Active Electrode Material
Niobium mixed oxides with specific compositional modifications address the limitations of graphite and LTO anodes by enhancing conductivity and capacity, enabling high-power lithium-ion batteries with improved safety and energy density.
Patent Information
- Application Number
- JP2023509494
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-09
- Filing Date
- 2021-08-27
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2041-08-27
AI Technical Summary
Lithium-ion batteries with graphite anodes face limitations in charging rates due to lithium dendrite formation, leading to safety issues and reduced capacity, while alternative materials like lithium titanate (LTO) and niobium mixed oxides suffer from low electronic conductivity and reduced energy density, limiting their application in high-power and fast-charging scenarios.
Development of niobium mixed oxides with specific compositions and modifications, such as cation and anion substitutions, to enhance electronic conductivity and improve electrochemical properties, allowing for higher charging rates and energy density without extensive nanoscale engineering.
The modified niobium mixed oxides exhibit improved electron conductivity, Coulombic efficiency, and delithiation voltage at high C rates, enabling high-power lithium-ion batteries with enhanced safety and energy density, suitable for fast charge/discharge applications.
Smart Images

Figure 0007587682000012 
Figure 0007587682000013 
Figure 0007587682000001
Abstract
Description
[Technical field]
[0001] The present invention relates to active electrode materials and methods for making active electrode materials. Such materials of interest are of interest, for example, as materials for the anode of lithium-ion batteries, and as active electrode materials in lithium-ion or sodium-ion batteries. [Background technology]
[0002] Lithium-ion (Li-ion) batteries are a type of commonly used rechargeable battery, with the global market predicted to grow to $200 billion by 2030. Li-ion batteries are the technology of choice for electric vehicles, which meet multiple requirements from technical capabilities to environmental impact, providing a feasible path for a greener automotive industry.
[0003] A typical lithium-ion battery consists of multiple cells connected in series or parallel. Each cell usually consists of an anode (negative electrode) and a cathode (positive electrode), separated by a porous, electrically insulating membrane (called a separator) and immersed in a liquid (called the electrolyte) that allows the transport of lithium ions.
[0004] In most systems, the electrode consists of an electrochemically active material, meaning that it can chemically react with lithium ions to reversibly store and release them in a controlled manner, optionally mixed with conductive additives (such as carbon) and a polymeric binder. A slurry of these components is coated as a thin film onto a current collector (typically a thin foil of copper or aluminum) so that when dried, it forms the electrode.
[0005] In known Li-ion battery technologies, graphite anodes have safety limitations during battery charging, which is a major obstacle for high-power electronic, automotive and industrial applications. Among various promising alternatives recently proposed, lithium titanate oxide (LTO) and niobium mixed oxide are promising candidates to replace graphite as the optimal active material for high-power and fast-charging applications.
[0006] Batteries relying on graphite anodes are fundamentally limited in terms of charge rate. Under nominal conditions, lithium ions are inserted into the anode active material during charging. At higher charge rates, typical graphite voltage profiles are at high risk of overpotentially driving the potential of the anode site below 0V vs. Li / Li+, resulting in lithium ions instead depositing as lithium metal on the surface of the graphite electrode, a phenomenon known as lithium dendrite electroplating. This results in an irreversible loss of active lithium and therefore a rapid loss of cell capacity. In some cases, these dendritic deposits can grow to such a large size that they can penetrate the battery separator, leading to a short circuit of the cell. This can trigger a catastrophic failure of the cell, resulting in fire or explosion. Therefore, the fastest charging batteries with graphite anodes are limited to charge rates of 5-7C, but often significantly lower.
[0007] Lithium titanate (LTO) anodes have excellent cycle life because they are not subject to dendrite electroplating at high charge rates due to their high potential (1.6 V vs. Li / Li+) and because their 3D crystalline structure supports them, they do not suffer from significant volume expansion of the active material upon lithium ion intercalation. For these two reasons, LTO cells are generally considered to be safer cells. However, LTO is a relatively poor electronic and ionic conductor, limiting its high rate capacity retention and power capability unless the material is nano-scaled to increase its specific surface area and carbon-coated to increase its electronic conductivity. This particle-level material engineering increases the porosity and specific surface area of the active material, significantly reducing the packing density achievable in the electrode. This leads to a lower density electrode and a higher proportion of electrochemically inactive materials (e.g., binders, carbon additives), which leads to significantly lower gravimetric and volumetric energy densities.
[0008] An important indicator of anode performance is the volumetric capacity (mAh / cm) of the electrode. 3), i.e., the amount of charge (i.e., lithium ions) that can be stored per unit volume of the anode. This amount, when combined with the cathode and appropriate cell design parameters, is a key factor in determining the overall battery energy density (Wh / L) on a volumetric basis. The volumetric capacity of an electrode is related to the electrode density (g / cm 3 ), the specific capacity of the active material (mAh / g), and the fraction of active material in the electrode. LTO anodes typically have a relatively low specific capacity (~165 mAh / g, compared to ~330 mAh / g for graphite), which accounts for the low electrode density mentioned above (typically 2.0 g / cm 3 This, combined with the small proportion of active material (less than 90%), results in a very small volumetric capacity (300 mAh / cm 3 The LTO battery / cells have a low energy density (less than 1000 kWh) and therefore a high cost per kWh in various applications. As a result, LTO batteries / cells are generally limited to niche specific applications, despite their long cycle life, fast charging capability, and high safety.
[0009] Niobium mixed oxide structures have recently been of interest for use in Li-ion cells. Zhu et al., J. Mater. Chem. A,2019, 7,25537 and Zhu et al., Chem. Commun., 2020,56, 7321-7324, have proposed the use of Zn as a possible active electrode material. 2 Nb 34 O 87 and Cu 2 Nb 34 O 87discloses. These papers rely on complex particle-level engineering to purportedly achieve superior properties while trying to control, for example, particle porosity and morphology. It is believed that the properties of these materials can be improved. For example, these materials may not have sufficient electronic conductivity to allow efficient charging and discharging in commercial Li-ion cells, resulting in excess impedance. In addition, there is still room for improvement in tuning Li-ion capacity, coulombic efficiency, and charge and discharge voltage profiles. Making these improvements described herein, which do not require extensive nanoscale or particle-level engineering and do not require coatings, is a critical step towards low-cost battery materials for mass market adoption. If these improvements are not addressed, the resulting devices will have excess electrical resistance, leading to reduced energy density, increased polarization, reduced power density, reduced energy efficiency, and increased cost. Thus, Zn 2 Nb 34 O 87 and Cu 2 Nb 34 O 87 There remains a need to improve the properties of for use in lithium ion batteries. Summary of the Invention
[0010] In a first aspect, the present invention provides an active electrode material comprising a niobium mixed oxide, the niobium mixed oxide having the composition M1 a M2 2-a M3 b Nb 34-b O 87-c-d Q d wherein M1 and M2 are different, M1 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi and mixtures thereof; M2 is Zn or Cu; M3 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi and mixtures thereof; Q is selected from F, Cl, Br, I, N, S, Se, and mixtures thereof; 0≦a<1.0, 0≦b≦3.4, −0.5≦c≦4.35, 0≦d≦4.35, One or more of a, b, c, and d is not equal to 0, and If a, b, and d are 0, then c is greater than 0.
[0011] The composition of niobium mixed oxide is stoichiometric Zn 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 It will be understood that the present invention does not correspond to Zn by incorporating additional cations (M1 and / or M3). 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 It has been found that by modifying the niobium mixed oxide and / or by creating an induced oxygen deficiency or excess and / or by forming an anion mixed material (containing O and Q), the resulting material has improved electrochemical properties, especially when used as an anode material. When a>0, the niobium mixed oxide is modified by partial substitution of M2 (Zn or Cu) by M1. When b>0, the niobium mixed oxide is modified by partial substitution of Nb by M3. When c≠0, the niobium mixed oxide is modified by oxygen deficiency or excess. When d>0, the niobium mixed oxide is modified by partial substitution of O by Q. As shown by this example, the inventors have found that the material according to the invention ..., compared to the unmodified "base" Zn 2 Nb 34 O 87We have found that compared to , the materials of the present invention have improved electronic conductivity, improved coulombic efficiency, and improved delithiation voltage at high C rates. These are important results in demonstrating the advantages of the materials of the present invention for use in high power batteries designed for rapid charge / discharge.
[0012] The active electrode material of the present invention is particularly useful in electrodes, preferably for use in the anodes of lithium-ion or sodium-ion batteries. Thus, in a further embodiment of the present invention, the active electrode material of the first aspect comprises a niobium mixed oxide and at least one other component. Optionally, the at least one other component is selected from a binder, a solvent, a conductive additive, a different active electrode material, and mixtures thereof. Such compositions are useful for the manufacture of electrodes. A further embodiment of the present invention is an electrode comprising the active electrode material of the first aspect in electrical contact with a current collector. A further embodiment of the present invention is an electrochemical device comprising an anode, a cathode, and an electrolyte disposed between the anode and the cathode, the anode comprising the active electrode material according to the first aspect, and optionally the electrochemical device being a lithium-ion or sodium-ion battery.
[0013] In a second aspect, the present invention provides a method for producing a niobium mixed oxide as defined according to the first aspect, the method comprising the steps of obtaining one or more precursor materials, mixing the precursor materials to form a precursor material mixture, and heat treating the precursor material mixture at a temperature in the range of 400° C. to 1350° C. or 800 to 1350° C., thereby obtaining a niobium mixed oxide. This represents a convenient and efficient method for producing the active electrode material of the first aspect.
[0014] The present invention includes combinations of the aspects and features described herein, except where such combinations are expressly disallowed or explicitly avoided.
[0015] The principles of the present invention will now be described with reference to the accompanying drawings. [Brief description of the drawings]
[0016]
Figure 1
Figure 2
[0017] Aspects and embodiments of the present invention will now be described with reference to the accompanying drawings. Further aspects and embodiments will be apparent to those skilled in the art. All documents mentioned in this text are incorporated herein by reference.
