Pigment dispersion and toner manufacturing method
The described method addresses the challenge of achieving small pigment particle sizes in toner production by using specific functional groups and ratios in the pigment, grinding agent, and binder to enhance productivity and prevent viscosity increases, resulting in efficient toner production.
Patent Information
- Application Number
- JP2020209740
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-17
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-12-17
AI Technical Summary
Conventional methods for reducing pigment particle size in toner production face challenges in achieving high productivity while maintaining small particle sizes, as increasing viscosity or grinding agent amounts leads to decreased throughput and equipment issues.
A method involving a pigment dispersion process with a pigment having an acidic functional group of 5 μmol/g or more, a grinding agent with a basic functional group of 5 μmol/g or more, and a binder with a basic functional group of 5 μmol/g or more, within a specific mass ratio of 0.01 to 0.30, to enhance acid-base interactions and reduce viscosity, allowing for finer pigments without productivity loss.
This approach enables the production of a pigment dispersion with small particle sizes and high productivity, suitable for toner applications, by leveraging acid-base interactions to maintain fluidity and prevent equipment overload.
Smart Images

Figure 0007587411000001 
Figure 0007587411000002 
Figure 0007587411000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a toner used in an electrophotographic system, an electrostatic recording system, an electrostatic printing system, or a toner jet system, and a method for producing a pigment dispersion used in the toner. [Background technology]
[0002] In recent years, full-color electrophotographic copiers have become widespread and are beginning to be applied to the printing market. In the printing market, there is a growing demand for high speed, high image quality, and high productivity while being compatible with a wide range of media (paper types). In order to achieve high image quality, there is a demand for further improvement in coloring power, and for this purpose, it is effective to reduce the particle size of pigments (Patent Document 1). Thus, solvent salt milling has been known as a method for reducing the particle size of pigments (Patent Document 2). In this method, a pigment with a large particle size is kneaded with a water-soluble inorganic salt as a grinding agent and a water-soluble organic solvent as a binder to disintegrate the pigment, thereby obtaining a pigment with a small particle size. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2007-100008 A [Patent Document 2] Japanese Patent Application Publication No. 3-84067 Summary of the Invention [Problem to be solved by the invention]
[0004] However, it is difficult to sufficiently reduce the diameter of the pigment by simply kneading the pigment, the water-soluble inorganic salt, and the water-soluble organic solvent. This is because, once the pigment is reduced in diameter to a certain extent, the rate at which the pigment aggregates exceeds the rate at which the pigment is reduced in diameter, and the pigment is no longer sufficiently small. In order to further reduce the diameter of the pigment, it is necessary to sufficiently increase the rate at which the pigment is reduced in diameter. If the viscosity of the binder is increased in order to apply a stronger shear stress in order to achieve this, the viscosity of the mixture of the pigment, the grinding agent, and the binder increases, reducing the processing capacity of the production equipment and reducing the amount of pigment that can be processed per unit time. In addition, if the amount of pigment is reduced and the grinding agent is increased, the speed of reducing the diameter increases, but the amount of pigment in the mixture of the pigment, the grinding agent, and the binder decreases, and this also reduces the amount of pigment that can be processed per unit time. In other words, when trying to further reduce the diameter of the pigment, the problem of reduced productivity occurs. In addition, from the viewpoint of protecting the kneading equipment, it is not preferable to increase the viscosity of the mixture of the pigment, the grinding agent, and the binder. [Means for solving the problem]
[0005] The present invention relates to a method for producing a pigment dispersion, which includes a pigment dispersion step of kneading a pigment, a binder, and a grinding agent, The pigment has an acidic functional group of 5 μmol / g or more, The grinding agent has a basic functional group content of 5 μmol / g or more, The binder contains a resin A having a basic functional group of 5 μmol / g or more, The mass ratio of the resin A to the pigment is 0.01 or more and 0.30 or less. The present invention relates to a method for producing a pigment dispersion. Effect of the Invention
[0006] According to the present invention, it is possible to provide a pigment dispersion having a small pigment diameter with high productivity and a method for producing the same, as well as a toner using the pigment dispersion and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] In the present invention, the description "XX to XX" representing a numerical range means a numerical range including the lower and upper limits which are the endpoints, unless otherwise specified.
[0008] A preferred method for producing the pigment dispersion in the present invention will be described in detail below. The present invention relates to a method for producing a pigment dispersion, which includes a pigment dispersion step of kneading a pigment, a binder, and a grinding agent, The pigment has an acidic functional group of 5 μmol / g or more, The grinding agent has a basic functional group content of 5 μmol / g or more, The binder contains a resin A having a basic functional group of 5 μmol / g or more, The mass ratio of the resin A to the pigment is 0.01 or more and 0.30 or less. The present invention relates to a method for producing a pigment dispersion.
[0009] Reducing the particle size of pigments is important to improve coloring power, but it is difficult to achieve further refinement using the conventional solvent salt milling method. This is thought to be because as the particle size of pigments becomes finer, they tend to aggregate, and when the pigments become small enough, the rate of aggregation exceeds the rate of refinement. Therefore, if one tries to increase the rate of refinement of pigments, the viscosity of the mixture of pigment, grinding agent, and binder increases, and the amount of pigment contained in the unit mixture decreases, resulting in a decrease in productivity.
[0010] The method of increasing the rate of fineness includes a method of increasing the viscosity of the mixture to strengthen the interaction between the pigment and the grinding agent when they meet, and a method of increasing the amount of grinding agent to increase the frequency of the pigment and the grinding agent meeting and increase the probability of fineness. When the viscosity of the binder is increased, the viscosity of the mixture of the pigment, grinding agent, and binder increases, thereby increasing the shear stress during kneading. On the other hand, when the viscosity of the mixture increases, productivity decreases due to deterioration of fluidity, adhesion to the wall of the production equipment, and overload of the equipment. In addition, increasing the amount of grinding agent relatively reduces the amount of pigment, which also reduces productivity. After extensive research, the inventors have succeeded in finerizing the pigment without increasing the viscosity of the mixture of the pigment, grinding agent, and binder when the pigment, grinding agent, and binder are under certain conditions.
[0011] The pigment of the present invention has acidic functional groups on its surface at 5 μmol / g or more, the grinding agent has basic functional groups on its surface at 5 μmol / g or more, and the binder contains resin A having basic functional groups on its surface at 5 μmol / g or more. When the pigment, grinding agent, and binder satisfy the above conditions, the pigment can be further refined while maintaining high productivity without increasing the viscosity of the mixture. The inventors of the present invention speculate that this mechanism is as follows. When the pigment has acidic functional groups, an acid-base interaction occurs between the pigment and resin A having basic functional groups contained in the binder, and resin A is adsorbed to the pigment, causing the pigment to behave as if it has a basic group. Here, when the grinding agent has basic functional groups, a repulsive force is generated between the pigment and the grinding agent due to the base-base repulsion action with the pigment behaving as if it has a basic group, and the pigment to which resin A is adsorbed slides on the surface of the grinding agent, reducing the viscosity. Therefore, even if a binder with a high viscosity is used to further refine the pigment, it is believed that the above-mentioned effect makes it possible to further refine the pigment without increasing the viscosity, i.e., without reducing productivity.
[0012] If the pigment does not have 5 μmol / g or more of acidic functional groups on its surface, the acid-base interaction between the pigment and resin A will not work sufficiently, and the effects of the present invention will not be obtained. Furthermore, if the grinding agent does not have 5 μmol / g or more of basic functional groups on its surface, the base-base repulsion between the grinding agent and the pigment will not work sufficiently, and the effects of the present invention will not be obtained. Furthermore, if the binder does not contain resin A having 5 μmol / g or more of basic functional groups on its surface, the pigment to which resin A is adsorbed will no longer behave as if it has basic groups, and the effects of the present invention will not be obtained.
[0013] The methods for measuring the acidic functional groups of the pigment of the present invention, the basic functional groups of the grinding agent, and the basic functional groups of Resin A will be described later.
[0014] The mass ratio of the resin A to the pigment of the present invention is 0.01 or more and 0.30 or less. When the mass ratio of the resin A to the pigment is less than 0.01, the amount of the resin A adsorbed to the pigment is small, and even if the resin A is adsorbed to the pigment, the pigment does not behave as if it has a basic group. As a result, the base-base repulsion between the pigment adsorbed by the resin A and the grinding agent is hardly generated, and the effect of the present invention cannot be obtained. In addition, when the mass ratio of the resin A to the pigment is greater than 0.30, the resin A is present in excess, and the amount of basic resin A that is not adsorbed to the pigment increases. Therefore, the base-base repulsion acting between the pigment adsorbed by the resin A and the grinding agent is weakened, and the effect of the present invention cannot be obtained.
[0015] In the method for producing the pigment dispersion of the present invention, for example, a batch type kneader such as a kneader, a pressure kneader, or a Banbury mixer, or a continuous type kneader can be used. Among these, a twin-screw kneading extruder is preferred from the viewpoints of fineness of the pigment and productivity.
[0016] From the viewpoint of coloring power, the toner particles of the present invention are preferably produced by at least one of the following methods (i) to (iv), and more preferably by method (i). (i) A method in which a pigment dispersion and a resin are melt-kneaded, and the resulting kneaded product is pulverized to obtain toner particles. (ii) A method in which a pigment dispersion and a resin are dissolved in an organic solvent, the resulting resin solution is dispersed in an aqueous medium, granulated, and the solvent is removed to obtain toner particles. (iii) A method in which a pigment dispersion and a polymerizable monomer are mixed, the resulting polymerizable monomer composition is dispersed in an aqueous medium, granulated, and the polymerizable monomer is polymerized to obtain toner particles. (iv) A method of obtaining toner particles through a step of mixing a dispersion liquid containing fine particles of a pigment dispersion with a dispersion liquid containing fine particles containing a resin, aggregating the fine particles of the pigment dispersion and the fine particles containing the resin to form aggregate particles, and heating and fusing the aggregate particles.
