Binder for power storage devices that improves the dispersibility of conductive additives

A specialized binder with enhanced dispersibility and flexibility addresses the uniform dispersion and cohesion issues of conductive additives in lithium ion secondary batteries, improving electrode performance and battery capacity.

JP7587508B2Active Publication Date: 2024-11-20FUJIFILM WAKO PURE CHEMICAL CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021543036
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-22
Filing Date
2020-08-28
Publication Date
2024-11-20
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Existing binders for lithium ion secondary batteries face challenges in achieving uniform dispersion of conductive additives, leading to increased internal resistance and reduced battery performance due to insufficient dispersibility and cohesion, while also compromising the flexibility and durability of electrodes.

Method used

A binder with specific properties, including a loss tangent greater than 1 and containing ethylenically unsaturated carboxylic acid monomers and neutralized polymers, is used to enhance the dispersibility and flexibility of conductive additives in the electrode slurry, ensuring uniform distribution and improved electrode performance.

Benefits of technology

The proposed binder achieves excellent dispersibility of conductive additives, maintaining high capacity and flexibility, thereby enhancing the electrical characteristics and durability of the electrodes in lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587508000001
    Figure 0007587508000001
  • Figure 0007587508000002
    Figure 0007587508000002
  • Figure 0007587508000003
    Figure 0007587508000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a binder which exhibits excellent dispersibility of a conductive assistant; a slurry composition and an electrode, each of which uses this binder; and an electricity storage device which is provided with this electrode. The present invention relates to: a binder for electricity storage devices, wherein the loss tangent tanδ in the linear region of an aqueous dispersion that contains 0.5% by mass of the binder and 4.6% by mass of a conductive assistant satisfies tanδ > 1 as determined by a strain dispersion measurement at a measurement temperature of 25°C and a frequency of 1 Hz, provided that the conductive assistant is an acetylene black having an average particle diameter of from 30 nm to 40 nm and a specific surface area of from 65 m2 / g to 70 m2 / g; a slurry composition and an electrode, each of which uses this binder; an electricity storage device which is provided with this electrode; and the like.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a binder, a slurry composition, and an electrode used in an electricity storage device, and to an electricity storage device including the electrode. [Background technology]

[0002] In recent years, batteries (electricity storage devices) used in notebook computers, mobile phones and other portable terminals, hybrid cars, electric vehicles, power-assisted bicycles, etc. have rapidly become widespread, and there is a demand for them to be made smaller and lighter. Lithium-ion secondary batteries, which have the advantages of being high energy density and lightweight, have been attracting attention as electricity storage devices for use in these products.

[0003] Usually, an electrode used in a lithium ion secondary battery or the like includes a current collector and an electrode mixture layer formed on the current collector. The negative electrode mixture layer, which is the electrode mixture layer in the negative electrode, is generally formed by applying a negative electrode mixture layer slurry (electrode mixture layer slurry) made by dispersing or dissolving a negative electrode active material such as graphite or silicon, a conductive assistant such as acetylene black or carbon black, a binder (binding agent) and the like in a dispersion medium onto a current collector, and drying the slurry to bind the negative electrode active material and the conductive assistant with the binder.

[0004] The properties required for the electrode mixture layer slurry include uniformity when the active material and conductive assistant are dispersed or dissolved in the dispersion medium. This is because the dispersion state of the active material and conductive assistant in the electrode mixture layer slurry is related to the distribution state of the active material and conductive assistant in the electrode mixture layer, and affects the electrode properties and, ultimately, the battery performance. In particular, carbon materials, which have excellent conductivity among conductive assistants, have small particle diameters and large specific surface areas, and therefore have strong cohesive forces, making it difficult to mix and disperse them uniformly in the electrode mixture layer slurry. And, if the dispersibility and particle size control of the carbon material are insufficient, a uniform conductive network is not formed, so the internal resistance of the electrode cannot be reduced, resulting in a problem that the performance of the electrode material cannot be fully brought out. Therefore, improving the dispersibility of the conductive assistant is an important issue.

[0005] Therefore, various methods for dispersing the conductive assistant in the slurry for the electrode mixture layer have been studied. For example, Patent Document 1 and Patent Document 2 describe an example in which a surfactant is used as a dispersant when dispersing carbon black in a solvent. In addition, Patent Document 3 and Patent Document 4 describe an example in which various additives are added when dispersing the conductive assistant.

[0006] In addition, various studies have been conducted on electrodes coated with a slurry to improve their flexibility in order to prevent cracks caused by the expansion and contraction of active materials during winding and trimming during battery manufacturing and repeated charging and discharging. For example, Patent Document 5 and Patent Document 6 describe examples of using polymers containing specific monomer components in a predetermined ratio. Patent Document 7 describes an example of improving flexibility by adding a carbon nanotube complex. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 63-236258 [Patent Document 2] Japanese Patent Application Publication No. 8-190912 [Patent Document 3] JP 2013-206759 A [Patent Document 4] JP 2012-195243 A [Patent Document 5] JP 2016-155927 A [Patent Document 6] International Publication No. 2018 / 003636 [Patent Document 7] JP 2016-054113 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the surfactants described in Patent Documents 1 and 2 have a weak adsorption force to the carbon material surface, so that a large amount must be added to obtain good dispersion stability, which results in a problem that the amount of active material that can be contained in the electrode mixture layer is reduced, resulting in a decrease in battery capacity. In addition, if the surfactant is not sufficiently adsorbed to the carbon material, the aggregation of the carbon material cannot be suppressed, and the dispersibility remains insufficient. In addition, the dispersants described in the above Patent Documents 3 and 4 have a possibility of dissolving from the electrode mixture layer into the electrolyte solution and adversely affecting the battery performance because they are low molecular weight. In addition, there is a problem that the battery performance is deteriorated when the compatibility of the added dispersant with the binder polymer or the solvent is poor.

[0009] On the other hand, in terms of electrode flexibility, the polymers to which the monomers described in the above-mentioned Patent Documents 5 and 6 have been added have a problem in that the main skeleton of the polymer becomes flexible, and therefore the conductive paths between the active materials are lost due to the expansion and contraction of the active materials accompanying charge and discharge, resulting in a decrease in battery capacity. In addition, there is a problem in that the aqueous dispersion type polymer has a low viscosity and therefore needs to be used in combination with a thickener such as carboxymethyl cellulose. In addition, since the carbon nanotube composite described in the above-mentioned Patent Document 7 does not contain a binder polymer, it may peel off from the electrode current collector foil after repeated charging and discharging, and may not be able to withstand long-term use. In addition, in order to increase the strength of the composite sheet, the amount of carbon nanotubes must be increased, which results in a decrease in the proportion of active material in the electrode, resulting in a problem of a decrease in the energy density of the battery.

[0010] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a binder having excellent dispersibility that solves the above-mentioned problems, or a binder that can impart excellent flexibility to an electrode, a slurry composition and an electrode using the same, and an electricity storage device including the electrode. [Means for solving the problem]

[0011] As a result of extensive research, the inventors have discovered that by using a binder in an electricity storage device, such that in a linear region of an aqueous dispersion containing specific amounts of a conductive additive and a binder, the loss tangent tanδ is tanδ>1 in strain dispersion measurements, an electricity storage device can be obtained that has excellent dispersibility of the conductive additive and can retain a high capacity for a long period of time, and have thus completed the first invention.

[0012] Furthermore, as a result of extensive research, the present inventors have found that the use of a binder containing a salt of a polymer neutralized with a specific neutralizing agent improves the flexibility of the electrode, making it possible to manufacture an electrode with excellent winding properties and an electricity storage device including the electrode, and have thus completed the second invention.

[0013] That is, the first invention includes the following inventions [i] to [xi]. [i] A binder for an electricity storage device; In a strain dispersion measurement under the measurement conditions of a measurement temperature of 25°C and a frequency of 1 Hz, the loss tangent tanδ in the linear region of an aqueous dispersion of the binder at 0.5 mass% and a conductive assistant at 4.6 mass% is tanδ>1, and the conductive assistant has an average particle size of 30 nm to 40 nm and a specific surface area of ​​65 m 2 / g or more 70m 2 / g or less of acetylene black (hereinafter, sometimes abbreviated as the binder of the first invention). [ii] The binder according to the above invention [i], which contains (i) an ethylenically unsaturated carboxylic acid monomer, and (ii) a polymer or a salt thereof containing a structural unit derived from an ethylenically unsaturated monomer having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group. [iii] The binder according to the above invention [ii], wherein the solubility of the monomer (ii) in water at 20°C is 1 g / L or more. [iv] The SP value of the monomer (ii) above is 11.5 (cal / cm 3 ) 1 / 2 The binder according to the above invention [ii] or [iii]. [v] The binder according to any one of the above inventions [ii] to [iv], wherein the monomer (ii) is a monomer represented by the following general formula [1]: TIFF0007587508000001.tif2555 (In general formula [1], R1 represents a hydrogen atom or a methyl group, Y1 represents -O- or -NR2-, R2 represents a hydrogen atom or a methyl group, and A1 represents a monovalent group having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group.) [vi] The binder according to any one of the above inventions [ii] to [v], wherein the monomer (ii) is a monomer represented by the following general formula [2]: TIFF0007587508000002.tif2555 (In general formula [2], R1 represents a hydrogen atom or a methyl group, Y1 represents -O- or -NR2-, R2 represents a hydrogen atom or a methyl group, and A2 represents an alkyl group having 1 to 10 carbon atoms and having 1 to 3 of any one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; or a linear alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain.) [vii] The binder according to any one of the above inventions [ii] to [vi], wherein the polymer or the salt thereof further contains (iii) a structural unit derived from a monomer having two or more polymerizable unsaturated groups. [viii] The binder according to any one of the above inventions [ii] to [vii], wherein the polymer or the salt thereof is neutralized with an alkali metal hydroxide and / or a polyvalent amine having an amine value of 21 or more. [ix] A slurry composition for an electricity storage device, comprising the binder according to any one of the above inventions [i] to [viii] (hereinafter sometimes abbreviated as the slurry composition of the first invention). [x] An electrode for an electricity storage device comprising the slurry composition according to the above invention [ix] (hereinafter, sometimes abbreviated as the electrode of the first invention). [xi] An electricity storage device comprising the electrode according to the above invention [x] (hereinafter, may be abbreviated as the electricity storage device of the first invention).

[0014] The second invention also includes the following inventions [xii] to [xxi]. [xii] A binder for an electricity storage device (hereinafter sometimes abbreviated as the binder of the second invention) which contains (i) an ethylenically unsaturated carboxylic acid monomer and (ii) a structural unit derived from an ethylenically unsaturated monomer having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group, and contains a salt of a polymer neutralized with a monoamine, a polyamine having an amine value of less than 21, and / or an onium hydroxide. [xiii] The binder according to the above invention [xii], wherein the molecular weight of the polyamine is 600 or less. [xiv] The binder according to the above invention [xii] or [xiii], wherein the solubility of the monomer (ii) in water at 20°C is 1 g / L or more. [xv] The SP value of the monomer (ii) above is 11.5 (cal / cm 3 ) 1 / 2 The binder according to any one of the above inventions [xii] to [xiv]. [xvi] The binder according to any one of the above inventions [xii] to [xv], wherein the monomer (ii) is a monomer represented by the following general formula [1]: TIFF0007587508000003.tif2655 (In general formula [1], R1 represents a hydrogen atom or a methyl group, Y1 represents -O- or -NR2-, R2 represents a hydrogen atom or a methyl group, and A1 represents a monovalent group having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group.) [xvii] The binder according to any one of the above inventions [xii] to [xvi], wherein the monomer (ii) is a monomer represented by the following general formula [2]: TIFF0007587508000004.tif2655 (In general formula [2], R1 represents a hydrogen atom or a methyl group, Y1 represents -O- or -NR2-, R2 represents a hydrogen atom or a methyl group, and A2 represents an alkyl group having 1 to 10 carbon atoms and having 1 to 3 of any one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; or a linear alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain.) [xviii] A slurry composition for an electricity storage device, comprising the binder according to any one of the above inventions [xii] to [xvii] (hereinafter sometimes abbreviated as the slurry composition of the second invention). [xix] An electrode for an electricity storage device comprising the slurry composition according to the above invention [xviii] (hereinafter sometimes abbreviated as the electrode of the second invention). [xx] An electricity storage device comprising the electrode according to the above invention [xix] (hereinafter, may be abbreviated as the electricity storage device of the second invention). Effect of the Invention

[0015] By using the binder of the first invention, it is possible to provide an electricity storage device that has excellent dispersibility of the conductive assistant and can retain a high capacity for a long period of time.

[0016] In addition, by using the binder of the second invention in the production of an electrode, it becomes possible to provide an electrode with improved flexibility and excellent winding property, and a power storage device including the electrode.

Embodiment for Carrying Out the Invention

[0017] [Binder of the First Invention] The binder of the first invention has a loss tangent tanδ > 1 in the linear region of an aqueous dispersion of 0.5 mass% of the binder and 4.6 mass% of a conductive auxiliary agent in the measurement of strain dispersion under the measurement conditions of a measurement temperature of 25°C and a frequency of 1 Hz. There is no particular limitation on the upper limit value of tanδ, but for example, 1 < tanδ ≤ 100, preferably 1 < tanδ ≤ 50, and more preferably 1 < tanδ ≤ 10.

[0018] The above-mentioned "linear region" refers to the region from the time when the measurement is started to the time when the structural destruction of the measurement sample starts in the measurement of strain dispersion, and is the region where the elastic modulus obtained in the measurement of strain dispersion shows a constant value without depending on the increase in the amount of strain. Note that the region after the start of structural destruction (the range where the elastic modulus decreases depending on the increase in the amount of strain) is called the non-linear region.

[0019] The above-mentioned "loss tangent tanδ" indicates the ratio of the storage elastic modulus G' to the loss elastic modulus G'' (loss elastic modulus G'' / storage elastic modulus G'), where the storage elastic modulus G' is an index of elastic properties and the loss elastic modulus G'' is an index of viscous properties. Both the storage elastic modulus G' and the loss elastic modulus G'' are obtained by performing strain dispersion measurement.

[0020] As a method for calculating the above-mentioned "loss tangent tanδ", specifically, using a rheometer MCR 102 (dynamic viscoelasticity measuring device: manufactured by Anton Paar), under the measurement conditions of a measurement temperature of 25°C and a frequency of 1 Hz, when the amount of strain is increased from 10 -2 % to 10 3 %, the storage elastic modulus G' and the loss elastic modulus G'' are measured, and loss elastic modulus G'' / storage elastic modulus G' may be calculated based on the obtained values.

