Toner and its manufacturing method
A toner with a specific ester group concentration in crystalline polyester and controlled calcium carbonate ratio addresses hot offset resistance and scratch resistance issues, enhancing both low-temperature fixability and image durability.
Patent Information
- Application Number
- JP2020209734
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-17
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Existing toners with crystalline resins have issues with hot offset resistance and scratch resistance, despite improvements in low-temperature fixability, and the addition of inorganic fillers like calcium carbonate does not adequately address these problems.
A toner formulation with a specific ester group concentration in crystalline polyester and a controlled ratio of calcium carbonate particles, interacting through ester groups and calcium atoms, enhances both low-temperature fixability and hot offset resistance while improving scratch resistance.
The toner achieves both low-temperature fixability and improved hot offset resistance, along with enhanced scratch resistance of fixed images, by optimizing the interaction between crystalline polyester and calcium carbonate particles.
Smart Images

Figure 0007587410000008 
Figure 0007587410000001 
Figure 0007587410000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner used in an electrophotographic image forming method and a method for producing the toner. [Background technology]
[0002] In recent years, there has been an increasing demand for faster printing speeds, and toners with excellent low-temperature fixing properties have been developed to meet this demand. In order to realize toners with excellent low-temperature fixing properties, toners using crystalline resins with excellent sharp melting properties have been developed (for example, Patent Document 1). In addition, toners containing calcium carbonate particles have been developed to improve the deterioration of transferability caused by the use of crystalline resins (Patent Document 2).
[0003] The inventors' investigations revealed that a toner using a crystalline polyester as described in Patent Document 1 has a reduced viscosity at high temperatures, and therefore reduced hot offset resistance.
[0004] To address this problem, the viscosity of the toner can be improved by adding an inorganic filler such as calcium carbonate as described in Patent Document 2, thereby improving the hot offset resistance. However, the inventors have found that, depending on the type of crystalline polyester and inorganic filler, the effect on hot offset resistance is insufficient. Furthermore, the inventors have also found that the presence of an inorganic filler in the toner can reduce the abrasion resistance of the fixed image. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Application No. 2017-90489 [Patent Document 2] JP 2016-114828 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and provides a toner which achieves both low-temperature fixability and hot offset resistance and also provides excellent abrasion resistance of fixed images. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by causing a crystalline polyester having a specific structure and calcium carbonate to be present in a toner particle in a specific quantitative ratio.
[0008] The crystalline polyester has a high ester group concentration Ec. The presence of calcium carbonate particles in the toner particles causes an interaction between the ester group of the crystalline polyester and the calcium atoms of the calcium carbonate. This interaction produces a strong filler effect and improves the cohesive force within the toner particles, improving the hot offset resistance of the toner and the abrasion resistance of the fixed product. In addition, the crystalline polyester has a flexible carbon skeleton due to having a structure derived from an aliphatic diol and a structure derived from an aliphatic dicarboxylic acid as constituent units, so that it easily comes into contact with calcium carbonate particles and the ester group and calcium carbonate particles easily interact with each other.
[0009] It is believed that the interaction between the ester group of the crystalline polyester and the calcium atom of calcium carbonate is weak when the ester group concentration Ec of the crystalline polyester is too low, because the number of interaction points with the calcium atom is reduced. On the other hand, when the ester group concentration Ec of the crystalline polyester is too high, the chain length of the aliphatic group is inevitably shortened, and the molecular mobility of the crystalline polyester is reduced, so that the ester group is less likely to come into contact with the calcium atom, and the interaction is reduced. Therefore, it is believed that the effect of the present invention is manifested by the toner particles containing a crystalline polyester having a specific range of ester group concentration Ec and calcium carbonate, as specified in the present invention.
[0010] That is, the toner of the present invention is a toner having toner particles containing a binder resin, a crystalline polyester, and calcium carbonate particles, the crystalline polyester contains a unit derived from an aliphatic diol and a unit derived from an aliphatic dicarboxylic acid, the ester group concentration Ec of the crystalline polyester is 27% by mass or more and 50% by mass or less, the content Ma of the calcium carbonate particles contained in the toner particles is 3% by mass or more and 40% by mass or less, and the ratio (Ma / Mc) of the content Ma of the calcium carbonate particles contained in the toner particles to the content Mc of the crystalline polyester contained in the toner particles is 0.2 or more and 20 or less on a mass basis. Effect of the Invention
[0011] As described above, according to the present invention, it is possible to provide a toner which achieves both low-temperature fixability and hot offset resistance, and which provides a fixed image with excellent abrasion resistance. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram of an apparatus for heat-treating the surfaces of toner particles. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The expression "XX to YY" representing a numerical range means a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified.
[0014] The toner of the present invention contains toner particles, and the toner particles contain a binder resin, a crystalline polyester, and calcium carbonate. Each of the components will be described below.
[0015] <Binding resin> As the binder resin contained in the toner particles, a known polymer can be used. Specifically, for example, the following polymers can be used. Examples of the styrene copolymers include polystyrene, poly-p-chlorostyrene, polyvinyltoluene, and other homopolymers of styrene and its substitutes; styrene-p-chlorostyrene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-acrylic acid ester copolymers, styrene-methacrylic acid ester copolymers, styrene-α-methyl chloromethacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl ethyl ether copolymers, styrene-vinyl methyl ketone copolymers, and styrene-acrylonitrile-indene copolymers; polyvinyl chloride, phenolic resins, natural resin-modified phenolic resins, natural resin-modified maleic acid resins, acrylic resins, methacrylic resins, polyvinyl acetate, silicone resins, polyesters, polyurethanes, polyamides, furan resins, epoxy resins, xylene resins, polyvinyl butyral, terpene resins, coumarone-indene resins, and petroleum-based resins. These resins may be used alone or in combination of two or more. Among these, polyesters having high compatibility with the crystalline polyesters described below are preferred from the viewpoint of low-temperature fixability. The content of the binder resin in the toner particles is preferably from 40% by mass to 90% by mass, and more preferably from 50% by mass to 80% by mass.
[0016] <Crystalline polyester> The crystalline polyester contained in the toner particles contains a unit derived from an aliphatic diol and a unit derived from an aliphatic dicarboxylic acid. The crystalline polyester is preferably a condensation polymer of an alcohol containing an aliphatic diol having 2 to 15 carbon atoms and a carboxylic acid containing an aliphatic dicarboxylic acid having 3 to 17 carbon atoms. The crystalline polyester is more preferably a condensation polymer of an alcohol containing an aliphatic diol having 4 to 12 carbon atoms in an amount of 80 mol % to 100 mol % (more preferably, 85 mol % to 100 mol %) relative to the total alcohol constituting the crystalline polyester, and an aliphatic dicarboxylic acid having 4 to 17 carbon atoms in an amount of 80 mol % to 100 mol % (more preferably, 85 mol % to 100 mol %) relative to the total carboxylic acid constituting the crystalline polyester.
[0017] The aliphatic diol is preferably a straight-chain aliphatic diol, and examples thereof include 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, and derivatives thereof. The derivative is not particularly limited as long as it can be used to obtain a crystalline polyester by condensation polymerization. For example, a derivative obtained by esterifying a diol can be used.
[0018] The aliphatic dicarboxylic acid is preferably a straight-chain aliphatic dicarboxylic acid, and examples thereof include malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, hexadecanedioic acid, eicosanedioic acid, and derivatives thereof. The derivative is not particularly limited as long as it can obtain a similar resin structure by condensation polymerization. For example, derivatives such as acid anhydrides of dicarboxylic acids, alkyl esters of dicarboxylic acids, and acid chlorides of dicarboxylic acids can be included.
[0019] On the other hand, the carboxylic acid may be used in combination with a carboxylic acid other than the aliphatic dicarboxylic acid.
