Toner and method for producing the same

A toner with a core-shell structure using crystalline and amorphous resins and a crosslinked shell layer addresses the challenges of low-temperature fixability, heat-resistant storage, and charging stability, ensuring effective performance in electrophotographic processes.

JP7587377B2Active Publication Date: 2024-11-20CANON KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020154162
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-11-20
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving low-temperature fixability, heat-resistant storage stability, and charging stability due to the limitations of crystalline resins and core-shell structures in electrophotographic processes.

Method used

A toner with a core-shell structure where the toner core contains a crystalline resin and an amorphous resin, with a crystalline resin having specific acid and hydroxyl values, and a shell layer formed by a thermosetting resin through a crosslinking reaction, ensuring a shell layer thickness of 3 nm to 200 nm.

Benefits of technology

The toner achieves excellent low-temperature fixability, heat-resistant storage stability, and charging stability by selectively covering the crystalline resin, preventing exposure and enhancing the core-shell interface reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587377000001
    Figure 0007587377000001
  • Figure 0007587377000002
    Figure 0007587377000002
  • Figure 0007587377000003
    Figure 0007587377000003
Patent Text Reader

Abstract

To provide a toner which is excellent in low temperature fixability, charging stability and storage property.SOLUTION: A toner has toner particles including a core-shell structure that a surface of a toner core is covered with a shell layer, in which the toner core contains a crystalline resin A and an amorphous resin B, the crystalline resin A has a carboxy group, an acid value of the crystalline resin A is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, a hydroxyl value of the crystalline resin A is 20.0 mgKOH / g or less, the shell layer contains a thermosetting resin C having a functional group that can react with the carboxy group, an interface between the toner core and the shell layer has a resin component formed by crosslinking reaction of the carboxy group of the crystalline resin A and a functional group of a thermosetting resin C having a functional group that can react with the carboxy group of the crystalline resin A, and a thickness of the shell layer is 3 nm or more and 200 nm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, and a toner jet system, and a method for producing the toner. [Background technology]

[0002] In recent years, as full-color electrophotographic copying machines have come into widespread use, there is a demand for further energy saving. To achieve this, a toner that can be fixed well even when the temperature of the fixing roller is low is required. In Patent Document 1, various toners containing crystalline resins with sharp melting properties have been proposed to improve low-temperature fixing performance, but the crystalline resins may cause deterioration in heat-resistant storage stability and charging stability.

[0003] Patent Document 2 proposes using a core-shell structure with a crystalline resin and an amorphous resin in the core and a resin with a high glass transition point in the shell. This method can improve heat-resistant storage stability and charging stability. However, the thickness of the shell inhibits low-temperature fixability, so further improvement is required.

[0004] Patent Document 3 proposes a toner in which the surface of the toner core is coated with a thin film containing a thermosetting component. However, even a small amount of the crystalline resin is exposed on the toner surface, which reduces the charging stability and the concentration stability, and therefore further improvement is required. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-123352 A [Patent Document 2] JP 2018-180188 A [Patent Document 3] JP 2013-109330 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a toner which overcomes the above problems, specifically, to provide a toner which is excellent in low-temperature fixing property, heat-resistant storage stability, and charging stability. [Means for solving the problem]

[0007] The toner according to the present invention is a toner having toner particles with a core-shell structure in which the surface of a toner core is covered with a shell layer, The toner core contains a crystalline resin A and an amorphous resin B, The crystalline resin A has a carboxy group, The acid value of the crystalline resin A is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, The hydroxyl value of the crystalline resin A is 20.0 mgKOH / g or less, the shell layer contains a thermosetting resin C having a functional group capable of reacting with the carboxy group, The interface between the toner core and the shell layer is the carboxy group of the crystalline resin A; a resin component formed by a crosslinking reaction between the carboxy group of the crystalline resin A and a functional group of a thermosetting resin C having a functional group capable of reacting with the carboxy group of the crystalline resin A; The shell layer has a thickness of 3 nm or more and 200 nm or less.

[0008] The method for producing a toner according to the present invention comprises the steps of: A method for producing a toner having toner particles with a core-shell structure in which a surface of a toner core is covered with a shell layer, comprising the steps of: a step of reacting a crystalline resin A contained in the toner core with a shell material in an aqueous medium to form a shell layer covering the surface of the toner core, thereby obtaining toner particles; The shell material comprises a thermosetting resin C having an oxazoline group; the toner core contains the crystalline resin A and the amorphous resin B, The crystalline resin A contains a carboxy group, The acid value of the crystalline resin A is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, The hydroxyl value of the crystalline resin A is 20.0 mgKOH / g or less, the shell layer contains a resin component including a unit having an oxazoline group and a unit having an amide bond, The amide bond is characterized in that it is formed by a reaction between the oxazoline group of the thermosetting resin C contained in the shell material and the carboxy group of the crystalline resin A contained in the toner core. Effect of the Invention

[0009] According to the present invention, it is possible to provide a toner having excellent low-temperature fixing property, heat-resistant storage stability, and charging stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The toner according to the present invention is A toner having toner particles with a core-shell structure in which the surface of a toner core is covered with a shell layer, The toner core contains a crystalline resin A and an amorphous resin B, The crystalline resin A has a carboxy group, The acid value of the crystalline resin A is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, The hydroxyl value of the crystalline resin A is 20.0 mgKOH / g or less, the shell layer contains a thermosetting resin C having a functional group capable of reacting with the carboxy group, The interface between the toner core and the shell layer is the carboxy group of the crystalline resin A; a resin component formed by a crosslinking reaction between the carboxy group of the crystalline resin A and a functional group of a thermosetting resin C having a functional group capable of reacting with the carboxy group of the crystalline resin A; The shell layer has a thickness of 3 nm or more and 200 nm or less.

[0011] The present inventors consider the following regarding the effects of using the toner of the present invention having such a configuration. Since the acid value of the crystalline resin A used in the present invention falls within a specific range, the interface between the core and the shell layer contains a resin component formed by a crosslinking reaction between a carboxy group of the crystalline resin A and a functional group of the thermosetting resin C used in the shell layer. This resin component gives the shell layer a structure that selectively covers the crystalline resin A. Therefore, even if an extremely thin shell layer is formed, the crystalline resin A is unlikely to be exposed, and it is possible to achieve both low-temperature fixability, charge stability, and heat-resistant storage stability.

[0012] Here, the resin component refers to a polymer formed by a crosslinking reaction between a polymer constituting the crystalline resin A and a polymer constituting the thermosetting resin.

[0013] The acid value of the crystalline resin A is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, more preferably 25.0 mgKOH / g or more and 40.0 mgKOH / g or less. If the acid value of the crystalline resin A is less than 10 mgKOH / g, the reaction with the functional group of the thermosetting resin C of the shell layer becomes insufficient, the crystalline resin A is exposed, and the heat resistance storage stability and the charge stability are deteriorated. If the acid value of the crystalline resin is too large, the amount of remaining carboxyl groups after the reaction with the functional group of the thermosetting resin of the shell layer increases, and the charge stability is deteriorated. By making the hydroxyl value of the crystalline resin A 20.0 mgKOH / g or less, the amount of moisture adsorption can be reduced, and the charge stability can be maintained even in harsh environments such as high temperature and high humidity environments.

[0014] By setting the thickness of the shell layer to 3 nm or more and 200 nm or less, the low-temperature fixability, heat-resistant storage stability, and charge stability of the toner can be ensured. The thickness is more preferably 3 nm or more and 20 nm or less. If the thickness of the shell layer is too thin, the heat-resistant storage stability and charge stability of the toner become insufficient. If the thickness of the shell layer is too thick, the low-temperature fixability of the toner becomes insufficient.

[0015] The acid value of the amorphous resin B is preferably 20.0 mgKOH / g or less. This allows the functional group of the thermosetting resin C used in the shell layer to selectively react with the carboxyl group of the crystalline resin A, improving the charge stability and heat-resistant storage stability. The hydroxyl value of the amorphous resin B is preferably 40.0 mgKOH / g or less. This suppresses moisture adsorption and improves charge stability.

[0016] The functional group capable of crosslinking with the carboxy group of the crystalline resin is preferably an unopened oxazoline group. In this case, the resin component has a structural unit derived from the oxazoline group formed by the crosslinking reaction with the carboxy group. The unopened oxazoline group is easily reactive with the carboxy group, and can form a strong amide bond with the crystalline resin of the toner core while keeping the shell layer thin, improving low-temperature fixing properties, charge stability, and heat-resistant storage stability. As an example of a method for confirming this amide bond, the toner particles are measured by infrared spectroscopy and a strong amide bond is formed with the crystalline resin of the toner core while keeping the shell layer thin, improving low-temperature fixing properties, charge stability, and heat-resistant storage stability. -1 Another method to show that it is abundant at the core-shell interface is the 1630 cm peak obtained using Ge as an ATR crystal. -1 The peak intensity of 1720 cm originating from the ester group of the polyester resin is -1 The peak intensity (C=O peak of polyester) of Pb(Ge) was calculated using diamond as the ATR crystal at 1630 cm -1 The peak intensity is expressed as Pa (Dy) and 1720 cm -1 When the peak intensity of Pb(Dy) is taken as Pb(Dy), Pa(Dy) / Pb(Dy) is smaller than Pa(Ge) / Pb(Ge).

[0017] From the viewpoints of charge stability and low-temperature fixability, the amorphous resin B is preferably a polyester resin.

