Polyester resin for toner and toner
The use of an α-terpinyl structure in polyester resin for toners improves both heat-and-moisture storage stability and low-temperature fixability by maintaining high glass transition points while reducing hygroscopicity, thus addressing the stability and fixing challenges in existing toners.
Patent Information
- Application Number
- JP2023076610
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-01
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2043-05-08
AI Technical Summary
Toner binders with low molecular weight for low-temperature fixing have reduced glass transition points, leading to poor heat-resistant storage stability and increased hygroscopicity, which affects humidity-resistant storage stability.
Incorporating an α-terpinyl structure into the polyester resin for toner using carboxylic acids and alcohols as raw material monomers, which results in a resin with high glass transition points and low melt viscosity, reducing hygroscopicity and enhancing moisture resistance.
The α-terpinyl structure in the polyester resin provides toners with excellent heat-and-moisture storage stability and low-temperature fixability, addressing the issues of reduced stability and high hygroscopicity in existing toners.
Smart Images

Figure 0007587633000001 
Figure 0007587633000002 
Figure 0007587633000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester resin for a toner and a toner. [Background technology]
[0002] In recent years, with the trend toward higher speeds and energy saving in printers and copiers, there has been an increasing need for toners with excellent low-temperature fixability. However, when the molecular weight of the binder resin in a toner is reduced in order to melt it at a low temperature, the glass transition point of the resin is lowered, and the heat-resistant storage stability is reduced. To solve this problem, polyesters obtained using carboxylic acids having aromatic rings, such as terephthalic acid or isophthalic acid, or alcohols having a bisphenol A structure as raw material monomers are widely used as binder resins for toners that have a high glass transition point even though they have a low molecular weight (Patent Document 1). On the other hand, since aromatic rings have higher polarity than aliphatic structures, the moisture absorption of the binder resin increases, resulting in a problem of deterioration in the humidity and heat resistance storage stability of the toner. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-251248 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a toner having excellent humidity and heat resistance storage stability and low-temperature fixability by using the polyester resin for toner of the present invention. [Means for solving the problem]
[0005] As a result of extensive research aimed at solving these problems, the present invention was achieved. That is, the present invention relates to a polyester resin for a toner, characterized by having an α-terpinyl structure. Effect of the Invention
[0006] By using the polyester resin for toner of the present invention, it is possible to provide a toner having excellent humidity and heat resistance storage stability and low-temperature fixability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The polyester resin for toner of the present invention is a polyester resin characterized by having an α-terpinyl structure. By having the α-terpinyl structure in the polyester resin, a toner having excellent moist heat resistant storage stability and low temperature fixing property can be obtained. The reason for this is believed to be that by using a compound having an α-terpinyl structure as a raw material monomer for the polyester resin, a resin having a low melt viscosity can be obtained even if the glass transition point is high, and the toner has excellent heat resistant storage stability and low temperature fixing property, and due to the hydrophobicity of the α-terpinyl structure, the resin has low moisture absorption property, resulting in excellent moist resistant storage stability.
[0008] In the present invention, the polyester resin for toner is preferably a resin obtained by using, as raw material monomers, a carboxylic acid component containing at least a carboxylic acid compound having an α-terpinyl structure and / or an alcohol component containing an alcohol having an α-terpinyl structure, and polycondensing the carboxylic acid component and the alcohol component. The α-terpinyl structure is a structure represented by general formula (1).
[0009] [ka] In general formula (1), R represents a residue of a carboxylic acid compound having an α-terpinyl structure or an alcohol having an α-terpinyl structure.
[0010] A carboxylic acid compound and an alcohol having an α-terpinyl structure can be obtained, for example, by reacting α-pinene and / or β-pinene with a compound having a hydroxyl group, followed by post-treatment such as hydrolysis or isolation and purification as necessary.
[0011] The compound having a hydroxyl group is not particularly limited as long as it produces a compound having a hydroxyl group and / or a carboxyl group after reaction with α-pinene and / or β-pinene. From the viewpoint of ease of use as a monomer for a polyester resin, however, it is preferably a hydroxycarboxylic acid compound and / or a polyhydric alcohol compound having three or more functional groups. Examples of the hydroxycarboxylic acid compound include aliphatic hydroxycarboxylic acids and aromatic hydroxycarboxylic acids, such as salicylic acid, malic acid, citramalic acid, tartaric acid, xylonic acid, glucaric acid, and gluconic acid. Among these, from the viewpoint of ease of use as a monomer, aliphatic hydroxycarboxylic acids are preferred, dicarboxylic acid compounds such as malic acid, citramalic acid, tartaric acid, and glucaric acid are more preferred, and malic acid is even more preferred. Examples of polyhydric alcohol compounds with three or more functionalities include polyhydric aliphatic alcohols having three to 36 carbon atoms and having three or more valences, AO adducts of polyhydric aliphatic alcohols (number of moles added: 2 to 120), AO adducts of trisphenols (such as trisphenol PA) (number of moles added: 2 to 30), AO adducts of novolak resins (such as phenol novolak and cresol novolak) (number of moles added: 2 to 30), and acrylic polyols [such as copolymers of hydroxyethyl (meth)acrylate and other vinyl monomers]. Examples of the trihydric or higher polyhydric aliphatic alcohol having 3 to 36 carbon atoms include alkane polyols and their intramolecular or intermolecular dehydration products, as well as sugars (such as sucrose) and their methyl glucosides. Specific examples of alkane polyols and their intramolecular or intermolecular dehydration products include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, and polyglycerin. Of the above tri- or higher functional polyhydric alcohol compounds, from the viewpoint of acetalization described later, tri- or higher functional polyhydric aliphatic alcohols having 3 to 36 carbon atoms are preferred, alkane polyols and their intramolecular or intermolecular dehydration products are more preferred, glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol are further preferred, and glycerin is particularly preferred. When reacting the above-mentioned trifunctional or higher polyhydric alcohol compounds with α-pinene and / or β-pinene, a part of the alcohol may be acetalized in advance with an aldehyde compound or a ketone compound. In this case, an alcohol having an α-terpinyl structure can be obtained by hydrolyzing the acetal moiety after the reaction with α-pinene and / or β-pinene. An example of an acetalized trifunctional or higher polyhydric alcohol compound is 2,2-dimethyl-1,3-dioxolane-4-methanol, which is obtained by acetalizing glycerin with acetone.
[0012] Examples of the carboxylic acid compound having an α-terpinyl structure include aliphatic carboxylic acids having an α-terpinyl structure (2-α-terpinoxy-succinic acid, 2-α-terpinoxy-adipic acid, 2-α-terpinoxy-sebacic acid, 2-α-terpinoxy-azelaic acid) and aromatic carboxylic acids having an α-terpinyl structure (α-terpinoxy-phthalic acid), and one of them may be used alone or two or more of them may be used in combination. In addition, the carboxylic acid compound having an α-terpinyl structure may be a carboxylic anhydride or a lower alkyl (carbon number 1 to 4) ester (methyl ester, ethyl ester, isopropyl ester, etc.). Among the carboxylic acid compounds having an α-terpinyl structure, from the viewpoint of controlling the glass transition temperature of the resulting polyester, aliphatic carboxylic acids having an α-terpinyl structure are preferred, and 2-α-terpinoxy-succinic acid is more preferred.
[0013] Examples of the alcohol having an α-terpinyl structure include 3-α-terpinoxy-1,2-propanediol, 4-α-terpinoxy-3,3-dihydroxymethyl-butane, and the like. One type may be used alone, or two or more types may be used in combination. Among the alcohols having an α-terpinyl structure, 3-α-terpinoxy-1,2-propanediol is preferred from the viewpoint of controlling the glass transition temperature of the resulting polyester.
[0014] From the viewpoint of the moist heat resistance storage stability and low temperature fixing property of the toner, the total amount of the carboxylic acid compound having an α-terpinyl structure and the alcohol having an α-terpinyl structure is preferably 10 to 100 mol %, more preferably 20 to 98 mol %, of the total amount of the carboxylic acid component and the alcohol component.