[0020] In the present invention, the ester group concentration Ec of the crystalline polyester is a value indicating the ratio of the mass of the ester group [-C(=O)O-] to the mass of 1 mole of the crystalline polyester, and specifically, is a value represented by the following formula (1). Ester group concentration Ec (mass%)=[(N×44) / (1×number average molecular weight)]×100 Formula (1) In formula (1), N is the average number of ester groups contained in one molecule of the crystalline polyester, 44 is the formula weight of the ester group [-C(=O)O-], and the number average molecular weight is the number average molecular weight of the crystalline polyester.
[0021] The ester group concentration Ec of the crystalline polyester is 27% by mass or more and 50% by mass or less, and preferably 27% by mass or more and 40% by mass or less. When it is in the above range, the interaction with calcium carbonate described below becomes appropriate, and the hot offset resistance of the toner is improved.
[0022] On the other hand, when the ratio of the mass of the ester group [-C(=O)O-] to the mass of 1 mole of the binder resin is defined as the ester group concentration Ea of the binder resin, the relationship (Ea / Ec) between the ester group concentration Ec of the crystalline polyester and the ester group concentration Ea of the binder resin is preferably 0.5 or more and 0.7 or less. The above range improves the low-temperature fixability of the toner. When Ea / Ec is higher than 0.7, the interaction between the binder resin and the calcium carbonate particles is too strong, so the compatibility between the binder resin and the crystalline polyester decreases, and the low-temperature fixability decreases. When Ea / Ec is less than 0.5, the interaction between the crystalline polyester and the calcium carbonate particles is too strong, so the compatibility between the crystalline polyester and the binder resin decreases, and the low-temperature fixability decreases. The acid value of the crystalline polyester is preferably from 0 mgKOH / g to 10 mgKOH / g in terms of low-temperature fixation, and more preferably from 0 mgKOH / g to 5 mgKOH / g.
[0023] The content Mc of the crystalline polyester contained in the toner particles is preferably 0.1% by mass or more and 5.0% by mass or less with respect to the mass of the toner particles. When the content of the crystalline polyester is in the above range, the binder resin exhibits sufficient plasticity, and the crystalline polyester is easily finely dispersed in the toner particles, thereby further improving low-temperature fixability.
[0024] <Calcium carbonate particles> The toner particles include calcium carbonate particles. As the calcium carbonate particles, for example, light calcium carbonate or colloidal calcium carbonate can be used.
[0025] The content Ma of calcium carbonate particles contained in the toner particles is 3% by mass or more and 40% by mass or less, and preferably 10% by mass or more and 33% by mass or less. When the content is in the above range, the interaction with the crystalline polyester becomes appropriate, the hot offset resistance of the toner is improved, and the abrasion resistance of the fixed image is also improved.
[0026] The ratio (Ma / Mc) of the content Ma of calcium carbonate particles contained in the toner particles to the content Mc of crystalline polyester contained in the toner particles is, by mass, from 0.2 to 20, preferably from 1 to 10, and more preferably from 5 to 10. When it is in the above range, the filler effect is efficiently exhibited, and the hot offset resistance of the toner is improved.
[0027] In the cross section of the toner particle observed by a transmission electron microscope, the average aspect ratio (long axis / short axis) of the calcium carbonate particles is preferably 1.5 to 6.0, more preferably 1.8 to 2.7, and even more preferably 2.0 to 2.5. When the aspect ratio is within the above range, the hot offset resistance and low temperature fixability of the toner are improved. When the aspect ratio is less than 1.5, the specific surface area of the calcium carbonate particles decreases, reducing the filler effect, thereby reducing the hot offset resistance. When the aspect ratio is more than 3.0, the filler effect becomes excessive, thereby reducing the low temperature fixability.
[0028] In the cross section of a toner particle observed under a transmission electron microscope, the standard deviation of the aspect ratio of calcium carbonate particles is preferably 1.3 or less, and more preferably 1.0 or less. If the standard deviation of the aspect ratio is more than 1.3, there will be a distribution of areas where the interaction between the crystalline polyester and the calcium carbonate particles is strong and areas where it is weak, which is thought to result in a decrease in the hot offset resistance of the toner.
[0029] In the cross section of the toner particles observed by a transmission electron microscope, the average number particle diameter of the calcium carbonate particles is preferably 100 nm or more and 600 nm or less, more preferably 300 nm or more and 400 nm or less. By being in the above range, the interaction between the ester group of the crystalline polyester and the calcium carbonate particles is improved, and the scratch resistance of the fixed image is improved. On the other hand, when the average number particle diameter of the calcium carbonate particles is less than 100 nm, the interaction between the ester group of the crystalline polyester and the calcium carbonate particles is small, and the scratch resistance of the fixed image is not improved. Also, when the average number particle diameter of the calcium carbonate particles is more than 600 nm, the interaction between the ester group of the crystalline polyester and the calcium carbonate particles is large, the dispersibility of the calcium carbonate particles in the binder resin is deteriorated, and the scratch resistance of the fixed image is not improved.
[0030] The calcium atom abundance ratio A of the toner surface calculated by X-ray photoelectron spectroscopy is preferably 0 atom% or more and 0.5 atom% or less, more preferably 0 atom% or more and 0.3 atom% or less. By being in the above range, the interaction between the ester group of the crystalline polyester and the calcium carbonate particles is improved, the filler effect is efficiently expressed, and the hot offset resistance of the toner and the abrasion resistance of the fixed image are improved. If the abundance ratio A is higher than the above range, many calcium carbonate particles are present between the toner particles in the toner layer formed on the paper, that is, the dispersibility of the calcium carbonate particles is deteriorated, and the filler effect is reduced, so that the hot offset resistance is reduced. The calcium atom abundance ratio A of the toner surface can be controlled by the hot air temperature in the hot air treatment process described later.
[0031] <Polymer a> From the viewpoint of hot offset resistance of the toner, it is preferable that the toner particles contain polymer a, which is a polymer obtained by graft polymerization of a styrene-acrylic resin to a polyolefin. If the toner particles do not contain polymer a, there is no interaction between the calcium carbonate particles and polymer a, and the dispersibility of the calcium carbonate particles in the binder resin may deteriorate. In this case, the filler effect is reduced, and the hot offset resistance of the toner may be reduced.
[0032] The polyolefin is not particularly limited, but examples thereof include low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymer, microcrystalline wax, ester wax, paraffin wax, and Fischer-Tropsch wax. From the viewpoint of reactivity during the production of the polymer a, it is preferable that the polyolefin has a branched structure like polypropylene.
[0033] In the present invention, the method of graft-modifying the styrene-acrylic resin with a hydrocarbon compound is not particularly limited, and any conventionally known method can be used. In the polymer a of the present invention, it is more preferable that the styrene-acrylic resin has a structural portion derived from a saturated alicyclic compound. For example, the styrene-acrylic resin may have a monomer unit represented by the following formula (A). [ka] In formula (A), R 1 represents a hydrogen atom or a methyl group, R 2 represents a saturated alicyclic group. R 2 The saturated alicyclic group represented by the formula (I) is preferably a saturated alicyclic hydrocarbon group, more preferably a saturated alicyclic hydrocarbon group having from 3 to 18 carbon atoms, and further preferably a saturated alicyclic hydrocarbon group having from 4 to 12 carbon atoms. Saturated alicyclic hydrocarbon groups include cycloalkyl groups, condensed polycyclic hydrocarbon groups, bridged ring hydrocarbon groups, spiro hydrocarbon groups, and the like.