[0017] <Method of manufacturing pigment dispersion> Next, the procedure of the method for producing the pigment dispersion of the present invention will be described, but the method is not limited thereto, and the details are not particularly important as long as a heating mechanism is provided, the pigment is disintegrated, and a pigment dispersion can be obtained by the method. In the method for producing a pigment dispersion, it is desirable to uniformly mix the raw materials including the pigment, grinding agent, and binder, and then perform kneading. First, the raw material mixing process will be described as a process for uniformly mixing the raw materials. In the raw material mixing process, at least the pigment, grinding agent, resin A, and binder components other than resin A are weighed out in predetermined amounts as the raw materials for the pigment dispersion, and then mixed. Examples of mixing devices include a double con mixer, a V-type mixer, a drum mixer, a super mixer, a Henschel mixer, and a Nauta mixer. Furthermore, the pigment dispersion raw materials blended and mixed as described above are fed into a melt kneader and melt kneaded at a desired temperature, whereby the pigment is disintegrated by the grinding agent in the shear field within the melt kneader to obtain a pigment dispersion. At this time, an acid-base interaction occurs between the pigment and resin A, causing the pigment and the grinding agent to associate with each other. As described above, for example, a batch type kneader such as a kneader, pressure kneader, or Banbury mixer, or a continuous type kneader can be used in the melt kneading step.
[0018] <Raw materials for pigment dispersions> Next, the raw materials for the pigment dispersion containing at least the pigment, the grinding agent, and the binder containing the resin A used in the present invention will be described.
[0019] (Pigments) The pigment that can be contained in the pigment dispersion may have acidic functional groups on its surface in an amount of 5 μmol / g or more, and examples thereof include the following. Examples of the pigment include known organic pigments and carbon black. Examples of cyan pigments include copper phthalocyanine compounds and derivatives thereof, anthraquinone compounds, and basic dye lake compounds. Examples of magenta pigments include condensed azo compounds, diketopyrrolopyrrole compounds, anthraquinone compounds, quinacridone compounds, basic dye lake compounds, naphthol compounds, benzimidazolone compounds, thioindigo compounds, and perylene compounds. Examples of yellow pigments include condensed azo compounds, isoindolinone compounds, anthraquinone compounds, azo metal complexes, methine compounds, and allylamide compounds. Examples of black colorants include carbon black, or colorants toned to black using yellow pigments, magenta pigments, and cyan pigments. Examples of acidic functional groups include sulfonic groups, carboxyl groups, etc. These may be originally present on the surface of the pigment, or may be introduced by surface treatment of a general pigment. The pigments may be used alone or in combination of two or more. It is preferable that the number average particle diameter of the pigment before kneading is 80 nm to 150 nm, and that the number average particle diameter of the pigment disintegrated in the pigment dispersion in the pigment disintegration step is 60 nm to 80 nm, because this improves coloring power. The number average particle diameter of the pigment is measured by the method described below.
[0020] (grinding agent) The grinding agent that can be contained in the pigment dispersion is any agent having basic functional groups on its surface in an amount of 5 μmol / g or more, and examples of such agents include known resin particles, inorganic salts, inorganic oxides, and minerals. The resin particles include acrylic resin particles. Examples of inorganic salts include particles of chlorides (such as sodium chloride); carbonates (such as calcium carbonate); sulfates (such as barium sulfate), and titanates (such as strontium titanate). Examples of inorganic oxides include particles of silica, alumina, and titania. Minerals include kaolinite and talc. Here, the grinding agent of the present invention is preferably an inorganic fine particle since it can further refine the pigment, and calcium carbonate, kaolin clay, talc, or barium sulfate is more preferable since their refractive indices are close to those of the resin. If the refractive indices of the grinding agent and the resin are close to each other, light scattering at the interface between the grinding agent and the resin can be suppressed, and as a result, the saturation of the pigment dispersion is increased. The basic functional group may be an amino group, etc. The basic functional group may be originally present on the surface of the grinding agent, or may be introduced by a general surface treatment. From the viewpoint of fine pigment production, the number-average particle size of the grinding agent of the present invention is preferably 0.1 μm or more and 20 μm or less. The number-average particle size of the grinding agent is measured by the method described below.
[0021] (Resin A) The resin A contained in the binder that can be contained in the pigment dispersion may have basic functional groups on its surface in an amount of 5 μmol / g or more, and examples thereof include the following. Examples of the amorphous resin include polyesters having 5 μmol / g or more of basic functional groups on their surface, styrene-acrylic acid copolymers, polyolefin resins, vinyl resins, fluororesins, phenolic resins, silicone resins, epoxy resins, polyamines, and hybrid resins thereof. Examples of the crystalline resin include polyesters, polyamides, polyimides, polyolefins, polyethylenes, polybutylenes, polyisobutyrates, polyvinyls, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, polypropylenes, and mixtures thereof, each of which has a basic functional group on its surface at 5 μmol / g or more. Among these, polyesters are preferred. Examples of the basic functional group include amino groups. The basic functional group may be introduced by modifying the resin during synthesis, or may be introduced into the resin by a polymer reaction.
[0022] (Binding agent components other than resin A) There is no particular restriction on the binder component other than the resin A that can be contained in the pigment dispersion as long as it has little effect on the color and charge retention of the toner. Among them, it is preferable that it is a material that constitutes the toner, and examples thereof include amorphous resins and crystalline resins that are toner binder resins, thermoplastic elastomers, and low-molecular-weight crystalline compounds that are release agents used to suppress hot offset during fixing and plasticizers used to improve low-temperature fixing properties.
[0023] The amorphous resin is not particularly limited as long as it is a general resin used in toners, and examples thereof include polyester, styrene-acrylic acid copolymer, polyolefin-based resin, vinyl-based resin, fluororesin, phenolic resin, silicone resin, epoxy resin, hybrid resin thereof, etc. Among these, it is preferable to use polyester, styrene-acrylic acid copolymer, and hybrid resin thereof, which have good charge retention and low-temperature fixing properties.
[0024] The crystalline resin is not particularly limited as long as it is a general resin used in toners, and examples of the crystalline resin include polyester, polyamide, polyimide, polyolefin, polyethylene, polybutylene, polyisobutyrate, polyvinyl, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, polypropylene, and mixtures thereof. Among these, polyester, which has good low-temperature fixing properties, is preferable.
[0025] The amorphous resins and crystalline resins as binder components other than resin A do not have basic functional groups, or even if they have basic functional groups, the content of the basic functional groups on the surface is less than 5 μmol / g.
[0026] The thermoplastic elastomer is not particularly limited as long as it is a general resin used in toner, and may be a thermoplastic elastomer such as a polystyrene-based thermoplastic elastomer, a polyolefin-based thermoplastic elastomer, a vinyl chloride-based thermoplastic elastomer, a polybutadiene-based thermoplastic elastomer, a polyurethane-based thermoplastic elastomer, a polyester-based thermoplastic elastomer, etc. From the viewpoint of controlling the melting point of the crystalline portion, a polyurethane-based thermoplastic elastomer or a polyester-based thermoplastic elastomer is preferred.
[0027] The low molecular weight crystalline compound may be any material generally used in toners. In particular, hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, alkylene copolymers, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax used as release agents, oxides of hydrocarbon waxes such as oxidized polyethylene wax or block copolymers thereof, waxes mainly composed of fatty acid esters such as carnauba wax, and partially or completely deoxidized fatty acid esters such as deoxidized carnauba wax are more preferred.
[0028] Similarly, crystalline long-chain alkyl carboxylic acids such as stearic acid and behenic acid, and crystalline long-chain alkyl alcohols such as 1-docosanol and 1-octacosanol are more preferred.
[0029] <Toner raw materials> Next, the binder resin and other raw materials used in the toner of the present invention will be described.
[0030] (Binding resin) As the binder resin used in the toner for electrophotographic image formation, a general resin can be used, and examples thereof include polyester, styrene-acrylic acid copolymer, polyolefin resin, vinyl resin, fluororesin, phenol resin, silicone resin, epoxy resin, etc. Among these, from the viewpoint of improving low-temperature fixing property, amorphous polyester is used, and from the viewpoint of achieving both low-temperature fixing property and hot offset resistance, it is known to use a low-molecular-weight polyester having a weight-average molecular weight of about 1000 to 10,000 in combination with a high-molecular-weight polyester having a weight-average molecular weight of about 10,000 to 100,000.
[0031] (Release agent) If necessary, a release agent that suppresses the occurrence of hot offset during the heat fixing of the toner may be used. Typical examples of such release agents include low molecular weight polyolefins, silicone wax, fatty acid amides, ester waxes, carnauba wax, and hydrocarbon waxes.
[0032] <Toner manufacturing method> The toner can be produced by using the pigment dispersion obtained in the pigment crushing process, for example, by a kneading and pulverizing method, a dissolution suspension method, a suspension polymerization method, or an emulsion aggregation method. The toner can be produced by any one of the methods alone or by a combination of the methods. For example, a method can be used in which a shell is formed on toner particles obtained by the kneading and pulverizing method or the dissolution suspension method, for example, by an emulsion aggregation method.
