Dislocation distribution in silicon carbide crystalline materials
Optimizing SiC boule growth with supersaturated conditions reduces dislocation density and improves uniformity, addressing the limitations of conventional SiC wafer manufacturing for large diameter wafers, thereby enhancing the quality and yield of SiC wafers for semiconductor applications.
Patent Information
- Application Number
- JP2022546447
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-29
- Filing Date
- 2021-01-12
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2041-01-12
AI Technical Summary
Conventional silicon carbide (SiC) wafer manufacturing faces challenges in producing large diameter wafers with high quality due to structural defects such as dislocations and wafer shape irregularities, which limit their scalability and economic viability.
The growth of SiC boules and wafers is optimized by providing source material at a supersaturation level higher than typical, resulting in reduced dislocation density and improved uniformity, enabling the production of large diameter SiC wafers with lower total dislocation density (TDD) and radial uniformity.
This approach allows for the production of SiC wafers with reduced dislocation densities and improved uniformity, enhancing the quality and yield of large diameter SiC boules and wafers, suitable for high-power and high-frequency semiconductor devices.
Smart Images

Figure 0007587591000001 
Figure 0007587591000002 
Figure 0007587591000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to crystalline materials, and more particularly to dislocation distributions in silicon carbide crystalline materials. [Background technology]
[0002] Silicon carbide (SiC) exhibits many attractive electrical and thermophysical properties. SiC is particularly useful due to its physical strength and high resistance to chemical attack, as well as various electrical properties including radiation hardness, high breakdown field, relatively wide band gap, high saturation electron drift velocity, high operating temperature, and absorption and emission of high energy photons in the blue, violet, and ultraviolet regions of the spectrum. Compared to conventional wafer or substrate materials including silicon and sapphire, such properties make SiC more suitable for the fabrication of wafers or substrates for high power density semiconductor devices such as power electronic devices, radio frequency devices, and optoelectronic devices. SiC exists in many different crystal structures, referred to as polytypes, with certain polytypes (e.g., 4H-SiC and 6H-SiC) having a hexagonal crystal structure.
[0003] While SiC exhibits excellent material properties, the crystal growth techniques required to grow SiC are very different and significantly more challenging than conventional growth processes for other crystal materials. Conventional crystal materials used in semiconductor manufacturing, such as silicon and sapphire, have much lower melting points, allowing direct crystal growth techniques from molten source material that can produce large diameter crystal materials. In contrast, bulk crystalline SiC is often produced by a sublimation growth process at high temperatures using seed crystals, which presents various challenges, among them the incorporation of impurities, structural defects associated with heat and crystal stress, and the formation of different polytypes. In a typical SiC growth technique, both the substrate and the source material are placed inside a reaction crucible. When the crucible is heated, a thermal gradient is generated that promotes the movement of the gas phase of the material from the source material towards the substrate, which then condenses on the substrate, resulting in bulk crystal growth. It is known that impurities can be introduced into SiC as dopants and that certain properties can be controlled by these dopants. In the case of sublimation growth of SiC, dopants can be introduced into the chamber in a variety of ways such that the dopants are present in the SiC crystal produced from the process. The process is controlled to obtain the appropriate concentration of dopants for a particular application. After bulk crystal growth, individual wafers of SiC can be obtained by slicing the bulk crystal ingot or boule of SiC, and the individual wafers can subsequently be subjected to further processes such as lapping or polishing.
[0004] The unique properties of SiC wafers enable the design and fabrication of arrays of high power and / or high frequency semiconductor devices. Continuing development has brought SiC wafer fabrication to a level of maturity that allows the fabrication of such semiconductor devices for an ever-expanding range of commercial applications. As the semiconductor device industry continues to grow, SiC wafers with larger effective diameters are desired. The effective diameter of SiC wafers may be limited by certain structural defects in the material composition of SiC as well as certain wafer topography properties. Structural defects in the material composition may include dislocations (e.g., micropipes, threading blades, threading screws, and / or basal plane dislocations), hexagonal voids, and stacking faults, among others. Wafer topography properties associated with SiC may include warps, bows, and thickness variations that may be related to the flatness of the wafer. These various structural defects and wafer topography properties may contribute to crystal stresses that may be detrimental to the fabrication and proper operation of semiconductor devices subsequently formed on conventional SiC wafers. Such crystal stress is generally proportional to the square of the wafer radius, and as a result, it is difficult to economically manufacture high quality large diameter SiC semiconductor wafers.
[0005] There is a continuing need in the art for improved larger diameter SiC wafers and associated semiconductor devices that overcome the challenges associated with conventional SiC wafers. Summary of the Invention
[0006] Silicon carbide (SiC) wafers, SiC boules, and associated methods are disclosed that provide improved dislocation distribution. SiC boules are provided that exhibit reduced dislocation density and improved dislocation uniformity across the length of the boule. Corresponding SiC wafers have reduced total dislocation density (TDD) values with improved TDD radial uniformity. Growth conditions for the SiC crystal material include providing source material at a significantly higher supersaturation amount than the amount of source material present during growth would typically be required. Such SiC crystal material and associated methods are suitable for providing large diameter SiC boules and corresponding SiC wafers with improved crystal quality.
[0007] In one embodiment, the SiC wafer has a diameter of at least 145 millimeters (mm), a width of 1 mm, and an outer diameter of 1 square centimeter (cm) at any annular ring portion corresponding to a radial position of the wafer within a range of 3 mm to 50 mm from the center of the SiC wafer. 2 and a total dislocation density (TDD) of 3000 or less per cm. In a specific embodiment, the TDD is 1 mm wide and has an outer diameter of 1 mm or less at any annular ring portion corresponding to a radial position of the wafer within a range including a position 3 mm from the center of the SiC wafer to a position 2 mm from the edge of the SiC wafer. 2 In a specific embodiment, the TDD has a width of 1 mm and an outer diameter of 1 cm at any annular ring portion corresponding to a radial position of the wafer within a range of 3 mm to 50 mm from the center of the SiC wafer. 2 In one particular embodiment, the TDD has a width of 1 mm and an outer diameter of 1 cm for any annular ring portion that corresponds to a wafer radial position for at least 50% of all wafer radial positions of the SiC wafer. 2 In one particular embodiment, the TDD has a width of 1 mm and an outer diameter of 1 cm or less at any annular ring portion that corresponds to the radial position of the wafer for at least 50% of all radial positions of the SiC wafer. 2In certain embodiments, the diameter is within the range of 145 mm to 205 mm, inclusive. In certain embodiments, the diameter is within the range of 145 mm to 155 mm, inclusive. In certain embodiments, the SiC wafer comprises a 4H—SiC wafer. In certain embodiments, the SiC wafer comprises semi-insulating SiC. In certain embodiments, the SiC wafer comprises n-type SiC. In certain embodiments, the TDD is within the range of 1 cm 2 More than 1000 per
[0008] In another aspect, the SiC wafer has a diameter that is at least 145 mm and a coefficient of variation of the TDD that is 0.3 or less in an area of the wafer divided into annular rings having a width of 1 mm, the area of the wafer being bounded by a boundary line that is 3 mm from the center of the SiC wafer and 2 mm from the edge of the SiC wafer. In a particular embodiment, the coefficient of variation is 0.2 or less. In a particular embodiment, the coefficient of variation is 0.1 or more. In a particular embodiment, the TDD has a width of 1 mm and an outer diameter that is 0.3 or less in any annular ring that is 3 mm to 50 mm from the center of the SiC wafer, inclusive, in a radial position of the wafer. 2 In one particular embodiment, the TDD has a width of 1 mm and an outer diameter of 1 cm for any annular ring portion that corresponds to a wafer radial position for at least 50% of all wafer radial positions of the SiC wafer. 2 2000 or less per 1000. In certain embodiments, the SiC wafer comprises a 4H—SiC wafer. In certain embodiments, the SiC wafer comprises semi-insulating SiC. In certain embodiments, the SiC wafer comprises n-type SiC. In certain embodiments, the diameter is in the range of 145 mm to 155 mm, inclusive. In certain embodiments, the diameter is in the range of 145 mm to 205 mm, inclusive.
[0009] In another aspect, the SiC boule has a diameter in the range of 145 mm to 180 mm, inclusive, and a boule height of greater than 50 mm. In one particular embodiment, at least 75% of the height of the SiC boule is configured to provide a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers having a wafer area that is bounded by a boundary line that includes the center of the SiC wafer and has a radius of 2 mm from the periphery of the SiC wafer, the wafer area being within 1 cm. 2 In one particular embodiment, the TDD is 1 cm or less. 2 In one particular embodiment, at least 40% of the height of the SiC boule is configured to provide a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers having a TDD of 3000 or less per square centimeter for a wafer area bounded by a perimeter that includes a center of the SiC wafer and has a radius from a periphery of the SiC wafer at a radial position of the wafer of 2 mm. In one particular embodiment, the TDD is 3000 or less per square centimeter. 2 In certain embodiments, the boule height is in the range of 60 mm to 300 mm, inclusive. In certain embodiments, the boule height is in the range of 55 mm to 80 mm, inclusive. In certain embodiments, the boule height is in the range of 60 mm to 70 mm, inclusive. In certain embodiments, the boule height is 65 mm or less. In certain embodiments, the boule height is 55 mm or more and 65 mm or less.