[0018] The term "mixed niobium oxide" (MNO) may refer to an oxide containing niobium and at least one other cation. MNO materials have a high redox voltage vs. lithium, greater than 0.8 V, allowing for safe, long-life operation, essential for fast charging of battery cells. Additionally, the niobium cation can undergo two redox reactions per atom, resulting in a higher theoretical capacity than, for example, LTO. The niobium mixed oxides described herein are Zn 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 It comes from the basic structure of:
[0019] Zinc 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 is ReO 3 Origin of MO 3-x Preferably, the niobium mixed oxide has the Wadsley-Roth crystal structure. The Wadsley-Roth crystal structure is a MO structure that includes crystallographic shear. 3 (ReO 3 ) crystal structure, and is considered to be the crystallographic off-stoichiometry of MO 3-x As a result, these structures usually have [MO6 MNO materials with these structures are believed to have advantageous properties for use as active electrode materials in, for example, lithium ion batteries.
[0020] In addition, the open tunnel-like MO of the MNO material 3 The crystal structure also makes it an ideal candidate for achieving high capacity Li-ion storage and high rates of exchangeable intercalation / deintercalation. The crystallographic off-stoichiometry present in the MNO structure gives rise to Wadsley-Roth crystallographic superstructures. These superstructures, compounded by other properties such as the Jahn-Teller effect and greater crystallographic disorder by utilizing multiple mixed cations, stabilize the crystal, keep it stable by opening tunnels during intercalation, and provide high lithium diffusion rates (approximately 10 -13 cm 2 s -1 This allows for the ability to achieve very high rates of
[0021] Zinc 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 The crystal formula of is [MO 6 It can be described as having a 3x4x∞ crystallographic block structure composed of octahedra, where M is Cu, Zn, or Nb. The Cu and Zn octahedra may be randomly distributed in the structure or may prefer specific locations such as the edges or corners of the blocks. This equates to one Zn or 2 / 3 Cu cation per block. Zn 2 Nb 34 O 87 The crystal formula is Cu 2 Nb 34 O 87 It can be described as an isostructural phase of , with slight differences in bond lengths and bond enthalpies.
[0022] The entire crystalline composition of the materials described herein is preferably charge neutral and thermodynamically favorable to comply with the above description. x O y M x O y-δ Oxygen-deficient structures are preferred when they reduce the electrical resistivity of the material so that, for example, oxygen vacancies are introduced. Oxygen-deficient structures may include shear defects. Structures in which cations (i.e., Zn, Cu, and Nb) or anions (i.e., O) are substituted may be done so with matching valences (i.e., 5+ cations for equal proportions of 4+ and 6+ cations) or with mismatched valences, which may induce oxygen deficiencies or excesses if the substitutions are made at equivalent crystal sites. Substitutions may also occur at different crystal sites, such as intermediate sites.
[0023] The crystal structure of a material can be determined by analysis of X-ray diffraction (XRD) patterns, as is widely known. For example, an XRD pattern obtained from a particular material can be compared to known XRD patterns to ascertain the crystal structure via a public database, for example, the ICDD Crystallography Database. Rietveld refinement can also be used to determine the crystal structure of a material, in particular the unit cell parameters. Thus, the active electrode material can have a Wadsley-Roth crystal structure, as determined by X-ray diffraction.
[0024] Preferably, the crystal structure of the niobium mixed oxide is determined by X-ray diffraction and is 2 Nb 34 O 87 or Cu 2 Nb 34 O 87 , most preferably Zn 2 Nb 34 O 87 Thus, it can be seen that the "base" material has been modified without significantly affecting the crystal structure, which is believed to have advantageous properties for use as an active electrode material. Zn 2 Nb 34 O 87The crystal structure of can be found in ICDD crystallography database entry JCPDS28-1478.
[0025] The niobium mixed oxides with cation / anion exchange may have unit cell parameters a, b, and c, where a is 15.52-15.58 angstroms, preferably 15.53-15.57 angstroms, b is 3.79-3.84 angstroms, preferably 3.80-3.83 angstroms, and c is c=20.53-20.66 angstroms, preferably 20.54-20.65 angstroms. The niobium mixed oxides may have unit cell parameters α and γ that are each about 90°, preferably α=γ=90°, while β is 113.05-113.75. 0 , preferably 113.08 to 113.69 0 The unit cell volume is 1115 to 1135 angstroms. 3 , preferably 1117 to 1133 angstroms 3 The unit cell parameters can be determined by X-ray diffraction. The niobium mixed oxide can have a crystallite size of 5 to 150 nm, preferably 30 to 60 nm, determined according to the Scherrer formula.
[0026] Here, the term "corresponding" is intended to reflect that the peaks in the X-ray diffraction pattern may be shifted by 0.5 degrees or less (preferably by 0.25 degrees or less, more preferably by 0.1 degrees or less) from the corresponding peaks in the X-ray diffraction pattern of the material listed above.
[0027] Niobium mixed oxide has the composition M1 a M2 2-a M3 b Nb 34-b O 87-cd Q d wherein M1 and M2 are different, M1 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi and mixtures thereof; M2 is Zn or Cu; M3 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi and mixtures thereof; Q is selected from F, Cl, Br, I, N, S, Se, and mixtures thereof; 0≦a<1.0, 0≦b≦3.4, −0.5≦c≦4.35, 0≦d≦4.35, One or more of a, b, c, and d is not equal to 0, and If a, b, and d are 0, then c is greater than 0.
[0028] "and mixtures thereof" is intended to mean that M1, M3, and Q can each represent two or more elements from the individual enumerations. Examples of such materials are Mg 0.1 Ge 0.1 Zinc 1.8 Nb 34 O 87.1 Here, M1 is Mg a’ Ge a’’ (a'+''=a), M2 is Zn, a=0.2, b=0, c=-0.1, d=0. Here, c is the typical oxidation state of each cation, i.e., Mg 2+ , Ge 4+ ,zinc 2+ , and Nb 5+ The calculations are based on the assumption that
[0029] The exact values of a, b, c, d within the defined ranges may be selected to provide a charge-balanced or substantially charge-balanced crystal structure. Additionally or alternatively, the exact values of a, b, c, d within the defined ranges may be selected to obtain a crystal structure that is thermodynamically stable or thermodynamically metastable.
[0030] If exchange of cations or anions in the structure (i.e., Zn, Cu, Nb, O) occurs without preserving the original valence, it can cause both oxygen deficiency and excess. For example, to some extent Zn 2+ Ge 4+ The replacement material has a slight excess of oxygen (i.e., ZnO vs. GeO 2 ), while Nb 5+ Al 3+ Replacement with Nb 2 O 5 Against Al 2 O 3 ) Oxygen deficiency can also be induced by heat treatment under inert or reducing conditions, resulting in the induction of oxygen vacancy defects in the structure.
[0031] There may be partial oxidation or partial reduction that compensates for the exchange, without retaining the original valence. For example, Ge 4+ Zn by 2+ The substitution of Nb 5+ From Nb 4+ This can be at least partially compensated for by reduction of
[0032] M2 is Zn or Cu. Preferably, M2 is Zn, in which case the material is Zn 2 Nb 34 O 87 Based on.
[0033] M1 is a cation that substitutes for M2 in the crystal structure. M1 can be selected from Mg, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Ge, Sn, P, and mixtures thereof, preferably Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P, and mixtures thereof, most preferably Mg, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, Ge, P, and mixtures thereof. M1 is M2 2+ This results in an oxygen deficiency or excess. Optionally, M1 can have a valence different from M2 2+ has a valence equal to or higher than that, and preferably has a valence higher than that.
[0034] M1 may also be selected from each of the specific elements used by itself in the examples.
[0035] When more than one element is present as M1 or M3, it is understood that the valence refers to M1 or M3 as a whole. For example, if 25 at% of M1 is Ti and 75 at% of M1 is W, then the valence of M1 is 0.25 x 4 (contribution from Ti) + 0.75 x 6 (contribution from W).
[0036] M1 is M2 2+ Preferably, the ionic radii of the niobium mixed oxides are different from, and most preferably smaller than, Zn. This causes a change in the unit cell dimensions, resulting in local distortions in the crystal structure, leading to the advantages described herein. The ionic radii referred to herein are Shannon's ionic radii (available from RD Shannon, Acta Cryst., A32, 1976, 751-767) for the coordination and valence that the ions are expected to adopt in the crystal structure of niobium mixed oxides. For example, Zn 2 Nb 34 O 87 The crystal structure of 5+ O 6 Octahedron and Zn 2+ O6 It contains an octahedron. Therefore, if M3 is Zr, the ionic radius is 6-coordinate Zr 4+ This is considered to be the ionic radius of Zn 2 Nb 34 O 87 This is because this is the typical valence and coordination of Zr when substituting Nb in the above.
[0037] The amount of M1 is determined by a, which meets the criteria 0≦a<1.0.a. a can be 0≦a≦0.6, preferably 0≦a≦0.2. Most preferably a>0, for example a≧0.01. If M1 has the same valence as M2, higher values of a can be more easily achieved. When M1 contains a cation with a valence of 2+ (e.g. Mg), a can be 0≦a<1.0. When M1 does not contain a cation with a valence of 2+, a can be 0≦a≦0.15.
[0038] M3 is a cation that substitutes for Nb in the crystal structure. M3 can be selected from Mg, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Sn, P, and mixtures thereof, preferably Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P, and mixtures thereof, most preferably Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P, and mixtures thereof. M3 is Nb 5+ This results in a deficiency or excess of oxygen. Preferably, M3 is Nb 5+ It has a lower valence, which creates an oxygen deficiency, i.e., the presence of oxygen vacancies, which provide the advantages discussed herein.
[0039] M3 may also be selected from each of the specific elements used by itself in the examples.
[0040] M3 is Nb 5+Preferably, the ionic radius is different from, and most preferably larger than, , which causes a change in the unit cell dimensions and local distortions in the crystal structure, resulting in the benefits described herein.
[0041] The amount of M3 is determined by b and satisfies the criterion 0≦b≦3.4, where b may be 0≦b≦1.5, preferably 0≦b≦0.3. In each of these cases, b>0, for example b≧0.01. 5+ When M3 has the same valence as M, higher values of b can be more easily achieved. When M3 contains a cation with a valence of 5+ (e.g., Ta), b can be 0≦b<3.4. When M3 does not contain a cation with a valence of 5+, b can be 0≦b≦0.2.
