toner

A toner with specific ester wax and fatty acid metal salt formulation physically crosslinks to prevent coalescence, addressing the challenge of low-temperature fixability and gloss reduction, enhancing adhesion and scratch resistance.

JP7587384B2Active Publication Date: 2024-11-20CANON KK
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020162551
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-28
Publication Date
2024-11-20
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving both low-temperature fixability and suppressing image gloss reduction, as large amounts of plasticizers used for improved fixability tend to coalesce and crystallize, forming large crystals that roughen the image surface and reduce gloss.

Method used

A toner formulation containing specific amounts of ester wax and a fatty acid metal salt, represented by the structural formula (RCOO)pM(OH)q, with a THF-insoluble content of 30.0% by mass or more, which physically crosslinks with the ester wax to reduce its mobility and prevent coalescence during heating, maintaining low-temperature fixability while minimizing gloss loss.

Benefits of technology

The toner achieves both low-temperature fixability and effective suppression of image gloss reduction, ensuring improved adhesion and scratch resistance of the fixed image.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587384000001
    Figure 0007587384000001
  • Figure 0007587384000002
    Figure 0007587384000002
  • Figure 0007587384000003
    Figure 0007587384000003
Patent Text Reader

Abstract

To provide a toner that achieves both low temperature fixability and a reduction in glossiness of an image.SOLUTION: A toner has a toner particle containing a binder resin, ester wax, and a fatty acid metal salt. The toner particle contains the ester wax in an amount of 15.0% by mass or more and 40.0% by mass or less. The tetrahydrofuran (THF) insoluble in the toner particle when Soxhlet extraction of the toner particle is performed by using THF is 30.0% by mass or more, and the THF insoluble contains a resin having an ester group. The fatty acid metal salt is represented by a structural formula of the following formula (1). In the following formula (1), R is an aliphatic alkyl group, M is metal, q is an integer of 1 or more, and p is a value obtained by subtracting q from the valence of M. (1) (RCOO)pM(OH)q.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner used in an image forming method such as an electrophotographic method. [Background technology]

[0002] In recent years, from the viewpoint of energy conservation, there has been an increasing demand for printers and copiers to carry out the process of fixing toner onto a recording medium by applying heat and pressure at lower temperatures. In the fixing process, it is preferable that the binder resin is sufficiently plasticized when the toner is subjected to heat, and that the adhesiveness to the recording medium is enhanced. Therefore, toners to which a plasticizer is added have been proposed in order to promote the thermoplasticization of the binder resin even at lower temperatures and ensure sufficient fixing properties.

[0003] As the toner plasticizer, a compound that is easily soluble in the binder resin is preferable. A characteristic of a compound that is easily soluble in the binder resin is, for example, that it has a chemical structure that strengthens the intermolecular force with the binder resin. Patent Document 1 discloses a toner that has improved low-temperature fixability by adding an ester wax as a toner plasticizer.

[0004] However, when a large amount of such a plasticizer is used to further improve low-temperature fixability, the plasticizer is likely to coalesce in the binder resin when the toner is heated in the fixing process. In such a case, when the image cools and the plasticizer crystallizes, large crystals are formed in the image, causing the image surface to become rough, resulting in a decrease in image gloss. Thus, achieving both low-temperature fixability and suppressing a decrease in image gloss is an issue. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6020458 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention can achieve both low-temperature fixability and suppression of a decrease in image gloss. [Means for solving the problem]

[0007] The present invention provides a toner having toner particles containing a binder resin, an ester wax, and a fatty acid metal salt, The toner particles contain an ester wax in an amount of 15.0% by mass or more and 40.0% by mass or less, the toner particles have a THF-insoluble content of 30.0% by mass or more when the toner particles are subjected to Soxhlet extraction using tetrahydrofuran (THF), and the THF-insoluble content contains a resin having an ester group; The toner is characterized in that the fatty acid metal salt is a fatty acid metal salt represented by the following structural formula (1). (RCOO)pM(OH)q (1) In formula (1), R is an aliphatic alkyl group, M is a metal, q is an integer of 1 or more, and p is the value obtained by subtracting q from the valence of M. Effect of the Invention

[0008] According to the present invention, it is possible to provide a toner which achieves both low-temperature fixability and suppression of deterioration in image gloss. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment. As a result of extensive research, the inventors have found that the above problem can be solved by using toner particles that contain an ester wax in a specific range and a fatty acid metal salt having a specific structure, and have a THF-insoluble content of 30.0% by mass or more.