[0034] Examples of such saturated alicyclic groups include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, tricyclodecanyl, decahydro-2-naphthyl, tricyclo[5.2.1.02,6]decan-8-yl, pentacyclopentadecanyl, bicyclo[2.2.1]heptan-2-yl, adamantyl, dicyclopentanyl, and tricyclopentanyl. The saturated alicyclic group may also have an alkyl group, a halogen atom, a carboxy group, a carbonyl group, or a hydroxyl group as a substituent. The alkyl group is preferably an alkyl group having 1 to 4 carbon atoms.
[0035] Of these saturated alicyclic groups, a cycloalkyl group, a condensed polycyclic hydrocarbon group, or a bridged ring hydrocarbon group is preferred, a cycloalkyl group having from 3 to 18 carbon atoms, a substituted or unsubstituted dicyclopentanyl group, or a substituted or unsubstituted tricyclopentanyl group is more preferred, a cycloalkyl group having from 4 to 12 carbon atoms is even more preferred, and a cycloalkyl group having from 6 to 10 carbon atoms is particularly preferred.
[0036] The positions and number of the substituents are optional, and when there are two or more substituents, the substituents may be the same or different.
[0037] The styrene-acrylic resin may be a homopolymer of a vinyl monomer (a) having a structural portion derived from a saturated alicyclic compound, or may be a copolymer with another monomer (b).
[0038] Examples of the vinyl monomer (a) having a structure portion derived from a saturated alicyclic compound include cyclopropyl acrylate, cyclobutyl acrylate, cyclopentyl acrylate, cyclohexyl acrylate, cycloheptyl acrylate, cyclooctyl acrylate, cyclopropyl methacrylate, cyclobutyl methacrylate, cyclopentyl methacrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, cyclooctyl methacrylate, dihydrocyclopentadiethyl acrylate, dicyclopentanyl acrylate, dicyclopentanyl methacrylate, and the like monomers, and their combinations.Among these, from the viewpoint of hydrophobicity, cyclohexyl acrylate, cycloheptyl acrylate, cyclooctyl acrylate, cyclohexyl methacrylate, cycloheptyl methacrylate, and cyclooctyl methacrylate are preferred.
[0039] Examples of other monomers (b) include styrene-based monomers such as styrene, α-methylstyrene, p-methylstyrene, m-methylstyrene, p-methoxystyrene, p-hydroxystyrene, p-acetoxystyrene, vinyltoluene, ethylstyrene, phenylstyrene, and benzylstyrene; alkyl esters of unsaturated carboxylic acids (alkyl having 1 to 18 carbon atoms) such as methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, and 2-ethylhexyl methacrylate; vinyl ester-based monomers such as vinyl acetate; vinyl ether-based monomers such as vinyl methyl ether; halogen-containing vinyl monomers such as vinyl chloride; olefin-based monomers such as butadiene and isobutylene; and combinations of these.
[0040] The ratio (Mo / Mc) of the content Mo of polymer a contained in the toner particles to the content Mc of crystalline polyester contained in the toner particles is preferably 0.3 to 25, and more preferably 0.4 to 15, by mass. The ratio (Mo / Ma) of the content Mo of polymer a contained in the toner particles to the content Ma of calcium carbonate particles contained in the toner particles is preferably 0.08 to 6, and more preferably 0.1 to 4, by mass. When the ratio is within the above range, the interaction between polymer a and the calcium carbonate particles is improved, and the abrasion resistance of the fixed image is improved.
[0041] <Release agent> The toner particles may contain a release agent. Examples of the release agent include the following: low molecular weight polyolefins such as polyethylene; silicones having a melting point; fatty acid amides such as oleic acid amide, erucic acid amide, ricinoleic acid amide, and stearic acid amide; ester waxes such as stearyl stearate; vegetable waxes such as carnauba wax, rice wax, candelilla wax, wood wax, and jojoba oil; animal waxes such as beeswax; mineral and petroleum waxes such as montan wax, ozokerite, ceresin, paraffin wax, microcrystalline wax, Fischer-Tropsch wax, and ester wax; and modified products thereof.
[0042] The release agent may be used alone or in combination of two or more. The melting point of the release agent is preferably 150° C. or lower, more preferably 40° C. or higher and 130° C. or lower, and even more preferably 40° C. or higher and 110° C. or lower. The content of the release agent is preferably 1 part by mass or higher and 30 parts by mass or lower relative to 100 parts by mass of the binder resin.
[0043] <Coloring agent> The toner particles may contain a colorant, such as a known organic pigment or oil-based dye, carbon black, or a magnetic material.
[0044] Examples of cyan colorants include copper phthalocyanine compounds and their derivatives, anthraquinone compounds, basic dye lake compounds, etc. Specific examples include CI Pigment Blue 1, 7, 15, 15:1, 15:2, 15:3, 15:4, 60, 62, 66, etc.
[0045] Examples of magenta colorants include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, perylene compounds, etc. Specific examples include CI Pigment Red 2, 3, 5, 6, 7, 23, 48:2, 48:3, 48:4, 57:1, 81:1, 122, 144, 146, 166, 169, 177, 184, 185, 202, 206, 220, 221, 254, CI Pigment Violet 19, etc.
[0046] Examples of yellow colorants include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds.Specific examples include CI Pigment Yellow 12, 13, 14, 15, 17, 62, 74, 83, 93, 94, 95, 97, 109, 110, 111, 120, 127, 128, 129, 147, 151, 154, 155, 168, 174, 175, 176, 180, 181, 191, and 194.
[0047] Examples of black colorants include carbon black, magnetic materials, and those toned to black using yellow colorants, magenta colorants, and cyan colorants.
[0048] The colorant may be used alone or in combination of two or more. It may also be used in the form of a solid solution. The colorant may be selected from the viewpoints of hue angle, chroma, brightness, light resistance, OHP transparency, and dispersibility in toner particles. The content of the colorant is preferably 1 part by mass or more and 20 parts by mass or less with respect to 100 parts by mass of the binder resin.
[0049] <External additives> The toner may contain inorganic fine particles as necessary. The inorganic fine particles may be added internally to the toner particles, or may be mixed with the toner particles as an external additive.
[0050] When inorganic fine particles are contained as an external additive, inorganic fine particles such as silica fine particles, titanium oxide fine particles, and aluminum oxide fine particles are preferred. The inorganic fine particles are preferably hydrophobized with a hydrophobizing agent such as a silane compound, silicone oil, or a mixture thereof. When the inorganic fine particles are used to improve the flowability of the toner, the inorganic fine particles are preferably those having a specific surface area of 50 m 2 / g or more 400m 2 On the other hand, when inorganic fine particles are used to improve the durability of the toner, it is preferable that the specific surface area is 10 m 2 / g or more 50m 2 / g or less. In order to achieve both fluidity and durability, inorganic fine particles having a specific surface area in the above range may be used in combination. When inorganic fine particles are contained as an external additive, the amount is preferably 0.1 parts by mass or more and 10.0 parts by mass or less relative to 100 parts by mass of toner particles. The toner particles and the inorganic fine particles may be mixed using a known mixer such as a Henschel mixer.
[0051] <Toner manufacturing method> The method for producing the toner is not particularly limited, and known methods such as emulsion aggregation, pulverization, and suspension polymerization can be used. Preferably, the method for producing the toner includes a step of melt-kneading a mixture containing a binder resin, a crystalline polyester, calcium carbonate particles, and a colorant to obtain a melt-kneaded product, and a step of pulverizing the melt-kneaded product to obtain toner particles. By performing the melt-kneading, the crystalline polyester and the calcium carbonate particles are dispersed in the binder resin, the interaction between the crystalline polyester and the calcium carbonate particles is improved, a filler effect is expressed, and the hot offset resistance of the toner is improved.