[0021] The conductive additive has an average particle size of 30 nm or more and 40 nm or less and a specific surface area of ​​65 m 2 / g or more 70m 2 The acetylene black that satisfies the average particle size and specific surface area conditions is specifically, for example, Denka Black (registered trademark) powder (average particle size: 35 nm, specific surface area: 68 m) manufactured by Denka Co., Ltd. 2 / g (representative value listed on the Denka Corporation website) etc. can be used.

[0022] As the "water" which is the dispersion medium in the "aqueous dispersion", ion-exchanged water may be used.

[0023] Specific examples of the binder of the first invention include a polymer containing structural units derived from an ethylenically unsaturated monomer having at least one group selected from (i) an ethylenically unsaturated carboxylic acid monomer and (ii) a hydroxyl group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group (hereinafter, sometimes abbreviated as the polymer according to the first invention) or a salt thereof.

[0024] The above (i) ethylenically unsaturated carboxylic acid monomer (hereinafter sometimes abbreviated as monomer (i)) is a monomer having both an ethylenically unsaturated group and a carboxy group in one molecule. However, unlike monomer (iii) described below, monomer (i) has one ethylenically unsaturated group. Furthermore, monomer (i) may be an acid anhydride.

[0025] Specific examples of the monomer (i) include ethylenically unsaturated monocarboxylic acid monomers such as acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, mono(2-acryloyloxyethyl)succinate, mono(2-acryloyloxyethyl)phthalate, and mono(2-acryloyloxyethyl)hexahydrophthalate; and ethylenically unsaturated dicarboxylic acid monomers such as maleic acid, fumaric acid, itaconic acid, maleic anhydride, and itaconic anhydride. Among these specific examples, ethylenically unsaturated monocarboxylic acid monomers are preferred, acrylic acid and methacrylic acid are more preferred, and acrylic acid is particularly preferred. The monomer (i) may be used alone or in combination of two or more types, and is preferably used alone.

[0026] The above (ii) ethylenically unsaturated monomer having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphoric acid group, and a cyano group (hereinafter, sometimes abbreviated as a monomer (ii)) is a monomer having both a "group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphoric acid group, and a cyano group" and an ethylenically unsaturated group in one molecule, and is not particularly limited as long as it is one that is usually used in this field. However, the monomer (i) and the monomer (ii) have different structures, and the hydroxy group in the monomer (ii) does not include a carboxy group, a sulfo group, and a phosphoric acid group (OH present in a carboxy group, a sulfo group, and a phosphoric acid group does not correspond to a hydroxy group in the monomer (ii)). Also, unlike the monomer (iii) described later, the monomer (ii) has one ethylenically unsaturated group.

[0027] The dialkylamino group in the monomer (ii) may, for example, be a dialkylamino group having 2 to 12 carbon atoms, preferably 2 to 8 carbon atoms. The two alkyl groups in the dialkylamino group may be linear, branched, or cyclic, preferably linear or branched. The two alkyl groups in the dialkylamino group may be the same or different, and the two alkyl groups may be bonded to form a heterocyclic structure. Specific examples include a dimethylamino group, a diethylamino group, a di(n-propyl)amino group, a diisopropylamino group, a di(n-butyl)amino group, a diisobutylamino group, a morpholino group, and a piperidino group.

[0028] The monomer (ii) may be a monomer having high solubility in water. Specifically, the monomer preferably has a solubility in water of 1 g / L or more at 20° C., more preferably has a solubility of 100 g / L or more, and particularly preferably is soluble in water in any proportion.

[0029] In addition, the monomer (ii) has an SP value of 11.5 (cal / cm 3 ) 1 / 2 The SP value of the monomer (ii) is not particularly limited, but is preferably 25 (cal / cm 3 ) 1 / 2 The following is preferred: The SP value (Solubility Parameter) in the present invention (first invention and second invention) is calculated according to the Fedors method, and specifically, can be determined from the following calculation formula. Calculation formula: δ=(ΔE coh / ΔV) 1 / 2 (In the above formula, δ is the SP value (cal / cm 3 ) 1 / 2 , ΔE coh is the molar cohesive energy (cal / mol), and ΔV is the molar volume (cm 3 / mol).

[0030] Examples of the ethylenically unsaturated group in the monomer (ii) include an allyl group, a vinylaryl group, a vinyloxy group, an acryloyl group, and a methacryloyl group. Of these, an acryloyl group and a methacryloyl group are preferred, and an acryloyl group is more preferred.

[0031] Examples of the monomer (ii) include monomers having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphoric acid group, and a cyano group, and having an acryloyl group or a methacryloyl group. More specifically, examples of the monomer (ii) include monomers represented by the following general formula [1]: TIFF0007587508000005.tif2555 (In general formula [1], R1 represents a hydrogen atom or a methyl group, Y1 represents -O- or -NR2-, R2 represents a hydrogen atom or a methyl group, and A1 represents a monovalent group having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group.)

[0032] R1 in the general formula [1] is preferably a hydrogen atom.

[0033] In Y1 of the general formula [1], R2 in -NR2- is preferably a hydrogen atom.

[0034] As Y1 in the general formula [1], -O- and -NH- are preferable, and -O- is more preferable.

[0035] The dialkylamino group in A1 of the general formula [1] may be the same as the dialkylamino group in the monomer (ii).

[0036] The "group selected from hydroxyl group, dialkylamino group, acetyl group, sulfo group, phosphoric acid group and cyano group" of A1 in the general formula [1] may be one or more; any one of groups selected from hydroxyl group, dialkylamino group, acetyl group, sulfo group, phosphoric acid group and cyano group is preferred; any one of groups selected from hydroxyl group, sulfo group, phosphoric acid group and cyano group is more preferred; any one of groups selected from hydroxyl group, sulfo group and phosphoric acid group is even more preferred; and a hydroxyl group is particularly preferred. A1 in the general formula [1] may have at least one "group selected from hydroxyl group, dialkylamino group, acetyl group, sulfo group, phosphoric acid group and cyano group", and among them, those having 1 to 3 groups are preferred, those having 1 to 2 groups are more preferred, and those having 1 group are particularly preferred.

[0037] An example of the "monovalent group" in A1 of the general formula [1] is an alkyl group which may have an ester bond in the chain. When the above-mentioned "alkyl group which may have an ester bond in the chain" does not have an ester bond, examples of the alkyl group include alkyl groups having 1 to 30 carbon atoms, preferably those having 1 to 10 carbon atoms, more preferably those having 1 to 6 carbon atoms, and even more preferably those having 1 to 4 carbon atoms. The alkyl group may be linear, branched, or cyclic, preferably linear or branched, and more preferably linear. When the "alkyl group which may have an ester bond in the chain" has an ester bond, for example, an alkyl group having 3 to 66 carbon atoms can be mentioned, among which an alkyl group having 3 to 36 carbon atoms is preferable, an alkyl group having 5 to 24 carbon atoms is more preferable, and an alkyl group having 7 to 18 carbon atoms is even more preferable. The number of carbon atoms in the alkyl group includes the number of carbon atoms in the ester bond. The alkyl group is preferably linear. The number of ester bonds in the alkyl group can be 1 to 10, preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 to 2.

[0038] Examples of A1 in the general formula [1] include an alkyl group having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group, and which may have an ester bond in the chain. Among these, preferred are an alkyl group having 1 to 30 carbon atoms and having 1 to 3 groups selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; and an alkyl group having 3 to 66 carbon atoms and having one hydroxy group and 1 to 10 ester bonds in the chain, more preferred are an alkyl group having 1 to 10 carbon atoms and having 1 to 3 groups selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; and a linear alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain, and even more preferred are an alkyl group having 1 to 10 carbon atoms and having 1 to 2 hydroxy groups; an alkyl group having 1 to 10 carbon atoms and having one group selected from a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; and a linear alkyl group having 5 to 24 carbon atoms and having one hydroxy group and 1 to 3 ester bonds in the chain.

[0039] Specific examples of A1 in the general formula [1] include groups represented by the following general formulas [1-1] to [1-4], and among these, the group represented by the general formula [1-1] is preferred. TIFF0007587508000006.tif5491(in general formula [1-1]~[1-4], A 1-1 and A 1-2 each independently represents an alkylene group having 1 to 10 carbon atoms, R3 represents a dialkylamino group, an acetyl group, a sulfo group, a phosphate group or a cyano group, a represents an integer of 0 to 4, b represents an integer of 1 to 5, c represents an integer of 1 to 6, d represents an integer of 3 to 5, and e represents an integer of 1 to 3.

[0040] A in the general formula [1-1] 1-1The alkylene group having 1 to 10 carbon atoms in the formula (I) is preferably one having 1 to 6 carbon atoms, and more preferably one having 1 to 4 carbon atoms. The alkylene group may be linear, branched, or cyclic, and is preferably linear or branched, and more preferably linear. Specific examples of such groups include a methylene group, an ethylene group, a methylmethylene group, a trimethylene group, a propylene group, an ethylmethylene group, a dimethylmethylene group, a tetramethylene group, a 1-methyltrimethylene group, a 2-methyltrimethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, an ethylethylene group, a propylmethylene group, an ethylmethylmethylene group, a pentamethylene group, a 1-methyltetramethylene group, a 1-ethyltrimethylene group, a n-propylethylene group, a n-butylmethylene group, a hexamethylene group, a 1-methylpentamethylene group, a 1-ethyltetramethylene group, a 1-n-propyltrimethylene group, a n-butylethylene group, a n-pentylmethylene group, a heptamethylene group, an octamethylene group, a nonamethylene group, a decamethylene group, -CH 10 - group, -CH2-C6H 10 - group, -C2H4-C6H 10 - group, -C3H6-C6H 10 - group, -C4H8-C6H 10 -group, -C6H 10 -CH2- group, -C6H 10 -C2H4- group, -C6H 10 -C3H6- group, -C6H 10 -C4H8- group, -CH2-C6H 10 -CH2- group, -C2H4-C6H 10 Among these specific examples, a linear or branched alkylene group having 1 to 6 carbon atoms and a cyclic alkylene group having 6 to 8 carbon atoms are preferred, a linear or branched alkylene group having 1 to 4 carbon atoms is more preferred, and a linear or branched alkylene group having 2 to 4 carbon atoms is even more preferred.

[0041] The dialkylamino group in R3 of the general formula [1-2] may be the same as the dialkylamino group in the monomer (ii).

[0042] Specific examples of the group represented by the general formula [1-1] include, for example, a hydroxymethyl group, a 2-hydroxyethyl group, a 1-hydroxyethyl group, a 3-hydroxypropyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, a 1-hydroxypropyl group, a 1-hydroxy-1-methylethyl group, a 4-hydroxybutyl group, a 3-hydroxybutyl group, a 3-hydroxy-2-methylpropyl group, a 3-hydroxy-1-methylpropyl group, a 2-hydroxybutyl group, a 2-hydroxy-2-methylpropyl group, a 2-hydroxy-1-methylpropyl group, a 2-hydroxy-1,1-dimethylethyl group, a 1-hydroxybutyl group, a 1-hydroxy-1-methylpropyl group, a 5-hydroxy ... -hydroxypentyl, 4-hydroxypentyl, 2-hydroxypentyl, 1-hydroxypentyl, 6-hydroxyhexyl, 5-hydroxyhexyl, 2-hydroxyhexyl, 1-hydroxyhexyl, 7-hydroxyheptyl, 6-hydroxyheptyl, 2-hydroxyheptyl, 1-hydroxyheptyl, 8-hydroxyoctyl, 7-hydroxyoctyl, 2-hydroxyoctyl, 1-hydroxyoctyl, 9-hydroxynonyl, 8-hydroxynonyl, 2-hydroxynonyl, 1-hydroxynonyl, 10-hydroxydecyl, 9-hydroxydecyl, 2-hydroxydecyl, 1-hydroxydecyl, -CH 10 -OH group, -CH2-C6H 10 -CH2-OH group, -C2H4-C6H 10 -C2H4-OH group and the like.

[0043] Among the above specific examples, linear or branched hydroxyalkyl groups having 1 to 6 carbon atoms and cyclic hydroxyalkyl groups having 6 to 8 carbon atoms are preferred, linear or branched hydroxyalkyl groups having 1 to 4 carbon atoms are more preferred, and linear or branched hydroxyalkyl groups having 2 to 4 carbon atoms are even more preferred. More specifically, hydroxymethyl groups, 2-hydroxyethyl groups, 1-hydroxyethyl groups, 3-hydroxypropyl groups, 2-hydroxypropyl groups, 2-hydroxy-1-methylethyl groups, 1-hydroxypropyl groups, 4-hydroxybutyl groups, 3-hydroxybutyl groups, 2-hydroxybutyl groups, 2-hydroxy-2-methylpropyl groups, 2-hydroxy-1-methylpropyl groups, 1-hydroxybutyl groups, 5-hydroxypentyl groups, 2-hydroxypentyl groups, 1-hydroxypentyl groups, 6-hydroxyhexyl groups, 5-hydroxyhexyl groups, 2-hydroxyhexyl groups, 1-hydroxyhexyl groups, -CH 10 -OH group, -CH2-C6H 10 Preferred is a -CH2-OH group, and more preferred is a hydroxymethyl group, a 2-hydroxyethyl group, a 1-hydroxyethyl group, a 3-hydroxypropyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, a 1-hydroxypropyl group, a 4-hydroxybutyl group, a 3-hydroxybutyl group, a 2-hydroxybutyl group, a 2-hydroxy-2-methylpropyl group, a 2-hydroxy-1-methylpropyl group, a 1-hydroxybutyl group, a 5-hydroxypentyl group, a 6-hydroxyhexyl group, a -CH2-CH 10 A -CH2-OH group is more preferred, a hydroxymethyl group, a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, a 4-hydroxybutyl group, and a 2-hydroxybutyl group are even more preferred, and a 2-hydroxyethyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, and a 4-hydroxybutyl group are particularly preferred.

[0044] A in the general formula [1-2] 1-2 As the alkylene group having 1 to 10 carbon atoms, A in the general formula [1-1] 1-1Among them, a straight-chain or branched alkylene group having 1 to 6 carbon atoms is preferred, and a straight-chain or branched alkylene group having 1 to 4 carbon atoms is more preferred.

[0045] As R3 in the general formula [1-2], a sulfo group, a phosphate group, or a cyano group is preferable, and a sulfo group or a phosphate group is more preferable.