[0010] That is, the present invention provides a toner having toner particles containing a binder resin, an ester wax, and a fatty acid metal salt, The toner particles contain an ester wax in an amount of 15.0% by mass or more and 40.0% by mass or less, the toner particles have a THF-insoluble content of 30.0% by mass or more when the toner particles are subjected to Soxhlet extraction using tetrahydrofuran (THF), and the THF-insoluble content contains a resin having an ester group; The fatty acid metal salt is characterized in that it is a fatty acid metal salt represented by the following structural formula (1). (RCOO)pM(OH)q (1) In formula (1), R is an aliphatic alkyl group, M is a metal, q is an integer of 1 or more, and p is the value obtained by subtracting q from the valence of M.

[0011] Hereinafter, each of the characteristics of the toner of the present invention will be described in detail. The present invention is characterized by containing a specific range of amount of ester wax and a fatty acid metal salt having a specific structure. In particular, by adding the fatty acid metal salt having a specific structure internally to the toner particles, it is possible to achieve both remarkable low-temperature fixing property and suppression of deterioration in image gloss compared to the case where it is added externally. In order to improve low-temperature fixability, when a large amount of ester wax is added to the toner particles, the ester wax is likely to coalesce in the binder resin when the toner is heated in the fixing process. At that time, by adding a fatty acid metal salt having the structure represented by the above formula (1) to the toner particles, the fatty acid metal salt forms a physical bridge between the ester wax and the THF-insoluble matter containing an ester group. The THF-insoluble matter contained in the toner particles has a very large molecular weight and low molecular mobility, so it reduces the mobility of the ester wax bound by the physical bridge. As a result, the coalescence of the ester wax in the binder resin when the toner is heated in the fixing process is suppressed, and it is possible to suppress the decrease in image gloss while maintaining low-temperature fixability.

[0012] The content of the ester wax in the present invention must be 15.0% by mass or more and 40.0% by mass or less. When the content of the ester wax is within this range, the thermoplasticization of the toner proceeds sufficiently even during low-temperature fixing, so that the abrasion resistance (low-temperature fixing ability) of the fixed image can be improved.

[0013] The toner particles in the present invention must have a THF-insoluble content of 30.0% by mass or more, and the THF-insoluble content must contain a resin having an ester group. The THF-insoluble content has a very large molecular weight and low molecular mobility. Therefore, if the THF-insoluble content is 30% by mass or more, the mobility of the ester wax bonded to the THF-insoluble content by physical crosslinking is sufficiently reduced. As a result, the coalescence of the ester wax in the binder resin when the toner is subjected to heat in the fixing process is suppressed, thereby suppressing the decrease in image gloss.

[0014] The toner of the present invention must contain a fatty acid metal salt represented by the structural formula (1) above, and it is particularly preferable that the fatty acid metal salt is internally contained in the toner particles. In the above formula (1), R is an aliphatic alkyl group, M is a metal, q is an integer of 1 or more, and p is a value obtained by subtracting q from the valence of M. When q is an integer of 1 or more, positive charges tend to accumulate on the hydrogen of the hydroxyl group adjacent to the central metal. This bias in charge makes it possible to electrostatically form physical crosslinks with the ester groups contained in the wax and the THF-insoluble matter.

[0015] The alcohol component of the ester wax is preferably a diol having 2 to 6 carbon atoms, and more preferably ethylene glycol having 2 carbon atoms, since this has a higher compatibility with the binder resin and can further improve the scratch resistance of the image.

[0016] Examples of diols having 2 to 6 carbon atoms include ethylene glycol, 1,3-propanediol, 1,2-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, and 1,6-hexanediol. Among these, the use of ethylene glycol is preferred because the resulting ester wax has excellent compatibility with the styrene-acrylic copolymer portion of the binder resin, and as a result, the scratch resistance of the fixed image can be improved.

[0017] The acid component of the ester wax is preferably an aliphatic monocarboxylic acid having a carbon number of 14 to 22. When the acid component of the ester wax has such a structure, the compatibility with the binder resin is further improved.

[0018] Examples of the aliphatic monocarboxylic acid having 14 to 22 carbon atoms include stearic acid, arachidic acid, behenic acid, oleic acid, vaccenic acid, linoleic acid, and linolenic acid. Among these, stearic acid is preferred from the viewpoint of improving the abrasion resistance of the fixed image.

[0019] The ester wax may be a single compound or two or more compounds.

[0020] In the present invention, in addition to the ester wax, other waxes may be added. The other waxes may be a release agent that improves the separation between the molten toner and the fixing member in the fixing process. A plasticizer may also be added, and waxes may be added for other purposes such as improving the gloss of the image, and waxes having multiple functions may also be added.

[0021] Such wax is not particularly limited, and known waxes can be used. For example, ester waxes other than the above-mentioned ester compounds, aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof, and waxes obtained by grafting aliphatic hydrocarbon waxes with vinyl monomers such as styrene and acrylic acid can be mentioned.