[0010] In another aspect, the SiC boule has a diameter in the range of 145 mm to 180 mm, inclusive, and a boule height of 40 mm or more, and at least 50% of the height of the SiC boule is configured to produce a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers having a wafer area bounded by a boundary having a radius that includes a center of the SiC wafer and is 2 mm from a peripheral edge of the SiC wafer, the wafer area being 1 cm or less. 2In certain embodiments, the boule height is in the range of 40 mm to 300 mm, inclusive. In certain embodiments, the boule height is in the range of 40 mm to 80 mm, inclusive. In certain embodiments, the TDD is less than 1 cm 2 In one particular embodiment, at least 80% of the height of the SiC boule is greater than or equal to 1000 per cm 2 In one particular embodiment, at least 40% of the height of the SiC boule is configured to produce a plurality of SiC wafers having an average TDD of 4600 or less per SiC wafer. In one particular embodiment, at least 40% of the height of the SiC boule is configured to produce a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers having a wafer area bounded by a perimeter having a radius of 1 cm2 or less that includes a center of the SiC wafer and having a radius of 2 mm from the peripheral edge of the SiC wafer. 2 In certain embodiments, the TDD is less than or equal to 3000 per cm. 2 More than 1000 per
[0011] In another embodiment, the SiC wafer is a wafer having a radius of 1 cm for a wafer area bounded by a boundary line including the center of the SiC wafer and having a radius of 2 mm from the edge of the SiC wafer. 2 The SiC wafer has a TDD of 3500 or less per cm, and the SiC wafer is taken from a boule location 40 mm or greater measured from the seed. In certain embodiments, the boule location is in the range of 40 mm to 300 mm, inclusive, or in the range of 40 mm to 80 mm, inclusive, or in the range of 40 mm to 65 mm, inclusive. In certain embodiments, the TDD is 1 cm 2 In certain embodiments, the TDD is greater than or equal to 500 per cm. 2 2500 or less per cm 2 In one particular embodiment, the SiC wafer has a diameter that is equal to or greater than 145 mm and equal to or less than 180 mm.
[0012] In another aspect, any of the above individual or combined aspects, and / or various separate aspects and features described herein may be combined for additional advantage. Any of the various features and elements disclosed herein may be combined with one or more other disclosed features and elements, unless otherwise indicated to the contrary herein.
[0013] Those skilled in the art will appreciate the scope of the present disclosure and realize additional aspects thereof upon reading the following detailed description of the preferred embodiments in conjunction with the accompanying drawing figures. The accompanying drawings, which are incorporated in and form a part of this specification, illustrate several aspects of the disclosure and, together with the description, serve to explain the principles of the disclosure. [Brief description of the drawings]
[0014] [Figure 1A] FIG. 1A illustrates a method of growing crystalline silicon carbide (SiC) according to an embodiment disclosed herein. [Figure 1B] FIG. 1B illustrates a method of growing crystalline silicon carbide (SiC) according to an embodiment disclosed herein. [Diagram 2] FIG. 2 includes a first frame providing a perspective view of a crystalline ingot housed in a conventional wire saw tool and undergoing a wire sawing process, and a second frame providing a perspective view of a number of wafers obtained by the wire sawing process. [Diagram 3] FIG. 3 is a first perspective view of a crystal plane diagram showing the coordinate system in a hexagonal crystal such as 4H—SiC. [Figure 4] FIG. 4 is a second perspective view of the crystal planes in a hexagonal crystal showing planes that are not parallel to the c-plane. [Figure 5A] FIG. 5A is a perspective view of a wafer orientation diagram showing the orientation of a vicinal wafer relative to the c-plane. [Figure 5B] FIG. 5B is a simplified cross-sectional view of the vicinal wafer of FIG. 5A superimposed on a portion of an ingot. [Figure 6A]FIG. 6A is a top view of an exemplary SiC wafer with arrows superimposed to indicate crystallographic planes. [Figure 6B] FIG. 6B is a top view of an example SiC wafer with arrows superimposed to indicate crystallographic planes. [Figure 7] FIG. 7 is a schematic perspective view of an exemplary laser tool configured to focus laser radiation inside a crystalline material for laser separation. [Figure 8] FIG. 8 is a cross-sectional view of a SiC growth system similar to the view of FIG. 1B, with the addition of arrows showing the vapor flux between the source material and the seed crystal. [Figure 9] FIG. 9 is a cross-sectional view of a SiC growth system including a source material configured to provide a supersaturating amount of vapor flux to a seed crystal. [Figure 10] FIG. 10 is a cross-sectional view of a SiC growth system configured to provide a supersaturating amount of vapor flux to the seed crystal using a deeper crucible than the SiC growth system of FIG. [Figure 11] FIG. 11 is a cross-sectional view of a SiC growth system configured to provide a supersaturating amount of vapor flux to the seed crystal using a wider crucible than the SiC growth system of FIG. [Figure 12A] FIG. 12A is a perspective view of an exemplary SiC crystal boule according to embodiments disclosed herein. [Figure 12B] FIG. 12B is a comparative plot showing the difference in average total dislocation density (TDD) by boule position in crystalline SiC grown as described for the SiC crystal of FIG. 8 and the SiC crystal with supersaturated growth conditions of FIG. [Figure 13A] FIG. 13A is a contour plot showing TDD values for a SiC wafer grown as described for the SiC crystal of FIG. [Figure 13B] FIG. 13B is a contour plot showing TDD values for SiC wafers grown as described for the supersaturated growth conditions SiC crystals of FIG. [Figure 13C] FIG. 13C is a contour plot of FIG. 13A with the TDD values redrawn on a log10 scale. [Figure 13D] FIG. 13D is a contour plot of FIG. 13B with the TDD values redrawn on the same log10 scale as FIG. 13C. [Figure 14A] FIG. 14A is a plot showing total TDD values by radial position across the SiC wafer of FIG. 13A. [Figure 14B] FIG. 14B is a plot showing total TDD values by radial position across the SiC wafer of FIG. 13B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The embodiments set forth below represent the information necessary to enable one skilled in the art to practice the embodiments and illustrate the best modes of practicing the embodiments. By reading the following description in light of the accompanying drawings, one skilled in the art will understand the concepts of the present disclosure and will also recognize applications of these concepts not specifically addressed herein. It is understood that these concepts and applications are encompassed within the scope of the present disclosure and the appended claims.
[0016] Terms such as first, second, etc. may be used herein to describe various elements, but it is understood that these elements should not be limited by these terms. These terms are used only to distinguish one element from another. For example, a first element can be referred to as a second element, and similarly, a second element can be referred to as a first element, without departing from the scope of the present disclosure. As used herein, the term "and / or" includes any and all combinations of one or more of the items listed with it.
[0017] When an element, such as a layer, region, or substrate, is referred to as being "on" or extending "up" another element, it is understood that it may be directly on or extending directly onto the other element, or that intervening elements may be present. In contrast, when an element is referred to as being "directly on" or extending "directly onto" another element, there are no intervening elements. Similarly, when an element, such as a layer, region, or substrate, is referred to as being "on" or extending "up" another element, it is understood that it may be directly on or extending directly onto the other element, or that intervening elements may be present. In contrast, when an element is referred to as being "directly on" or extending "up" another element, there are no intervening elements. Also, when an element is referred to as being "connected" or "coupled" to another element, it is understood that it may be directly connected or coupled to the other element, or that intervening elements may be present. In contrast, when an element is referred to as being "directly connected" or "directly coupled" to another element, there are no intervening elements present.
[0018] Relative terms such as "bottom" or "top" or "upper" or "lower" or "horizontal" or "vertical" may be used herein to describe the relationship of one element, layer, or region to another element, layer, or region as shown in the figures. It is understood that these terms, and those discussed above, are intended to encompass different orientations of the device in addition to the orientation shown in the figures.
[0019] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the disclosure. As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms unless the context clearly indicates otherwise. It is further understood that the terms "comprises", "comprising", "includes" and / or "including" as used herein specify the presence of stated features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0020] The embodiments are described herein with reference to schematic diagrams of the embodiments of the present disclosure. In that case, the actual dimensions of the layers and elements may vary and variations from the shapes of the figures are possible, for example, as a result of manufacturing techniques and / or tolerances. For example, a region shown or described as a square or rectangle may have rounded or curved features, and a region shown as a straight line may have some irregularity. Thus, the regions shown in the figures are schematic, and the shapes are not intended to show the exact shape of the region of the device, nor are they intended to limit the scope of the present disclosure. Elements common between the figures may be indicated by common reference numbers herein and may not be described again thereafter.
[0021] Unless otherwise specified, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by those skilled in the art to which this disclosure belongs. It is further understood that the terms used herein should be interpreted as having a meaning consistent with their meaning in the context of the present specification and the relevant art, and are not to be interpreted in an idealized or overly formal sense unless expressly so defined herein.
[0022] Silicon carbide (SiC) wafers, SiC boules, and associated methods are disclosed that provide improved dislocation distribution. SiC boules are provided that exhibit reduced dislocation density and improved dislocation uniformity across the length of the boule. Corresponding SiC wafers have reduced total dislocation density (TDD) values with improved TDD radial uniformity. Growth conditions for the SiC crystal material include providing source material at a significantly higher supersaturation amount than the amount of source material present during growth would typically be required. Such SiC crystal material and associated methods are suitable for providing large diameter SiC boules and corresponding SiC wafers with improved crystal quality.