[0018] The constitution of the toner of the present invention will be described in detail below. [Crystalline resin A] The crystalline resin A used in the toner of the present invention has a carboxy group, an acid value of 10.0 mgKOH / g or more and 50.0 mgKOH / g or less, and a hydroxyl value of 20 mgKOH / g or less. The crystalline resin is a resin in which an endothermic peak is observed in differential scanning calorimetry (DSC).

[0019] The crystalline resin A is not particularly limited, but from the viewpoint of ensuring low-temperature fixing ability and having a suitable acid value that leads to ensuring the above-mentioned heat-resistant storage stability and charging stability, it is preferable that the crystalline resin A contains a polyester resin as a main component.

[0020] The crystalline polyester is preferably one obtained by polycondensation reaction of a monomer composition containing, as main components, an aliphatic diol having 2 to 22 carbon atoms and an aliphatic dicarboxylic acid having 2 to 22 carbon atoms.

[0021] The aliphatic diol having 2 to 22 carbon atoms (more preferably 6 to 12 carbon atoms) is not particularly limited, but is preferably a chain (more preferably a linear) aliphatic diol.

[0022] Examples include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propanediol, 1,3-propanediol, dipropylene glycol, 1,4-butanediol, 1,4-butadiene glycol, trimethylene glycol, tetramethylene glycol, pentamethylene glycol, hexamethylene glycol, octamethylene glycol, nonamethylene glycol, decamethylene glycol, and neopentyl glycol.

[0023] Among these, particularly preferred examples include straight-chain aliphatic α,ω-diols such as ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,6-hexanediol.

[0024] Of the above alcohol components, preferably 50% by mass or more, more preferably 70% by mass or more, is an alcohol selected from aliphatic diols having 2 to 22 carbon atoms.

[0025] Polyhydric alcohol monomers other than the above aliphatic diols can also be used. Among the polyhydric alcohol monomers, examples of dihydric alcohol monomers include aromatic alcohols such as polyoxyethylenated bisphenol A and polyoxypropylenated bisphenol A; 1,4-cyclohexanedimethanol, etc. Among the polyhydric alcohol monomers, examples of trihydric or higher polyhydric alcohol monomers include aromatic alcohols such as 1,3,5-trihydroxymethylbenzene; and aliphatic alcohols such as pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerin, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, and trimethylolpropane.

[0026] Furthermore, monohydric alcohols may be used to the extent that they do not impair the properties of the crystalline polyester. Examples of the monohydric alcohols include monoalcohols such as n-butanol, isobutanol, sec-butanol, n-hexanol, n-octanol, 2-ethylhexanol, cyclohexanol, and benzyl alcohol, capryl alcohol (decanol), undecanol, lauryl alcohol (dodecanol), tridecanol, myristyl alcohol (tetradecanol), pentadecanol, palmityl alcohol (hexadecanol), margaryl alcohol (heptadecanol), stearyl alcohol (octadecanol), nonadecanol, and arachidyl alcohol (icosanol).

[0027] On the other hand, the aliphatic dicarboxylic acid having 2 to 22 carbon atoms (more preferably 6 to 12 carbon atoms) is not particularly limited, but is preferably a chain (more preferably linear) aliphatic dicarboxylic acid.

[0028] Specific examples include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, nonanedicarboxylic acid, decanedicarboxylic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, maleic acid, fumaric acid, mesaconic acid, citraconic acid, and itaconic acid, as well as hydrolyzates of these acid anhydrides or lower alkyl esters.

[0029] Of the carboxylic acid components, preferably 50% by mass or more, more preferably 70% by mass or more, is a carboxylic acid selected from aliphatic dicarboxylic acids having 2 to 22 carbon atoms.

[0030] It is also possible to use polyvalent carboxylic acids other than the above-mentioned aliphatic dicarboxylic acids having 2 to 22 carbon atoms. Among the other polyvalent carboxylic acid monomers, examples of divalent carboxylic acids include aromatic carboxylic acids such as isophthalic acid and terephthalic acid, aliphatic carboxylic acids such as n-dodecylsuccinic acid and n-dodecenylsuccinic acid, and alicyclic carboxylic acids such as cyclohexanedicarboxylic acid, as well as their acid anhydrides and lower alkyl esters.

[0031] Furthermore, among the other carboxylic acid monomers, examples of polyvalent carboxylic acids having a valence of three or more include aromatic carboxylic acids such as 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and pyromellitic acid, and aliphatic carboxylic acids such as 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, and 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, as well as derivatives such as acid anhydrides and lower alkyl esters thereof.

[0032] Furthermore, monovalent carboxylic acids may be contained to the extent that the properties of the crystalline polyester are not impaired. Examples of monovalent carboxylic acids include benzoic acid, naphthalene carboxylic acid, salicylic acid, 4-methylbenzoic acid, 3-methylbenzoic acid, phenoxyacetic acid, biphenyl carboxylic acid, acetic acid, propionic acid, butyric acid, octanoic acid, capric acid (decanoic acid), undecylic acid, lauric acid (dodecanoic acid), tridecylic acid, myristic acid (tetradecanoic acid), pentadecylic acid, palmitic acid (hexadecanoic acid), margaric acid (heptadecanoic acid), stearic acid (octadecanoic acid), nonadecylic acid, and arachidic acid (icosanoic acid).

[0033] The content of the crystalline resin A is preferably 3 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the amorphous resin B from the viewpoint of low-temperature fixability and chargeability in a high-temperature and high-humidity environment.

[0034] Crystalline polyester can be produced according to a normal polyester synthesis method. For example, the above-mentioned carboxylic acid monomer and alcohol monomer are subjected to esterification reaction or ester exchange reaction, and then the crystalline polyester can be obtained by carrying out a polycondensation reaction according to a normal method under reduced pressure or by introducing nitrogen gas. Then, the above-mentioned aliphatic compound is further added and the esterification reaction is carried out, thereby obtaining the desired crystalline polyester.

[0035] The above esterification or transesterification reaction can be carried out, if necessary, using a common esterification catalyst or transesterification catalyst such as sulfuric acid, titanium butoxide, dibutyltin oxide, manganese acetate, magnesium acetate, etc.

[0036] The polycondensation reaction can be carried out using a conventional polymerization catalyst, such as titanium butoxide, dibutyltin oxide, tin acetate, zinc acetate, tin disulfide, antimony trioxide, germanium dioxide, etc. The polymerization temperature and the amount of catalyst are not particularly limited and may be appropriately determined.

[0037] In the esterification or transesterification reaction or polycondensation reaction, in order to increase the strength of the resulting crystalline polyester, a method of charging all the monomers at once may be used. Also, in order to reduce low molecular weight components, a method of first reacting a divalent monomer and then adding and reacting a trivalent or higher monomer may be used. The peak molecular weight of the crystalline resin A is preferably 1,000 or more and 6,000 or less from the viewpoints of low-temperature fixability and heat-resistant storage stability. The weight average molecular weight Mw of the crystalline resin A is preferably 4,000 or more and 30,000 or less from the viewpoints of low-temperature fixability and heat-resistant storage stability.

[0038] [Amorphous resin B] The amorphous resin B used in the toner of the present invention is not particularly limited, and the following polymers or resins can be used.

[0039] For example, homopolymers of styrene and its substitutes such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-acrylic acid ester copolymers, styrene-methacrylic acid ester copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers, and styrene-acrylonitrile-indene copolymers; polyvinyl chloride, phenolic resins, natural resin-modified phenolic resins, natural resin-modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyester resins, polyurethane resins, polyamide resins, furan resins, epoxy resins, xylene resins, polyvinyl butyral, terpene resins, coumarone-indene resins, and petroleum-based resins can be used.

[0040] Among these, it is preferable to use a polyester resin as the main component from the viewpoint of low temperature fixability. The term "main component" means that the content thereof is 50% by mass or more.

[0041] Monomers used for the polyester resin include polyhydric alcohols (divalent, trivalent or higher alcohols), polyvalent carboxylic acids (divalent, trivalent or higher carboxylic acids), acid anhydrides thereof, or lower alkyl esters thereof.

[0042] Here, from the viewpoint of improving heat-resistant storage stability and electrostatic chargeability, when preparing a branched polymer, it is effective to partially crosslink within the molecule of the amorphous resin B, and for this purpose, it is preferable to use a polyfunctional compound having a valence of three or more. Therefore, it is preferable to include a trivalent or higher carboxylic acid, an acid anhydride or a lower alkyl ester thereof, and / or a trivalent or higher alcohol as a raw material monomer for the polyester resin.

[0043] As the polyhydric alcohol monomer used in the polyester resin, the following monomers can be used.

[0044] Examples of the dihydric alcohol component include ethylene glycol, propylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 2-ethyl-1,3-hexanediol, hydrogenated bisphenol A, bisphenol and its derivatives represented by formula (A); and diols represented by formula (B). [ka] (In the formula, R is an ethylene or propylene group, x and y are each an integer of 0 or more, and the average value of x+y is 0 or more and 10 or less.) [ka] (In formula (B), R' represents -CH2CH2-, -CH2-CH(CH3)-, or -CH2-C(CH3)2-, x' and y' are integers of 0 or more, and the average value of x+y is 0 to 10.)

[0045] Examples of trihydric or higher alcohol components include sorbitol, 1,2,3,6-hexanetetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methylpropanetriol, 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, and 1,3,5-trihydroxymethylbenzene. Among these, glycerol, trimethylolpropane, and pentaerythritol are preferably used. These dihydric alcohols and trihydric or higher alcohols can be used alone or in combination.

[0046] As the polyvalent carboxylic acid monomer used in the polyester resin, the following monomers can be used.