[0022] The fatty acid metal salt used in the present invention may be any of the conventionally known fatty acid metal salts. R in the above formula (1) is preferably an aliphatic alkyl group having a carbon number of 14 to 22. When R has such a structure, the physical crosslinking with the aliphatic alkyl group contained in the ester wax can be further strengthened. Examples of aliphatic monocarboxylic acids in which R is an aliphatic alkyl group having 14 to 22 carbon atoms include stearic acid, arachidic acid, behenic acid, oleic acid, vaccenic acid, linoleic acid, and linolenic acid.

[0023] In the above formula (1), M is preferably any one of the metals Al, Mg, and Zn. These central metals have a high valence and a small ionic radius, and therefore have high electrostatic stability and can further strengthen physical crosslinking with the ester group.

[0024] The toner particles preferably contain the fatty acid metal salt in an amount of 0.1% by mass or more and 0.5% by mass or less. When the content of the fatty acid metal salt is within this range, the fatty acid metal salt binds the ester wax and the THF insoluble matter more strongly, thereby reducing the mobility of the ester wax. As a result, when the toner is subjected to heat in the fixing process, the coalescence of the ester wax in the binder resin is suppressed, thereby suppressing the decrease in image gloss.

[0025] The binder resin in the present invention preferably contains a styrene-acrylic resin. Examples of the styrene-acrylic resin include resins having a styrene-acrylic copolymer moiety produced from a styrene monomer and an acrylic monomer (acrylic acid or methacrylic acid and its alkyl ester). As long as it has a styrene-acrylic copolymer moiety, it may be composed of only a styrene-acrylic copolymer, or may be a block copolymer or graft copolymer of a styrene-acrylic copolymer and another polymer, or a mixture thereof.

[0026] The styrene acrylic resin and the ester wax are highly compatible with each other, and the thermoplasticization of the binder resin is easily promoted. Therefore, the toner is easily wetted and spread even during low-temperature fixing, and the adhesion of the image to the recording medium is increased. Therefore, the abrasion resistance (low-temperature fixing ability) of the image can be improved.

[0027] Furthermore, since the ester wax has high compatibility with styrene-acrylic copolymers, it is unlikely to seep out to the interface between the image and the recording medium during the fixing process. Generally, if the ester wax seeps out to the interface, it reduces the adhesion between the image and the recording medium, and therefore reduces the scratch resistance of the image.

[0028] Specific methods for producing the toner of the present invention will be described below, but the methods are not limited thereto. The preferred methods for producing toner particles are suspension polymerization, solution suspension, and emulsion aggregation, with suspension polymerization being the most preferred. In suspension polymerization, the organosilicon polymer is easily precipitated uniformly on the surface of the toner particles, and this effectively reduces the contact area between the projections on the fixed image and the paper discharge member.

[0029] The suspension polymerization method will be further described below. The suspension polymerization method is a method in which a polymerizable monomer and a colorant (and, if necessary, a polymerization initiator, a crosslinking agent, a charge control agent, and other additives) are uniformly dissolved or dispersed to prepare a polymerizable monomer composition, and then this polymerizable monomer composition is dispersed in a continuous layer (e.g., an aqueous phase) containing a dispersion stabilizer using an appropriate stirrer while simultaneously carrying out a polymerization reaction, thereby obtaining a toner having a desired particle size.

[0030] The polymerizable monomer composition may contain a release agent and other resins as necessary. After the polymerization step is completed, the generated particles are washed, collected by filtration, and dried to obtain toner particles. The temperature may be raised in the latter half of the polymerization step. In addition, in order to remove unreacted polymerizable monomers or by-products, it is also possible to distill off a part of the dispersion medium from the reaction system in the latter half of the polymerization step or after the polymerization step is completed.

[0031] The above-mentioned release agents include the following: petroleum waxes such as paraffin wax, microcrystalline wax, and petrolatum and their derivatives, montan wax and its derivatives, hydrocarbon waxes and their derivatives by the Fischer-Tropsch method, polyolefin waxes such as polyethylene and polypropylene and their derivatives, natural waxes and their derivatives such as carnauba wax and candelilla wax, higher aliphatic alcohols, fatty acids such as stearic acid and palmitic acid, or compounds thereof, acid amide waxes, ester waxes, ketones, hardened castor oil and its derivatives, vegetable waxes, animal waxes, and silicone resins. The derivatives include oxides, block copolymers with vinyl monomers, and graft modified products. The release agents can be used alone or in combination.