[0023] SiC can be a very difficult crystalline material to grow because it does not have a liquid state at atmospheric pressure, but rather transforms directly from solid to gas and back to solid. This makes SiC different from most materials in that liquid phase growth is not available. Another major challenge in growing SiC crystals is the very low stacking fault energy observed in SiC, which makes it very easy to introduce additional atomic planes and associated defect structures into the crystal lattice. This low stacking fault energy, combined with the very high temperatures used in conventional physical vapor transport growth of SiC, makes it difficult to sustain growth at conditions where the energy available from the local stress field is lower than the energy required to generate stacking faults. Crystal stress in SiC can be controlled by many factors. Crystal height and crystal diameter can play important roles, as stress can increase proportionally to the crystal height and proportionally to the square of the diameter. Conventional SiC growth techniques have achieved SiC crystals with diameters of 100 and 150 millimeters (mm). The dimensions of such SiC crystals may be limited to prevent inducing crystal stresses that exceed the critical resolved shear stress for the SiC crystal at which a high density of dislocations forms. As disclosed herein, larger diameter SiC crystals (e.g., ≧150 mm) are produced with shorter crystal heights during growth because the crystal stresses may increase excessively with the amount that the diameter is increased. In this regard, conventional crystal growth techniques are not necessarily scalable to larger diameters.
[0024] The general aspects of seeded sublimation growth processes for SiC are well established. Thus, those skilled in the art of crystal growth, particularly in the art of SiC growth and related systems, will recognize that the specific details of a technique or process may vary depending on many applicable circumstances, processing conditions, and equipment configurations. Thus, the description provided herein is best given in a general and general sense, with the understanding that those skilled in the art will be able to implement and use the various embodiments disclosed herein based on the disclosure provided without undue experimentation. In addition, those skilled in the art will recognize that SiC sublimation systems of the type described herein are commercially available in a variety of standard configurations. Alternatively, sublimation systems may be designed and implemented in custom configurations, if necessary or applicable. Thus, the embodiments described herein are not limited to a particular subset of sublimation systems, or to any particular system configuration. Instead, many different types and configurations of sublimation systems may be used to grow crystalline SiC materials according to the embodiments disclosed herein.
[0025] 1A and 1B show a method of growing a crystal according to an embodiment disclosed herein. In FIG. 1A, a crucible 100 contains a source material 102, with the interior of the crucible 100 serving as a growth zone. The source material 102 may include any suitable material, such as silicon (Si), carbon (C), SiC, silicon compounds, carbon compounds, or combinations of any or all of these in any of a variety of forms, including, but not limited to, one or more combinations of solids, powders, and gases. Other optional elements, such as dopants (e.g., nitrogen (N) among others) and strain-tuning components (e.g., germanium (Ge), tin (Sn), arsenic (As), and phosphorus (P) among others), may also be included in the source material 102. The strain-tuning components, if present, are preferably isoelectronic or have the same majority carrier type (e.g., n-type or p-type, donor or acceptor) as the dopants. Alternatively, one, some, or all of the other elements may be introduced to the growth zone in a manner other than as contained in the source material 102. A seed crystal 104, such as crystalline SiC, may be placed near the crucible lid 110, which is then placed on top of the crucible 100, as shown by the dashed arrow in FIG. 1A. In this manner, the seed crystal 104 is suspended in the crucible 100 above the source material 102 as the crucible 100 is heated. In other arrangements, the seed crystal 104 may be placed anywhere within the crucible 100, such as along the bottom or sides of the crucible 100.
[0026] During the crystal growth, the source material 102 sublimes and forms SiC on the seed crystal 104. Sublimation can occur when the source material 102 is heated to a temperature within a range including 1200° C. to 3000° C., or 1800° C. to 3000° C., or 1800° C. to 2500° C., or 1800° C. to 2000° C., or 2000° C. to 2200° C., among other temperature ranges. While the temperature of the source material 102 is being increased, the temperature of the growth surface of the seed crystal 104 is likewise increased to a temperature close to that of the source material 102. Typically, the growth surface of the seed crystal 104 is heated to a temperature in the range including 1200°C to 3000°C, or 1800°C to 3000°C, or 1800°C to 2500°C, or 1700°C to 2400°C, or 1800°C to 2000°C, or 2000°C to 2200°C, among other temperature ranges. During the growth process, the crucible 100 is slowly evacuated to a reduced pressure. In certain embodiments, the growth may be performed at a pressure in the range including 0.1 Torr to 50 Torr, or 0.1 Torr to 25 Torr, or 0.1 Torr to 15 Torr, or 1 Torr to 15 Torr, among other pressure ranges. The growth temperature and growth pressure may generally be altered relative to one another. For example, a higher growth temperature may be accompanied by a higher growth pressure, or a lower growth temperature may be accompanied by a lower growth pressure, depending on the growth conditions. By maintaining the growth surfaces of the source material 102 and the seed crystal 104 at their corresponding temperatures for a sufficient period of time, a macroscopic growth of single crystal SiC of the desired polytype can be formed on the seed crystal 104.
[0027] Referring to FIG. 1B, a SiC crystal 112 is grown from the sublimation of source material 102 in a crucible 100 using a physical vapor transport process. The crystal growth is performed until the growth of the SiC crystal 112 reaches a certain length. This length (or height from the seed crystal 104) depends, in part, on the type of post-formation processing that is to be used. The length may also be limited by various crystal quality characteristics of the SiC crystal 112, including structural crystal defects. The point at which the growth of the SiC crystal 112 is stopped also depends on parameters such as the size and type of crucible 100 and the concentration of dopants and strain-tuning components, if present in the source material 102. This point can be determined in advance by performing experimental growth in conjunction with testing the resulting SiC crystal 112 to identify the concentration of impurities. After the SiC crystal 112 reaches the desired size, the system may be backfilled with an inert gas to increase the pressure back up, and the temperature may be reduced slowly to an intermediate temperature and then more quickly to room temperature. In certain embodiments, the intermediate temperature may be about 90%, or 80%, or 70%, of the growth temperature, among other temperatures. The intermediate temperature may include a range of 150° C. to 2000° C., or 150° C. to 1200° C., or 150° C. to 500° C., or 175° C. to 225° C., among other temperature ranges. The resulting SiC crystals 112 may form a crystal boule or ingot.
[0028] Sublimation growth of SiC may be accomplished by using a variety of growth systems, different sized crucibles, different types of crucibles made of different materials, and a variety of heating methods. Specific growth temperatures and pressures can be adapted to accommodate these variables by one of ordinary skill in the art. In a typical case, if variables such as the type or size of the crucible are changed, as discussed above, several experimental growths may need to be performed to determine the best growth conditions for a particular system. After crystal growth, the SiC crystal 112 forms a bulk crystal material, sometimes referred to as a boule or ingot.
[0029] Various microelectronics, optoelectronics, and microfabrication require thin layers of crystalline materials as starting structures for manufacturing various useful systems. Various methods for forming thin layers of crystalline materials from bulk crystalline materials include sawing and laser separation techniques. In one particular embodiment, a method for cutting thin layers (e.g., wafers or substrates) from a crystalline boule or ingot involves the use of a wire saw. Wire sawing techniques have been applied to various crystalline materials such as Si, sapphire, and SiC. A wire saw tool may include an extremely fine steel wire (typically having a diameter of 0.2 mm or less) that is threaded through the grooves of one or many guide rollers. There are two types of slicing methods: loose abrasive slicing and fixed abrasive slicing. Loose abrasive slicing involves applying a slurry (typically a suspension of abrasive grains in oil) to a steel wire moving at high speed, whereby the boule or ingot is cut as a result of the rotational movement of the abrasive grains between the wire and the workpiece. In the case of fixed abrasive slicing, a wire with fixed diamond grits may be used in a manner that requires only an aqueous cooling liquid (i.e., no slurry). Highly efficient parallel slicing allows the production of multiple wafers in a single slicing step. FIG. 2 shows a typical wire saw tool 114 including parallel wire sections 116 extending between rollers 118A-118C and arranged to simultaneously saw an ingot 120 into multiple slices (e.g., wafers 122A-122G), each having a surface that is generally parallel to an edge surface 120' of the ingot 120. During the sawing process, the wire sections 116 supported by the rollers 118A-118C may be forced downward 124 toward a holder 126 that is located below the ingot 120. When end face 120' is parallel to the crystallographic c-plane of ingot 120 and wire section 116 saws ingot 120 parallel to end face 120', each of the resulting wafers 122A-122G has an "on-axis" end face 120'' that is parallel to the crystallographic c-plane.Wire sawing can introduce various stresses associated with the separation process that affect the shape of the resulting wafer, especially for large diameter wafers.