[0033] Specific examples of the toner production method, including the kneading and pulverizing method, the dissolution suspension method, the suspension polymerization method, and the emulsion aggregation method, will be described below, but the method is not limited to these. <Kneading and grinding method> In the kneading and pulverizing method, first, the pigment dispersion and binder resin, which are the constituent materials of the toner, as well as the release agent, colorant, and other additives added as necessary, are thoroughly mixed and melt-kneaded using a known heat kneader such as a heated roll or kneader (kneading step).Then, the mixture is mechanically pulverized to a desired toner particle size (pulverizing step), and classified to a desired particle size distribution (classification step) to produce a toner.
[0034] (Kneading process) The melt-kneading of the toner constituent materials can be carried out using a known heat kneading machine such as a heating roll, a kneader, etc. It is preferable that the toner constituent materials are sufficiently mixed in advance using a mixer before the kneading step. Examples of mixers include Henschel mixer (manufactured by Mitsui Mining Co., Ltd.); Super mixer (manufactured by Kawata Co., Ltd.); Ribocone (manufactured by Okawara Manufacturing Co., Ltd.); Nauta mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation); Spiral pin mixer (manufactured by Pacific Machinery Co., Ltd.); and Loedige mixer (manufactured by Matsubo Co., Ltd.). Examples of thermal kneaders include the KRC kneader (manufactured by Kurimoto Iron Works); the Buss-Co kneader (manufactured by Buss); the TEM type extruder (manufactured by Toshiba Machine Co., Ltd.); the TEX twin-screw kneader (manufactured by Japan Steel Works); the PCM kneader (manufactured by Ikegai Iron Works); the three-roll mill, mixing roll mill, kneader (manufactured by Inoue Seisakusho Co., Ltd.); the Kneadex (manufactured by Mitsui Mining Co., Ltd.); the MS-type pressure kneader, Niderruder (manufactured by Moriyama Seisakusho Co., Ltd.); and the Banbury mixer (manufactured by Kobe Steel, Ltd.).
[0035] (Crushing process) The pulverization step is a step in which the kneaded product obtained in the kneading step is cooled until it reaches a pulverizable hardness, and then mechanically pulverized to a desired toner particle size by a known pulverizer such as a collision plate jet mill, a fluidized bed jet mill, or a rotary mechanical mill. From the viewpoint of pulverization efficiency, it is desirable to use a fluidized bed jet mill as the pulverizer. Examples of grinding machines include counter jet mills, micron jets, and innomizers (manufactured by Hosokawa Micron Corporation); IDS type mills, PJM jet grinders (manufactured by Japan Pneumatic Mfg. Co., Ltd.); cross jet mills (manufactured by Kurimoto Iron Works); Urmax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Kogyo Co., Ltd.); and Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).
[0036] (Classification process) The classification step is a step in which the pulverized product obtained in the pulverization step is classified to obtain a toner having a desired particle size distribution. As a classifier used for classification, known devices such as a wind classifier, an inertial classifier, and a sieve classifier can be used.Specific examples include Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turbo Flex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).
[0037] To the toner produced through the above steps, inorganic fine particles such as silica, alumina, titania, calcium carbonate, etc., and resin fine particles such as vinyl resin, polyester, silicone resin, etc., may be added by applying a shear force in a dry state, as necessary. These inorganic fine particles and resin fine particles function as external additives such as a flow aid or cleaning aid.
[0038] <Dissolution suspension method> The solution suspension method is a method in which a pigment dispersion, a resin component, and, if necessary, a release agent and the like are dissolved or dispersed in an organic solvent, the resulting solution or dispersion is dispersed in a poor solvent such as water to a size approximately equal to that of toner particles, and the organic solvent is distilled off in this state to produce toner particles. In the solution suspension method, the toner is manufactured through a resin dissolving step, a granulating step, a solvent removing step, and a washing and drying step.
[0039] (Resin melting process) The resin dissolving step is, for example, a step of preparing a resin composition by heating and dissolving a pigment dispersion and a styrene-acrylic acid copolymer as a resin in an organic solvent. If necessary, other resins, plasticizers, colorants, release agents, etc. may be dissolved or dispersed. In addition, a pigment dispersant or a release agent dispersant may be added during dispersion. The organic solvent used may be any solvent that dissolves the binder and resin in the pigment dispersion, and specific examples include toluene and xylene. The amount of the organic solvent used is not limited, but may be an amount that provides a viscosity that allows the resin composition to be dispersed and granulated in an aqueous medium. Specifically, from the viewpoint of granulation properties and toner production efficiency, it is preferable that the mass ratio of the resin composition containing the pigment dispersion, styrene-acrylic acid copolymer, and other resins, plasticizers, colorants, etc., as necessary, to the organic solvent is 10 / 90 to 50 / 50. On the other hand, the pigment and grinding agent in the pigment dispersion, and the colorant and release agent added as necessary, do not need to be dissolved in an organic solvent and may be dispersed. When the colorant and release agent are used in a dispersed state, they are preferably dispersed using a dispersing machine such as a bead mill.
[0040] (granulation process) The granulation process is a process in which the resin composition obtained in the resin dissolving process is dispersed in an aqueous medium using a dispersant to a predetermined toner particle size, to prepare a dispersion (granulated material). The aqueous medium is mainly water. The aqueous medium preferably contains 1% by mass or more and 30% by mass or less of a monovalent metal salt. By containing the monovalent metal salt, the organic solvent in the resin composition is prevented from diffusing into the aqueous medium, and the particle size distribution of the toner is easily improved. Examples of monovalent metal salts include sodium chloride, potassium chloride, lithium chloride, and potassium bromide, and among these, sodium chloride and potassium chloride are preferred. The mixing ratio (mass ratio) of the aqueous medium to the resin composition is preferably 90 / 10 to 50 / 50 (aqueous medium / resin composition).
[0041] The dispersant is not particularly limited, but cationic, anionic and nonionic surfactants are used as organic dispersants, and anionic surfactants are preferred. Examples of the dispersant include sodium alkylbenzenesulfonate, sodium α-olefinsulfonate, sodium alkylsulfonate, sodium alkyldiphenyletherdisulfonate, etc. On the other hand, inorganic dispersants include tricalcium phosphate, hydroxyapatite, calcium carbonate, titanium oxide and silica powder. Among these, the inorganic dispersant tricalcium phosphate is preferred because of its granulation properties and stability, and because it has an extremely small adverse effect on the properties of the toner obtained. The amount of dispersant added is determined according to the particle size of the granulated material, and the particle size becomes smaller as the amount of dispersant added increases. Therefore, the amount of dispersant added varies depending on the desired particle size, but is preferably 0.1 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the resin composition. If it is 0.1 parts by mass or more, coarse powder is unlikely to be generated, and if it is 15% by mass or less, unnecessary fine particles are unlikely to be generated.
[0042] In addition, when preparing a dispersion of the resin composition in an aqueous medium, it is preferable to carry out the preparation under high speed shearing. The dispersion of the resin composition dispersed in the aqueous medium is preferably granulated to a volume average particle size of 10 μm or less, more preferably about 4 to 9 μm. Examples of devices that can impart high-speed shear include various high-speed dispersers and ultrasonic dispersers. On the other hand, the volume average particle size of the dispersion can be measured using a particle size distribution analyzer (product name: Coulter Multisizer III, manufactured by Beckman Coulter) using the Coulter method.
[0043] (Solvent removal process) The desolvation step is a step of removing the organic solvent from the dispersion obtained in the granulation step. The organic solvent is preferably removed while stirring the dispersion. The removal rate of the organic solvent can also be controlled by heating or reducing pressure as necessary.
[0044] (Washing and drying process) After the solvent removal step, a washing and drying step may be carried out in which the dispersion is washed multiple times with water or the like, and then filtered and dried. When a dispersant that dissolves under acidic conditions, such as tricalcium phosphate, is used as the dispersant, it is preferable to wash with water after washing with hydrochloric acid or the like. By performing washing, the dispersant used for granulation can be removed, and the toner properties can be improved. After washing, the toner particles can be obtained by filtering and drying. The obtained toner particles may be used as a toner as they are. Alternatively, a toner may be obtained by adding inorganic fine particles such as silica, alumina, titania, calcium carbonate, or resin particles such as vinyl resin, polyester, or silicone resin to the toner particles as necessary by applying a shear force in a dry state. These inorganic fine particles and resin particles function as external additives such as a charging aid, a flow aid, and a cleaning aid.
[0045] <Suspension polymerization method> First, the pigment dispersion and other necessary components (e.g., release agent, crosslinking agent, charge control agent, chain transfer agent, plasticizer, pigment dispersant, release agent dispersant) are dissolved or dispersed in the polymerizable monomer to prepare a polymerizable monomer composition. In the preparation, a dispersing machine such as a homogenizer, a ball mill, a colloid mill, or an ultrasonic dispersing machine can be used. Next, the polymerizable monomer composition is put into an aqueous medium containing a dispersion stabilizer prepared in advance, and suspended using a high-speed dispersing machine such as a high-speed stirrer or an ultrasonic dispersing machine to perform granulation. The polymerization initiator may be mixed with other additives when preparing the polymerizable monomer composition, or may be mixed into the polymerizable monomer composition immediately before suspending it in the aqueous medium. In addition, the polymerization initiator may be added in a state dissolved in the polymerizable monomer or another solvent, as necessary, during or after the granulation is completed, i.e., immediately before starting the polymerization reaction. Thereafter, the suspension is heated, and a polymerization reaction is carried out while stirring so that the droplet particles of the polymerizable monomer composition in the suspension maintain a particle state and do not float or settle, thereby forming toner particles. Thereafter, the suspension is cooled, washed as necessary, and dried and classified by various methods to obtain toner particles. The obtained toner particles may be used as a toner as they are. Alternatively, a toner may be obtained by adding inorganic fine particles such as silica, alumina, titania, and calcium carbonate, or resin particles such as vinyl resin, polyester resin, and silicone resin to the toner particles as necessary by applying a shear force in a dry state. These inorganic fine particles and resin particles function as external additives such as charging assistants, flow assistants, and cleaning assistants.