[0047] Examples of the divalent carboxylic acid component include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, n-dodecenylsuccinic acid, isododecenylsuccinic acid, n-dodecylsuccinic acid, isododecylsuccinic acid, n-octenylsuccinic acid, n-octylsuccinic acid, isooctylsuccinic acid, isooctylsuccinic acid, anhydrides of these acids, and lower alkyl esters thereof. Of these, maleic acid, fumaric acid, terephthalic acid, and n-dodecenylsuccinic acid are preferably used.

[0048] Examples of trivalent or higher carboxylic acids, their acid anhydrides, and their lower alkyl esters include 1,2,4-benzenetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl-2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra(methylenecarboxyl)methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empol trimer acid, their acid anhydrides, and their lower alkyl esters.

[0049] Among these, 1,2,4-benzenetricarboxylic acid, i.e., trimellitic acid or its derivatives, is particularly preferred because it is inexpensive and the reaction can be easily controlled. These divalent carboxylic acids and trivalent or higher carboxylic acids can be used alone or in combination.

[0050] The method for producing the polyester resin is not particularly limited, and a known method can be used. For example, the above-mentioned alcohol monomer and carboxylic acid monomer are simultaneously charged, and polymerized through an esterification reaction or an ester exchange reaction and a condensation reaction to produce the polyester resin. The polymerization temperature is not particularly limited, but is preferably in the range of 180°C to 290°C.

[0051] In the polymerization of polyester, for example, a polymerization catalyst such as a titanium-based catalyst, a tin-based catalyst, zinc acetate, antimony trioxide, or germanium dioxide can be used. A polyester resin polymerized using a tin-based catalyst is more preferred.

[0052] From the viewpoint of low-temperature fixing property and hot offset resistance, the peak molecular weight of the amorphous resin B is preferably 4000 or more and 13000 or less. Also, from the viewpoint of suppressing reaction with the functional group of the thermosetting resin C of the shell layer and from the viewpoint of charging stability in a high-temperature and high-humidity environment, the acid value of the amorphous resin B is preferably 20 mgKOH / g or less. Furthermore, from the viewpoint of charging stability in a high-temperature and high-humidity environment, the hydroxyl value of the amorphous resin B is preferably 40 mgKOH / g or less.

[0053] The amorphous resin may be a mixture of a low molecular weight amorphous resin B and a high molecular weight amorphous resin B'. From the viewpoint of low temperature fixability and hot offset resistance, the content ratio (B / B') of the low molecular weight amorphous resin B to the high molecular weight amorphous resin B' is preferably 60 / 40 or more and 90 / 10 or less by mass. The peak molecular weight of the low-molecular-weight amorphous resin B is preferably 3,000 or more and 8,000 or less from the viewpoint of low-temperature fixability. The peak molecular weight of the high molecular weight amorphous resin B' is preferably more than 8,000 and not more than 30,000 from the viewpoint of hot offset resistance. The weight average molecular weight Mw of the low molecular weight amorphous resin B is preferably 4,000 or more and 10,000 or less from the viewpoint of low temperature fixability. The weight average molecular weight Mw of the high molecular weight amorphous resin B' is preferably more than 10,000 and not more than 100,000 from the viewpoint of hot offset resistance.

[0054] [Thermosetting resin C] The thermosetting resin C is a resin having a site capable of crosslinking with the carboxyl group of the crystalline resin A. The site capable of crosslinking is preferably an oxazoline group. The thermosetting resin C can be obtained, for example, by copolymerization of an oxazoline having a double bond, such as 2-vinyl-2-oxazoline, with a compound having a double bond, such as methyl methacrylate. The constituent monomers of the thermosetting resin C are not particularly limited. The thermosetting resin C may be a polymer of only a monomer having a unit having a site capable of crosslinking. Alternatively, the thermosetting resin C may be a copolymer further containing a compound other than a compound such as methyl methacrylate in addition to a monomer having a unit having a site capable of crosslinking. The weight average molecular weight Mw of the thermosetting resin C is preferably more than 30,000 and not more than 150,000 from the viewpoint of dispersibility.

[0055] [Resin component formed by cross-linking crystalline resin A and thermosetting resin C] An endothermic peak is observed in differential scanning calorimetry (DSC) for the resin component in which crystalline resin A and thermosetting resin C are crosslinked. When thermosetting resin C contains an oxazoline group, the resin component in which crystalline resin A and thermosetting resin C are crosslinked has an amide bond. From the viewpoints of low-temperature fixability and heat-resistant storage stability, it is preferable that the weight-average molecular weight Mw of the resin component formed by the crosslinking reaction of crystalline resin A and thermosetting resin C is 34,000 or more and 200,000 or less.

[0056] As commercially available oxazoline-based crosslinking agents, EPOCROS (registered trademark) K2010E, K2020E, K2030E, WS-300, WS-500, WS-700 (all manufactured by Nippon Shokubai Kagaku Kogyo Co., Ltd.) and the like can also be used.

[0057] It is preferable that the thermosetting resin C does not contain a basic substance. In the shell layer forming step described later, by not including a basic substance in the shell layer, it is possible to prevent inhibition of the crosslinking reaction due to the neutralization reaction of the carboxyl group of the crystalline resin A in the toner core.

[0058] [Release agent] Examples of release agents that can be used in the toner of the present invention include the following: hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof; waxes containing fatty acid esters as the main component such as carnauba wax; and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax.

[0059] Further examples include the following: saturated straight-chain fatty acids such as palmitic acid, stearic acid, and montanic acid; unsaturated fatty acids such as brassidic acid, eleostearic acid, and valinaric acid; saturated alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; polyhydric alcohols such as sorbitol; esters of fatty acids such as palmitic acid, stearic acid, behenic acid, and montanic acid with alcohols such as stearyl alcohol, aralkyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, and melissyl alcohol; fatty acid amides such as linoleic acid amide, oleic acid amide, and lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, hexamethylene Saturated fatty acid bisamides such as bisstearamide; unsaturated fatty acid amides such as ethylene bisoleamide, hexamethylene bisoleamide, N,N' dioleyl adipamide, and N,N' dioleyl sebacamide; aromatic bisamides such as m-xylene bisstearamide and N,N' distearyl isophthalamide; fatty metal salts (commonly known as metal soaps) such as calcium stearate, calcium laurate, zinc stearate, and magnesium stearate; waxes grafted onto aliphatic hydrocarbon waxes using vinyl monomers such as styrene and acrylic acid; partial esters of fatty acids and polyhydric alcohols such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils and fats.

[0060] The content of the release agent is preferably 1 part by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the binder resin. Here, the binder resin refers to the total of the crystalline resin A and the amorphous resin B.

[0061] In addition, in an endothermic curve during temperature rise measured by a differential scanning calorimetry (DSC) device, the peak temperature of the maximum endothermic peak of the wax is preferably 60° C. or more and 110° C. or less. If the peak temperature of the maximum endothermic peak of the wax is within the above range, it is preferable because it is possible to achieve both storage stability and hot offset resistance of the toner.

[0062] [Coloring agent] Colorants that can be contained in the toner of the present invention include the following.

[0063] Examples of black colorants include carbon black, and a mixture of a yellow colorant, a magenta colorant, and a cyan colorant toned to black. As the colorant, a pigment may be used alone, but it is more preferable to use a dye and a pigment in combination to improve the clarity of the colorant from the viewpoint of the image quality of a full-color image.

[0064] Magenta toner pigments include the following: CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48:2, 48:3, 48:4, 49, 50, 51, 52, 53, 54, 55, 57:1, 58, 60, 63, 64, 68, 81:1, 83, 87, 88, 89, 90, 112, 114, 122, 123, 146, 147, 150, 163, 184, 202, 206, 207, 209, 238, 269, 282; CI Pigment Violet 19; CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35.

[0065] Dyes for magenta toners include solvent dyes such as CI Solvent Red 1, 3, 8, 23, 24, 25, 27, 30, 49, 81, 82, 83, 84, 100, 109, 121; CI Disperse Red 9; CI Solvent Violet 8, 13, 14, 21, 27; CI Disperse Violet 1; basic dyes such as CI Basic Red 1, 2, 9, 12, 13, 14, 15, 17, 18, 22, 23, 24, 27, 29, 32, 34, 35, 36, 37, 38, 39, 40; and CI Basic Violet 1, 3, 7, 10, 14, 15, 21, 25, 26, 27, 28.

[0066] Pigments for cyan toners include the following: CI Pigment Blue 2, 3, 15:2, 15:3, 15:4, 16, 17; CI Vat Blue 6; CI Acid Blue 45; copper phthalocyanine pigments having 1 to 5 phthalimidomethyl groups substituted on the phthalocyanine skeleton. Cyan toner dyes include CI Solvent Blue 70.

[0067] Yellow toner pigments include: CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 62, 65, 73, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 185; CI Vat Yellow 1, 3, 20. Yellow toner dyes include CI Solvent Yellow 162.

[0068] The amount of the colorant used is preferably 0.1 parts by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the binder resin.

[0069] [Charge control agent] The toner of the present invention may contain a charge control agent as necessary. Known charge control agents may be used as the charge control agent contained in the toner, but metal compounds of aromatic carboxylic acids are particularly preferred because they are colorless, can charge the toner quickly, and can stably maintain a constant charge amount.

[0070] Examples of the negative charge control agent include metal salicylate compounds, metal naphthoate compounds, metal dicarboxylate compounds, polymeric compounds having sulfonic acid or carboxylic acid on the side chain, polymeric compounds having sulfonate or sulfonate ester on the side chain, polymeric compounds having carboxylate or carboxylate ester on the side chain, boron compounds, urea compounds, silicon compounds, and calixarenes. Examples of the positive charge control agent include quaternary ammonium salts, polymeric compounds having the quaternary ammonium salt on the side chain, guanidine compounds, and imidazole compounds. The charge control agent may be added internally or externally to the toner particles. The amount of the charge control agent added is preferably 0.05 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the binder resin.