[0015] Furthermore, the content of the carboxylic acid compound having an α-terpinyl structure is preferably 10 to 100 mol %, more preferably 20 to 98 mol %, of the carboxylic acid component, from the viewpoints of low-temperature fixability and moist heat resistance storage stability of the toner.
[0016] The content of the alcohol having an α-terpinyl structure in the alcohol component is preferably 10 to 100 mol %, more preferably 20 to 98 mol %, from the viewpoints of low-temperature fixability and moist heat resistance storage stability of the toner.
[0017] The polyester resin for toner of the present invention may contain at least a carboxylic acid compound having an α-terpinyl structure and / or an alcohol having an α-terpinyl structure as a raw material monomer, and may also contain a conventionally known alcohol component and / or carboxylic acid component in combination. The alcohol component includes a diol (g) and a trihydric or higher polyol (h).
[0018] Examples of the diol (g) include alkylene glycols having 2 to 36 carbon atoms, alkylene ether glycols having 4 to 36 carbon atoms, alicyclic diols having 4 to 36 carbon atoms, alkylene oxide adducts of alkylene glycols or alicyclic diols, alkylene oxide adducts of bisphenols, polylactone diols, and polybutadiene diols. Specific examples of alkylene glycols having 2 to 36 carbon atoms include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, octanediol, decanediol, dodecanediol, tetradecanediol, neopentyl glycol, and 2,2-diethyl-1,3-propanediol. Specific examples of alkylene ether glycols having 4 to 36 carbon atoms include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol. Specific examples of the alicyclic diol having 4 to 36 carbon atoms include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. In the alkylene oxide adduct of an alkylene glycol or an alicyclic diol, examples of the alkylene glycol or alicyclic diol include those mentioned above, and examples of the alkylene oxide (hereinafter abbreviated as AO) adduct include an ethylene oxide (hereinafter abbreviated as EO) adduct, a propylene oxide (hereinafter abbreviated as PO) adduct, and a butylene oxide (hereinafter abbreviated as BO) adduct, etc. Examples of AO adducts of bisphenol include AO (EO, PO, BO, etc.) adducts of bisphenol A, bisphenol F, bisphenol S, etc. (molar number of addition: 2 to 30). An example of the polylactone diol is poly-ε-caprolactone diol.
[0019] As the diol (g), in addition to the above diols having no functional groups other than hydroxyl groups, diols (g1) having other functional groups may be used. Examples of (g1) include diols having a carboxyl group, diols having a sulfonic acid group or a sulfamic acid group, and salts thereof. The diol having a carboxyl group may be a dialkylolalkanoic acid having 6 to 24 carbon atoms, specifically 2,2-dimethylolpropionic acid (DMPA), 2,2-dimethylolbutanoic acid, 2,2-dimethylolheptanoic acid, 2,2-dimethyloloctanoic acid, etc. Examples of diols having a sulfonic acid group or a sulfamic acid group include 3-(2,3-dihydroxypropoxy)-1-propanesulfonic acid, sulfoisophthalic acid di(ethylene glycol) ester, sulfamic acid diol, and bis(2-hydroxyethyl)phosphate.
[0020] Preferred diols (g) are alkylene glycols having 2 to 12 carbon atoms, diols having a carboxyl group, AO adducts of bisphenols, and combinations of these.
[0021] Examples of the trihydric or higher polyol (h) include trihydric or higher polyhydric aliphatic alcohols having 3 to 36 carbon atoms, AO adducts of polyhydric aliphatic alcohols (number of moles added: 2 to 120), AO adducts of trisphenols (trisphenol PA, etc.) (number of moles added: 2 to 30), AO adducts of novolak resins (phenol novolak, cresol novolak, etc.) (number of moles added: 2 to 30), and acrylic polyols [copolymers of hydroxyethyl (meth)acrylate and other vinyl monomers, etc.]. Examples of the trihydric or higher polyhydric aliphatic alcohol having 3 to 36 carbon atoms include alkane polyols and their intramolecular or intermolecular dehydration products, as well as sugars (such as sucrose) and their methyl glucosides. Specific examples of alkane polyols and their intramolecular or intermolecular dehydration products include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, and polyglycerin.
[0022] The trihydric or higher polyol (h) is preferably a trihydric or higher polyhydric aliphatic alcohol and an AO adduct of a novolak resin, and more preferably an AO adduct of a novolak resin.
[0023] Examples of the carboxylic acid component include dicarboxylic acids (i), trivalent or higher polycarboxylic acids (j), and acid anhydrides or lower alkyl esters thereof.
[0024] Examples of the dicarboxylic acid (i) include alkane dicarboxylic acids having 4 to 36 carbon atoms, alkenyl succinic acids, alicyclic dicarboxylic acids having 6 to 40 carbon atoms, alkene dicarboxylic acids having 4 to 36 carbon atoms, and aromatic dicarboxylic acids having 8 to 36 carbon atoms. Examples of the alkanedicarboxylic acid having 4 to 36 carbon atoms include succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedicarboxylic acid, octadecanedicarboxylic acid, and decylsuccinic acid. Examples of the alkenylsuccinic acid include dodecenylsuccinic acid, pentadecenylsuccinic acid, and octadecenylsuccinic acid. Examples of the alicyclic dicarboxylic acid having 6 to 40 carbon atoms include dimer acid (dimerized linoleic acid). Examples of the alkene dicarboxylic acid having 4 to 36 carbon atoms include maleic acid, fumaric acid, and citraconic acid. Examples of the aromatic dicarboxylic acid having 8 to 36 carbon atoms include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. Among these dicarboxylic acids (i), preferred are alkanedicarboxylic acids having 4 to 36 carbon atoms and aromatic dicarboxylic acids having 8 to 36 carbon atoms, and more preferred are alkanedicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms.
[0025] Examples of the trivalent or higher polycarboxylic acid (j) include aromatic polycarboxylic acids having 9 to 20 carbon atoms (such as trimellitic acid and pyromellitic acid) and aliphatic (including alicyclic) tricarboxylic acids having 6 to 36 carbon atoms (such as hexanetricarboxylic acid and decanetricarboxylic acid).
[0026] Among these trivalent or higher polycarboxylic acids (j), preferred are aromatic polycarboxylic acids having 9 to 20 carbon atoms, and more preferred are trimellitic acid and pyromellitic acid.
[0027] As the dicarboxylic acid (i) or the tri- or higher carboxylic acid (j), acid anhydrides or lower alkyl esters having 1 to 4 carbon atoms (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compounds may be used.
[0028] The reaction ratio of the alcohol component and the carboxylic acid component, expressed as the molar ratio [OH] / [COOH] of the hydroxyl group [OH] to the carboxyl group [COOH], is preferably 1 / 5 to 2 / 1, more preferably 1 / 4 to 1.5 / 1, and particularly preferably 1 / 3 to 1 / 1.3. In order to adjust the acid value of the polyester resin to fall within the preferred range described below, a polyester having an excess of hydroxyl groups may be treated with a polycarboxylic acid.
[0029] The polyester resin can be produced by a known production method. For example, a method can be mentioned in which a carboxylic acid component containing at least a carboxylic acid compound having an α-terpinyl structure and / or an alcohol component containing an alcohol having an α-terpinyl structure is used as raw material monomers, and the carboxylic acid component and the alcohol component are subjected to a polycondensation reaction in an inert gas (nitrogen gas, etc.) atmosphere at a reaction temperature of preferably 150 to 280°C for a reaction time of preferably 30 minutes or more.
[0030] In addition, when terephthalic acid is used as the carboxylic acid component in this reaction, a terephthalic acid component derived from PET (polyethylene terephthalate) may be used in place of terephthalic acid or may be mixed together with terephthalic acid. Similarly, when ethylene glycol is used as the alcohol component, an ethylene glycol component derived from PET (polyethylene terephthalate) may be used in place of ethylene glycol or may be mixed together with ethylene glycol.
