hand, a thickness of 200 μm or less can maintain low ion diffusion resistance within the electrode. Therefore, sufficient output characteristics can be obtained, and the cell volume can be reduced, thereby increasing the energy density. Note that when the current collector has through-holes or irregularities, the thickness of the positive electrode active material layer refers to the average thickness per side of the portion of the current collector that does not have through-holes or irregularities.

[0091] [Method for identifying alkali metal compounds in the positive electrode] <Quantitative determination of carbon materials, lithium transition metal oxides, and alkali metal compounds in the positive electrode active material layer> The method for quantifying the mass proportion A1 of the carbon material, the mass proportion A2 of the lithium transition metal oxide, and the mass proportion A3 of the alkali metal compound contained in the positive electrode active material layer is not particularly limited, but they can be quantified, for example, by the following method.

[0092] The area of ​​the positive electrode precursor to be measured is not particularly limited, but in order to reduce the variation in the measurement, a 5 cm 2 More than 200cm 2 Preferably it is less than 25cm 2 More than 150cm 2 The area is 5cm or less. 2 If the area is 200cm or more, the reproducibility of the measurement is ensured. 2 If the value is less than this, the sample is easy to handle.

[0093] First, the positive electrode precursor is cut to the above-mentioned area and vacuum-dried. The vacuum drying conditions are preferably, for example, a temperature of 100 to 200°C, a pressure of 0 to 10 kPa, and a time of 5 to 20 hours, so that the residual moisture content in the positive electrode precursor is 1% by mass or less. The residual moisture content can be quantified by the Karl Fischer method.

[0094] The weight (M0) of the positive electrode precursor obtained after vacuum drying is measured. The positive electrode precursor is then immersed in distilled water in an amount 100 to 150 times the weight of the positive electrode precursor for at least three days to dissolve the alkali metal compound into the water. It is preferable to cover the container during immersion to prevent the distilled water from volatilizing. After immersion for at least three days, the positive electrode precursor is removed from the distilled water and vacuum dried in the same manner as above. The weight (M1) of the resulting positive electrode precursor is measured. The positive electrode active material layer applied to one or both sides of the positive electrode current collector is then removed using a spatula, brush, paintbrush, or the like. The weight (M2) of the remaining positive electrode current collector is measured, and the mass proportion A3 of the alkali metal compound is calculated using the following formula (1): A3=(M0-M1) / (M0-M2)×100 (1) Formula Next, in order to calculate A1 and A2, the TG curve of the positive electrode active material layer obtained by removing the alkali metal compound is measured under the following conditions. Sample pan: platinum Gas: atmospheric air or compressed air Heating rate: 0.5℃ / min or less Temperature range: 25°C to 500°C (or higher) (50°C below the melting point of lithium transition metal oxide) The mass at 25°C on the obtained TG curve is designated as M3, and the mass at the first temperature above 500°C at which the mass loss rate becomes M3 x 0.01 / min or less is designated as M4.

[0095] Carbon materials are oxidized and burned when heated at temperatures below 500°C in an oxygen-containing atmosphere (e.g., air). On the other hand, lithium transition metal oxides do not lose mass even in an oxygen-containing atmosphere up to a temperature 50°C below their melting point. Therefore, the content A2 of the lithium transition metal oxide in the positive electrode active material layer can be calculated by the following formula (2). A2=(M4 / M3)×{1-(M0-M1) / (M0-M2)}×100 (2) formula The content A1 of the carbon material in the positive electrode active material layer can be calculated by the following formula (3). A1={(M3-M4) / M3}×{1-(M0-M1) / (M0-M2)}×100 (3) formula

[0096] Note that when a positive electrode active material layer contains multiple alkali metal compounds; when the positive electrode active material layer contains, in addition to alkali metal compounds, oxides such as MO, hydroxides such as MOH, halides such as MF and MCl, oxalates such as M(CO) and carboxylates such as RCOOM (wherein R is H, an alkyl group, or an aryl group), where M in the following formula is one or more selected from Na, K, Rb, and Cs; or when the positive electrode active material layer contains alkaline earth metal carbonates selected from BeCO, MgCO, CaCO, SrCO, and BaCO, or alkaline earth metal oxides, alkaline earth metal hydroxides, alkaline earth metal halides, alkaline earth metal oxalates, or alkaline earth metal carboxylates, the total amount of these is calculated as the amount of alkali metal compounds.

[0097] When the positive electrode active material layer contains a conductive material, a binder, a thickener, etc., the total amount of the carbon material and these materials is calculated as A1.

[0098] <Method for identifying alkali metals in electrodes> The method for identifying the alkali metal compound contained in the positive electrode is not particularly limited, but the alkali metal compound can be identified, for example, by the following method. The alkali metal compound is preferably identified by a combination of the following analytical techniques.

[0099] If the alkali metal compounds cannot be identified using the analytical method, other analytical methods are available: 7 Alkali metal compounds can also be identified using Li-solid-state NMR, XRD (X-ray diffraction), TOF-SIMS (time-of-flight secondary ion mass spectrometry), AES (Auger electron spectroscopy), TPD / MS (thermal evolved gas mass spectrometry), DSC (differential scanning calorimetry), etc.

[0100] [Scanning Electron Microscope-Energy Dispersive X-ray Analysis (SEM-EDX)] When the positive electrode active material does not contain a lithium transition metal oxide, alkali metal compounds and positive electrode active materials can be identified by oxygen mapping using SEM-EDX images of the positive electrode surface measured at 1000x to 4000x magnification. For example, SEM-EDX images can be measured at an acceleration voltage of 10 kV, an emission current of 10 μA, 256 × 256 pixel measurement, and 50 integration times. To prevent sample charging, surface treatment with gold, platinum, osmium, or the like can be performed using methods such as vacuum deposition or sputtering. For SEM-EDX image measurement, it is preferable to adjust the brightness and contrast so that no pixels reach the maximum brightness value in the mapping image and the average brightness value is within the range of 40% to 60% of the maximum brightness value. Particles containing bright areas binarized based on the average brightness value in the obtained oxygen mapping, which account for 50% or more of their area, are considered alkali metal compounds.

[0101] [Microscopic Raman spectroscopy] Alkali metal compounds and positive electrode active materials can be identified by Raman imaging of carbonate ions on the positive electrode surface, measured at a magnification of 1000x to 4000x. Measurement conditions include an excitation light of 532 nm, an excitation light intensity of 1%, a long working distance of the objective lens of 50x, a diffraction grating of 1800 gr / mm, a point scanning mapping method (slit 65 mm, binning 5 pix), 1 mm steps, an exposure time of 3 seconds per point, one integration, and a noise filter. The measured Raman spectrum shows peaks from 1071 to 1104 cm. -1 A linear baseline is set within the range, and the area is calculated assuming that positive values ​​from the baseline are carbonate ion peaks, and the frequency is integrated. At this time, the frequency for the carbonate ion peak area, which is obtained by approximating noise components with a Gaussian function, is subtracted from the carbonate ion frequency distribution.

[0102] [X-ray photoelectric spectroscopy (XPS)] By analyzing the electronic state of the positive electrode precursor using XPS, the bonding state of the compounds contained in the positive electrode precursor can be determined. Measurement conditions include, for example, a monochromatic AlKα X-ray source, an X-ray beam diameter of 100 μmφ (25 W, 15 kV), a narrow scan pass energy of 58.70 eV, charge neutralization, narrow scan sweeps of 10 (carbon, oxygen), 20 (fluorine), 30 (phosphorus), 40 (alkali metal), and 50 (silicon), and a narrow scan energy step of 0.25 eV. It is preferable to clean the surface of the positive electrode by sputtering before XPS measurement. For example, the positive electrode surface can be cleaned under sputtering conditions of an acceleration voltage of 1.0 kV, a 2 mm x 2 mm area, and 1 minute (1.25 nm / min in terms of SiO2). In the obtained XPS spectrum, the peak of Li1s binding energy 50-54 eV corresponds to LiO2 or Li-C bond, and the peak of 55-60 eV corresponds to LiF, Li2CO3, Li x PO y F z(where x, y, and z are integers between 1 and 6), the C1s bond energy peak of 285 eV corresponds to a C-C bond, the peak of 286 eV corresponds to a C-O bond, the peak of 288 eV corresponds to a CO-O bond, and the peak of 290 to 292 eV corresponds to a CO3 2- The C-F bond, O1s binding energy peak at 527-530 eV 2- (Li2O), and the peaks at 531-532 eV are CO, CO3, OH, and PO x (wherein x is an integer of 1 to 4), SiO x (wherein x is an integer of 1 to 4), and the peak at 533 eV is CO, SiO x (where x is an integer of 1 to 4), the peak at 685 eV of F1s binding energy corresponds to LiF, the peak at 687 eV corresponds to C—F bond, and Li x PO y F z (wherein x, y, and z are integers from 1 to 6), PF6 - For the binding energy of P2p, the peak at 133 eV is x (wherein x is an integer of 1 to 4), and the peaks of 134 to 136 eV are determined by PF x (where x is an integer of 1 to 6), the peak at the Si2p binding energy of 99 eV is Si silicide, and the peak at 101 to 107 eV is Si x O y (where x and y are any integers). If the peaks of the obtained spectrum overlap, it is preferable to separate the peaks by assuming a Gaussian function or a Lorentzian function and assign the spectrum. The alkali metal compounds present can be identified from the results of the measurement of the electronic state and the results of the ratio of the elements present obtained above.

[0103] [Ion Chromatography] The anion species eluted in the water can be identified by analyzing the distilled water wash solution from the positive electrode using ion chromatography. Ion exchange, ion exclusion, and reversed-phase ion-pair columns can be used. Detectors that can be used include electrical conductivity detectors, ultraviolet-visible absorbance detectors, and electrochemical detectors. Suppressor-based detectors, in which a suppressor is installed before the detector, and non-suppressor-based detectors, in which a solution with low electrical conductivity is used as the eluent without a suppressor, can also be used. Measurements can also be performed in combination with a mass spectrometer and / or a charged aerosol detector.

[0104] Once the column, eluent, and other conditions are determined, the sample retention time is constant for each ionic species, and the magnitude of the peak response differs for each ionic species but is proportional to the concentration. Qualitative and quantitative determination of ionic species is possible by measuring standard solutions of known concentrations with traceability in advance.

[0105] <Method for determining alkali metal elements: ICP-MS> The positive electrode precursor is acid-decomposed using a strong acid such as concentrated nitric acid, concentrated hydrochloric acid, or aqua regia, and the resulting solution is diluted with pure water to an acid concentration of 2% to 3%. The acid decomposition can also be performed by heating or pressurizing as appropriate. The resulting diluted solution is analyzed by ICP-MS, but it is preferable to add a known amount of an element as an internal standard. If the alkali metal element to be measured exceeds the upper limit of measurable concentration, it is preferable to further dilute the diluted solution while maintaining the acid concentration. Each element can be quantified based on the obtained measurement results using a calibration curve previously prepared using standard solutions for chemical analysis.

[0106] <Negative electrode> The negative electrode has a negative electrode current collector and a negative electrode active material layer present on one or both sides of the negative electrode current collector.

[0107] [Negative electrode active material layer] The negative electrode active material layer contains a negative electrode active material capable of absorbing and releasing alkali metal ions, and may further contain optional components such as a conductive filler, a binder, a dispersant, etc., as necessary.

[0108] [Negative electrode active material] The negative electrode active material may be a material capable of absorbing and releasing alkali metal ions. Specific examples include carbon materials, titanium oxides, silicon, silicon oxides, silicon alloys, silicon compounds, tin, and tin compounds. The carbon material content relative to the total amount of the negative electrode active material is preferably 50% by mass or more, and more preferably 70% by mass or more. While the carbon material content can be 100% by mass, from the viewpoint of obtaining the desired effect of the combined use of other materials, it is preferably 90% by mass or less, and may be 80% by mass or less. The upper and lower limits of the range of the carbon material content can be arbitrarily combined.

[0109] Examples of carbon materials include non-graphitizable carbon materials; graphitizable carbon materials; carbon black; carbon nanoparticles; activated carbon; artificial graphite; natural graphite; graphitized mesophase carbon microspheres; graphite whiskers; amorphous carbonaceous materials such as polyacene-based substances; carbonaceous materials obtained by heat-treating carbon precursors such as petroleum-based pitch, coal-based pitch, mesocarbon microbeads, coke, and synthetic resins (e.g., phenolic resins); pyrolysates of furfuryl alcohol resins or novolac resins; fullerenes; carbon nanophones; and composite carbon materials thereof.