[0052] Hereinafter, a procedure for producing a toner containing pulverized toner particles using a pulverization method will be described as an example. First, materials constituting the toner particles, such as binder resin, crystalline polyester, calcium carbonate particles, and pigment, as well as other components such as a release agent and a charge control agent as necessary, are weighed out in predetermined amounts, blended, and mixed. Examples of mixing devices include a double con mixer, a V-type mixer, a drum mixer, a super mixer, a Henschel mixer, a Nauta mixer, and a Mechano Hybrid.
[0053] Next, the mixed materials are melt-kneaded. In the melt-kneading process, a batch-type kneader such as a pressure kneader or a Banbury mixer, or a continuous kneader can be used, and a single-screw or twin-screw extruder is preferred because of its advantage of being able to produce continuously. The temperature of the melt-kneading is preferably about 100 to 200°C. Examples of twin-screw extruders include a KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a PCM kneader (manufactured by Ikegai Iron Works Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a Co-kneader (manufactured by Buss Co., Ltd.), and Kneadex (manufactured by Nippon Coke and Engineering Co., Ltd.). Furthermore, the resin composition obtained by melt-kneading is rolled with a two-roller or the like, and quenched with water or the like in a cooling process.
[0054] The cooled resin composition is then pulverized to a desired particle size in a pulverization process, which involves coarse pulverization using a pulverizer such as a crusher, hammer mill, or feather mill, followed by further pulverization using a pulverizer such as a Cryptron System (Kawasaki Heavy Industries), a Super Rotor (Nisshin Engineering), a Turbo Mill (Turbo Kogyo), or an air jet type pulverizer.
[0055] Thereafter, as necessary, the mixture is classified using a classifier or sieve such as an inertial classification type Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), a centrifugal classification type Turboplex (manufactured by Hosokawa Micron Corporation), a TSP Separator (manufactured by Hosokawa Micron Corporation), or a Faculty (manufactured by Hosokawa Micron Corporation), to obtain pulverized toner particles as a classified product.
[0056] <Surface treatment using hot air> The toner particles are desirably surface-treated with hot air. The surface treatment with hot air allows the shape of the classified product to be adjusted or the surface to be treated. The temperature of the hot air is preferably in the range of 100°C or higher and 450°C or lower. By being in the above range, it is possible to control the abundance ratio A of calcium atoms on the toner surface to be in the above range.
[0057] An example of a thermal surface treatment apparatus is shown in Fig. 1. In Fig. 1, a mixture supplied by a material supplying means 1 is introduced into an inlet pipe 3 installed on the central axis of a treatment chamber 6 by compressed gas adjusted by a compressed gas adjusting means 2. The mixture passing through the inlet pipe 3 is uniformly dispersed by a conical protruding member 4 provided in the center of the inlet pipe 3, and introduced into eight supply pipes 5 that radiate outward, and then introduced into the treatment chamber 6 where heat treatment is carried out from a powder particle supply port 14.
[0058] At this time, the flow of the mixture supplied to the processing chamber 6 is regulated by a regulating means 9 for regulating the flow of the mixture, which is provided in the processing chamber 6. Therefore, the mixture supplied to the processing chamber 6 is heat-treated while swirling inside the processing chamber 6, and then cooled by cold air supplied from the cold air supplying means 8 (cold air supplying means 8-1, cold air supplying means 8-2, and cold air supplying means 8-3).
[0059] Hot air for heat-treating the supplied mixture is supplied from hot air inlet 11 of hot air supplying means 7, and is introduced into treatment chamber 6 by spirally swirling it using swirling member 13 for swirling the hot air. In terms of configuration, swirling member 13 for swirling the hot air has multiple blades, and the swirling of the hot air can be controlled by the number and angle of the blades. At this time, the approximately conical distribution member 12 can reduce bias in the swirling hot air.
[0060] The hot air supplied into the processing chamber 6 preferably has a temperature of 100° C. to 300° C. at the hot air outlet 10 of the hot air supplying means 7. If the temperature at the hot air outlet 10 of the hot air supplying means 7 is within the above range, it becomes possible to uniformly sphericalize the toner particles while preventing fusion and coalescence of the toner particles caused by overheating the mixture.
[0061] The toner particles obtained through the above steps may be used as a toner as it is. If necessary, an external additive may be added to the surface of the toner particles to form a toner. As a method for adding an external additive, a method may be used in which a predetermined amount of a known external additive is mixed with the toner particles, and the mixture is stirred and mixed using a mixing device such as a double con mixer, a V-type mixer, a drum type mixer, a super mixer, a Henschel mixer, a Nauta mixer, a Mechano Hybrid (manufactured by Nippon Coke & Engineering Co., Ltd.), or a Nobilta (manufactured by Hosokawa Micron Corporation) as an external additive machine.
[0062] The volume-based median diameter of the toner is preferably 3.0 μm or more and 30.0 μm or less, and more preferably 4.0 μm or more and 20.0 μm or less.
[0063] The methods for measuring physical properties related to the present invention will be described below. [Measurement of acid value of resin] The acid value of a resin is the number of milligrams of potassium hydroxide required to neutralize the acid components, such as free fatty acids or resin acids, contained in 1 g of a sample. The acid value is measured in accordance with JIS K 0070-1992, and specifically, is measured according to the following procedure.
[0064] (1) Preparation of reagents Dissolve 1.0 g of phenolphthalein in 90 mL of ethanol (95% by volume), add ion-exchanged water to make 100 mL, and obtain a phenolphthalein solution. Dissolve 7 g of special grade potassium hydroxide in 5 mL of water, and add ethanol (95% by volume) to make 1 L. Place in an alkali-resistant container to avoid contact with carbon dioxide, etc., leave for 3 days, then filter to obtain a potassium hydroxide solution. Store the resulting potassium hydroxide solution in an alkali-resistant container. The factor of the potassium hydroxide solution is calculated by placing 25 mL of 0.1 mol / L hydrochloric acid in an Erlenmeyer flask, adding a few drops of phenolphthalein solution, and titrating with potassium hydroxide solution, and determining the amount of potassium hydroxide solution required for neutralization. Use 0.1 mol / L hydrochloric acid prepared in accordance with JIS K 8001-1998.
[0065] (2) Operation (A) Main Test Weigh out 2.0 g of the crushed sample into a 200 mL Erlenmeyer flask, add 100 mL of a toluene / ethanol (2:1) mixed solution, and dissolve for 5 hours. Next, add a few drops of phenolphthalein solution as an indicator, and titrate with potassium hydroxide solution. The end point of the titration is when the indicator remains a pale red color for about 30 seconds. (B) Blank test The titration is carried out in the same manner as above, except that no sample is used (i.e., only the toluene / ethanol (2:1) mixed solution is used).
[0066] (3) The obtained result is substituted into the following formula to calculate the acid value. A = [(CB) × f × 5.61] / 2.0 In the above formula, A is the acid value of the resin (mgKOH / g), B is the amount of potassium hydroxide solution added in the blank test (mL), C is the amount of potassium hydroxide solution added in the main test (mL), and f is the factor of the potassium hydroxide solution.
[0067] [Surface composition analysis by X-ray photoelectron spectroscopy (ESCA)] The abundance ratio A of calcium atoms on the surface of the toner is calculated by performing a surface composition analysis by X-ray photoelectron spectroscopy (ESCA). The ESCA device and measurement conditions are as follows: Equipment used: PHI5000 VersaProbeII Scanning XPS Microprobe manufactured by PHI (Physical Electronics Industries, INC.) Measurement conditions: X-ray source; AlKα (100μ25W15KV) Angle; 45° Pass Energy: 58.70 eV From the peak intensity of each element measured under the above conditions, the surface atomic concentration (atomic %) is calculated using the relative sensitivity factor provided by PHI Co., Ltd. The surface atomic concentration of calcium atoms is defined as the abundance ratio A of calcium atoms. The six elements measured are C, O, Si, Ti, and Ca, and the percentage of calcium atoms among these six elements is calculated. For each atom, the peak intensities based on the C: 1s, O: 1s, Si: 2p, Ca: 2p, and Ti: 2p orbitals are referenced.