[0031] In this case, an esterification catalyst can be used as necessary. Esterification catalysts include tin-containing catalysts, antimony trioxide, titanium-containing catalysts, zirconium-containing catalysts, zinc acetate, and the like. Specifically, the tin-containing catalyst may be dibutyltin oxide. Examples of the titanium-containing catalyst include titanium alkoxide, potassium oxalate titanate, titanium terephthalate, the catalysts described in JP-A-2006-243715 (titanium dihydroxybis(triethanolaminate), titanium monohydroxytris(triethanolaminate), and intramolecular polycondensates thereof, etc.), and the catalysts described in JP-A-2007-11307 (titanium tributoxyterephthalate, titanium triisopropoxyterephthalate, titanium diisopropoxyditerephthalate, etc.). Zirconium-containing catalysts include zirconyl acetate.
[0032] Of the esterification catalysts, titanium-containing catalysts are preferred from the viewpoint of the electrostatic properties of the polyester resin, and the catalysts described in JP-A-2006-243715 and JP-A-2007-11307 are more preferred.
[0033] The polyester resin for toner of the present invention preferably contains a structural unit of a metal carboxylate from the viewpoint of charging characteristics. When the polyester resin contains a structural unit of a metal carboxylate, the resin can be obtained, for example, by synthesizing a polyester having a COOH group (with an acid value of preferably 1 to 100 mgKOH / g, more preferably 5 to 50 mgKOH / g), and converting at least a part of the COOH group into a salt of at least one metal selected from Al, Ti, Cr, Mn, Fe, Zn, Ba, and Zr. The metal salt can be obtained, for example, by reacting a polyester having a COOH group with a hydroxide of the corresponding metal.
[0034] In the present invention, the number average molecular weight (Mn) and the weight average molecular weight (Mw) can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment: "HLC-8120" [Tosoh Corporation] Column: "TSK GEL GMH6" [Tosoh Corporation] x 2 Measurement temperature: 40℃ Sample solution: 0.25% by weight tetrahydrofuran solution (insolubles were filtered off using a glass filter) Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]
[0035] The number average molecular weight (Mn) of the polyester resin is preferably from 1,000 to 10,000, and more preferably from 1,500 to 8,000, from the viewpoints of low-temperature fixability and moist heat storage stability.
[0036] The weight average molecular weight (Mw) of the polyester resin is preferably from 2,000 to 50,000, and more preferably from 3,000 to 30,000, from the viewpoints of low-temperature fixability and moist heat storage stability.
[0037] The acid value of the polyester resin is preferably 0 to 40 mgKOH / g from the viewpoint of humidity and heat resistance storage stability. The acid value can be measured by the method specified in JIS K0070.
[0038] The hydroxyl value of the polyester resin is preferably 20 to 80 mgKOH / g from the viewpoint of humidity and heat resistance storage stability. The hydroxyl value can be measured by the method specified in JIS K0070.
[0039] The glass transition temperature (Tg) of the polyester resin is preferably 40 to 120°C, and more preferably 50 to 80°C. In the present invention, Tg can be measured by the method (DSC) specified in ASTM D3418-82 using "DSC20, SSC / 580" [manufactured by Seiko Instruments Inc.].
[0040] The toner of the present invention is a toner containing the above-mentioned polyester resin for toner. By using a binder resin containing the polyester resin for toner of the present invention, a toner having excellent low-temperature fixing property and humidity and heat storage resistance can be obtained.
[0041] The toner of the present invention may contain other resins in addition to the polyester resins described above. Any known resins may be used as the other resins, and specific examples of such resins include polyester resins other than the polyester resins described above, vinyl resins, polyurethane resins, epoxy resins, polyamide resins, polyimide resins, silicon resins, phenol resins, melamine resins, urea resins, aniline resins, ionomer resins, and polycarbonate resins. Preferable examples of the other resins include polyester resins other than the above polyester resins, vinyl resins, polyurethane resins, epoxy resins, and combinations of these resins, and more preferably combinations of polyester resins other than the above polyester resins and vinyl resins.
[0042] When the other resin is a polyester resin other than the polyester resin of the present invention, the polyester resin may be a crystalline polyester resin or an amorphous polyester resin, and as raw materials, the same conventionally known alcohol components and / or carboxylic acid components as exemplified for the polyester resin of the present invention can be used, and preferred alcohol components and carboxylic acid components are the same as those for the polyester resin of the present invention described above, and the polyester resin can be produced in the same manner except that alcohols and carboxylic acid compounds having an α-terpinyl structure are not used. In the present invention, "crystalline" refers to a state in which a differential scanning calorimetry (DSC) curve has a maximum and an endothermic peak during the temperature rise process of the differential scanning calorimetry curve obtained by DSC measurement, whereas "amorphous" refers to a state in which the DSC curve does not have an endothermic peak.
[0043] When the other resin is a vinyl resin, the vinyl resin is a polymer obtained by homopolymerizing or copolymerizing a vinyl monomer. Examples of the vinyl monomer include the following (1) to (10). (1) Vinyl hydrocarbons Examples of the vinyl hydrocarbon include (1-1) aliphatic vinyl hydrocarbons, (1-2) alicyclic vinyl hydrocarbons, and (1-3) aromatic vinyl hydrocarbons. (1-1) Aliphatic vinyl hydrocarbons Aliphatic vinyl hydrocarbons include alkenes and alkadienes. Specific examples of alkenes include ethylene, propylene, and α-olefins. Specific examples of alkadienes include butadiene, isoprene, 1,4-pentadiene, 1,6-heptadiene, and 1,7-octadiene. (1-2) Alicyclic vinyl hydrocarbons Examples of the alicyclic vinyl hydrocarbon include mono- or di-cycloalkenes and alkadienes, and specific examples thereof include (di)cyclopentadiene and terpene. (1-3) Aromatic vinyl hydrocarbons Examples of aromatic vinyl hydrocarbons include styrene and its hydrocarbyl (alkyl, cycloalkyl, aralkyl and / or alkenyl) substituted derivatives, and specific examples thereof include α-methylstyrene, 2,4-dimethylstyrene and vinylnaphthalene.
[0044] (2) Carboxyl-containing vinyl monomers and their salts Examples of the carboxyl group-containing vinyl monomer and its salt include unsaturated monocarboxylic acids (salts) having 3 to 30 carbon atoms, unsaturated dicarboxylic acids (salts), and their anhydrides (salts), and their monoalkyl (carbon number 1 to 24) esters or salts. Specific examples thereof include carboxyl group-containing vinyl monomers such as (meth)acrylic acid, (anhydride) maleic acid, maleic acid monoalkyl esters, fumaric acid, fumaric acid monoalkyl esters, crotonic acid, itaconic acid, itaconic acid monoalkyl esters, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl esters, and cinnamic acid, and metal salts thereof.
[0045] In the present invention, "(salt)" means a salt of a compound. For example, an unsaturated monocarboxylic acid (salt) means an unsaturated monocarboxylic acid or a salt thereof.
[0046] In the present invention, "(meth)acrylic" means methacryl or acrylic. In the present invention, "(meth)acryloyl" means methacryloyl or acryloyl. In the present invention, "(meth)acrylate" means methacrylate or acrylate.
[0047] (3) Sulfonic acid-containing vinyl monomers, vinyl sulfate monoesters, and their salts Examples of sulfone group-containing vinyl monomers, vinyl sulfate monoesters, and salts thereof include alkene sulfonic acids (salts) having 2 to 14 carbon atoms, alkyl sulfonic acids (salts) having 2 to 24 carbon atoms, sulfo(hydroxy)alkyl-(meth)acrylates (salts), sulfo(hydroxy)alkyl-(meth)acrylamides (salts), and alkylarylsulfosuccinic acids (salts). Specifically, an example of an alkene sulfonic acid having 2 to 14 carbon atoms is vinyl sulfonic acid (salt), etc., an example of an alkyl sulfonic acid (salt) having 2 to 24 carbon atoms is α-methylstyrene sulfonic acid (salt), etc., and an example of a sulfo(hydroxy)alkyl-(meth)acrylate (salt) or (meth)acrylamide (salt) is sulfopropyl(meth)acrylate (salt), sulfuric acid ester (salt), or a sulfonic acid group-containing vinyl monomer (salt), etc.