[0032] As the other resins, the following resins can be used as long as they do not affect the effects of the present invention. Homopolymers of styrene and its substitutes such as polystyrene and polyvinyltoluene; styrene-based copolymers such as styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-dimethylaminoethyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-dimethylaminoethyl methacrylate copolymer, styrene-vinyl methyl ether copolymer, styrene-vinyl ethyl ether copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-maleic acid copolymer, and styrene-maleic acid ester copolymer; polymethyl methacrylate, polybutyl methacrylate, polyvinyl acetate, polyethylene, polypropylene, polyvinyl butyral, silicone resin, polyester resin, polyamide resin, epoxy resin, polyacrylic resin, rosin, modified rosin, terpene resin, phenolic resin, aliphatic or alicyclic hydrocarbon resin, and aromatic petroleum resin. These resins may be used alone or in combination.

[0033] Suitable examples of the polymerizable monomer in the suspension polymerization method include the vinyl polymerizable monomers shown below. Styrene; styrene derivatives such as α-methylstyrene, β-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, pn-butylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octyl, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, p-methoxystyrene, and p-phenylstyrene; methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-amyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, n-nonyl acrylate, cyclohexyl acrylate, benzyl acrylate, dimethyl phosphate ethyl acrylate, diethyl phosphate ethyl acrylate, and dibutyl phosphate ethyl acrylate. methacrylic polymerizable monomers such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-amyl methacrylate, n-hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, diethyl phosphate ethyl methacrylate, and dibutyl phosphate ethyl methacrylate; methylene aliphatic monocarboxylic acid esters; vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate, vinyl butyrate, vinyl benzoate, and vinyl formate; vinyl ethers such as vinyl methyl ether, vinyl ethyl ether, and vinyl isobutyl ether; vinyl methyl ketone, vinyl hexyl ketone, and vinyl isopropyl ketone.

[0034] Among these vinyl polymers, styrene polymers, styrene-acrylic copolymers, and styrene-methacrylic copolymers are preferred.

[0035] A polymerization initiator may be added when polymerizing the polymerizable monomer. Examples of the polymerization initiator include the following: azo-based or diazo-based polymerization initiators such as 2,2'-azobis-(2,4-divaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile; and peroxide-based polymerization initiators such as benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyloxycarbonate, cumene hydroperoxide, 2,4-dichlorobenzoyl peroxide, and lauroyl peroxide. These polymerization initiators are preferably added in an amount of 0.5 to 30.0% by mass relative to the polymerizable monomer, and may be used alone or in combination.

[0036] In order to control the molecular weight of the binder resin constituting the toner particles, a chain transfer agent may be added during polymerization of the polymerizable monomer. The amount of the chain transfer agent added is preferably 0.001 to 15,000% by mass of the polymerizable monomer.

[0037] On the other hand, in order to control the molecular weight of the binder resin constituting the toner particles, a crosslinking agent may be added during polymerization of the polymerizable monomer. Examples of the crosslinkable monomer include the following: divinylbenzene, bis(4-acryloxypolyethoxyphenyl)propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol #200, #400, and #600 diacrylates, dipropylene glycol diacrylate, polypropylene glycol diacrylate, polyester type diacrylate (MANDA Nippon Kayaku), and those in which the above acrylates are replaced with methacrylates.

[0038] Examples of polyfunctional crosslinkable monomers include pentaerythritol triacrylate, trimethylolethane triacrylate, trimethylolpropane triacrylate, tetramethylolmethane tetraacrylate, oligoester acrylate and its methacrylate, 2,2-bis(4-methacryloxy-polyethoxyphenyl)propane, diacryl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, and diaryl chlorendate. The preferred amount of addition is 0.001 to 15,000% by mass based on the polymerizable monomer.

[0039] When the medium used in the suspension polymerization is an aqueous medium, the following can be used as a dispersion stabilizer for the particles of the polymerizable monomer composition: tricalcium phosphate, magnesium phosphate, zinc phosphate, aluminum phosphate, calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, bentonite, silica, and alumina. Examples of organic dispersants include polyvinyl alcohol, gelatin, methyl cellulose, methylhydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, and starch.

[0040] Commercially available nonionic, anionic, or cationic surfactants may also be used. Examples of such surfactants include sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, and potassium stearate.

[0041] The colorant used in the toner of the present invention is not particularly limited, and any known colorant can be used. The content of the colorant is preferably 3.0 to 15.0 parts by mass with respect to 100 parts by mass of the binder resin or polymerizable monomer.

[0042] In the toner of the present invention, a charge control agent can be used during the production of the toner, and a known charge control agent can be used. The amount of the charge control agent added is preferably 0.01 to 10.00 parts by mass per 100 parts by mass of the binder resin or polymerizable monomer.

[0043] The toner of the present invention may, if necessary, contain various organic or inorganic fine powders as external additives added to the toner particles. From the viewpoint of durability when added to the toner particles, the organic or inorganic fine powders preferably have a particle size of 1 / 10 or less of the weight average particle size of the toner particles.