[0030] 3 is a first perspective view of the crystal planes showing the coordinate system in a hexagonal crystal such as 4H-SiC, in which the c-plane ((0001) plane), which corresponds to the 0001 (vertical) direction of epitaxial crystal growth, is perpendicular to both the m-plane ((1-100) plane) and the a-plane ((11-20) plane), but not perpendicular to the r-plane ((1-102) plane). On-axis SiC wafers with small offcuts (e.g., less than 0.5 degrees from the crystallographic c-plane) are often used as growth substrates for high-quality epitaxial growth of homoepitaxial layers of SiC as well as other materials (e.g., aluminum nitride (AlN) and other Group III nitrides).
[0031] It is also possible to produce vicinal (also known as offcut or "off-axis") wafers with edge faces that are not parallel to the crystallographic c-plane. Vicinal wafers (e.g., of SiC) that are offcut at various angles (e.g., 0.1 degrees, 0.25 degrees, 0.5 degrees, 0.75 degrees, 1 degree, 2 degrees, 4 degrees, 6 degrees, 8 degrees, or more) are often used as growth substrates for high-quality epitaxial growth of homoepitaxial layers of SiC as well as other materials (e.g., AlN and other Group III nitrides). Vicinal wafers can be produced by growing a boule or ingot in an orientation off the c-axis (e.g., growing on a vicinal seed material and sawing the ingot perpendicular to the ingot sidewalls) or by starting the ingot growth on an on-axis seed material and sawing or cutting the ingot at an angle off perpendicular to the ingot sidewalls.
[0032] FIG. 4 is a second perspective view of a crystal plane diagram in a hexagonal crystal showing a plane 128 that is not parallel to the c-plane, in which vector 130 (perpendicular to plane 128) is tilted at a tilt angle β from the
[0001] direction, and the tilt angle β is (slightly) tilted toward the [11-20] direction.
[0033] FIG. 5A is a perspective view of a wafer orientation diagram showing the orientation of a vicinal wafer 132 relative to the c-plane ((0001) plane), where vector 130A (perpendicular to wafer plane 132′) is tilted from the 0001 direction by tilt angle β. This tilt angle β is equal to the orthogonal tilt (or misorientation angle) β between the (0001) plane and a projection 134 of the wafer plane 132′. FIG. 5B is a simplified cross-sectional view of a vicinal wafer 132 superimposed on a portion of an ingot 135 (e.g., an on-axis ingot having an end face 135′ that is parallel to the (0001) plane along which the vicinal wafer 132 may be defined). FIG. 5B shows that the wafer plane 132′ of the vicinal wafer 132 is misaligned with the (0001) plane by tilt angle β.
[0034] 6A and 6B are plan views of exemplary SiC wafers 136-1 and 136-2, each including an upper surface 136′ (e.g., parallel to the (0001) plane (c-plane) and perpendicular to the
[0001] direction) and laterally bounded by a roughly circular edge 136″ (having a diameter Φ). In FIG. 6A , the circular edge 136″ of SiC wafer 136-1 includes a major flat 138 (having a length L ) perpendicular to the (11-20) plane and parallel to the [11-20] direction. F In FIG. 6B, the circular edge 136'' of the SiC wafer 136-2 includes a notch 140 instead of the primary flat 138 shown in FIG. 6A. Depending on the particular application, the notch 140 may be provided for compatibility with various semiconductor manufacturing tools in which the SiC wafer 136-2 may be processed. As previously mentioned, the SiC wafers 136-1, 136-2 may be misaligned with the c-plane (e.g., off-axis at an oblique angle to the c-plane).
[0035] Another method for separating a wafer or substrate from a bulk crystalline material includes a laser separation technique that involves forming a superficial laser damage in the bulk crystalline material and then separating the wafer from the bulk crystalline material along the superficial laser damage. A tool for forming superficial damage in a crystalline material allows for focusing laser radiation inside the crystalline material and for moving the laser laterally relative to the crystalline material. A typical laser damage pattern may include the formation of parallel lines spaced laterally relative to each other at a depth within the crystalline material. Parameters such as focus depth, laser power, movement speed, and superficial damage line spacing can be adjusted to impart laser damage, although adjustment of certain factors involves tradeoffs. Increasing laser power tends to impart larger surface damage, which may improve fracture susceptibility (e.g., by lowering the stress required for complete fracture), but larger surface damage increases surface irregularities along the surfaces exposed by the fracture, which may require additional processing to make such surfaces smooth enough for subsequent processing (e.g., for incorporation into an electronic device), which leads to further kerf loss. Reducing the lateral spacing of the surface laser damage lines may also improve fracture susceptibility, but reducing the spacing between laser damage lines increases the number of travel passes between the substrate and the laser, thereby reducing tool throughput. Such laser separation techniques may reduce kerf loss compared to wire sawing techniques. Kerf loss refers to the total amount of material loss associated with forming individual wafers from a bulk crystalline material.
[0036] FIG. 7 is a schematic perspective view of an example of a laser tool 142 configured to focus laser radiation within a crystalline material 144 (e.g., SiC, etc.) to form a superficial damage 146. The crystalline material 144 includes an upper surface 144′ and an opposing lower surface 144″, and the superficial damage 146 is formed within the crystalline material 144 between the upper surface 144′ and the lower surface 144″. The laser radiation 148 is focused by a lens assembly 150 to obtain a focused beam 152, the focal point of which is within the crystalline material 144. Such laser radiation 148 may be pulsed at any suitable frequency (typically in the nanosecond, picosecond, or femtosecond range) and beam intensity, with a wavelength below the bandgap of the crystalline material 144, allowing the laser radiation 148 to be focused at a targeted depth below its surface. At the focal point, the beam size and short pulse width result in an energy density high enough to result in very localized absorption that forms the superficial damage 146. One or more characteristics of the lens assembly 150 may be altered to adjust the focus of the focused beam 152 to a desired depth within the crystalline material 144. As shown diagrammatically by the dashed lines, relative lateral movement (e.g., translation) between the lens assembly 150 and the crystalline material 144 may be performed to advance the superficial damage 146 in a desired direction 154. Such lateral movement may be repeated in a variety of patterns, including those described below.
[0037] As used herein, "substrate" or "wafer" refers to a crystalline material, such as a single crystal semiconductor material. In certain embodiments, the substrate may have (i) a sufficient thickness to perform surface processing (e.g., lapping and polishing) to support epitaxial deposition of one or more layers of semiconductor material, and, if desired, (ii) a sufficient thickness to be self-supporting when separated from a rigid carrier. In certain embodiments, the substrate may have a roughly cylindrical or circular shape and / or may have at least about one or more of the following thicknesses: 200 microns (μm), 300 μm, 350 μm, 500 μm, 750 μm, 1 mm, 2 mm, or more or less than these. In certain embodiments, the substrate may include a thicker substrate that is divisible into two thinner substrates. In certain embodiments, the substrate may be part of a thicker substrate or wafer with one or more epitaxial layers (optionally with one or more metal contacts) disposed on the wafer as part of a device wafer with multiple electrically operating devices. The device wafer may be split according to aspects of the present disclosure to obtain a thinner device wafer and a second thinner wafer on which one or more epitaxial layers (optionally with one or more metal contacts) may be subsequently formed. In certain embodiments, the large diameter wafer or substrate may have a diameter of 145 mm or more, or 150 mm or more, or 195 mm or more, or 200 mm or more, or 300 mm or more, or 450 mm or more, or within a range including 145 mm to 455 mm, or 195 mm to 455 mm, or 145 mm to 205 mm.In certain embodiments, the wafer or substrate may comprise 4H-SiC having a diameter of 145 mm or more, or 150 mm or more, or 195 mm or more, or 200 mm or more, and a thickness in the range of 100 μm to 1000 μm, or in the range of 100 μm to 800 μm, or in the range of 100 μm to 600 μm, or in the range of 150 μm to 500 μm, or in the range of 150 μm to 400 μm, or in the range of 200 μm to 500 μm, or in the range of 300 μm to 1000 μm, or in the range of 500 μm to 2000 μm, or in the range of 500 μm to 1500 μm, or any other thickness range or any other thickness value specified herein. In certain embodiments, the terms "substrate" and "wafer" may be used interchangeably, since a wafer is typically used as a substrate for semiconductor devices that may be formed thereon. Thus, a substrate or wafer can refer to a larger bulk crystalline material or a free-standing crystalline material separated from a substrate.
[0038] With respect to relative dimensions, the term "approximately" is defined to mean a nominal dimension within a certain tolerance, such as plus or minus 5 mm from the diameter dimension. For example, as used herein, a "150 mm" diameter wafer may encompass a diameter range including 145 mm to 155 mm, a "200 mm" diameter wafer may encompass a diameter range including 195 mm to 205 mm, a "300 mm" diameter wafer may encompass a diameter range including 295 mm to 305 mm, and a "450 mm" diameter wafer may encompass a diameter range including 445 mm to 455 mm. In further embodiments, such tolerances may be less, such as plus or minus 1 mm or plus or minus 0.25 mm.