[0048] (4) Phosphate-containing vinyl monomers and their salts: Examples of the phosphoric acid group-containing vinyl monomer and its salt include (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphoric acid monoester (salt) and (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphonic acid (salt). Specific examples of the (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphate monoester (salt) include 2-hydroxyethyl (meth)acryloyl phosphate (salt) and phenyl-2-acryloyloxyethyl phosphate (salt). Specific examples of (meth)acryloyloxyalkyl (carbon number: 1 to 24)phosphonic acids (salts) include 2-acryloyloxyethylphosphonic acid (salts).
[0049] Examples of the salts of (2) to (4) above include alkali metal salts (sodium salts, potassium salts, etc.), alkaline earth metal salts (calcium salts, magnesium salts, etc.), ammonium salts, amine salts, and quaternary ammonium salts.
[0050] (5) Hydroxyl-containing vinyl monomers Examples of hydroxyl group-containing vinyl monomers include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)allyl alcohol, crotyl alcohol, isocrotyl alcohol, 1-buten-3-ol, 2-buten-1-ol, 2-butene-1,4-diol, propargyl alcohol, 2-hydroxyethyl propenyl ether, and sucrose allyl ether.
[0051] (6) Nitrogen-containing vinyl monomers Examples of the nitrogen-containing vinyl monomer include (6-1) an amino group-containing vinyl monomer, (6-2) an amide group-containing vinyl monomer, (6-3) a nitrile group-containing vinyl monomer, (6-4) a quaternary ammonium cation group-containing vinyl monomer, and (6-5) a nitro group-containing vinyl monomer. (6-1) Examples of amino group-containing vinyl monomers include aminoethyl (meth)acrylate. (6-2) Examples of the amide group-containing vinyl monomer include (meth)acrylamide and N-methyl(meth)acrylamide. (6-3) Examples of nitrile group-containing vinyl monomers include (meth)acrylonitrile, cyanostyrene, and cyanoacrylate. (6-4) Examples of the vinyl monomer containing a quaternary ammonium cation group include quaternized products of tertiary amine group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and diallylamine (which are quaternized with a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate). (6-5) Nitro group-containing vinyl monomers include nitrostyrene and the like.
[0052] (7) Epoxy group-containing vinyl monomer Examples of the epoxy group-containing vinyl monomer include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and p-vinylphenylpropylene oxide.
[0053] (8) Halogen-containing vinyl monomers Examples of halogen-containing vinyl monomers include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluoroethylene, fluoroacrylate, tetrafluorostyrene, and chloroprene.
[0054] (9) (Meth)acrylic acid alkyl esters, vinyl esters, vinyl (thio)ethers, vinyl ketones (9-1) Examples of alkyl esters of (meth)acrylic acid include (meth)acrylic acid esters having an alkyl group having 1 to 50 carbon atoms [methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, and behenyl (meth)acrylate, etc.]. (9-2) Examples of vinyl esters include vinyl acetate, vinyl butyrate, vinyl propionate, and vinyl butyrate. (9-2) Examples of vinyl (thio)ethers include vinyl methyl ether, vinyl ethyl ether, vinyl propyl ether, vinyl butyl ether, vinyl-2-ethylhexyl ether, vinyl phenyl ether, vinyl-2-methoxyethyl ether, methoxybutadiene, vinyl-2-butoxyethyl ether, 3,4-dihydro-1,2-pyran, 2-butoxy-2'-vinyloxydiethyl ether, vinyl-2-ethylmercaptoethyl ether, acetoxystyrene, and phenoxystyrene. (9-3) Examples of vinyl ketones include vinyl methyl ketone, vinyl ethyl ketone, and vinyl phenyl ketone.
[0055] (10) Other vinyl monomers Other vinyl monomers include tetrafluoroethylene, fluoroacrylate, isocyanatoethyl (meth)acrylate, and m-isopropenyl-α,α-dimethylbenzyl isocyanate.
[0056] In synthesizing the vinyl resin, the above vinyl monomers (1) to (10) may be used alone or in combination of two or more. As the vinyl resin, from the viewpoints of particle size distribution and electrostatic chargeability, styrene-(meth)acrylic acid ester copolymers and (meth)acrylic acid ester copolymers are preferred, and styrene-(meth)acrylic acid ester copolymers are more preferred.
[0057] The toner of the present invention may contain various known additives such as a colorant, a releasing agent, a charge control agent, a fluidizing agent, etc., if necessary.
[0058] The colorant preferably contains at least one selected from the group consisting of black colorants, blue colorants, red colorants and yellow colorants. As the colorant, any dye, pigment, etc. used as a toner colorant can be used. Specific examples of the pigment include carbon black, iron black, Sudan Black SM, Fast Yellow G, Benzidine Yellow, Solvent Yellow (21, 77, 114, etc.), Pigment Yellow (12, 14, 17, 83, etc.), India Fast Orange, Irgasin Red, Paranitoaniline Red, Toluidine Red, Solvent Red (17, 49, 128, 5, 13, 22, 48·2, etc.), Disperse Red, Carmine FB, Pigment Orange R, Lake Red 2G, Rhodamine FB, Rhodamine B Lake, Methyl Violet B Lake, Phthalocyanine Blue, Solvent Blue (25, 94, 60, 15·3, etc.), Pigment Blue, Brilliant Green, Phthalocyanine Green, Oil Yellow GG, Kayaset YG, Orasol Brown B, and Oil Pink OP. If necessary, magnetic powder (powders of ferromagnetic metals such as iron, cobalt and nickel, and compounds such as magnetite, hematite and ferrite) may be contained to function as a colorant. The content of the colorant is preferably 1 to 40 parts by weight, more preferably 2 to 15 parts by weight, based on 100 parts by weight of the total of the polyester resin of the present invention and other resins. When magnetic powder is used, the content of the magnetic powder is preferably 20 to 150 parts by weight, more preferably 30 to 120 parts by weight, based on 100 parts by weight of the total of the polyester resin of the present invention and other resins.
[0059] Examples of the release agent include natural waxes (beeswax, carnauba wax, montan wax, etc.), petroleum waxes (paraffin wax, microcrystalline wax, petrolatum, etc.), synthetic waxes (Fischer-Tropsch wax, polyethylene wax, polypropylene wax, oxidized polyethylene wax, oxidized polypropylene wax, etc.), and synthetic ester waxes (fatty acid esters synthesized from fatty acids having 10 to 30 carbon atoms and alcohols having 10 to 30 carbon atoms, etc.), and it is preferable to contain one or more types selected from the group consisting of these release agents. The content of the release agent is preferably 0 to 30 parts by weight, more preferably 0.5 to 20 parts by weight, and even more preferably 1 to 10 parts by weight, based on 100 parts by weight of the total of the polyester resin of the present invention and other resins.
[0060] When using the above-mentioned release agent, modified wax may be used in combination as necessary. The modified wax is a release agent to which a vinyl polymer chain is grafted. The release agent used in the modified wax may be the same as the above-mentioned release agent, and the preferred ones are also the same. Examples of the vinyl monomer constituting the vinyl polymer chain of the modified wax include styrene and methacrylic acid ester. The vinyl polymer chain may be a homopolymer or copolymer of a vinyl monomer. The content of the modified wax is preferably 0 to 15 parts by weight, more preferably 0.5 to 10 parts by weight, and even more preferably 1 to 5 parts by weight, based on 100 parts by weight of the total of the polyester resin of the present invention and other resins.