[0068] [Aspect ratio of calcium carbonate particles] The cross-section observation of the toner and the evaluation of the aspect ratio of the calcium carbonate particles can be carried out by cross-sectional observation as follows. The cross section of a toner particle can be prepared by placing the toner particles on a carbon tape, sputtering PtPd for 60 seconds, and scraping it off with argon ion beam irradiation. Cross-sectional images of the toner particles are obtained using a backscattered electron imaging method using a Hitachi ultra-high resolution field emission scanning electron microscope S-4800 (Hitachi High-Technologies Corporation). By observing the cross section of the toner, calcium carbonate particles can be obtained as a clear contrast. Note that particles in the cross-sectional images of the toner particles are identified using an energy dispersive X-ray spectrometer (EDAX) or the like. The aspect ratio of calcium carbonate particles is defined as the major axis / minor axis of the calcium carbonate particles. The major axis of calcium carbonate particles can be measured as the length in the longitudinal direction (the length of the long side) when the calcium carbonate particles are regarded as a rectangle. The minor axis of calcium carbonate particles can be measured as the length in the lateral direction (the length of the short side) when the calcium carbonate particles are regarded as a rectangle. The above aspect ratio is measured for 100 calcium carbonate particles, and the average value and standard deviation are calculated.
[0069] [Particle size of calcium carbonate particles] The number-average particle size of calcium carbonate particles means the number-average of the major axis of primary particles of calcium carbonate. The number-average particle size of calcium carbonate particles can be measured from a backscattered electron image of calcium carbonate particles obtained by photographing the cross section of a toner particle using the S-4800 described above. Specifically, the major axis of 100 calcium carbonate particles is measured and the average value is calculated.
[0070] [Method of measuring the content Mc of crystalline polyester and the ester group concentration Ec of crystalline polyester] Add 160 g of sucrose (Kishida Chemical) to 100 mL of ion-exchanged water and dissolve in a hot water bath to prepare a concentrated sucrose solution. Add 31 g of the concentrated sucrose solution and 6 mL of Contaminon N (a 10% aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of nonionic surfactants, anionic surfactants, and organic builders, manufactured by Wako Pure Chemical Industries, Ltd.) to a centrifuge tube to prepare a dispersion. Add 1.0 g of toner to this dispersion, and break up the toner clumps with a spatula or the like. Next, shake the centrifuge tube with a shaker. After shaking, transfer the solution to a glass tube (50 mL) for a swing rotor and separate it in a centrifuge at 3,500 rpm for 30 minutes. This operation separates the toner particles from the external additives that have been removed. After visually confirming that the toner particles and the aqueous solution have been sufficiently separated, the toner particles are collected and filtered with a vacuum filter, and then dried in a dryer for at least one hour to obtain toner particles from which the external additives have been separated. The weight of the toner particles obtained is measured.
[0071] From the toner particles from which the external additives have been separated by the above method, the binder resin and polymer a are dissolved in methyl ethyl ketone at 23° C., and filtered to obtain filtrate 1 and filtered product 1. After drying the filtrate 1, the crystalline polyester and the release agent are dissolved at 100°C using heated methyl ethyl ketone, and filtered to obtain filtrate 2 and filtrate 2. After drying the filtrate 2, the crystalline polyester is dissolved using chloroform, and filtered to obtain filtrate 3 and filtrate 3. The filtrate 3 is concentrated and dried, and the content Mc of the crystalline polyester is measured based on the weight of the toner particles.
[0072] The ester group concentration Ec of the obtained crystalline polyester can be measured by using GPC and gas chromatography (GS / MS). For example, the ester group concentration Ec of the crystalline polyester can be calculated from the formula (1). Ester group concentration Ec (mass%) = [(N×44) / (1×number average molecular weight Mn)]×100 Formula (1) In formula (1), N is the average number of ester groups contained in one molecule of the crystalline polyester, 44 is the formula weight of the ester group, and the number average molecular weight Mn is the number average molecular weight of the crystalline polyester.
[0073] The number average molecular weight Mn of the crystalline polyester can be calculated using a GPC measurement system, for example, by a method using the following apparatus. First, a column (trade name: PLgel 5μm Guard 50×7.5mm, manufactured by Agilent Technologies) is used as a guard column, and a GPC measurement system (manufactured by Shimadzu Corporation) in which two columns (trade name: PLgel Mixed C, manufactured by Agilent Technologies) are connected in series is used to measure standard polystyrene (trade name: TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, and A-500, all manufactured by Toso Corporation), and a calibration curve is created from the peaks detected by the RI detector to obtain the molecular weight distribution. Next, 50 mg of the crystalline polyester obtained above is dissolved in 5 mL of chloroform and allowed to stand for about 5 hours to obtain a solution. This solution is filtered through a solvent-resistant membrane filter with a pore size of 0.5 μm (product name: Myshoridisk H-25-5, manufactured by Tosoh Corporation) to obtain a sample solution. The obtained sample solution is measured under the same conditions as standard polystyrene, and the molecular weight corresponding to the obtained peak is obtained from the calibration curve, and the number average molecular weight Mn of the crystalline polyester is calculated.
[0074] The alcohol containing aliphatic diol and the carboxylic acid containing aliphatic dicarboxylic acid contained in the crystalline polyester can be identified by the following method, for example, using pyrolysis gas chromatography. Approximately 200 μg of crystalline polyester to which 1 μL of tetramethylammonium hydroxide has been added as a pyrolysis assistant is used as a sample. This sample is wrapped in F590 pyrofoil and heated at 590 ° C for 5 seconds using a pyrolysis device (for example, trade name: JPS-900, manufactured by Japan Analytical Industry Co., Ltd.) to decompose the crystalline polyester. The gas generated by the decomposition of the crystalline polyester is identified from the mass spectrum pattern obtained using, for example, a precise mass analyzer attached to a GC / MS measurement system (trade name: Accurate-Mass Q-TOF GC / MS7200, manufactured by Agilent Technologies) equipped with a column (trade name: HP-5MS, manufactured by Agilent Technologies) and a detector (trade name: JPS-900, manufactured by Japan Analytical Industry Co., Ltd.) to identify the alcohol containing aliphatic diol and the carboxylic acid containing aliphatic dicarboxylic acid contained in the crystalline polyester and the areas of the peaks derived therefrom.
[0075] Next, a calibration curve is created using a standard sample of the identified monomer, and the peak area and calibration curve derived from each monomer obtained by pyrolysis gas chromatography are used to determine the number of moles of the monomer. In this way, the molar ratio of the alcohol including the aliphatic diol and the carboxylic acid including the aliphatic dicarboxylic acid constituting the crystalline polyester (a, b, ..., x, y, ... in the composition formula below) is determined. (Carboxylic acid A) a (Carboxylic acid B) b… (Alcohol X) x (Alcohol Y) y…
[0076] The molecular weights of carboxylic acid A, carboxylic acid B, … are M A , M B , …, and the molecular weights of alcohol X, alcohol Y, … are M X , M Y , ..., the following formula (2) is established between the number average molecular weight Mn of the crystalline polyester: In formula (2), n is a positive number. Mn = {(M A +M B +…MX +M Y +…)-(a+b+…x+y+…-1)×18}×n Formula (2)
[0077] The value of n is calculated from formula (2), and the average number N of ester groups contained in one molecule of the crystalline polyester can be calculated from the following formula (3). N=(a+b+…x+y+…-1)×n Formula (3)
[0078] The ester group concentration Ea can be calculated by substituting the number average molecular weight Mn of the crystalline polyester and the average number N of ester groups per molecule of the crystalline polyester resin calculated above into formula (1).
