Semiconductor device manufacturing method and chemical solution used in the semiconductor device manufacturing method

A two-step cleaning process with hydroxylamine and orthoperiodic acid solutions effectively removes ruthenium residues, enhancing etching rates and reducing surface deposits in semiconductor manufacturing.

JP7587418B2Active Publication Date: 2024-11-20TOKYO OHKA KOGYO CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020218757
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-11-20
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

Conventional methods for removing ruthenium residues in semiconductor manufacturing face challenges such as low etching rates, toxicity issues, and durability problems, particularly in the BEOL and MOL processes, leading to increased resistance and patterning variations.

Method used

A two-step cleaning process using a first chemical solution containing hydroxylamine or its derivative and a more basic alkaline compound, followed by a second solution with orthoperiodic acid and a basic compound, effectively removes ruthenium residues by etching and oxidation.

Benefits of technology

The method achieves enhanced removal of ruthenium residues, improving etching rates and reducing surface deposits, thereby addressing resistance and patterning issues in semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587418000001
    Figure 0007587418000001
  • Figure 0007587418000002
    Figure 0007587418000002
Patent Text Reader

Abstract

To provide a manufacturing method of a semiconductor element including a step capable of sufficiently cleaning and removing a ruthenium residue formed on a substrate surface by bringing a chemical solution into contact with the substrate surface after performing dry etching or chemical mechanical polishing on a ruthenium-containing layer which is positioned in an outermost surface layer of a substrate, and the chemical solution used for the manufacturing method of the semiconductor element.SOLUTION: The present invention relates to a manufacturing method of a semiconductor element including the steps of: performing dry etching or chemical mechanical polishing onto a ruthenium-containing layer which is positioned in an outermost surface layer of a substrate, and then bringing a surface of the substrate into contact with a first chemical solution; and bringing the surface of the substrate after the step of contact with the first chemical solution into contact with a second chemical solution. The manufacturing method is used in which the first chemical solution contains hydroxylamine or a derivative (A1) thereof and an alkali compound (B1) of which the basicity is stronger than that of the hydroxylamine or the derivative (A1) thereof, and the second chemical solution contains ortho-periodic acid (A2) and a basic compound (B2).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor device and a chemical solution used in the method for manufacturing a semiconductor device. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, there is a demand for forming metal wiring with a metal pitch of 20 nm or less. In this case, the conventional dual damascene structure that uses copper as the metal wiring material in the BEOL (Back End of Line) process has problems such as patterning variations and resistance increase that is close to its limit. For this reason, a semi-damascene structure using ruthenium, a low-resistance metal, has been proposed. When forming the semi-damascene structure, dry etching is performed on the ruthenium layer formed on the surface of the substrate. When dry etching is performed, a reaction product between ruthenium and the etching gas (hereinafter, sometimes simply referred to as "ruthenium residue") is formed on the surface of the ruthenium layer and other surface exposed films. For this reason, a chemical solution capable of cleaning and removing the ruthenium residue formed by dry etching is required. In addition, in the MOL (Middle End of Line) process, in contact wiring using tungsten or cobalt as a metal wiring material, the resistance increase due to miniaturization is close to the limit, and low-resistance ruthenium has been proposed. When ruthenium CMP is performed to form a contact, an oxidizing agent is used, so when CMP is performed, a reaction product with the oxidizing agent is formed on the surface of the ruthenium layer.

[0003] Conventionally, known removal solutions used for removing ruthenium residues include a composition containing orthoperiodic acid and having a pH of 11 or more (Patent Document 1), and a composition containing orthoperiodic acid and a quaternary ammonium salt compound or an amine compound (Patent Document 2). The removal solution described in Patent Document 1 is highly alkaline, so the etching rate of ruthenium is low and the removal of residues is insufficient. The removal solution described in Patent Document 2 has a low pH, and there is a concern that toxic gas ruthenium tetroxide (RuO4) will be generated during ruthenium cleaning. In addition, there are still issues to be addressed when using this solution in wafer cleaning equipment for mass production of semiconductors, from the standpoint of component resistance and particle control. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2016 / 068183 [Patent Document 2] JP 2018-121086 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in view of the above circumstances, and has an object to provide a method for manufacturing a semiconductor device, which includes a step of contacting a chemical solution with a substrate surface after dry etching or chemical mechanical polishing of a ruthenium-containing layer located at the outermost layer of the substrate, thereby enabling ruthenium residue formed on the substrate surface to be sufficiently washed and removed, and a chemical solution that is suitably used in the method for manufacturing a semiconductor device. [Means for solving the problem]