[0071] [Inorganic fine particles] The toner may contain inorganic fine particles as required. The inorganic fine particles may be added internally to the toner particles or may be mixed with the toner particles as an external additive. As the external additive, inorganic fine powder such as silica, titanium oxide, and aluminum oxide is preferable. The inorganic fine powder is preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof.

[0072] As an external additive to improve fluidity, 2 / g or more 400m 2 For stable durability, inorganic fine powders with a specific surface area of ​​10 m 2 / g or more 50m 2 In order to simultaneously improve the flowability and stabilize the durability, inorganic fine powders having a specific surface area within the above range may be used in combination.

[0073] The external additive is preferably used in an amount of 0.1 parts by mass to 10.0 parts by mass based on 100 parts by mass of toner particles. The toner particles and the external additive can be mixed using a known mixer such as a Henschel mixer.

[0074] [Developer] The toner of the present invention can be used as a one-component developer, but in order to further improve dot reproducibility, it is preferable to mix it with a magnetic carrier and use it as a two-component developer, and also in terms of obtaining stable images over a long period of time.

[0075] Examples of magnetic carriers that can be used include generally known magnetic carriers such as surface-oxidized or unoxidized iron powder, metal particles such as iron, lithium, calcium, magnesium, nickel, copper, zinc, cobalt, manganese, chromium, and rare earth elements, alloy particles thereof, oxide particles, and magnetic materials such as ferrite, and magnetic material-dispersed resin carriers (so-called resin carriers) that contain a magnetic material and a binder resin that holds the magnetic material in a dispersed state.

[0076] When the toner of the present invention is mixed with a magnetic carrier to be used as a two-component developer, the carrier mixing ratio in the two-component developer is preferably 2% by mass or more and 15% by mass or less in terms of the toner concentration, and more preferably 4% by mass or more and 13% by mass or less, to obtain good results.

[0077] [Manufacturing method] The method for producing the toner particles of the present invention includes a shell layer formation step in which a carboxy group of the crystalline resin A contained in the toner core reacts with a crosslinkable site contained in the thermosetting resin C. The toner core can be produced by a known method such as a dry method such as a pulverization method, or a wet method such as an emulsion aggregation method or a solution suspension method.

[0078] An example of a toner production process using the pulverization method will be described below. In the raw material mixing process, materials constituting the toner particles, such as crystalline resin A, amorphous resin B, and other components such as a release agent, colorant, and charge control agent as necessary, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include a double cone mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid (manufactured by Nippon Coke and Engineering Co., Ltd.).

[0079] Next, the mixed materials are melt-kneaded to disperse the release agent in the binder resin. The kneading discharge temperature can be adjusted appropriately depending on the binder resin and colorant used, but is generally preferably 100 to 180°C. In the melt-kneading process, a batch kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and single-screw or twin-screw extruders are mainstream due to their advantage of being able to be produced continuously. For example, a KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.) can be mentioned. Furthermore, the resin composition obtained by melt-kneading may be rolled with a two-roller or the like, and cooled with water or the like in a cooling process.

[0080] The cooled resin composition is then pulverized to a desired particle size in a pulverization process, which involves coarse pulverization using a pulverizer such as a crusher, hammer mill, or feather mill, followed by further pulverization using a pulverizer such as a Cryptron System (Kawasaki Heavy Industries, Ltd.), a Super Rotor (Nisshin Engineering, Inc.), a Turbo Mill (Freund Turbo, Inc.), or an air jet type pulverizer.

[0081] Thereafter, as necessary, the toner is classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation) to obtain a classified product (toner core). Among these, the Faculty (manufactured by Hosokawa Micron Corporation) is preferred in terms of improving transfer efficiency because it can perform a spheronization process on the toner cores simultaneously with classification.

[0082] Next, the toner cores and a shell material (e.g., an aqueous polymer solution containing an oxazoline group) are mixed in an aqueous medium to obtain a dispersion. Next, the dispersion is reacted at a predetermined temperature while being stirred to form a shell layer. For example, when the shell material is an aqueous polymer solution containing an oxazoline group, the formed shell layer has a resin component containing a unit having an oxazoline group and a unit having an amide bond. In the case of the present invention, the amide bond is formed by the reaction between the oxazoline group of the thermosetting resin C of the shell material and the carboxy group of the crystalline resin A contained in the toner core.

[0083] The above-mentioned predetermined temperature is preferably 50°C or higher and 70°C or lower. At this time, a carboxylic acid such as acetic acid as a ring-opening agent or a basic substance such as ammonia or sodium hydroxide as a reaction inhibitor may be added. The progress of the crosslinking reaction can be adjusted by the reaction temperature, reaction time, and additives, and the thickness of the shell layer and the interface state between the core part and the shell layer can be adjusted. The aqueous medium is a medium containing water as a main component and may contain alcohol miscible with water. After the shell layer is formed, the mixture is cooled to room temperature, and the dispersion of the toner particles is filtered, washed, and dried using a Buchner funnel to obtain toner particles.

[0084] The toner particles may be used as they are as a toner, or may be used as a toner by adding an external additive to the surface of the toner particles as necessary. Methods for adding external additives include a method in which a predetermined amount of a known external additive is mixed with the toner particles, and the mixture is stirred and mixed using a mixing device such as a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), or a Nobilta (manufactured by Hosokawa Micron Corporation) as an external additive machine.

[0085] Next, the methods for measuring the various physical properties related to the present invention will be described. [Isolation of crystalline resin A, amorphous resin B, thermosetting resin C, and resin components crosslinked between crystalline resin A and thermosetting resin C from toner] The physical properties of crystalline resin A, amorphous resin B, thermosetting resin C, and the resin component obtained by polymerizing crystalline resin A and thermosetting resin C, which are isolated by the following method, can be measured. First, the toner is mixed with a solvent such as THF and stirred at room temperature or under heat to dissolve the resin components: crystalline resin A, amorphous resin B, thermosetting resin C, and the polymerized mixture of crystalline resin A and thermosetting resin C. Next, insoluble matters contained in the obtained solution, such as external additives, release agents, charge control agents, colorants (pigments, etc.), etc., are removed by centrifugation, filtration, washing, etc. Thereafter, by using, for example, GPC or high performance liquid chromatography (HPLC) equipped with a separation mechanism, it is possible to isolate the crystalline resin A, the amorphous resin B, the thermosetting resin C, and the resin components in which the crystalline resin A and the thermosetting resin C are crosslinked. The solvent is preferably removed by evaporation, and examples of the method for evaporating the solvent include heating, reducing pressure, and ventilation.

[0086] [Molecular weight measurement of resin by GPC] First, the resin is dissolved in o-dichlorobenzene or THF at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Maeshori Disk" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is preferably adjusted so that the concentration of components soluble in THF is about 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC-8121GPC / HT (Tosoh Corporation) Column: TSKgel GMHHR-H HT 7.8cm ID x 30cm 2-way (Tosoh Corporation) Detector: High temperature RI Temperature: 135℃ Solvent: o-dichlorobenzene (with 0.05% ionol) or THF Flow rate: 1.0ml / min Sample: 0.4 ml of 0.1% sample injected The measurement is performed under the above conditions, and the molecular weight of the sample is calculated using a molecular weight calibration curve made with monodisperse polystyrene standard samples. Furthermore, the molecular weight is calculated by converting it into polyethylene using a conversion formula derived from the Mark-Houwink viscosity formula.

[0087] [Method for measuring the softening point of amorphous resin B] The softening point of resin B is measured using a constant load extrusion type capillary rheometer "Flow characteristic evaluation device Flow Tester CFT-500D" (manufactured by Shimadzu Corporation) according to the manual that comes with the device. With this device, a constant load is applied from above the measurement sample with a piston while the measurement sample filled in a cylinder is heated and melted, and the molten measurement sample is extruded from the die at the bottom of the cylinder, and a flow curve showing the relationship between the piston descent amount and temperature can be obtained.

[0088] In the present invention, the "melting temperature in the 1 / 2 method" described in the manual attached to the "Flow characteristic evaluation device Flow Tester CFT-500D" is used as the softening point. The melting temperature in the 1 / 2 method is calculated as follows. First, 1 / 2 of the difference between the amount of piston descent Smax at the time when the outflow ends and the amount of piston descent Smin at the time when the outflow starts is calculated (this is designated as X; X=(Smax-Smin) / 2). Then, the temperature of the flow curve when the amount of piston descent on the flow curve is X is the melting temperature in the 1 / 2 method.

[0089] The measurement sample is prepared by compressing approximately 1.0 g of resin at approximately 10 MPa for approximately 60 seconds using a tablet molding machine (e.g., NT-100H, manufactured by NPA Systems) in an environment of 25°C to form a cylindrical shape with a diameter of approximately 8 mm.

[0090] The measurement conditions for the CFT-500D are as follows. Test mode: Temperature rise method Starting temperature: 50℃ Achieved temperature: 200℃ Measurement interval: 1.0℃ Heating rate: 4.0℃ / min Piston cross-sectional area: 1.000cm 2 Test load (piston load): 10.0kgf (0.9807MPa) Preheat time: 300 seconds Die hole diameter: 1.0mm Die length: 1.0mm

[0091] [Measurement of glass transition temperature (Tg) of amorphous resin B] The glass transition temperature of the resin is measured using a differential scanning calorimeter "Q2000" (manufactured by TA Instruments) in accordance with ASTM D3418-82. The melting points of indium and zinc are used for temperature correction of the device detection section, and the heat of fusion of indium is used for heat correction.