[0039] The embodiments disclosed herein can be applied to substrates or wafers of various crystalline materials, both monocrystalline and polycrystalline. In certain embodiments, the substrates or wafers may include cubic, hexagonal, and other crystalline structures, and may include crystalline materials having on-axis and off-axis crystal orientations. Exemplary embodiments may include monocrystalline semiconductor materials having hexagonal crystal structures, such as 4H-SiC or 6H-SiC. Various exemplary embodiments described hereinafter refer to SiC generally or specifically to 4H-SiC, although it should be understood that other suitable crystalline materials may be used. Among the various SiC polytypes, the 4H-SiC polytype is particularly attractive in power electronic devices due to its high thermal conductivity, wide band gap, and isotropic electron mobility. The embodiments disclosed herein may be applicable to on-axis SiC (i.e., no intentional angular deviation from its c-plane) or off-axis SiC (i.e., typically offset at a non-zero angle from a growth axis such as the c-axis, typically within the range of 0.5-10 degrees, or within a sub-range therein, such as 2-6 degrees or another sub-range). Certain embodiments disclosed herein may use on-axis 4H-SiC, or vicinal (off-axis) 4H-SiC with an offcut within a range including 1-10 degrees or 2-6 degrees, or about 2, 4, 6, or 8 degrees.
[0040] The embodiments disclosed herein may also be applied to doped crystalline semiconductor materials (e.g., N-doped conductive SiC and / or P-doped SiC), co-doped, and / or undoped crystalline semiconductor materials (e.g., semi-insulating SiC or high resistivity SiC). In certain embodiments, SiC crystalline materials, including SiC boules and SiC wafers, among others, are 1×10 17 cm -3 ~1×10 21 cm -3 Within the range including 1×10 17 cm -3 ~3×10 18 cm -3 Within the range including 1×10 18 cm -3 ~1×1019 cm -3 Within the range of 1×10 18 cm -3 ~3×10 18 cm -3 Within the range of 1×10 17 cm -3 In certain embodiments, the N-doped SiC crystal material may have a resistivity in the range of 0.001 Ω·cm to 0.05 Ω·cm, inclusive, or in the range of 0.001 Ω·cm to 0.03 Ω·cm, inclusive, or in the range of 0.005 Ω·cm to 0.05 Ω·cm, or in the range of 0.005 Ω·cm to 0.03 Ω·cm. In other embodiments, higher resistivity SiC crystal materials, including semi-insulating SiC boules and semi-insulating SiC wafers, may have a resistivity of at least 1500 Ω·cm, or at least 5000 Ω·cm, or at least 50,000 Ω·cm, or at least 1×10 5 Ω cm, or at least 1×10 6 Ω cm, or at least 1×10 9 Ω cm, or 1500 Ω cm to 1×10 9 Within the range including Ω cm or 1×10 5 Ω cm~1×10 9 Semi-insulating SiC wafers may include unintentionally doped or undoped SiC having resistivity in the range including Ω·cm. Semi-insulating SiC wafers may be doped with vanadium (V), aluminum (Al), or combinations thereof. Co-doped SiC wafers may include combinations of two or more dopants such as N, Al, and V, among others, depending on the embodiment.
[0041] Crystalline SiC may contain various structural crystal defects including dislocations (e.g., micropipes, threading edge, threading screw, and / or basal plane dislocations, among others), hexagonal voids, and stacking faults. Structural crystal defects may form during crystal growth and / or during cooling after growth, resulting in one or more discontinuities in the material lattice structure of the crystalline SiC. Such structural crystal defects may be detrimental to the fabrication, proper operation, device yield, and reliability of semiconductor devices subsequently formed on the SiC wafer. The presence of various structural crystal defects may result in stresses in a free-standing SiC wafer, which may contribute to various deviations in wafer shape (e.g., reduced flatness characteristics). Further deviations to the wafer shape may be formed during separation of the wafer from the boule or ingot by either wire cutting or laser separation techniques, as previously mentioned.
[0042] During bulk growth, crystal defects tend to initially form at higher densities in the portions of the SiC boule closer to the seed. As growth progresses further away from the seed, the crystal defect density may decrease in the center of the SiC boule, and then increase to levels closer to or even higher than the earlier portions of the SiC boule. In this regard, the center of the SiC boule typically yields the most useful SiC wafers, while the overall boule length may be limited by the increased defect density, especially for larger boules. According to embodiments disclosed herein, growth conditions for SiC boules are provided that exhibit a decrease in defect density, including at later stages of growth, thereby enabling the growth of longer SiC boules with increased yields of SiC wafers with lower defect densities. In certain embodiments, such growth conditions include providing source material at a significantly higher supersaturation amount than the amount of source material present during growth would typically be required for growth. Under this growth condition, an increased portion of the source material may not be incorporated into the growing SiC boule, thereby increasing the amount of waste source material that may be lost to parasitic deposition in the crucible or through evacuation while maintaining the crucible at a certain pressure, if any. As disclosed herein, growth under such conditions of supersaturated source material, previously considered wasteful, can provide crystalline SiC with reduced dislocation density and longer overall length SiC boules. This can be particularly useful for large diameter SiC boules, such as greater than 145 mm, where defect density may limit the useful boule length.
[0043] 8 is a cross-sectional view of a SiC growth system 156 including a crucible 100, source material 102, seed crystal 104, and crucible lid 110 used to form a SiC crystal 112 as described for FIG. 1B. Both source material 102 and seed crystal 104 are generally contained within crucible 100, and source material 102 may be positioned above, below, or adjacent to seed crystal 104. In certain embodiments, crucible 100 may be made of a material that is relatively stable to Si- and C-containing gases. In certain embodiments, crucible 100 may include one or more of graphite, tantalum carbide (TaC)- and niobium carbide (NbC)-coated graphite, and solid TaC and NbC, among others. In certain embodiments, the crucible 100 may be sealed to prevent gas leakage or may be partially open to allow some gas to flow out of the crucible 100. In certain embodiments, the crucible 100 may be electrically conductive to allow induction heating, while in other embodiments, radiative heating may be used, and in still other embodiments, a combination of induction and radiative heating may be used. In certain embodiments, the temperature profile within the crucible 100 may be controlled to take into account the amount of heat input into the system and to control heat flow through the use of insulating baffles. In certain embodiments, the source material 102 may be maintained at a higher temperature than the seed crystal 104 such that a temperature gradient is created within the crucible 100. This temperature gradient helps to cause the transport of the vapor flux 158 containing Si- and C-containing gas species from the source material 102 to the seed crystal 104. A vapor flux 158 may be delivered by gas flow from the source material 102 to the seed crystal 104 as the source material 102 sublimes and condenses on the seed crystal 104 to form a SiC crystal 112. In certain embodiments, the gas source may be delivered through a high temperature region to allow the gas to break down into its constituent parts to interact with the seed crystal 104, or the various gas species may directly interact with the seed crystal 104. In certain embodiments, one or more radio frequency electric fields are used to assist the gas breakdown process.
[0044] The growth conditions for the SiC crystal 112 may typically be implemented by providing a vapor flux 158 to the seed crystal 104 to deposit Si and C constituents thereon. There are many ways to achieve this, and embodiments described herein are provided to modify certain aspects of the SiC crystal growth to reduce crystal defects in the SiC boule and resulting SiC wafers. The vapor flux 158 may be provided by generating one or more of SiC, SiC2, Si2C, and Si gases through heating of a source material 102, which may include one or more of: polycrystalline SiC; single crystal SiC; polymers of Si and C; a mixture of Si and C powders with a Si to C ratio of 1:1 or within a 20% tolerance of the 1:1 ratio; a mixture of SiC, Si, and C powders with a Si to C ratio of 1:1 or within a 20% tolerance of the 1:1 ratio; pucks or chunks of amorphous or crystalline SiC (e.g., polycrystalline or single crystal); and a porous mesh of SiC. In certain embodiments, a gas source may be used to provide the vapor flux 158, either separately or in addition to the source material 102 described above. Such gas sources may include one or more species such as SiH4, Si2H6, SiCl2H2, SiCl3H, SiCl4, CH4, C2H6, and Si(CH3)4. In embodiments including a combination of gas and solid sources, the ratio of Si to C in the solid source may be altered away from 1:1 since a portion of the Si or C supply is provided by the gas.
[0045] In certain embodiments, these raw materials may contain primarily pure SiC, but impurities may often be added to achieve deliberate doping of the crystal, modification of surface energy, deliberate creation of point defects, and modification of lattice size. These impurities may include almost any element in the periodic table, and often include Group III elements such as boron (B) for p-type doping, or atoms with larger atomic radii, including N, Ge, and Sn, V, and some lanthanides for n-type doping, to modify surface energy and resultant crystal lattice parameter size changes, or induce deep level electrical defects.
[0046] FIG. 9 is a cross-sectional view of a SiC growth system 160 including a source material 162 configured to provide a supersaturated amount of vapor flux 164 to the seed crystal 104 that is greater than the amount required for crystal growth. In certain embodiments, the source material 162 may have a higher density than the source material 102 of FIG. 8. In this regard, an increased amount of vapor flux 164 may be provided to the seed crystal 104 at otherwise similar growth conditions. In other embodiments, the source material 162 may have a similar density to the source material 102 of FIG. 8, and an increased amount of vapor flux 164 may be provided by modifying one or more growth conditions, such as temperature and pressure. For example, the overall temperature within the crucible 100 may be increased, or the temperature of the source material 162 may be increased relative to the seed crystal 104. In certain embodiments, the growth pressure within the crucible 100 may be reduced to provide an increased vapor flux 164. Additionally, the increased vapor flux 164 may be provided by one or more combinations of increasing the density of the source material 162, increasing the growth temperature, and decreasing the growth pressure, as discussed above. Because the vapor flux 164 is provided in a supersaturated state, parasitic deposition may occur within the crucible 100 away from the seed crystal 104, or some of the vapor flux 164 may be exhausted through the exhaust of the SiC growth system 160 without depositing or sublimating. Providing a supersaturated vapor flux 164 may result in the formation of a SiC crystal 166 with a reduced defect density relative to the SiC crystal 112 of FIG. 8, particularly as the SiC crystal 166 continues to grow further away from the seed crystal 104.