[0110] [Composite carbon materials] The BET specific surface area of ​​the composite carbon material is 100m 2 / g or more 350m 2 / g or less, and more preferably 150m 2 / g or more 300m 2 / g or less. BET specific surface area is 100m 2 / g or more, the amount of alkali metal ions pre-doped can be made sufficiently large, allowing the negative electrode active material layer to be thin. 2If the average molecular weight is 1 / g or less, the coating property of the negative electrode active material layer is excellent.

[0111] The composite carbon material was used with lithium metal as the counter electrode, and the current value was 0.5 mA / cm at a measurement temperature of 25°C. 2 After constant current charging was performed until the voltage reached 0.01 V, the current was increased to 0.01 mA / cm 2 The initial charge capacity when constant-voltage charging is performed until the initial charge capacity reaches 100 mAh / g is preferably 300 mAh / g or more and 1,600 mAh / g or less, more preferably 400 mAh / g or more and 1,500 mAh / g or less, and even more preferably 500 mAh / g or more and 1,450 mAh / g or less per unit mass of the composite carbon material. If the initial charge capacity is 300 mAh / g or more, the amount of alkali metal ions pre-doped can be sufficiently large, so that high output characteristics can be obtained even when the negative electrode active material layer is thinned. Furthermore, if the initial charge capacity is 1,600 mAh / g or less, swelling and shrinkage of the composite carbon material when alkali metal ions are doped and undoped into the composite carbon material is reduced, and the strength of the negative electrode is maintained.

[0112] From the viewpoint of obtaining a good internal resistance value, the above-mentioned negative electrode active material is particularly preferably a composite porous material that satisfies the following conditions (1) and (2). (1) Mesopore volume (the amount of pores with a diameter of 2 nm to 50 nm) Vm1 (cm) calculated using the BJH method 3 / g) satisfies the condition 0.01≦Vm1<0.10. (2) Micropore volume (volume of pores with a diameter of less than 2 nm) Vm2 (cm) calculated using the MP method described above 3 / g) satisfies the condition 0.01≦Vm2<0.30.

[0113] The negative electrode active material is preferably in particulate form.

[0114] The particle diameter of the silicon, silicon oxide, silicon alloy, and silicon compound, as well as the tin and tin compound, is preferably 0.1 μm or more and 30 μm or less. If the particle diameter is 0.1 μm or more, the contact area with the electrolyte increases, thereby reducing the resistance of the nonaqueous lithium energy storage element. Furthermore, if the particle diameter is 30 μm or less, swelling and shrinkage of the negative electrode caused by doping and dedoping of alkali metal ions into and from the negative electrode during charge and discharge is reduced, thereby maintaining the strength of the negative electrode.

[0115] The silicon, silicon oxides, silicon alloys and silicon compounds, as well as tin and tin compounds, can be pulverized into fine particles by using a jet mill with a built-in classifier, an agitation ball mill, etc. The pulverizer is equipped with a centrifugal classifier, and the fine particles pulverized in an inert gas environment such as nitrogen or argon can be collected with a cyclone or dust collector.

[0116] The content of the negative electrode active material in the negative electrode active material layer of the negative electrode precursor is preferably 70 mass % or more, and more preferably 80 mass % or more, based on the total mass of the negative electrode active material layer.

[0117] [Other optional components of the negative electrode active material layer] The negative electrode active material layer according to this embodiment may contain optional components such as a binder, a conductive filler, a dispersant, and the like, in addition to the negative electrode active material, as needed.

[0118] Examples of binders that can be used include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide, fluororubber, latex, styrene-butadiene copolymer, fluororubber, and acrylic copolymer. The amount of binder used in the negative electrode active material layer is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, per 100 parts by mass of the negative electrode active material. If the amount of binder used is less than 1 part by mass per 100 parts by mass of the negative electrode active material, sufficient adhesion cannot be ensured between the current collector and the negative electrode active material layer in the negative electrode (precursor), resulting in increased interfacial resistance between the current collector and the active material layer. On the other hand, if the amount of binder used is more than 30 parts by mass per 100 parts by mass of the negative electrode active material, the binder will excessively cover the surface of the active material in the negative electrode (precursor), increasing the ion diffusion resistance within the active material pores.

[0119] The conductive filler is preferably made of a conductive carbonaceous material having higher conductivity than the negative electrode active material. Examples of such conductive fillers include ketjen black, acetylene black, vapor-grown carbon fiber, graphite, flake graphite, carbon nanotubes, graphene, graphene oxide, and mixtures thereof. The amount of conductive filler mixed in the negative electrode active material layer is preferably 20 parts by mass or less, more preferably 1 to 15 parts by mass, per 100 parts by mass of the negative electrode active material. While mixing the conductive filler in the negative electrode active material layer is preferable from the viewpoint of high input power, mixing the conductive filler in an amount greater than 20 parts by mass is undesirable because the content of the negative electrode active material in the negative electrode active material layer decreases, resulting in a decrease in energy density per volume.

[0120] The dispersion stabilizer is not particularly limited, and examples thereof include PVP (polyvinylpyrrolidone), PVA (polyvinyl alcohol), and cellulose derivatives. The amount of the dispersion stabilizer used is preferably 0 to 10 parts by mass relative to 100 parts by mass of the negative electrode active material. When the amount of the dispersion stabilizer is 10 parts by mass or less, the ingress and egress of ions into and diffusion from the negative electrode active material are not inhibited, and high input / output characteristics are achieved.

[0121] [Negative electrode current collector] The material constituting the negative electrode current collector according to this embodiment is preferably a metal foil that has high electronic conductivity and is not susceptible to degradation due to leaching into the electrolyte or reaction with the electrolyte or ions. Such metal foils are not particularly limited, and examples thereof include aluminum foil, copper foil, nickel foil, and stainless steel foil. Copper foil is preferred as the negative electrode current collector in the nonaqueous lithium storage element according to this embodiment. The metal foil may be a normal metal foil without irregularities or through holes, or may be a metal foil with irregularities obtained by embossing, chemical etching, electrolytic deposition, blasting, or the like, or may be a metal foil with through holes, such as expanded metal, punched metal, or etched foil.

[0122] The thickness of the negative electrode current collector is not particularly limited as long as it can sufficiently maintain the shape and strength of the negative electrode, and is, for example, 1 to 100 μm.

[0123] [Manufacturing of negative electrodes] The negative electrode comprises a negative electrode active material layer on one or both sides of a negative electrode current collector. In a typical embodiment, the negative electrode active material layer is adhered to the negative electrode current collector.

[0124] The negative electrode can be manufactured by known electrode manufacturing techniques for lithium ion batteries, electric double layer capacitors, etc. For example, various materials including the negative electrode active material are dispersed or dissolved in water or an organic solvent to prepare a slurry coating liquid, and this coating liquid is applied to one or both sides of a negative electrode current collector to form a coating film, which is then dried to obtain a negative electrode. The obtained negative electrode may then be pressed to adjust the film thickness or bulk density of the negative electrode active material layer.

[0125] The coating liquid may be prepared by dry-blending some or all of the various material powders, including the negative electrode active material, and then adding water or an organic solvent and / or a liquid or slurry-like substance in which a binder and a dispersion stabilizer are dissolved or dispersed therein. Alternatively, the coating liquid may be prepared by adding the various material powders, including the negative electrode active material, to a liquid or slurry-like substance in which a binder and a dispersion stabilizer are dissolved or dispersed in water or an organic solvent. While the method for preparing the coating liquid is not particularly limited, dispersers such as a homodisper, a multi-axis disperser, a planetary mixer, and a thin-film rotary high-speed mixer can be used. To obtain a coating liquid in a well-dispersed state, dispersion is preferably performed at a peripheral speed of 1 m / s to 50 m / s. A peripheral speed of 1 m / s or higher is preferred because the various materials are well dissolved or dispersed. A speed of 50 m / s or lower is preferred because the various materials are not destroyed by the heat or shear force generated by dispersion, and re-agglomeration does not occur.

[0126] The viscosity (ηb) of the coating liquid is preferably 500 mPa·s or more and 20,000 mPa·s or less, more preferably 1,000 mPa·s or more and 10,000 mPa·s or less, and even more preferably 1,500 mPa·s or more and 5,000 mPa·s or less. A viscosity (ηb) of 500 mPa·s or more suppresses dripping during coating film formation, allowing for good control of the coating film width and thickness. Furthermore, a viscosity of 20,000 mPa·s or less allows for stable coating with minimal pressure loss in the coating liquid flow path when using a coating machine, and allows for control of the coating film thickness to a desired level or less.

[0127] The TI value (thixotropy index value) of the coating liquid is preferably 1.1 or more, more preferably 1.2 or more, and even more preferably 1.5 or more. If the TI value is 1.1 or more, the coating film width and film thickness can be well controlled.

[0128] The coating film may be formed using any suitable coating machine, such as a die coater, comma coater, knife coater, or gravure coater. The coating film may be formed by single-layer coating or multi-layer coating. The coating speed is preferably 0.1 m / min or more and 100 m / min or less, more preferably 0.5 m / min or more and 70 m / min or less, and even more preferably 1 m / min or more and 50 m / min or less. A coating speed of 0.1 m / min or more ensures stable coating. On the other hand, a coating speed of 100 m / min or less ensures sufficient coating precision.

[0129] The method for drying the coating film is not particularly limited, but suitable drying methods include hot air drying and infrared (IR) drying. The coating film may be dried at a single temperature or at multiple stages with varying temperatures. Alternatively, a combination of multiple drying methods may be used. The drying temperature is preferably 25°C or higher and 200°C or lower, more preferably 40°C or higher and 180°C or lower, and even more preferably 50°C or higher and 160°C or lower. A drying temperature of 25°C or higher can sufficiently volatilize the solvent in the coating film. On the other hand, a drying temperature of 200°C or lower can suppress cracking of the coating film due to rapid solvent evaporation, uneven distribution of the binder due to migration, and oxidation of the negative electrode current collector and negative electrode active material layer.

[0130] The method for pressing the negative electrode is not particularly limited, but a press such as a hydraulic press or a vacuum press can be used. The film thickness, bulk density, and electrode strength of the negative electrode active material layer can be adjusted by the press pressure, gap, and surface temperature of the press unit, as described below. The press pressure is preferably 0.5 kN / cm or more and 20 kN / cm or less. It is more preferably 1 kN / cm or more and 10 kN / cm or less, and even more preferably 2 kN / cm or more and 7 kN / cm or less. A press pressure of 0.5 kN / cm or more can sufficiently increase the electrode strength. On the other hand, a press pressure of 20 kN / cm or less can be adjusted to the desired film thickness and bulk density of the negative electrode active material layer without causing bending or wrinkling in the negative electrode. The gap between the press rolls can be set to any value depending on the film thickness of the negative electrode after drying so as to achieve the desired film thickness and bulk density of the negative electrode active material layer. Furthermore, the press speed can be set to any speed that does not cause bending or wrinkling in the negative electrode. The surface temperature of the press unit can be room temperature, or it can be heated as necessary. The lower limit of the surface temperature of the press part when heated is preferably 60°C minus the melting point of the binder used, more preferably 45°C or higher, and even more preferably 30°C or higher. On the other hand, the upper limit of the surface temperature of the press part when heated is preferably 50°C or lower than the melting point of the binder used, more preferably 30°C or lower, and even more preferably 20°C or lower. For example, when PVdF (polyvinylidene fluoride: melting point 150°C) is used as the binder, heating is preferably from 90°C to 200°C. Heating is more preferably from 105°C to 180°C, and even more preferably from 120°C to 170°C. Furthermore, when styrene-butadiene copolymer (melting point 100°C) is used as the binder, heating is preferably from 40°C to 150°C. Heating is more preferably from 55°C to 130°C, and even more preferably from 70°C to 120°C.

[0131] [Negative electrode properties] The thickness of the negative electrode active material layer is preferably 5 μm or more and 100 μm or less per side, more preferably 10 μm or more and 60 μm or less. If this thickness is 10 μm or more, a good charge / discharge capacity can be exhibited. On the other hand, if this thickness is 100 μm or less, the cell volume can be reduced, thereby increasing the energy density. When the current collector has holes, the thickness of the negative electrode active material layer refers to the average value of the thickness per side of the portion of the current collector that does not have holes. In addition, the true density (cm) expressed as solid content (mass%) / material true density (g / cc) 3 / g) and 1 / electrode bulk density (g / cm 3 ) expressed as the actual volume (cm 3 / g), the porosity (%)=(1-true density / actual volume)*100 is preferably 50% or more.