[0046] Specific examples of the group represented by the general formula [1-2] include, for example, a dimethylaminomethyl group, a 2-(dimethylamino)ethyl group, a 3-(dimethylamino)propyl group, a 4-(dimethylamino)butyl group, a diethylaminomethyl group, a 2-(diethylamino)ethyl group, a 3-(diethylamino)propyl group, a 4-(diethylamino)butyl group, a di(n-propyl)aminomethyl group, a 2-[di(n-propyl)amino]ethyl group, a 3-[di(n-propyl)amino]propyl group, a 4-[di(n-propyl)amino]butyl group, a diisopropylaminomethyl group, a 2-(diisopropylamino)ethyl group, a 3-(diisopropylamino)propyl group, a 4-(diisopropylamino)butyl group, a di(n-butyl)aminomethyl group, a 2-[di(n-butyl)amino]ethyl group, a 3-[di(n-butyl)amino]propyl group, a 4-[di(n-butyl)amino]butyl group, a diisobutylaminomethyl group, a 2-(diisopropylamino)ethyl group, a 3-[di(n-butyl)amino]propyl group, a 4-[di(n-butyl)amino]butyl group, a diisobutylaminomethyl group, dialkylaminoalkyl groups having 3 to 12 carbon atoms, such as a 3-(diisobutylamino)ethyl group, a 3-(diisobutylamino)propyl group, a 4-(diisobutylamino)butyl group, a morpholinomethyl group, a 2-morpholinoethyl group, a 3-morpholinopropyl group, a 4-morpholinobutyl group, a piperidinomethyl group, a 2-piperidinoethyl group, a 3-piperidinopropyl group, and a 4-piperidinobutyl group; an acetomethyl group, a 2-acetoethyl group, a 3-acetopropyl group, a 4-aceto acetoalkyl groups having 3 to 6 carbon atoms, such as a butyl group, or a 1,1-dimethyl-2-acetoethyl group; sulfoalkyl groups having 1 to 6 carbon atoms, such as a sulfomethyl group, a 2-sulfoethyl group, a 1-sulfoethyl group, a 3-sulfopropyl group, a 2-sulfopropyl group, a 1-sulfopropyl group, a 4-sulfobutyl group, a 3-sulfobutyl group, a 2-sulfobutyl group, a 1,1-dimethyl-2-sulfoethylene group, a 1-sulfobutyl group, a 5-sulfopentyl group, or a 6-sulfohexyl group;Examples of the phosphonooxyalkyl groups (alkyl phosphate groups) having 1 to 6 carbon atoms include a phosphonooxymethyl group, a 2-phosphonooxyethyl group, a 1-phosphonooxyethyl group, a 3-phosphonooxypropyl group, a 2-phosphonooxypropyl group, a 1-phosphonooxypropyl group, a 4-phosphonooxybutyl group, a 3-phosphonooxybutyl group, a 2-phosphonooxybutyl group, a 1-phosphonooxybutyl group, a 5-phosphonooxypentyl group, and a 6-phosphonooxyhexyl group; and cyanoalkyl groups having 2 to 7 carbon atoms, such as a cyanomethyl group, a 2-cyanoethyl group, a 1-cyanoethyl group, a 3-cyanopropyl group, a 2-cyanopropyl group, a 1-cyanopropyl group, a 4-cyanobutyl group, a 3-cyanobutyl group, a 2-cyanobutyl group, a 1-cyanobutyl group, a 5-cyanopentyl group, and a 6-cyanohexyl group.

[0047] Among the above specific examples, a linear or branched sulfoalkyl group having 1 to 4 carbon atoms, a linear phosphonooxyalkyl group having 1 to 4 carbon atoms, and a linear cyanoalkyl group having 2 to 5 carbon atoms are preferred; a linear or branched sulfoalkyl group having 1 to 4 carbon atoms, and a linear phosphonooxyalkyl group having 1 to 4 carbon atoms are more preferred. More specifically, 2-(dimethylamino)ethyl group, 2-(diethylamino)ethyl group, 2-[di(n-propyl)amino]ethyl group, 2-(diisopropylamino)ethyl group, 2-[di(n-butyl)amino]ethyl group, 2-(diisobutylamino)ethyl group, 2-morpholinoethyl group, 2-piperidinoethyl group; acetomethyl group, 2-acetoethyl group, 1,1-dimethyl-2-acetoethyl group; sulfomethyl group, 2-sulfoethyl group, 3-sulfopropyl group, 2-sulfopropyl group, 1-sulfopropyl group, 4-sulfobutyl group, 3-sulfobutyl group, 2-sulfobutyl group, 1,1-dimethyl-2-sulfoethylene group; phosphonooxymethyl group, 2-phosphonooxyethyl group, 1-phosphonooxyethyl group, 3 Preferred are a 2-phosphonooxypropyl group, a 2-phosphonooxypropyl group, a 4-phosphonooxybutyl group; a cyanomethyl group, a 2-cyanoethyl group, a 1-cyanoethyl group, a 3-cyanopropyl group, a 1-cyanopropyl group, a 4-cyanobutyl group, and a 1-cyanobutyl group; more preferred are a sulfomethyl group, a 2-sulfoethyl group, a 3-sulfopropyl group, a 4-sulfobutyl group, and a 1,1-dimethyl-2-sulfoethylene group; a phosphonooxymethyl group, a 2-phosphonooxyethyl group, a 3-phosphonooxypropyl group, and a 4-phosphonooxybutyl group; a cyanomethyl group, a 2-cyanoethyl group, a 3-cyanopropyl group, and a 4-cyanobutyl group; and even more preferred are a 2-sulfoethyl group, a 3-sulfopropyl group, and a 2-phosphonooxyethyl group.

[0048] In the general formula [1-3], a and b are preferably an integer of 1 to 4, more preferably 1 or 2, and more preferably 1.

[0049] Specific examples of the group represented by the general formula [1-3] include, for example, a 1,2-dihydroxypropyl group, a 1,3-dihydroxypropyl group, a 2,3-dihydroxypropyl group, a 1,2-dihydroxybutyl group, a 1,3-dihydroxybutyl group, a 1,4-dihydroxybutyl group, a 2,3-dihydroxybutyl group, a 2,4-dihydroxybutyl group, a 3,4-dihydroxybutyl group, a 1,2-dihydroxypentyl group, a 1,3-dihydroxypentyl group, a 1,4-dihydroxypentyl group, a 1,5-hydroxypentyl group, a 2,3-dihydroxypentyl group, a 2,4-dihydroxypentyl group, a 2,5-hydroxypentyl group, a 3,4-dihydroxypentyl group, a 3,5-dihydroxypentyl group, a 4,5-hydroxypentyl group, a 1,2-dihydroxyhexyl group, a 1,3-dihydroxyhexyl group, a 1,4-dihydroxyhexyl group, a 1,5- ...5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a 2,5-hydroxypentyl group, a Examples of the hydroxyhexyl group include a 1,6-hydroxyhexyl group, a 2,3-dihydroxyhexyl group, a 2,4-dihydroxyhexyl group, a 2,5-hydroxyhexyl group, a 2,6-hydroxyhexyl group, a 3,4-dihydroxyhexyl group, a 3,5-dihydroxyhexyl group, a 3,6-dihydroxyhexyl group, a 4,5-hydroxyhexyl group, a 4,6-hydroxyhexyl group, and a 5,6-hydroxyhexyl group. Of these, a 2,3-dihydroxypropyl group, a 2,4-dihydroxybutyl group, a 3,4-dihydroxybutyl group, a 2,5-hydroxypentyl group, a 4,5-hydroxypentyl group, a 2,6-hydroxyhexyl group, and a 5,6-hydroxyhexyl group are preferred, a 2,3-dihydroxypropyl group, a 2,4-dihydroxybutyl group, and a 3,4-dihydroxybutyl group are more preferred, and a 2,3-dihydroxypropyl group is even more preferred.

[0050] As c in the general formula [1-4], 2 or 4 is preferable, and 2 is more preferable.

[0051] In the general formula [1-4], d is preferably 3 or 5, and more preferably 5.

[0052] In the general formula [1-4], e is preferably 1 or 2.

[0053] Specific examples of the group represented by the general formula [1-4] include the groups shown below. TIFF0007587508000007.tif93148

[0054] Among the above specific examples, the groups shown below are preferred. TIFF0007587508000008.tif48148

[0055] Among the above specific examples, the groups shown below are more preferable. TIFF0007587508000009.tif19142

[0056] Preferred specific examples of A1 in the general formula [1] include the same as the specific examples of the groups represented by the above-mentioned general formulas [1-1] to [1-4], among which are a hydroxymethyl group, a 2-hydroxyethyl group, a 1-hydroxyethyl group, a 3-hydroxypropyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, a 1-hydroxypropyl group, a 4-hydroxybutyl group, a 3-hydroxybutyl group, a 2-hydroxybutyl group, a 2-hydroxy-2-methylpropyl group, a 2-hydroxy-1-methylpropyl group, a 1-hydroxybutyl group, a 5-hydroxypentyl group, a 6-hydroxyhexyl group, -CH2-CH6H 10 -CH2-OH group; sulfomethyl group, 2-sulfoethyl group, 3-sulfopropyl group, 4-sulfobutyl group, 1,1-dimethyl-2-sulfoethylene group; phosphonooxymethyl group, 2-phosphonooxyethyl group, 3-phosphonooxypropyl group, 4-phosphonooxybutyl group; cyanomethyl group, 2-cyanoethyl group, 3-cyanopropyl group, 4-cyanobutyl group; 2,3-dihydroxypropyl group, 2,4-dihydroxybutyl group, 3,4-dihydroxybutyl group; and the groups shown below are more preferred. TIFF0007587508000010.tif20154

[0057] Among the above preferred specific examples, a hydroxymethyl group, a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, a 4-hydroxybutyl group, a 2-hydroxybutyl group, a 2-sulfoethyl group, a 3-sulfopropyl group, a 2-phosphonooxyethyl group, and a 2,3-dihydroxypropyl group are more preferred, and a 2-hydroxyethyl group, a 2-hydroxypropyl group, a 2-hydroxy-1-methylethyl group, and a 4-hydroxybutyl group are particularly preferred.

[0058] Combinations of A1, R1 and Y1 in general formula [1] include, for example, combinations 1 to 12 shown in the following table. Among these combinations, combinations 1 to 10 are preferred, combinations 1, 2, 9 and 10 are more preferred, combinations 1, 2 and 9 are even more preferred, and combination 1 is particularly preferred. TIFF0007587508000011.tif77124

[0059] A preferred specific example of the monomer represented by the general formula [1] is a monomer represented by the following general formula [2]. TIFF0007587508000012.tif2555 (In the general formula [2], A2 represents an alkyl group having 1 to 10 carbon atoms and having 1 to 3 groups selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; or a linear alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain, and R1 and Y1 are the same as above.)

[0060] Specific examples of the "alkyl group having 1 to 10 carbon atoms and having 1 to 3 of any one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group" and the "straight-chain alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain" of A2 in general formula [2] are the same as the specific examples of the groups represented by general formulas [1-1] to [1-4], and the preferred examples are also the same.

[0061] A2 in the general formula [2] is preferably an alkyl group having 1 to 10 carbon atoms and having 1 to 2 hydroxyl groups, an alkyl group having 1 to 10 carbon atoms and having one of any one of groups selected from a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group, and a linear alkyl group having 5 to 24 carbon atoms and having one hydroxyl group and 1 to 3 ester bonds in the chain, more preferably a group represented by the general formula [1-1] to [1-4], and even more preferably a group represented by the general formula [1-1]. More specifically, the same as the preferred specific examples of A1 in the general formula [1] can be mentioned, and the preferred ones are also the same.

[0062] The combinations of A2, R1 and Y1 in the general formula [2] include the same as the combinations of A1, R1 and Y1 in the general formula [1], and the preferred combinations are also the same.

[0063] Specific examples of the monomer represented by the general formula [2] include the following monomers. TIFF0007587508000013.tif121155

[0064] TIFF0007587508000014.tif123156

[0065] Among the above specific examples, hydroxymethyl acrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxybutyl acrylate, 2-(acryloyloxy)ethanesulfonic acid, 3-(acryloyloxy)ethanesulfonic acid, 2-(acryloyloxy)ethyl acid phosphate, 2,3-dihydroxypropyl acrylate, hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxy-1-methylethyl methacrylate, 4-hydroxybutyl methacrylate, 2-hydroxybutyl methacrylate, 2-(methacryloyloxy)ethanesulfonic acid, 3-(methacryloyloxy)ethanesulfonic acid, 2-(methacryloyloxy)ethyl acid phosphate, and 2,3-dihydroxypropyl methacrylate are preferred.

[0066] A more preferred example of the monomer represented by the general formula [1] is a monomer represented by the following general formula [3]. TIFF0007587508000015.tif2665 (In the general formula [3], A3 represents a linear or branched alkylene group having 1 to 4 carbon atoms, and R1 is the same as above.)

[0067] A3 in the general formula [3] is preferably a linear or branched alkylene group having 2 to 4 carbon atoms. Specific examples include a methylene group, an ethylene group, a trimethylene group, a propylene group, a tetramethylene group, and an ethylethylene group, with an ethylene group, a propylene group, and a tetramethylene group being preferred, and an ethylene group and a tetramethylene group being more preferred.

[0068] Specific examples of the monomer represented by the general formula [3] include hydroxymethyl acrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxybutyl acrylate, hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxy-1-methylethyl methacrylate, 4-hydroxybutyl methacrylate, and 2-hydroxybutyl methacrylate. Among these, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 2-hydroxy-1-methylethyl methacrylate, and 4-hydroxybutyl methacrylate are preferred, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, and 4-hydroxybutyl acrylate are more preferred, and 2-hydroxyethyl acrylate and 4-hydroxybutyl acrylate are particularly preferred.

[0069] The monomer (ii) may be used alone or in combination of two or more kinds, and it is preferable to use alone or in combination of two kinds.

[0070] In the polymer according to the first invention, the content ratio (molar ratio) of the structural unit derived from the monomer (i) to the structural unit derived from the monomer (ii) is usually (i) monomer:(ii) monomer=5:95 to 95:5, preferably 10:90 to 90:10, and more preferably 15:85 to 85:15. When two or more kinds of the monomer (i) and / or the monomer (ii) are used in combination, the ratio of the total number of moles of the structural unit derived from the monomer (i) to the total number of moles of the structural unit derived from the monomer (ii) may be the above content ratio.

[0071] The polymer according to the first invention may further contain, in addition to the monomer (i) and the monomer (ii), a structural unit derived from a monomer (iii) having two or more polymerizable unsaturated groups.

[0072] The above-mentioned (iii) monomer having two or more polymerizable unsaturated groups (hereinafter sometimes abbreviated as (iii) monomer) has a structure different from the (i) monomer and the (ii) monomer.

[0073] Specific examples of the polymerizable unsaturated group in the monomer (iii) include ethylenically unsaturated groups such as a vinyloxy group, an allyl group, a vinylaryl group, an acryloyl group, and a methacryloyl group; an isocyanate group; and a carbodiimide group. Among these, an ethylenically unsaturated group is preferred, an allyl group, an acryloyl group, and a methacryloyl group are more preferred, and an acryloyl group is particularly preferred.