[0061] The charge control agent may be either a positively charged charge control agent or a negatively charged charge control agent. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes having a tertiary amine as a side chain, quaternary ammonium salts, polyamine resins, imidazole derivatives, and quaternary ammonium salts. Examples of the charge control agent include um base-containing polymers, metal-containing azo dyes, copper phthalocyanine dyes, metal salts of salicylic acid, boron complexes of benzilic acid, sulfonic acid group-containing polymers, fluorine-containing polymers, halogen-substituted aromatic ring-containing polymers, etc. The content of the charge control agent may be 0 to 20 parts by weight, preferably 0.1 to 10 parts by weight, more preferably 0.5 to 7.5 parts by weight, based on 100 parts by weight of the total of the polyester resin of the present invention and other resins.
[0062] Examples of the fluidizing agent include silica, titania, alumina, fatty acid metal salt, silicone resin particles, and fluororesin particles, and two or more of them may be used in combination. From the viewpoint of the chargeability of the toner, silica is preferred. From the viewpoint of the transferability of the toner, the silica is preferably hydrophobic. The content of the fluidizing agent may be 0 to 10 parts by weight, preferably 0 to 5 parts by weight, and more preferably 0.1 to 4 parts by weight, based on 100 parts by weight of the toner of the present invention in total.
[0063] The total weight of additives such as colorants, release agents, charge control agents, and fluidizing agents may be 3 to 70% by weight, preferably 4 to 58% by weight, and more preferably 5 to 50% by weight, based on the weight of the toner.
[0064] The method for producing the toner is not particularly limited, and the toner may be obtained by a known kneading and grinding method, a suspension polymerization method described in JP-B-10231 / 1961, JP-A-53856 / 1984, and JP-A-61842 / 1984, an emulsion polymerization method represented by a soap-free polymerization method in which a toner is produced by directly polymerizing a monomer in the presence of a water-soluble polymerization initiator that is soluble in the monomer, an interfacial polymerization method such as a microcapsule production method, an in-site polymerization method, a coacervation method in which at least one type of fine particles are aggregated to obtain a toner of a desired particle size as disclosed in JP-A-106473 / 1987 and JP-A-186253 / 1988, a dispersion polymerization method characterized by monodispersion, a dissolution suspension method in which a necessary resin is dissolved in a water-insoluble organic solvent and then resin particles are formed in an aqueous medium, or an ester elongation polymerization method, or a method in which the toner is dispersed in carbon dioxide in a supercritical state.
[0065] The aqueous medium in the present invention can be any liquid containing water as an essential component, and examples of the aqueous medium that can be used include water, an aqueous solution of an organic solvent, an aqueous solution of a surfactant (s), an aqueous solution of a water-soluble polymer (t), and mixtures thereof, as described below. As a method for stably forming a dispersion containing the polyester resin of the present invention in an aqueous medium, there may be mentioned a method in which the polyester resin is added to an aqueous medium and dispersed by shear force. When using other resins, the polyester resin or the like and the other resins may be mixed in advance and dispersed in the aqueous medium. When other resins are used as fine particles, the fine particles of the resin are not particularly limited as long as they can form fine particles in an aqueous medium and can be adsorbed to the polyester resin of the present invention.
[0066] The method for producing resin fine particles is not particularly limited, but examples thereof include the following [1] and [2]. [1] In the case of vinyl resins, a method of directly producing a fine particle dispersion of resin by a polymerization reaction using a monomer as a starting material, such as suspension polymerization, emulsion polymerization, seed polymerization, or dispersion polymerization. [2] In the case of polyaddition or condensation resins such as polyester resins, polyurethane resins, and epoxy resins, a method in which a precursor (monomer, oligomer, etc.) or a solvent solution thereof is dispersed in a medium in the presence of an appropriate dispersant, and then heated or a curing agent is added to harden the precursor to produce a fine particle dispersion of the resin.
[0067] In the above method [1] or [2], the emulsifier or dispersant used in combination may be a known surfactant (s) or water-soluble polymer (t) described below. Also, an organic solvent or the like described below may be used in combination as an emulsifying or dispersing aid.
[0068] In the present invention, other raw materials such as colorant, release agent, modified wax, and charge control agent do not necessarily need to be mixed when forming particles in an aqueous medium, but may be added after forming the particles. For example, after forming particles not containing a colorant, a colorant may be added by a known dyeing method.
[0069] The dispersion method is not particularly limited, but known equipment such as low-speed shear type, high-speed shear type, friction type, high-pressure jet type, and ultrasonic type can be applied. A high-speed shear type is preferred in order to make the particle size of the dispersion 2 to 20 μm. When using a high-speed shear type disperser, the rotation speed is not particularly limited, but is generally 1000 to 30000 rpm, preferably 5000 to 20000 rpm. The dispersion time is not particularly limited, but in the case of a batch method, it is generally 0.1 to 5 minutes. Examples of the dispersion device include batch-type emulsifiers such as homogenizers (manufactured by IKA), Polytrons (manufactured by Kinematica), and TK Auto Homo Mixers (manufactured by Tokushu Kika Kogyo Co., Ltd.), Ebara Milders (manufactured by Ebara Corporation), TK Filmix, TK Pipeline Homo Mixers (manufactured by Tokushu Kika Kogyo Co., Ltd.), colloid mills (manufactured by Kobe Steel Pantech Co., Ltd.), Ultra Visco Mills (manufactured by Imex), Slashers, and Trigonal wet fine grinding mills (manufactured by Mitsui Miike Kakoki Co., Ltd.), etc. Examples of such machines include continuous emulsifiers such as the Microfluidizer (manufactured by Mizuho Kogyo Co., Ltd.), Capitron (manufactured by Eurotech Co., Ltd.), Fine Flow Mill (manufactured by Pacific Machinery Co., Ltd.), high-pressure emulsifiers such as the Microfluidizer (manufactured by Mizuho Kogyo Co., Ltd.), Nanomizer (manufactured by Nanomizer Co., Ltd.), APV Gaulin (manufactured by Gaulin Co., Ltd.), membrane emulsifiers such as the Membrane Emulsifier (manufactured by Reika Kogyo Co., Ltd.), vibration emulsifiers such as the Vibro Mixer (manufactured by Reika Kogyo Co., Ltd.), and ultrasonic emulsifiers such as the Ultrasonic Homogenizer (manufactured by Branson Co., Ltd.). Among these, from the viewpoint of particle size uniformity, APV Gaulin, homogenizer, TK Auto Homo Mixer, Ebara Milder, TK Filmix, and TK Pipeline Homo Mixer are preferred.
[0070] When dispersing the polyester resin of the present invention in an aqueous medium, the polyester resin is preferably liquid. When the polyester resin is solid at room temperature, it may be dispersed in a liquid state at a high temperature above the melting point, or an organic solvent solution of the polyester resin may be used. Using an organic solvent is preferable in that the particle size distribution becomes sharper.
[0071] Examples of the organic solvent include aromatic hydrocarbon solvents, aliphatic or alicyclic hydrocarbon solvents, halogenated solvents, ester or ester ether solvents, ether solvents, ketone solvents, alcohol solvents, amide solvents, sulfoxide solvents, heterocyclic compound solvents, and mixed solvents of two or more of these. Specific examples of organic solvents include aromatic hydrocarbon solvents (toluene, xylene, ethylbenzene, tetralin, etc.); aliphatic or alicyclic hydrocarbon solvents (n-hexane, n-heptane, mineral spirits, cyclohexane, etc.); halogenated solvents such as methyl chloride, methyl bromide, methyl iodide, methylene dichloride, carbon tetrachloride, trichloroethylene, and perchloroethylene; ester or ester ether solvents such as ethyl acetate, butyl acetate, methoxybutyl acetate, methyl cellosolve acetate, and ethyl cellosolve acetate; diethyl ether, tetrahydrofuran, dioxane, ethyl cellosolve, butyl ether ... Examples of suitable organic solvents include ether solvents such as Rosolve and propylene glycol monomethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, di-n-butyl ketone and cyclohexanone; alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, t-butanol, 2-ethylhexyl alcohol and benzyl alcohol; amide solvents such as dimethylformamide and dimethylacetamide; sulfoxide solvents such as dimethylsulfoxide, heterocyclic compound solvents such as N-methylpyrrolidone, and mixed solvents of two or more of these. Among the above organic solvents, volatile ones with a boiling point of less than 100°C are preferred. Preferred organic solvents include ethyl acetate, acetone and methyl ethyl ketone.