[0132] [Measurement item] The BET specific surface area, average pore diameter, mesopore volume, and micropore volume used in this specification are values ​​determined by the following methods: A sample is vacuum-dried overnight at 200°C, and adsorption / desorption isotherms are measured using nitrogen as the adsorbate. Using the adsorption isotherm obtained here, the BET specific surface area is calculated by the BET multipoint method or BET single-point method, the average pore diameter is calculated by dividing the total pore volume per mass by the BET specific surface area, the mesopore volume is calculated by the BJH method, and the micropore volume is calculated by the MP method.

[0133] The BJH method is a calculation method commonly used to analyze mesopores, and was proposed by Barrett, Joyner, Halenda et al. (EP Barrett, LG Joyner and P. Halenda, J. Am. Chem. Soc., 73, 373 (1951)).

[0134] The MP method refers to a method for determining the micropore volume, micropore area, and micropore distribution using the "t-plot method" (BC Lippens, JH de Boer, J. Catalysis, 4319 (1965)), and is a method devised by M. Mikhail, Brunauer, and Bodor (RS Mikhail, S. Brunauer, EE Bodor, J. Colloid Interface Sci., 26, 45 (1968)).

[0135] The average particle size in this specification refers to the particle size at the point where the cumulative curve is 50% when the particle size distribution is measured using a particle size distribution analyzer and the total volume is taken as 100% (i.e., the 50% diameter (Median diameter)). This average particle size can be measured using a commercially available laser diffraction particle size distribution analyzer.

[0136] The doping amount of lithium ions in the negative electrode active material of the nonaqueous lithium-type electricity storage element at the time of shipment and after use in this specification can be determined, for example, as follows. First, the negative electrode active material layer in this embodiment is washed with ethyl methyl carbonate or dimethyl carbonate and air-dried, and then extracted with a mixed solvent of methanol and isopropanol to obtain an extract and the negative electrode active material layer after extraction. This extraction is typically performed in an Ar box at an ambient temperature of 23°C.

[0137] The amounts of lithium contained in the extracted solution and the negative electrode active material layer after extraction are respectively quantified using, for example, an ICP-MS (inductively coupled plasma mass spectrometry) and the sum thereof is calculated to determine the amount of lithium ions doped in the negative electrode active material. The obtained value is then assigned to the amount of negative electrode active material subjected to extraction to calculate the numerical value of the above unit.

[0138] The primary particle diameter in this specification can be obtained by photographing several fields of view of a powder using an electron microscope, measuring the particle diameters of approximately 2,000 to 3,000 particles in those fields of view using a fully automatic image processing device or the like, and taking the arithmetic average of these values ​​as the primary particle diameter. In this specification, the degree of dispersion is a value determined by a dispersion evaluation test using a particle gauge as specified in JIS K5600. Specifically, a sufficient amount of sample is poured into the deep end of a particle gauge with a groove of the desired depth corresponding to the particle size, allowing it to slightly overflow the groove. Next, the long side of the scraper is placed parallel to the width direction of the gauge, with the cutting edge in contact with the deep end of the groove of the particle gauge. While holding the scraper so that it is on the surface of the gauge, the scraper is dragged across the surface of the gauge at a uniform speed perpendicular to the long side of the groove to a depth of 0 over 1 to 2 seconds. Within 3 seconds after the scraper is finished, the scraper is observed by shining light at an angle of 20° to 30°, and the depth at which the particles appear in the groove of the particle gauge is read.

[0139] The viscosity (η b The TI value is determined by the following method. First, an E-type viscometer is used at a temperature of 25°C and a shear rate of 2 s -1 The stable viscosity (η a ) is obtained. Then, the shear rate is increased to 20 s -1 The viscosity (η b ) is obtained. Using the viscosity value obtained above, the TI value is calculated as TI value = η a / η b It is calculated by the formula: Shear rate 2s -1 From the 20s -1 When increasing the shear rate, the increase may be made in one step, or the shear rate may be increased in multiple steps within the above range, while appropriately obtaining the viscosity at each shear rate.

[0140] [Non-aqueous electrolyte] The electrolytic solution of this embodiment is a non-aqueous electrolytic solution. That is, this electrolytic solution contains a non-aqueous solvent described below. The non-aqueous electrolytic solution preferably contains 0.5 mol / L or more of a lithium salt based on the total amount of the non-aqueous electrolytic solution. That is, the non-aqueous electrolytic solution preferably contains lithium ions as an electrolyte.

[0141] [Lithium salt] In the nonaqueous electrolyte of this embodiment, as the lithium salt, for example, (LiN(SO2F)2), LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C2F5), LiN(SO2CF3)(SO2C2F4H), LiC(SO2F)3, LiC(SO2CF3)3, LiC(SO2C2F5)3, LiCF3SO3, LiC4F9SO3, LiPF6, LiBF4, etc. can be used alone or in combination of two or more. Since high conductivity can be achieved, the nonaqueous electrolyte preferably contains at least one selected from the group consisting of LiPF6, LiN(SO2F)2, and LiBF4, and more preferably contains LiPF6 and / or LiBF4 and LiN(SO2F)2.

[0142] The lithium salt concentration in the nonaqueous electrolyte solution is preferably 0.5 mol / L or more, more preferably 0.5 mol / L or more and 2.0 mol / L or less, based on the total amount of the nonaqueous electrolyte solution. If the lithium salt concentration is 0.5 mol / L or more, sufficient anions are present, allowing the capacity of the energy storage device to be sufficiently high. Furthermore, if the lithium salt concentration is 2.0 mol / L or less, this is preferable because it can prevent undissolved lithium salt from precipitating in the nonaqueous electrolyte solution and the viscosity of the nonaqueous electrolyte solution from becoming too high, preventing a decrease in conductivity and a decrease in output characteristics.

[0143] The nonaqueous electrolyte solution of this embodiment preferably contains LiN(SO2F)2 at a concentration of 0.1 mol / L to 1.5 mol / L, based on the total volume of the nonaqueous electrolyte solution. The LiN(SO2F)2 concentration is more preferably 0.4 mol / L to 1.2 mol / L. A LiN(SO2F)2 concentration of 0.1 mol / L or higher increases the ionic conductivity of the nonaqueous electrolyte solution, and an appropriate amount of electrolyte film is deposited at the negative electrode interface, thereby reducing gas generation due to decomposition of the nonaqueous electrolyte solution. On the other hand, a concentration of 1.5 mol / L or lower prevents precipitation of electrolyte salt during charge and discharge, and prevents an increase in the viscosity of the nonaqueous electrolyte solution even after a long period of time.

[0144] [Non-aqueous solvent] The non-aqueous electrolyte solution of this embodiment preferably contains a cyclic carbonate as a non-aqueous solvent. The inclusion of a cyclic carbonate in the non-aqueous electrolyte solution is advantageous in that it dissolves a lithium salt at a desired concentration and deposits an appropriate amount of a lithium compound on the positive electrode active material layer. Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, vinylene carbonate, and fluoroethylene carbonate.

[0145] The total content of the cyclic carbonate is preferably 15% by mass or more, more preferably 20% by mass or more, based on the total amount of the non-aqueous electrolyte. When the total content is 15% by mass or more, it is possible to dissolve a lithium salt at a desired concentration, and high lithium ion conductivity can be achieved. Furthermore, it is possible to deposit an appropriate amount of lithium compound on the positive electrode active material layer, and it is possible to suppress oxidative decomposition of the non-aqueous electrolyte.

[0146] The nonaqueous electrolyte solution of this embodiment preferably contains, as a nonaqueous solvent, chain carbonate compounds dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC). The volume ratio of the ethyl methyl carbonate to the dimethyl carbonate (DMC / EMC) is preferably 0.5 to 8.0, more preferably 0.8 to 6.0, and even more preferably 1.0 to 4.0. When the DMC / EMC ratio is 0.5 or more, the viscosity of the nonaqueous electrolyte solution can be reduced, and high lithium ion conductivity can be achieved. When the DMC / EMC ratio is 8.0 or less, the melting point of the mixed solvent can be kept low, and high input / output characteristics can be achieved even in low-temperature environments.

[0147] The nonaqueous electrolyte solution of this embodiment may contain other chain carbonates as the nonaqueous solvent. Examples of other chain carbonates include dialkyl carbonate compounds such as diethyl carbonate, dipropyl carbonate, and dibutyl carbonate. The dialkyl carbonate compounds are typically unsubstituted.

[0148] The total content of the chain carbonate is preferably 30% by mass or more, more preferably 35% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, based on the total amount of the non-aqueous electrolyte solution. If the content of the chain carbonate is 30% by mass or more, the viscosity of the non-aqueous electrolyte solution can be reduced, and high lithium ion conductivity can be achieved. If the total concentration is 95% by mass or less, the non-aqueous electrolyte solution can further contain the additives described below.

[0149] [Additives] The nonaqueous electrolyte solution of the present embodiment may further contain an additive. The additive is not particularly limited, and examples thereof include sulfur-containing compounds, phosphate ester compounds, acyclic fluorine-containing ethers, cyclic phosphazenes, fluorine-containing cyclic carbonates, cyclic carbonate esters, cyclic carboxylic acid esters, and cyclic acid anhydrides, which may be used alone or in combination of two or more.

[0150] Among these, it is preferable to contain an additive selected from sulfur-containing compounds selected from compounds represented by the following general formulas (1-2) to (1-6), phosphate ester compounds, and acyclic fluorine-containing ethers. [ka] {R in general formula (1-2) 1 ~R 4 each independently represents a hydrogen atom, a halogen atom, a formyl group, an acetyl group, a nitrile group, an acetyl group, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, or an alkyl ester having 1 to 6 carbon atoms.} {R in general formula (1-3) 9 ~R 14 each independently represents at least one selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, and a halogenated alkyl group having 1 to 12 carbon atoms, and may be the same or different; and n is an integer of 0 to 3. {R in general formula (1-4) 15 ~R 20 each independently represents at least one selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, and a halogenated alkyl group having 1 to 12 carbon atoms, and may be the same or different; and n is an integer of 0 to 3. {R in general formula (1-5) 21 ~R 26 each independently represents one selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, and a halogenated alkyl group having 1 to 12 carbon atoms, and may be the same or different.} {R in general formula (1-6) 27 ~R 30 each independently represents at least one selected from the group consisting of a hydrogen atom, a halogen atom, an alkyl group having 1 to 12 carbon atoms, and a halogenated alkyl group having 1 to 12 carbon atoms, and may be the same or different; and n is an integer of 0 to 3.

[0151] It is preferable that the non-aqueous electrolyte solution contains a sulfur-containing compound selected from the compounds represented by general formulas (1-2) to (1-6). More preferably, the compound represented by general formula (1-2) is thiophene, 2-methylthiophene, 3-methylthiophene, 2-cyanothiophene, 3-cyanothiophene, 2,5-dimethylthiophene, 2-methoxythiophene, 3-methoxythiophene, 2-chlorothiophene, 3-chlorothiophene, 2-acetylthiophene, or 3-acetylthiophene, and the sultone compound represented by general formula (1-3) is 1,3-propane sultone, 2,4-butane sultone, 1,4- butane sultone, 1,3-butane sultone, or 2,4-pentane sultone; the sultone compound represented by general formula (1-4) is 1,3-propene sultone or 1,4-butene sultone; the compound represented by general formula (1-5) is 3-sulfolene; and the cyclic sulfite compound represented by general formula (1-6) is ethylene sulfite, 1,2-propylene sulfite, or 1,3-propylene sulfite. It is more preferable that one or more compounds selected from these are contained in the nonaqueous electrolytic solution.

[0152] The total content of sulfur-containing compounds in the nonaqueous electrolyte solution of the nonaqueous lithium-type storage element of this embodiment is preferably 0.1% by mass or more and 5% by mass or less, based on the total amount of the nonaqueous electrolyte solution. When the total content of sultone compounds in the nonaqueous electrolyte solution is 0.1% by mass or more, decomposition of the nonaqueous electrolyte solution at high temperatures can be suppressed, thereby suppressing gas generation. On the other hand, when this total content is 5% by mass or less, a decrease in the ionic conductivity of the nonaqueous electrolyte solution can be suppressed, thereby maintaining high input / output characteristics. Furthermore, from the viewpoint of achieving both high input / output characteristics and durability, the content of sultone compounds present in the nonaqueous electrolyte solution of the nonaqueous lithium-type storage element is preferably 0.3% by mass or more and 4% by mass or less, more preferably 0.5% by mass or more and 3% by mass or less.

[0153] <Separator> The positive electrode precursor and the negative electrode are stacked with a separator interposed therebetween, or are stacked and wound together, to form an electrode stack or an electrode wound body having the positive electrode precursor, the separator, and the negative electrode.

[0154] As the separator, separators used in lithium ion secondary batteries, electric double layer capacitors, lithium ion capacitors, etc. can be suitably used.