[0042] Surprisingly, it has been found that the cation substitution approach of the present invention can result in niobium mixed oxides that are more economically synthesized than the unmodified "base" material. Optionally, both a and b are greater than 0. When both a and b are greater than 0, the "base" material is substituted on both the M2 and Nb sites.
[0043] c reflects the oxygen content of the niobium mixed oxide. If c is greater than 0, it forms an oxygen deficient material, i.e., the material has oxygen vacancies. Such a material does not have exact charge balance without changing the oxygen state of the cations, but is considered to be "substantially charge balanced" as described above. Alternatively, c may be equal to 0, in which case it is not an oxygen deficient material. c may be less than 0, which is an oxygen rich material. c may be -0.25≦c≦4.35.
[0044] When c is 4.35, the number of oxygen vacancies is equal to 5% of the total oxygen in the 5% crystal structure. c may be greater than 0.0435, greater than 0.087, greater than 0.174, or greater than 0.435. c may be between 0 and 2, between 0 and 0.75, between 0 and 0.5, or between 0 and 0.25. For example, c may satisfy 0.01≦c≦4.35. When a material is oxygen deficient, e.g., oxygen deficiency is induced, the electrochemical properties of the material may be improved, e.g., electrical conductivity may be improved in resistive measurements, compared to a comparable non-oxygen deficient material. As will be understood, the percentage values expressed herein are atomic percentages.
[0045] The present invention relates to niobium mixed oxides which may contain oxygen vacancies (oxygen deficient niobium mixed oxides) or may have an oxygen excess. Oxygen vacancies may be formed in niobium mixed oxides by the substitution of secondary valences of the base material as described above, and oxygen excess may be formed in niobium mixed oxides by the substitution of increased valences. Oxygen vacancies may also be formed by heating niobium mixed oxides under reducing conditions, which may be referred to as the formation of induced oxygen deficiencies. The amount of oxygen vacancies and excess is determined based on the total amount of oxygen in the base material, i.e. the amount of oxygen in the non-substituted material (e.g. Zn 2 Nb 34 O 87 ) relative to the amount of oxygen.
[0046] There are many methods to determine whether oxygen deficiencies, e.g., oxygen vacancies, exist in a material. For example, thermogravimetric analysis (TGA) can be performed to measure the mass change of a material when heated in an air atmosphere. A material containing oxygen vacancies may gain mass when heated in air as the material "reoxidizes" and the oxygen vacancies are filled with oxide anions. The magnitude of the mass increase can be used to quantify the concentration of oxygen vacancies in the material. This is assuming that the mass increase occurs because oxygen vacancies are filled across the board. It should be noted that a material containing oxygen vacancies may experience an initial mass increase as the oxygen vacancies are filled, and then a mass loss at higher temperatures as the material undergoes thermal decomposition. Additionally, the mass loss and mass gain processes may overlap, i.e., some materials containing oxygen vacancies may not show a mass increase (and in some cases may show neither a mass loss nor a mass gain) during TGA analysis.
[0047] Other methods to determine whether oxygen deficiencies, such as oxygen vacancies, are present include Raman spectroscopy, electron paramagnetic resonance (EPR), X-ray photoelectron spectroscopy (XPS, e.g., XPS of oxygen 1s and / or XPS of cations of mixed oxides), X-ray absorption near edge structure (XANES, e.g., XANES of cations of mixed metal oxides), and TEM (e.g., scanning TEM (STEM) with high angle annular dark field (HAADF) and annular bright field (ABF) detector). The presence of oxygen deficiencies can be qualitatively determined by evaluating the color of the material compared to a non-oxygen deficient sample of the same material, indicating a change in electronic band structure upon interaction with light. For example, stoichiometric Zn, which is not oxygen deficient, exhibits a change in the color of the material due to interaction with light. 2 Nb 34 O 87 The white color is due to oxygen deficiency. 2 Nb 34 O <87 has a grey / black colour. The presence of vacancies can also be inferred from the properties of a stoichiometric material, e.g. electrical conductivity, compared to the properties of an oxygen deficient material.
[0048] When d>0, additional anions Q are introduced into the niobium mixed oxides. Their electronic structures are different (i.e., F - vs. O 2- ), and the ionic radius is different (6 coordinates O 2- = 1.40 Å, 6 coordinates F - =1.33 Å), they may improve the electrochemical capabilities of the active material. This is because they modify the properties of the unit cell with different ionic radii, allowing for improved Li-ion capacity or improved reversibility. They may further improve electrical conductivity by modifying the electronic structure of the crystal (i.e., doping effect), with respect to oxygen vacancy defects, or subvalent cation substitution. d may be 0≦d≦3.0, or 0≦d≦2.17. In each of these cases, d>0. Q may be selected from F, Cl, N, S, and mixtures thereof, or F, N, and mixtures thereof, or Q is F.
[0049] Optionally, d=0, in which case the material has composition M1 a M2 2-a M3 b Nb 34-b O 87-c where M1, M2, M3, a, b, and c are as defined herein. Advantageously, materials with d=0 do not contain the anion Q and may be easier to synthesize.
[0050] When a>0 and b=d=0, the material is M1 a M2 2-a Nb 34 O 87-c where M1, M2, a and c are as defined herein, e.g., 0≦c≦4.35. This represents a material modified at the site of M2, optionally modified by induced oxygen deficiency. Such a material can be prepared by simple synthetic means from the "base" oxide M2. 2 Nb 34 O 87where M1 can represent Ti, Mg, V, Cr, W, Zr, Mo, Cu, Ga, Ge, Ni, Al, Hf, Ta, Zn and mixtures thereof, preferably Ti, Mg, V, Cr, W, Zr, Mo, Ga, Ge, Al, Zn and mixtures thereof.
[0051] When a=b=d=0 and c>0, the substance has composition M2 2 Nb 34 O 87-c where M2 and c are as defined herein. This represents a material that has been modified solely by inducing oxygen deficiency, imparting improved properties as shown in the examples. For example, a material with a=b=d=0 and c>0 has been found to have surprisingly improved electronic conductivity.
[0052] It is to be understood that the discussion of the compositional variables (M1, M2, M3, Q, a, b, c, and d) are intended to be read in combination. For example, preferably, M1 is selected from Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P, and mixtures thereof, M3 is selected from Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P, and mixtures thereof, and Q is selected from F, Cl, N, S, and mixtures thereof. It is preferred that 0≦a≦0.6, 0≦b≦1.5, 0≦c≦4.35, and 0≦d≦3.0.
[0053] For example, niobium mixed oxide has the composition M1 a M2 2-a M3 b Nb 34-b O 87-cd Q d wherein M1 and M2 are different, M1 is selected from Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P, and mixtures thereof; M2 is Zn or Cu; M3 is selected from Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P, and mixtures thereof; Q is selected from F, N, and mixtures thereof; 0≦a≦0.6, 0≦b≦1.5, −0.5≦c≦4.35, 0≦d≦4.35, One or more of a, b, c, and d is not equal to 0, and If a, b, and d are 0, then c is greater than 0.
[0054] For example, niobium mixed oxide has the composition M1 a Zinc 2-a M3 b Nb 34-b O 87-c-d Q d wherein M1 is selected from Mg, Zr, V, Cr, Mo, W, Fe, Cu, Al, Ge, P, and mixtures thereof; M3 is selected from Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P, and mixtures thereof; Q is selected from F, N, and mixtures thereof; 0 <a≦0.2、0≦b≦0.3、0≦c≦4.35、0≦d≦3.0である。
[0055] M1, M3, and Q may also be selected from each of the specific elements used as these dopants in the embodiments.
[0056] Optionally, the niobium mixed oxide is titanium free.
[0057] Niobium mixed oxide has the composition M1 a M2 2-a M3 b Nb 34-b O 87-c wherein M1 is selected from Cr, Al, Ge, and mixtures thereof, preferably M1 is Cr; M2 is Zn or Cu, preferably M2 is Zn; M3 is selected from Ti, Zr, Fe, and mixtures thereof, optionally including Ti. Preferably, M3 is selected from Ti, Zr, and mixtures thereof, optionally including Ti. Most preferably, M3 is Ti. 0 < a < 1.0, preferably 0.01 < a < 1.0. 0 < b ≤ 1.5, preferably 0.01 < b < 1.0. -0.5 ≤ c ≤ 4.35, preferably -0.5 ≤ c ≤ 2. Most preferably, c = 0.
[0058] The niobium mixed oxide has the composition Cr a Zn 2-a M3 b Nb 34-b O 87-c wherein M3 is selected from Ti, Zr, and mixtures thereof, optionally including Ti. Preferably, M3 is Ti. 0.01 < a < 1.0, preferably 0.1 < a < 1.0. 0.01 < b < 1.0, preferably 0.1 < b < 1.0. -0.5 ≤ c ≤ 2, preferably c = 0.
[0059] The niobium mixed oxide may further contain Li and / or Na. For example, Li and / or Na may enter the crystal structure when the niobium mixed oxide is used as an electrode in a metal ion battery.
[0060] The niobium mixed oxide is preferably granular. The substance may have a particle size D in the range of 0.1 - 100 μm, or 0.5 - 50 μm, or 1 - 20 μm. These particle sizes are advantageous because they facilitate processing and manufacturing into electrodes. Furthermore, these particle sizes eliminate the need to use complex and / or expensive methods that result in nanosized particles. Nanosized particles (e.g., particles having a particle size D of 100 nm or less) are usually more complex to synthesize and further require consideration of safety. 50 The niobium mixed oxide is preferably granular. The substance may have a particle size D in the range of 0.1 - 100 μm, or 0.5 - 50 μm, or 1 - 20 μm. These particle sizes are advantageous because they facilitate processing and manufacturing into electrodes. Furthermore, these particle sizes eliminate the need to use complex and / or expensive methods that result in nanosized particles. Nanosized particles (e.g., particles having a particle size D of 100 nm or less) are usually more complex to synthesize and further require consideration of safety. 50 of the particle size) are usually more complex to synthesize and further require consideration of safety.