[0079] <Method for measuring the ester group concentration Ea of the binder resin> After drying the filtrate 1, the binder resin (amorphous polyester) is dissolved with ethyl acetate to obtain a filtrate 4 and a residue 4. The filtrate 4 is concentrated and dried to obtain a binder resin. The ester group concentration Ea of the obtained binder resin can be measured using GPC and gas chromatography (GS / MS). The measurement of the ester group concentration Ea of the binder resin using GPC and gas chromatography (GS / MS) can be performed in the same manner as the measurement of the ester group concentration Ec of the crystalline polyester described above.
[0080] <Method for measuring calcium carbonate content Ma> The filtered matter 2 is centrifuged, concentrated and dried, and the calcium carbonate content Ma is measured based on the weight of the toner particles.
[0081] <Method of measuring the content Mo of polymer a> The content Mo of polymer a is measured based on the weight of the toner particles by drying the residue 4. The structure of polymer a is measured by using nuclear magnetic resonance spectroscopy (NMR) and infrared spectroscopy (IR). EXAMPLES
[0082] The present invention will be described in more detail below using examples and comparative examples, but these are not intended to limit the present invention in any way. In the following examples, the number of parts is based on parts by mass. Moreover, Examples 6 to 8 and 12 to 41 are reference examples.
[0083] <Production Example of Binder Resin A1> Fumaric acid: 54.3 parts Bisphenol A propylene oxide adduct (BPA-PO): 22.0 parts Dipropanol: 23.8 parts · Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts The above materials were weighed into a reaction vessel equipped with a condenser, stirrer, nitrogen inlet, and thermocouple. After the atmosphere in the reaction vessel was replaced with nitrogen gas, the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 140° C. with stirring. Next, the pressure in the reaction vessel was reduced to 8.3 kPa, and the temperature was raised to 200° C. with stirring, and the reaction was carried out for 4 hours (reaction step 1). Thereafter, the pressure in the reaction tank was reduced again to 5 kPa or less, and the mixture was reacted at 200° C. for 3 hours to obtain a binder resin A1 (reaction step 2).
[0084] <Production Examples of Binder Resins A2 to A11> Binder Resins A2 to A11 were obtained in the same manner as in the production example of Binder Resin A1, except that the types of carboxylic acid and alcohol were changed as shown in Table 1.
[0085] [Table 1] BPA-PO Propylene oxide adduct of bisphenol A BPA-EO Bisphenol A with ethylene oxide *The numbers in parentheses for alcohol and carboxylic acid components indicate the molar ratio (%) of each component.
[0086] <Production Example of Crystalline Polyester C1> Adipic acid: 40.9 parts (0.31 moles; 100.0 mol% of total moles of alcohol) 1,5-Pentanediol: 59.1 parts (0.31 moles; 100.0 mol% of total moles of carboxylic acid) ·Tin 2-ethylhexanoate: 0.5 parts The above materials were weighed into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. After replacing the inside of the reaction vessel with nitrogen gas, the temperature was gradually raised while stirring, and the reaction was carried out for 3 hours at a temperature of 140°C while stirring. Next, the pressure in the reaction vessel was reduced to 8.3kPa, and the temperature was raised to 200°C while stirring, and the reaction was carried out for 1 hour to obtain crystalline polyester C1. The ester group concentration Ec of the obtained crystalline polyester C1 was measured as described above. The results are shown in Table 2.
[0087] <Production Examples of Crystalline Polyesters C2 to C8> Crystalline polyesters C2 to C8 were obtained in the same manner as in the production example of crystalline polyester C1, except that the conditions were appropriately changed so that the types of aliphatic dicarboxylic acid and aliphatic diol were as shown in Table 2. The ester group concentration Ec of the obtained crystalline polyesters was measured as described above. The results are shown in Table 2.
[0088] [Table 2]
[0089] <Production Example of Polymer a1> In an autoclave reactor equipped with a thermometer and a stirrer, 300.0 parts of xylene and 10.0 parts of polypropylene (melting point 90°C) were added and thoroughly dissolved. After nitrogen replacement, a mixed solution of 68.0 parts of styrene, 5.0 parts of methacrylic acid, 5.0 parts of cyclohexyl methacrylate, 12.0 parts of butyl acrylate, and 250.0 parts of xylene was dropped at 180°C for 3 hours to carry out polymerization. After maintaining the mixture at this temperature for 30 minutes, the solvent was removed to obtain polymer a1.
[0090] <Toner 1 Manufacturing Example> Binder resin A1: 100 parts Crystalline polyester C1: 2 parts Calcium carbonate particles - 1: 15 parts (500 nm, aspect ratio 3.0) Fischer-Tropsch Wax 1: 6 parts (Hydrocarbon wax, melting point: 90℃) Colorant 1 (CI Pigment Blue 15:3) 7 parts Polymer A1 20 parts The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 The mixture was mixed at 100° C. for 5 minutes. The mixture was then kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Corporation) set at a temperature of 130° C. The kneaded mixture was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). The mixture was then classified using a Faculty F-300 (manufactured by Hosokawa Micron Corporation). The operating conditions for the Faculty F-300 were a classification rotor rotation speed of 130 s -1 , Distributed rotor speed 120s -1 It was decided. The classified particles were subjected to heat treatment using the surface treatment device shown in Figure 1. The operating conditions were feed rate = 3 kg / hr, hot air temperature = 130°C, hot air flow rate = 6 m 3 / min, cold air temperature = -5℃, cold air flow rate = 4m 3 / min, Blower air volume = 20m 3 / min, injection air flow rate = 1m 3 By carrying out the heat treatment, toner particles 1 having an average circularity of 0.96 were obtained.
[0091] 100 parts of the obtained toner particles, 1.0 part of hydrophobic silica fine particles (BET: 200 m2 / g) that had been hydrophobized with hexamethyldisilazane, and 1.0 part of titanium oxide fine particles (BET: 80 m2 / g) that had been surface-treated with isobutyltrimethoxysilane were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 30 s. -1The mixture was mixed at 100° C. for a rotation time of 10 minutes to obtain Toner 1. The volume average particle size of Toner 1 was 6.5 μm.
[0092] <Production Examples of Toners 2 to 21> Toners 2 to 21 were obtained in the same manner as in Production Example of Toner 1, except that the binder resin, crystalline polyester, calcium carbonate particles, polymer a, and heat treatment temperature were changed as shown in Table 3.
[0093] <Production Examples of Toners 22, 24 to 41 and Comparative Toners 1 to 12> In the production example of toner 1, the binder resin, crystalline polyester, and calcium carbonate particles were changed as shown in Table 3, and toners 22, 24 to 41, and comparative toners 1 to 12 were obtained in the same manner as in the production example of toner 1, except that the heat treatment was not performed.
[0094] <Production Example of Toner 23> For toner 23, the toner particles were prepared by an emulsion aggregation method.
[0095] Preparation of dispersion (Binder resin A8 dispersion) The binder resin A8 was mixed with 80% ion-exchanged water and 20% binder resin, and the pH was adjusted to 8.5 with ammonia. The mixture was heated to 100°C and operated at 4000 rpm using ultra-high speed stirrers T, K, and Robomix (manufactured by Primix Corporation), to obtain a dispersion of binder resin A8 (solid content: 20%).
[0096] (Crystalline polyester C4 dispersion) 80 parts of crystalline polyester C4 and 720 parts of ion-exchanged water were placed in a stainless steel beaker and heated to 100°C. When the crystalline polyester C4 was melted, it was stirred at 4000 rpm using an ultra-high speed stirrer T, K, Robomix (manufactured by Primix Co., Ltd.). Next, emulsification and dispersion were carried out while dropping 1.0 part of an anionic surfactant (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.: Neogen RK), to obtain a crystalline polyester C4 dispersion (solid content: 10%).