[0155] The separator in this embodiment is preferably a separator containing at least one selected from the group consisting of polyolefin, cellulose, and aramid resin. Examples of the separator in this embodiment include a separator containing a polyolefin microporous membrane, a separator that is a laminate having a film made of inorganic fine particles on at least one surface of a polyolefin microporous membrane, a separator that is a laminate having a coating layer containing an aramid resin on at least one surface of a polyolefin microporous membrane, and a separator that contains cellulose nonwoven paper.

[0156] Examples of polyolefins include polyethylene, polypropylene, etc. The separator may contain organic or inorganic fine particles inside.

[0157] <Method of manufacturing a non-aqueous lithium-type energy storage element> The manufacturing method of the nonaqueous lithium-type storage element of this embodiment relates to a nonaqueous lithium-type storage element configured by housing the electrode stack or electrode wound body described below in the above-mentioned outer casing together with the nonaqueous electrolyte solution described above.

[0158] The method for producing the nonaqueous lithium-ion storage element according to this embodiment includes, for example, the following steps: (1) preparing a plurality of laminates obtained by laminating a positive electrode precursor containing a positive electrode active material made of a carbon material and lithium carbonate, and a negative electrode containing a negative electrode active material capable of absorbing and releasing lithium ions, with a separator interposed therebetween, and housing the laminates in each of a plurality of exterior bodies; (2) a liquid injection step of injecting a non-aqueous electrolyte solution containing lithium ions into each of the exterior bodies; (3) a storage element precursor formation step of electrically bonding a plurality of exterior bodies to obtain a non-aqueous lithium-ion storage element precursor; (4) a first voltage application step of dividing the total number of the plurality of exterior bodies into an exterior body group I, which comprises 30% to 70% of the total number of the plurality of exterior bodies, and an exterior body group II, arranging the exterior body groups I and II so that the maximum number of consecutively adjacent exterior bodies belonging to the exterior body group II is 0% to 10% of the total number of the plurality of exterior bodies, and applying a voltage to the exterior body group I; and (5) a second voltage application step of applying a voltage to the outer casing group II after a predetermined delay time has elapsed since the first voltage application step; a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution are housed in each of the multiple exterior bodies, and the multiple exterior bodies are electrically connected to each other.

[0159] In the method for producing a nonaqueous lithium-ion battery element according to this embodiment, as described above, a positive electrode and its material, a negative electrode and its material, a separator and its material, a nonaqueous electrolyte and its material, etc. may be used. The outer casing and its material will be described later. If desired, the method for producing a nonaqueous lithium-ion battery element may further include steps other than steps (1) to (5) or steps known in the art, as described later.

[0160] <Secondary drying of electrodes> The residual solvent in the positive electrode precursor and the negative electrode can be further reduced by secondary drying. Secondary drying is preferably performed using methods such as hot air drying, infrared (IR) drying, and vacuum drying. Far-infrared drying, hot air drying, and vacuum drying are more preferred, and a combination of multiple drying methods may also be used. Secondary drying may be performed at a single temperature or at multiple stages with varying temperatures. Hot air drying and infrared (IR) drying can be performed using a roll-to-roll method, eliminating the need to individually transport long electrodes and improving mass productivity. Infrared (IR) drying allows for efficient drying in a short time because energy radiated from a heat source is directly directed toward the material to be dried, rather than heat transfer through the atmosphere as in convection. The drying oven does not need to be filled with air; it can easily be filled with an inert gas to prevent oxidation of the material to be dried. To prevent oxidation and eliminate potential flammable or explosive elements, it is preferable to maintain the oxygen concentration in the drying oven below 20% by supplying and exhausting an inert gas. In addition, in the case of vacuum drying, the boiling point of the solvent decreases under reduced pressure, accelerating the evaporation rate. -5 The pressure is preferably from 0.1 Pa to 10 Pa, and more preferably from 0.1 Pa to 10 Pa. -5 If the pressure is 1000 Pa or higher, the cost of the equipment can be reduced. On the other hand, if the pressure is 1000 Pa or lower, the boiling point of the solvent is lowered and the evaporation rate is sufficiently accelerated, allowing for efficient drying.

[0161] The secondary drying temperature of the positive electrode precursor is preferably 60°C or higher and 250°C or lower, more preferably 65°C or higher and 240°C or lower, and even more preferably 70°C or higher and 235°C or lower. If the drying temperature is 60°C or higher, the solvent remaining in the positive electrode active material layer can be efficiently reduced. On the other hand, if the drying temperature is 250°C or lower, slippage of the positive electrode active material layer due to embrittlement of the binder can be suppressed.

[0162] The secondary drying temperature for the negative electrode is preferably 60°C or higher and 200°C or lower, more preferably 65°C or higher and 190°C or lower, and even more preferably 70°C or higher and 180°C or lower. A drying temperature of 60°C or higher can efficiently reduce the amount of solvent remaining in the negative electrode active material layer. On the other hand, a drying temperature of 200°C or lower can suppress the sliding of the negative electrode active material layer due to embrittlement of the binder and the oxidation of the negative electrode current collector foil.

[0163] After secondary drying, the positive electrode precursor and the negative electrode are preferably stored in a dry environment with a dew point of −30° C. or less to avoid adsorption of moisture from the atmosphere.

[0164] <Measurement of remaining solvent amount> The residual solvent amount in this specification is a value determined by the following method. The positive electrode precursor and current collector are cut into 80 mm x 80 mm pieces and weighed using an electronic balance. The resulting measurements are designated as weights W1 [g] and W2 [g], respectively. Next, the surface is heated and dried at 170°C for 5 minutes using a heat-dry moisture meter. If a positive electrode active material layer is applied to both sides, the back side is also heated and dried at 170°C for 5 minutes. After heat drying, the positive electrode precursor is transferred to an electronic balance, and its weight W3 [g] is recorded 10 seconds after the end of heat drying. The residual solvent amount is calculated using the following formula: Residual solvent amount = {(W1-W3) / (W1-W2)} x 100 (%)

[0165] <Residual solvent amount> In this specification, when the solvent is water, the residual solvent amount is preferably 0.0010% by mass or more and 7.0% by mass or less, and more preferably 0.005% by mass or more and 3.0% by mass or less. If it is 0.0010% by mass or more, the positive electrode active material layer will not peel off and will maintain a moderate strength. On the other hand, if it is 7.0% by mass or less, a good energy density can be obtained. Furthermore, when the solvent contains an organic solvent, it is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.5% by mass or more and 6% by mass or less. If it is 0.1% by mass or more, the positive electrode active material layer will not peel off and will maintain a moderate strength. On the other hand, if it is 10% by mass or less, a good energy density can be obtained.

[0166] <Assembly> In connection with step (1), the assembly step typically involves stacking the positive electrode precursor and negative electrode cut into sheet shapes with a separator interposed therebetween to obtain an electrode laminate (sometimes simply referred to as a "laminate" in this specification), which are then electrically bonded, for example, by connecting a positive electrode terminal and a negative electrode terminal, and optionally, lead wires, tabs, electric wires, connectors, etc., to the electrode laminate. Alternatively, the positive electrode precursor and negative electrode are stacked and wound with a separator interposed therebetween to obtain an electrode wound body, which are then electrically integrated, for example, by connecting a positive electrode terminal and a negative electrode terminal, and optionally, lead wires, tabs, electric wires, connectors, etc., to the electrode wound body. The electrode wound body may be cylindrical or flat in shape.

[0167] The method for connecting the positive electrode terminal and the negative electrode terminal is not particularly limited, but may be resistance welding, ultrasonic welding, or the like.

[0168] [Storage in exterior body] In relation to step (1), the electrode laminate or electrode wound body is preferably housed in an exterior body such as a metal can or a laminate packaging material, and sealed with only one opening remaining. The method for sealing the exterior body is not particularly limited, and when a laminate packaging material is used, methods such as heat sealing and impulse sealing can be used.

[0169] In this embodiment, from the viewpoint of steps (1), (4), and (5), it is preferable to prepare a plurality of exterior bodies, such as metal cans or laminate packaging materials, and it is more preferable that each of the plurality of exterior bodies has a front surface and a back surface. In this specification, the front surface of the exterior body refers to the surface on which the positive electrode tab is observed on the left side when viewed from the front.

[0170] [Drying] The electrode laminate or electrode wound body housed in the outer casing is preferably dried to remove the remaining solvent. The drying method is not limited, and drying by vacuum drying or the like is possible. The remaining solvent is preferably 1.5 mass% or less per mass of the positive electrode active material layer or the negative electrode active material layer. If the remaining solvent is 1.5 mass% or less, the self-discharge characteristics and cycle characteristics are less likely to deteriorate, which is preferable.

[0171] [Pressure] It is preferable to apply pressure from both sides of the exterior of the package housing the dried electrode laminate or electrode wound body in a direction perpendicular to the electrode surface. 2 More than 1000kgf / cm 2 Preferably less than 0.01kgf / cm 2 More than 100kgf / cm 2 Less than 0.01 kgf / cm is more preferable. 2 More than 30kgf / cm 2 More preferably, the pressure is 0.01 kgf / cm or less. 2 If the above conditions are met, distortions in the positive electrode precursor and the negative electrode are corrected by pressure, and the distance between the opposing positive electrode precursor and the negative electrode becomes uniform within the plane. This allows lithium doping to be carried out uniformly within the plane in the lithium doping step, and improves durability, which is preferable.

[0172] Any tool capable of applying pressure may be used as a means for applying pressure from the outside of the exterior body containing the dried electrode laminate or electrode wound body. As an example, a pair of flat metal plates may be prepared, aligned with the surface of the electrode laminate, and the four corners of the metal plates may be screwed together to apply pressure.

[0173] [Pressure measurement method] The pressure is measured using the I-SCAN surface pressure distribution measurement system (manufactured by Nitta Corporation). The sensor sheet used to measure the surface pressure preferably has an area that covers the entire pressure surface of the exterior body. For example, if the pressure surface is 60 mm long x 100 mm wide, an I-SCAN100 sensor (measurement surface dimensions: 112 mm x 112 mm) can be used.

[0174] The sensor sheet is disposed between the main surface of the exterior body and a pair of jigs having pressure surfaces.

[0175] The maximum measurement pressure of the sensor sheet is preferably equal to or greater than the maximum pressure applied to the exterior body, but is preferably three times or less than the maximum pressure. For example, if the maximum pressure applied to the exterior body is 5 kgf / cm 2 In this case, the maximum measurement pressure of the sensor sheet is 5kgf / cm 2 Above, 15kgf / cm 2 The following is preferable, so for example, the sensor sheet should be I-SCAN100(R) (maximum measurement pressure: 13 kgf / cm 2 It is preferable to use a sensor sheet having a maximum measurement pressure that is equal to or greater than the maximum pressure applied to the exterior body and is equal to or less than three times the maximum pressure, since this allows for accurate measurement of the in-plane pressure applied to the exterior body.

[0176] The number of sensors on the sensor sheet is preferably 400 points (20 points vertically × 20 points horizontally) or more, and more preferably 900 points or more (30 points vertically × 30 points horizontally). For example, when the pressure area S1 is 60 mm vertically × 100 mm horizontally (60 cm 2 ), I-SCAN100 sensor (measurement area S s :112mm×112mm=125.44cm 2 By applying the 1936 sensor points, the number of sensors used on the entire pressure surface is S1 / S s × 1936 points = 926 points, which is preferable.

[0177] In this specification, the unit of pressure is kgf / cm 2is used as an example, but any unit that indicates pressure may be used, such as Pa, mmHg, Bar, or atm.

[0178] The data obtained by I-SCAN as described above is not used as data for evaluating pressure unevenness within the surface, as it is easy to detect excessive pressure unrelated to the actual pressure force at the edges or corners of the jig due to the influence of burrs on the jig. Specifically, of all the pressure data measured within the pressure surface, three points of data on the four sides are not used as data. For example, if the data within the pressure surface is 44 points vertically by 30 points horizontally, the first three points of the row and the last three points of the row are deleted from the 44 points vertically, and the first three points of the column and the last three points of the column are deleted from the 30 points horizontally, and the pressure distribution within the surface is obtained using this data. The average value P of the obtained pressure distribution is avg (Equation (4) below) is the pressure applied to the exterior body.

number

[0179] <Injection, impregnation, sealing process> After the assembly process is completed, in connection with step (2), a nonaqueous electrolyte solution is injected into the electrode stack or electrode winding housed in the outer casing. The injection method can be a method of injecting the electrode stack or electrode winding under atmospheric pressure or reduced pressure, with injection under reduced pressure being preferred. Injecting the electrolyte under reduced pressure can shorten the injection process time and improve production efficiency. Furthermore, the positive electrode, negative electrode, and separator can be uniformly impregnated with the nonaqueous electrolyte solution.