[0061] The niobium mixed oxide has a D of at least 0.05 μm, or at least 0.1 μm, or at least 0.5 μm, or at least 1 μm. 10 D 10 Maintaining the particle size in these ranges reduces the potential for parasitic reactions in Li-ion cells due to reduced surface area and allows for easier processing, requiring less binder in the electrode slurry.
[0062] Niobium mixed oxides are those with a D of 200 μm or less, 100 μm or less, 50 μm or less, or 20 μm or less. 90 D 90 By maintaining the particle size in these ranges, the proportion of the particle size distribution at larger particle sizes is minimized, making it easier to fabricate the material into a homogenous electrode.
[0063] The term "particle size" refers to the equivalent spherical diameter (esd), i.e., the diameter of a sphere having the same volume as a given particle, the volume of the particle being understood to include the volume of any intraparticle pores. n " and "D n The term "diameter of a particle" refers to the diameter below which n% of the particle population is found. 50 " and "D 50 The term "particle size" refers to the volume-based median particle size below which 50% by volume of the particle population are found. It will be understood that where the material contains primary crystallites aggregated into secondary particles, the particle size refers to the diameter of the secondary particles. Particle size can be determined by laser diffraction. Particle size can be measured in accordance with ISO 13320:2009, e.g., using Mie theory.
[0064] Niobium mixed oxide is 0.1 to 100m 2 / g, or 0.5 to 50m 2 / g, or 1 to 20m 2The niobium mixed oxide may have a BET surface area in the range of 0.1 to 1.0 μm / g. In general, a low BET surface area is preferred to minimize the reaction of the niobium mixed oxide with the electrolyte, for example, to minimize the formation of a solid electrolyte interphase (SEI) layer during the first charge-discharge cycle of an electrode containing the material. However, if the BET surface area is too low, a large portion of the niobium mixed oxide will not be accessible to the metal ions in the surrounding electrolyte, resulting in unacceptably low charge rates and capacities.
[0065] The term "BET surface area" refers to the surface area per unit mass calculated from measurements of the physical adsorption of gas molecules on a solid surface using the Brunauer-Emmett-Teller theory. For example, the BET surface area can be determined in accordance with ISO9277:2010.
[0066] The specific capacity / reversible delithiation capacity of the niobium mixed oxides can be 180 mAh / g or more, 190 mAh / g or more, or 197 mAh / g or more, where the specific capacity is defined as measured in the second cycle of a galvanostatic cycling test of the half-cell at a rate of 0.1 C in the half-cell voltage window of 1.1 to 3.0 V vs. Li / Li+. Obtaining a material with a high specific capacity can be advantageous since it can provide improved performance in electrochemical devices that include the niobium mixed oxides.
[0067] According to the description below, when formulated or coated as an electrode (optionally with conductive carbon additives and binder materials), the sheet resistivity of the active electrode material, measured as defined in the examples, can be 2.5 kΩ per square or less, more preferably 1.2 kΩ per square or less. Sheet resistivity is useful as a surrogate measure of the electronic conductivity of such materials. Providing a material with a suitably low sheet resistivity can be advantageous, as it can result in improved performance in electrochemical devices that include niobium mixed oxides.
[0068] Niobium mixed oxide is 10 -15 cm 2 s-1 Greater than, or more preferably, 10 -13 cm 2 s -1 Providing a material with a suitably high lithium diffusion rate can be advantageous as it can result in improved performance in electrochemical devices that include the niobium mixed oxide.
[0069] The niobium mixed oxide was formed into a composite electrode with suitable binder and conductive additives according to the following description, and after calendering, had a mass of 2.5 g / cm 3 This allows composite electrodes with electrode porosity (calculated by average of measured electrode density / true density of each component) in the range of 30-40%, in line with industrial requirements for high energy and high power cells. For example, up to 2.9 g / cm 3 Electrode densities of up to 10 ...
[0070] The initial coulombic efficiency is measured as the difference between the lithiation capacity and the delithiation capacity measured as the difference between the lithiation capacity and the delithiation capacity in the first charge / discharge cycle at C / 10 of the half cell. The initial coulombic efficiency of the active electrode material may be greater than 97.9% or greater than 98.8%. Providing a material with a suitably high initial coulombic efficiency may be advantageous as it may result in improved performance in electrochemical devices containing niobium mixed oxides.
[0071] The active electrode material of the first aspect of the present invention comprises a niobium mixed oxide and at least one other component, optionally selected from a binder, a solvent, a conductive additive, a different active electrode material, and mixtures thereof. Such a composition is useful for making an electrode, for example an anode for a lithium-ion battery. Preferably, the different active electrode material is selected from a different niobium mixed oxide having a composition defined by the first aspect, a lithium titanium oxide, a niobium oxide, and mixtures thereof. Alternatively, the active electrode material may consist of a niobium mixed oxide.
[0072] The active electrode material may comprise a mixed niobium oxide and a lithium titanium oxide, preferably a mixture of a mixed niobium oxide and a lithium titanium oxide.
[0073] The lithium titanium oxide preferably has a spinel or ramsdellite crystal structure, for example as determined by X-ray diffraction. An example of a lithium titanium oxide having a spinel crystal structure is Li 4 Ti 5 O 12 An example of a lithium titanium oxide with the ramsdellite crystal structure is Li 2 Ti 3 O 7 These materials have been shown to have excellent properties for use as active electrode materials. Thus, lithium titanium oxide is Li 4 Ti 5 O 12 and / or Li 2 Ti 3 O 7 The lithium titanium oxide may have a crystal structure as determined by X-ray diffraction corresponding to Li 4 Ti 5 O 12 , Li 2 Ti 3 O 7 and mixtures thereof.
[0074] The lithium titanium oxide may be doped with additional cations or anions. The lithium titanium oxide may be oxygen deficient. The lithium titanium oxide may include a coating, optionally selected from carbon, polymer, metal, metal oxide, metalloid, phosphate, and fluoride.
[0075] The lithium titanium oxide can be synthesized by conventional ceramic techniques, such as solid-state or sol-gel synthesis, or it can be obtained from a commercial supplier.
[0076] The lithium titanium oxide is preferably granular. The lithium titanium oxide has a diameter of D in the range of 0.1 to 50 μm, or 0.25 to 20 μm, or 0.5 to 15 μm. 50 The lithium titanium oxide may have a particle size of at least 0.01 μm, or at least 0.1 μm, or at least 0.5 μm. 10 The lithium titanium oxide may have a particle size of 100 μm or less, 50 μm or less, or 25 μm or less. 90 D 90 Maintaining the particle size in this range improves the packing of the lithium titanium oxide particles in admixture with the niobium mixed oxide particles.
[0077] Lithium titanium oxide is usually used in battery anodes with small particle size due to the low electronic conductivity of the material. In contrast, niobium mixed oxide as defined herein typically has a higher lithium ion diffusion coefficient than lithium titanium oxide and can be used with a larger particle size. Advantageously, in the composition, lithium titanium oxide can have a smaller particle size than niobium mixed oxide, e.g., the D of niobium mixed oxide. 50 D of lithium titanium oxide versus particle size 50The particle size ratio of the smaller lithium titanium oxide particles is in the range of 0.01:1 to 0.9:1, or 0.1:1 to 0.7:1, in this way the smaller lithium titanium oxide particles can be accommodated in the voids between the larger niobium mixed oxide particles, increasing the packing efficiency of the composition.
[0078] Lithium titanium oxide is 0.1 to 100m 2 / g, or 1 to 50m 2 / g, or 3 to 30m 2 The nanoparticles may have a BET surface area in the range of 1 / g.
[0079] The mass ratio of lithium titanium oxide to niobium mixed oxide may be in the range of 0.5:99.5 to 99.5:0.5, preferably in the range of 2:98 to 98:2. In one embodiment, the active electrode material comprises a higher proportion of lithium titanium oxide than niobium mixed oxide, for example a mass ratio of at least 2:1, at least 5:1, or at least 8:1. Advantageously, this allows the niobium mixed oxide to be gradually introduced into existing electrodes based on lithium titanium oxide without the need to significantly change the manufacturing technology, providing an efficient way to improve the properties of existing electrodes. In another embodiment, the active electrode material comprises a higher proportion of niobium mixed oxide than lithium titanium oxide, for example a mass ratio of lithium titanium oxide to niobium mixed oxide of less than 1:2, or less than 1:5, or less than 1:8. Advantageously, this allows the cost of the active electrode material to be reduced by replacing part of the niobium mixed oxide with lithium titanium oxide.
[0080] The active electrode material can include niobium mixed oxides and niobium oxides. Niobium oxides include Nb 12 O 29 , NbO 2 , NbO, and Nb 2 O 5 Preferably, the niobium oxide is selected from Nb 2 O 5 It is.
[0081] Niobium oxide is, for example, a crystalline structure of an oxide composed of Nb and O, for example, Nb 12 O 29 , NbO 2 , NbO, and Nb 2 O 5 The niobium oxide may be doped with additional cations or anions, provided that it corresponds to: The niobium oxide may be oxygen deficient. The niobium oxide may include a coating, optionally selected from carbon, polymer, metal, metal oxide, metalloid, phosphate, and fluoride.
[0082] Niobium oxide is Nb as determined by X-ray diffraction. 12 O 29 , NbO 2 , NbO, or Nb 2 O 5 For example, niobium oxide can have the crystal structure of orthorhombic Nb 2 O 5 Crystal structure of monoclinic Nb 2 O 5 Preferably, the niobium oxide has a monoclinic Nb 2 O 5 and most preferably H-Nb 2 O 5 It has the crystal structure of Nb 2 O 5 Further information regarding the crystal structure can be found in Griffith et al., J. Am. Chem. Soc. 2016, 138, 28, 8888-8899.
[0083] Niobium oxide can be synthesized by conventional ceramic techniques, such as solid state or sol-gel synthesis, or it can be obtained from commercial suppliers.
[0084] The niobium oxide is preferably in the form of particles. The niobium oxide has a diameter of D in the range of 0.1 to 100 μm, or 0.5 to 50 μm, or 1 to 20 μm. 50The niobium oxide may have a particle size of at least 0.05 μm, or at least 0.5 μm, or at least 1 μm. 10 The niobium oxide may have a particle size of 100 μm or less, 50 μm or less, or 25 μm or less. 90 D 90 Maintaining the particle size in this range improves the packing of the niobium oxide particles in the mixture with the niobium mixed oxide particles.