[0097] (Calcium carbonate particle-1 dispersion) Calcium carbonate particles-1 200 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK): 10 parts Ion-exchanged water 790 parts The above was mixed and stirred at 7000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation).Furthermore, it was dispersed at a pressure of 200 MPa using a high-pressure impact type disperser Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a calcium carbonate particle-1 dispersion liquid (concentration 20% by mass).
[0098] (Preparation of colorant dispersion) Colorant 1 100 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK): 10 parts Ion-exchanged water 890 parts The above was mixed and stirred at 7000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation). Further, it was dispersed at a pressure of 200 MPa using a high-pressure impact type dispersing device Nanomizer (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a dispersion liquid of Colorant 1 (concentration 10% by mass).
[0099] (Preparation of release agent dispersion) Fischer-Tropsch wax 1,200 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK): 10 parts Ion-exchanged water 790 parts The above was put into a mixing vessel equipped with a stirrer, heated to 90°C, and circulated to a Clearmix W Motion (M Techniques), where the mixture was stirred at a rotor rotation speed of 19,000 rpm and a screen rotation speed of 19,000 rpm at a shear stirring section with a rotor outer diameter of 3 cm and a clearance of 0.3 mm, and dispersed for 60 minutes. After that, the mixture was cooled to 40°C under cooling treatment conditions of a rotor rotation speed of 1,000 rpm, a screen rotation speed of 0 rpm, and a cooling rate of 10°C / min, to obtain a release agent dispersion (concentration 20% by mass).
[0100] (Toner 23 Production) Binder resin A8 dispersion: 100 parts Crystalline polyester C4 dispersion: 4 parts Calcium carbonate particle-1 dispersion: 15 parts Colorant dispersion: 14 parts Release agent dispersion: 6 parts Polyaluminum chloride: 0.2 parts The above materials were put into a homogenizer (IKA Ultra Turrax T50) and dispersed to prepare a slurry. The slurry was put into a stirrer equipped with a mantle heater, and the temperature was raised to 60°C while adjusting the rotation speed of the stirrer so that the slurry was sufficiently stirred. After holding at 60°C for 15 minutes, the particle size of the particles generated was measured every 10 minutes with a Coulter Multisizer III (aperture diameter: 50 μm, manufactured by Beckman Coulter, Inc.) while raising the temperature at 0.05°C / min, and when the volume average particle size reached 6.5 μm, the pH was adjusted to 9.0 using a 5% aqueous sodium hydroxide solution. Thereafter, the temperature was raised to 96°C at a heating rate of 1°C / min while adjusting the pH to 9.0 every 5°C, and the temperature was maintained at 96°C. The particle shape and surface properties were observed every 30 minutes with an optical microscope and a scanning electron microscope (FE-SEM), and when the average circularity reached 0.960, the temperature was lowered to 20°C at 1°C / min to solidify the particles. Thereafter, the reaction product was filtered, thoroughly washed with ion-exchanged water, and then dried using a vacuum dryer to obtain toner particles. 100 parts of the obtained toner particles and hydrophobic silica fine particles (BET: 200 m) that had been hydrophobized with hexamethyldisilazane were mixed. 2 / g) 1.0 part, and titanium oxide fine particles surface-treated with isobutyltrimethoxysilane (BET: 80m 2 The mixture was mixed with 1.0 part of 1.0 parts of 1 / g of water in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for a rotation time of 10 minutes to obtain Toner 23. The volume average particle size of the toner particles in Toner 23 was 6.6 μm.
[0101] [Table 3]
[0102] The results of the toner analysis are shown in Table 4. [Table 4]
[0103] The above toners were used to carry out the following evaluation tests. <Production Example of Magnetic Core Particle 1> Step 1 (weighing and mixing step) Fe 2 O 3 : 62.7 copies MnCO 3 : 29.5 copies Mg(OH) 2 : 6.8 copies SrCO 3 : 1.0 copies The above materials were weighed, and ground and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch to obtain a ground mixture.
[0104] Step 2 (Pre-firing step) The resulting pulverized mixture was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the obtained calcined ferrite is as follows: (MnO) 0.257 (MgO) 0.117 (SrO) 0.007 (Fe 2 O 3 ) 0.393
[0105] Step 3 (Crushing step) The obtained calcined ferrite was crushed to about 0.3 mm using a crusher, and then 30 parts of water was added to 100 parts of the calcined ferrite, and the mixture was crushed in a wet ball mill using zirconia beads with a diameter of 1 / 8 inch for 1 hour. The obtained slurry was crushed in a wet ball mill using alumina beads with a diameter of 1 / 16 inch for 4 hours to obtain a ferrite slurry (finely crushed calcined ferrite).
[0106] ·Process 4 (granulation process) To the ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of calcined ferrite, and the mixture was spray-dried using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.) to granulate into spherical particles. After adjusting the particle size of the obtained particles, the particles were heated at 650°C for 2 hours in a rotary kiln to remove the organic components of the dispersant and binder.
[0107] Step 5 (firing process) In order to control the sintering atmosphere, the temperature was raised from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then the spherical particles were sintered for 4 hours at a temperature of 1150°C. The temperature of the electric furnace was then lowered to 60°C over a period of 4 hours, the nitrogen atmosphere was returned to the air, and the spherical particles were taken out at a temperature of 40°C or less.
[0108] Step 6 (sorting step): After crushing the spherical particles that had aggregated during the firing process, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with a mesh size of 250 μm to obtain magnetic core particles 1 with a volume distribution-based 50% particle size (D50) of 37.0 μm.
[0109] <Preparation of Coating Resin 1> Cyclohexyl methacrylate monomer: 26.8% by mass Methyl methacrylate monomer: 0.2% by weight Methyl methacrylate macromonomer: 8.4% by mass (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene: 31.3% by mass Methyl ethyl ketone: 31.3% by mass Azobisisobutyronitrile 2.0% by mass The above materials were placed in a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer. Nitrogen gas was introduced into the flask to create a sufficient nitrogen atmosphere, and the flask was then heated to 80°C. Thereafter, 2.0% by mass of azobisisobutyronitrile was added and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate the copolymer, and the precipitate was filtered off and dried in vacuum to obtain coating resin 1. 30 parts of the obtained coating resin 1 were dissolved in 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain a polymer solution 1 (resin solid content concentration: 30% by mass).
[0110] <Preparation of coating resin solution 1> ·Polymer solution 1 (resin solid content concentration 30% by mass): 33.3% by mass Toluene: 66.4% by mass Carbon black (Regal 330; Cabot Corporation): 0.3% by mass (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m 2 / g, DBP oil absorption 75ml / 100g) The above materials were dispersed for 1 hour using zirconia beads with a diameter of 0.5 mm in a paint shaker. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.
[0111] <Magnetic Carrier 1 Manufacturing Example> (Resin coating process) Into a vacuum degassing kneader maintained at room temperature, 2.5 parts of coating resin solution 1 was added as a resin component to 100 parts of magnetic core particles 1. After the addition, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes. After a certain amount of the solvent (80% by mass) had evaporated, the mixture was heated to 80° C. while mixing under reduced pressure, and the toluene was distilled off over 2 hours, followed by cooling. The obtained magnetic carrier was subjected to magnetic separation to separate out low magnetic particles, which were passed through a sieve with 70 μm openings and then classified with an air classifier to obtain magnetic carrier 1 having a volume distribution standard 50% particle size (D50) of 38.2 μm.
[0112] <Production example of two-component developer 1> Toner 1 (8.0 parts) was added to magnetic carrier 1 (92.0 parts), and mixed in a V-type mixer (V-20, manufactured by Seishin Enterprises) to obtain two-component developer 1.