[0180] When at least a portion of the positive electrode, negative electrode, and separator is not immersed in a nonaqueous electrolyte solution, the lithium compounds present in the portion of the positive electrode precursor not immersed in the nonaqueous electrolyte solution, or in the portion of the negative electrode not immersed in the nonaqueous electrolyte solution and the portion of the positive electrode precursor facing the separator remain undecomposed during the lithium doping process described below. As a result, when a storage device in which the nonaqueous electrolyte solution has sufficiently penetrated into the pores of the positive electrode, negative electrode, and separator is exposed to high temperature and high voltage, a decomposition reaction of the lithium compounds occurs, generating gas. Furthermore, since the doping proceeds unevenly, in-plane doping spots and localized lithium (Li) deposition occur, resulting in increased resistance, reduced durability, and reduced yield of the resulting nonaqueous lithium-type storage device. Examples of storage devices in which the nonaqueous electrolyte solution has sufficiently penetrated into the pores of the positive electrode, negative electrode, and separator include completed storage devices and storage devices that have been used for a long time.

[0181] The injection is preferably carried out under reduced pressure of -10 kPa to -1000 kPa, more preferably -50 kPa to -300 kPa, based on atmospheric pressure. Injecting the solution in an environment of -10 kPa or less based on atmospheric pressure allows the positive electrode, negative electrode, and separator to be uniformly impregnated with the nonaqueous electrolyte solution. On the other hand, an environment of -1000 kPa or more based on atmospheric pressure suppresses evaporation of the nonaqueous solvent in the electrolyte solution during injection, preventing changes in the composition of the nonaqueous electrolyte solution and stabilizing the characteristics of the resulting nonaqueous lithium-type storage element.

[0182] The temperature of the nonaqueous electrolyte solution during injection is preferably 5°C to 60°C, more preferably 15°C to 45°C. If the temperature of the nonaqueous electrolyte solution during injection is 5°C or higher, the viscosity of the nonaqueous electrolyte solution can be prevented from increasing, and the positive electrode, negative electrode, and separator can be uniformly impregnated with the nonaqueous electrolyte solution. On the other hand, if the temperature of the nonaqueous electrolyte solution during injection is 60°C or lower, evaporation of the nonaqueous solvent in the nonaqueous electrolyte solution during injection can be prevented, and changes in the composition of the nonaqueous electrolyte solution can be prevented, thereby stabilizing the characteristics of the resulting nonaqueous lithium-type storage element.

[0183] After the injection step, it is desirable to further perform impregnation so that the positive electrode, negative electrode, and separator are sufficiently immersed in the nonaqueous electrolyte. The impregnation method is not particularly limited, but for example, a method can be used in which the electrode laminate or electrode wound body after injection is placed in a reduced pressure chamber with the outer casing open, the chamber is reduced in pressure using a vacuum pump, and the pressure is returned to atmospheric pressure. After the injection step and the impregnation step, if a laminate packaging material is used, the electrode laminate or electrode wound body with the outer casing open is sealed while being reduced in pressure to be sealed. If a metal can is used, a sealing method such as welding or crimping is used.

[0184] In connection with the energy storage device precursor formation step (3), a plurality of outer casings each contain an electrode stack or electrode winding and a non-aqueous electrolyte, and the plurality of outer casings are electrically integrated to obtain a non-aqueous lithium-ion energy storage device precursor. In this specification, the non-aqueous lithium-ion energy storage device precursor refers to the state of the energy storage device before the doping step is performed. Electrical integration can be achieved by means of welding (e.g., resistance welding, ultrasonic welding), interlocking, soldering, or crimping, using, for example, a positive electrode terminal, a negative electrode terminal, lead wires, tabs, electric wires, connectors, screws, solder, jigs, or the like.

[0185] In step (3), from the viewpoint of the effectiveness of subsequent steps, it is preferable to arrange the multiple exterior bodies so that one of the front or rear surfaces of one exterior body faces one of the front or rear surfaces of another exterior body, and then electrically connect the multiple exterior bodies.

[0186] [Re-pressurize] After the injection, it is preferable to increase the pressure applied from the outside of the exterior body. The pressure is 0.1 kgf / cm 2 More than 1000kgf / cm 2 Less than 0.5kgf / cm is preferable. 2 More than 100kgf / cm 2 Less than 1kgf / cm is more preferable. 2 More than 10kgf / cm 2 More preferably, the pressure is 0.1 kgf / cm or less. 2When the pressure is 1000 kgf / cm or more, distortions in the positive electrode precursor and the negative electrode are corrected by the pressure, and the distance between the facing positive electrode precursor and the negative electrode becomes uniform within the plane, so that lithium doping is uniform within the plane during the lithium doping step, and durability is improved, which is preferable. 2 If the pressure is less than this, excessive pressure is not applied to the electrode laminate or the electrode wound body, and the constituent materials, that is, the positive electrode precursor, the negative electrode, and the separator, are not damaged, which is preferable.

[0187] <Doping process> A preferred operation of lithium doping is to apply a voltage between the positive electrode precursor and the negative electrode, decompose the lithium compound in the positive electrode precursor to release lithium ions, and reduce the lithium ions at the negative electrode, thereby pre-doping the negative electrode active material layer with liolium ions. Specifically, a method can be used in which a constant current is applied at the beginning of lithium doping to increase the voltage, and after reaching a desired voltage, a constant voltage is applied.

[0188] During lithium doping, gases such as CO2 are generated as the lithium compound in the positive electrode precursor decomposes. Therefore, when applying voltage, it is preferable to take measures to release the generated gas to the outside of the exterior body. Examples of such measures include applying voltage with a portion of the exterior body open; or applying voltage with a suitable gas release means, such as a gas vent valve or gas permeable film, already installed in a portion of the exterior body. Furthermore, when applying voltage, heat is generated as the lithium compound decomposes. Therefore, when applying voltage, it is preferable to take measures to appropriately control the generated heat. In particular, when doping multiple cells simultaneously, it is necessary to control the heat of decomposition in order to promote lithium ion doping into the negative electrode, obtain excellent input / output characteristics, and prevent micro-short circuits. One such measure is to use a unit described below to stagger the timing of voltage application to disperse the heat generation peak.

[0189] [Applied voltage] The voltage applied during the constant voltage doping with lithium is preferably 4.4 V or more and 4.8 V or less, more preferably 4.4 V or more and 4.6 V or less. A voltage of 4.4 V or more during the lithium doping is preferable because the lithium compound contained in the positive electrode precursor decomposes efficiently and lithium is released into the non-aqueous electrolyte. A voltage of 4.8 V or less is preferable because the withstand voltage of the separator exceeds the potential difference between the positive and negative electrodes, and micro-short circuits can be suppressed by the lithium doping.

[0190] [unit] When multiple nonaqueous lithium-ion storage element precursors are simultaneously doped, a unit consisting of multiple connected storage element precursors is used. The unit is equipped with a mechanism for applying pressure to both sides of the exterior body of the storage element precursor with an interlayer plate. The interlayer plate is preferably made primarily of one of aluminum, iron, and copper. Aluminum, iron, or copper has a large heat capacity and can store heat generated during doping, thereby mitigating heat accumulation in the storage element precursor. Furthermore, the surface of the interlayer plate is preferably electrically insulated to prevent problems such as external short circuits in the storage element. For example, if the interlayer plate is made of aluminum, the surface can be anodized. The thickness of the interlayer plate, which represents the distance between adjacent storage element precursors, is preferably 5 mm or more and 20 mm or less. A thickness of 5 mm or more can reduce thermal interference between adjacent storage element precursors. A thickness of 20 mm or less can reduce the size of the unit during manufacturing. The number of energy storage element precursors per unit is preferably 5 to 50, and more preferably 10 to 40. If the number of energy storage element precursors is 5 or more per unit, the number of units during production can be reduced. If the number of energy storage element precursors is 50 or less per unit, the size of the unit during production can be reduced.

[0191] [Timing at which voltage application begins] After forming a unit by connecting a plurality of nonaqueous lithium-ion storage element precursors (i.e., a plurality of exterior bodies each containing an electrode laminate or electrode wound body and a nonaqueous electrolyte solution and electrically integrated), doping is performed by applying a voltage to the storage element. Of the number of storage element precursors constituting the unit, it is preferable to apply a voltage to 30% to 70% of the nonaqueous lithium-ion storage element precursors, and then, after a certain delay time, apply a voltage to the remaining less than 70% or more than 30% of the nonaqueous lithium-ion storage element precursors. It is more preferable to apply a voltage to 40% to 60% of the nonaqueous lithium-ion storage element precursors, and then, after a certain delay time, apply a voltage to the remaining less than 60% or more than 40% of the nonaqueous lithium-ion storage element precursors. By first applying voltage to 30% to 70% of the nonaqueous lithium-ion battery element precursor and then applying voltage with a delay to the remaining 70% or more, or to the remaining 30% or more, the peaks of decomposition heat generated during the doping process are optimally dispersed, suppressing abnormal temperature increases in the battery element precursor. This reduces side reactions such as electrolyte decomposition and the formation of a coating due to the reaction between the doped lithium ions and the electrolyte, thereby accelerating the doping of lithium ions into the negative electrode and achieving excellent input / output characteristics. Furthermore, by reducing heat spots within the unit, the self-discharge rate is stabilized and micro-short circuits are suppressed.

[0192] More specifically, a first voltage application step (4) is carried out, followed by a second voltage application step (5).

[0193] In the first voltage application step (4), the total number of multiple exterior packaging bodies is divided into an exterior packaging body group I, which comprises 30% to 70% of the total number of multiple exterior packaging bodies, and an exterior packaging body group II, which comprises the remaining multiple exterior packaging bodies. Exterior packaging body groups I and II are arranged so that the maximum number of consecutively adjacent exterior packaging bodies belonging to exterior packaging body group II is 0% to 10% of the total number of multiple exterior packaging bodies, and a voltage is applied to exterior packaging body group I. It is preferable that exterior packaging body group I be selected from within a range of 40% to 60% of the total number of multiple exterior packaging bodies prepared. In this specification, "adjacent multiple exterior packaging bodies belonging to group I or II" means that the multiple exterior packaging bodies in the same group are consecutively adjacent along the voltage application direction.

[0194] In the first voltage application step (4), from the viewpoint of suitably controlling the heat generated when an alkali metal compound such as lithium carbonate in the positive electrode precursor is decomposed, it is preferable that exterior bodies belonging to exterior body group I are not adjacent to each other.

[0195] In the first voltage application step (4), from the viewpoint of suitably controlling the heat generated when an alkali metal compound such as lithium carbonate in the positive electrode precursor is decomposed, it is preferable that the maximum number of consecutively adjacent outer casings belonging to outer casing group II is 3 or less, and it is more preferable that when the total number of multiple outer casings belonging to outer casing group I and II is within the range of 10 to 50, the maximum number of consecutively adjacent outer casings belonging to outer casing group II is 3 or less.

[0196] In the first voltage application step (4), from the viewpoint of suitably controlling the heat generated when an alkali metal compound such as lithium carbonate in the positive electrode precursor is decomposed, it is preferable that outer casings belonging to outer casing group I and outer casings belonging to outer casing group II are arranged alternately.

[0197] In the second voltage application step (5), a voltage is applied to the exterior body group II selected and arranged as described above after a certain delay time has elapsed since the first voltage application step (4). From the viewpoints of suppressing heat generation from the positive electrode precursor and accelerating doping of lithium ions into the negative electrode, it is preferable that the doping of lithium ions into the negative electrode contained in the exterior body belonging to exterior body group I and the negative electrode contained in the exterior body belonging to exterior body group II is performed sequentially.

[0198] The nonaqueous lithium-ion storage element precursors to which a delay time is applied are preferably selected such that, among the exterior bodies constituting the storage element precursors, in exterior body group I to which a voltage is applied first and the remaining exterior body group II to which a voltage is applied after a delay time, the number of adjacent, facing surfaces of multiple exterior bodies belonging to the same exterior body group in both exterior body group I and exterior body group II is 0% to 50% of the total number of surfaces of the exterior bodies belonging to both groups. For example, when a delay time is applied to 50% of the storage element precursors, it is preferable to select them spaced apart one by one from the viewpoint of heat dissipation.