[0044] As the organic or inorganic fine powder, for example, the following can be used. (1) Fluidity imparting agents: silica, alumina, titanium oxide, carbon black and carbon fluoride. (2) Abrasives: metal oxides (e.g., strontium titanate, cerium oxide, alumina, magnesium oxide, chromium oxide), nitrides (e.g., silicon nitride), carbides (e.g., silicon carbide), metal salts (e.g., calcium sulfate, barium sulfate, calcium carbonate). (3) Lubricants: Fluorine-based resin powder (e.g., vinylidene fluoride, polytetrafluoroethylene), fatty acid metal salts (e.g., zinc stearate, calcium stearate). (4) Charge control particles: metal oxides (e.g., tin oxide, titanium oxide, zinc oxide, silica, alumina), carbon black.

[0045] The organic or inorganic fine powder may be subjected to a hydrophobic treatment on the surface of the toner particles in order to improve the fluidity of the toner and to make the toner particles uniformly charged. Examples of the treatment agent for the hydrophobic treatment of the organic or inorganic fine powder include unmodified silicone varnish, various modified silicone varnishes, unmodified silicone oil, various modified silicone oils, silane compounds, silane coupling agents, other organic silicon compounds, and organic titanium compounds. These treatment agents may be used alone or in combination.

[0046] Various measurement methods related to the present invention will be described below. <Method for Measuring THF-Insoluble Content in Toner Particles> Precisely weigh 1 g of toner, charge it into a cylindrical filter paper, and perform Soxhlet extraction with 200 ml of tetrahydrofuran (THF) for 20 hours. Then, take out the cylindrical filter paper, dry it under vacuum at 40 °C for 20 hours, measure the residue mass, and when the mass of the resin component initially charged is W1 g and the mass of the resin component in the extraction residue is W2 g, calculate the tetrahydrofuran (THF) insoluble content of the toner resin component from the following formula. (W2 / W1)×100 (mass%)

[0047] <Method for Detecting Ester Groups Contained in THF-Insoluble Content> The detection of ester groups contained in the THF-insoluble content was performed by measuring the FT-IR spectrum. For the measurement of the FT-IR spectrum using the ATR method, use a Fourier transform infrared spectrometer (Frontier; manufactured by PerkinElmer) equipped with a Universal ATR Sampling Accessory. The software for measurement and analysis used was PerkinElmer Spectrum ver.10.4.3 (manufactured by PerkinElmer). Also, set the incident angle of the infrared light to 45°.

[0048] The specific conditions are shown below. Attach a Universal ATR top plate with a diamond ATR crystal (one-time reflection diamond / KRS5; the ATR crystal has a two-layer structure of diamond and KRS5, and the crystal in contact with the sample is diamond). Set the scan type to background, the vertical axis unit to energy, and perform background measurement. Set the scan type to sample and the vertical axis unit to A. Place it on the ATR crystal so that the bottom surface of the pellet of the THF-insoluble content comes into contact, and press it tightly with the pressure arm. Perform the measurement.

[0049] Select bidirectional baseline correction, and for the obtained FT-IR spectrum, at 3100 cm -1More than 3500cm -1 In the following range, two points without a peak were selected as base points, and the 2000 cm -1 More than 2700cm -1 Within the following range, select two points that do not have a peak as base points and perform baseline correction. The spectrum after baseline correction, 3022 cm -1 More than 3032cm -1 The spectrum is normalized so that the maximum peak intensity in the following range is 1.00. 1735cm -1 More than 1750cm -1 The presence or absence of ester groups contained in the THF-insoluble matter was determined based on the presence or absence of peaks in the following range. EXAMPLES

[0050] In the following examples and comparative examples, "parts" means "parts by mass". [Example 1: Production Example of Toner 1] (Preparation of aqueous medium) In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 650.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (Rasa Kogyo Co., Ltd., 12-hydrate) were added, and the mixture was kept at 65°C for 1.0 hour while purging with nitrogen. Using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), while stirring at 15,000 rpm, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, 10% by mass of hydrochloric acid was added to the aqueous medium to adjust the pH to 5.0, and an aqueous medium was obtained.

[0051] (Preparation process of polymerizable monomer composition 1) Styrene: 60.0 parts Carbon black: 6.5 parts Aluminum distearate: 0.2 parts The above materials were charged into an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed using zirconia particles having a diameter of 1.7 mm at 220 rpm for 5.0 hours to prepare a pigment dispersion. The following materials were added to the above pigment dispersion. Styrene: 20.0 parts n-Butyl acrylate: 20.0 parts Crosslinking agent (divinylbenzene): 0.9 parts Ethylene glycol stearate: 30.9 parts Saturated polyester resin: 5.0 parts (Polycondensation product of propylene oxide modified bisphenol A (2 mole adduct) and terephthalic acid (molar ratio 10:12), glass transition temperature Tg = 68°C, weight average molecular weight Mw = 10,000, molecular weight distribution Mw / Mn = 5.12) The mixture was kept at 65° C. and uniformly dissolved and dispersed using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) at 500 rpm to prepare a polymerizable monomer composition 1.