[0047] 10 is a cross-sectional view of a SiC growth system 168 configured to provide a supersaturating amount of vapor flux 170 to the seed crystal 104 using a deeper crucible 172 than the crucible 100 of the SiC growth system 156 of FIG. 8. As shown, by providing the crucible 172 with a deeper dimension, the amount of source material 162 to the seed crystal 104 may be increased. In this regard, the overall volume of source material 162 to the seed crystal 104 may be increased to provide an increased amount of vapor flux 170. In certain embodiments, the source material 162 may have the same density as the source material 102 of FIG. 8. In certain embodiments, the amount of vapor flux 170 may be further increased by providing one or more combinations of an increased density of the source material 162, an increased growth temperature, and a decreased growth pressure, as described in FIG.
[0048] 11 is a cross-sectional view of a SiC growth system 174 configured to provide a supersaturating amount of vapor flux 176 to the seed crystal 104 using a wider crucible 178 than the crucible 100 of the SiC growth system 156 of FIG. 8. As shown, by providing the wider dimension of the crucible 178, the amount of source material 162 to the seed crystal 104 may be increased. Similar to the deeper crucible 172 of FIG. 10, the overall volume of source material 162 to the seed crystal 104 may be increased to provide an increased amount of vapor flux 176. In certain embodiments, the source material 162 may have the same density as the source material 102 of FIG. 8. In certain embodiments, the amount of vapor flux 176 may be further increased by providing one or more combinations of an increased density of the source material 162, an increased growth temperature, and a decreased growth pressure, as described in FIG. 9.
[0049] 12A is a perspective view of an exemplary SiC crystal boule 180 according to embodiments disclosed herein. As shown, the SiC crystal boule 180 includes a first end face 182, a second end face 184 opposite the first end face 182, a side face 186 therebetween that may form a generally cylindrical shape along the circumference of the SiC crystal boule 180, and a central axis 188. Depending on the application, the first end face 182 may correspond to a crystallographic c-plane and the central axis 188 may correspond to a 0001 direction. In other embodiments, the first end face 182 may correspond to an off-axis plane relative to the crystallographic c-plane, or the first end face 182 may correspond to another crystallographic plane of SiC. During growth, the second end face 184 grows first closest to the seed crystal (e.g., 104 in FIG. 9 ) and the remainder of the SiC crystal boule 180 grows away from the seed crystal (e.g., 104 in FIG. 9 ). Boule length or height 190 may be measured from second end face 184 to first end face 182, and boule diameter 192 may be measured across first end face 182. In FIG. 12A , a curved dashed line is superimposed on SiC crystal boule 180 to indicate the location of an exemplary SiC wafer 194 that may be separated from SiC crystal boule 180.
[0050] During the crystal growth process, various structural crystal defects may form in the material composition of the SiC crystal boule 180, including dislocations (e.g., micropipes, threading edge, threading screw, and / or basal plane dislocations), hexagonal voids, and stacking faults, among others. As described herein, TDD or total dislocation density may be defined as the total number of all micropipes and other dislocations (e.g., threading edge, threading screw, and / or basal plane dislocations) in any region of the SiC material. To quantify the number of TDDs in any region or area of the SiC crystal boule 180, defect characterization is performed on one or more SiC wafers separated from the SiC crystal boule 180. In further embodiments, multiple SiC wafers from different vertical positions of the SiC boule 180 may be quantified to obtain an overall TDD profile for the SiC boule 180. In certain embodiments, synchrotron x-ray topography (SXRT) may be used to characterize TDD values, but SXRT may not always be practical in a manufacturing environment where results typically need to be obtained quickly. Etch-based dislocation characterization is more commonly used to obtain results more quickly over larger wafer areas, but interpretation of etch-based results may be less accurate than that of SXRT. For example, in some etch-based dislocation characterization techniques, etching may cause closely spaced micropipes to merge together, resulting in counting and reporting as a single micropipe when in fact there are two or more micropipes. In this regard, many existing literature reports may under-report actual TDD values for SiC materials. To ensure accuracy of etch-based dislocation characterization results, etching protocols have been developed that produce recognizable and unique features associated with each dislocation type.
[0051] Etching SiC reveals features such as etch pits that are recognizable and can be correlated with other characterization methods such as SXRT. Etching-based characterization can be accomplished by accurately delineating the etch pits, identifying the corresponding defect type, and counting them manually or with automated microscopy tools. Wafer etching is substantially destructive of the useful wafer area, is costly, requires corrosive chemicals, and requires constant care to maintain a viable process. In this regard, in practice, only a few sacrificial wafers per boule are typically sampled. As an example, to perform defect characterization on SiC wafers, the carbon side (C-side) of the SiC wafer is etched to highlight extended defects, and the SiC wafer is subsequently imaged. For example, n-type doped SiC wafers (>10 17 cm 2 Or ≒ 10 17 cm 2) may be etched with molten salts (KOH / EOH) and then the SiC wafer is scanned and image processed for defect detection. The observed etch pits and defects are then identified, counted and reported for dislocation type either manually or by automated defect recognition. An optical scanner or manual or automated optical microscope may be used for counting defects from the images. For materials that are not properly doped (low doped n-type, or insulating and p-type), this method may not work well due to poor delineation of defects by the etching method. In addition, the silicon side (Si-face) of the SiC wafer may also be etched to characterize the etching from the Si-face. Etching the Si-face may provide more accurate counting of micropipes and basal plane dislocations, while etching the C-face may provide more accurate counting of threading screw dislocations. Thus, an improvement in accuracy to TDD etching-based dislocation characterization should include combining counting of identified defects from both the C-face and Si-face of a representative SiC wafer. Further discussion of etch-based characterization protocols for accurate TDD counts can be found in “Dislocation Characterization in 4H-SiC Crystals” by Sumakeris et al., published in Materials Science Forum 858 (2016) 393. Another characterization technique that can be used to characterize the TDD values of SiC wafers can include analyzing non-destructive images of SiC wafers using a deep convolutional neural network (DCNN) trained for defect identification in destructively etched wafer images, as shown in U.S. patent application Ser. No. 16 / 750,358, filed Jan. 23, 2020, entitled “NONDESTRUCTIVE CHARACTERIZATION FOR CRYSTALLINE WAFERS,” the entire contents of which are incorporated herein by reference.