[0199] [Delay Time] The voltage application delay time X (min), where A is the charge rate during voltage application, is preferably (120 / A-10)≦X and 1≦A≦8. Here, the charge rate A is based on the initial capacity of the nonaqueous lithium-type energy storage element when discharged at 4V-2V. If X is (120 / A-10) or more, the peak due to the generation of heat of decomposition can be efficiently dispersed. A charge rate A of 1 or more is preferable because it reduces the time required for doping. A charge rate A of 8 or less is preferable because it allows more uniform decomposition of the lithium compound in the positive electrode and results in a uniform lithium doping state in the negative electrode.

[0200] [Decomposition speed] When a voltage is applied to the nonaqueous lithium-ion storage element precursor, the lithium compound contained in the positive electrode precursor decomposes, generating heat. The heat of decomposition increases or decreases depending on the decomposition rate of the lithium compound, and therefore must be controlled within an appropriate range. When the voltage of the nonaqueous lithium-ion storage element (e.g., the voltage applied in the first and second voltage application steps) is in the range of 4.3 V to 4.5 V, the decomposition rate (% / 0.1 V) of the lithium compound (e.g., lithium carbonate) per 0.1 V voltage increase is preferably 4.5 to 7.5. A decomposition rate (% / 0.1 V) of 4.5 or higher generates appropriate heat within the storage element, promoting the decomposition of the lithium compound and thereby accelerating the doping of lithium into the negative electrode. A decomposition rate (% / 0.1 V) of 7.5 or lower suppresses excessive heat generation and suppresses side reactions between the lithium ions doped in the negative electrode and the electrolyte, thereby suppressing dedoping of the lithium ions doped in the negative electrode.

[0201] [Temperature during doping process] The nonaqueous lithium-ion storage element precursor is composed of a unit formed by connecting multiple nonaqueous lithium-ion storage element precursors. When T1 (°C) is the temperature of the nonaqueous lithium-ion storage element precursor immediately after the start of the voltage application step and T2 (°C) is the maximum temperature of the nonaqueous lithium-ion storage element precursor during the voltage application step, it is preferable that T1 be 35 ≦ T1 ≦ 50 and 0 ≦ T2 − T1 ≦ 10. If T1 is 35 ≦ T1, the decomposition starting voltage of the lithium compound (e.g., lithium carbonate) can be reduced, allowing the lithium compound to be efficiently decomposed and lithium ions to be doped into the negative electrode. If T1 ≦ 50, de-doping of the lithium ions doped into the negative electrode can be suppressed. Furthermore, if T2 − T1 is 0 ≦ T2, the lithium compound can be doped without a decrease in its decomposition rate during the doping step. If T2 − T1 ≦ 10, uneven heat generation within the unit can be reduced, suppressing variations in the self-discharge rate and reducing the rate of micro-short circuits.

[0202] <Charge / discharge cycle process> The electrode laminate or electrode wound body is preferably subjected to a charge-discharge cycle process in which it is repeatedly charged and discharged. The effects of the cycle process include: (i) repeated charge-discharge cycles allow cations, anions, and solvents coordinated to the anions in the nonaqueous electrolyte to enter and exit the pores of the positive electrode activated carbon, stabilizing unstable functional groups on the surface of the activated carbon (the positive electrode active material), thereby improving cycle durability; (ii) exposing the positive electrode to a high potential completely decomposes alkali metal compounds that were not completely decomposed during the doping process, thereby improving high-temperature durability; and (iii) consuming by-products of the oxidative decomposition reaction of the alkali metal compounds generated during the doping process, thereby improving high-temperature durability. Because performing the cycle process under excessive load increases the resistance of the nonaqueous lithium-ion storage element, the charge-discharge cycle process must be performed under appropriate conditions (e.g., temperature, voltage, number of charge-discharge cycles, etc.).

[0203] The method of the charge-discharge cycle step is not particularly limited, but examples thereof include a method in which the voltage of the nonaqueous lithium-type storage element is repeatedly charged and discharged within a target voltage range by a charging method typified by constant current charging, constant current / constant voltage charging, pulse charging, etc., or a discharging method typified by constant current discharging, constant current / constant voltage discharging, or pulse discharging.

[0204] There are no particular restrictions on the current rate during constant current charging / discharging and pulse charging / discharging, but it is preferably 0.2 C or more and 50 C or less, based on the capacity at 4 V - 2 V described below. If it is 0.2 C or more, the time required for charging / discharging can be shortened, which reduces the equipment load and improves production efficiency. If it is 50 C or less, the current distribution becomes uniform, so the above-mentioned effects of the cycle process can be significantly obtained.

[0205] The time for which the constant voltage is maintained when constant-current / constant-voltage charging is used is not particularly limited, but is preferably 0.5 minutes or more and 120 minutes or less. If the time for maintaining the constant voltage is 0.5 minutes or more, the above-mentioned effects of the cycle process are significantly obtained, and if it is 120 minutes or less, the time required for charging and discharging can be shortened, thereby reducing the load on the equipment and improving production efficiency.

[0206] In the charge-discharge cycle step, charge and discharge are preferably performed within the range of the upper and lower voltage limits described below. The upper voltage limit is preferably 3.8V to 4.8V, more preferably 4.0V to 4.7V, and particularly preferably 4.1V to 4.6V. If the upper voltage limit is 3.8V or higher, the rate of increase in resistance after a high-temperature, high-load cycle test can be suppressed. If the upper voltage limit is 4.8V or lower, the nonaqueous lithium-type energy storage element can be maintained at a low resistance. The lower voltage limit is preferably 1.5V to 3.5V, more preferably 1.6V to 3.4V, particularly preferably 1.7V to 3.3V, and most preferably 1.75V to 3.0V. If the lower voltage limit is 1.5V or higher, elution of copper, which is the negative electrode current collector, can be suppressed, and the nonaqueous lithium-type energy storage element can be maintained at a low resistance. If the lower voltage limit is 3.5V or lower, the rate of increase in resistance after a high-temperature, high-load cycle test can be suppressed.

[0207] The temperature in the charge-discharge cycle step is preferably 30°C or higher and 100°C or lower, more preferably 35°C or higher and 85°C or lower, and particularly preferably 35°C or higher and 75°C or lower. If the temperature is 30°C or higher, the rate of increase in resistance after a high-temperature, high-load cycle test can be suppressed. If the temperature is 100°C or lower, the resistance of the nonaqueous lithium-type energy storage element can be maintained at a low level, and the equipment load required for temperature increase can be suppressed, thereby improving production efficiency.

[0208] The number of cycles in the charge / discharge cycle step is preferably 1 to 10, more preferably 2 to 8. Performing the cycle at least once has the effect of suppressing the rate of increase in resistance after a high-temperature, high-load cycle test. Performing the cycle 10 or less allows the nonaqueous lithium-type energy storage element to maintain low resistance. Furthermore, performing the cycle 10 or less is also preferable from the viewpoint of production efficiency, since the load on the necessary charge / discharge equipment can be suppressed.

[0209] In the charge-discharge cycle process, it is preferable to increase the pressure applied from the outside of the exterior body. 2 More than 1000kgf / cm 2 Less than 0.5kgf / cm is preferable. 2 More than 100kgf / cm 2Less than 1kgf / cm is more preferable. 2 More than 10kgf / cm 2 More preferably, the pressure is 0.1 kgf / cm or less. 2 When the pressure is 1000 kgf / cm or more, distortions in the positive electrode precursor and the negative electrode are corrected by the pressure, and the distance between the opposing positive electrode precursor and the negative electrode becomes uniform in the plane, so that the reaction in the charge-discharge cycle process proceeds uniformly, and durability under high temperature and high load cycles is improved, which is preferable. 2 If the thickness is less than this, a space for the non-aqueous electrolyte solution to penetrate into the electrode laminate or electrode wound body is ensured, and durability at high temperatures and high load cycles is improved, which is preferable.

[0210] <High-temperature aging process> The electrode stack or electrode wound body is preferably subjected to a high-temperature aging process in which it is heated. The effects of the aging process include (a) improving durability by decomposing the solvents and additives in the nonaqueous electrolyte and forming organic or inorganic coatings on the surfaces of the positive and negative electrodes, and (b) improving cycle durability by chemically reacting and stabilizing unstable functional groups on the surface of the activated carbon (the positive electrode active material) and impurities contained in the positive electrode, negative electrode, separator, and electrolyte. While organic and inorganic coatings improve high-temperature durability, the formation of excessive coatings increases the resistance of nonaqueous lithium-ion storage devices. Therefore, the high-temperature aging process must be performed under appropriate conditions (temperature, voltage, time, etc.).

[0211] The method for the high-temperature aging step is not particularly limited, but examples include a method in which the voltage of the nonaqueous lithium-type storage element is adjusted to a target voltage by a charging method typified by constant current charging, constant current / constant voltage charging, pulse charging, etc., or a discharging method typified by constant current discharging, constant current / constant voltage discharging, pulse discharging, and then charging and discharging are stopped and the element is stored in a high-temperature environment for a certain period of time.

[0212] The high-temperature aging step is (1 HVS) High-voltage storage step: This step includes a step of adjusting the voltage of the nonaqueous lithium-ion storage element precursor to a high voltage, and then adjusting the temperature of the nonaqueous lithium-ion storage element precursor to 45°C or higher and 100°C or lower, and storing the precursor. The voltage is preferably 4.03V or higher and 5.0V or lower, more preferably 4.05V or higher and 4.8V or lower, and particularly preferably 4.1V or higher and 4.5V or lower. If the voltage is 4.03V or higher, the rate of increase in resistance after a high-temperature, high-load cycle test can be suppressed. If the voltage is 5.0V or lower, excessive film formation can be prevented, and the nonaqueous lithium-ion storage element can be maintained at a low resistance.

[0213] The high-temperature aging process is as follows: HVS ) High voltage storage process (2 LVS ) A low voltage storage step may be further included. (2 LVS ) Low-voltage storage step: This step includes adjusting the voltage of the nonaqueous lithium-ion storage element precursor to a low voltage, and then adjusting the temperature of the nonaqueous lithium-ion storage element precursor to 45°C or higher and 100°C or lower, and storing the precursor. The voltage is preferably 1.5V or higher and 2.8V or lower, more preferably 1.6V or higher and 2.7V or lower, and particularly preferably 1.7V or higher and 2.5V or lower. If the voltage is 2.8V or lower, the capacity retention rate after a high-temperature, high-load cycle test can be improved. If the voltage is 1.5V or higher, elution of copper, which is the negative electrode current collector, can be suppressed, and low resistance can be maintained.

[0214] The order of the high voltage storage step and the low voltage storage step described above is not particularly limited.

[0215] The temperature in the high-voltage storage step and low-voltage storage step described above is preferably 45°C or higher and 100°C or lower, more preferably 50°C or higher and 85°C or lower, and particularly preferably 55°C or higher and 75°C or lower. A temperature of 45°C or higher has the effect of suppressing the rate of resistance increase after a high-temperature, high-load cycle test and improving the capacity retention rate after a high-temperature, high-load cycle test. A temperature of 100°C or lower can maintain low resistance of the nonaqueous lithium-type energy storage element and can reduce the equipment load required for temperature increase, thereby improving production efficiency. The temperature may be constant during the aging step, or may be varied in multiple stages to form a coating in stages or uniformly.

[0216] The aging time is preferably 0.25 to 340 hours, more preferably 0.5 to 100 hours, and most preferably 1 to 50 hours. Aging for 0.25 hours or longer has the effect of suppressing the rate of resistance increase after high-temperature, high-load cycle testing and improving the capacity retention rate after high-temperature, high-load cycle testing. Aging for 340 hours or shorter can maintain low resistance of the nonaqueous lithium-type energy storage element and reduce the time and number of facilities required for aging, thereby improving production efficiency.

[0217] In the aging process, it is preferable to increase the pressure applied from the outside of the exterior body. 2 More than 1000kgf / cm 2 Less than 0.5kgf / cm is preferable. 2 More than 100kgf / cm 2 Less than 1kgf / cm is more preferable. 2 More than 10kgf / cm 2 More preferably, the pressure is 0.1 kgf / cm or less. 2 When the pressure is 1000 kgf / cm or more, distortions in the positive electrode precursor and the negative electrode are corrected by the pressure, and the distance between the opposing positive electrode precursor and the negative electrode becomes uniform in the plane, so that the reaction in the high-temperature aging step proceeds uniformly, improving the durability under high-temperature and high-load cycles. 2 If the thickness is less than this, a space for the non-aqueous electrolyte solution to penetrate into the electrode laminate or electrode wound body is ensured, and durability at high temperatures and high load cycles is improved, which is preferable.

[0218] <Order of doping process, cycle process, and aging process> Regarding the order of performing the doping step, the cycling step, and the aging step, it is preferable to perform the doping step first. There are no particular restrictions on the order or number of times the cycling step and the aging step are performed thereafter. The doping step may also be performed multiple times.