[0074] Examples of the monomer (iii) include monomers represented by the following general formula

[11] or

[12] , and the monomer represented by the general formula

[11] is preferred. TIFF0007587508000016.tif2782{In general formula

[11] , R 11 represents a hydrogen atom or a methyl group, Y 11 is -O- or -NR 12 - represents R 12 represents a hydrogen atom or a methyl group, A 11 represents a group represented by the following general formulas [11-1] to [11-3], and two R 11 and two Y's 11 are equivalent to: TIFF0007587508000017.tif75156 (in general formulas [11-1] to [11-3], R 13 and R 14 each independently represents a hydrogen atom or a methyl group; Y 12 is -O- or -NR 15 - represents R 15 represents a hydrogen atom or a methyl group, A 12 ~A 15each independently represents an alkylene group having 1 to 6 carbon atoms; A 16 and A 17 each independently represents an alkylene group having 1 to 6 carbon atoms which may have an ether bond in the chain; g represents an integer of 0 to 30; h represents an integer of 1 to 3; i represents an integer of 0 to 6; j represents an integer of 1 to 3; 16 , two R 14 and two Y's 12 are the same.)

[0075] TIFF0007587508000018.tif3390(in general formula

[12] , R 16 ~R 22 each independently represents an alkylene group having 1 to 3 carbon atoms.

[0076] R in the general formula

[11] 11 is preferably a hydrogen atom.

[0077] Y in the general formula

[11] 11 In the above, -NR 12 -R in 12 is preferably a hydrogen atom.

[0078] Y in the general formula

[11] 11 As the group, -O- and -NH- are preferable, and -NH- is more preferable.

[0079] A in the general formula [11-1] 12 and A 13The alkylene group having 1 to 6 carbon atoms in the formula (I) is preferably one having 1 to 4 carbon atoms, and more preferably one having 2 to 3 carbon atoms. The alkylene group may be linear, branched, or cyclic, and is preferably linear or branched, and more preferably linear. Specific examples of such groups include a methylene group, an ethylene group, a methylmethylene group, a trimethylene group, a propylene group, an ethylmethylene group, a dimethylmethylene group, a tetramethylene group, a 1-methyltrimethylene group, a 2-methyltrimethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, an ethylethylene group, a propylmethylene group, an ethylmethylmethylene group, a pentamethylene group, a 1-methyltetramethylene group, a 1-ethyltrimethylene group, a n-propylethylene group, a n-butylmethylene group, a hexamethylene group, a 1-methylpentamethylene group, a 1-ethyltetramethylene group, a 1-n-propyltrimethylene group, a n-butylethylene group, a n-pentylmethylene group, -CH 10 Among them, a linear or branched alkylene group having 1 to 4 carbon atoms is preferred, and a methylene group, an ethylene group, a trimethylene group, a propylene group, or a tetramethylene group is more preferred.

[0080] In the general formula [11-1], the g repeating units may be the same or different, and it is preferable that all of the g repeating units are the same. 13 may be the same or different. When g in the general formula [11-1] is an integer of 1 or more, A 12 and A in the gth repeating unit 13 and are preferably identical; 12 and A in the gth repeating unit 13 and A in the 1st to g-1th repeating units are the same. 13 It is more preferable that all of the repeating units in the general formula [11-1] are the same. 12 The gth repeating unit is counted from the side adjacent to A, and the gth repeating unit is A. 12 The one located furthest from the 11 (one adjacent to the other).

[0081] As g in the general formula [11-1], an integer of 0 to 15 is preferable, an integer of 0 to 10 is more preferable, and an integer of 0 to 3 is even more preferable.

[0082] A in the general formula [11-1] 12 , A 13 Examples of the combinations of and g include combinations 1 to 29 in the table below. Among these combinations, combinations 1, 2, 7 to 13, 15, 17 to 19, 24, and 25 are preferred, and combinations 1, 7 to 10, 12, 15, 17, 18, and 24 are more preferred. TIFF0007587508000019.tif202148

[0083] In the general formula [11-2], the repeating units may be the same or different, and it is preferable that all of the repeating units are the same. 13 may be the same or different, and all R 13 are preferably the same, and all R 13 R in the general formula

[11] 11 It is more preferable that it is the same as

[0084] A in the general formula [11-2] 14 and A 15 As the alkylene group having 1 to 6 carbon atoms, A in the general formula [11-1] 12 and A 13 Among them, a linear alkylene group having 1 to 4 carbon atoms is preferred, and an ethylene group is more preferred.

[0085] h A's in the general formula [11-2] 15 may be the same or different, and all A 15 In addition, A in the general formula [11-2] is preferably the same. 14 and A in the h-th repeating unit 15 and are preferably identical, and A 14 and A in all repeat units 15It is more preferable that the repeating unit in the general formula [11-2] is the same as A 14 The h-th repeating unit is counted from the side adjacent to A, and the h-th repeating unit is A. 14 The one located furthest from the 11 (one adjacent to the other).

[0086] In the general formula [11-2], e is preferably 1 or 2.

[0087] A in the general formula [11-2] 14 , A 15 , R 13 Examples of the combinations of and h include combinations 1 to 12 shown in the following table. Among these combinations, combinations 4 to 6 are preferred, and combinations 4 and 5 are more preferred. TIFF0007587508000020.tif74148

[0088] In the general formula [11-3], the j repeating units may be the same or different, and it is preferable that all of the repeating units are the same. 14 may be the same or different, and all R 14 are preferably the same, and all R 14 R in the general formula

[11] 11 However, it is more preferable that two R 14 are always identical.

[0089] Y in the general formula [11-3] 12 In the above, -NR 15 -R in 15 is preferably a hydrogen atom.

[0090] 2j Y in the general formula [11-3] 12 may be the same or different, and all Y 12 are preferably the same, and all Y 12 is the general formula

[11] Y 11However, it is more preferable that two Y present in the same repeating unit are the same as 12 are always identical.

[0091] A in the general formula [11-3] 16 and A 17 Specific examples of the "alkylene group having 1 to 6 carbon atoms which may have an ether bond in the chain" having no ether bond include A in the general formula [11-1]: 12 and A 13 Among them, a linear alkylene group having 1 to 4 carbon atoms is preferred, and a methylene group is more preferred.

[0092] A in the general formula [11-3] 16 and A 17 Specific examples of the "alkylene group having 1 to 6 carbon atoms which may have an ether bond in the chain" having an ether bond include -CH2-O-CH2-, -CH2-O-(CH2)2-, -CH2-O-(CH2)3-, -CH2-O-(CH2)4-, -CH2-O-(CH2)5-, -(CH2)2-O-CH2-, -(CH2)2-O-(CH2)2-, -(CH2)2-O-(CH2)3-, -(CH2) Examples include 2-O-(CH2)4-, -(CH2)3-O-CH2-, -(CH2)3-O-(CH2)2-, -(CH2)3-O-(CH2)3-, -(CH2)4-O-CH2-, -(CH2)4-O-(CH2)2- and -(CH2)5-O-CH2-. Of these, a straight-chain alkylene group having 2 to 4 carbon atoms and an ether bond in the chain is preferred, and -CH2-O-CH2- and -CH2-O-(CH2)3- are more preferred.

[0093] 2j A in the general formula [11-3] 16 and j A's 17 may be the same or different, provided that two A present in the same repeating unit 16 In addition, all A in the general formula [11-3] 16 and A in the jth repeating unit 17It is preferable that the repeating unit in the general formula [11-3] is the same as -(CH2) i Counting from the side adjacent to -, the jth repeating unit is -(CH2) i - (Y in general formula

[11] ) 11 (one adjacent to the other).

[0094] As i in the general formula [11-3], an integer of 0 to 4 is preferable, 0 or 1 is more preferable, and 0 is even more preferable.

[0095] In the general formula [11-3], j is preferably 1 or 2, and more preferably 1.

[0096] The two A's in the general formula [11-3] 16 , A 17 , two Y's 12 , two R 14 Examples of the combinations of i, j include combinations 1 to 20 shown in the table below. Among these combinations, combinations 1 to 6 and 11 to 16 are preferred, combinations 1, 2, 11, 12, 13 and 14 are more preferred, and combinations 1, 11 and 13 are particularly preferred. 16 In the formula, "-CH2-O-(CH2)3-" is attached to the main chain at the left end and to Y at the right end. 12 is assumed to be bound to TIFF0007587508000021.tif127156

[0097] A in the general formula

[11] 11 , two Y's 11 and two R 11 Examples of the combinations include combinations 1 to 14 in the table below. TIFF0007587508000022.tif90132

[0098] R in the general formula

[12] 16 ~R 22The alkylene group having 1 to 3 carbon atoms in the formula (I) may be linear or branched, with linear being preferred. Specific examples include methylene, ethylene, methylmethylene, trimethylene, propylene, ethylmethylene and dimethylmethylene groups, with methylene, ethylene and trimethylene groups being preferred, methylene and trimethylene groups being more preferred, and methylene being particularly preferred.

[0099] R in the general formula

[12] 16 ~R 22 may be the same or different, R 17 ~R 19 and R 20 ~R 22 are preferably the same, and R 16 ~R 22 are preferably all identical.

[0100] R in the general formula

[12] 16 ~R 22 Examples of the combinations include combinations 1 to 27 shown in the table below. Among these combinations, combinations 1 to 3 are preferred, combinations 1 and 3 are more preferred, and combination 1 is particularly preferred. TIFF0007587508000023.tif155117

[0101] Specific examples of the monomers represented by the general formulae

[11] and

[12] include the following monomers. TIFF0007587508000024.tif191155

[0102] TIFF0007587508000025.tif196155

[0103] TIFF0007587508000026.tif32122

[0104] Among the above specific examples, the following monomers are preferred. TIFF0007587508000027.tif113156

[0105] TIFF0007587508000028.tif137156

[0106] Among the above-mentioned preferred specific examples, methylene diacrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylene diacrylate, propylene diacrylate, tetramethylene diacrylate, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, N,N'-(4,7,10-trioxytridecamethylene)bisacrylamide, N,N',N''-triacryloyldiethylenetriamine, N,N',N'',N'''-tetraacryloyltriethylenetetramine, N-[tris(3-acrylamidopropoxymethyl)methyl]acrylamide, methylene dimethacrylate, ethylene More preferred are ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylene dimethacrylate, propylene dimethacrylate, tetramethylene dimethacrylate, N,N'-methylene bismethacrylamide, N,N'-ethylene bismethacrylamide, N,N'-(4,7,10-trioxytridecamethylene) bismethacrylamide, N,N',N''-trimethacryloyl diethylene triamine, N,N',N'',N''''-tetramethacryloyl triethylene tetramine, N-[tris(3-methacrylamidopropoxymethyl)methyl]methacrylamide, and pentaerythritol triallyl ether. These more preferred specific examples are hereinafter referred to as "more preferred specific examples of the monomer (iii)".

[0107] In addition to the specific examples described above, the monomer (iii) may be any monomer commonly used in this field as a "crosslinking agent." For example, the crosslinking agents described in WO 2014 / 065407, WO 2015 / 163302, WO 2018 / 143382, WO 2018 / 143383, etc. may be used.

[0108] When the polymer according to the first invention contains a structural unit derived from the monomer (iii), the content thereof is usually from 0.01 mol% to 5 mol%, preferably from 0.05 mol% to 2 mol%, and more preferably from 0.1 mol% to 1 mol%, based on the total content of the structural units derived from the monomer (i) and the monomer (ii).

[0109] The monomers (i), (ii) and (iii) may each be a commercially available product or may be appropriately synthesized by a method known per se.

[0110] The polymer according to the first invention may appropriately contain structural units derived from monomers generally used in this field (hereinafter, sometimes abbreviated as other monomers) in addition to the monomers (i), (ii), and (iii). When the polymer according to the first invention contains structural units derived from other monomers, the content thereof is usually 0.01 mol% or more and 5 mol% or less, preferably 0.05 mol% or more and 2 mol% or less, more preferably 0.1 mol% or more and 1 mol% or less, based on the total content of the structural units derived from the monomers (i) and (ii).

[0111] The polymer according to the first invention may contain two or more types of structural units derived from the monomer (i), the monomer (ii), and the monomer (iii).

[0112] The polymer according to the first invention is preferably a polymer comprising structural units derived from one monomer of (i) and one or two monomers of (ii); or a polymer comprising structural units derived from one monomer of (i), one or two monomers of (ii), and one monomer of (iii), and more preferably a polymer comprising structural units derived from one monomer of (i) and one or two monomers of (ii) having a solubility in water at 20° C. of 1 g / L or more at 20° C. ... 3 ) 1 / 2a polymer comprising structural units derived from one or two kinds of monomers having a solubility in water of 1 g / L or more at 20° C.; a polymer comprising structural units derived from one kind of monomer (i), one or two kinds of monomers among (ii) having a solubility in water of 1 g / L or more at 20° C., and one kind of monomer (iii); or a polymer comprising structural units derived from one kind of monomer (i) and one or two kinds of monomers among (ii) having a SP value of 11.5 (cal / cm 3 ) 1 / 2 A polymer comprising structural units derived from one or two of the above monomers and one type of monomer (iii) is more preferred.

[0113] More specifically, a polymer consisting of structural units derived from one ethylenically unsaturated monocarboxylic acid monomer and one or two monomers represented by the general formula [1]; or a polymer consisting of structural units derived from one ethylenically unsaturated monocarboxylic acid monomer, one or two monomers represented by the general formula [1], and one monomer represented by the general formula

[11] is preferred, and a polymer consisting of structural units derived from one ethylenically unsaturated monocarboxylic acid monomer and one or two monomers represented by the general formula [2]; or A polymer consisting of structural units derived from one kind of carboxylic unsaturated monocarboxylic acid monomer, one or two kinds of monomers represented by the general formula [2], and one kind of monomer represented by the general formula

[11] is more preferred, and a polymer consisting of structural units derived from one kind of acrylic acid or methacrylic acid, and one or two kinds of monomers represented by the general formula [3]; or a polymer consisting of structural units derived from one kind of acrylic acid or methacrylic acid, one or two kinds of monomers represented by the general formula [3], and one kind of monomer represented by the general formula

[11] is even more preferred.

[0114] More specifically, preferred are polymers consisting of structural units derived from one of acrylic acid or methacrylic acid, and one or two selected from 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, and 4-hydroxybutyl acrylate; or polymers consisting of structural units derived from one of acrylic acid or methacrylic acid, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxy-1-methylethyl acrylate, and 4-hydroxybutyl acrylate, and one selected from the more preferred specific examples of the monomer (iii), and more preferred are polymers consisting of structural units derived from one of acrylic acid and 2-hydroxyethyl acrylate and / or 4-hydroxybutyl acrylate; or polymers consisting of structural units derived from one of acrylic acid, 2-hydroxyethyl acrylate and / or 4-hydroxybutyl acrylate, and one selected from the more preferred specific examples of the monomer (iii).