[0006] The present inventors have found that the above-mentioned problems can be solved by subjecting the surface of a substrate, after dry etching or chemical mechanical polishing, to a ruthenium-containing layer located at the outermost layer of the substrate, to a cleaning treatment with a cleaning solution containing hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) that is more basic than the hydroxylamine or derivative thereof (A1), prior to the cleaning treatment with the ruthenium-removal solution containing orthoperiodic acid, and have thus completed the present invention.

[0007] A first aspect of the present invention is a method for producing a ruthenium-containing layer comprising the steps of: performing dry etching or chemical mechanical polishing on a ruthenium-containing layer located on the outermost layer of a substrate; and then contacting the surface of the substrate with a first chemical solution. and contacting the surface of the substrate after the step of contacting the surface with the first chemical liquid with a second chemical liquid, the first chemical solution contains hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) having a stronger basicity than the hydroxylamine or the derivative thereof (A1); This is a production method in which the second chemical solution contains orthoperiodic acid (A2) and a basic compound (B2).

[0008] A second aspect of the present invention is a first chemical solution used in the method for manufacturing a semiconductor device according to the first aspect, The chemical solution contains hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) that is more basic than the hydroxylamine or the derivative thereof (A1). Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for manufacturing a semiconductor device, which includes a step of contacting a substrate surface after dry etching or chemical mechanical polishing of a ruthenium-containing layer located at the outermost layer of the substrate with the first chemical liquid and then with a second chemical liquid, thereby cleaning and removing ruthenium residue formed on the substrate surface, and a chemical liquid suitable for use in the method for manufacturing a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Method for manufacturing semiconductor element> A method for manufacturing a semiconductor device includes the steps of: performing dry etching or chemical mechanical polishing on a ruthenium-containing layer located on the outermost layer of a substrate; and then contacting the surface of the substrate with a first chemical solution. and contacting the surface of the substrate after the step of contacting the surface with the first chemical liquid with a second chemical liquid, the first chemical solution contains hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) having a stronger basicity than the hydroxylamine or the derivative thereof (A1); This is a production method in which the second chemical solution contains orthoperiodic acid (A2) and a basic compound (B2).

[0011] <Step of performing cleaning treatment with first chemical solution> (Object to be treated) In the step of performing the cleaning treatment with the first chemical solution, the workpiece to be cleaned is a substrate after dry etching or chemical mechanical polishing has been performed on a ruthenium-containing layer located at the outermost layer of the substrate.

[0012] The substrate on which the dry etching or chemical mechanical polishing is performed has a ruthenium-containing layer on the outermost surface thereof. The method for forming the ruthenium-containing layer on the substrate is not particularly limited, and any known method can be used, such as physical vapor deposition (PVD) such as sputtering, chemical vapor deposition (CVD), and atomic layer deposition (ALD). The process of performing dry etching or chemical mechanical polishing on the substrate is not particularly limited, but preferably includes a process of using ruthenium as the metal wiring material and forming a metal wiring pattern on the substrate by a semi-damascene method, a process of forming MOL contact wiring, and a process of forming a buried power rail.

[0013] As described above, the substrate after dry etching or chemical mechanical polishing is performed on the ruthenium-containing layer located at the top surface of the substrate is the substrate. In dry etching, when O2 / Cl2 is used as an etching gas, for example, Ru oxide, Ru chloride, other exposed films and unspecified residues derived from the etching gas reaction products are formed on the surface of the Ru-containing layer after etching, and these are deposited or layers are formed. In addition, since metal oxidant particles are used in chemical mechanical polishing, Ru oxide, unspecified residues, and the like are formed on the surface of the ruthenium-containing layer after CMP, and these are deposited or layers are formed. In the manufacturing method of semiconductor devices, the deposits or layers formed on the substrate are the objects to be removed, and these surfaces are the surfaces to be treated.