[0072] When dispersing the polyester resin of the present invention in an aqueous medium, a known surfactant (s) can be used as an emulsifier or dispersant to be used in combination. The use of the surfactant (s) is preferred in that the volume average particle size of the toner is easily reduced.
[0073] The surfactant (s) is not particularly limited, and examples thereof include anionic surfactants (s-1), cationic surfactants (s-2), amphoteric surfactants (s-3), and nonionic surfactants (s-4), etc. The surfactant (s) may be a combination of two or more surfactants.
[0074] Examples of the anionic surfactant (s-1) include carboxylic acids or salts thereof, sulfate salts, salts of carboxymethyl compounds, sulfonates, and phosphate salts. Examples of the cationic surfactant (s-2) include quaternary ammonium salt surfactants and amine salt surfactants. Examples of the amphoteric surfactant (s-3) include carboxylate-type amphoteric surfactants, sulfate-type amphoteric surfactants, sulfonate-type amphoteric surfactants, and phosphate-type amphoteric surfactants. Examples of the nonionic surfactant (s-4) include AO addition type nonionic surfactants and polyhydric alcohol type nonionic surfactants. Specific examples of these surfactants (s) include those described in JP-A-2002-284881.
[0075] The amount of the surfactant (s) used relative to 100 parts by weight of water as the aqueous medium is preferably 0 to 300 parts by weight, more preferably 0.001 to 10 parts by weight, and particularly preferably 0.01 to 5 parts by weight.
[0076] When dispersing the polyester resin of the present invention in an aqueous medium, a known water-soluble polymer (t) can be used as an emulsifier or dispersant to be used in combination. The use of the water-soluble polymer (t) is preferred in that the volume average particle diameter of the toner is small and the particle size distribution (volume average particle diameter / number average particle diameter) is easily narrowed.
[0077] Examples of the water-soluble polymer (t) include cellulose compounds (e.g., methyl cellulose, ethyl cellulose, hydroxyethyl cellulose, ethylhydroxyethyl cellulose, carboxymethyl cellulose, hydroxypropyl cellulose, and saponified products thereof, etc.), gelatin, starch, dextrin, gum arabic, chitin, chitosan, polyvinyl alcohol, polyvinylpyrrolidone, polyethylene glycol, polyethyleneimine, polyacrylamide, acrylic acid (salt)-containing polymers (sodium polyacrylate, potassium polyacrylate, ammonium polyacrylate, partially neutralized polyacrylic acid with sodium hydroxide, and sodium acrylate-acrylic acid ester copolymers, etc.), sodium hydroxide (partially) neutralized styrene-maleic anhydride copolymers, and water-soluble polyurethanes (polyethylene glycol, and reaction products of polycaprolactone diol, etc. with polyisocyanate, etc.).
[0078] The amount of the water-soluble polymer (t) used is preferably 0 to 5 parts by weight based on 100 parts by weight of water as the aqueous medium.
[0079] The polyester resin of the present invention is a raw material for a toner that is fixed to a support (paper, polyester film, etc.) by a copier, printer, etc. to become a recording material. As a method for fixing to a support, a known hot roll fixing method, flash fixing method, etc. can be used.
[0080] The toner of the present invention is used for developing electrostatic images or magnetic latent images in electrophotography, electrostatic recording, electrostatic printing, etc. More specifically, the present invention relates to a toner used for developing electrostatic images or magnetic latent images, which is particularly suitable for full color use. EXAMPLES
[0081] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the following, "parts" refers to parts by weight unless otherwise specified.
[0082] The physical properties of the polyester resin and the toner were measured by the following methods.
[0083] [Measurement method] <Acid value and hydroxyl value> The measurement was performed according to the method specified in JIS K0070, except that the measurement solvent for the acid value was a mixed solvent of acetone, methanol, and toluene (acetone:methanol:toluene=12.5:12.5:75), and the measurement solvent for the hydroxyl value was THF.
[0084] <Number average molecular weight (Mn) and weight average molecular weight (Mw)> The resin was dissolved in tetrahydrofuran (THF), and the resulting solution was used as a sample solution for measurement by gel permeation chromatography (GPC) under the following conditions. Equipment: HLC-8120 (Tosoh Corporation) Column: 2 TSK GEL GMH6 (Tosoh Corporation) Measurement temperature: 40℃ Sample solution: 0.25% by weight THF solution (undissolved matter was removed using a glass filter) Solution injection volume: 100μL Detector: Refractive index detector Reference material: Standard polystyrene (TSKstandard POLYSTYRENE)
[0085] <Solid concentration and volatile content of dispersion liquid> Taking care not to cause precipitation of toner or resin particles, etc., 2.00 g of the sample before drying was weighed out and dried at 120°C for 1 hour. The dried sample was then removed and its weight was measured to two decimal places. The solid content concentration (weight %) was calculated by (weight of sample after drying / weight of sample before drying) x 100, and the volatile content (weight %) was calculated by {(weight of sample before drying-weight of sample after drying) / weight of sample before drying} x 100.
[0086] <Volume-based median diameter of resin particle dispersion> The volume-based median diameter of the resin fine particles was measured using a dynamic light scattering particle size distribution measuring device "SZ-100" (manufactured by Horiba, Ltd.). The resin fine particle dispersion was diluted 100 times with ion-exchanged water, and the temperature was adjusted to 25° C., and then the solution was filled into a disposable cell (transparent on all four sides). Next, the measurement mode was changed to the particle size measurement mode, and the volume-based median diameter was measured.
[0087] <Volume-based median diameter of crystalline polyester dispersion and colorant dispersion> The volume-based median diameters of the crystalline polyester dispersion and the colorant dispersion were measured using a laser diffraction particle size distribution measuring device "LA-920" (manufactured by Horiba, Ltd.). The resin particle dispersion was diluted with ethyl acetate so that the diffracted light intensity was within the measurement range, and the volume-based median diameter was measured at 25°C.
[0088] <Toner volume average particle size (D50) (μm), number average particle size (μm), particle size distribution (volume average particle size / number average particle size)> Measurements were performed using a Coulter counter [product name: Multisizer III (manufactured by Beckman Coulter, Inc.)]. First, 0.1 to 5 mL of a surfactant (alkylbenzene sulfonate) was added as a dispersant to 100 to 150 mL of an electrolyte solution, ISOTON-II (manufactured by Beckman Coulter). 2 to 20 mg of a measurement sample was then added, and the electrolyte solution in which the sample was suspended was dispersed for approximately 1 to 3 minutes using an ultrasonic disperser. The toner volume and number were measured using a 50 μm aperture with the above-mentioned measuring device, and the volume distribution and number distribution were calculated. From the distribution obtained, the volume average particle diameter (D50) (μm), number average particle diameter (μm), and particle size distribution (volume average particle diameter / number average particle diameter) of the toner were obtained.
[0089] <Production Example 1> [Synthesis of 2-α-terpinoxy-succinic acid] In a 2 L reaction vessel equipped with a stirrer, 1000 parts of acetone, 268 parts of malic acid, 10 parts of anhydrous iron (III) chloride, and 408 parts of α-pinene were charged and reacted for 24 hours at 60° C. with stirring. After the reaction, 500 parts of water were added, and the acetone was distilled off with an evaporator. 1000 parts of toluene were added, and the upper layer was recovered by a separation operation, dried with magnesium sulfate, and the filtrate after filtration was dried to obtain 480 parts of 2-α-terpinoxy-succinic acid, a carboxylic acid compound having an α-terpinyl structure.