[0115] When the polymer according to the first invention is neutralized (forms a salt), it is preferable that the carboxyl group in the structural unit derived from the monomer (i) and / or the sulfo group or phosphate group in the structural unit derived from the monomer (ii) are partially or completely neutralized. In addition, examples of the neutralizing agent used when neutralizing the polymer according to the first invention include inorganic bases such as hydroxides, carbonates, and hydrogencarbonates of alkali metals or alkaline earth metals; and organic bases such as polyamines having an amine value of 21 or more, ammonium salts, aliphatic phosphines, aromatic phosphines, phosphonium salts, aliphatic thiols, aromatic thiols, thiol derivatives, and sulfonium salts. Specific examples of the hydroxides include alkali metals such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; carbonates of alkali metals such as sodium carbonate, lithium carbonate, and potassium carbonate; hydrogen carbonates of alkali metals such as lithium hydrogen carbonate, sodium hydrogen carbonate, and potassium hydrogen carbonate; hydroxides of alkaline earth metals such as magnesium hydroxide and calcium hydroxide; carbonates of alkaline earth metals such as magnesium carbonate and calcium carbonate; polyamines having an amine value of 21 or more, such as ethylenediamine, 1,2-propanediamine, N-methyl-1,3-propanediamine, bis(2-aminoethyl)amine, tris(2-aminoethyl)amine, and polyethyleneimine; Examples of the ammonium salts include tetrabutylammonium tetrafluoroborate, hexadecyltrimethylammonium hexafluorophosphate, etc.; aliphatic phosphines such as trimethylphosphine; aromatic phosphines such as triphenylphosphine; phosphonium salts such as tetraethylphosphonium hexafluorophosphate, 1H-benzotriazol-1-yloxytris(dimethylamino)phosphonium hexafluorophosphate, 1H-benzotriazol-1-yloxytris(dimethylamino)phosphonium hexafluorophosphate, etc.; aliphatic thiols such as 1-butanethiol; aromatic thiols such as phenylmethanethiol, thiophene, etc.; thiol derivatives such as 2-hydroxyethyl mercaptan, etc.; and sulfonium salts such as 1,3-benzodithiolylium tetrafluoroborate, dimethylphenacylsulfonium tetrafluoroborate, etc.Among these specific examples, alkali metal hydroxides and polyvalent amines having an amine value of 21 or more are preferred, sodium hydroxide, lithium hydroxide, potassium hydroxide, ethylenediamine, 1,2-propanediamine, N-methyl-1,3-propanediamine, tris(2-aminoethyl)amine, and polyethyleneimine are more preferred, and sodium hydroxide and polyethyleneimine are particularly preferred. The neutralizing agent may be used alone or in combination of two or more, and it is preferred to use one alone or two in combination. In particular, it is preferred to use one alkali metal hydroxide alone; or to use one alkali metal hydroxide in combination with one polyvalent amine having an amine value of 21 or more.

[0116] The above-mentioned "polyamine with an amine value of 21 or more" refers to a polyamine having two or more basic functional groups such as amino groups, and an amine value indicating the amount of basic functional groups in the structure is 21 or more. The amine value in the present invention (first invention and second invention) can be specifically calculated from the calculation formula shown below. The basic functional group in the present invention (first invention and second invention) refers to a functional group exhibiting basicity, such as an amino group, an amidino group (amidine structure), a guanidino group (guanidine structure), a pyridino group (pyridine structure), or a phosphazeno group (phosphazene structure). Calculation formula: Amine value (meq. / g) = Number of basic functional groups / Molecular weight (However, in the case of a high molecular weight substance, the above molecular weight is calculated as the molecular weight per monomer unit, and the above number of basic functional groups is calculated as the number of basic functional groups per monomer unit.)

[0117] When the polymer according to the first invention is neutralized, the degree of neutralization is usually 50% or more and 200% or less, preferably 60% or more and 150% or less, and more preferably 70% or more and 100% or less. The degree of neutralization here refers to the ratio of the total number of moles of the neutralizer to the total number of moles of the carboxyl group, sulfo group, and phosphate group contained in the polymer according to the first invention. When the binder according to the first invention contains a salt of the polymer according to the first invention, the dispersibility of the conductive assistant is further improved, and the conductive assistant can be distributed more uniformly on the current collector, which makes it possible to further improve the electrical properties of the electrode.

[0118] The polymer according to the first invention may be produced by carrying out a polymerization reaction according to a method known per se. Specifically, for example, the polymer may be produced by polymerizing the monomer (i) and the monomer (ii), and optionally the monomer (iii) and / or other monomers, in accordance with the desired polymer, in the presence of a polymerization initiator.

[0119] The amounts of the monomer (i) and the monomer (ii) used in the polymerization reaction may be appropriately set according to the content ratio (molar ratio) of the structural unit derived from the monomer (i) and the structural unit derived from the monomer (ii) in the polymer according to the first invention. The amounts of the monomer (iii) and / or other monomers used in the polymerization reaction may be appropriately set according to the content when the polymer according to the first invention contains the structural unit derived from the monomer (iii) and / or other monomers.

[0120] The polymerization reaction may be carried out in accordance with a method known per se. Specifically, the reaction may be carried out in a suitable solvent at a temperature of usually 30° C. or higher and 200° C. or lower, preferably 60° C. or higher and 150° C. or lower, and more preferably 70° C. or higher and 100° C. or lower, for usually 0.1 hours or longer and 24 hours or shorter, and preferably 1 hour or longer and 10 hours or shorter.

[0121] The polymerization initiator is not particularly limited as long as it is one that is usually used in this field, and specific examples thereof include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylpropionate), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], ammonium persulfate (ammonium peroxodisulfate), potassium persulfate (potassium peroxodisulfate), benzoyl peroxide, lauroyl peroxide, and the like. These may be used alone or in combination of two or more. The amount of the polymerization initiator used is usually 0.001 mol % or more and 30 mol % or less based on the total mass of the reactants.

[0122] The above-mentioned solvent is not particularly limited as long as it is one that is usually used in this field, and specifically includes, for example, water, methanol, N-methyl-2-pyrrolidone (NMP), toluene, 1,4-dioxane, tetrahydrofuran, isopropanol, methyl ethyl ketone, propylene glycol monomethyl ether acetate, etc., among which water is preferred. These may be used alone or in combination of two or more. The amount of the solvent used is 1 time (equivalent amount) or more and 20 times or less of the total mass of the reactants.

[0123] The product obtained after the polymerization reaction may be subjected to general post-treatment and purification procedures usually performed in this field, as necessary, such as filtration, washing, extraction, vacuum concentration, recrystallization, distillation, column chromatography, etc.

[0124] When the polymer according to the first invention is neutralized, the polymer according to the first invention obtained by the above polymerization reaction may be neutralized according to a method known per se. Specifically, for example, the neutralization may be performed by adding the neutralizing agent in an amount that allows the polymer according to the first invention to have a desired degree of neutralization. The solvent used in neutralization may be the same as the solvent used in the above polymerization reaction.

[0125] Specifically, the polymer or salt thereof according to the first aspect of the present invention is produced as follows. That is, the monomer (i) and the monomer (ii) in a molar ratio of 5:95 to 95:5, and optionally the monomer (iii) and / or other monomers in an amount of 0.01 mol% to 5 mol% based on the content of the structural units derived from the monomer (i) and the monomer (ii), are dissolved or dispersed in a solvent such as water in an amount equal to or greater than 20 times the total mass of the reactants in the presence of a polymerization initiator such as 2,2'-azobis(isobutyronitrile) in an amount of 0.001 mol% to 30 mol% based on the total mass of the reactants. Then, a polymerization reaction is carried out at 30°C to 200°C for 0.1 to 24 hours to produce a polymer according to the first invention. If necessary, the above neutralizing agent may be added in an amount such that the obtained polymer according to the first invention has a desired degree of neutralization, to form a salt of the polymer according to the first invention.

[0126] [Binder solution] The binder of the first invention may be dissolved in a solvent and contained in the slurry composition of the first invention or the electrode of the first invention, which will be described later. In the first invention, the binder dissolved in a solvent is called a "binder solution", and in particular, the binder of the first invention dissolved in a solvent is called the "binder solution according to the first invention".

[0127] The solvent in the binder solution according to the first invention is not particularly limited as long as it is one that is usually used in this field, and specifically includes, for example, water, N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, methylformamide, dimethylsulfoxide, acetonitrile, tetrahydrofuran, γ-butyrolactone, toluene, methyl ethyl ketone, ethyl acetate, dioxane, etc., and among them, water is preferred. These may be used alone or in combination of two or more, and it is preferable to use only one type alone. In addition, when the solvent is water, it may be called "aqueous binder solution according to the first invention".

[0128] The content (mass of solids) of the binder of the first invention in the binder solution of the first invention may be appropriately set according to the desired concentration of the binder solution of the first invention, and is usually from 1 mass % to 70 mass %, preferably from 5 mass % to 50 mass %.

[0129] The binder solution according to the first invention may contain various additives generally used in this field in addition to the binder and solvent of the first invention. For example, dispersants, thickeners, metal binders (e.g., aminotriazole, etc.), reducing agents (e.g., ascorbic acid, etc.), preservatives (e.g., cetylpyridinium chloride, etc.), rust inhibitors, antifungal agents, antibacterial agents, deodorants, leveling agents, defoamers, blister inhibitors, yellowing inhibitors, antistatic agents, charge regulators, electrolyte decomposition inhibitors, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, thixotropic agents, freeze stabilizers, pH adjusters, lubricants, rheology control agents, film-forming assistants, etc. may be mentioned. These may be used alone or in combination of two or more types depending on the purpose. The content of various additives in the binder solution according to the first invention is usually 10% by mass or less, preferably 5% by mass or less, more preferably 1% by mass or less, based on the content of the binder of the first invention.

[0130] [Slurry composition of the first invention] The slurry composition of the first invention is a composition for producing an electrode for an electricity storage device, containing the binder of the first invention. More specifically, it is a composition containing an active material and a solvent, and optionally a conductive assistant, in addition to the binder of the first invention (or the binder solution according to the first invention). The slurry composition of the first invention may be for producing either a positive electrode or a negative electrode, but is preferably for producing a negative electrode.

[0131] The content of the binder of the first invention in the slurry composition of the first invention is usually 0.1 mass % or more and 30 mass % or less, preferably 0.5 mass % or more and 20 mass % or less, and more preferably 1 mass % or more and 10 mass % or less, based on the total mass of the slurry composition of the first invention not including the solvent.

[0132] The active material in the slurry composition of the first invention is not particularly limited as long as it is one that is usually used in this field, and specifically includes, for example, carbon, silicon, germanium, tin, lead, zinc, aluminum, indium, antimony, bismuth, sodium, magnesium, titanium, compounds containing these elements (oxides, etc.), and among them, carbon, silicon, or compounds containing silicon as an element are preferred. These may be used alone or in combination of two or more.

[0133] Examples of the carbon include graphite-based carbon materials (graphite) such as natural graphite, artificial graphite, and expanded graphite, carbon black, activated carbon, carbon fiber, coke, soft carbon, and hard carbon. Among these specific examples, graphite such as natural graphite, artificial graphite, and expanded graphite is preferred. Examples of the natural graphite include flake graphite and lump graphite. Examples of the artificial graphite include lump graphite, vapor-grown graphite, flake graphite, and fibrous graphite.

[0134] Examples of the silicon or compounds containing silicon as an element include silicon, silicon oxides such as SiO and SiO2, silicon bonded to a metal SiM (M represents a metal such as magnesium, iron, calcium, cobalt, nickel, boron, copper, manganese, silver, vanadium, cerium, zinc, etc.), and among these, silicon and silicon oxide are preferred, and silicon is more preferred. Also, the silicon may be one whose surface is partially or entirely covered (coated) with carbon, and examples thereof include carbon-coated silicon, silicon oxide, silicon bonded to a metal, and among these, carbon-coated silicon and silicon oxide are preferred, and carbon-coated silicon oxide is more preferred.

[0135] The active material in the slurry composition of the first invention preferably contains one or more of the above carbons and / or one or more of the above silicon or compounds containing silicon as an element, and more preferably contains one or more of the above carbons and one or more of the above silicon or compounds containing silicon as an element. More specifically, the active material may contain a mixture of at least one selected from natural graphite, artificial graphite, or expanded graphite with at least one selected from silicon, silicon oxide, carbon-coated silicon, or carbon-coated silicon oxide, and an active material containing natural graphite and carbon-coated silicon oxide is preferred.

[0136] The average particle size of the active material in the slurry composition of the first invention varies depending on the type of active material used, but is usually 0.001 μm to 100 μm, preferably 0.01 μm to 50 μm, and more preferably 0.1 μm to 30 μm.

[0137] The content of the active material in the slurry composition of the first invention is usually 30 mass% or more and 99.9 mass% or less, preferably 40 mass% or more and 99 mass% or less, and preferably 50 mass% or more and 98 mass% or less, based on the total mass of the slurry composition of the first invention not including the solvent.

[0138] The conductive assistant in the slurry composition of the first invention is not particularly limited as long as it is one that is usually used in this field, and specifically includes, for example, carbon black such as acetylene black, ketjen black, furnace black, and thermal black; nanocarbon such as carbon nanotube and carbon nanohorn; among them, acetylene black and ketjen black are preferable, and acetylene black is more preferable. These may be used alone or in combination of two or more.

[0139] The average particle size of the conductive assistant in the slurry composition of the first invention varies depending on the type of conductive assistant used, but is usually 0.001 μm or more and 50 μm or less, preferably 0.01 μm or more and 10 μm or less, and more preferably 0.02 μm or more and 1 μm or less.

[0140] The content of the conductive assistant in the slurry composition of the first invention is usually 0.1 mass% or more and 40 mass% or less, preferably 0.5 mass% or more and 30 mass% or less, and preferably 1 mass% or more and 20 mass% or less, based on the total mass of the slurry composition of the first invention not including the solvent.

[0141] The solvent in the slurry composition of the first invention is not particularly limited as long as it is one that is usually used in this field, and specifically includes, for example, water, N-methyl-2-pyrrolidone (NMP), dimethylformamide, dimethylacetamide, methylformamide, dimethylsulfoxide, acetonitrile, tetrahydrofuran, γ-butyrolactone, toluene, methyl ethyl ketone, ethyl acetate, dioxane, etc., and water is preferred. These may be used alone or in combination of two or more, and it is preferable to use only one. In addition, when the binder of the first invention is contained in the slurry composition of the first invention in the form of a binder solution, it is preferable that the solvent in the slurry composition of the first invention is the same as the solvent in the binder solution according to the first invention.