[0092] Specifically, about 3 mg of resin or toner is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and measurement is performed under the following conditions. Heating rate: 10℃ / min Measurement start temperature: 30℃ End of measurement temperature: 180℃ Measurements are performed at a heating rate of 10°C / min in the measurement range of 30 to 180°C. The temperature is raised to 180°C once and held for 10 minutes, then cooled to 30°C, and then raised again. During this second heating process, the specific heat change is obtained in the temperature range of 30 to 100°C. The point at which the line midway between the baselines before and after the specific heat change appears and the differential thermal curve intersects is taken as the glass transition temperature (Tg) of the resin.

[0093] [Measurement of melting points of crystalline resin A and release agent] The melting points of indium and zinc are used for temperature correction of the device detection unit, and the heat of fusion of indium is used for heat correction. Specifically, about 2 mg of sample is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and the measurement is performed at a temperature rise rate of 10°C / min in the measurement temperature range of 30 to 200°C. In the measurement, the temperature is raised to 200°C once, then lowered to 30°C, and then raised again. The peak temperature of the maximum endothermic peak of the DSC curve in the temperature range of 30 to 200°C during this second heating process is taken as the melting point. There is no holding time after the temperature is raised to 200°C, and the temperature is lowered to 30°C immediately after reaching 200°C.

[0094] [Method for measuring weight-average particle size (D4) of toner particles] The weight-average particle diameter (D4) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 100 μm aperture tube, and the accompanying dedicated software for setting measurement conditions and analyzing measurement data, "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), and the measurement data is analyzed and calculated.

[0095] The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).

[0096] Before carrying out the measurements and analyses, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 2 μm to 60 μm.

[0097] The specific measurement method is as follows. (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube.

[0098] (2) Approximately 30 ml of the above-mentioned aqueous electrolyte solution is placed in a 100 ml flat-bottom glass beaker, and approximately 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, with a pH of 7, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water is added as a dispersant.

[0099] (3) A specified amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) that has two oscillators with an oscillation frequency of 50 kHz built in with a phase shift of 180 degrees and an electrical output of 120 W, and approximately 2 ml of the Conaminon N is added to this water tank.

[0100] (4) The beaker (2) is set in the beaker fixing hole of the ultrasonic disperser, and the ultrasonic disperser is operated. Then, the height position of the beaker is adjusted so that the resonance state of the liquid surface of the electrolyte solution in the beaker is maximized.

[0101] (5) While the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted to be 10°C or higher and 40°C or lower.

[0102] (6) Using a pipette, add the electrolyte solution (5) in which the toner is dispersed to the round-bottom beaker (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000.

[0103] (7) The measurement data is analyzed using the dedicated software that comes with the device, and the weight-average particle size (D4) is calculated. Note that when the dedicated software is set to Graph / Volume%, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the weight-average particle size (D4).

[0104] [Method for measuring average circularity of toner] The average circularity of the toner is measured using a flow type particle image analyzer "FPIA-3000" (manufactured by Sysmex Corporation) under the measurement and analysis conditions during the calibration process.

[0105] The measurement principle of the flow-type particle image analyzer "FPIA-3000" (Sysmex Corporation) is to capture still images of flowing particles and perform image analysis. The sample added to the sample chamber is sent to the flat sheath flow cell by the sample suction syringe. The sample sent to the flat sheath flow is sandwiched between the sheath liquid and forms a flat flow. The sample passing through the flat sheath flow cell is irradiated with a strobe light at 1 / 60 second intervals, making it possible to capture still images of the flowing particles. In addition, since the flow is flat, the image is captured in focus. The particle images are captured by a CCD camera, and the captured images are processed with an image processing resolution of 512 x 512 pixels (0.37 x 0.37 μm per pixel), and the contours of each particle image are extracted, and the projected area S and perimeter L of the particle image are measured.

[0106] Next, the equivalent circle diameter and circularity are calculated using the above area S and perimeter L. The equivalent circle diameter is the diameter of a circle having the same area as the projected area of ​​the particle image, and the circularity C is defined as the perimeter of the circle calculated from the equivalent circle diameter divided by the perimeter of the projected particle image, and is calculated using the following formula. Circularity C=2×(π×S)1 / 2 / L

[0107] When the particle image is circular, the circularity is 1.000, and the greater the degree of unevenness of the particle image periphery, the smaller the circularity value. After calculating the circularity of each particle, the range of circularity from 0.200 to 1.000 is divided into 800, and the arithmetic mean of the obtained circularities is calculated, and this value is regarded as the average circularity.

[0108] The specific measurement method is as follows. First, about 20 ml of ion-exchanged water from which impurities such as solids have been removed is placed in a glass container. About 0.2 ml of a dilution obtained by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7, consisting of a nonionic surfactant, an anionic surfactant, and an organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) with ion-exchanged water by about 3 times by weight as a dispersant is added thereto. Furthermore, about 0.02 g of a measurement sample is added, and a dispersion process is performed for 2 minutes using an ultrasonic disperser to obtain a dispersion liquid for measurement. At that time, the dispersion liquid is appropriately cooled so that the temperature is 10°C or higher and 40°C or lower. As the ultrasonic disperser, a tabletop ultrasonic cleaner disperser (e.g., "VS-150" (manufactured by Vervoclear Co., Ltd.) with an oscillation frequency of 50 kHz and an electrical output of 150 W is used, a predetermined amount of ion-exchanged water is placed in the water tank, and about 2 ml of the Contaminon N is added to the water tank.

[0109] For the measurement, the flow type particle image analyzer equipped with a standard objective lens (10x) was used, and the particle sheath "PSE-900A" (manufactured by Sysmex Corporation) was used as the sheath liquid. The dispersion liquid prepared according to the procedure was introduced into the flow type particle image analyzer, and 3000 toner particles were measured in HPF measurement mode and total count mode. Then, by setting the binarization threshold value during particle analysis to 85% and specifying the analyzed particle diameter, the number ratio (%) of particles in that range and the average circularity can be calculated. The average circularity of the toner was calculated with a circle equivalent diameter of 1.98 μm or more and 39.96 μm or less.

[0110] Before starting the measurement, automatic focus adjustment is performed using standard latex particles (e.g., Duke Scientific's "RESEARCH AND TEST PARTICLES Latex Microsphere Suspensions 5200A" diluted with ion-exchanged water). After that, it is preferable to perform focus adjustment every 2 hours from the start of the measurement.

[0111] In the examples of the present application, a flow-type particle image analyzer was used that had been calibrated by Sysmex Corp. and had a calibration certificate issued by Sysmex Corp. Except for limiting the particle diameter to be analyzed to a circle-equivalent diameter of 1.98 μm or more and less than 39.69 μm, measurements were performed under the same measurement and analysis conditions as when the calibration certificate was received.

[0112] [Acid value measurement method] In the present invention, the acid value is the mass [mg] of potassium hydroxide required to neutralize the acid contained in 1 g of a sample. In other words, the acid value is the mass [mg] of potassium hydroxide required to neutralize the free fatty acids and resin acids contained in 1 g of a sample.

[0113] In the present invention, the acid value was measured in accordance with JIS K 0070-1992. Specifically, the acid value was measured according to the following procedure.

[0114] (1) Preparation of reagents 1.0 g of phenolphthalein was dissolved in 90 mL of ethyl alcohol (95% by volume), and ion-exchanged water was added to make up to 100 mL to obtain a phenolphthalein solution. 7 g of special grade potassium hydroxide was dissolved in 5 mL of water, and ethyl alcohol (95% by volume) was added to make 1 L. The solution was left in an alkali-resistant container for 3 days to avoid contact with carbon dioxide gas, etc. After leaving it, it was filtered to obtain a potassium hydroxide solution. The obtained potassium hydroxide solution was stored in an alkali-resistant container. The factor of the potassium hydroxide solution was calculated from the amount of the potassium hydroxide solution required for neutralization by placing 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution. The 0.1 mol / L hydrochloric acid prepared in accordance with JIS K 8001-1998 was used.

[0115] (2) Operation (A) Main Test 2.0 g of sample was weighed precisely in a 200 mL Erlenmeyer flask, and 100 mL of a mixed solution of toluene / ethanol (2:1) was added and the sample was dissolved for 5 hours. Then, several drops of the above phenolphthalein solution were added as an indicator, and titration was performed using the above potassium hydroxide solution. The end point of the titration was when the light red color of the indicator continued for 30 seconds.

[0116] (B) Blank test The same titration as above was carried out, except that no sample was added (that is, only the mixed solution of toluene / ethanol (2:1) was used).

[0117] (3) Calculation of acid value The obtained results were substituted into the following formula to calculate the acid value. AV = [(BA) × f × 5.61] / S In the above formula, AV represents the acid value [mgKOH / g], A represents the amount of potassium hydroxide solution added in the blank test [mL], B represents the amount of potassium hydroxide solution added in the main test [mL], f represents the factor of the potassium hydroxide solution, and S represents the mass of the sample [g]. In the present invention, when amorphous resin B and amorphous resin B' were mixed and used, 1 g of the mixed sample was used to measure the acid value.

[0118] [Method for measuring hydroxyl value] The hydroxyl value is the amount of potassium hydroxide (mg) required to neutralize the acetic acid bonded to the hydroxyl group when 1 g of a sample is acetylated. The hydroxyl value of the binder resin is measured in accordance with JIS K 0070-1992, and more specifically, it is measured according to the following procedure.