[0113] <Production Examples of Two-Component Developers 2 to 39 and Comparative Two-Component Developers 1 to 12> In the manufacturing example of two-component developer 1, the same operation was carried out except that the toner and magnetic carrier 1 shown in Table 5 were combined, to obtain two-component developers 2 to 39 and comparative two-component developers 1 to 12.
[0114] [Table 5]
[0115] A modified digital commercial printer (product name: imageRUNNER (trademark) ADVANCE C9075 PRO, manufactured by Canon) was used as the image forming device. A two-component developer was placed in the developer unit in the cyan position, and the DC voltage V of the developer carrier was adjusted so that the amount of toner on the electrostatic latent image carrier or paper was as desired. DC , the charging voltage of the electrostatic latent image carrier V D The laser power was adjusted and the evaluation described below was performed. The modification was made so that the fixing temperature and process speed could be freely set.
[0116] Test Example 1 [Evaluation of low-temperature fixability] In a low temperature and low humidity environment (temperature 15°C / humidity 10% RH), the evaluation paper (product name: CF-C104, manufactured by Canon Marketing Japan Inc., A4 size paper, basis weight: 104.0 g / m 2 ) The toner load on the 2 After adjusting the DC voltage VDC of the developer carrier, the charging voltage VD of the electrostatic latent image carrier, and the laser power so that the image was printed on the evaluation paper at a 25 cm 2 An image of 1000 x 1000 mm was printed and the low temperature fixability of the image was evaluated. The image density reduction rate was used as an evaluation index for low temperature fixability, and was measured using an X-Rite color reflection densitometer (500 series: manufactured by X-Rite). First, the image density in the center was measured, and then the part where the image density was measured was subjected to pressure of 4.9 kPa (50 g / cm 2 The fixed image was rubbed (five times back and forth) with Silbon paper under a load of 1000 g / m2, and the image density was measured again. The image density reduction rate (%) before and after rubbing was then measured. A grade of C or higher was deemed to be good. The evaluation results are shown in Table 6. The evaluation criteria were as follows: A: Concentration reduction rate less than 1.0% B: Concentration reduction rate: 1.0% or more and less than 5.0% C: Concentration reduction rate: 5.0% or more and less than 10.0% D: Concentration decrease rate 10.0% or more
[0117] Test Example 2 [Evaluation of Toner Hot Offset Resistance] Toner load on paper: 0.60mg / cm 2 Evaluation paper before image output (product name: CF-C104, manufactured by Canon Marketing Japan Inc., A4 paper, basis weight: 104.0 g / m 2 The reflectance of each of the five points was measured using a reflectometer (product name: REFLECTOMETER MODEL TC-6DS, manufactured by Tokyo Denshoku Co., Ltd.), and the average value measured at five points was taken as DA (%). The fixing temperature of the fixing unit of the image forming apparatus was changed, and the toner loading amount on the paper was 0.60 mg / cm 2At each fixing temperature when an image was printed so that the reflectance of the portion other than the image forming portion was measured with a reflectometer, and the maximum value was taken as DB (%). The highest fixing temperature at which the difference between DA (%) and DB (%) did not exceed 0.5% was taken as the upper limit fixing temperature. The hot offset resistance of the toner was evaluated based on the upper limit fixing temperature according to the following criteria. C or higher was judged to be good. The evaluation results are shown in Table 6. (Evaluation Criteria) A: 200℃ or higher B: 190℃ or higher but less than 200℃ C: 180℃ or higher but lower than 190℃ D: 170℃ or higher but lower than 180℃ E: Less than 170℃
[0118] Test Example 3 [Evaluation of Abrasion Resistance of Fixed Image] Evaluation paper (product name: OK Topcoat+, Oji Paper, basis weight: 127g / m 2 A halftone image with an image density of 0.20 to 0.25 was printed on the paper and used as the evaluation image. The image density of the evaluation image was measured using a "Macbeth Reflection Densitometer RD918" (manufactured by Macbeth) according to the attached instruction manual by measuring the relative density to the image of the white background part with an image density of 0.00, and the obtained relative density was used as the image density value. The evaluation paper was placed on top of the evaluation image, and a 500g weight was placed on top of it with a contact area of 12.6cm 2 The paper was then placed on the paper so that the paper was 12.6 cm long and rubbed 10 times to perform the rub resistance test. 2 The toner adhering to the area (the area where the weight was placed) was measured with a fog meter, and the fog values obtained were evaluated according to the following criteria. D or higher was judged to be good. The evaluation results are shown in Table 6. (Evaluation Criteria) A: Fog is 2% or less B: Fog is 2% or more but less than 5% C: Fog is 5% or more but less than 10% D: Fog is 10% or more but less than 15% E: Fog is 15% or more
[0119] [Table 6] [Explanation of symbols]
[0120] 1 Raw material quantitative supply means 2. Compressed gas regulation means 3 Introductory tube 4. Cone-shaped protruding member 5 Supply pipe 6 Processing Room 7 Hot air supply means 8 Cold air supply means 8-1 Cold air supply means 8-2 Cold air supply means 8-3 Cold air supply means 9. Regulatory measures 10 Hot air outlet 11 Hot air inlet 12 Distribution member
Claims
1. A toner having toner particles containing a binder resin, a crystalline polyester, and calcium carbonate particles, The crystalline polyester contains a unit derived from an aliphatic diol and a unit derived from an aliphatic dicarboxylic acid, The ester group concentration Ec of the crystalline polyester is 27% by mass or more and 50% by mass or less, the content Ma of the calcium carbonate particles contained in the toner particles is 3% by mass or more and 40% by mass or less, a ratio (Ma / Mc) of a content Ma of the calcium carbonate particles contained in the toner particles to a content Mc of the crystalline polyester contained in the toner particles, the ratio being 5 or more and 10 or less on a mass basis;
2. 2. The toner according to claim 1, wherein an average aspect ratio (major axis / minor axis) of the calcium carbonate particles in a cross section of the toner particle observed with a transmission electron microscope is 1.5 or more and 6.0 or less.
3. 3. The toner according to claim 1, wherein the calcium carbonate particles have an average particle size by number of 100 nm or more and 600 nm or less.
4. 4. The toner according to claim 1, wherein the acid value of the crystalline polyester is from 0 mgKOH / g to 10 mgKOH / g.
5. 5. The toner according to claim 1, wherein the amount Mc of the crystalline polyester contained in the toner particles is 0.1% by mass or more and 5.0% by mass or less.
6. 6. The toner according to claim 1, wherein an abundance ratio A of calcium atoms on the surface of the toner calculated by X-ray photoelectron spectroscopy is 0 atom % or more and 0.5 atom % or less.
7. 7. The toner according to claim 1, wherein the ester group concentration Ec of the crystalline polyester is 27% by mass or more and 40% by mass or less.
8. 8. The toner according to claim 1, wherein a relationship (Ea / Ec) between an ester group concentration Ea of the binder resin and an ester group concentration Ec of the crystalline polyester is 0.5 or more and 0.7 or less on a mass basis.
9. 9. The toner according to claim 1, wherein the toner particles further contain a polymer a in which a styrene-acrylic resin is graft-polymerized to a polyolefin.
10. 10. The toner according to claim 9, wherein a ratio (Mo / Mc) of a content Mo of the polymer a contained in the toner particles to a content Mc of the crystalline polyester contained in the toner particles is 0.3 to 25 on a mass basis, and a ratio (Mo / Ma) of a content Mo of the polymer a contained in the toner particles to a content Ma of calcium carbonate particles contained in the toner particles is 0.08 to 6 on a mass basis.
Citation Information
Patent Citations
Toner for electrostatic charge image development
JP2013200559A
Electrophotographic toner
JP2016114828A
Toner
JP2017003901A
Toner
JP2017054001A
Toner
JP2017090489A