[0219] <Gas removal process> After the aging step, degassing may be further performed to reliably remove gas remaining in the nonaqueous electrolyte solution, the positive electrode, and the negative electrode. Degassing improves durability. The degassing method is not particularly limited, but for example, a method can be used in which the electrode stack or the electrode wound body is placed in a reduced pressure chamber with the outer casing open, and the chamber is reduced pressure using a vacuum pump.

[0220] <Characteristics evaluation of non-aqueous lithium-based energy storage devices> [Decomposition rate measurement] In the doping step, when a constant current is applied to the nonaqueous lithium-ion storage element precursor, the decomposition rate (%) of the lithium compound contained in the positive electrode precursor per 0.1 V increase in voltage in the range of 4.3 V to 4.5 V is defined as the decomposition rate (% / 0.1 V). Three nonaqueous lithium-ion storage element precursors are prepared, and after the voltages reach 4.3 V, 4.4 V, and 4.5 V, they are discharged to 3.0 V. The removed nonaqueous lithium-ion storage element precursors are then disassembled, the positive electrodes are removed, and the amounts of remaining lithium carbonate X1 (%), X2 (%), and X3 (%) are quantified using the XRD described above. The horizontal axis is voltage (4.3V, 4.4V, 4.5V) and the vertical axis is voltage (X1 (%), X2 (%), X3 (%)). The decomposition rate per 0.1V increase (% / 0.1V) is calculated from the slope of the approximate line fitted by the least squares method.

[0221] [Anode doping amount measurement] After adjusting the voltage of the nonaqueous lithium-ion storage element to 4.0 V, disassemble it and remove the negative electrode. In the case of a double-sided negative electrode, one side is peeled off with a rag or the like and punched out, and metallic lithium, a separator, a glass filter, and the punched negative electrode are stacked to form a single-electrode negative electrode cell. Each component is impregnated with an electrolyte and charged until the voltage reaches 2.5 V. The negative electrode doping amount Q is calculated as Q = q / m (mAh / g), where q (mAh) is the obtained capacity and m (g) is the weight of the negative electrode active material. From the viewpoint of ensuring sufficient durability, the negative electrode doping amount is preferably 260 mAh or more, more preferably 290 mAh or more, and even more preferably 320 mAh or more.

[0222] [Temperature measurement during the doping process] A thermocouple is attached to the outer casing of the nonaqueous lithium-ion storage element precursor immediately after the start of the voltage application step, and the temperature T1 (°C) and the maximum temperature T2 (°C) of the outer casing during voltage application are measured. The measurement point is selected to be near the center of the unit, which is thought to be the easiest place to store heat.

[0223] [Normal temperature discharge internal resistance] In this specification, the room temperature discharge internal resistance Ra (Ω) is a value obtained by the following method: First, a cell corresponding to the nonaqueous lithium-ion storage element is charged at a constant current of 20 C in a thermostatic chamber set at 25°C until it reaches 4.0 V, and then a constant voltage charge of 4.0 V is applied for a total of 30 minutes. Subsequently, a constant current discharge is performed at a current of 20 C down to 2.0 V to obtain a discharge curve (time-voltage). In this discharge curve, the voltage at 0 seconds of discharge, obtained by linear approximation from the voltage values ​​at 2 seconds and 4 seconds of discharge, is defined as Eo. The voltage drop ΔE is calculated as 4.0 - Eo, and Ra is calculated as ΔE / (20 C (current value A)). From the viewpoint of achieving sufficient capacity for a large current, Ra is preferably 2.8 mΩ or less, more preferably 2.0 mΩ or less, and even more preferably 1.1 mΩ or less.

[0224] [Micro-short circuit inspection test] In this specification, a minor short circuit in a nonaqueous lithium-type storage element is determined by the following method. First, the battery is discharged at a constant current of 1 C to 2.5 V, then charged at a constant current of 1 C to 4.0 V, followed by a constant voltage charge of 4.0 V for one hour, adjusting the voltage to 4.0 V. The electrode assembly is then placed in a thermostatic chamber set at 45°C and pressurized at 100 kPa for one week, and a voltage drop of 3.8 V or less is determined to be a micro-short circuit. Heating and pressurization enable highly sensitive detection of nonaqueous lithium-based energy storage elements that have undergone a micro-short circuit. The yield is calculated by dividing the number of energy storage elements that have not undergone a micro-short circuit by the number of energy storage elements manufactured. From the viewpoint of reducing manufacturing costs, the yield is preferably 60% or higher, more preferably 70% or higher, and even more preferably 80% or higher. [Example]

[0225] EXAMPLES The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to these.

[0226] [Preparation of positive electrode active material] [Preparation of activated carbon 1] The crushed coconut shell carbonized material was placed in a small carbonization furnace and carbonized at 500°C for 3 hours under a nitrogen atmosphere to obtain a carbonized material. The obtained carbonized material was placed in an activation furnace, and steam heated in a preheating furnace was introduced into the furnace at 1 kg / h. The temperature was raised to 900°C over 8 hours for activation. After activation, the carbonized material was removed and cooled under a nitrogen atmosphere to obtain activated activated carbon. The obtained activated activated carbon was washed with water for 10 hours, drained, dried for 10 hours in an electric dryer maintained at 115°C, and then pulverized in a ball mill for 1 hour to obtain activated carbon 1.

[0227] The average particle diameter of activated carbon 1 was measured using a laser diffraction particle size distribution analyzer (SALD-2000J) manufactured by Shimadzu Corporation, and was found to be 5.5 μm. In addition, the pore size distribution of activated carbon 1 was measured using a pore size distribution analyzer (AUTOSORB-1 AS-1-MP) manufactured by Yuasa Ionics Corporation. As a result, the BET specific surface area was found to be 2360 m2 / g, mesopore volume (V1) is 0.52 cm 3 / g, micropore volume (V2) is 0.88 cm 3 / g, V1 / V2=0.59.

[0228] [Preparation of cathode precursor] [Production of positive electrode precursor 1] A positive electrode precursor was produced using activated carbon 1 as a positive electrode active material.

[0229] 58.0 parts by mass of activated carbon 1, 32.0 parts by mass of lithium carbonate, 4.0 parts by mass of acetylene black, 3.5 parts by mass of acrylic latex, 1.5 parts by mass of CMC (carboxymethyl cellulose), 1.0 part by mass of PVP (polyvinylpyrrolidone), and distilled water were mixed so that the mass proportion of solids was 43.0%, and the mixture was dispersed for 2 minutes using a thin-film swirling high-speed mixer "FILMIX (registered trademark)" manufactured by PRIMIX Corporation at a peripheral speed of 10 m / s, to obtain positive electrode coating solution 1.

[0230] The viscosity (ηb) and TI value of the obtained positive electrode coating solution 1 were measured using a Toki Sangyo Co., Ltd. E-type viscometer TVE-35H. The viscosity (ηb) was 2,030 mPa s and the TI value was 4.2. The degree of dispersion of the obtained positive electrode coating solution 1 was also measured using a particle gauge manufactured by Yoshimitsu Seiki Co., Ltd. The particle size was found to be 22 μm.

[0231] Using a double-sided die coater manufactured by Toray Engineering Co., Ltd., positive electrode coating solution 1 was applied to both sides of a 15 μm thick aluminum foil at a coating speed of 1 m / s and dried to obtain positive electrode precursor 1. The obtained positive electrode precursor 1 was pressed using a roll press under conditions of a pressure of 6 kN / cm and a surface temperature of 25°C. The total thickness of positive electrode precursor 1 was measured at 10 random locations on positive electrode precursor 1 using a film thickness meter, Linear Gauge Sensor GS-551 manufactured by Ono Keiki Co., Ltd. The measurement results showed that the film thickness of the positive electrode active material layer on each side of positive electrode precursor 1 was 61 μm.

[0232] [Production of positive electrode precursor 2] A positive electrode precursor was produced using activated carbon 1 as a positive electrode active material.

[0233] 42.0 parts by mass of activated carbon 1, 14.0 parts by mass of LiFePO4 as a lithium transition metal oxide having an average particle size of 3.5 μm, 32.0 parts by mass of lithium carbonate, 4.0 parts by mass of acetylene black, 3.5 parts by mass of acrylic latex, 1.5 parts by mass of CMC (carboxymethyl cellulose), 1.0 part by mass of PVP (polyvinylpyrrolidone), and distilled water were mixed so that the mass proportion of solids was 43.0%, and the mixture was dispersed for 2 minutes using a thin-film swirling high-speed mixer "FILMIX (registered trademark)" manufactured by PRIMIX Corporation at a peripheral speed of 10 m / s to obtain positive electrode coating solution 2.

[0234] The viscosity (ηb) and TI value of the obtained positive electrode coating solution 2 were measured using a Toki Sangyo Co., Ltd. E-type viscometer TVE-35H. The viscosity (ηb) was 2,330 mPa s and the TI value was 4.5. The degree of dispersion of the obtained positive electrode coating solution 2 was also measured using a Yoshimitsu Seiki Co., Ltd. particle gauge. The particle size was found to be 22 μm.

[0235] Using a double-sided die coater manufactured by Toray Engineering Co., Ltd., positive electrode coating solution 2 was applied to both sides of a 15 μm thick aluminum foil at a coating speed of 1 m / s and dried to obtain positive electrode precursor 2. The obtained positive electrode precursor 2 was pressed using a roll press under conditions of a pressure of 6 kN / cm and a surface temperature of 25°C. The total thickness of positive electrode precursor 2 was measured at 10 arbitrary locations on positive electrode precursor 2 using a film thickness meter, Linear Gauge Sensor GS-551 manufactured by Ono Keiki Co., Ltd. From the obtained measurement results, the film thickness of the positive electrode active material layer on one side of positive electrode precursor 2 was 48 μm.

[0236] [Preparation of negative electrode 1] 83 parts by mass of artificial graphite with an average particle size of 4.5 μm, 4 parts by mass of composite carbon material, and 9 parts by mass of acetylene black were dry-blended in powder form in a planetary mixer, to which 2 parts by mass of styrene-butadiene copolymer and an aqueous CMC (carboxymethyl cellulose) solution were added, and the solid content was gradually reduced while dispersing. Finally, 2 parts by mass of CMC was added, and water was added to the mixed solution so that the solid content was 39% by mass, to obtain a negative electrode coating solution.

[0237] The viscosity (ηb) and TI value of the resulting negative electrode coating solution were measured using an E-type viscometer TVE-35H manufactured by Toki Sangyo Co., Ltd. The viscosity (ηb) was 3,221 mPa·s and the TI value was 2.1.

[0238] Using a die coater manufactured by Toray Engineering Co., Ltd., the negative electrode coating solution was applied to both sides of a 10 μm-thick electrolytic copper foil at a coating speed of 1 m / s, and then dried at a drying temperature of 60°C to obtain negative electrode 1. Pressing was performed using a roll press under conditions of a pressure of 5 kN / cm and a surface temperature of the press part of 25°C. The total thickness of the pressed negative electrode 1 was measured at 10 random locations on the negative electrode 1 using a film thickness meter, Linear Gauge Sensor GS-551 manufactured by Ono Keiki Co., Ltd. From the measurement results obtained, the film thickness of the negative electrode active material layer of negative electrode 1 was 30 μm per side.

[0239] [Preparation of electrolyte] A mixed solvent of ethylene carbonate (EC): dimethyl carbonate (DMC): methyl ethyl carbonate (EMC) = 34:44:22 (volume ratio) was used as the organic solvent, and the respective electrolyte salts were dissolved therein so that the concentration ratio of LiN(SO2F)2 and LiPF6 to the total non-aqueous electrolyte solution was 25:75 (molar ratio) and the sum of the concentrations of LiN(SO2F)2 and LiPF6 was 1.2 mol / L.

[0240] The concentrations of LiN(SO2F)2 and LiPF6 in the prepared non-aqueous electrolyte were 0.3 mol / L and 0.9 mol / L, respectively.

[0241] Examples 1 and 2 [Manufacturing of non-aqueous lithium-type energy storage elements] In Example 1, positive electrode precursor 1 was used as the positive electrode precursor, and in Example 2, positive electrode precursor 2 was used.

[0242] [Secondary drying of electrodes] The positive electrode precursor and negative electrode were dried roll-to-roll using far-infrared light at a temperature of 80°C for 5 minutes with an oxygen concentration of 1000 ppm in the drying oven. The positive electrode precursor emerging from the drying oven was wound up in a dry environment with a dew point of -45°C.