[0119] (1) Preparation of reagents Put 25 g of special grade acetic anhydride into a 100 ml measuring flask, add pyridine to make the total volume 100 ml, and shake thoroughly to obtain an acetylation reagent. Store the obtained acetylation reagent in a brown bottle to avoid contact with moisture, carbon dioxide, etc. Dissolve 1.0 g of phenolphthalein in 90 ml of ethyl alcohol (95 vol%) and add ion-exchanged water to make 100 ml to obtain a phenolphthalein solution. Dissolve 35g of special grade potassium hydroxide in 20ml of water and add ethyl alcohol (95vol%) to make 1L. Leave in an alkali-resistant container for 3 days without contacting with carbon dioxide gas, etc., and then filter to obtain potassium hydroxide solution. Store the obtained potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is obtained by placing 25ml of 0.5 mol / L hydrochloric acid in an Erlenmeyer flask, adding several drops of the phenolphthalein solution, and titrating with the potassium hydroxide solution, from the amount of the potassium hydroxide solution required for neutralization. The 0.5 mol / L hydrochloric acid used is prepared in accordance with JIS K 8001-1998.

[0120] (2) Operation (A) Main Test Weigh out 1.0 g of sample into a 200 ml round-bottom flask, and add 5.0 ml of the acetylation reagent using a volumetric pipette. If the sample is difficult to dissolve in the acetylation reagent, add a small amount of special grade toluene to dissolve it. Place a small funnel on the mouth of the flask and immerse about 1 cm of the bottom of the flask in a glycerin bath at about 97°C and heat it. At this time, it is preferable to cover the base of the neck of the flask with a piece of cardboard with a round hole in it to prevent the temperature of the neck of the flask from rising due to the heat of the bath. After 1 hour, remove the flask from the glycerin bath and allow it to cool. After allowing it to cool, add 1 ml of water through the funnel and shake to hydrolyze the acetic anhydride. To further hydrolyze it completely, heat the flask again in the glycerin bath for 10 minutes. After allowing it to cool, wash the funnel and the walls of the flask with 5 ml of ethyl alcohol. Add a few drops of the phenolphthalein solution as an indicator and titrate with the potassium hydroxide solution. The end point of the titration is when the light red color of the indicator continues for about 30 seconds.

[0121] (B) Blank test The titration is carried out in the same manner as above, except that no sample is used.

[0122] (3) The obtained result is substituted into the following formula to calculate the hydroxyl value. A = [{(BC) × 28.05 × f} / S] + D Here, A: hydroxyl value (mgKOH / g), B: amount of potassium hydroxide solution added for the blank test (ml), C: amount of potassium hydroxide solution added for the main test (ml), f: factor of the potassium hydroxide solution, S: sample (g), D: acid value of the sample (mgKOH / g).

[0123] [Measuring the thickness of the shell layer of toner particles] The thickness of the shell layer of the toner particle can be measured by observing a cross section with a transmission electron microscope (TEM) as follows. Using an osmium plasma coater (Filgen, OPC80T), an Os film (5 nm) and a naphthalene film (20 nm) were applied to the toner as a protective film, which was then embedded in photocurable resin D800 (JEOL). Then, a toner particle cross-section with a film thickness of 60 nm (or 70 nm) was prepared using an ultrasonic ultramicrotome (Leica, UC7) at a cutting speed of 1 mm / s. The obtained cross section was stained for 15 minutes in a RuO4 gas atmosphere of 500 Pa using a vacuum electron staining device (Filgen, VSC4R1H) and subjected to STEM observation using a TEM (JEOL, JEM2800). The STEM probe size was 1 nm, and the image size was 1024 x 1024 pixels. The obtained image was binarized (threshold 120 / 255 steps) using image processing software "Image-Pro Plus (Media Cybernetics)". The obtained image was binarized to extract the shell in the toner particle and measure its thickness. The thickness was measured at four points, top, bottom, left and right, for one toner particle, and the average shell thickness per toner particle was calculated. The same measurement was performed on 20 randomly selected toner particles, and the average value was calculated to be the shell layer thickness of the toner particle in the present invention.

[0124] [Measurement of BET specific surface area of ​​inorganic fine particles] The BET specific surface area of ​​the inorganic fine particles was measured in accordance with JIS Z8830 (2001). The specific measurement method is as follows. The measurement device used was the "Automatic Specific Surface Area / Porosity Distribution Measurement Device TriStar3000 (manufactured by Shimadzu Corporation)" which uses the constant volume gas adsorption method as the measurement method. The measurement conditions were set and the measurement data was analyzed using the dedicated software "TriStar3000 Version4.00" that comes with this device, and the device was connected to a vacuum pump, nitrogen gas piping, and helium gas piping. Nitrogen gas was used as the adsorption gas, and the value calculated by the BET multipoint method was taken as the BET specific surface area of ​​the inorganic microparticles in the present invention.

[0125] The BET specific surface area was calculated as follows. First, nitrogen gas is adsorbed onto the inorganic fine particles, and the equilibrium pressure P (Pa) in the sample cell and the amount of nitrogen adsorbed by the external additive Va (mol g -1 The relative pressure Pr, which is the equilibrium pressure P (Pa) in the sample cell divided by the saturated vapor pressure Po (Pa) of nitrogen, is plotted on the horizontal axis, and the amount of nitrogen adsorption Va (mol g -1 Next, the amount of adsorption required to form a monolayer on the surface of the external additive, Vm (mol g -1 ) was calculated by applying the BET equation below. Pr / Va(1-Pr)=1 / (Vm×C)+(C-1)×Pr / (Vm×C) (Here, C is the BET parameter, which varies depending on the type of sample to be measured, the type of adsorbed gas, and the adsorption temperature.) The BET equation can be interpreted as a straight line with a slope of (C-1) / (Vm×C) and an intercept of 1 / (Vm×C) when the X-axis is Pr and the Y-axis is Pr / Va(1-Pr) (this straight line is called a BET plot). Slope of the line = (C-1) / (Vm×C) Line intercept = 1 / (Vm×C) By plotting the measured values ​​of Pr and Pr / Va(1-Pr) on a graph and drawing a line using the least squares method, the slope and intercept of the line can be calculated. By using these values ​​to solve the simultaneous equations for the slope and intercept, Vm and C can be calculated. Furthermore, the calculated Vm and the molecular occupancy cross section of the nitrogen molecule (0.162 nm 2 ) and the BET specific surface area S (m 2 / g) is calculated. S = Vm × N × 0.162 × 10 -18 (where N is Avogadro's number (mol -1 )

[0126] Measurements using this device were performed in accordance with the "TriStar3000 Instruction Manual V4.0" that came with the device, and specifically, the measurements were performed in the following procedure. The tar of a thoroughly washed and dried special glass sample cell (stem diameter 3 / 8 inch, volume approximately 5 ml) was precisely weighed. Then, approximately 0.1 g of the external additive was placed in the sample cell using a funnel. The sample cell containing the inorganic fine particles was set in a "pretreatment device VacuPrep 061 (manufactured by Shimadzu Corporation)" connected to a vacuum pump and nitrogen gas piping, and vacuum degassing was continued for about 10 hours at 23°C. During vacuum degassing, the valve was adjusted to gradually degas the inorganic fine particles so that they would not be sucked into the vacuum pump. The pressure in the cell gradually decreased with degassing, and finally reached about 0.4 Pa (about 3 mTorr). After completion of vacuum degassing, nitrogen gas was gradually injected to return the inside of the sample cell to atmospheric pressure, and the sample cell was removed from the pretreatment device. The mass of this sample cell was then precisely weighed, and the exact mass of the external additive was calculated from the difference with the tare weight. During this time, the sample cell was covered with a rubber stopper during weighing to prevent the external additive in the sample cell from being contaminated by moisture in the air.

[0127] Next, a special "isothermal jacket" was attached to the stem of the sample cell containing the inorganic fine particles. A special filler rod was then inserted into the sample cell, and the sample cell was set in the analysis port of the device. The isothermal jacket is a cylindrical member whose inner surface is made of a porous material and whose outer surface is made of an impermeable material, and which is capable of sucking up liquid nitrogen to a certain level by capillary action.

[0128] Next, the free space of the sample cell including the connecting device was measured. The free space was calculated by measuring the volume of the sample cell at 23°C using helium gas, then measuring the volume of the sample cell after cooling it with liquid nitrogen in the same manner using helium gas, and converting it from the difference between these volumes. The saturated vapor pressure Po (Pa) of nitrogen was also measured automatically using a Po tube built into the device.

[0129] Next, the sample cell was evacuated, and then cooled with liquid nitrogen while continuing the evacuated state. Nitrogen gas was then gradually introduced into the sample cell to adsorb nitrogen molecules to the toner. At this time, the adsorption isotherm was obtained by measuring the equilibrium pressure P (Pa) at any time, and this adsorption isotherm was converted into a BET plot. The relative pressure Pr points for collecting data were set to 0.05, 0.10, 0.15, 0.20, 0.25, and 0.30, for a total of six points. A straight line was drawn by the least squares method for the obtained measurement data, and Vm was calculated from the slope and intercept of the straight line. Furthermore, the BET specific surface area of ​​the inorganic fine particles was calculated using this Vm value as described above. EXAMPLES

[0130] The present invention will be described below with reference to examples, etc. However, the description of these examples does not limit the technical scope of the present invention.