[0090] <Production Example 2> [Synthesis of 3-α-terpinoxy-1,2-propanediol] In a 1L reaction vessel equipped with a stirrer, 290 parts of acetone, 132 parts of 2,2-dimethyl-1,3-dioxolane-4-methanol, 3 parts of anhydrous iron(III) chloride, and 136 parts of turpentine (a mixture of 80% α-pinene and 20% β-pinene) were charged and reacted for 24 hours at 25° C. with stirring. After the reaction, 300 parts of water were added and reacted for 6 hours at 60° C., and then the acetone was distilled off under reduced pressure while keeping the temperature at 60° C., 1000 parts of toluene were added, and the upper layer was recovered by a separation operation, dried over magnesium sulfate, filtered, and the toluene was distilled off to obtain 205 parts of 3-α-terpinoxy-1,2-propanediol, an alcohol compound having an α-terpinyl structure.
[0091] <Example 1> [Synthesis of amorphous polyester (L-1)] In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 295 parts of propylene glycol, 860 parts of 2-α-terpinoxy-succinic acid obtained in Production Example 1, 71 parts of succinic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the generated water while heating to 200°C under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 38 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out, and an amorphous polyester (L-1) was obtained.
[0092] <Example 2> [Synthesis of amorphous polyester (L-2)] In a reaction tank equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 521 parts of 3-α-terpinoxy-1,2-propanediol obtained in Production Example 2, 367 parts of terephthalic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the generated water while heating to 220°C under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 27 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out, and an amorphous polyester (L-2) was obtained.
[0093] <Example 3> [Synthesis of amorphous polyester (L-3)] In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 399 parts of recovered PET (polyethylene terephthalate), 247 parts of 3-α-terpinoxy-1,2-propanediol, 113 parts of neopentyl glycol and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and depolymerized at 220°C under normal pressure for 3 hours. Thereafter, the mixture was reacted while distilling off ethylene glycol at 220°C under a reduced pressure of 0.5 to 2.5 kPa. When the hydroxyl value became less than 45 mgKOH / g, 22 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out to obtain amorphous polyester (L-3).
[0094] <Example 4> [Synthesis of amorphous polyester (L-4)] In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 495 parts of 3-α-terpinoxy-1,2-propanediol, 563 parts of 2-α-terpinoxy-succinic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the water produced while heating to 220°C under reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 33 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out to obtain amorphous polyester (L-4).
[0095] <Example 5> [Synthesis of amorphous polyester (L-5)] In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 292 parts of propylene glycol, 848 parts of 2-α-terpinoxy-succinic acid obtained in Production Example 1, 98 parts of terephthalic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the generated water while heating to 200°C under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 37 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out to obtain amorphous polyester (L-5).
[0096] <Example 6> [Synthesis of amorphous polyester (L-6)] In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 397 parts of propylene glycol, 288 parts of 2-α-terpinoxy-succinic acid obtained in Production Example 1, 63 parts of succinic acid, 575 parts of terephthalic acid and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were added, and the mixture was reacted while distilling off the generated water while heating up to 200°C under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 37 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out to obtain amorphous polyester (L-6).
[0097] Comparative Example 1 [Synthesis of Comparative Amorphous Polyester (LR-1)] In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 381 parts of propylene glycol, 534 parts of terephthalic acid, 61 parts of succinic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the generated water while heating to 230°C under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mgKOH / g, 25 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mgKOH / g, the mixture was taken out, and an amorphous polyester (LR-1) was obtained.
[0098] Comparative Example 2 [Synthesis of Comparative Amorphous Polyester (LR-2)] In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 677 parts of bisphenol A·EO 2-mol adduct, 294 parts of terephthalic acid, and 2.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the water generated while heating to 230°C under reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 2 mg KOH / g, 29 parts of trimellitic anhydride were added, and the mixture was further reacted at 180°C under normal pressure. When the acid value became 18 mg KOH / g, the mixture was removed, and an amorphous polyester (LR-2) was obtained.
[0099] The compositions and physical properties of the amorphous polyesters (L-1) to (L-6) obtained in Examples 1 to 6 and the comparative amorphous polyesters (LR-1) to (LR-2) obtained in Comparative Examples 1 and 2 are shown in Table 1.
[0100] [Table 1]
[0101] <Production Example 3> [Synthesis of crystalline polyester (C-1)] 434 parts of 1,6-hexanediol, 686 parts of sebacic acid, and 1.5 parts of titanium diisopropoxy bistriethanolamine as a condensation catalyst were placed in a reaction vessel equipped with a stirrer, a heating / cooling device, a thermometer, a cooling tube, and a nitrogen inlet tube, and reacted for 8 hours under a nitrogen stream at 220°C while distilling off the water generated. Then, the reaction was continued under a reduced pressure of 0.001 to 0.026 MPa while removing water, to obtain a crystalline polyester (C-1). The resin had an Mn of 4500, an Mw of 15000, a melting point (Tm) of 68°C, an acid value of 1 mgKOH / g, and a hydroxyl value of 21 mgKOH / g.
[0102] <Production Example 4> [Production of Crystalline Polyester Dispersion (CDO-1)] In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, and a thermometer, 10 parts of crystalline polyester (C-1) and 90 parts of ethyl acetate were added, heated to 78°C, stirred at the same temperature for 3 hours, and then cooled to 30°C over 1 hour to crystallize the crystalline polyester (C-1) into fine particles, which were then wet-pulverized in an Ultraviscomill (manufactured by Imex Co., Ltd.) to obtain a crystalline polyester dispersion (CDO-1). The volume-based median diameter of the crystalline polyester dispersion (CDO-1) measured with an "LA-920" was 0.25 μm.
[0103] <Production Example 5> [Production of aqueous dispersion of resin fine particles (OW-1)] In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 790 parts of water and 5 parts of sodium alkylaryl sulfosuccinate (Eleminol JS-20, manufactured by Sanyo Chemical Industries, Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. This was heated to raise the temperature inside the system to 75°C, and then 5 parts of a 10% by weight aqueous solution of ammonium persulfate was added, followed by dropping a monomer mixture consisting of 89.6 parts of styrene, 49.0 parts of butyl acrylate, and 61.4 parts of methacrylic acid over a period of 2 hours. After dropping, the mixture was aged at 75°C for 10 hours to obtain 1000 parts of a microparticle dispersion (OW-1) containing resin microparticles. The volume-based median diameter of the microparticles contained in the microparticle dispersion was 0.047 μm. A part of the microparticle dispersion was dried to isolate the resin. The resin had an Mn of 30,900, an Mw of 321,000, a Tg of 60° C., and an acid value of 200 mg KOH / g.
[0104] <Production Example 6> [Production of modified wax (WD-1)] In a pressure-resistant reaction vessel equipped with a stirrer, a heating / cooling device, a thermometer, and a dropping cylinder, 454 parts of xylene and 150 parts of low molecular weight polyethylene "Sanwax LEL-400" [softening point: 128 ° C, manufactured by Sanyo Chemical Industries, Ltd.] were charged, and after nitrogen replacement, the temperature was raised to 170 ° C under stirring, and a mixed solution of 595 parts of styrene, 255 parts of methyl methacrylate, 34 parts of di-t-butylperoxyhexahydroterephthalate, and 119 parts of xylene was dropped at the same temperature over 3 hours, and the mixture was maintained at the same temperature for 30 minutes. Next, xylene was distilled off under a reduced pressure of 0.039 MPa to obtain a modified wax. The Mn of the modified wax was 1,900, Mw was 5,200, and Tg was 56.9 ° C.
[0105] <Production Example 7> [Production of release agent dispersion (WO-1)] In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, and a thermometer, 10 parts of paraffin wax "HNP-9" [melting point: 73°C, manufactured by Nippon Seiro Co., Ltd.], 5 parts of the modified wax (WD-1) obtained in Production Example 6, and 85 parts of ethyl acetate were added, heated to 78°C, and stirred at the same temperature for 3 hours, then cooled to 30°C over 1 hour to crystallize the release agent into fine particles, which were then wet-pulverized with Ultraviscomill (manufactured by Imex Co., Ltd.) to obtain a release agent dispersion (WO-1). The volume-based median diameter of the release agent dispersion (WO-1) measured with "LA-920" was 0.25 μm.