[0243] [Assembly process] The obtained positive electrode precursor was placed in a container with a positive electrode active material layer of 10.0 cm × 10.0 cm (100 cm 2 Then, the negative electrode 1 was cut into 20 pieces with a negative electrode active material layer of 10.1 cm × 10.1 cm (102 cm 2 ) size, cut out 21 pieces, 10.3cm x 10.3cm (106cm 2 Forty polyethylene separators (manufactured by Asahi Kasei Corporation, thickness 10 μm) were prepared. These were stacked in the order of positive electrode precursor, separator, and negative electrode, with the separator sandwiched between them, so that the outermost layer was negative electrode 1, with the positive electrode active material layer and the negative electrode active material layer facing each other, to obtain an electrode laminate. A positive electrode terminal and a negative electrode terminal were ultrasonically welded to the obtained electrode laminate, which was then placed in a container made of aluminum laminate packaging material, and the three sides including the electrode terminals were heat-sealed.

[0244] [Pressure process] The aluminum laminate packaging was sandwiched between a pair of metal plates (height 150 mm x width 150 mm x thickness 5 mm) from the outside, and pressure was applied by screwing the four corners of the metal plates. When the pressure was measured using the I-SCAN surface pressure distribution measurement system (manufactured by Nitta Corporation) and the I-SCAN100 sensor (measurement surface dimensions: 112 mm x 112 mm), the confining pressure was found to be 0.08 kgf / cm. 2 It was.

[0245] [Injection, impregnation and sealing process] The electrode stack housed in the aluminum laminate packaging material was placed in a vacuum chamber in a dry air environment with a temperature of 25°C and a dew point of -40°C or less, and the pressure was reduced from normal pressure to -100 kPa. After that, approximately 80 g of the nonaqueous electrolyte solution at a liquid temperature of 25°C was poured into the chamber. The pressure was then returned to normal pressure and the chamber was left standing for 60 minutes. Next, the nonaqueous lithium-ion storage element was placed in a vacuum sealing machine, and the aluminum laminate packaging material was sealed by sealing at a pressure of 0.1 MPa at 180°C for 10 seconds under a reduced pressure of -95 kPa.

[0246] [Unit Preparation] A unit was prepared that had a mechanism for applying pressure to both sides of the exterior body of the non-aqueous lithium-ion battery element precursor using an interlayer plate. The interlayer plate was a 10 mm thick aluminum plate with an anodized surface. The unit was large enough to accommodate 30 non-aqueous lithium-ion battery element precursors and could also apply spring pressure.

[0247] [Re-pressurization process] After the injection, 30 non-aqueous lithium storage element precursors were placed in a unit and restrained under a pressure of 1.2 kgf / cm 2 The compression amount of the spring was adjusted so that

[0248] [Doping process] Thirty nonaqueous lithium-ion battery element precursors were attached to a unit, and the unit was placed in a thermostatic chamber at 45°C. After confirming that the temperature of the nonaqueous lithium-ion battery element precursors' outer packaging had reached 45°C, 15 of the 30 nonaqueous lithium-ion battery element precursors were selected, spaced one apart from the end, as shown in Table 2, as part of packaging group I, and voltage application was initiated. After a 20-minute delay, voltage application was initiated for the remaining packaging group II. Voltage application was performed using an Asuka Electronics Co., Ltd. charge / discharge tester (ACD-10APS(01)). A constant-current charge of 6 A was performed until a voltage of 4.5 V was reached, followed by a constant-voltage charge of 4.5 V for 1 hour, for initial charging, and lithium was doped into the negative electrode.

[0249] [Charge / discharge cycle process] Pressure: 1.2kgf / cm 2 The doped non-aqueous lithium-type electricity storage element was placed in an environment of 30°C. (1) The battery was charged at a constant current of 10.0 A until the voltage reached 4.3 V, and then charged at a constant voltage of 4.3 V for 5 minutes. (2) A constant current discharge of 10.0 A was performed until the voltage reached 2.0 V, and then a constant voltage discharge of 2.0 V was performed for 5 minutes. (1) and (2) constitute one cycle, and a total of five cycles were performed.

[0250] [High-temperature aging process] (1) High voltage storage process: 1.2 kgf / cm 2 The nonaqueous lithium-type storage element after the charge-discharge cycle process was subjected to constant current discharge at 10.0 A in a 25°C environment until the voltage reached 4.2 V, and then subjected to constant current charging at 4.2 V for 30 minutes to adjust the voltage to 4.2 V. Thereafter, the nonaqueous lithium-type storage element was stored in a thermostatic chamber at 60°C for 10 hours. (2) Low voltage storage process: 1.2 kgf / cm 2 The nonaqueous lithium-type storage element after the low-voltage step was then subjected to constant current discharge at 10.0 A in a 25°C environment until the voltage reached 2.0 V, and then subjected to constant current charging at 2.0 V for 30 minutes to adjust the voltage to 2.0 V. The nonaqueous lithium-type storage element was then stored in a constant temperature bath at 60°C for 10 hours.

[0251] [Gas removal and sealing process] The aluminum laminate packaging material for the aged nonaqueous lithium-ion storage element was partially opened in a dry air environment at a temperature of 25°C and a dew point of -40°C. Next, the nonaqueous lithium-ion storage element was placed in a vacuum chamber, and the pressure was reduced from atmospheric pressure to -80 kPa over 3 minutes using a diaphragm pump (N816.3KT.45.18) manufactured by KNF, and then the pressure was returned to atmospheric pressure over 3 minutes. This process was repeated three times in total. The nonaqueous lithium-ion storage element was then placed in a vacuum sealing machine, and the pressure was reduced to -90 kPa. The aluminum laminate packaging material was then sealed by sealing at 200°C for 10 seconds at a pressure of 0.1 MPa.

[0252] Through the above steps, a non-aqueous lithium-type energy storage element was completed.

[0253] [Evaluation of energy storage elements] [Decomposition rate measurement] Of the 30 nonaqueous lithium storage elements installed in the unit, three were randomly selected and the decomposition rate measurement described above was carried out. In Example 1, the decomposition rate of lithium carbonate was 5.5 (% / 0.1V).

[0254] [Temperature measurement] Of the 30 non-aqueous lithium-type storage element precursors installed in the unit, a thermocouple (Rika Kogyo: ST-51) was attached to the 15th storage element precursor from the end, and the temperature change was read using a data logger.In Example 1, T1 was 45°C, T2 was 50°C, and T2 - T1 = 5°C.

[0255] [Anode doping amount measurement] Of the 27 nonaqueous lithium-type storage elements produced, five were randomly selected and subjected to the above-described measurement of the negative electrode doping amount. In Example 1, the average negative electrode doping amount was 340 mAh / g.

[0256] [Micro-short circuit inspection process] The above-mentioned micro-short circuit inspection test was carried out on the 27 fabricated nonaqueous lithium-type storage elements, and the number of micro-short circuits was found to be 0 in Example 1. Therefore, the yield of Example 1 was 100%.

[0257] Examples 3 to 20 A nonaqueous lithium-type storage element was produced and the subsequent evaluations were carried out in the same manner as in Example 1, except for the production conditions in the doping step. The results are shown in Tables 1 and 2.

[0258] Examples 21 to 34, Comparative Examples 1 to 10 The type of positive electrode precursor and the manufacturing conditions in the doping step were changed as shown in Table 1 or Table 2, and the assembly step and evaluation were carried out in the same manner as in Example 1. The results are shown in Tables 1 and 2.

[0259] [Table 1-1]

[0260] [Table 1-2]

[0261] [Table 1-3]

[0262] [Table 2]

[0263] From the above examples, it was verified that the energy storage element of this embodiment can promote the doping of lithium ions into the negative electrode by suitably controlling the heat generated when the lithium compound contained in the positive electrode precursor is decomposed, thereby providing excellent input / output characteristics and suppressing micro-short circuits during production. [Industrial Applicability]

[0264] The nonaqueous lithium-type energy storage element according to the present invention has excellent input / output characteristics and can suppress micro-short circuits during production, and therefore can be suitably used, for example, in the field of hybrid drive systems in automobiles that combine internal combustion engines or fuel cells, motors, and energy storage elements, as well as for assisting momentary power peaks.

Claims

1. A method for producing a non-aqueous lithium-type storage element, comprising the steps of: The nonaqueous lithium-type energy storage element includes a plurality of exterior bodies, each of the plurality of exterior bodies contains a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution and is electrically connected to the other; The following steps: (1) a step of stacking a positive electrode precursor containing a positive electrode active material made of a carbon material and lithium carbonate, and a negative electrode containing a negative electrode active material capable of absorbing and releasing lithium ions, with the separator interposed therebetween, to obtain a laminate, and housing the laminate in each of the exterior bodies; (2) a liquid injection step of injecting the nonaqueous electrolyte solution containing lithium ions into each of the exterior bodies; (3) a storage element precursor forming step of electrically bonding the plurality of exterior bodies to obtain a nonaqueous lithium-type storage element precursor; (4) a first voltage application step of dividing the total number of the plurality of exterior bodies into an exterior body group I that is 30% to 70% and an exterior body group II that is the remaining number, arranging the exterior body groups I and II such that the maximum number of consecutively adjacent exterior bodies among those belonging to the exterior body group II is 0% to 10% of the total number of the plurality of exterior bodies, and applying a voltage to the exterior body group I; and (5) a second voltage application step of applying a voltage to the exterior body group II after a certain delay time has elapsed since the first voltage application step; When the delay time is X (min.) and the charging rate during voltage application is A, the first and second voltage application steps satisfy the following relational expression: (120 / A-10)≦X, and 1≦A≦8 The method for producing a nonaqueous lithium-type storage element is carried out so as to satisfy the above.

2. The method for producing a nonaqueous lithium-type energy storage element according to claim 1 , wherein in the first voltage application step, the maximum number of adjacent consecutive exterior bodies among those belonging to the exterior body group II is three or less.

3. 3. The method for manufacturing a nonaqueous lithium-type storage element according to claim 1 or 2, wherein, in the first voltage application step, when the total number of exterior bodies belonging to the exterior body groups I and II is within the range of 10 to 50, the maximum number of consecutively adjacent exterior bodies belonging to the exterior body group II is 3 or less.

4. Each of the multiple exterior bodies has a front surface and a back surface, In the energy storage element precursor forming step, after one exterior body is arranged so that one of the front and rear surfaces faces one of the front and rear surfaces of another exterior body, the multiple exterior bodies are electrically coupled to each other, A method for manufacturing a nonaqueous lithium-type storage element according to any one of claims 1 to 3, wherein in the first voltage application step, multiple exterior bodies belonging to both groups I and II are arranged so that the number of adjacent faces of multiple exterior bodies belonging to the same exterior body group facing each other in both groups is 0% to 50% of the total number of faces of the exterior bodies belonging to both groups, and a voltage is applied to the exterior body group I.

5. The method for producing a nonaqueous lithium-type energy storage element according to any one of claims 1 to 4, wherein in the first voltage application step, the exterior bodies belonging to the exterior body group I are not adjacent to each other.

6. The method for manufacturing a nonaqueous lithium-type storage element according to any one of claims 1 to 5, wherein in the first voltage application step, the exterior bodies belonging to the exterior body group I and the exterior bodies belonging to the exterior body group II are arranged alternately.

7. A method for manufacturing a non-aqueous lithium-type storage element described in any one of claims 1 to 6, wherein the charging rate A is based on the initial capacity of the non-aqueous lithium-type storage element when discharged to 4V-2V.

8. 8. The method for producing a nonaqueous lithium-type storage element according to claim 1, wherein when the applied voltages in the first and second voltage application steps are within a range of 4.3 V to 4.5 V, a decomposition rate of the lithium carbonate per unit time is 4.5% / 0.1 V to 7.5% / 0.1 V.

9. When the temperature of the nonaqueous lithium type storage element precursor immediately after the start of the first and second voltage application steps is T1 (°C), and the maximum temperature of the nonaqueous lithium type storage element precursor during the first and second voltage application steps is T2 (°C), The method for producing a nonaqueous lithium-type storage element according to any one of claims 1 to 8, wherein 35≦T1≦50 and 0≦T2−T1≦10.

10. The method for producing a nonaqueous lithium-type storage element according to any one of claims 1 to 9, wherein the negative electrode contained in the outer casing belonging to group I and the negative electrode contained in the outer casing belonging to group II are doped with lithium ions sequentially.

Citation Information

Patent Citations

  • Method for manufacturing power storage device and doping tank

    JP2014120701A

  • Method for manufacturing electricity storage device

    JP2014211950A

  • Power storage system

    JP2016167912A

  • Power storge module having nonaqueous lithium power storage elements

    JP2019029632A

  • Lithium ion capacitor and manufacturing method thereof

    JP2019145723A