[0142] The slurry composition of the first invention may contain, in addition to the binder, active material, conductive assistant and solvent of the first invention, supporting salts, additives and the like that are generally used in this field. Examples of the supporting salt include Li(C2F5SO2)2N(LiBETI), LiPF6, LiBF4, LiClO4, LiAsF6, and LiCF3SO3. Examples of the additives include dispersants, thickeners, metal binders, reducing agents, preservatives, rust inhibitors, antifungal agents, antibacterial agents, deodorants, leveling agents, defoamers, blister inhibitors, yellowing inhibitors, antistatic agents, charge regulators, electrolyte decomposition inhibitors, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, thixotropic agents, freeze stabilizers, pH adjusters, lubricants, rheology control agents, and film-forming assistants. These may be used alone or in combination of two or more depending on the purpose. The content of the supporting salt and the additives may be appropriately set according to the amount usually used in this field.

[0143] The slurry composition of the first invention may be prepared in accordance with a method known per se. Specifically, for example, the slurry composition may be prepared by appropriately mixing the binder of the first invention, the active material, and, if necessary, the conductive assistant, the supporting salt and / or the additive in the solvent in the above-mentioned contents according to the desired slurry composition.

[0144] [Electrode of the first invention] The electrode of the first invention is an electrode for an electricity storage device, which is made of the slurry composition of the first invention. More specifically, it has an electrode mixture layer derived from the slurry composition of the first invention, which contains the binder of the first invention (or the binder solution according to the first invention), an active material, a solvent, and optionally a conductive assistant, a supporting salt and / or an additive, and a current collector. The electrode of the first invention can be used as either a negative electrode or a positive electrode, but is preferably used as a positive electrode.

[0145] The current collector in the electrode of the first invention is not particularly limited as long as it is one that is usually used in this field, and specifically, for example, it is made of a conductive material such as platinum, copper, stainless steel (SUS), Hastelloy, aluminum, iron, chromium, nickel, titanium, Inconel, molybdenum, graphite, carbon, etc., and has a shape such as a plate, foil (sheet, paper), mesh, expanded grid (expanded metal), punched metal, etc. are listed. The mesh opening, wire diameter, mesh number, etc. of the current collector are not particularly limited, and a conventionally known one can be used. The thickness of the current collector is usually 1 μm or more and 300 μm or less, preferably 5 μm or more and 30 μm or less. The size of the current collector is determined according to the use of the battery. If a large electrode to be used in a large battery is to be produced, a current collector with a large area is used, and if a small electrode is to be produced, a current collector with a small area is used.

[0146] The electrode of the first invention may be produced according to a method known per se, specifically, for example, by applying or pressing the slurry composition of the first invention onto a current collector and drying it to form an electrode mixture layer on the current collector. The thickness of the electrode mixture layer is usually 1 μm or more and 1000 μm or less, preferably 1 μm or more and 500 μm or less, and more preferably 1 μm or more and 300 μm or less.

[0147] In the manufacture of the electrode of the first invention, the amount of the slurry composition of the first invention used may be appropriately set so that the thickness of the electrode mixture layer after drying falls within the above-mentioned range.

[0148] In the manufacture of the electrode of the first invention, the application or pressure bonding of the slurry composition of the first invention onto a current collector may be performed in accordance with a method known per se, and specific examples of the application or pressure bonding method include a self-propelled coater, an inkjet method, a doctor blade method, a spray method, a die coating method, or a combination of these. Among these specific examples, the doctor blade method, the inkjet method, and the die coating method, which can form a thin layer, are preferred, and the doctor blade method and the die coating method are more preferred.

[0149] In the manufacture of the electrode of the first invention, the slurry composition of the first invention may be dried according to a method known per se, and is usually performed by a heat treatment. The drying conditions during heating (whether or not a vacuum is required, drying time, drying temperature) may be appropriately set according to the coating amount of the slurry composition of the first invention and the evaporation rate of the solvent in the slurry composition of the first invention. A specific drying method may be, for example, drying in air or in a vacuum, usually at 50°C to 400°C, preferably 70°C to 200°C, usually for 1 hour to 20 hours, preferably 3 hours to 15 hours. In addition, the heating treatment may be performed two or more times by changing the drying conditions.

[0150] In the production of the electrode of the first invention, a pressing treatment may be carried out before or after the drying, if necessary. The pressing treatment may be carried out in accordance with a method known per se, and specific examples of the pressing treatment method include a calendar roll method and a flat plate press, with the calendar roll method being preferred.

[0151] [Electricity storage device of the first invention] The electricity storage device of the first invention refers to a device or element that has the electrode of the first invention and can store electricity chemically, physically, or physicochemically, and specific examples include devices that can be charged and discharged, such as secondary batteries (storage batteries) such as multivalent ion secondary batteries such as magnesium ions, lithium ion secondary batteries, sodium ion secondary batteries, potassium ion secondary batteries, nickel hydrogen storage batteries, nickel cadmium storage batteries, lead storage batteries, and electric double layer capacitors (electric double layer capacitors) such as lithium ion capacitors. Among these specific examples, electricity storage devices using lithium ions such as lithium ion capacitors and lithium ion secondary batteries are preferred, and lithium ion secondary batteries are more preferred.

[0152] The configuration of the electricity storage device of the first invention may be the same as that of a general electricity storage device usually used in this field, specifically, for example, a positive electrode and a negative electrode are arranged opposite each other with a separator interposed therebetween, and if necessary, are impregnated with an electrolyte solution. The electricity storage device of the first invention may be any device that includes the electrodes of the first invention as the positive electrode and / or negative electrode, and as members constituting the electricity storage device of the first invention other than the electrodes of the first invention, members usually commonly used in this field may be appropriately adopted.

[0153] The separator in the electricity storage device of the first invention may be any material that electrically insulates the positive and negative electrodes while allowing ions to pass through, and examples of such materials include microporous polymers such as glass fibers and porous polyolefins. Specific examples of such porous polyolefins include porous polyethylene, porous polypropylene, and a multilayer structure in which porous polyethylene and porous polypropylene are stacked together.

[0154] The electrolyte in the electricity storage device of the first invention is preferably a non-aqueous electrolyte containing an electrolyte, an organic solvent and an additive. The electrolyte varies depending on the desired electricity storage device. For example, in the case of a lithium ion secondary battery, lithium salts such as LiBF4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiCl, LiBr, LiClO4, LiBrO4, LiIO4, LiCH3SO3, and LiCF3SO3 are listed, and LiPF6 is preferred. These may be used alone or in combination of two or more. The content of the electrolyte in the non-aqueous electrolyte is usually 0.05 mol / L or more and 15 mol / L or less, and preferably 0.1 mol / L or more and 5 mol / L or less.

[0155] Specific examples of the organic solvent in the non-aqueous electrolyte include ethylene carbonate, dimethyl carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone (lactones), sulfolane, etc., and among these, ethylene carbonate, ethyl methyl carbonate, diethyl carbonate, and dimethyl carbonate are preferred. These may be used alone or in combination of two or more.

[0156] Specific examples of additives in the non-aqueous electrolyte include vinylene carbonate, fluorovinylene carbonate, methylvinylene carbonate, fluoromethylvinylene carbonate, ethylvinylene carbonate, propylvinylene carbonate, butylvinylene carbonade, dipropylvinylene carbonate, 4,5-dimethylvinylene carbonate, 4,5-diethylvinylene carbonate, vinylethylene carbonate, divinylethylene carbonate, phenylethylene carbonate, diallyl carbonate, fluoroethylene carbonate, catechol carbonate, 1,3-propane sultone, butane sultone, and the like. Among these, vinylene carbonate and fluoroethylene carbonate are preferred. These may be used alone or in combination of two or more. The content of additives in the non-aqueous electrolyte is usually 0.05% by mass or more and 15% by mass or less, and preferably 0.1% by mass or more and 5% by mass or less.

[0157] The nonaqueous electrolyte in the electricity storage device of the first invention may contain, in addition to the electrolyte and the organic solvent, additives typically used in this field, such as a film-forming agent, an overcharge inhibitor, an oxygen scavenger, a dehydrating agent, and a flame retardant, as well as coordinating additives such as crown ether.

[0158] The shape of the electricity storage device of the first invention is not particularly limited, and the internal shape may be a wound type, a laminated type, etc., and the external shape may be a coin type, a laminated type (pouch type), a square type, a cylindrical type, etc., and any other shapes that are generally used in this field may be appropriately adopted.

[0159] [Binder of the second invention] The binder according to the second invention contains (i) an ethylenically unsaturated carboxylic acid monomer, and (ii) a structural unit derived from an ethylenically unsaturated monomer having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group, and contains a salt of a polymer neutralized with a monoamine, a polyamine having an amine value of less than 21, and / or an onium hydroxide (hereinafter, may be abbreviated as the polymer according to the second invention).

[0160] Specific examples of the monomer (i) and the monomer (ii) in the polymer according to the second invention are the same as those of the monomer (i) and the monomer (ii) in the polymer according to the first invention, and the preferred examples are also the same. The content ratio (molar ratio) of the structural unit derived from the monomer (i) and the structural unit derived from the monomer (ii) in the polymer according to the second invention is the same as that in the polymer according to the first invention.

[0161] The polymer according to the second invention may further contain a structural unit derived from a monomer (iii) having two or more polymerizable unsaturated groups in addition to the monomer (i) and the monomer (ii). Specific examples of the monomer (iii) in the polymer according to the second invention include the same as the specific examples of the monomer (iii) in the polymer according to the first invention, and the preferred examples are also the same. In addition, when the polymer according to the second invention contains a structural unit derived from the monomer (iii), the content thereof is the same as the content of the monomer (iii) in the case where the polymer according to the first invention contains a structural unit derived from the monomer (iii).

[0162] The polymer according to the second invention may appropriately contain structural units derived from monomers generally used in this field, in addition to the monomers (i), (ii), and (iii). The monomers are the same as the other monomers in the polymer according to the first invention, and the content thereof is the same as the content of the other monomers when the polymer according to the first invention contains structural units derived from the other monomers.

[0163] The polymer according to the second invention may contain two or more types of structural units derived from the monomer (i), the monomer (ii), and the monomer (iii).

[0164] Specific examples of the polymer according to the second invention include the same as the specific examples of the polymer according to the first invention, and the preferred examples are also the same.

[0165] The polymer according to the second invention is a salt of a polymer neutralized with a monoamine, a polyamine having an amine value of less than 21, and / or an onium hydroxide (hereinafter sometimes abbreviated as the neutralizing agent according to the second invention). The polymer according to the second invention is preferably one in which a part or all of the carboxyl group in the structural unit derived from the monomer (i) and / or the sulfo group or phosphate group in the structural unit derived from the monomer (ii) are neutralized with the neutralizing agent according to the second invention.

[0166] The monoamine in the neutralizing agent according to the second invention is a monovalent amine having only one basic functional group. Specific examples of the monoamine include monoamines having one amino group, such as tert-butylamine, amylamine (pentylamine), octylamine, diisopropylethylamine, dibutylamine, triethylamine, benzylamine, aniline, monoethanolamine, N,N-diethylethanolamine, bis(2-cyanoethyl)amine, tris(2-cyanoethyl)amine, 3-aminopropionitrile, 3-methoxypropylamine, 3-aminotriazole, and 3-aminopropyltrimethoxysilane. Derivatives thereof; monoamines or derivatives thereof having one amidino group (amidine structure) such as diazabicyclononene; monoamines or derivatives thereof having one guanidino group (guanidine structure) such as tetramethylguanidine and diazabicycloundecene; monoamines or derivatives thereof having one pyridino group (pyridine structure) such as pyridine; monoamines or derivatives thereof having one phosphazeno group (phosphazene structure) such as hexafluorocyclotriphosphazene and hexachlorocyclotriphosphazene, etc. Among these specific examples, monoethanolamine, N,N-diethylethanolamine, 3-methoxypropylamine, and 3-aminotriazole are preferred, and 3-methoxypropylamine and 3-aminotriazole are particularly preferred.

[0167] The polyamine having an amine value of less than 21 in the neutralizing agent according to the second invention is a polyamine having two or more basic functional groups, and an amine value indicating the amount of basic functional groups in the structure is less than 21. Among the polyamines, low molecular weight amines are preferred, and specifically, polyamines having a molecular weight of 600 or less are preferred. Specific examples include 3,5-diaminotriazole, 4-dimethylaminopyridine, poly(propylene glycol) bis(2-aminopropyl ether) (JEFFAMINE® D-400), O,O'-bis(2-aminopropyl) polypropylene glycol-block-polyethylene glycol-block-polypropylene glycol (JEFFAMINE® ED-600), and the like. Among these specific examples, 3,5-diaminotriazole, poly(propylene glycol) bis(2-aminopropyl ether), and O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethylene glycol-block-polypropylene glycol are preferred, and 3,5-diaminotriazole and O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethylene glycol-block-polypropylene glycol are particularly preferred.

[0168] The onium hydroxide in the neutralizing agent according to the second invention may include ammonium hydroxide, phosphonium hydroxide, sulfonium hydroxide, etc., which may have a substituent. Specific examples include ammonium hydroxides such as benzyltrimethylammonium hydroxide and tetrabutylammonium hydroxide; phosphonium hydroxides such as tetrabutylphosphonium hydroxide; and sulfonium hydroxides such as trimethylsulfonium hydroxide. Among these specific examples, ammonium hydroxide is preferred, and benzyltrimethylammonium hydroxide and tetrabutylammonium hydroxide are particularly preferred.

[0169] Among the specific examples of the neutralizing agent according to the second invention, 3-methoxypropylamine, 3-aminotriazole, 3,5-diaminotriazole, poly(propylene glycol) bis(2-aminopropyl ether) (JEFFAMINE® D-400), O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethylene glycol-block-polypropylene glycol (JEFFAMINE® ED-600), and tetrabutylammonium hydroxide are preferred, and 3-methoxypropylamine, 3-aminotriazole, 3,5-diaminotriazole, poly(propylene glycol) bis(2-aminopropyl ether) (JEFFAMINE® D-400), O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethylene glycol-block-polypropylene glycol (JEFFAMINE® ED-600), and tetrabutylammonium hydroxide are preferred. ED-600), more preferred are 3,5-diaminotriazole, O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethyleneglycol-block-polypropyleneglycol (JEFFAMINE® ED-600), particularly preferred are 3,5-diaminotriazole, O,O'-bis(2-aminopropyl)polypropyleneglyco-block-polyethyleneglycol-block-polypropyleneglycol (JEFFAMINE® ED-600). The neutralizing agent according to the second invention may be used alone or in combination of two or more kinds, and is preferably used alone.