[0085] Niobium oxide is 0.1 to 100m 2 / g, or 1 to 50m 2 / g, or a BET surface area in the range of 1 to 20 m2 / g.
[0086] The mass ratio of niobium oxide to niobium mixed oxide may be in the range of 0.5:99.5 to 99.5:0.5, or in the range of 2:98 to 98:2, or preferably in the range of 15:85 to 35:55.
[0087] The invention also provides an electrode comprising the active electrode material of the first aspect of the invention in electrical contact with a current collector. The electrode may form part of a cell. The electrode may form the anode as part of a metal-ion battery, optionally a lithium-ion battery.
[0088] The present invention also provides the use of the active electrode material of the first aspect of the invention in an anode for a metal-ion battery, optionally where the metal-ion battery is a lithium-ion battery.
[0089] A further embodiment of the invention is an electrochemical device comprising an anode, a cathode, and an electrolyte disposed between the anode and the cathode, the anode comprising an active electrode material according to the first aspect of the invention, and optionally the electrochemical device is a metal ion battery such as a lithium ion battery or a sodium ion battery. Preferably, the electrochemical device is a lithium ion battery having a reversible anode active material specific capacity of greater than 190 mAh / g at 20 mA / g, such that the battery can be charged and discharged at current densities relative to the anode active material of 200 mA / g or greater, or 1000 mA / g or greater, or 2000 mA / g or greater, or 4000 mA / g or greater, while retaining 70% or more of the initial cell capacity at 20 mA / g. It has been found that the use of the active electrode material of the first aspect of the invention can enable the fabrication of lithium ion batteries having this combination of properties, representing lithium ion batteries particularly suitable for use in applications where high charge and discharge current densities are desired. In particular, the examples show that the active electrode material according to the first aspect of the invention has improved electronic conductivity and improved delithiation voltage at high C-rates.
[0090] Niobium mixed oxides can be synthesized by conventional ceramic techniques. For example, the material is made by one or more of solid synthesis or sol-gel synthesis. The material can be further synthesized by one or more of commonly used alternative techniques, such as hydrothermal or microwave hydrothermal synthesis, solvothermal or microwave solvothermal synthesis, co-precipitation synthesis, spark or microwave plasma synthesis, combustion synthesis, electrospinning, and mechanical alloying.
[0091] A second aspect of the present invention provides a method for producing a niobium mixed oxide as defined according to the first aspect of the present invention, the method comprising the steps of obtaining one or more precursor materials, mixing the precursor materials to form a precursor material mixture, and heat treating the precursor material mixture at a temperature in the range of 400°C to 1350°C or 800 to 1350°C, thereby obtaining the niobium mixed oxide.
[0092] To obtain a niobium mixed oxide comprising element Q, the method may further comprise the steps of mixing the niobium mixed oxide with a precursor comprising element Q to obtain a further precursor substance mixture, and optionally heat treating the further precursor substance mixture under reducing conditions in a temperature range of 300-1200°C or 800-1200°C, thereby obtaining a niobium mixed oxide comprising element Q.
[0093] For example, to obtain a niobium mixed oxide containing N as element Q, the method includes the steps of mixing the mixed niobium oxide with a precursor containing N (e.g., melamine) to obtain a further precursor material mixture, and reducing the further precursor material mixture under reducing conditions (e.g., N 2 The method may further include a step of heat treating the niobium oxide powder at a temperature in the range of 300 to 1200° C. in a room temperature atmosphere (at 200° C.) to obtain a mixed niobium oxide containing N as the element Q.
[0094] For example, to obtain a niobium mixed oxide containing F as the element Q, the method may further comprise the steps of mixing the mixed niobium oxide with a precursor containing F (e.g., polyvinylidene fluoride) to obtain a further precursor material mixture, and heat treating the further precursor material mixture under oxidizing conditions (e.g., in air) at a temperature range of 300-1200°C, thereby obtaining a mixed niobium oxide containing F as the element Q.
[0095] The method may comprise the further step of heat treating the niobium mixed oxide or the niobium mixed oxide containing element Q in the temperature range of 400-1350°C or 800-1350°C under reducing conditions, thereby inducing oxygen vacancies in the niobium mixed oxide. The induced oxygen vacancies may be in addition to oxygen vacancies already present in the niobium mixed oxide, for example by secondary valence substitution of M2 and / or Nb with M1 and / or M3. Alternatively, the induced oxygen vacancies may be new oxygen vacancies, for example when M1 and M3 have the same valence as M2 and Nb. The presence of induced oxygen vacancies provides the advantages discussed herein.
[0096] The precursor material may include one or more metal oxides, metal hydroxides, metal salts, or ammonium. For example, the precursor material may include one or more metal oxides or metal salts of different oxidation states and / or different crystal structures. Examples of suitable precursor materials include Nb 2 O 5 , Nb(OH) 5 , Niobic acid, NbO, Ammonium oxalate niobate, NH 4 H 2 PO 4 , (NH 4 ) 2 PO 4 , (NH 4 ) 3 PO 4 , P 2 O 5 , H 3 PO 3 , Ta 2 O 5 , WO 3 , ZrO 2 , TiO 2 , MoO 3 , V 2 O 5 , ZrO 2 , CuO, ZnO, Al 2 O 3 , K 2 O, KOH, CaO, GeO 2 , Ga 2 O 3 , SnO 2 , CoO, Co 2 O 3 , Fe 2 O 3 , Fe 3 O 4 , MnO, MnO 2 , NiO, Ni 2 O 3 , H 3 BO 3 , ZnO, and MgO. The precursor material may not include a metal oxide or may include an ion source other than an oxide. For example, the precursor material may include a metal salt (e.g., NO 3 - , S.O. 3 -) or other compounds (e.g., oxalates, carbonates). To replace the oxygen anions with other electronegative anions Q, precursors containing element Q may include one or more organic compounds, polymers, inorganic salts, organic salts, gases, or ammonium salts. Examples of suitable precursor materials containing element Q include melamine, NH 4 HCO 3 , N.H. 3 , N.H. 4 F 、 PVDF, PTFE, NH 4 Cl, NH 4 Br, N.H. 4 I, Br 2 , Cl 2 , I 2 , ammonium oxychloride amide, and hexamethylenetetramine.
[0097] Some or all of the precursor materials may be particulate materials. If they are particulate materials, then preferably they have a diameter of less than 20 μm, for example a D of 10 nm to 20 μm. 50 Obtaining particulate material with such a particle size can help promote more intimate mixing of the precursor materials, thereby resulting in a more efficient solid-state reaction during the heat treatment step. However, it is not essential that the precursor materials have an initial particle size of less than 20 μm, since the particle size of one or more precursor materials can be mechanically reduced during the step of mixing the precursor materials to form a precursor material mixture.
[0098] The step of mixing the precursor materials to form the precursor material mixture and / or the further precursor material mixture may be carried out by a process selected from, but not limited to, dry or wet planetary ball milling, rolling ball milling, high energy ball milling, high shear milling, air jet milling, steam jet milling, planetary mixing, and / or impact milling. The force used for mixing / milling may depend on the morphology of the precursor materials. For example, if some or all of the precursor materials are mixed into larger particle sizes (e.g., D greater than 20 μm), the mixing / milling force may be increased by 100%. 50When the precursor mixture has a particle size of 20 μm or less, the milling force can be selected to reduce the particle size of the precursor material such that the particle size of the precursor mixture is reduced to 20 μm or less in diameter. A particle size of 20 μm or less of the precursor mixture can more efficiently promote solid-state reaction of the precursor material of the precursor mixture during the heat treatment step. Solid-state synthesis can also be performed on pellets formed at high pressure (greater than 10 MPa) from the precursor powder.
[0099] The step of heat treating the precursor material mixture and / or the further precursor material mixture may be carried out for a time period between 1 hour and 24 hours, more preferably between 3 hours and 18 hours. For example, the heat treating step may be carried out for 1 hour or more, 2 hours or more, 3 hours or more, 6 hours or more, or 12 hours or more. The heat treating step may be carried out for 24 hours or less, 18 hours or less, 16 hours or less, or 12 hours or less.
[0100] The step of heat treating the precursor material mixture can be carried out in a gas atmosphere, preferably air. Suitable gas atmospheres include air, N 2 , Ar, He, CO 2 , C.O., O 2 , H 2 , N.H. 3 and mixtures thereof. The gas atmosphere may be a reducing atmosphere. If it is desired to create an oxygen deficient material, preferably the step of heat treating the precursor material mixture is carried out in an inert or reducing atmosphere.
[0101] The step of heat treating the further precursor material mixture is carried out under reducing conditions, including under an inert gas such as nitrogen, helium, argon, or under a mixture of an inert gas and hydrogen, or under vacuum. Preferably, the step of heat treating the further precursor material mixture comprises heating under an inert gas.
[0102] The further step of heat treating the niobium mixed oxide and / or the niobium mixed oxide containing element Q under reducing conditions can be carried out for a time period of 0.5 to 24 hours, more preferably 2 to 18 hours. For example, the heat treatment step may be carried out for 0.5 hours or more, 1 hour or more, 3 hours or more, 6 hours or more, or 12 hours or more. The heat treatment of the further step can be carried out for 24 hours or less, 18 hours or less, 16 hours or less, or 12 hours or less. Reducing conditions include under an inert gas such as nitrogen, helium, argon, or under a mixture of an inert gas and hydrogen, or under a vacuum. Preferably, the heating under reducing conditions includes heating under an inert gas.
[0103] In some methods, it may be beneficial to carry out a two-step heat treatment. For example, the precursor material mixture and / or the further precursor material mixture may be heated at a first temperature for a first time, followed by heating at a second temperature for a second time. Preferably, the second temperature is higher than the first temperature. Such a two-step heat treatment may assist the solid-state reaction to form the desired crystal structure. This may be carried out consecutively or with an intermediate regrinding step.