[0052] (granulation process) While maintaining the temperature of the aqueous medium at 70° C. and the rotation speed of the TK homomixer at 15,000 rpm, the polymerizable monomer composition 1 was added to the aqueous medium, and 10.0 parts of t-butyl peroxypivalate, a polymerization initiator, was added. Granulation was continued for 10 minutes while maintaining the stirring speed at 15,000 rpm.

[0053] (Polymerization and distillation process) After the granulation step, the agitator was replaced with a propeller agitator and the mixture was stirred at 150 rpm while maintaining the temperature at 70° C. for 5.0 hours, and then the temperature was raised to 85° C. and heated for 2.0 hours to carry out the polymerization reaction. Thereafter, the reflux tube of the reaction vessel was replaced with a cooling tube, and the slurry was heated to 100° C. to perform distillation for 6 hours to distill off the unreacted polymerizable monomer, thereby obtaining a toner particle dispersion liquid.

[0054] (Washing and drying process) After the polymerization process was completed, the toner particle dispersion was cooled, and hydrochloric acid was added to the toner particle dispersion to adjust the pH to 1.5 or less, and the dispersion was left to stand with stirring for 1 hour, after which the dispersion was subjected to solid-liquid separation using a pressure filter to obtain a toner cake. This was reslurried in ion-exchanged water to make a dispersion again, and then the dispersion was subjected to solid-liquid separation using the aforementioned filter to obtain a toner cake. The obtained toner cake was dried and classified in a thermostatic chamber at 40° C. for 72 hours to obtain toner particles 1. The amount of the ester wax and the amount of the THF insoluble matter in the toner particles are shown in Table 4. 1.0 part of silica fine particles having a primary particle number average particle size of 40 nm was added to 100.0 parts of the obtained toner particles, and mixed using an FM mixer (manufactured by Nippon Coke & Co., Ltd.) to obtain Toner 1. The results of each evaluation of the obtained toner are shown in Table 5.

[0055] [Examples 2 to 14, 16, and 17: Production Examples of Toner 2 to Toner 14, Toner 16, and Toner 17] Toners 2 to 14, 16 and 17 were obtained in the same manner as Toner 1, except that the type and number of parts of the ester wax, the type and number of parts of the fatty acid metal salt, and the number of parts of the crosslinking agent were changed to the conditions shown in Table 1. The types of ester wax and fatty acid metal salt are shown in Tables 2 and 3. The amount of ester wax and the amount of THF insoluble matter in the toner particles are shown in Table 4, and the results of each evaluation of the obtained toners are shown in Table 5.

[0056] [Table 1]

[0057] [Table 2]

[0058] [Table 3]

[0059] [Table 4]

[0060] [Example 15: Production Example of Toner 15] Toner 15 was obtained in the same manner as Toner 1, except that polymerizable monomer composition 1 was changed to polymerizable monomer composition 2 prepared as shown below. The amount of ester wax and the amount of THF insoluble matter in the toner particles are shown in Table 4, and the results of each evaluation of the obtained toner are shown in Table 5.

[0061] (Preparation step of polymerizable monomer composition 2) Styrene: 60.0 parts Carbon black: 6.5 parts Aluminum distearate: 0.2 parts The above materials were charged into an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed using zirconia particles having a diameter of 1.7 mm at 220 rpm for 5.0 hours to prepare a pigment dispersion. The following materials were added to the above pigment dispersion. Styrene: 40.0 parts Crosslinking agent (divinylbenzene): 0.9 parts Ethylene glycol stearate: 30.8 parts Saturated polyester resin: 5.0 parts (Polycondensation product of propylene oxide modified bisphenol A (2 mole adduct) and terephthalic acid (molar ratio 10:12), glass transition temperature Tg = 68°C, weight average molecular weight Mw = 10,000, molecular weight distribution Mw / Mn = 5.12) The mixture was kept at 65° C. and was uniformly dissolved and dispersed at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a polymerizable monomer composition 2.

[0062] [Comparative Examples 1 to 4: Production Examples of Comparative Toners 1 to 4] Comparative toner particles 1 to 4 were obtained in the same manner as toner particles 1, except that the type and number of parts of the ester wax, the type and number of parts of the fatty acid metal salt, and the number of parts of the crosslinking agent were changed to the conditions shown in Table 1. The types of ester wax and fatty acid metal salt are shown in Tables 2 and 3. The amounts of ester wax and THF-insoluble matter in the comparative toner particles are shown in Table 4, and the results of each evaluation of the obtained toner are shown in Table 5.