[0014] (First chemical solution) The first chemical solution contains hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) that is more basic than the hydroxylamine or the derivative thereof (A1).

[0015] Examples of hydroxylamine or its derivative (A1) include hydroxylamine and N,N-dialkylhydroxylamine. These may be used alone or in combination.

[0016] N,N-dialkylhydroxylamines have the general formula R 1 R 2 NOH (in the formula, R 1 and R 2 Each independently represents an alkyl group. 1 or R 2 As the alkyl group, for example, a methyl group, an ethyl group, a propyl group, and a butyl group are preferable.

[0017] Examples of N,N-dialkylhydroxylamines include N,N-dimethylhydroxylamine, N,N-diethylhydroxylamine, N,N-dipropylhydroxylamine, and N,N-dibutylhydroxylamine.

[0018] The content of hydroxylamine or a derivative thereof (A1) is preferably from 0.1% by mass to 20% by mass, and more preferably from 0.3% by mass to 10% by mass, based on the total mass of the first chemical solution.

[0019] The alkaline compound (B1) is a compound that is more basic than the above-mentioned hydroxylamine or its derivative (A1). A compound that is more basic than the above-mentioned component (A1) means that it has the property of shifting the pH of an aqueous solution consisting of only the above-mentioned component (A1) and water to the alkaline side.

[0020] The alkaline compound (B1) is not particularly limited as long as it has the above-mentioned properties, and both organic alkaline compounds and inorganic alkaline compounds can be used. Suitable examples of the organic alkaline compound include quaternary ammonium salts such as organic quaternary ammonium hydroxides; alkanolamines; and organic amines other than alkanolamines, such as primary amines, secondary amines, tertiary amines, and amidines.

[0021] Examples of organic quaternary ammonium hydroxides include tetramethylammonium hydroxide, bis(2-hydroxyethyl)dimethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltriethylammonium hydroxide, trimethyl(hydroxyethyl)ammonium hydroxide, and triethyl(hydroxyethyl)ammonium hydroxide.

[0022] Examples of alkanolamines include monoethanolamine, diethanolamine, monoisopropanolamine, diisopropanolamine, methylethanolamine, N-methylethanolamine, and aminoethylethanolamine.

[0023] Other organic amines include, for example, diazabicycloundecene.

[0024] Examples of inorganic alkaline compounds include inorganic compounds containing ammonia, alkali metals, or alkaline earth metals, and salts thereof. Specific examples of inorganic compounds containing alkali metals or alkaline earth metals and salts thereof include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide.

[0025] The content of the alkali compound (B1) is preferably from 0.01% by mass to 20% by mass, and more preferably from 0.1% by mass to 10% by mass, based on the total mass of the first chemical solution.

[0026] The pH of the first chemical solution is not particularly limited, but from the viewpoint of improving the removability of ruthenium residues, the pH is preferably 10 or higher, and more preferably 11 or higher at 20°C.

[0027] (Other ingredients) The first chemical solution may contain other components in addition to the above components, such as water, a surfactant, an alcohol-based solvent, an ether-based solvent, and a sulfoxide-based solvent, as long as the effects of the present invention are not impaired.

[0028] The first chemical liquid preferably contains water as a solvent. As the water, water that has been subjected to a purification treatment, such as distilled water, ion-exchanged water, or ultrapure water, is preferable, and ultrapure water that is generally used in semiconductor manufacturing is more preferable. The water content is not particularly limited, but is preferably 20% by mass or more, more preferably 80% by mass or more, based on the total mass of the first chemical solution. The upper limit is not particularly limited, but is preferably less than 99.95% by mass, more preferably 99.9% by mass or less.

[0029] The first chemical solution can be obtained by mixing the above-mentioned compound (A1), compound (B1), and other components as required, by a known method.