[0170] In addition to the neutralizing agent according to the second invention, a conventionally known neutralizing agent may be used in combination. Examples of the neutralizing agent to be used in combination include inorganic bases such as hydroxides, carbonates, and hydrogen carbonates of alkali metals or alkaline earth metals. Specific examples include hydroxides of alkali metals such as sodium hydroxide, lithium hydroxide, and potassium hydroxide; carbonates of alkali metals such as sodium carbonate, lithium carbonate, and potassium carbonate; hydrogen carbonates of alkali metals such as lithium hydrogen carbonate, sodium hydrogen carbonate, and potassium hydrogen carbonate; hydroxides of alkaline earth metals such as magnesium hydroxide and calcium hydroxide; carbonates of alkaline earth metals such as magnesium carbonate and calcium carbonate. Among these specific examples, hydroxides of alkali metals are preferred, and sodium hydroxide is particularly preferred. The neutralizing agent to be used in combination may be used alone with the neutralizing agent according to the second invention, or may be used in combination with the neutralizing agent according to the second invention in two or more types, and it is preferable to use only one type with the neutralizing agent according to the second invention. In particular, it is preferable to use only one hydroxide of an alkali metal with the neutralizing agent according to the second invention.

[0171] The degree of neutralization of the polymer according to the second invention is usually 50% or more and 300% or less, preferably 60% or more and 200% or less, and more preferably 70% or more and 150% or less. The degree of neutralization here refers to the ratio of the total number of moles of the neutralizer according to the second invention to the total number of moles of the carboxyl group, sulfo group, and phosphate group contained in the polymer according to the second invention. The binder according to the second invention contains the polymer according to the second invention, thereby improving the flexibility of the electrode produced, and making it possible to produce an electrode with excellent winding properties.

[0172] The polymer according to the second invention may be produced by carrying out a polymerization reaction and neutralization according to a method known per se. Specifically, for example, a polymerization reaction similar to that for the polymer according to the first invention may be carried out, and the polymer obtained by the polymerization reaction may be neutralized by adding the neutralizing agent according to the second invention in an amount that results in a desired degree of neutralization. The solvent used in the neutralization may be the same as that used in the polymerization reaction for the polymer according to the first invention.

[0173] [Binder solution] The binder of the second invention may be dissolved in a solvent and contained in the slurry composition of the second invention or the electrode of the second invention, which will be described later. In the second invention, the binder dissolved in a solvent is called a "binder solution", and in particular, the binder of the second invention dissolved in a solvent is called the "binder solution according to the second invention".

[0174] The solvent in the binder solution according to the second invention may be the same as that in the binder solution according to the second invention, and the preferred solvents are also the same. When the solvent is water, this may be called the "aqueous binder solution according to the second invention."

[0175] The content (mass of solids) of the binder of the second invention in the binder solution of the second invention may be appropriately set according to the desired concentration of the binder solution of the second invention, and is usually from 1 mass % to 70 mass %, preferably from 5 mass % to 50 mass %.

[0176] The binder solution according to the second invention may contain various additives generally used in this field in addition to the binder and solvent according to the second invention. The additives may be the same as the various additives in the binder solution according to the first invention, and the content of the additives is the same as the content of the additives in the binder solution according to the first invention.

[0177] [Slurry composition of the second invention] The slurry composition of the second invention is a composition for producing an electrode for an electricity storage device, containing the binder of the second invention. More specifically, it is a composition containing an active material and a solvent, and optionally a conductive assistant, in addition to the binder of the second invention (or the binder solution according to the second invention). The slurry composition of the second invention may be for producing either a positive electrode or a negative electrode, but is preferably for producing a negative electrode.

[0178] The content of the binder of the second invention in the slurry composition of the second invention is usually 0.1 mass % or more and 30 mass % or less, preferably 0.5 mass % or more and 20 mass % or less, and more preferably 1 mass % or more and 10 mass % or less, based on the total mass of the slurry composition of the second invention not including the solvent.

[0179] The active material, conductive assistant and solvent in the slurry composition of the second invention may be the same as the active material, conductive assistant and solvent in the slurry composition of the first invention, and the preferred ones are also the same. The contents of the active material, conductive assistant and solvent in the slurry composition of the second invention are the same as the contents of the active material, conductive assistant and solvent in the slurry composition of the first invention.

[0180] The slurry composition of the second invention may contain supporting salts, additives, etc. that are generally used in this field in addition to the binder, active material, conductive assistant, and solvent of the second invention. The supporting salts and additives may be the same as the supporting salts and additives in the slurry composition of the first invention, and the content thereof may be appropriately set in accordance with the amount generally used in this field.

[0181] The slurry composition of the second invention may be prepared in accordance with a method known per se. Specifically, for example, the slurry composition may be prepared by appropriately mixing the binder of the second invention, the active material, and, if necessary, the conductive assistant, the supporting salt and / or the additive in the solvent in the above-mentioned contents according to the desired slurry composition.

[0182] [Electrode of the second invention] The electrode of the second invention is an electrode for an electricity storage device, which is made of the slurry composition of the second invention. More specifically, it has an electrode mixture layer derived from the slurry composition of the second invention, which contains the binder of the second invention (or the binder solution according to the second invention), an active material, a solvent, and optionally a conductive assistant, a supporting salt and / or an additive, and a current collector. The electrode of the second invention can be used as either a negative electrode or a positive electrode, but is preferably used as a positive electrode.

[0183] The current collector in the electrode of the second invention may be the same as the current collector in the electrode of the first invention, and the preferred current collectors are also the same.

[0184] The electrode of the second invention may be produced by the same production method as that for the electrode of the first invention.

[0185] In the manufacture of the electrode of the second invention, the amount of the slurry composition of the second invention used may be appropriately set so that the thickness of the electrode mixture layer after drying is the desired thickness.

[0186] In producing the electrode of the second invention, the slurry composition of the second invention may be applied or pressed onto a current collector in the same manner as the slurry composition of the first invention is applied or pressed onto a current collector.

[0187] In the production of the electrode of the second invention, the slurry composition of the second invention may be dried in the same manner as the slurry composition of the first invention.

[0188] In the production of the electrode of the second invention, a pressing treatment may be carried out before or after the drying, if necessary. The pressing treatment may be carried out in the same manner as in the production of the electrode of the first invention.

[0189] [Electricity storage device of the second invention] The electric storage device of the second invention refers to a device or element that has the electrode of the second invention and can store electricity chemically, physically, or physicochemically. Specific examples include the same ones as the electric storage device of the first invention, and the preferred ones are also the same.

[0190] The configuration of the electricity storage device of the second invention may be the same as that of the electricity storage device of the first invention. In addition, the members constituting the electricity storage device of the second invention other than the electrodes of the second invention may be the same as those constituting the electricity storage device of the first invention other than the electrodes of the first invention, and the preferred members are also the same.

[0191] The shape of the electricity storage device of the second invention is not particularly limited, and the internal shape may be a wound type, a laminated type, etc., and the external shape may be a coin type, a laminated type (pouch type), a square type, a cylindrical type, etc., and any other shapes that are generally used in this field may be appropriately adopted.

[0192] The present invention (first invention and second invention) will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples in any way. EXAMPLES

[0193] Example 1 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 435 parts by mass of ion-exchanged water, 22 parts by mass (0.31 mol) of acrylic acid (manufactured by Toagosei Co., Ltd.), 22 parts by mass (0.19 mol) of 2-hydroxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.21 parts by mass (0.0014 mol) of N,N-methylenebisacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed and heated under a nitrogen stream until the internal temperature reached 77° C. Next, 0.34 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate (trade name: VA-057, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and the resulting solution was reacted at 77° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and 20 parts by mass of a 48% aqueous sodium hydroxide solution (manufactured by Toagosei Co., Ltd.) was added to obtain an aqueous binder solution 1 (solid content 10%).

[0194] Example 2 A binder aqueous solution 2 (solid content 10%) was obtained in the same manner as in Example 1, except that 461 parts by mass of ion-exchanged water was used instead of 435 parts by mass, 5.0 parts by mass (0.069 mol) of acrylic acid was used instead of 22 parts by mass, 45 parts by mass (0.39 mol) of 2-hydroxyethyl acrylate was used instead of 22 parts by mass, 0.20 parts by mass (0.0013 mol) of N,N-methylenebisacrylamide was used instead of 0.21 parts by mass, 0.31 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate was used instead of 0.34 parts by mass, and 4.6 parts by mass of 48% aqueous sodium hydroxide solution was used instead of 20 parts by mass.

[0195] Example 3 A binder aqueous solution 3 (solid content 10%) was obtained in the same manner as in Example 1, except that 521 parts by mass of ion-exchanged water was used instead of 435 parts by mass, 11 parts by mass (0.15 mol) of acrylic acid was used instead of 22 parts by mass, 44 parts by mass (0.38 mol) of 2-hydroxyethyl acrylate was used instead of 22 parts by mass, 0.27 parts by mass (0.0018 mol) of N,N-methylenebisacrylamide was used instead of 0.21 parts by mass, 0.42 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate was used instead of 0.34 parts by mass, and 4.9 parts by mass of 48% aqueous sodium hydroxide solution was used instead of 20 parts by mass.

[0196] Example 4 A 1000mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube was charged with 460 parts by mass of ion-exchanged water, 36 parts by mass (0.50mol) of acrylic acid, 9 parts by mass (0.11mol) of 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.20 parts by mass (0.00078mol) of pentaerythritol triallyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and heated under a nitrogen stream until the internal temperature reached 77°C. Then, 0.084 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate was added, and the resulting solution was reacted at 77°C for 4 hours. After the reaction, the mixture was cooled to room temperature, and 32 parts by mass of a 50% aqueous sodium hydroxide solution (manufactured by Toagosei Co., Ltd.) was added to obtain an aqueous binder solution 4 (10% solid content).

[0197] Example 5 Binder aqueous solution 5 (solid content 10%) was obtained in the same manner as in Example 1, except that 400 parts by mass of ion-exchanged water was used instead of 435 parts by mass, 5.0 parts by mass (0.069 mol) of acrylic acid was used instead of 22 parts by mass, 45 parts by mass (0.39 mol) of 2-hydroxyethyl acrylate was used instead of 22 parts by mass, 0.38 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate was used instead of 0.34 parts by mass, 4.6 parts by mass of 48% aqueous sodium hydroxide solution was used instead of 20 parts by mass, and N,N-methylenebisacrylamide was not used.

[0198] Example 6 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 720 parts by mass of ion-exchanged water, 9.0 parts by mass (0.12 mol) of acrylic acid, and 81 parts by mass (0.70 mol) of 2-hydroxyethyl acrylate were placed and heated under a nitrogen stream until the internal temperature reached 77° C. Then, 0.69 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate was added, and the resulting solution was reacted at 77° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and 7.3 parts by mass of a 48% aqueous sodium hydroxide solution and 0.43 parts by mass of an aqueous polyethyleneimine solution (molecular weight about 10,000, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to obtain an aqueous binder solution 6 (solid content 11%).

[0199] Example 7 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 350 parts by mass of ion-exchanged water, 5.0 parts by mass (0.069 mol) of acrylic acid, 40 parts by mass (0.34 mol) of 2-hydroxyethyl acrylate, and 5.0 parts by mass (0.035 mol) of 4-hydroxybutyl acrylate were placed and heated under a nitrogen stream until the internal temperature reached 77 ° C. Then, 0.38 parts by mass of 2,2'-azobis [N- (2-carboxyethyl) -2-methylpropionamidine] tetrahydrate was added, and the resulting solution was reacted at 77 ° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and 4.5 parts by mass of a 48% aqueous sodium hydroxide solution was added to obtain an aqueous binder solution 7 (solid content 11%).

[0200] Example 8 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 320 parts by mass of ion-exchanged water, 4.0 parts by mass (0.056 mol) of acrylic acid, 32 parts by mass (0.28 mol) of 2-hydroxyethyl acrylate, and 4.0 parts by mass (0.028 mol) of 4-hydroxybutyl acrylate were placed and heated under a nitrogen stream until the internal temperature reached 77°C. Then, 0.31 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate was added, and the resulting solution was reacted at 77°C for 4 hours. After the reaction, the mixture was cooled to room temperature, and 4.5 parts by mass of 48% aqueous sodium hydroxide solution and 0.19 parts by mass of aqueous polyethyleneimine solution (molecular weight about 10,000) were added to obtain an aqueous binder solution 8 (solid content 11%).

[0201] Comparative Example 1 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 420 parts by mass of ion-exchanged water, 40 parts by mass (0.59 mol) of acrylic acid, and 0.24 parts by mass (0.0016 mol) of N,N-methylenebisacrylamide were placed and heated under a nitrogen stream until the internal temperature reached 77° C. Then, 0.30 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate was added, and the resulting solution was reacted at 77° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and 37 parts by mass of a 48% aqueous sodium hydroxide solution was added to obtain an aqueous binder solution 101 (10% solids).

[0202] Comparative Example 2 In a 200 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 135 parts by mass of ion-exchanged water and 15 parts by mass (0.13 mol) of 2-hydroxyethyl acrylate were placed and heated under a nitrogen stream until the internal temperature reached 75° C. Then, 0.054 parts by mass of 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate was added, and the resulting solution was reacted at 75° C. for 4 hours. After the reaction, the mixture was cooled to room temperature to obtain a binder aqueous solution 102 (solid content 10%).

[0203] Comparative Example 3 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 575 parts by mass of ion-exchanged water, 45 parts by mass (0.62 mol) of acrylic acid, 11 parts by mass (0.056 mol) of 2-acryloyloxyethyl acid phosphate (trade name: Light Acrylate P-1A (N), manufactured by Kyoeisha Chemical Co., Ltd.), and 0.18 parts by mass (0.00097 mol) of diethylene glycol diallyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed and heated under a nitrogen stream until the internal temperature reached 77 ° C. Next, 0.10 parts by mass of 2,2'-azobis [N- (2-carboxyethyl) -2-methylpropionamidine] tetrahydrate was added, and the resulting solution was reacted at 77 ° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and 41 parts by mass of 48% sodium hydroxide aqueous solution was added to obtain a binder aqueous solution 103 (solid content 10%).

[0204] For the binder aqueous solutions 1 to 8 obtained in Examples 1 to 8 and the binder aqueous solutions 101 to 103 obtained in Comparative Examples 1 to 3, the "binder constituent component corresponding to the monomer (i)", "binder constituent component corresponding to the monomer (ii)", "content ratio (molar ratio) of the structural unit derived from the monomer (i) and the structural unit derived from the monomer (ii)", "binder constituent component corresponding to the monomer (iii)", and "content (mol%) of the structural unit derived from the monomer (iii) relative to the total content of the structural unit derived from the monomer (i) and the monomer (ii)" in the binder in each binder aqueous solution are shown in Table 1. In addition, the "constituent component of the neutralizing agent" and "degree of neutralization by the neutralizing agent (%)" for the binder in each binder aqueous solution are also shown in Table 1.