[0046] <Emulsification aggregation method> The emulsion aggregation method is a manufacturing method in which a dispersion of fine resin particles having a particle size sufficiently small relative to the target particle size is prepared in advance, and the fine resin particles are aggregated in an aqueous medium to produce toner particles. In the emulsion aggregation method, a toner is produced through a process of preparing a resin fine particle dispersion, an aggregation process, a fusion process, a cooling process, a washing process, and a drying process. A specific method for producing a toner using the emulsion aggregation method will be described below, but the method is not limited thereto.
[0047] (Preparation process of resin particle dispersion) In the emulsion aggregation method, resin fine particles are first prepared. The resin fine particles can be produced by a known method, but are preferably produced by the following method. First, a resin is dissolved in an organic solvent to form a uniform solution. An example of the resin is polyester. Then, a basic compound and a surfactant are added as necessary. Furthermore, an aqueous medium is added to the solution to form fine particles. Then, the solvent is removed to obtain a resin fine particle dispersion in which the resin fine particles are dispersed. More specifically, the resin is dissolved in an organic solvent by heating, and a surfactant or a base is added as necessary. Then, the aqueous medium is slowly added while applying shear with a homogenizer or the like, or after adding the aqueous medium, shear with a homogenizer or the like to form resin microparticles. Then, the solvent is removed by heating or decompression to prepare a resin microparticle dispersion.
[0048] The concentration of the resin when dissolved in the organic solvent is preferably 10% by mass or more and 50% by mass or less, more preferably 30% by mass or more and 50% by mass or less. Any organic solvent can be used as long as it can dissolve the polyester, but a solvent that has high solubility for the resin, such as toluene, xylene, or tetrahydrofuran, is preferred. The surfactant is not particularly limited, and examples thereof include anionic surfactants such as sulfate salts, sulfonates, carboxylates, phosphates, and soaps, cationic surfactants such as amine salts and quaternary ammonium salts, and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. Examples of the base include inorganic bases such as sodium hydroxide and potassium hydroxide, and organic bases such as triethylamine, trimethylamine, dimethylaminoethanol, diethylaminoethanol, etc. The base may be used alone or in combination of two or more kinds. The volume-based median diameter of the resin fine particles is preferably 0.05 μm or more and 1.0 μm or less, more preferably 0.1 μm or more and 0.6 μm or less. When the median diameter is within the above range, toner particles having a desired particle size are easily obtained. The volume-based median diameter can be measured using a dynamic light scattering particle size distribution meter (product name: Nanotrac UPA-EX150, manufactured by Nikkiso).
[0049] It is also preferable to prepare a dispersion of the pigment dispersion. As the dispersion of the pigment dispersion, a fine particle dispersion consisting of a resin and a pigment dispersion may be prepared, or a fine particle dispersion (emulsion) consisting of the pigment dispersion alone may be prepared. When preparing a fine particle dispersion by mixing a resin and a pigment dispersion, the fine particle dispersion consisting of the resin and the pigment dispersion is obtained by adding the pigment dispersion when dissolving the resin in an organic solvent in preparing the resin fine particle dispersion. When preparing a fine particle dispersion (emulsion) alone, the pigment dispersion, a surfactant, and an aqueous medium are mixed, and then heated to a temperature at which the binder in the pigment dispersion melts, and shear is applied by a homogenizer or the like, and then cooled, to obtain a dispersion of the pigment dispersion in which the pigment dispersion is dispersed in the aqueous medium.
[0050] (Agglutination process) The aggregation step is a step of preparing a mixed liquid by mixing a microparticle dispersion liquid consisting of a resin and a pigment dispersion, or a dispersion liquid of a resin microparticle dispersion and a pigment dispersion with a release agent microparticle dispersion liquid as necessary, and aggregating the particles contained in the mixed liquid to form aggregate particles. Suitable examples of the method for forming aggregate particles include a method of adding and mixing an aggregating agent into the mixed liquid, raising the temperature, appropriately applying mechanical power, etc. The above-mentioned release agent microparticle dispersion is prepared by dispersing the above-mentioned release agent. The release agent microparticles are dispersed by a known method, for example, by mixing the release agent with an aqueous medium, heating the mixture to a temperature at which the release agent melts, shearing the mixture using a media-type dispersing machine such as a rotary shearing homogenizer, a ball mill, a sand mill, or an attritor, or a high-pressure counter-collision type dispersing machine, and then cooling the mixture to obtain a release agent dispersion in an aqueous medium. In addition, a surfactant or a polymer dispersing agent that provides dispersion stability can be added as necessary.
[0051] Examples of the flocculant used in the flocculation step include metal salts of monovalent metals such as sodium and potassium, metal salts of divalent metals such as calcium and magnesium, metal salts of trivalent metals such as iron and aluminum, and polyvalent metal salts such as polyaluminum chloride. From the viewpoint of particle size controllability in the flocculation step, divalent metal salts such as calcium chloride and magnesium sulfate are preferred. The addition and mixing of the flocculant is preferably carried out in the temperature range of room temperature (25° C.) to 75° C. When mixing is carried out under these temperature conditions, flocculation proceeds in a stable state. Mixing can be carried out using a known mixing device, homogenizer, mixer, etc. The average particle size of the aggregate particles formed in the aggregation process is not particularly limited, but it is usually preferable to control the volume average particle size to 4.0 μm or more and 7.0 μm or less so that it is approximately the same as the average particle size of the toner particles to be obtained. The control can be easily performed, for example, by appropriately setting and changing the temperature during addition and mixing of the aggregating agent and the like and the stirring and mixing conditions. The particle size distribution of the aggregate particles can be measured using a particle size distribution analyzer (product name: Coulter Multisizer III, manufactured by Beckman Coulter, Inc.) using the Coulter method.
[0052] (fusion process) The fusion process is a process in which aggregate particles are heated to a temperature equal to or higher than the glass transition temperature of the resin to fuse them, thereby producing particles with a smooth surface. Prior to the primary fusion process, a chelating agent, a pH adjuster, a surfactant, etc. can be appropriately added to prevent fusion between particles. Examples of chelating agents include ethylenediaminetetraacetic acid (EDTA) and its alkali metal salts such as the Na salt, sodium gluconate, sodium tartrate, potassium and sodium citrate, nitrilotriacetate (NTA) salts, and many water-soluble polymers containing both COOH and OH functionality (polyelectrolytes). The heating temperature should be equal to or higher than the glass transition temperature of the resin contained in the aggregate, and lower than the temperature at which the resin thermally decomposes. The heating / fusion time is shorter if the heating temperature is high, and longer if the heating temperature is low. In other words, the heating / fusion time depends on the heating temperature and cannot be generally specified, but is generally between 10 minutes and 10 hours.
[0053] (cooling process) The cooling step is a step of cooling the temperature of the aqueous medium containing the particles obtained in the fusion step to a temperature lower than the glass transition temperature of the resin. By cooling to a temperature lower than the glass transition temperature, the generation of coarse particles can be suppressed. The specific cooling rate is 0.1 to 50°C / min.
[0054] (Cleaning process) The particles produced through the above steps can be washed, filtered, and then repeatedly washed to remove impurities from the particles. Specifically, it is preferable to wash the particles using an aqueous solution containing a chelating agent such as ethylenediaminetetraacetic acid (EDTA) and its Na salt, and then further wash the particles with ion-exchanged water. By repeatedly filtering the particles with ion-exchanged water multiple times, metal salts, surfactants, and the like can be removed from the toner particles. The number of filtrations is preferably 3 to 20 times from the viewpoint of production efficiency, and more preferably 3 to 10 times.
[0055] (drying process) The particles obtained in the above process are dried to obtain toner particles. The obtained toner particles may be used as a toner as is. If necessary, an external additive may be added to the toner. Examples of the external additive include inorganic particles such as silica, alumina, titania, and calcium carbonate, and resin particles such as vinyl resin, polyester resin, and silicone resin. These can be added by applying a shear force in a dry state. These inorganic particles and resin particles function as external additives such as a flowability aid and a cleaning aid.
[0056] The methods for measuring various physical properties of the toner and raw materials are described below. <Measurement of the amount of acidic groups on the pigment surface> Pigment (2 g) is added to 1 / 100 N potassium hydroxide-ethanol solution (100 ml). Next, the supernatant is subjected to potentiometric titration with 1 / 100 N hydrochloric acid-ethanol solution using an automatic potentiometric titrator (product name: AT-510, manufactured by Kyoto Electronics Manufacturing Co., Ltd.), and the amount of surface acidic groups on the pigment is calculated from the difference between the amount of hydrochloric acid required for neutralization and the amount of potassium hydroxide initially present.