[0030] In the step of performing a cleaning process with a first chemical liquid, the surface of the workpiece is brought into contact with the first chemical liquid. Here, the surface of the workpiece means the surface of the workpiece to be treated. The method of bringing the surface of the workpiece into contact with the first chemical liquid is not particularly limited, and any known method can be used. Examples of such methods include, but are not limited to, a spray method, an immersion method, and a puddle method. In the spray method, for example, the workpiece is transported or rotated in a predetermined direction, and the first chemical liquid is sprayed toward the transported or rotated workpiece, thereby bringing the first chemical liquid into contact with the treatment surface of the workpiece. In the immersion method, the object to be treated is immersed in the first chemical liquid to bring the object to be treated into contact with the first chemical liquid. In the puddle method, the first chemical liquid is puddled on the object to be treated, and the object to be treated is brought into contact with the first chemical liquid. These cleaning methods can be appropriately selected depending on the structure, material, etc. of the object to be treated. In the case of the spray method or the puddle method, the amount of the etching liquid supplied to the object to be treated may be an amount that allows the surface of the object to be treated to be sufficiently wetted with the etching liquid.

[0031] The cleaning temperature is not particularly limited, but is preferably from 23° C. to 85° C., and more preferably from 30° C. to 70° C. The cleaning time is not particularly limited, but is preferably from 30 seconds to 30 minutes, and more preferably from 1 minute to 10 minutes.

[0032] <Step of performing cleaning treatment with second chemical solution> (Second chemical solution) The second chemical solution contains orthoperiodic acid (A2) and a basic compound (B2).

[0033] Ruthenium is converted to ruthenium tetroxide (RuO4) by bonding with four oxygen atoms. Orthoperiodic acid (A2) (H5IO6) is an oxidizing agent that releases oxygen atoms to oxidize ruthenium. The redox potential of orthoperiodic acid (A2) is high enough to oxidize ruthenium. Therefore, the second chemical solution containing orthoperiodic acid (A2) can efficiently oxidize ruthenium and effectively dissolve the RuO4 produced by the oxidation.

[0034] The content of orthoperiodic acid (A2) is, for example, 0.01 to 8 mass% relative to the total mass of the second chemical solution, preferably 0.02 to 7 mass%, and more preferably 0.03 to 5 mass%. When the content of orthoperiodic acid is within the above range, the etching rate for ruthenium is further improved.

[0035] As the basic compound (B2), both organic and inorganic basic compounds can be used. Suitable examples of the organic basic compound include quaternary ammonium salts such as organic quaternary ammonium hydroxides, amine oxides, and tertiary amines.

[0036] Examples of organic quaternary ammonium hydroxides include tetramethylammonium hydroxide, bis(2-hydroxyethyl)dimethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, methyltriethylammonium hydroxide, trimethyl(hydroxyethyl)ammonium hydroxide, and triethyl(hydroxyethyl)ammonium hydroxide.

[0037] Examples of the amine oxide include trimethylamine N-oxide, triethylamine N-oxide, 4-methylmorpholine N-oxide, and pyridine N-oxide.

[0038] Examples of tertiary amines include trimethylamine, triethylamine, tripropylamine, tributylamine, 4-methylmorpholine, and N,N-dimethylaniline.

[0039] Examples of inorganic basic compounds include inorganic compounds containing ammonia, alkali metals, or alkaline earth metals, and salts thereof. Specific examples of inorganic compounds containing alkali metals or alkaline earth metals and salts thereof include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide.

[0040] The content of the basic compound (B2) is preferably from 0.002% by mass to 10% by mass, and more preferably from 0.005% by mass to 5% by mass, based on the total mass of the second chemical solution.

[0041] The pH of the second chemical solution is not particularly limited, but is preferably 8 or more and 10 or less, and more preferably 8.5 or more and 10 or less, at 20°C, for example.

[0042] (Other ingredients) The second chemical solution may contain other components in addition to the above components, such as water, a surfactant, and a tertiary alcohol, as long as the effects of the present invention are not impaired.

[0043] The second chemical liquid preferably contains water as a solvent. As the water, water that has been subjected to a purification treatment, such as distilled water, ion-exchanged water, or ultrapure water, is preferable, and ultrapure water that is generally used in semiconductor manufacturing is more preferable. The water content is not particularly limited, but is preferably 50% by mass or more, more preferably 80% by mass or more, based on the total mass of the second chemical solution. The upper limit is not particularly limited, but is preferably less than 99.95% by mass, more preferably 99.9% by mass or less.