[0131] <Production Example of Crystalline Resin A1> Hexanediol: 30.4 parts by mass (46.0 mol%) Dodecanedioic acid: 69.6 parts by mass (54.0 mol%) The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 140°C with stirring. Tin 2-ethylhexanoate: 0.5 parts by weight Thereafter, the above materials were added, the pressure in the reaction vessel was reduced to 8.3 kPa, and the reaction was carried out for 4 hours while maintaining the temperature at 200° C., thereby obtaining crystalline resin A1. The obtained crystalline resin A1 had a weight average molecular weight Mw of 12000, an acid value of 33.0 mgKOH / g, and a hydroxyl value of 3.0 mgKOH / g.

[0132] <Production Example of Crystalline Resin A2> Hexanediol: 32.5 parts by mass (47.0 mol%) Dodecanedioic acid: 67.5 parts by mass (50.0 mol%) Tin 2-ethylhexanoate: 0.5 parts by weight The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. After replacing the atmosphere in the flask with nitrogen gas, the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 140°C with stirring. Next, the above materials were added, the pressure in the reaction vessel was reduced to 8.3 kPa, and the temperature was maintained at 200° C. while the reaction was carried out for 4 hours. Furthermore, the pressure in the reaction vessel was gradually released to return to normal pressure, and then 5.0 parts by mass (3.0 mol%) of stearic acid was added and reacted at 200° C. for 2 hours under normal pressure. Thereafter, the pressure in the reaction tank was reduced to 5 kPa or less again, and the reaction was carried out at 200° C. for 3 hours to obtain a crystalline polyester resin A2. The obtained crystalline resin A2 had a weight average molecular weight Mw of 12000, an acid value of 26.0 mgKOH / g, and a hydroxyl value of 2.0 mgKOH / g.

[0133] <Production Examples of Crystalline Resins A3 to A10> Crystalline Resins A3 to A10 were obtained by carrying out the reaction in the same manner as in the production example of Crystalline Resin A2, except that the monomers used were changed as shown in Table 1. The compositions and physical properties of the obtained Crystalline Resins A3 to A10 are shown in Table 1.

[0134] [Table 1]

[0135] <Production Example of Amorphous Resin B1> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane (BPA-PO): 68.2 parts by mass (49.0 mol%) Terephthalic acid: 24.7 parts by mass (38.0 mol%) ·Adipic acid: 5.7 parts by mass (10.0 mol%) ·Benzoic acid: 1.4 parts by mass (3.0 mol%) Titanium tetrabutoxide (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 5 hours at a temperature of 200°C with stirring. Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 160 and returned to atmospheric pressure (first reaction step). tert-Butylcatechol (polymerization inhibitor): 0.1 parts by mass The above materials were then added, the pressure in the reaction vessel was lowered to 8.3 kPa, and the reaction was carried out for 1 hour while maintaining the temperature at 180°C. After confirming that the softening point measured according to ASTM D36-86 reached 88°C, the temperature was lowered to stop the reaction, and amorphous resin B1 was obtained. The glass transition point of amorphous resin B1 was 49°C, the acid value was 6.0 mgKOH / g, and the hydroxyl value was 32.0 mgKOH / g.

[0136] <Production Examples of Amorphous Resins B2 to B5> Amorphous resins B2 to B5 were obtained by carrying out the reaction in the same manner as in Production Example of Amorphous Resin B1, except that the monomers used were changed as shown in Table 2. The compositions and physical properties of the obtained Amorphous Resins B2 to B5 are shown in Table 2.

[0137] <Production Example of Amorphous Resin B6> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane (BPA-PO): 71.4 parts by mass (55.0 mol%) Terephthalic acid: 22.4 parts by mass (37.0 mol%) Titanium tetrabutoxide (esterification catalyst): 0.5 parts by mass The above materials were weighed and placed in a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the reaction was carried out for 2 hours at a temperature of 200°C with stirring. Furthermore, the pressure inside the reaction vessel was reduced to 8.3 kPa and maintained for 1 hour, after which it was cooled to 160 and returned to atmospheric pressure (first reaction step). Trimellitic anhydride: 6.2 parts by mass (8.0 mol%) tert-Butylcatechol (polymerization inhibitor): 0.1 parts by mass The above materials were then added, the pressure in the reaction vessel was lowered to 8.3 kPa, and the reaction was continued for 15 hours while maintaining the temperature at 200° C. After it was confirmed that the softening point measured according to ASTM D36-86 reached 140° C., the temperature was lowered to terminate the reaction (second reaction step), thereby obtaining amorphous resin B6. The composition and physical properties of the obtained amorphous resin B6 are shown in Table 2.

[0138] [Table 2]

[0139] <Production Example of Amorphous Resin B7> 100 parts by mass of xylene, 97.5 parts by mass of styrene, and 2.5 parts by mass of acrylic acid were charged into a reaction vessel, mixed, and the resulting mixture was heated to 75°C. Under a nitrogen atmosphere, a solution of 5.0 parts by mass of tert-butyl hydroperoxide, a radical polymerization initiator, dissolved in 10.0 parts by mass of xylene was dropped into the mixture over about 30 minutes. The mixture was then kept at that temperature for 5 hours to terminate the radical polymerization reaction. The mixture was then heated and decompressed to remove 60.0 parts by mass of xylene, thereby obtaining a reaction solution. Meanwhile, 500.0 parts by mass of methanol was charged into a vessel equipped with an agitator and stirred. The above reaction solution was added dropwise thereto over 1 hour, and the resulting precipitate was filtered, washed, and then dried to obtain amorphous resin B7. The glass transition point was 55°C, the softening point was 110°C, and the acid value was 17mgKOH / g.

[0140] <Release agent> The release agent used in the present invention was Fischer-Tropsch wax, which had a maximum endothermic peak temperature of 90° C. and an acid value of 0 mgKOH / g.

[0141] <Production Example of Dispersion of Thermosetting Resin C> 1200 parts by mass of water, 5 parts by mass of sodium persulfate, 70 parts by mass of 2-vinyl-2-oxazoline, and 30 parts by mass of methyl acrylate were charged into a reaction vessel and heated to 60°C under a nitrogen atmosphere. Stirring was continued for 8 hours to complete the reaction, and then the mixture was cooled to obtain a 10% dispersion of thermosetting resin C. The weight average molecular weight of thermosetting resin C was 50,000.

[0142] <Production Example of Dispersion of Amorphous Resin B7> 400 parts by mass of tetrahydrofuran (manufactured by Wako Pure Chemical Industries, Ltd.), 100 parts by mass of amorphous resin B7, and 0.7 parts by mass of anionic surfactant Neogen RK (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were mixed and dissolved. Then, 20.0 g of 1 mol / L ammonia water was added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Co., Ltd.). Furthermore, 700 g of ion-exchanged water was added at a rate of 8 g / min to precipitate amorphous resin fine particles. Then, tetrahydrofuran was removed using an evaporator, and the concentration was adjusted with ion-exchanged water to obtain an aqueous dispersion of amorphous resin fine particles B7 at a concentration of 10% (amorphous resin fine particle B7 dispersion). This dispersion was used when forming the shell layer of toner 19 described in Table 3.

[0143] <Toner Production Example 1> <Creating the toner core> ·Crystalline resin A1 10 parts by mass ·Amorphous resin B1 70 parts by mass ·Amorphous resin B6 30 parts by mass Release agent: 4 parts by weight CI Pigment Blue 15:3 5 parts by weight 0.5 parts by weight of 3,5-di-t-butylsalicylic acid aluminum compound The above materials were mixed in a Henschel mixer (FM-75, manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotation speed of 20 s -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at a discharge temperature of 140°C in a twin-screw kneader (PCM-30, Ikegai Corporation) set at a temperature of 130°C. The kneaded mixture was cooled and coarsely crushed to 1 mm or less in a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed in a mechanical crusher (T-250, Freund Turbo Corporation). It was further classified using a Faculty F-300 (Hosokawa Micron Corporation) to obtain toner core 1. The operating conditions were a classifying rotor rotation speed of 130 s -1 , Dispersion rotor speed 120s -1 It was decided.

[0144] <Shell layer formation process> A 1 L three-neck flask equipped with a stirring blade was set in a water bath, and 100 parts by mass of toner core 1 and 300 ml of a 20% by mass aqueous solution of 2-propanol were added to the flask, and the temperature inside the flask was raised to 60° C. while stirring the contents of the flask at a rotation speed of 150 rpm. Next, a dispersion liquid of thermosetting resin C was added to the flask. The amount added was such that the thickness of the shell layer became the value shown in Table 1. After that, stirring was continued for 30 minutes while maintaining the temperature at 60° C., and then the dispersion liquid was filtered, washed, and dried to obtain toner particles 1.

[0145] <External addition process> To 100 parts by mass of toner particles 1, 1.0 part by mass of hydrophobic silica fine particles surface-treated with 4% by mass of hexamethyldisilazane (BET: 25 m 2 / g), hydrophobic silica (BET:200m 2 / g) 1.0 part, and titanium oxide fine particles surface-treated with isobutyltrimethoxysilane (BET: 80m 2 1.0 part of 1 / g of 1000g of water was mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s.-1 The mixture was mixed at a rotation time of 5 minutes to obtain toner 1. The weight average particle size (D4) of toner 1 was 6.5 μm, and the average circularity of the toner was 0.96.

[0146] <Production Examples of Toners 2 to 24> Toners 2 to 24 were obtained in the same manner as in the production example of toner 1, except that the crystalline resin A, the amorphous resin B, the resin of the shell layer, and the thickness of the shell layer were changed as shown in Table 3. The thickness of the shell layer tended to increase as the amount of thermosetting resin C added increased.

[0147] [Table 3]

[0148] <Production Example of Magnetic Core Particle 1> Step 1 (weighing and mixing): Fe2O362.7 parts by mass MnCO329.5 parts by mass Mg(OH)26.8 parts by mass SrCO31.0 parts by mass The ferrite raw materials were weighed so as to obtain the above composition ratio, and then pulverized and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch.