[0057] <Measurement of the amount of surface basic groups on the grinding agent> The grinding agent (2 g) is added to a 1 / 100 N aqueous solution of acetic acid (100 ml). Next, the supernatant is subjected to potentiometric titration with a 1 / 100 N potassium hydroxide-ethanol solution using an automatic potentiometric titrator (product name: AT-510, manufactured by Kyoto Electronics Manufacturing Co., Ltd.), and the amount of surface basic groups on the grinding agent is calculated from the difference between the amount of potassium hydroxide required for neutralization and the amount of acetic acid initially present.
[0058] <Measurement of the amount of surface basic groups on resin A> Resin A (2 g) is added to a 1 / 100 N hydrochloric acid-ethanol solution (100 ml). Next, the supernatant is subjected to potentiometric titration with a 1 / 100 N potassium hydroxide-ethanol solution using an automatic potentiometric titrator (product name: AT-510, manufactured by Kyoto Electronics Manufacturing Co., Ltd.), and the amount of basic groups in Resin A is calculated from the difference between the amount of potassium hydroxide required for neutralization and the amount of hydrochloric acid initially present. In the present invention, the acidic functional groups of the pigment are more acidic than potassium hydroxide, the basic functional groups of the grinding agent are more basic than acetic acid, and the basic functional groups of the resin are more basic than hydrochloric acid, as determined by the back titration method described above.
[0059] <Measurement of number-average particle size of pigments and grinding agents> The number average particle size of the primary particles of the pigment and the grinding agent is measured using a transmission electron microscope (TEM) (trade name: JEM2800, manufactured by JEOL Ltd.). First, a measurement sample is prepared. 1 ml of ion-exchanged water containing a dispersible surfactant is added to approximately 5 mg of pigment or grinding agent, and the mixture is dispersed for 5 minutes using an ultrasonic disperser (ultrasonic cleaner). Next, a drop of the above dispersion liquid is placed on a microgrid (150 mesh) with a support membrane for TEM, and the mixture is dried to prepare a measurement sample. Next, images are taken using a transmission electron microscope (TEM) at an accelerating voltage of 200 kV at a magnification (e.g., 20k to 100k) that allows the pigment or grinding agent in the field of view to be measured sufficiently, and the particle size of 100 randomly selected primary particles of the pigment or grinding agent is measured to determine the number-average particle size. The particle size of the primary particles may be measured manually or using a measuring tool.
[0060] In order to measure the number average particle diameter of the pigment contained in the pigment dispersion after the pigment crushing step, it is necessary to extract the pigment from the pigment dispersion. As an example, a method for measuring the number average particle diameter of the pigment is shown below. In order to dissolve the binder in the pigment dispersion with a solvent, a solvent is selected according to the type of binder, and the binder is melted using a swing roll mixer or the like. For example, if the binder is an amorphous polyester resin, tetrahydrofuran or methyl ethyl ketone can be used. Thereafter, the binder is separated from the pigment dispersion by filtration and washing, and a mixture of the pigment and grinding agent is extracted. The extracted mixture of the pigment and grinding agent is observed in the same manner as above, and only the pigment is extracted based on the shape of the pigment and grinding agent, and the number-average particle size is measured manually or with a measuring tool.
[0061] <Measurement of resin glass transition temperature (Tg)> The glass transition temperature of the resin is measured in accordance with ASTM D3418-82 using a differential scanning calorimeter (product name: Q2000, manufactured by TA Instruments). The melting points of indium and zinc are used for temperature correction of the detector of the device, and the heat of fusion of indium is used for heat correction. Specifically, about 5 mg of the resin is precisely weighed and placed in an aluminum pan, and an empty aluminum pan is used as a reference, and the measurement is performed at a temperature rise rate of 10°C / min in the measurement range of 30°C to 180°C. The temperature is raised to 180°C once and held for 10 minutes, then cooled to 30°C, and then raised again. During this second heating process, a specific heat change is obtained in the temperature range of 30°C to 100°C. The temperature at the point where a straight line equidistant in the vertical direction from a straight line extending the baseline before and after the specific heat change appears and the curve of the stepwise change part of the glass transition in the DSC curve intersect is taken as the glass transition temperature (Tg:°C) of the resin.
[0062] <Method for measuring the volume average particle size (D3) of toner particles> The volume average particle size (D3) of the toner particles is measured with an effective measurement channel count of 25,000 channels using a precision particle size distribution measuring device using the narrow hole electrical resistance method, "Coulter Counter Multisizer 3" (registered trademark, manufactured by Beckman Coulter, Inc.), equipped with a 50 μm aperture tube, and the accompanying dedicated software for setting measurement conditions and analyzing measurement data, "Beckman Coulter Multisizer 3 Version 3.51" (manufactured by Beckman Coulter, Inc.), and the measurement data is analyzed and calculated. The electrolyte solution used for the measurement is prepared by dissolving special grade sodium chloride in ion-exchanged water to a concentration of approximately 1% by mass, for example, "ISOTON II" (manufactured by Beckman Coulter).
[0063] Before performing measurements and analysis, the dedicated software is set up as follows. In the "Change Standard Measurement Method (SOM) screen" of the dedicated software, set the total count number in the control mode to 50,000 particles, the number of measurements to 1, and the Kd value to the value obtained using "Standard Particle 10.0 μm" (Beckman Coulter). Press the threshold / noise level measurement button to automatically set the threshold and noise level. In addition, set the current to 1600 μA, the gain to 2, the electrolyte to ISOTON II, and check the aperture tube flush after measurement. In the "Pulse to particle size conversion setting screen" of the dedicated software, set the bin interval to logarithmic particle size, the particle size bin to 256 particle size bins, and the particle size range to 1 μm or more and 30 μm or less.
[0064] The specific measurement method is as follows. (1) Pour about 200 ml of the electrolyte solution into a 250 ml round-bottom glass beaker made exclusively for the Multisizer 3, set it on the sample stand, and stir the stirrer rod counterclockwise at 24 revolutions per second. Then, use the "aperture flush" function of the analysis software to remove dirt and air bubbles from inside the aperture tube. (2) Pour approximately 30 ml of the electrolyte solution into a 100 ml flat-bottom glass beaker and add approximately 0.3 ml of a solution prepared by diluting "Contaminon N" (a 10% by weight aqueous solution of a neutral detergent for cleaning precision measuring instruments with a pH of 7 consisting of a nonionic surfactant, anionic surfactant, and organic builder, manufactured by Wako Pure Chemical Industries, Ltd.) three times by weight with ion-exchanged water as a dispersant. (3) A specified amount of ion-exchanged water is placed in the water tank of an ultrasonic disperser "Ultrasonic Dispension System Tetora150" (manufactured by Nikkaki Bios Co., Ltd.) with an electrical output of 120 W and equipped with two oscillators with an oscillation frequency of 50 kHz and shifted in phase by 180 degrees. Approximately 2 ml of Conaminon N is added to this water tank. (4) Set the beaker prepared in (2) above in the beaker fixing hole of the ultrasonic disperser, operate the ultrasonic disperser, and adjust the height of the beaker so that the resonance state of the electrolyte solution level in the beaker is maximized. (5) In the state where the electrolyte solution in the beaker in (4) is irradiated with ultrasonic waves, about 10 mg of toner is added little by little to the electrolyte solution and dispersed. Then, ultrasonic dispersion treatment is continued for another 60 seconds. During ultrasonic dispersion, the water temperature in the water tank is appropriately adjusted so that it is between 10°C and 40°C. (6) Using a pipette, add the electrolyte solution containing the toner dispersed therein prepared in (5) to the round-bottom beaker prepared in (1) placed in the sample stand, and adjust the measurement concentration to about 5%. Then, measurements are continued until the number of particles measured reaches 50,000. (7) The measurement data is analyzed using the dedicated software that comes with the device, and the volume average particle size (D3) is calculated. Note that when the dedicated software is set to Graph / Volume %, the "Average diameter" on the Analysis / Volume Statistics (Arithmetic Mean) screen is the volume average particle size (D3). EXAMPLES
[0065] The present invention will be specifically described below with reference to Production Examples and Examples, which are not intended to limit the present invention in any way. In the following formulations, all parts and percentages are by weight unless otherwise specified.
[0066] <Production of Pigment Dispersion 1> Pigment 35 parts (Cyan pigment: Pigment Blue 15:3, volume average particle size 102 nm, acidic functional group content: 10 μmol / g) Grinding agent 35 parts (Light calcium carbonate, number average particle size 0.4 μm, basic functional group content: 10 μmol / g) Binder other than Resin A 28 parts (Resin B: Polyester made of a polymer of polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane, isophthalic acid, and terephthalic acid in a molar ratio of 100:50:50, with a glass transition temperature (Tg) of 70°C) Resin A1 2 parts (Product name: SOLPLUS L300, manufactured by Lubrizol Japan, Basic functional group content: 10 μmol / g) The above materials were mixed in a Henschel mixer (product name: FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100°C, the mixture was kneaded at 190°C in a twin-screw kneader (product name: PCM-30, manufactured by Ikegai Corporation). The motor of the twin-screw kneader was adjusted so as to maximize the feed rate while preventing overloading. The resulting kneaded product was cooled and roughly crushed in a pin mill to a volume average particle size of 100 μm or less, to obtain a roughly crushed product of pigment dispersion A. The number average particle size of the pigment in the resulting pigment dispersion was 62 nm. The production volume per hour was 30 kg.