[0104] The method may include one or more post-treatment steps after the formation of the niobium mixed oxide. In some cases, the method may include a post-treatment step of heat treating the niobium mixed oxide, sometimes referred to as "annealing". This post-treatment heat treatment step may be performed in a different gas atmosphere than the step of heat treating the precursor material mixture to form the niobium mixed oxide. The post-treatment heat treatment step may be performed in an inert gas atmosphere or a reducing gas atmosphere. Such a post-treatment heat treatment step may be performed at a temperature above 500°C, for example at about 900°C. The inclusion of a post-treatment heat treatment step may be beneficial, for example, to form deficiencies or defects in the niobium mixed oxide, such as to induce oxygen deficiencies, or to perform anion exchange, for example N exchange of O anions, in the formed niobium mixed oxide.
[0105] The method may include milling and / or classifying the niobium mixed oxide (e.g., impact milling, jet milling, steam jet milling, high energy milling, high shear milling, pin milling, air classification, wheel classification, sieving) to obtain a material having any of the particle size parameters listed above.
[0106] There may be a step of coating the niobium mixed oxide with carbon to improve the electrical conductivity of the surface and prevent reaction with the electrolyte. This typically consists of combining the niobium mixed oxide with a carbon precursor to form an intermediate material, which may include milling, preferably high-energy milling. Alternatively or additionally, the step may include mixing the niobium mixed oxide with the carbon precursor in a solvent such as water, ethanol or THF. These represent an efficient way to ensure uniform mixing of the niobium mixed oxide with the carbon precursor.
[0107] polyaromatic sp 2 It has been found that a carbon-containing carbon precursor provides a particularly beneficial carbon coating on the niobium mixed oxide of the first aspect of the invention. Thus, the method for producing a niobium mixed oxide comprises the steps of: reacting a niobium mixed oxide or a niobium mixed oxide containing an element Q with a polyaromatic sp 2 It may further include combining with a carbon precursor comprising carbon to form an intermediate material, and heating the intermediate material under reducing conditions to pyrolyze the carbon precursor, form a carbon coating on the niobium mixed oxide, and induce oxygen vacancies in the niobium mixed oxide.
[0108] The intermediate material may contain the carbon precursor in an amount of up to 25 wt%, or 0.1-15 wt%, or 0.2-8 wt%, based on the total weight of the niobium mixed oxide and the carbon precursor. The carbon coating on the niobium mixed oxide may be present in an amount of up to 10 wt%, or 0.05-5 wt%, or 0.1-3 wt%, based on the total weight of the niobium mixed oxide. These amounts of carbon precursor and / or carbon coating provide a good balance between improving the electronic conductivity due to the carbon coating without excessively reducing the capacity of the niobium mixed oxide by excessively reducing the proportion of the niobium mixed oxide. The mass of the carbon precursor lost during pyrolysis may range from 30 to 70 wt%.
[0109] The step of heating the intermediate under reducing conditions may be carried out at a temperature ranging from 400 to 1,200° C., or from 500 to 1,100° C., or from 600 to 900° C. The step of heating the intermediate under reducing conditions may be carried out for a duration ranging from 30 minutes to 12 hours, from 1 to 9 hours, or from 2 to 6 hours.
[0110] The step of heating the intermediate under reducing conditions can be carried out under an inert gas such as nitrogen, helium, argon, or a mixture of an inert gas and hydrogen, or can be carried out under vacuum.
[0111] polyaromatic sp 2 The carbon-containing carbon precursor may be selected from pitch carbon, graphene oxide, graphene, and mixtures thereof. Possibly polyaromatic sp 2 The carbon-containing carbon precursor may be selected from pitch carbon, graphene oxide, and mixtures thereof. Most preferably, the polyaromatic sp 2 The carbon-containing carbon precursor is selected from pitch carbon, which may be selected from coal tar pitch, petroleum pitch, mesophase pitch, wood tar pitch, isotropic pitch, bitumen, and mixtures thereof.
[0112] Pitch carbon is a mixture of aromatic hydrocarbons of different molecular weights. Pitch carbon is a low-cost by-product from petroleum refineries and is widely available. The use of pitch carbon is advantageous because pitch has a low oxygen content. Thus, in combination with heating the intermediate under reducing conditions, the use of pitch favors the formation of oxygen vacancies in the niobium mixed oxide.
[0113] Other carbon precursors usually contain significant amounts of oxygen. For example, carbohydrates such as glucose and sucrose are commonly used as carbon precursors. These are represented by the empirical formula C m (H 2 O) n and thus contains a significant amount of covalently bonded oxygen (e.g., sucrose has the formula C 12 H 22 O 11 (having about 42 wt. % oxygen). It is believed that pyrolysis of a carbon precursor containing a significant amount of oxygen prevents or inhibits the reduction of the niobium mixed oxide or even leads to oxidation, meaning that oxygen vacancies may not be induced in the niobium mixed oxide. Thus, the carbon precursor may have an oxygen content of less than 10 wt. %, preferably less than 5 wt. %.
[0114] The carbon precursor is sp 3 It may be substantially free of carbon. For example, the carbon precursor may contain less than 10 wt.% sp 3 Carbon source, preferably less than 5 wt% sp 3 The carbohydrate may include a carbon source. 3 A carbon source. The carbon precursor may not contain carbohydrates. Some carbon precursors used in the present invention are sp 3 It is understood that it may contain carbon impurities, for example up to 3 wt% carbon.
[0115] The niobium mixed oxide of the first aspect of the present invention may include a carbon coating. The carbon coating is a polyaromatic sp 2 It is preferred that it contains carbon. 2Hybridization is largely preserved during pyrolysis, so polyaromatic sp 2 Such coatings are formed by pyrolyzing a carbon-containing carbon precursor, preferably under reducing conditions. Typically, polyaromatic sp 2 The pyrolysis of the carbon precursor produces sp 2 This leads to an increase in the size of the aromatic carbon domains. Thus, polyaromatic sp 2 The presence of a carbon coating containing polyaromatic sp can be established by knowing the precursors used to make the coating. 2 It can be defined as a carbon coating formed from the pyrolysis of a carbon-containing carbon precursor. Preferably, the carbon coating is derived from pitch carbon.
[0116] polycyclic aromatic sp 2 The presence of carbon-containing carbon coatings can also be established by conventional spectroscopic techniques. For example, Raman spectroscopy detects characteristic peaks (1,000–3,500 cm -1 (most prevalent in the sp region) which can be used to distinguish the various forms of carbon present. 3 For highly crystalline samples of carbon (such as diamond), the peak is approximately 1332 cm -1 A narrow characteristic peak is obtained at . Polyaromatic sp 2 Carbon usually exhibits characteristic D, G, and 2D peaks. The relative intensities of the D and G peaks (I D / I G ) is sp 2 Carbon vs sp 3 Niobium mixed oxides, when viewed by Raman spectroscopy, have I values in the ranges of 0.85–1.15, or 0.90–1.10, or 0.95–1.05. D / I G The ratio may be:
[0117] X-ray diffraction can also be used to obtain information about the type of carbon coating, for example the XRD pattern of a carbon coated niobium mixed oxide can be compared to the XRD pattern of an uncoated niobium mixed oxide and / or the XRD pattern of a pyrolyzed sample of the carbon precursor used to apply the carbon coating.
[0118] The carbon coating may be semi-crystalline, for example, capable of obtaining a niobium mixed oxide XRD pattern peak centered at about 26° 2θ with a width (full width at half maximum) of at least 0.20°, or at least 0.25°, or at least 0.30°. EXAMPLES
[0119] Niobium mixed oxides were synthesized by a solid-state route. In the first step, the precursor material (Nb 2 O 5 , GeO 2 , ZnO, TiO 2 , Cr 2 O 3 , Al 2 O 3 , Fe 2 O 3 , ZrO 2 , and CuO) with a D of less than 20 μm 50 The materials were mixed in stoichiometric ratios (50 g total) and milled to a uniform powder mixture at 20,000 rpm in an impact mill. The resulting powders were then cooled in alumina crucibles in a muffle furnace at 37° C. for 0.5–24 h in air at 37° C. 1 = 600–1350 °C to obtain the desired Wadsley-Roth phase. Selected samples (9–11) were removed from the furnace after heat treatment and crushed by impact milling at 20,000 rpm, after which the heat treatment was repeated under similar conditions. Specifically, the precursor mixture was heated at a ramp rate of 5° / min to a temperature below 800 °C, then at a ramp rate of 1° / min to the maximum temperature of the holding period. In some cases, T 2 N = 600 to 1350 °C 2An additional heat treatment step was also applied for 0.5–12 h under atmospheric conditions. 2a / T 2b = 300-1200°C for 0.5-12 hours, N 2 or there was an additional milling / mixing step with the precursor (PVDF with a mass ratio of 1:10 for F, C with a mass ratio of 1:3 to the base material if N was required) before heat treatment in 1 or 2 steps in air atmosphere. 3 H 6 N 6 can be used).
[0120] If necessary, a final deagglomeration step was used by impact milling or jet milling to adjust the particle size distribution to the desired size. Specifically, the material was deagglomerated by impact milling at 20,000 RPM for 10 seconds. The particle size distribution was obtained with a Horiba dry powder laser diffraction particle analyzer. The air pressure was kept at 0.3 MPa. The results are shown in Table 1. [Table 1]
[0121] Material characterization The phase purity of the samples was analyzed using a Rigaku Miniflex powder X-ray diffractometer over the 2θ range (10–70°) at a scan rate of 1° / min.
[0122] Figure 1 shows the measured XRD diffraction patterns for samples 1-4, and Figure 2 shows the measured XRD diffraction patterns for samples 5-12. The diffraction patterns have peaks at the same positions (with some shifts due to crystallographic modifications, up to about 0.2°) and are consistent with the crystallographic database entry JCPDS 28-1478. The particular samples have the same Wadsley-Roth block structure (Zn 2 Nb 34 O 87) are found to be mixed phases of monoclinic (JCPDS 28-1478, ref. a) and orthorhombic (PDF card, 04-021-7859, ref. b) crystal structures and refined to this mixture. There is no amorphous background noise and the peaks are sharp and intense. This is because all samples are crystalline, with crystallite sizes of 45-55 nm according to the Scherrer formula and a crystal structure of Zn. 2 Nb 34 O 87 This confirms the existence of the Wadsley-Roth crystal structure. [Table 2]
[0123] Electrochemical characterization The charge rate of a lithium-ion battery is usually expressed as a "C-rate". A 1C charge rate means a charging current such that the cell is fully charged in 1 hour, while a 10C charge means that the cell is fully charged in 1 / 10 of an hour (6 minutes). The C-rate here is defined from the reversible capacity seen by the anode within the voltage limits imposed by the second delithiation cycle, i.e., 1.0 mAh cm within the voltage limits of 1.1 to 3.0 V. -2 For an anode with a capacity of 1.0 mA cm, the 1C rate is 1.0 mA cm. -2 For the typical MNO materials described herein, this corresponds to an applied current density of about 200 mA / g active material.