[0106] <Production Example 8> [Production of colorant dispersion (PO-1)] 20 parts of carbon black "MA100" [manufactured by Mitsubishi Chemical Corporation], 4 parts of colorant dispersant "Solsperse 28000" [manufactured by Avecia Corporation], and 56 parts of ethyl acetate were added to a reaction vessel equipped with a stirrer, a heating / cooling device, a cooling tube, and a thermometer, and after stirring to disperse uniformly, the pigment was finely dispersed using a bead mill to obtain colorant dispersion (PO-1). The volume-based median diameter of colorant dispersion (PO-1) measured with "LA-920" was 0.2 μm.
[0107] <Example 7> [Preparation of Toner (T-1)] A toner was obtained by the following method (dissolution suspension method) using the aqueous dispersion (OW-1) obtained in Production Example 5, the amorphous polyester (L-1) obtained in Example 1, the colorant dispersion (PO-1) obtained in Production Example 8, the release agent dispersion (WO-1) obtained in Production Example 7, and the crystalline polyester dispersion (CDO-1) obtained in Production Example 4. In a beaker, 330 parts of ion-exchanged water, 30 parts of aqueous dispersion of resin fine particles (OW-1), 2 parts of sodium carboxymethyl cellulose, 52 parts of sodium dodecyl diphenyl ether disulfonate "Eleminol Mon-7" [manufactured by Sanyo Chemical Industries, Ltd.], and 28 parts of ethyl acetate were added, and an aqueous solution was obtained by uniformly mixing. Next, in another beaker, 90 parts of amorphous polyester (L-1), 32 parts of colorant dispersion (PO-1), 40 parts of release agent dispersion (WO-1), and 100 parts of crystalline polyester dispersion (CDO-1) were mixed to prepare a resin dispersion in which amorphous polyester was dissolved. The entire amount of this dispersion was added to the aqueous solution previously prepared and stirred for 2 minutes with a TK auto homomixer to obtain a mixed solution. Next, this mixed solution was transferred to a reactor equipped with a stirrer and a thermometer, and the ethyl acetate was distilled off at 50°C until the concentration was 0.5% by weight or less, and a composite process was performed to obtain an aqueous resin dispersion of resin particles. The resin particles were then filtered and washed with water three times, filtered, and dried for 18 hours in a 40°C air circulation dryer to obtain resin particles containing the polyester resin (L-1) for toner of the present invention with a volatile content of 0.5% by weight or less. Next, 100 parts of the resin particles and 1 part of hydrophobic silica "Aerosil R-972" [manufactured by Nippon Aerosil Co., Ltd.] were mixed in a sample mill to obtain the toner (T-1) of the present invention.
[0108] <Example 8> [Production of Toner (T-2)] The same production method as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (L-2) obtained in Example 2, and a toner (T-2) containing the polyester resin for toner (L-2) of the present invention was obtained.
[0109] <Example 9> [Production of Toner (T-3)] The same production method as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (L-3) obtained in Example 3, and a toner (T-3) containing the polyester resin for toner (L-3) of the present invention was obtained.
[0110] <Example 10> [Production of Toner (T-4)] The same production method as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (L-4) obtained in Example 4, and a toner (T-4) containing the polyester resin for toner (L-4) of the present invention was obtained.
[0111] <Example 11> [Production of Toner (T-5)] The procedure of Example 7 was repeated except that the amorphous polyester was changed to the amorphous polyester (L-5) obtained in Example 5, toner (T-5) containing the polyester resin for toner (L-5) of the present invention was obtained.
[0112] <Example 12> [Production of Toner (T-6)] The same production method as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (L-6) obtained in Example 6, and a toner (T-6) containing the polyester resin for toner (L-6) of the present invention was obtained.
[0113] <Comparative Example 3> [Production of Toner (TR-1)] The same production as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (LR-1) obtained in Comparative Example 1, and a toner (TR-1) containing the polyester resin for toner (LR-1) was obtained.
[0114] <Comparative Example 4> [Production of Toner (TR-2)] The same production as in Example 7 was carried out except that the amorphous polyester was changed to the amorphous polyester (LR-2) obtained in Comparative Example 2, and a toner (TR-2) containing the polyester resin for toner (LR-2) was obtained.
[0115] The low temperature fixability and heat resistance storage stability of the toners (T-1) to (T-6) and (TR-1) to (TR-2) of the examples and comparative examples were evaluated by the following methods. The blending amount, physical properties and evaluation results of each toner are shown in Table 2.
[0116] [Table 2]
[0117] <Low temperature fixability> Toner is applied on the paper at 0.8mg / cm 2 The powder is applied evenly to the paper surface using a printer without a heat fixing unit. Other methods may be used as long as they can apply the powder evenly at the above weight density. The paper was then fixed to the pressure roller at a fixing speed (heat roller peripheral speed) of 213 mm / sec and a fixing pressure (pressure roller pressure) of 10 kg / cm. 2 The temperature at which cold offset occurs (MFT) was measured when the paper was passed through the above conditions. The lower the temperature at which cold offset occurs, the better the low-temperature fixing property. In this evaluation condition for low-temperature fixability, a temperature of 125° C. or lower is considered to be preferable. ◎: 105℃ or less ○: 106~115℃ △: 116~125℃ ×: 126℃ or higher
[0118] <Heat and humidity resistance> The toners (T-1) to (T-6) and (TR-1) to (TR-2) were allowed to stand for 20 hours in an atmosphere of 40° C. and a relative humidity of 80%, and the humidity and heat resistance storage stability was evaluated according to the degree of blocking according to the following criteria. [Evaluation Criteria] ◎: No blocking occurs. ◯: Blocking occurs, but the particles disperse easily when force is applied. ×: Blocking occurs and the particles do not disperse even when force is applied.
[0119] The toners (T-1) to (T-6) of the examples containing the polyester resins (L-1) to (L-6) of the present invention exhibited excellent performance in both low-temperature fixing property and heat and humidity resistant storage stability. On the other hand, the toners (TR-1) and (TR-2) using the polyester resins (LR-1) and (LR-2) were poor in low temperature fixing property and humidity and heat resistance storage property. [Industrial Applicability]
[0120] The polyester resin for toner of the present invention can achieve both low-temperature fixing property and moist heat resistance storage stability at high levels, and is extremely useful as a resin for use in toner for developing electrostatic images used in electrophotography, electrostatic recording, electrostatic printing, etc.
Claims
1. A polyester resin for toner, characterized by having an α-terpinyl structure.
2. 2. The polyester resin for toner according to claim 1, wherein the polyester resin is obtained by using, as raw material monomers, a carboxylic acid component containing at least a carboxylic acid compound having an α-terpinyl structure and / or an alcohol component containing an alcohol having an α-terpinyl structure, and subjecting the carboxylic acid component and the alcohol component to condensation polymerization.
3. 3. The polyester resin for toner according to claim 2, wherein the total amount of the carboxylic acid compound having an α-terpinyl structure and the alcohol having an α-terpinyl structure is 10 to 100 mol % of the total amount of the carboxylic acid component and the alcohol component.
4. 2. The polyester resin for toner according to claim 1, which has a glass transition temperature of 40 to 120°C.
5. 3. The polyester resin for toner according to claim 2, wherein the carboxylic acid compound having an α-terpinyl structure is 2-α-terpinoxy-succinic acid.
6. 3. The polyester resin for toner according to claim 2, wherein the alcohol having an α-terpinyl structure is 3-α-terpinoxy-1,2-propanediol.
7. A toner comprising the polyester resin for toners according to any one of claims 1 to 6.
Citation Information
Patent Citations
Monomer, polymeric compound, photosensitive composition, pattern formation using the composition and production of electronic component
JP1999171835A
Novel biodegradable resin
JP2003261658A
Polyester resin for toner and toner composition
JP2009251248A
Toner for electrostatic charge image development, developer for electrostatic charge image development, toner cartridge, process cartridge, and image forming apparatus
JP2013068829A
Toner binder, manufacturing method of the same, and toner
JP2015172720A