[0063] [Comparative Example 5: Production Example of Comparative Toner 5] (Synthesis of cross-linked styrene resin) Styrene: 40.0 parts Crosslinking agent (divinylbenzene): 0.9 parts The above materials were charged into a reaction vessel equipped with a stirrer, a thermometer, and a reflux tube, and 1.5 parts of t-butyl peroxypivalate as a polymerization initiator was added. The polymerization reaction was carried out for 5.0 hours while maintaining the temperature at 70°C and stirring at 150 rpm using a propeller stirring blade, and then heated to 85°C for 2.0 hours. The obtained polymer was dried in a thermostatic chamber at 40°C for 72 hours to obtain a crosslinked styrene resin.

[0064] (Preparation of aqueous medium) In a reaction vessel equipped with a stirrer, a thermometer, and a reflux condenser, 650.0 parts of ion-exchanged water and 14.0 parts of sodium phosphate (Rasa Kogyo Co., Ltd., 12-hydrate) were added, and the mixture was kept at 65°C for 1.0 hour while purging with nitrogen. Using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), while stirring at 15,000 rpm, an aqueous calcium chloride solution in which 9.2 parts of calcium chloride (dihydrate) was dissolved in 10.0 parts of ion-exchanged water was added all at once to prepare an aqueous medium containing a dispersion stabilizer. Furthermore, 10% by mass of hydrochloric acid was added to the aqueous medium to adjust the pH to 5.0, and an aqueous medium was obtained.

[0065] (Preparation step of polymerizable monomer composition 3) Styrene: 30.0 parts Carbon black: 6.5 parts Aluminum distearate: 0.2 parts The above materials and cross-linked styrene resin were charged into an attritor (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and further dispersed at 220 rpm for 5.0 hours using zirconia particles having a diameter of 1.7 mm to prepare a pigment dispersion. The following materials were added to the above pigment dispersion. Styrene: 15.0 parts n-Butyl acrylate: 15.0 parts Ethylene glycol stearate: 30.9 parts Saturated polyester resin: 5.0 parts (Polycondensation product of propylene oxide modified bisphenol A (2 mole adduct) and terephthalic acid (molar ratio 10:12), glass transition temperature Tg = 68°C, weight average molecular weight Mw = 10,000, molecular weight distribution Mw / Mn = 5.12) The mixture was kept at 65° C. and was uniformly dissolved and dispersed at 500 rpm using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to prepare a polymerizable monomer composition 3.

[0066] (granulation process) While maintaining the temperature of the aqueous medium at 70° C. and the rotation speed of the TK homomixer at 15,000 rpm, the polymerizable monomer composition 3 was added to the aqueous medium, and 8.5 parts of t-butyl peroxypivalate as a polymerization initiator was added. Granulation was continued for 10 minutes while maintaining the stirring speed at 15,000 rpm.

[0067] (Polymerization and distillation process) After the granulation step, the agitator was replaced with a propeller agitator and the mixture was stirred at 150 rpm while maintaining the temperature at 70° C. for 5.0 hours, and then the temperature was raised to 85° C. and heated for 2.0 hours to carry out the polymerization reaction. Thereafter, the reflux tube of the reaction vessel was replaced with a cooling tube, and the slurry was heated to 100° C. to perform distillation for 6 hours to distill off the unreacted polymerizable monomer, thereby obtaining a toner particle dispersion liquid.

[0068] (Washing and drying process) After the polymerization process was completed, the toner particle dispersion was cooled, and hydrochloric acid was added to the toner particle dispersion to adjust the pH to 1.5 or less, and the dispersion was left to stand with stirring for 1 hour, after which the dispersion was subjected to solid-liquid separation using a pressure filter to obtain a toner cake. This was reslurried in ion-exchanged water to make a dispersion again, and then the dispersion was subjected to solid-liquid separation using the aforementioned filter to obtain a toner cake. The obtained toner cake was dried and classified in a thermostatic chamber at 40° C. for 72 hours to obtain comparative toner particles 5. The amount of ester wax and the amount of THF insoluble matter in the toner particles are shown in Table 4, and the results of each evaluation of the obtained toner are shown in Table 5.