[0124] Electrochemical testing was performed in half coin cells (CR2032 size) for analysis. In the half coin test, active materials are tested at the electrode against a Li metal electrode to evaluate the basic capabilities of the active material. In the following examples, the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black (Super P) acting as a conductive additive, and poly(vinyl difluoride) (PVDF) binder and mixed in a laboratory scale centrifugal planetary mixer into a slurry. The non-NMP composition of the slurry was 92 wt% active material, 3 wt% conductive additive, and 5 wt% binder. The slurry was doctor blade coated onto an Al foil current collector at the desired coating weight of 69-75 gm. 2 The electrodes were then coated with 2.6–2.9 g cm -3 The electrodes were then die-cut to the desired size and packed in a steel coin cell case with a separator (Celgard porous PP / PE), Li metal, and electrolyte (1.3 M LiPF in EC / DEC). 6 ) and sealed under pressure. The cells were then cycled at 23°C at a low current rate (C / 10) between 1.1 and 3.0V for two full cycles of lithiation and delithiation. The cells were then tested for performance at increasing current densities. During these tests, the cells were asymmetrically cycled at 23°C, slowing the lithiation (C / 5), and then increasing the rate of delithiation (e.g., 1C, 5C, 10C) to maintain capacity and to a nominal voltage of 5C. The nominal voltage for Li / Li+ was calculated from the integral of the V / Q curve divided by the total capacity at 5C during delithiation. No constant voltage step was used. Data was averaged from five cells prepared from the same electrode coating, with errors shown from the standard deviation. Thus, the data represents a robust study showing the improvements achieved by the material according to the invention compared to conventional materials. These data are shown in Tables 4 and 5.
[0125] Cell resistance is calculated from the direct current internal resistance (DCIR) of a half coin cell. In a typical measurement, the cell is lithiated to 100% state of charge (SOC), then delithiated at a rate of C / 10 to 50% SOC, then after a 0.5 hour rest, a 5C delithiation pulse is applied for 10 seconds, followed by another 0.5 hour rest. DCIR is then calculated from V=IR, using the voltage just before the peak from the pulse and the maximum voltage measured during the pulse.
[0126] The electrical resistivity of the electrode coatings was evaluated individually by a four-point probe method using an Ossila instrument (T2001A3-UK) at 23 °C. A slurry was formed (the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black acting as a conductive additive, and poly(vinyl difluoride) (PVDF) binder and mixed in a laboratory-scale centrifugal planetary mixer into a slurry, the non-NMP composition of the slurry was 80 w.%, the active material was 10 w.%, and the conductive additive was 10 w.% binder). The slurry was then applied to a dielectric Mylar film at 1 mg / cm. 2 The electrodes were coated at a load of 0.1 μm. Disks of the electrode size were then punched out and the resistance of the coated films was measured using a four-point probe. The sheet resistance (Ω / square) results are summarized in Table 3. The errors are based on the standard deviation of triplicate measurements.
[0127] Also, homogeneous, smooth coatings on both Cu and Al current collector foils, free of visible defects or agglomerates, can be prepared as described above for those samples using a centrifugal planetary mixer with compositions up to 94 wt% active material, 4 wt% conductive additive, and 2 wt% binder. These can be prepared with both PVDF (i.e., NMP-based) and CMC:SBR-based (i.e., aqueous) binder systems. Coatings can be produced at 80 °C for PVDF and 35-40% porosity for CMC:SBR, with 1.0 to 5.0 mAh cm. -2The materials can be calendered at 50°C under a load of 1000 MPa, which is important for demonstrating the viability of these materials in both high energy and high power applications, with high active material content. [Table 3] [Table 4] [Table 5] [Table 6]
[0128] Consideration Niobium mixed oxide sample 1 * Ge 4+ Cation Zn substituted with 2+ The cation substitution approach in sample 3 was focused on. Samples 5-8 were modified by the cation Zn over a wide range of variables a and b. 2+ is a cation C r3+ and cation Nb 5+ is the cation Ti 4+ Sample 10 is replaced by Nb 5+ Fe 3+ Sample 11 is substituted with Zn 2+ Al 3+ Sample 12 is replaced by Cu. 2 Nb 34 O 87 Based on the cation Cu 2+ is Cr 3+ and cation Nb 5+ is the cation Ti 4+ has been replaced with 。 The increase in valence is due to partial oxygen excess (i.e., c<0) and / or Nb 5+The reduction in vacancies can be compensated for by the formation of oxygen vacancies (i.e., c>0). These modifications can be achieved by a combination of (a) altered ionic radius, (b) altered valence, and (c) altered voltage in sample 1. * The altered ionic radius is expected to provide benefits over the basic crystal structure of the modified ionic radius. The altered ionic radius, due to altered unit cell size and local distortion of the crystal structure, may result in beneficial changes in electrochemical performance, altering the available lithiation sites or lithiation pathways and potentially improving coulombic efficiency, capacity, high rate capability, and lifetime. The altered valence makes intermediate energy levels available for charge carriers, thus significantly improving the electrical conductivity of the material. These effects are consistent with the improved conductivity of the modified sample versus sample 1. * This is shown by the low resistivity seen in Table 3, and by the improvements in specific capacity, coulombic efficiency, delithiation voltage at 5C, and capacity retention at 1C, 5C, and 10C seen in Tables 4-6. These are important results demonstrating the utility of the modified niobium mixed oxides according to the present invention for use in high power Li-ion cells designed for high rate charge / discharge.
[0129] Table 2 shows the changes in unit cell parameters observed upon cation exchange, which are seen due to changes in the ionic radii and electronic structures of these materials.
[0130] It is expected that similar benefits will be seen with the cation exchange approach described for this material for use in Li-ion cells.
[0131] Niobium mixed oxide sample 1 * is modified by the introduction of induced oxygen deficiencies by heat treatment in an inert or reducing atmosphere to give sample 2. By treating the "base" oxide in an inert or reducing atmosphere at high temperature, it is partially reduced, which can be maintained when returned to room temperature and exposed to an air atmosphere. This is accompanied by a clear color change, e.g. sample 2 is grey / black whereas sample 1 is white. *is white in color. This color change indicates a significant change in the electronic structure of the material, allowing it to interact with different energies (i.e. wavelengths) of visible light due to a reduction in the band gap. This is reflected in sample 2, which shows an improvement in the delithiation voltage at a rate of 5C corresponding to a reduction in the polarization level of the cell.
[0132] The induced oxygen deficiency leads to defects in the crystal structure, for example where oxygen anions are removed, which in turn reduces the overall redox state of the cations. This provides additional energy states that significantly improve the electrical conductivity of the material, and shifts the band gap energy as indicated by the color change. This is the case for Sample 2 vs Sample 1. * This is indicated by the lower resistivity seen in Table 3 for c > 4.35. If the induced oxygen deficiency is present in excess of 5 at. %, the stability of the crystal structure may be reduced.
[0133] Niobium mixed oxide sample 1 * is anion substitution (F - By O 2- (substitution of ) to obtain sample 4. An improvement in specific capacity was observed (Tables 4 and 5).
[0134] Similar benefits are expected to be seen in any of the described niobium mixed oxides utilizing any combination of M1, M2, M3, Q, a, b, c, and d within the described limitations for use in Li-ion cells.
[0135] Mixture with LTO The modified niobium mixed oxides were tested as active electrode materials in combination with commercially available materials to demonstrate the utility of the modified niobium mixed oxides for incorporation into and improvement of existing battery technology.
[0136] Commercial grade LTO (Li 4 Ti 5 O 12) was purchased from Targray Technology International Inc. with the properties outlined in Table E1 (Sample E1). The Wadsley-Roth material was synthesized in-house by a solid-state route. In the first step, the precursor material (Nb 2 O 5 , Cr 2 O 3 , ZnO, and TiO 2 ) were mixed in a stoichiometric ratio (total of 200 g) and ball milled at 550 rpm with a powder to ball ratio of 10:1 for 3 h. The resulting powder was heated in an alumina crucible in a muffle furnace at T 1 = 1100 °C to obtain the desired Wadsley-Roth phase.
[0137] The active electrode material blend of MNO and LTO was obtained by low to high energy powder mixing / blending techniques such as multi-directional rotary blending, single-axis rotary V-blending, planetary blending, centrifugal planetary blending, high shear blending, and other typical mixing / blending techniques. In this case, mixing was accomplished using a centrifugal planetary mixer with 5 g batches of materials mixed at 2000 rpm for 3 minutes, 10 times. [Table 7]
[0138] Material characterization The phase purity of the samples was analyzed using a Rigaku Miniflex powder X-ray diffractometer at a scan rate of 1° / min in the 2θ range (20–70°). The diffraction pattern of sample E1 was Li 4 Ti 5 O 12 The diffraction pattern of sample E2 matches the JCPDS crystallography database entry JCPDS49-0207, which corresponds to a spinel crystal structure of Zn. There is no amorphous background noise and the peaks are sharp and intense. This means that the sample is crystalline, with a crystallite size of 43 ± 7 nm according to the Scherrer formula. The diffraction pattern of sample E2 matches the desired Wadsley-Roth crystal structure Zn. 2 Nb34 O 87 Confirm the presence of . There is no amorphous background noise and the peak is sharp and intense, which means the sample is phase pure and crystalline with a crystallite size of 49±6 nm according to the Scherrer equation.
[0139] The particle size distribution was obtained using a Horiba dry powder laser diffraction particle analyzer. The air pressure was kept at 0.3 MPa. The results are shown in Table E1. 2 The BET surface area analysis was performed using the method shown in Table E1.