[0067] <Production of Pigment Dispersion 2> Styrene 75.9 parts n-Butyl acrylate 24.1 parts The above materials were placed in a four-neck flask equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen gas inlet tube, and a catalytic amount of AIBN was added. Nitrogen gas was passed through the four-neck flask and the temperature was gradually raised while stirring, and the reaction was carried out at 70°C for 12 hours to obtain a styrene-acrylic resin (resin C). A coarsely crushed pigment dispersion 2 was obtained in the same manner as in Pigment Dispersion 1, except that Resin C was used instead of Resin B. The number-average particle size of the pigment in the obtained pigment dispersion was 67 nm. The production amount per hour was 29 kg.
[0068] <Production of pigment dispersions 3 to 12 and 17> Table 1 shows the number average particle size and production volume per hour of the pigments in pigment dispersions 3 to 12 and 17 obtained by kneading the pigments, grinding agent, resin A1, and binder components other than resin A shown in Table 1 under the conditions shown in Table 1.
[0069] <Production of Pigment Dispersion 13> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane 100 copies Isophthalic acid 50 parts Terephthalic acid 50 parts Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts The above materials were weighed into a reaction vessel equipped with a condenser, stirrer, nitrogen inlet, and thermocouple. Next, the atmosphere in the flask was replaced with nitrogen gas, and the temperature was gradually raised with stirring, and the mixture was reacted at 200° C. for 4 hours with stirring. The pressure inside the reaction vessel was then reduced to 7 kPa and maintained for 1 hour, after which the vessel was cooled to 180° C. and returned to atmospheric pressure. Next, the pressure in the reaction vessel was gradually released to return to normal pressure, after which hexamethylene diisocyanate (8 parts) was added and reacted at 100° C. under normal pressure for 3 hours. Thereafter, tert-butylcatechol (0.1 part) was added, the pressure in the reaction vessel was reduced to 7 kPa, and the reaction was carried out for 1 hour while maintaining the temperature at 180° C., yielding Resin A2, a polyester having a glass transition temperature (Tg) of 76° C. The basic functional group content of Resin A2 was 5 μmol / g. A coarsely crushed pigment dispersion 13 was obtained in the same manner as in Pigment Dispersion 1, except that Resin A2 was used instead of Resin A1. The number-average particle size of the pigment in the obtained pigment dispersion was 77 nm. The production rate per hour was 15 kg.
[0070] <Production of Pigment Dispersion 14> 100 parts of fumed silica (silica base: spherical) was gradually added to a solution of 10 parts of 90% methanol water and 10 parts of hexamethylenedisilazane dissolved in 10,000 parts of hexane to cause a reaction, and the solvent and by-products were removed to obtain silica particles I. The removal time of the solvent and by-products was adjusted so that the pH value became 11.0. The number average particle size of the primary particles of the obtained silica particles I was 0.4 μm, and the basic functional group content was 5 μmol / g. A coarsely ground product of Pigment Dispersion 14 was obtained in the same manner as Pigment Dispersion 1, except that Silica Particles I was used as the grinding agent. The number-average particle size of the pigment in the obtained pigment dispersion was 79 nm. The production rate per hour was 16 kg.
[0071] <Production of Pigment Dispersion 15> A coarsely ground pigment dispersion 15 was obtained in the same manner as in Pigment Dispersion 1, except that the pigment was a rosin-treated pigment (cyan pigment: Pigment Blue 15:3, volume average particle size 102 nm, acidic functional group content: 5 μmol / g). The number average particle size of the pigment in the obtained pigment dispersion was 78 nm. The production rate per hour was 16 kg.
[0072] <Production of Pigment Dispersion 16> A coarsely crushed product of Pigment Dispersion 16 was obtained in the same manner as Pigment Dispersion 1, except that Resin A was not used. The number-average particle size of the pigment in the obtained pigment dispersion was 82 nm. The production amount per hour was 7 kg.
[0073] <Production of Pigment Dispersion 18> Polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane 100 copies Isophthalic acid 50 parts Terephthalic acid 50 parts Tin 2-ethylhexanoate (esterification catalyst): 0.5 parts The above materials were weighed into a reaction vessel equipped with a condenser, stirrer, nitrogen inlet, and thermocouple. Next, the inside of the flask was replaced with nitrogen gas, and the temperature was gradually raised while stirring, and the mixture was reacted for 4 hours while stirring at a temperature of 200°C. The pressure in the reaction vessel was then lowered to 7 kPa, and after maintaining the reaction for 1 hour, the mixture was cooled to 180°C and returned to atmospheric pressure. Then, tert-butylcatechol (0.1 part) was added, the pressure in the reaction vessel was lowered to 7 kPa, and the reaction was continued for 1 hour while maintaining the temperature at 180°C, to obtain Resin D, a polyester having a glass transition temperature (Tg) of 71°C. The basic functional group content of Resin D was 0 μmol / g. A coarsely crushed pigment dispersion 18 was obtained in the same manner as in Pigment Dispersion 1, except that Resin D was used instead of Resin A1. The number-average particle size of the pigment in the obtained pigment dispersion was 84 nm. The production rate per hour was 7 kg.
[0074] <Production of Pigment Dispersion 19> 100 parts of fumed silica (silica base: spherical) was gradually added to a solution obtained by diluting 20 parts of dimethyl silicone oil (kinematic viscosity at a temperature of 25°C: 50 cSt) with 10,000 parts of hexane, and the mixture was reacted at a temperature of 130°C, after which the solvent was removed. The mixture was then crushed using a pin-type crushing device, and was reacted in a solution obtained by dissolving 10 parts of 90% methanol water and 10 parts of hexamethylenedisilazane in 10,000 parts of hexane, and the solvent and by-products were removed to obtain silica particles II. The number-average particle size of the primary particles of the obtained silica particles II was 0.4 μm, and the basic functional group content was 0 μmol / g. A coarsely ground product of Pigment Dispersion 19 was obtained in the same manner as Pigment Dispersion 1, except that Silica Particles II was used as the grinding agent. The number-average particle size of the pigment in the obtained pigment dispersion was 82 nm. The production rate per hour was 8 kg.
[0075] <Production of Pigment Dispersion 20> A coarsely ground pigment dispersion 20 was obtained in the same manner as in Pigment Dispersion 1, except that the pigment was an amine-treated pigment (cyan pigment: Pigment Blue 15:3, volume average particle size 102 nm, acidic functional group content: 3 μmol / g). The number average particle size of the pigment in the obtained pigment dispersion was 83 nm. The production amount per hour was 9 kg.
[0076] [Table 1] In Table 1, PB15:3 indicates Pigment Blue 15:3.
[0077] <Toner 1 Manufacturing Example> ·Resin B 77.7 parts (Polyester made of polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane:isophthalic acid:terephthalic acid in a molar ratio of 100:50:50, with a glass transition temperature (Tg) of 70°C) Pigment Dispersion 1 14.3 parts Synthetic Wax I 8.0 parts (Hydrocarbon wax, maximum endothermic peak temperature 90℃) The above materials were mixed in a Henschel mixer (product name: FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 After mixing for 5 minutes at 100° C., the mixture was kneaded in a twin-screw kneader (product name: PCM-30, manufactured by Ikegai Corporation). The kneaded mixture was cooled and coarsely pulverized in a pin mill to a volume average particle size of 100 μm or less to obtain a coarsely pulverized product. The coarsely pulverized product was finely pulverized in a mechanical pulverizer (product name: T-250, manufactured by Turbo Kogyo Co., Ltd.) by adjusting the rotation speed and number of passes so as to obtain the target particle size. Further, classification was performed using a rotary classifier (product name: 200TSP, manufactured by Hosokawa Micron Corporation) to obtain toner particles. The rotation speed was adjusted under the operating conditions of the rotary classifier to obtain the target particle size and particle size distribution. 100 parts of the obtained toner particles were mixed with 100 parts of toner having a specific surface area of 200 m2 measured by the BET method. 2 1.8 parts of silica fine particles that had been hydrophobized with silicone oil were added, and the mixture was mixed in a Henschel mixer (product name: FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for a rotation time of 10 minutes to obtain Toner 1. Table 2 shows the volume average particle size of Toner 1.
[0078] <Toner 2 Manufacturing Example> 60 parts of Pigment Dispersion 1, 150 parts of toluene as a solvent, and 130 parts of glass beads (diameter 1 mm) were mixed and dispersed for 3 hours using an Attritor (manufactured by Nippon Coke and Engineering Co., Ltd.) to obtain a pigment dispersion. Next, 11.7 parts of trisodium phosphate dodecahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) and 1200 parts of ion-exchanged water were added to a beaker set in a water bath to dissolve the trisodium phosphate dodecahydrate. Then, the temperature of the water bath was raised to 60°C. After reaching 60°C, an aqueous solution in which 5.15 parts of calcium chloride (manufactured by Kishida Chemical Industries, Ltd.) was dissolved in 100 parts of ion-exchanged water was added. After the addition, the mixture was stirred for 30 minutes to obtain an aqueous medium containing tricalcium phosphate. Amorphous polyester I 75.7 parts Pigment dispersion 50 parts · 10 parts synthetic wax Toluene 350 parts The above materials were mixed and heated to 80° C. with stirring to dissolve and disperse each material, thereby preparing a resin composition. Meanwhile, 600 parts of the aqueous medium containing the above-mentioned tricalcium phosphate was heated to 80°C while stirring with Clearmix (manufactured by M Technique Co., Ltd.). A resin composition was added to the aqueous medium containing tricalcium phosphate, and a dispersion was obtained by stirring for 10 minutes at 10,000 rpm using a stirring blade. The obtained dispersion was stirred for 5 hours at 80°C to remove toluene. Thereafter, the mixture was cooled to 25°C for 10 minutes to obtain an aqueous dispersion of toner particles. Dilute hydrochloric acid was added to the obtained aqueous dispersion of toner particles while stirring it. After stirring for 2 hours at pH 1.5 to dissolve tricalcium phosphate, the mixture was subjected to solid-liquid separation using a filter to obtain toner particles. The mixture was poured into water and stirred to form a dispersion again, after which solid-liquid separation was performed using a filter. This operation was repeated until the tricalcium phosphate was sufficiently removed, and the obtained toner particles were sufficiently dried using a dryer. 100 parts of the obtained toner particles were mixed with a mixture having a specific surface area of 200 m2 measured by the BET method. 2 1.8 parts of silica fine particles that had been hydrophobized with silicone oil were added, and the mixture was mixed in a Henschel mixer (product name: FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for 10 minutes to obtain Toner 2. Table 2 shows the physical properties.