[0044] The second chemical solution can be obtained by mixing the above-mentioned compound (A2), compound (B2), and other components as required, by a known method.

[0045] In the step of performing a cleaning treatment with a second chemical solution, the surface of the substrate after the step of contacting with the first chemical solution is contacted with the second chemical solution. The method of contacting the surface of the substrate with the second chemical solution is not particularly limited, and the same method as the method described for the first chemical solution can be used.

[0046] The cleaning temperature is not particularly limited, but is preferably from 15° C. to 60° C., and more preferably from 20° C. to 50° C. The cleaning time is not particularly limited, but is preferably from 5 seconds to 10 minutes, and more preferably from 10 seconds to 3 minutes. EXAMPLES

[0047] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0048] [Examples 1 to 4 and Comparative Examples 1 to 17] (Preparation of drug solution) Chemical solutions S1 to S16 were prepared as shown in Table 1 below. Chemical solutions S2 to S16 are all aqueous solutions. Chemical solutions S10 to S14 and S16 each represent a mixed solution containing two types of chemical components at the concentrations shown in Table 1. Table 1 also shows the pH of each chemical solution.

[0049] [Table 1]

[0050] The abbreviations used in Table 1 are as follows: TMAH: Tetramethylammonium hydroxide TBAH: Tetrabutylammonium hydroxide AEEA: Aminoethylethanolamine MEA: Monoethanolamine DEHA: Diethylhydroxylamine

[0051] (Preparation of test board) Using an ICP dry etching device, the surface of a PVD-Ru substrate (Ru film thickness: 50 nm) formed by sputtering was dry etched under the following conditions to etch 3 nm of Ru. The Ru substrate after dry etching was cut into a 1.5 x 2 cm square to prepare a test substrate. Dry etching equipment: NE-550E (ULVAC) Gas type: O2 / Cl2 Gas flow rate: O2 / Cl2=46sccm / 4sccm Etching temperature: 23℃ Etching time: 15 seconds

[0052] (Cleaning treatment tests of Comparative Examples 1 to 15) Each of the above chemical solutions S1 to S15 was placed in a beaker, and each test substrate was immersed in each chemical solution. While stirring each chemical solution at 300 rpm, a cleaning process was performed at the process temperature and for the process time shown in Table 2 below. In Comparative Examples 1 to 15, cleaning treatment was performed using one type of chemical solution. In Table 2, of the columns "Cleaning with a first chemical solution" and "Cleaning with a second chemical solution", the former lists the type of chemical solution, treatment temperature, and treatment time used in Comparative Examples 1 to 14, and the latter lists the type of chemical solution, treatment temperature, and treatment time used in Comparative Example 15.

[0053] (Cleaning treatment tests for Examples 1 to 4 and Comparative Examples 16 to 17) The above-mentioned chemical solutions S4 to S5, S10 to S12, and S16 were placed in a beaker, and each test substrate was immersed in each chemical solution, and while each chemical solution was stirred at 300 rpm, a cleaning treatment with the first chemical solution and a water rinsing treatment were performed at the treatment temperature and treatment time shown in Table 2. Next, the above-mentioned chemical solution S15 was placed in each beaker, and each test substrate after the above-mentioned cleaning treatment was immersed in each chemical solution S15, and while each chemical solution S15 was stirred at 300 rpm, a cleaning treatment with the second chemical solution was performed at the treatment temperature and treatment time shown in Table 2.