[0205] [Table 1]

[0206] (Experimental Example 1) (1) Sample preparation 0.92 parts by mass of acetylene black as a conductive assistant (product name: Denka Black (registered trademark) powder product, average particle size: 35 nm, specific surface area: 68 m 2The obtained aqueous dispersion of the conductive additive and the binder was mixed and stirred using a planetary mixer (product name: Awatori Rentaro, model ARE-310, manufactured by Thinky Corporation), 1.0 part by mass of the aqueous binder solution 1 (solid content 10%) obtained in Example 1, and 18.1 parts by mass of water as a solvent. The obtained aqueous dispersion of the conductive additive and the binder was called the measurement slurry.

[0207] (2) Measurement method for loss tangent tan δ The obtained slurry for measurement was set on the sample stage, and the thickness of the slurry for measurement was adjusted to 1 mm using a parallel plate (PP50). Then, the slurry was measured using a rheometer (product name: MCR 102, manufactured by Anton Paar) at a measurement temperature of 25°C, a frequency of 1 Hz, and a strain amount of 10 -2 ~10 3 The strain dispersion measurement was carried out in the range of 100%. From the obtained values ​​of the storage modulus G' and loss modulus G'', the loss tangent tan δ (loss modulus G'' / storage modulus G') in the linear region of the measurement slurry was calculated.

[0208] (Experimental Examples 2 to 8) Measurement slurries were prepared in the same manner as in Experimental Example 1, except that the binder aqueous solution 1 was replaced with the binder aqueous solutions 2 to 8 obtained in Examples 2 to 8, respectively, and the loss tangent tan δ was calculated.

[0209] (Comparative Experimental Examples 1 to 3) Measurement slurries were prepared in the same manner as in Experimental Example 1, except that the binder aqueous solution 1 was replaced with the binder aqueous solutions 101 to 103 obtained in Comparative Examples 1 to 3, respectively, and the loss tangent tan δ was calculated.

[0210] (Experimental Example 9) (1) Preparation of Slurry Composition 2.1 g of carbon-coated SiO powder (particle size: 5 μm, manufactured by Osaka Titanium Co., Ltd.), 5.0 g of natural graphite (particle size: 20 μm, manufactured by Hitachi Chemical Co., Ltd.), 0.50 g of acetylene black (trade name: Denka Black (registered trademark) powder product, manufactured by Denka Co., Ltd.), and 4.0 g of the binder aqueous solution 1 (solid content 10%) obtained in Example 1 were weighed out, and 8.6 g of water was further added, and the mixture was mixed and stirred at a rotation speed of 2000 rpm for 30 minutes using a planetary mixer (product name: Awatori Rentaro, model ARE-310, manufactured by Thinky Co., Ltd.). The resulting mixture was used as a slurry composition.

[0211] (2) Manufacturing of electrodes for lithium secondary batteries The slurry composition obtained in (1) was applied to a copper current collector using a doctor blade to a thickness of 75 μm, which was then primarily dried in air at 80° C., and the dried electrode was then pressed into a roll press to a volume density of 1.5 g / cm. 3 The pressed electrode was dried in vacuum at 150° C. for 12 hours.

[0212] (3) Manufacturing of coin-cell batteries A coin-type battery was fabricated in a glove box filled with argon. Here, a coin-type battery was assembled consisting of the electrode obtained in (2), a lithium foil electrode, a solution of 1M LiPF6 in ethylene carbonate (EC) / dimethyl carbonate (DMC) (volume ratio 1:1) with 2% vinylene carbonate (VC) added, and a separator.

[0213] (4) Charge / discharge test Using the coin-type battery manufactured in (3), a charge / discharge test was carried out under the following conditions. Counter electrode: Lithium foil ·Electrolyte: 1M LiPF6EC / DMC mixed solution (volume ratio 1:1) + VC 2% by mass Measurement equipment: ABE1024-5V 0.1A-4 charge / discharge test equipment (manufactured by Electrofield) ·Charging and discharging conditions First Cycle Charging: Constant current, constant voltage 0.1C, 0.02V, 15 hours, terminated Discharge constant current 0.1C 1.5V end 2nd cycle onwards Charging: Constant current, constant voltage 0.5C, 0.02V, 3 hours, terminated Discharge constant current 0.5C 1.5V end The capacity retention rate (%) after 20 cycles was calculated from the discharge capacity values ​​of the negative electrode (the electrode obtained in (2)) after the initial charge / discharge and after 20 cycles using the following formula. Capacity retention rate (%) = discharge capacity after 20 cycles ÷ initial discharge capacity × 100

[0214] (Experimental Examples 10-16) Coin-type batteries were manufactured in the same manner as in Experimental Example 9, except that the binder aqueous solutions 2 to 8 obtained in Examples 2 to 8 were used instead of the binder aqueous solution 1, and the capacity retention rate (%) after 20 cycles in a charge-discharge test was calculated.

[0215] (Comparative Experimental Examples 4 to 6) Coin-type batteries were manufactured in the same manner as in Experimental Example 9, except that the binder aqueous solutions 101 to 103 obtained in Comparative Examples 1 to 3 were used instead of the binder aqueous solution 1, and the capacity retention rate (%) after 20 cycles in a charge-discharge test was calculated.

[0216] Table 2 shows the tan δ values ​​obtained in Experimental Examples 1 to 8 and Comparative Experimental Examples 1 to 3, and the capacity retention rates obtained in Experimental Examples 9 to 16 and Comparative Experimental Examples 4 to 6.

[0217] [Table 2]

[0218] As shown in Table 2, the binder aqueous solutions 1 to 8 obtained in Examples 1 to 8 exhibited a measurement slurry tan δ of greater than 1, and the capacity retention rate in the charge-discharge test was 80% or more. This is believed to be because the binder with tan δ>1 under the measurement conditions in the first invention had excellent dispersibility of the conductive assistant, and the battery using this binder was able to maintain good battery characteristics even after 20 charge-discharge cycles. On the other hand, in the binder aqueous solutions 101 to 103 obtained in Comparative Examples 1 to 3, the tan δ of the measurement slurry was 1 or less, and the capacity retention rate in the charge-discharge test was less than 80%. This is considered to be because the binder with tan δ≦1 under the measurement conditions in the first invention has insufficient dispersibility of the conductive assistant, and the battery using this binder cannot sufficiently transfer electrons.

[0219] Example 9 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 280 parts by mass of ion-exchanged water, 4 parts by mass (0.06 mol) of acrylic acid (manufactured by Toagosei Co., Ltd.), and 36 parts by mass (0.76 mol) of 2-hydroxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.) were placed and heated under a nitrogen stream until the internal temperature reached 77°C. Then, 0.31 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate (trade name: VA-057, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and the resulting solution was reacted at 77°C for 4 hours. After the reaction, the mixture was cooled to room temperature, and an aqueous solution of 4.6 parts by mass of pentylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 40 parts by mass of ion-exchanged water was added dropwise to obtain an aqueous binder solution 9 (solid content 14%).

[0220] (Examples 10 to 34) Aqueous binder solutions 10 to 34 were obtained in the same manner as in Example 9, except that each of the amines shown in Table 3 below was used instead of 4.6 parts by mass of pentylamine.

[0221] [Table 3]

[0222] Example 35 In a 1000 mL separable flask equipped with a stirrer, a cooling tube, a thermometer, and a nitrogen inlet tube, 320 parts by mass of ion-exchanged water, 20 parts by mass (0.28 mol) of acrylic acid (manufactured by Toagosei Co., Ltd.), 20 parts by mass (0.43 mol) of 2-hydroxyethyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd.), and 0.19 parts by mass (0.0013 mol) of N,N-methylenebisacrylamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were placed and heated under a nitrogen stream until the internal temperature reached 77° C. Next, 0.31 parts by mass of 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]tetrahydrate (trade name: VA-057, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and the resulting solution was reacted at 77° C. for 4 hours. After the reaction, the mixture was cooled to room temperature, and an aqueous solution of 18.5 parts by mass of 48% sodium hydroxide aqueous solution (manufactured by Toagosei Co., Ltd.) and 40 parts by mass of ion-exchanged water was added dropwise, and an aqueous solution of 3.6 parts by mass of pentylamine (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) and 40 parts by mass of ion-exchanged water was added dropwise to obtain Binder Aqueous Solution 35 (solid content 11%).

[0223] (Examples 36 to 39) Aqueous binder solutions 36 to 39 were obtained in the same manner as in Example 35, except that each of the amines shown in Table 4 below was used instead of 3.6 parts by mass of pentylamine.

[0224] [Table 4]

[0225] (Experimental Example 17) (1) Preparation of slurry composition and production of electrodes for lithium secondary batteries Except for using the binder aqueous solution 9 obtained in Example 9 instead of the binder aqueous solution 1, an electrode for a lithium secondary battery was produced in the same manner as in (1) Preparation of a slurry composition and (2) Production of an electrode for a lithium secondary battery in Experimental Example 9.

[0226] (2) Bending resistance test The electrodes manufactured in (1) were cut into pieces measuring 10 mm x 100 mm and set in a mandrel testing machine (BEVS1603 cylindrical bending tester). The diameter of the mandrel rod around which the electrodes were wound was gradually reduced from 32 mm, and the diameter at which cracks occurred in the electrode (mandrel diameter) was measured. Mandrel diameters of 2 mm to 6 mm were rated as A, 7 mm to 9 mm as B, 10 mm to 12 mm as C, and 13 mm or more as D.

[0227] (3) Manufacturing of coin-cell batteries A coin-type battery was fabricated in a glove box filled with argon. Here, a coin-type battery was assembled consisting of the electrode obtained in (1), a lithium foil electrode, a solution of 1M LiPF6 in ethylene carbonate (EC) / dimethyl carbonate (DMC) (volume ratio 1:1) with 2% vinylene carbonate (VC) added, and a separator.

[0228] (4) Charge / discharge test Using the coin-type battery produced in (3), a charge-discharge test was carried out under the same conditions as those described in (4) Charge-discharge test of Experimental Example 9.

[0229] (Examples 18-42) A bending resistance test and a charge / discharge test were carried out in the same manner as in Experimental Example 17, except that the binder aqueous solutions 10 to 34 obtained in Examples 10 to 34 were used instead of the binder aqueous solution 9, respectively.

[0230] Table 4 shows the evaluation results obtained in the bending resistance test in Experimental Examples 17 to 42, and the capacity retention rates obtained in the charge / discharge test in Experimental Examples 17 to 42.

[0231] [Table 5]

[0232] (Examples 43-47) A bending resistance test and a charge / discharge test were carried out in the same manner as in Experimental Example 17, except that the binder aqueous solutions 35 to 39 obtained in Examples 35 to 39 were used instead of the binder aqueous solution 9, respectively.

[0233] Table 6 shows the evaluation results obtained in the bending resistance test for Experimental Examples 43 to 47, and the capacity retention rates obtained in the charge / discharge test for Experimental Examples 43 to 47.

[0234] [Table 6]

[0235] From Table 5, the electrodes (Experimental Examples 17 to 34) using the binder aqueous solutions 9 to 29 obtained in Examples 9 to 29 were evaluated as having a mandrel diameter of A to C, had high bending resistance, and had a capacity retention rate of 80% or more. It is believed that the hydrophobic group of the amine used for neutralization lowered the glass transition point of the binder, softening the binder and thus improving bending resistance. In addition, since the structure is similar to that of the first invention, it is believed that good battery characteristics are maintained.

[0236] Furthermore, from Table 6, the electrodes (Examples 43 to 47) using the binder aqueous solutions 35 to 39 obtained in Examples 35 to 39 had mandrel diameters of A to B, high bending resistance, and capacity retention rates of 85% or more. Therefore, even if the molar ratio of the monomer (i) and the monomer (ii) and the presence or absence of a crosslinked structure were different, it is considered that the bending resistance was improved by the expression of the effect of reducing the glass transition point of the binder, as in the electrodes of Examples 17 to 34.

[0237] On the other hand, in the electrodes (Experimental Examples 38 to 42) using the binder aqueous solutions 30 to 34 obtained in Examples 30 to 34, the mandrel diameter evaluation was D, and the flex resistance was poor. It is considered that in the case of polyvalent amines with a high amine value, the distance between neutralized amines is short, so that the binder becomes rigid and the electrode also becomes hard, resulting in poor flex resistance.

Claims

1. A binder for an electricity storage device, comprising: In a strain dispersion measurement under the measurement conditions of a measurement temperature of 25° C. and a frequency of 1 Hz, the loss tangent tanδ in the linear region of an aqueous dispersion of 0.5% by mass of the binder and 4.6% by mass of the conductive assistant is tanδ>1; Here, the conductive assistant has an average particle size of 30 nm to 40 nm and a specific surface area of ​​65 m 2 / g or more 70m 2 / g or less, The binder for an electricity storage device contains (i) an ethylenically unsaturated carboxylic acid monomer, and (ii) a polymer or a salt thereof including a structural unit derived from an ethylenically unsaturated monomer having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group.

2. 2. The binder according to claim 1, wherein the monomer (ii) has a solubility in water at 20° C. of 1 g / L or more.

3. The SP value of the monomer (ii) is 11.5 (cal / cm 3 ) 1 / 2 The binder according to claim 1 .

4. The binder according to claim 1, wherein the monomer (ii) is a monomer represented by the following general formula [1]: [Formula 1] (In general formula [1], R 1 represents a hydrogen atom or a methyl group; Y 1 is -O- or -NR 2 - represents R 2 represents a hydrogen atom or a methyl group; A 1 represents a monovalent group having at least one group selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group.

5. The binder according to claim 1, wherein the monomer (ii) is a monomer represented by the following general formula [2]: [Case 2] (In general formula [2], R 1 represents a hydrogen atom or a methyl group; Y 1 is -O- or -NR 2 - represents R 2 represents a hydrogen atom or a methyl group; A 2 represents an alkyl group having 1 to 10 carbon atoms and having 1 to 3 groups selected from a hydroxy group, a dialkylamino group, an acetyl group, a sulfo group, a phosphate group, and a cyano group; or a linear alkyl group having 3 to 36 carbon atoms and having one hydroxy group and 1 to 5 ester bonds in the chain.

6. The binder according to claim 1 , wherein the polymer or the salt thereof further contains (iii) a structural unit derived from a monomer having two or more polymerizable unsaturated groups.

7. 2. The binder according to claim 1, wherein the polymer or the salt thereof is neutralized with an alkali metal hydroxide and / or a polyvalent amine having an amine value of 21 or more.

8. A slurry composition for an electrical storage device, comprising the binder according to claim 1 .

9. An electrode for an electricity storage device, comprising the slurry composition according to claim 8 .

10. An electricity storage device comprising the electrode according to claim 9.

Citation Information

Patent Citations

  • Manufacture of positive electrode of nonaqueous electrolyte battery

    JP1988236258A

  • Manufacture of negative mix of nonaqueous secondary battery

    JP1996190912A

  • Vibration-damping water-based coating composition

    JP1998324822A

  • Synthetic resin emulsion for damping paint