[0149] Step 2 (Pre-firing): The obtained pulverized material was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the calcined ferrite obtained was as follows: (MnO)a(MgO)b(SrO)c(Fe2O3)d In the above formula, a = 0.257, b = 0.117, c = 0.007, d = 0.393

[0150] Step 3 (Crushing): After crushing to about 0.3 mm using a crusher, 30 parts by mass of water was added to 100 parts by mass of the calcined ferrite using zirconia beads with a diameter of 1 / 8 inch, and the mixture was crushed in a wet ball mill for 1 hour. The slurry was crushed for 4 hours in a wet ball mill using alumina beads with a diameter of 1 / 16 inch to obtain a ferrite slurry (finely crushed calcined ferrite).

[0151] ·Process 4 (granulation process): To the ferrite slurry, 1.0 parts by mass of ammonium polycarboxylate as a dispersant and 2.0 parts by mass of polyvinyl alcohol as a binder were added per 100 parts by mass of the calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufacturer: Okawara Kakoki). After adjusting the particle size of the resulting particles, the mixture was heated at 650°C for 2 hours using a rotary kiln to remove the organic components of the dispersant and binder.

[0152] Step 5 (firing): In order to control the firing atmosphere, the material was heated from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1150°C for 4 hours. The material was then cooled to 60°C over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40°C or less.

[0153] Step 6 (sorting step): After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 having a volume distribution standard 50% particle size (D50) of 37.0 μm.

[0154] <Preparation of Coating Resin 1> Cyclohexyl methacrylate monomer 26.8% by mass Methyl methacrylate monomer 0.2% by mass Methyl methacrylate macromonomer 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3% by mass Methyl ethyl ketone 31.3% by mass Azobisisobutyronitrile 2.0% by mass Among the above materials, cyclohexyl methacrylate, methyl methacrylate, methyl methacrylate macromonomer, toluene, and methyl ethyl ketone were added to a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, and nitrogen gas was introduced to create a sufficient nitrogen atmosphere, and then the mixture was heated to 80°C, azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate a copolymer, and the precipitate was filtered and then vacuum dried to obtain coating resin 1. The resulting coating resin 1 was dissolved in 30 parts by mass, 40 parts by mass of toluene, and 30 parts by mass of methyl ethyl ketone to obtain polymer solution 1 (solid content 30% by mass).

[0155] <Preparation of coating resin solution 1> Polymer solution 1 (resin solids concentration 30%) 33.3% by mass Toluene 66.4% by mass Carbon black (Regal 330; manufactured by Cabot Corporation) 0.3% by mass (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m 2 / g, DBP oil absorption 75ml / 100g) The mixture was dispersed for 1 hour using a paint shaker with zirconia beads having a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.

[0156] <Magnetic Carrier 1 Manufacturing Example> (Resin coating process): The coating resin solution 1 was added to a vacuum degassing kneader maintained at room temperature so that the resin component was 2.5 parts by mass per 100 parts by mass of the filled core particles 1. After addition, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes, and after a certain amount of the solvent (80% by mass) had evaporated, the mixture was heated to 80°C while mixing under reduced pressure, and the toluene was distilled off over 2 hours, after which it was cooled. The magnetic carrier obtained was separated into low magnetic products by magnetic separation, passed through a sieve with an opening of 70 μm, and then classified with a wind classifier to obtain magnetic carrier 1 having a 50% particle size (D50) of 38.2 μm based on volume distribution.

[0157] <Example of manufacturing two-component developer> Mix toners 1 to 24 and magnetic carrier 1 in a V-type mixer (V-10 type: Tokuju Manufacturing Co., Ltd.) for 0.5 s so that the toner concentration becomes 8.0% by mass. -1 The mixture was mixed for a rotation time of 5 minutes to obtain two-component developers 1 to 24.

[0158] <Evaluation> Using the above two-component developer 1, the following low-temperature fixing property evaluation, heat-resistant storage property evaluation, and charge retention evaluation were carried out. The evaluation was performed based on the following evaluation methods, and the results are shown in Table 4.

[0159] [Evaluation 1. Low-temperature fixability evaluation] A full-color copier, imagePress C800, manufactured by Canon Inc., was modified so that the fixing temperature and process speed could be freely set, and a test was carried out in the fixing temperature range for the two-component developer 1. The image was printed in monochrome mode under normal temperature and humidity conditions (temperature 23°C, relative humidity 50% to 60%) with a toner loading of 1.2 mg / cm on paper. 2 The print ratio was adjusted to 25%, and the print was output without fixing. The evaluation paper was copy paper GF-C081 (A4, basis weight 81.4 g / m 2 , sold by Canon Marketing Japan Inc.) was used. Thereafter, in a low temperature and low humidity environment (temperature 15°C, relative humidity 10% or less), the process speed was set to 450 mm / sec, and the fixing temperature was increased in increments of 2.5°C from 120°C, until the lowest temperature at which offset did not occur was determined as the fixing temperature. (Evaluation criteria for fixable temperature) A: Less than 150℃ (Excellent) B: 150℃ or higher, less than 155℃ (good). C: 155°C or higher and lower than 160°C (this is the level at which the effects of the present invention are obtained). D: 160°C or higher (not acceptable in this invention) The evaluation results are shown in Table 5.

[0160] [Evaluation 2. Heat resistance storage evaluation] 5g of toner was placed in a 100cc resin cup and left in a temperature and humidity variable thermostatic chamber (55℃ 50%) for 10 hours, after which the cohesion of the toner was evaluated. The cohesion was evaluated by the remaining rate of toner when the toner was sieved with a 150μm mesh for 10 seconds at an amplitude of 0.5mm using a powder tester PT-X manufactured by Hosokawa Micron Corporation. A grade of C or higher was judged to be good. (Evaluation Criteria) A: Residual rate less than 2.0% B: Residual rate 2.0% or more and less than 5.0% C: Residual rate 5.0% or more and less than 10.0% D: Survival rate 10.0% or more

[0161] [Evaluation 3: Charge retention evaluation] Using a Canon full-color copier imageRUNNER ADVANCE C9075PRO, images were output in a high temperature and high humidity environment (30°C / 80%Rh) and at room temperature and humidity (23°C / 50%Rh). The output image was a cyan 4A horizontal, 10 cm wide vertical stripe image in monochrome mode, and the reflection density of cyan on the paper was adjusted to 1.35. The evaluation paper was copy paper GF-C081 (A4, basis weight 81.4 g / m 2A developing device (sold by Canon Marketing Japan Inc.) was used. The developing device was then removed and left for 150 hours, the main body was started up, the developing device was returned to the main body, and the same image was output again under the same developing conditions. The reflection density of the output image obtained was measured as an average value at nine points using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite), and compared with the reflection density before and after leaving it, and evaluated according to the following criteria. (Evaluation criteria: difference in reflection density of output image before and after leaving it) A: Less than Δ0.06 (very good) B: Δ0.06 or more and less than Δ0.12 (good). C: Δ0.12 or more and less than Δ0.18 (this is the level at which the effect of the present invention is obtained) D: Δ0.18 or more (not acceptable in the present invention)

[0162] <Examples 2 to 16 and Comparative Examples 1 to 8> Evaluation was performed in the same manner as in Example 1, except that the two-component developer used for evaluation was changed to the two-component developer shown in Table 4. The evaluation results are shown in Table 4.

[0163] [Table 4]

Claims

1. A toner having toner particles with a core-shell structure in which the surface of a toner core is covered with only one shell layer, The toner core contains a crystalline resin A and an amorphous resin B, The crystalline resin A has a carboxy group, The shell layer contains a thermosetting resin C having an oxazoline group, The thermosetting resin C is a copolymer of 2-vinyl-2-oxazoline and methyl acrylate or methyl methacrylate, the shell layer contains a resin component including a unit having an oxazoline group and a unit having an amide bond, the amide bond is formed by a reaction between the oxazoline group of the thermosetting resin C and the carboxy group of the crystalline resin A contained in the toner core, the acid value of the crystalline resin A (excluding the component bonded to the thermosetting resin C via the amide bond) is 10.0 mgKOH / g or more and 50.0 mgKOH / g or less; The hydroxyl value of the crystalline resin A is 20.0 mgKOH / g or less, The toner, wherein the shell layer has a thickness of 3 nm or more and 200 nm or less.

2. The acid value of the amorphous resin B is 20.0 mgKOH / g or less, 2. The toner according to claim 1, wherein the amorphous resin B has a hydroxyl value of 40.0 mgKOH / g or less.

3. 3. The toner according to claim 1, wherein the resin component has a structural unit derived from an oxazoline group formed by the crosslinking reaction with the carboxy group.

4. 4. The toner according to claim 1, wherein the crystalline resin A and the amorphous resin B are polyester resins.

5. 5. The toner according to claim 1, wherein the acid value of the crystalline resin A is from 25.0 mgKOH / g to 40.0 mgKOH / g.

6. 6. The toner according to claim 1, wherein the shell layer has a thickness of 3 nm or more and 20 nm or less.

7. 7. The toner according to claim 1, wherein a weight average molecular weight Mw of a resin component formed by a crosslinking reaction between the crystalline resin A and the thermosetting resin C is 34,000 or more and 200,000 or less.

Citation Information

Patent Citations

  • Method of manufacturing toner

    JP2011123352A

  • Toner and method for manufacturing the same

    JP2013109330A

  • Toner

    JP2018101069A

  • Core-shell type toner for electrostatic charge image development

    JP2018180188A