[0079] <Toner 3 Manufacturing Example> Styrene 47.6 parts n-Butyl acrylate 15.1 parts Pigment Dispersion 2 14.3 parts · Synthetic Wax I 20.0 parts Amorphous polyester I 3.0 parts A mixture of the above raw materials was prepared. The mixture was placed in an attritor (manufactured by Nippon Coke Corporation) and dispersed at 200 rpm for 2 hours using zirconia beads with a diameter of 5 mm to obtain a raw material dispersion. On the other hand, 735.0 parts of ion-exchanged water and 16.0 parts of trisodium phosphate (12-hydrate) were added to a container equipped with a homomixer (manufactured by Primix Corporation) as a high-speed stirring device and a thermometer, and the temperature was raised to 60°C while stirring at 12000 rpm. An aqueous calcium chloride solution in which 9.0 parts of calcium chloride (2-hydrate) was dissolved in 65.0 parts of ion-exchanged water was added thereto, and the mixture was stirred at 12000 rpm for 30 minutes while maintaining the temperature at 60°C. 10% hydrochloric acid was added thereto to adjust the pH to 6.0, and an aqueous medium containing a dispersion stabilizer was obtained. Subsequently, the raw material dispersion liquid was transferred to a vessel equipped with a stirrer and a thermometer, and heated to 60° C. while stirring at 100 rpm. 8.0 parts of t-butyl peroxypivalate (trade name: Perbutyl PV, manufactured by NOF Corp.) was added thereto as a polymerization initiator, and after stirring at 100 rpm for 5 minutes while maintaining 60° C., it was poured into the aqueous medium being stirred at 12000 rpm. Stirring was continued for 20 minutes at 12000 rpm with a high-speed stirrer while maintaining 60° C., to obtain a granulation liquid. The granulation liquid was transferred to a reaction vessel equipped with a reflux condenser, a stirrer, a thermometer, and a nitrogen inlet tube, and heated to 70° C. while stirring at 150 rpm under a nitrogen atmosphere. A polymerization reaction was carried out at 150 rpm for 10 hours while maintaining 70° C. Thereafter, the reflux condenser was removed from the reaction vessel, and the reaction liquid was heated to 95° C., and then stirred at 150 rpm for 5 hours while maintaining 95° C., to obtain a toner particle dispersion liquid. The obtained toner particle dispersion was cooled to 20°C while stirring at 150 rpm, and then dilute hydrochloric acid was added while maintaining stirring until the pH reached 1.5 to dissolve the dispersion stabilizer. The solid content was filtered off, thoroughly washed with ion-exchanged water, and then vacuum dried at 40°C for 24 hours to obtain toner particles. 100 parts of the obtained toner particles were mixed with a 100-ml ethanol solution having a specific surface area of 200 m2 measured by the BET method. 2 1.8 parts of silica fine particles that had been hydrophobized with silicone oil were added, and the mixture was mixed in a Henschel mixer (product name: FM-75 type, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 100° C. for 10 minutes to obtain Toner 3. Table 2 shows the physical properties.
[0080] <Toner 4 Manufacturing Example> - Manufacturing of amorphous resin particles Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts Amorphous polyester I 120 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 0.6 parts The above raw materials were mixed and then stirred for 12 hours to dissolve the resin. Next, 2.7 parts of N,N-dimethylaminoethanol was added and stirred at 4000 rpm using an ultra-high speed stirrer (product name: TK Robomix, manufactured by Primix Corporation). Furthermore, 359.4 parts of ion-exchanged water was added over about 6 hours to precipitate resin particles. Then, tetrahydrofuran was removed using an evaporator to obtain a dispersion of amorphous resin particles (resin concentration 25 wt%). - Manufacturing of pigment dispersion fine particles Tetrahydrofuran (Wako Pure Chemical Industries, Ltd.) 200 parts Pigment Dispersion 1 42.9 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.5 parts The above raw materials were mixed and then stirred for 12 hours to dissolve the binder in the pigment dispersion. Next, 0.3 parts of N,N-dimethylaminoethanol and 255.6 parts of ion-exchanged water were added, and the mixture was stirred at 4000 rpm using an ultra-high speed stirring device TK Robomix (manufactured by Primix Corporation). Further, the mixture was dispersed for about 1 hour using a high-pressure impact disperser (product name: Nanomizer, manufactured by Yoshida Kikai Kogyo Co., Ltd.) After that, tetrahydrofuran was removed using an evaporator, and the pigment dispersion was dispersed in water to prepare a dispersion of pigment dispersion fine particles (pigment dispersion concentration 14.3 wt%). - Manufacturing of release agent particles Synthetic Wax I 20.0 parts Anionic surfactant (Daiichi Kogyo Seiyaku: Neogen RK) 1.0 part Ion-exchanged water 79.0 parts The above raw materials were placed in a mixing vessel equipped with an agitator, heated to 90°C, and circulated through a Clearmix W Motion (manufactured by M Technique) while being stirred at a shear mixing section with a rotor outer diameter of 3 cm and clearance of 0.3 mm at a rotor rotation speed of 19,000 rpm and a screen rotation speed of 19,000 rpm for 60 minutes for dispersion processing. After that, the rotor rotation speed was 1000 rpm, the screen rotation speed was 0 rpm, and the cooling rate was 10 °C / min. The rotor rotation speed was then cooled to 40 °C. The dispersion liquid of the release agent particles (release agent concentration 20 wt%) was obtained. obtained.
[0081] The method for producing a toner using the above-prepared dispersion of amorphous resin particles, dispersion of pigment particles, and dispersion of releasing agent particles will be exemplified below. Dispersion of amorphous resin particles 302.8 parts Pigment dispersion fine particle dispersion liquid 100 parts Dispersion of release agent particles 50 parts -Ion-exchanged water 400 parts Each of the above dispersions was charged into a round stainless steel flask and mixed, after which an aqueous solution of 2 parts of magnesium sulfate dissolved in 98 parts of ion-exchanged water was added thereto, and the mixture was dispersed at 5000 rpm for 10 minutes using a homogenizer (product name: Ultra Turrax T50, manufactured by IKA). Thereafter, while the flask was heated in a heating water bath, the mixture was heated to 58°C using a stirring blade while appropriately adjusting the rotation speed so that the mixture was stirred. The mixture was held at 58°C for 1 hour to obtain aggregated particles. An aqueous solution in which 20 parts of trisodium citrate was dissolved in 380 parts of ion-exchanged water was added to the dispersion containing the aggregated particles, and then the mixture was heated to 95°C. After holding at 95°C for 2 hours, the mixture was cooled to 25°C while continuing to stir, to obtain a toner particle dispersion.
[0082] <Production Examples of Toner 5-22> Toners 5 to 22 were obtained in the same manner as Toner 1, except that the materials and production method were changed as shown in Table 2. Table 2 shows the physical properties.
[0083] [Table 2]
[0084] <Production Example of Magnetic Core Particle 1> Step 1 (weighing and mixing): Fe2O362.7 parts MnCO329.5 parts Mg(OH)26.8 parts SrCO31.0 parts The above ferrite raw material was weighed, and was ground and mixed for 5 hours in a dry vibration mill using stainless steel beads with a diameter of 1 / 8 inch to obtain a mixture. Step 2 (Pre-firing): The resulting mixture was made into pellets of about 1 mm square using a roller compactor. The pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then fired in a burner-type firing furnace at 1000°C for 4 hours in a nitrogen atmosphere (oxygen concentration 0.01% by volume) to produce calcined ferrite. The composition of the resulting calcined ferrite was as follows: (MnO) 0.257 (MgO) 0.117 (SrO) 0,007 (Fe2O3) 0.393 Step 3 (Crushing): The obtained calcined ferrite was crushed to about 0.3 mm using a crusher. Then, 30 parts of water were added to 100 parts of the calcined ferrite using zirconia beads with a diameter of 1 / 8 inch, and the mixture was crushed for 1 hour in a wet ball mill. The obtained slurry was crushed for 4 hours in a wet ball mill using alumina beads with a diameter of 1 / 16 inch to obtain a ferrite slurry (finely crushed calcined ferrite). ·Process 4 (granulation process): To the ferrite slurry, 1.0 part of ammonium polycarboxylate as a dispersant and 2.0 parts of polyvinyl alcohol as a binder were added per 100 parts of calcined ferrite, and the mixture was granulated into spherical particles using a spray dryer (manufactured by Okawara Kakoki Co., Ltd.). After adjusting the particle size of the resulting particles, the mixture was heated at 650°C for 2 hours in a rotary kiln to remove the organic components of the dispersant and binder. Step 5 (firing): In order to control the firing atmosphere, the material was heated from room temperature to 1300°C in a nitrogen atmosphere (oxygen concentration 1.00% by volume) in an electric furnace over a period of 2 hours, and then fired at 1150°C for 4 hours. The material was then cooled to 60°C over a period of 4 hours, returned from the nitrogen atmosphere to the air, and removed at a temperature of 40°C or less. Step 6 (sorting step): After crushing the agglomerated particles, low magnetic particles were removed by magnetic separation, and coarse particles were removed by sieving through a sieve with 250 μm openings to obtain magnetic core particles 1 having a volume distribution standard 50% particle size (D50) of 37.0 μm.