[0052] FIG. 12B is a comparative plot showing the difference in average TDD by boule position for crystalline SiC grown as described for SiC crystal 112 of FIG. 8 and SiC crystal 166 of FIG. 9 under supersaturated growth conditions. In both data sets, SiC crystals 112, 166 comprise 4H-SiC material. The x-axis represents the corresponding boule position in mm from which the SiC wafers were taken, where the boule position is measured as the distance from the seed crystal from which the boule was grown. The data set obtained for SiC crystal 112 includes data from a representative number of SiC boules grown with a boule diameter of approximately 150 mm. For comparison purposes, a representative number of SiC boules with a boule diameter of approximately 150 mm were grown according to the growth conditions for SiC crystal 166. The y-axis represents the square centimeters (cm ) for the SiC wafers obtained at each of the corresponding boule positions. 2 ) for each individual SiC wafer. For each individual SiC wafer, the TDD was determined for a wafer region bounded by a perimeter having a radius that includes the center of the SiC wafer and is 2 mm from the edge of the SiC wafer along the wafer radial position. As shown, the data sets for both SiC crystals 112, 166 show increasing average TDD values at lower boule positions (e.g., 10 mm) where growth is closer to the seed. Both data sets show generally decreasing average TDD values as the boule initially grows away from the seed (e.g., from 10 mm to about 20 mm). The data set for SiC crystal 112 shows a steep increase in average TDD values at a boule position of about 40 mm, thereby limiting the boule height, while the data set for SiC crystal 166 shows a continued decrease in average TDD as the boule position approaches 70 mm. Additionally, the SiC crystal 166 data set exhibits significantly lower average TDD values at all common boule locations (e.g., 10-50 mm) compared to the SiC crystal 112 data set, along with a continued drop in average TDD values at higher boule locations (e.g., >50 mm to 65 mm). For example, an individual SiC boule included in the SiC crystal 166 data set exhibits a 1 cm average TDD at the 8.3 mm boule location. 2 4572 TDD values per cm, 24.3 mm 22529 TDD values per cm, and 41.5 mm per cm 2 In this regard, for boule heights of 40 mm or greater, at least 40%, or at least 50%, or at least 75%, or at least 80% of the height of an individual SiC boule is configured to provide a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers being 1 cm 2 4600 TDD or less per cm 2 1000~1cm 2 In addition, at least 40% of the height of the individual SiC boules is configured to provide a plurality of SiC wafers, each SiC wafer of the plurality of SiC wafers having a TDD in the range of 1 cm 2 3000 TDD or less per cm 2 1000~1cm 2 In certain embodiments, supersaturated growth conditions for the SiC crystals 166 may be applied to produce boule heights as high as 300 mm with very low average TDD values. In certain embodiments, the boule height is in the range of 60 mm to 300 mm, inclusive, or in the range of 55 mm to 80 mm, inclusive, or in the range of 60 mm to 80 mm, inclusive, or in the range of 60 mm to 70 mm, inclusive, or in the range of greater than 50 mm and less than or equal to 65 mm, or in the range of greater than or equal to 55 mm and less than or equal to 65 mm. In certain embodiments, the boule diameters mentioned above are in the range of 145 mm to 180 mm, inclusive. As further shown in FIG. 12B, SiC wafers taken from boule positions of 40 mm or greater can be grown to a diameter of 1 cm. 2 The Boolean positions for such TDD values may be in the range of 40 mm to 300 mm, or 40 mm to 80 mm, or 50 mm to 65 mm, or 60 mm to 300 mm, or 60 mm to 80 mm, inclusive. The TDD values may be in the range of 1 cm to 300 mm, inclusive, or 60 mm to 80 mm, inclusive, depending on the embodiment. 2 The SiC wafer can also have a surface area of 1 cm or less. 2 2500 or less per cm 2 The TDD may be up to 1500 per
[0053] FIG. 13A is a contour plot showing TDD values for a SiC wafer 196 grown as described for the SiC crystal 112 of FIG. 8. For comparison, FIG. 13B is a contour plot showing TDD values for a SiC wafer 198 grown as described for the SiC crystal 166 of FIG. 9 under supersaturated growth conditions. For comparison purposes, SiC wafers 196, 198 were selected that are approximately 150 mm in diameter. In this manner, the x and y axes in both contour plots of FIG. 13A and FIG. 13B are shown in + and - mm values, with 0 mm representing the center point of the SiC wafer 196, 198. The SiC wafers 196, 198 were taken from their respective boules near the end of the boule that was formed furthest from the seed crystal during growth. The contour scales of the TDD values in FIG. 13A and FIG. 13B are intentionally kept the same for comparison purposes. The results shown in Figures 13A and 13B are determined by an xy mapping method that defines a grid of 5 mm x 5 mm square regions over the entire wafer. Four of such square regions are aligned with the radial center of the wafer. Exclusion regions, including the peripheral region 2 mm from the wafer edge and additional regions corresponding to the main and / or secondary wafer flats, are not counted. As shown, the SiC wafer 196 exhibits regions of significantly increased TDD near the wafer center and along the wafer periphery. At the same scale, the TDD value for the SiC wafer 198 is almost undetectable in Figure 13B. In this regard, the SiC wafer 198 in Figure 13B exhibits significantly lower and more uniform TDD values over the entire wafer area than the SiC wafer 196 in Figure 13A.
[0054] Figures 13C and 13D show the contour plots of Figures 13A and 13B, respectively, with the TDD values redrawn on a log10 scale. As can be seen, the contour plot of Figure 13C exhibits the same regions of rapidly increasing TDD near the wafer center and along the wafer periphery. In Figure 13D, the log10 scale improves the visibility of the TDD variations in the SiC wafer 198. Notably, the SiC wafer 198 does not have any regions of rapidly increasing TDD, thus significantly improving uniformity.
[0055] FIG 14A is a plot showing TDD values as a function of radial position across the SiC wafer 196 of FIG 13A. For comparison, FIG 14B is a plot showing TDD values as a function of radial position across the SiC wafer 198 of FIG 13B. In each of FIG 14A and FIG 14B, the y-axis is in units of 1 cm. 2 14A represents TDD per unit area, and the x-axis represents the wafer radial position in mm, with a value of 0 corresponding to the wafer center and a value of 75 corresponding to the wafer edge. The results shown in FIG. 14A were determined by radial mapping methodology, where the wafer radial position indicates the outer diameter of the annular ring (in mm), and the width of the annular ring from the outer diameter is set to 1 mm. The exception is that the wafer radial position of 3 mm corresponds to a circle containing the wafer center (0 mm), because an annular ring at such a position would be too small in area to obtain accurate results. Another exception is that the portions of the outer wafer radial position that are inlaid with exclusion areas corresponding to the primary and / or secondary wafer flats are not counted.
[0056] In FIG. 14A, the TDD value is 1 cm at a radial position from 0 mm (wafer center) to 10 mm. 2 More than 4500 per cm at radial positions between 10 mm and 25 mm 2 At radial positions of more than 6000 per cm and 60 mm to 75 mm (wafer edge), 2In FIG. 14B, the SiC wafer 198 shows a sharp peak of more than 6000 per cm at any radial position within a range of 3 mm to 50 mm from the wafer center, or within a range of 3 mm to 70 mm, or within a range of 3 mm from the wafer center to 2 mm from the edge of the wafer. 2 5000 or less per cm 2 4000 or less per cm 2 3000 or less per cm 2 2500 or less per cm 2 1000~1cm 2 14B, TDD data is provided out to a radial position of 73 mm, taking into account a peripheral 2 mm exclusion ring. In one particular embodiment, TDD values are within 1 cm at any radial position within 50 mm or 70 mm of the center of the SiC wafer 198. 2 3000 or less per cm 2 2500 or less per cm 2 1000~1cm 2 In particular, the SiC wafer 198 has a radial distance of 1 cm at any radial position between 10 mm and 57 mm, inclusive. 2 In other words, the TDD is less than 2000 per cm in any annular ring portion having a width of 1 mm and an outer diameter corresponding to the wafer radial positions for at least 50% or at least 60% of all radial positions of the SiC wafer 198. 2 Further, the SiC wafer 198 has a radial position of 13 mm to 50 mm inclusive, and the SiC wafer 198 has a radial position of 1 cm 2 In other words, the TDD is less than 1500 per cm in any annular ring portion having a width of 1 mm and an outer diameter corresponding to the wafer radial positions for at least 40% or at least 50% of all radial positions of the SiC wafer 198. 2 It is less than 1500 per
[0057] As disclosed herein, supersaturated growth conditions for SiC crystals can result in SiC boules and, consequently, SiC wafers with significantly improved uniformity of TDD distribution. One method for characterizing TDD uniformity involves quantifying the coefficient of variation of TDD, which is defined as the ratio of the standard deviation to the average TDD value in a particular SiC wafer. In this regard, the coefficient of variation of TDD can indicate the degree of variation of TDD relative to the average TDD. For example, the SiC wafer 196 represented by the plots in Figures 13A, 13C, and 14A has a 1 cm2 TDD distribution for a wafer area divided into 1 mm wide annular rings. 2 Calculated TDD standard deviation of 1576 per cm 2 13B, 13D, and 14B has an average TDD value of 3338 per wafer area bounded by a wafer radial position of 3 mm from the center of the SiC wafer 196 and 2 mm from the edge of the SiC wafer 196. In this regard, the coefficient of variation of the TDD of the SiC wafer 196 is 0.472. In comparison, the SiC wafer 198 represented by the plots of FIGS. 13B, 13D, and 14B has an average TDD value of 1 cm for a wafer area divided into 1 mm wide annular rings. 2 449 calculated TDD standard deviations per cm 2 The SiC wafer 198 has an average TDD value of 1612 per wafer, bounded by a wafer radial position of 3 mm from the center of the SiC wafer 198 and 2 mm from the edge of the SiC wafer 198. Thus, the coefficient of variation of the TDD of the SiC wafer 198 is 0.28, indicating that the TDD becomes significantly more uniformly distributed when the SiC boule is grown according to the supersaturated growth conditions described above. In certain embodiments, the coefficient of variation is 0.2 or less, or in the range of 0.1 to 0.3. Another method for characterizing the uniformity of the TDD may include simply characterizing the standard deviation value for each SiC wafer.
[0058] Although the above examples are provided for SiC wafers with a diameter of approximately 150 mm, the exemplary embodiments are applicable to SiC wafers with other diameters, including less than approximately 150 mm or more than approximately 150 mm. In certain embodiments, the SiC wafers may have a diameter of approximately 200 mm, or approximately 300 mm, or approximately 450 mm. In addition to the 4H-SiC provided in the examples, the exemplary embodiments are also applicable to other polytypes of SiC, including but not limited to 6H-SiC. As previously mentioned, the embodiments disclosed herein are applicable to both doped crystalline semiconductor materials (e.g., N-doped conductive SiC and / or P-doped SiC), co-doped, and / or undoped crystalline semiconductor materials (e.g., semi-insulating SiC or high resistivity SiC).
[0059] It is contemplated that any of the above aspects, and / or various separate aspects and features described herein may be combined for added advantage. Any of the various embodiments disclosed herein may be combined with one or more of the other disclosed embodiments, unless otherwise indicated herein to the contrary.
[0060] Those skilled in the art will recognize improvements and modifications to the preferred embodiments of the present disclosure, and all such improvements and modifications are deemed to be within the spirit and scope of what is disclosed in this specification and the following claims.