[0069] [Evaluation items] <Low temperature fixability> The fixing unit of the Canon laser beam printer LBP9600C was modified so that the fixing temperature could be adjusted. Using this modified LBP9600C, images were printed at a process speed of 300 mm / sec under normal temperature and humidity (25°C / 50% RH) while changing the fixing temperature from 140°C in 5°C increments. 2 The fixed image was rubbed 10 times with Silbon paper with a weight of 1000 g, and the temperature at which the density reduction rate of the fixed image after rubbing exceeded 10% was determined as the minimum fixing temperature. The temperature 5°C above the minimum fixing temperature was determined as the low fixing temperature. The toner load for evaluation was 0.40 mg / cm 2 A solid image was formed on the image receiving paper, and the image was fixed on the image receiving paper by heating and pressing it without oil. The image receiving paper was GF-600 (weight 60 g / m 2 (sold by Canon Marketing Japan Inc.) was used.

[0070] (Evaluation Criteria) The low-temperature fixability was judged according to the following criteria. Rank A: Low-temperature fixing temperature is 145°C or less Rank B: Low-temperature fixing temperature is higher than 145℃ and lower than 150℃ Rank C: Low-temperature fixing temperature is higher than 150℃ and lower than 155℃ Rank D: Low-temperature fixing temperature is higher than 155°C and lower than 160°C

[0071] <Toner durability> A laser printer (HP Color LaserJet 3525dn, manufactured by HP) was prepared, and 300 g of toner was filled into the toner cartridge. The toner cartridge was then left in a room temperature and humidity (25°C / 50% RH) environment for 24 hours, and 30,000 sheets of a horizontal line image with a printing rate of 1% were printed out in the same environment. After that, the image was printed on a receiving paper (XEROX 4200 paper, manufactured by XEROX, letter size, 75 g / m 2 ) to halftone (toner load: 0.6mg / cm 2 ) was printed out and durability was evaluated based on the occurrence of development streaks.

[0072] (Evaluation Criteria) The durability was judged according to the following criteria. Rank A: No development streaks Rank B: Development streaks occur in 1 to 3 places Rank C: 4 to 6 development streaks Rank D: Seven or more development streaks or streaks 0.5 mm or wider

[0073] <Loss in image gloss> Fixing temperature 180℃, solid image (toner load: 0.6mg / cm 2 ) was printed out, and the gloss value was measured using a PG-3D (manufactured by Nippon Denshoku Kogyo Co., Ltd.). Furthermore, the printed solid image was left in a high temperature and high humidity (40°C / 95% RH) environment for 72 hours, after which the gloss value was measured and the decrease in gloss value was calculated. The transfer material was LETTER size plain paper (XEROX 4200 paper, manufactured by XEROX, 75 g / m 2 ) was used.

[0074] (Evaluation Criteria) The presence or absence of an effect of suppressing the decrease in image gloss was evaluated according to the following criteria. Rank A: Decrease in gloss value is less than 10 Rank B: Decrease in gloss value is 10 or more but less than 15 Rank C: Decrease in gloss value is 15 or more but less than 20 Rank D: Gross value drop of 20 or more

[0075] The evaluation results are shown in Table 5. From the results in Table 5, Comparative Example 1 had a low-temperature fixing temperature of 160° C. and was judged as rank D, and Comparative Examples 2 to 5 had gloss value losses of 22 to 25 and were judged as rank D. Examples 1 to 17 had low-temperature fixing temperatures of 140° C. to 155° C. and gloss value losses of 4 to 18, and none were judged as rank D.

[0076] [Table 5]

Claims

1. A toner having toner particles containing a binder resin, an ester wax, and a fatty acid metal salt, The toner particles contain an ester wax in an amount of 15.0% by mass or more and 40.0% by mass or less, the toner particles have a THF-insoluble content of 30.0% by mass or more when the toner particles are subjected to Soxhlet extraction using tetrahydrofuran (THF), and the THF-insoluble content contains a resin having an ester group; The toner is characterized in that the fatty acid metal salt is a fatty acid metal salt represented by the following structural formula (1): (RCOO)pM(OH)q (1) (In formula (1), R is an aliphatic alkyl group, M is a metal, q is an integer of 1 or more, and p is the value obtained by subtracting q from the valence of M.)

2. 2. The toner according to claim 1, wherein the ester wax is an ester compound of a diol having 2 to 6 carbon atoms and an aliphatic monocarboxylic acid having 14 to 22 carbon atoms.

3. 3. The toner of claim 2, wherein the diol is ethylene glycol.

4. 4. The toner according to claim 1, wherein M in the formula (1) is any one of metals Mg, Zn, and Al, and R is an aliphatic alkyl group having 14 to 22 carbon atoms.

5. 5. The toner according to claim 1, wherein the binder resin contains a styrene-acrylic resin.

6. The toner according to any one of claims 1 to 5, wherein the toner particles contain the fatty acid metal salt in an amount of 0.1% by mass or more and 0.5% by mass or less.

Citation Information

Patent Citations

  • A sum-3 dry cell can be substituted for a sum-1 or sum-2 dry cell

    JP1985020458A

  • Developer and image forming device using the developer

    JP1999282194A