[0085] <Preparation of Resin 1> Cyclohexyl methacrylate monomer 26.8 parts Methyl methacrylate monomer 0.2 parts Methyl methacrylate macromonomer 8.4 parts (A macromonomer with a weight-average molecular weight of 5000 and a methacryloyl group at one end) Toluene 31.3 parts Methyl ethyl ketone 31.3 parts The above raw materials were placed in a four-necked separable flask equipped with a reflux condenser, a thermometer, a nitrogen inlet tube, and a stirrer, and nitrogen gas was introduced to create a sufficient nitrogen atmosphere. After that, the mixture was heated to 80°C, 2.0 parts of azobisisobutyronitrile was added, and the mixture was refluxed for 5 hours to polymerize. Hexane was poured into the resulting reaction product to precipitate a copolymer, and the precipitate was filtered and then dried in vacuum to obtain Resin 1. Next, 30 parts of resin 1 was dissolved in 40 parts of toluene and 30 parts of methyl ethyl ketone to obtain polymer solution 1 (solid content 30% by mass).
[0086] <Preparation of coating resin solution 1> Polymer solution 1 (resin solids concentration 30%) 3.3 parts Toluene 66.4 parts Carbon black Regal 330 (Cabot) 0.3 parts (Primary particle size 25 nm, nitrogen adsorption specific surface area 94 m 2 / g, DBP oil absorption 75mL / 100g) The above raw materials were dispersed for 1 hour using a paint shaker with zirconia beads having a diameter of 0.5 mm. The resulting dispersion was filtered through a 5.0 μm membrane filter to obtain a coating resin solution 1.
[0087] <Magnetic Carrier 1 Manufacturing Example> (Resin coating process): Magnetic core particles 1 and coating resin solution 1 were put into a vacuum degassing kneader maintained at room temperature (the amount of coating resin solution 1 put in was 2.5 parts as a resin component for 100 parts of magnetic core particles 1). After putting in, the mixture was stirred at a rotation speed of 30 rpm for 15 minutes, and after a certain amount of the solvent (80 mass%) had evaporated, the mixture was heated to 80°C while mixing under reduced pressure, and toluene was distilled off over 2 hours, after which it was cooled. The magnetic carrier obtained was separated into low magnetic products by magnetic separation, passed through a sieve with an opening of 70 μm, and then classified with a wind classifier to obtain magnetic carrier 1 having a 50% particle size (D50) of 38.2 μm based on volume distribution.
[0088] <Production example of two-component developer 1> 92.0 parts of magnetic carrier 1 and 8.0 parts of toner 1 were mixed in a V-type mixer (product name: V-20, manufactured by Seishin Enterprise Co., Ltd.) to obtain two-component developer 1.
[0089] <Production Examples of Two-Component Developers 2 to 22> Two-component developers 2 to 22 were obtained in the same manner as in the production example of two-component developer 1, except that toner 1 was changed to toners 2 to 22. <Example 1>
[0090] As shown below, the pigment dispersion 1 used in the production of the toner 1 and the coloring power of the toner 1 used in the two-component developer 1 were evaluated.
[0091] <Evaluation method for pigment particle size> The particle size of the pigment in Pigment Dispersion 1 was measured using the above-mentioned method for measuring the number-average particle size of a pigment. (Evaluation Criteria) A: Less than 70 nm B: 70nm or more, less than 80nm C: 80nm or more, less than 90nm D: 90nm or more, less than 100nm E:100nm or more In the present invention, a grade of D or higher was deemed to have succeeded in finely refining the pigment, and a grade of E was deemed to have failed to finely refining the pigment.
[0092] <Method for evaluating the productivity of pigment dispersions> During the production of Pigment Dispersion 1, the evaluation was carried out based on the production volume per hour when the feed amount was maximized so as not to overload the motor of the kneading device. (Evaluation Criteria) A:25kg / h or more B: 20kg / h or more, less than 25kg / h C: 15kg / h or more, less than 20kg / h D: 10kg / h or more, less than 15kg / h E: Less than 10kg / h In the present invention, a grade of D or higher is deemed to be at a level where productivity is acceptable, and a grade of E is deemed to be unacceptable.
[0093] <Method for evaluating toner coloring power> A modified full-color copying machine (product name: imageRUNNER (trademark) ADVANCE C5255, manufactured by Canon) was used as the image forming apparatus, and evaluation was performed by putting two-component developer 1 into the developing device of the cyan station. The evaluation environment was a normal temperature and humidity environment (23°C, 50% RH), and the evaluation paper was plain copy paper (product name: GFC-081, sold by Canon Marketing Japan Inc., A4, basis weight 81.4 g / m 2) was used. First, in the above evaluation environment, the amount of toner applied on the paper was changed to examine the relationship between image density and the amount of toner applied on the paper. Next, the image density of the FFH image (solid area) was adjusted to 1.40, and the amount of toner applied when the image density was 1.40 was determined. An FFH image is a value in which 256 gradations are expressed in hexadecimal, with 00H being the first gradation (white area) and FFH being the 256th gradation (solid area). Image density was measured using an X-Rite color reflection densitometer (product name: 500 series, manufactured by X-Rite). Toner applied amount (mg / cm 2 The coloring power of the toner was evaluated based on the following criteria. The evaluation results are shown in Table 3. (Evaluation Criteria) A: Less than 0.35 B: 0.35 or more, less than 0.45 C: 0.45 or more, less than 0.55 D: 0.55 or more, less than 0.65 E: 0.65 or higher In the present invention, a grade of D or higher is considered to be acceptable, and a grade of E is considered to be unacceptable.
[0094] <Examples 2 to 17 and Comparative Examples 1 to 5> Except for changing the two-component developer used as shown in Table 3, the coloring power of the toner used in the two-component developer and the pigment dispersion used in the production of the toner were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 3.
[0095] [Table 3]
Claims
1. A method for producing a pigment dispersion, comprising a pigment dispersing step of melt-kneading a pigment, a binder, and a grinding agent, The pigment has acidic functional groups on its surface in an amount of 5 μmol / g or more, The grinding agent has basic functional groups on its surface in an amount of 5 μmol / g or more; The grinding agent is at least one selected from the group consisting of calcium carbonate, kaolin clay, talc, and barium sulfate; The binder contains a resin A having a basic functional group on its surface, The amount of basic functional groups on the surface of the resin A is 5 μmol / g or more, as determined by the following measurement method; The mass ratio of the resin A to the pigment is 0.01 or more and 0.30 or less. A method for producing a pigment dispersion comprising the steps of: Measurement method: Resin A (2 g) is added to a 1 / 100 N hydrochloric acid-ethanol solution (100 ml), and the supernatant is subjected to potentiometric titration using a 1 / 100 N potassium hydroxide-ethanol solution. The amount of basic functional groups on the surface of Resin A is determined from the difference between the amount of potassium hydroxide required for neutralization and the amount of hydrochloric acid initially present.
2. 2. The method for producing a pigment dispersion according to claim 1, wherein the number average particle diameter of the grinding agent is 0.1 μm or more and 20 μm or less.
3. 3. The method for producing a pigment dispersion according to claim 1, wherein the grinding agent is at least one selected from the group consisting of calcium carbonate, kaolin clay, and talc.
4. 4. The method for producing a pigment dispersion according to claim 1, wherein the resin A is a polyester resin having an amino group.
5. 5. The method for producing a pigment dispersion according to claim 1, wherein the pigment dispersion step is carried out using a twin-screw kneading extruder.
6. A method for producing a toner, comprising obtaining toner particles by using a pigment dispersion obtained by the method for producing a pigment dispersion according to any one of claims 1 to 5.
7. The method for producing the toner according to claim 6, which is carried out by at least one of the following methods (i) to (iv): (i) A method in which the pigment dispersion and a resin are melt-kneaded, and the resulting kneaded product is pulverized to obtain the toner particles. (ii) A method in which the above-mentioned pigment dispersion and a resin are dissolved in an organic solvent, the resulting resin solution is dispersed in an aqueous medium, granulated, and the solvent is removed to obtain the above-mentioned toner particles. (iii) A method of obtaining the toner particles by mixing the pigment dispersion with a polymerizable monomer, dispersing the obtained polymerizable monomer composition in an aqueous medium, granulating the resulting polymerizable monomer, and polymerizing the polymerizable monomer. (iv) A method of obtaining the toner particles by a process comprising the steps of mixing a dispersion liquid containing fine particles of the pigment dispersion and a dispersion liquid containing fine particles containing the resin, aggregating the fine particles of the pigment dispersion and the fine particles containing the resin to form aggregate particles, and heating the aggregate particles to fuse them.
Citation Information
Patent Citations
Preparation of beta type copper phtalocyanine pigment
JP1991084067A
Easily-dispersible copper phthalocyanine pigment composition, method for producing the same, and method for producing coloring composition
JP2003335976A
METHOD FOR PREPARING epsilon-PHTHALOCYANINE PIGMENT
JP2007100008A
Green coloring composition for color filter
JP2014002314A