Claims
1. A silicon carbide (SiC) wafer having a diameter of at least 145 millimeters (mm), a width of 1 mm, and an outer diameter of 1 square centimeter (cm) at any annular ring portion corresponding to a radial position of the wafer within a range of 3 mm to 50 mm from the center of the SiC wafer. 2 a total dislocation density (TDD) of 3000 or less per 1000 cm-thick steel sheet; The TDD is the total number of micropipes, threading edge dislocations, threading screw dislocations, and basal plane dislocations; Silicon carbide (SiC) wafers.
2. The TDD has a width of 1 mm, and the outer diameter is within a range from a position 3 mm from the center of the SiC wafer to a position 2 mm from the peripheral edge of the SiC wafer, and the outer diameter is within a range from a position 3 mm from the center of the SiC wafer to a position 2 mm from the peripheral edge of the SiC wafer. 2 The SiC wafer of claim 1 , wherein the number of defects is 3000 or less per defect.
3. The TDD has a width of 1 mm, and the outer diameter is within 1 cm at any annular ring portion corresponding to a radial position of the wafer within a range of 3 mm to 50 mm from the center of the SiC wafer. 2 2. The SiC wafer of claim 1 , wherein the number of defects is 2500 or less per defect.
4. The TDD has a width of 1 mm and an outer diameter of 1 cm or less at any annular ring portion corresponding to the wafer radial positions for at least 50% of all wafer radial positions of the SiC wafer. 2 The SiC wafer of claim 1 , wherein the number of defects is 2000 or less per defect.
5. The TDD has a width of 1 mm and an outer diameter of 1 cm or less at any annular ring portion corresponding to the radial positions of the wafer for at least 50% of all radial positions of the SiC wafer. 2 2. The SiC wafer of claim 1, wherein the number of defects is 1500 or less per defect.
6. 2. The SiC wafer of claim 1, wherein the diameter is in the range of 145 mm to 205 mm inclusive.
7. 2. The SiC wafer of claim 1, wherein the diameter is in the range of 145 mm to 155 mm inclusive.
8. 10. The SiC wafer of claim 1 comprising a 4H—SiC wafer.
9. 10. The SiC wafer of claim 1 comprising semi-insulating SiC.
10. 10. The SiC wafer of claim 1 comprising n-type SiC.
11. The TDD is 1000 cm 2 The SiC wafer according to claim 1 .
12. A silicon carbide (SiC) wafer having a diameter that is at least 145 millimeters (mm) and a coefficient of variation of total dislocation density (TDD) that is less than or equal to 0.3 across the wafer; The wafer region is divided into annular ring portions each having a width of 1 mm and is surrounded by a boundary line at a radial position of the wafer that is 3 mm from the center of the SiC wafer and 2 mm from the peripheral edge of the SiC wafer; The coefficient of variation is defined as the ratio of the standard deviation to the average TDD value in the annular ring portion, where TDD is the total number of micropipes, threading edge dislocations, threading screw dislocations, and basal plane dislocations. Silicon carbide (SiC) wafers.
13. The SiC wafer of claim 12, wherein the coefficient of variation is 0.2 or less.
14. The SiC wafer according to claim 12, wherein the coefficient of variation is 0.1 or greater.
15. The TDD has a width of 1 mm and an outer diameter of 1 square centimeter (cm) at any annular ring portion corresponding to a radial position of the wafer within a range of 3 mm to 50 mm from the center of the SiC wafer. 2 13. The SiC wafer of claim 12, wherein the number of nanoparticles per nanoparticle is 3,000 or less.
16. The TDD has a width of 1 mm and an outer diameter of 1 square centimeter (cm) at any annular ring portion corresponding to the wafer radial positions for at least 50% of all wafer radial positions of the SiC wafer. 2 13. The SiC wafer of claim 12, wherein the number of nanoparticles per nanoparticle is 2000 or less.
17. 13. The SiC wafer of claim 12 comprising a 4H—SiC wafer.
18. 13. The SiC wafer of claim 12 comprising semi-insulating SiC.
19. 13. The SiC wafer of claim 12 comprising n-type SiC.
20. 13. The SiC wafer of claim 12, wherein the diameter is in the range of 145 mm to 155 mm inclusive.
21. 13. The SiC wafer of claim 12, wherein the diameter is in the range of 145 mm to 205 mm inclusive.
22. a silicon carbide (SiC) boule having a diameter in the range of 145 millimeters (mm) to 180 mm, inclusive, and a boule height greater than 50 mm; At least 75% of the boule height of the SiC boule is configured to provide a plurality of first SiC wafers, each first SiC wafer of the plurality of first SiC wafers having a wafer area of 1 square centimeter (cm) for a perimeter including a center of the first SiC wafer defined by a diameter of the first SiC wafer and having a radius of 2 mm from a wafer radial position of the first SiC wafer. 2 ) having a total dislocation density (TDD) of 4600 or less per Silicon carbide (SiC) boule, wherein the TDD is the total number of micropipes, threading edge dislocations, threading screw dislocations, and basal plane dislocations.
23. The TDD is 1 cm 2 23. The SiC boule of claim 22, wherein the number of pores is 1000 or more per pore.
24. At least 40% of the boule height of the SiC boule is configured to provide a plurality of second SiC wafers, each second SiC wafer of the plurality of second SiC wafers having a wafer area of 1 square centimeter (cm) for a perimeter including a center of the second SiC wafer defined by a diameter of the second SiC wafer and having a radius of 2 mm from a peripheral edge of the second SiC wafer. 2 23. The SiC boule of claim 22 having a total dislocation density (TDD) of 3000 or less per square inch.
25. The TDD is 1 cm 2 24. The SiC boule of claim 23, wherein the number of pores is 1000 or more per pore.
26. 23. The SiC boule of claim 22, wherein the boule height is in the range of 60 mm to 300 mm inclusive.
27. 23. The SiC boule of claim 22, wherein the boule height is within the range of 55 mm to 80 mm inclusive.
28. 23. The SiC boule of claim 22, wherein the boule height is in the range of 60 mm to 70 mm inclusive.
29. 23. The SiC boule of claim 22, wherein the boule height is 65 mm or less.
30. 23. The SiC boule of claim 22, wherein the boule height is greater than or equal to 55 mm and less than or equal to 65 mm.
31. a silicon carbide (SiC) boule having a diameter in the range of 145 millimeters (mm) to 180 mm, inclusive, and a boule height of 40 mm or greater; At least 50% of the boule height of the SiC boule is configured to produce a plurality of first SiC wafers, each first SiC wafer of the plurality of first SiC wafers having a wafer area of 1 square centimeter (cm) for a perimeter including a center of the first SiC wafer defined by a diameter of the first SiC wafer and having a radius of 2 mm from a wafer radial position of the first SiC wafer. 2 ) having a total dislocation density (TDD) of 4600 or less per The TDD is the total number of micropipes, threading edge dislocations, threading screw dislocations, and basal plane dislocations; Silicon carbide (SiC) boule.
32. 32. The SiC boule of claim 31 , wherein the boule height is in the range of 40 mm to 300 mm inclusive.
33. 32. The SiC boule of claim 31 , wherein the boule height is in the range of 40 mm to 80 mm inclusive.
34. The TDD is 1 cm 2 32. The SiC boule of claim 31 , wherein the number of pores per pore is 1000 or more.
35. At least 80% of the boule height of the SiC boule is greater than 1 cm 2 32. The SiC boule of claim 31 , configured to produce a plurality of SiC wafers having an average TDD of 4600 or less per SiC boule.
36. At least 40% of the boule height of the SiC boule is configured to produce a plurality of second SiC wafers, each second SiC wafer of the plurality of second SiC wafers having a wafer area bounded by a perimeter having a radius of 1 cm for a wafer area that includes the center of the second SiC wafer defined by a diameter of the second SiC wafer and has a wafer radial position of 2 mm from the periphery of the second SiC wafer. 2 32. The SiC boule of claim 31 having an average TDD per boule of 3000 or less.
37. The TDD is 1 cm 2 37. The SiC boule of claim 36, wherein the number of pores is 1000 or more per pore.
38. A silicon carbide (SiC) wafer having a diameter of 145 mm or greater, the diameter of the SiC wafer being defined by a center of the SiC wafer and a perimeter having a radius of 2 millimeters (mm) from a peripheral edge of the SiC wafer, the perimeter being defined by a radius of 1 square centimeter (cm) for a wafer area that is bounded by a perimeter having a radius of 2 millimeters (mm) from a peripheral edge of the SiC wafer. 2 ) having a total dislocation density (TDD) of 3500 or less per The TDD is the total number of micropipes, threading edge dislocations, threading screw dislocations, and basal plane dislocations; Silicon carbide (SiC) wafers.
39. The TDD is 1 cm 2 39. The SiC wafer of claim 38, wherein the number of nuclei per unit area is 500 or more.
40. The TDD is 1 cm 2 39. The SiC wafer of claim 38, having 2500 or less per unit area.
41. The TDD is 1 cm 2 39. The SiC wafer of claim 38, having 1500 or less per square inch.
42. A SiC wafer as described in claim 38, further having a diameter of 180 mm or less.
Citation Information
Patent Citations
Large diameter silicon carbide single crystal, and device and method of manufacturing those
JP2018039715A
Sic single crystal ingot
WO2017057742A1
Cited By
Off axis laser-based surface processing operations for semiconductor wafers
US12438001B1
Off Axis Laser-Based Surface Processing Operations for Semiconductor Wafers
US20250316480A1