[0054] (Measurement of chlorine removal rate on ruthenium surface) After the above cleaning test, each substrate was washed with water and dried under a nitrogen stream. X-ray photoelectron spectroscopy (XPS analysis) was performed on the surface of the dried substrate to determine the peak area derived from Cl2. The peak area derived from Cl2 was also determined for the test substrate before the above cleaning test, and the chlorine removal rate was calculated based on the following formula. Chlorine removal rate (%) = ((peak area before cleaning test - peak area after cleaning test / peak area before cleaning test)) x 100

[0055] The chlorine removal ability was evaluated on a 5-point scale, A to E, according to the chlorine removal rate. The results are shown in Table 2. A: 75% or more - 100% B: 50% or more but less than 75% C: 25% or more but less than 50% D: 10% or more but less than 25% E: Less than 10%

[0056] (Measurement of Ru etching amount) The thickness of the Ru film was measured by fluorescent X-ray analysis for the substrates that had been dried after the cleaning test. The thickness of the Ru film was also measured for the test substrates before the cleaning test. The amount of Ru etching (Å) was calculated from the Ru film thickness before and after the cleaning test. The results are shown in Table 2.

[0057] [Table 2]

[0058] In Comparative Examples 1 to 15, in which the cleaning treatment was performed using one type of chemical solution, the chlorine removal rate was at most less than 50% of that in Comparative Example 15. The amount of Ru etched was also at most less than that in Comparative Example 15. The thickness was only 2 Å. These results show that in Comparative Examples 1 to 15, the removability of etching residues and the like formed on the Ru surface of the test substrate was insufficient. In Comparative Examples 16 and 17, the cleaning treatment was performed using the chemical solutions S4 and S5, respectively, as a pre-cleaning treatment before the cleaning treatment with the same chemical solution S15 as in Comparative Example 15. However, the chlorine removal performance was insufficient in both cases. On the other hand, in Comparative Example 16, when the pre-cleaning process was performed with any of the chemical solutions S10 to 12 or S16 instead of the chemical solution S4, as shown in Examples 1 to 4, the chlorine removal rate was at least 50% or more, and the etching amount of Ru increased to at least 7 Å. These experimental results show that performing a cleaning treatment with a first chemical solution containing hydroxylamine (A1) and an alkaline compound (B1) as a pre-cleaning treatment before performing a cleaning treatment with a second chemical solution containing orthoperiodic acid (A2) and a basic compound (B2) provides excellent residue removal properties.

Claims

1. a cleaning step of contacting a surface of the substrate with a first chemical solution after dry etching the ruthenium-containing layer located at the outermost layer of the substrate; a cleaning process step of contacting the surface of the substrate with a second chemical liquid after the cleaning process step of contacting the surface with the first chemical liquid, the first chemical solution contains hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) having a stronger basicity than the hydroxylamine or the derivative thereof (A1); The second chemical solution contains orthoperiodic acid (A2) and a basic compound (B2).

2. 2. The method for producing a semiconductor device according to claim 1, wherein the second chemical solution contains ammonia as the basic compound (B2).

3. The method for manufacturing a semiconductor device according to claim 1 , wherein the second chemical solution has a pH of 8 or more and 10 or less.

4. 4. The method for producing a semiconductor device according to claim 1, wherein the hydroxylamine or derivative thereof (A1) is at least one member selected from the group consisting of hydroxylamine and N,N-dialkylhydroxylamine.

5. The method for manufacturing a semiconductor device according to any one of claims 1 to 4, wherein the first chemical solution has a pH of 10 or more.

6. A first chemical solution used in the method for manufacturing a semiconductor device according to any one of claims 1 to 5, A chemical solution comprising hydroxylamine or a derivative thereof (A1) and an alkaline compound (B1) having a stronger basicity than the hydroxylamine or the derivative thereof (A1).

7. The drug solution according to claim 6, having a pH of 10 or more.

8. The chemical solution according to claim 6 or 7, wherein the hydroxylamine or derivative thereof (A1) is at least one member selected from the group consisting of hydroxylamine and N,N-dialkylhydroxylamine.

Citation Information

Patent Citations

  • Removing liquid for removing ruthenium deposit on substrate with ruthenium-containing film formed thereon

    JP2018121086A

  • Etchant, method of treating treatment target, and method for producing semiconductor element

    JP2020097765A

  • Stripper solution and method of using the stripper solution

    JP2020536138A

  • Compositions and methods for post-CMP cleaning of cobalt substrates

    JP2022514611A

  • Stripper Solutions and Methods of Using Stripper Solutions

    US20190101830A1