[0140] Electrochemical characterization Electrochemical testing was performed in half coin cells (CR2032 size) for analysis. There are some differences in the test methods used in samples 1-12 above, meaning that the results may not be directly comparable. In half coin testing, materials are tested on an electrode against a Li metal electrode to evaluate the basic capabilities of the material. In the following examples, the active material composition to be tested was combined with N-methylpyrrolidone (NMP), carbon black to act as a conductive additive, and a poly(vinyl difluoride) (PVDF) binder and mixed in a laboratory scale centrifugal planetary mixer into a slurry. The non-NMP composition of the slurry was 90 wt% active material, 6 wt% conductive additive, and 4 wt% binder. The slurry was doctor blade coated onto an Al foil current collector to the desired coverage of 5.7-6.5 mg cm. -2 The electrodes were then coated with 2.00–3.75 g cm−1 at 80 °C and dried. -3 The electrodes were then calendered to a density of 1000 Å (depending on the density of the material) to achieve a target porosity of 35-40%. The porosity was calculated by dividing the measured electrode density by the weighted average density of each component of the composite electrode coating film. Electrodes were punched to the desired size and packed in a steel coin cell case with the separator (Celgard porous PP / PE), Li metal, and electrolyte (1.3 M LiPF in EC / DEC). 6) and sealed under pressure. It was then cycled at a low current rate (C / 10) between 1.1 and 3.0 V for two full cycles of lithiation and delithiation. The cell's capabilities were then tested at increasing current densities. During the rate tests, the cell was cycled asymmetrically, slowing the lithiation (current densities from C / 5 to C / 20 with a CV step of 1.1 V) followed by increasing the rate of delithiation for the delithiation rate test. All electrochemical tests were performed at 23 o The experiment was carried out in a temperature-controlled environment at C.
[0141] The first cycle efficiency was calculated as the ratio of the delithiation capacity / lithiation capacity of the first cycle at C / 10. The nominal voltage at each C-rate was determined by integrating the voltage-capacity curve and then dividing it by the total capacity.
[0142] To quantify the significance of the differences in the data seen, error calculations were performed and applied to the values of specific capacitance. These errors were calculated based on the microbalance used (±0.1 mg) and the minimum loaded electrode for the 14 mm electrode disk (5.7 mg cm -2 ) was estimated as the maximum possible error. This results in an error of ±1.1%, which is applied to each capacity measurement. Errors in coulombic efficiency, capacity retention, and voltage were assumed to be negligible for the tested cells, since the accuracy of the measuring equipment far exceeds the stated significant figures and the values are independent of the balance error. [Table 8] [Table 9] [Table 10] [Table 11]
[0143] Although the present invention has been described in conjunction with the exemplary embodiments set forth above, many equivalent modifications and variations will become apparent to those skilled in the art given this disclosure. Accordingly, the exemplary embodiments of the present invention described above are considered to be illustrative and not limiting. Various modifications to the described implementations may be made without departing from the spirit and scope of the present invention. For the avoidance of doubt, the theoretical explanations presented herein are presented for the purpose of enhancing the reader's understanding. The inventors do not wish to be bound by any of these theoretical explanations. Any section headings used herein are for organizational purposes only and are not to be construed as limiting the subject matter described. Specific embodiments of the present invention are as follows. [Embodiment 1] An active electrode material containing a niobium mixed oxide, wherein the niobium mixed oxide has a composition M1 a M2 2-a M3 b Nb 34-b O 87-c-d Q d wherein, in the formula, M1 and M2 are different, M1 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof, M2 is Zn or Cu, M3 is selected from Mg, Ca, Sr, Y, La, Ce, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, In, Si, Ge, Sn, Pb, P, Sb, Bi, and mixtures thereof, Q is selected from F, Cl, Br, I, N, S, Se, and mixtures thereof, 0 ≦ a < 1.0, 0 ≦ b ≦ 3.4, -0.5 ≦ c ≦ 4.35, 0 ≦ d ≦ 4.35, one or more of a, b, c, and d are not equivalent to 0, and when a, b, and d are 0, c is greater than 0, the active electrode material. [Embodiment 2] (i) a > 0, and / or (ii) 0 ≦ a ≦ 0.6 and / or (iii) 0 ≦ a ≦ 0.2, the active electrode material according to Embodiment 1. [Embodiment 3] (i) b > 0, and / or (ii) 0 ≦ b ≦ 1.5, and / or (iii) 0 ≦ b ≦ 0.3, or (iv) b = 0, the active electrode material according to any of the preceding embodiments. [Embodiment 4] (i) c ≠ 0, or (ii) 0 ≦ c ≦ 4.35, or (iii) 0 < c ≦ 4.35, the active electrode material according to any of the preceding embodiments. [Embodiment 5] (i) d > 0, and / or (ii) 0 ≦ d ≦ 3.0, and / or (iii) 0 ≦ d ≦ 2.17, or (iv) d = 0, the active electrode material according to any of the preceding embodiments. [Embodiment 6] when at least one of a and b is greater than 0, or when both a and b are greater than 0, the active electrode material according to any of the preceding embodiments. [Embodiment 7] M1 is (i) Mg, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Ge, Sn, P, and mixtures thereof, or (ii) Mg, Ti, Zr, V, Nb, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, B, Al, Si, Ge, P, and mixtures thereof, or (iii) The active electrode material according to any of the preceding aspects, selected from Mg, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, Ge, P, and mixtures thereof. [Aspect 8] The active electrode material according to any of the preceding aspects, wherein M2 is Zn. [Aspect 9] M3 is (i) selected from Mg, Ti, Zr, Hf, V, Ta, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Ga, Si, Sn, P, and mixtures thereof, or (ii) selected from Mg, Ti, Zr, V, Cr, Mo, W, Mn, Fe, Co, Ni, Cu, Zn, Cd, B, Al, Si, P, and mixtures thereof, or (iii) the active electrode material according to any of the preceding aspects, selected from Ti, Zr, V, Cr, Mo, W, Fe, Cu, Zn, Al, P, and mixtures thereof. [Aspect 10] (i) M1 has a six - coordinate ionic radius of 0.1 < r < 1.0 angstroms, and / or (ii) M1 has a six - coordinate ionic radius different from that of six - coordinate M2 2+ and optionally has a six - coordinate ionic radius smaller than that of six - coordinate M2 2+ and / or (iii) M1 has a six - coordinate ionic radius of 0.52 < r < 0.84 angstroms, the active electrode material according to any of the preceding aspects. [Aspect 11] (i) M3 has a six - coordinate ionic radius of 0.1 < r < 1.0 angstroms, and / or (ii) M3 has a six - coordinate ionic radius different from that of six - coordinate Nb 5+ and optionally has a six - coordinate ionic radius larger than that of six - coordinate Nb 5+ and / or (iii) M3 has a six - coordinate ionic radius of 0.54 < r < 0.74 angstroms, the active electrode material according to any of the preceding aspects. [Aspect 12] (i) M1 has a valence equal to or higher than 2 +, optionally has a higher valence, or (ii) M3 has a valence lower than 5 +, or (iii) M1 has a valence equal to or higher than 2 + and M3 has a valence lower than 5 +, the active electrode material according to any of the preceding aspects. [Aspect 13] The active electrode material according to any of the preceding aspects, wherein M1 does not contain Nb and M3 does not contain Zn and / or Cu. [Aspect 14] (i) Q is selected from F, Cl, N, S, and mixtures thereof, or (ii) Q is selected from F, N, and mixtures thereof, or (iii) Q is F, the active electrode material according to any of the preceding aspects. [Aspect 15] M1 is selected from Cr, Al, Ge, and mixtures thereof; M3 is selected from Ti, Zr, Fe, and mixtures thereof, optionally including Ti; 0<a<1.0、 0<b≦1.5、 -0.5≦c≦4.35、 The active electrode material of any of the preceding embodiments, wherein d=0. [Aspect 16] M1 is Cr; M2 is Zn; M3 is selected from Ti, Zr, and mixtures thereof, optionally including Ti; 0.01<a<1.0、 0.01<b<1.0、 -0.5≦c≦2、 The active electrode material of any of the preceding embodiments, wherein d=0. [Aspect 17] The active electrode material of any of the preceding aspects, wherein the niobium mixed oxide is oxygen deficient, and optionally, the niobium mixed oxide induces oxygen deficiency. [Aspect 18] 2. The active electrode material of any of the preceding aspects, wherein the niobium mixed oxide is coated with carbon. [Aspect 19] The carbon coating is a polyaromatic sp 2 20. The active electrode material of embodiment 18, comprising carbon, and optionally the carbon coating is derived from pitch carbon. [Aspect 20] The niobium mixed oxide is in particulate form, and optionally the niobium mixed oxide has a D in the range of 0.1 to 100 μm, or 0.5 to 50 μm, or 1 to 20 μm. 50 The active electrode material of any of the preceding aspects, having a particle size of [Aspect 21] The niobium mixed oxide has a viscosity of 0.1 to 100 m 2 / g, or 0.5 to 50m 2 / g, or 1 to 20m 2 The active electrode material of any preceding embodiment, having a BET surface area in the range of 1 / g. [Aspect 22] 2. The active electrode material of any one of the preceding embodiments, wherein the niobium mixed oxide further comprises Li and / or Na. [Aspect 23] The crystal structure of the niobium mixed oxide, as determined by X-ray diffraction, is 2 Nb 34 O 87 and Cu 2 Nb 34 O 87 or Zn 2 Nb 34 O 87 4. The active electrode material of any of the preceding aspects, wherein the active electrode material corresponds to a crystal structure of [Aspect 24] 13. The active electrode material of any of the preceding aspects, comprising the niobium mixed oxide and at least one other component, optionally wherein the at least one other component is selected from a binder, a solvent, a conductive additive, a different active electrode material, and mixtures thereof. [Aspect 25] 25. The active electrode material of embodiment 24, wherein the at least one other component is a different active electrode material selected from a different niobium mixed oxide having a composition defined by any of the preceding embodiments, a lithium titanium oxide, a niobium oxide, and mixtures thereof. [Aspect 26] 26. An electrode comprising the active electrode material according to any one of aspects 1 to 25 in electrical contact with a current collector. [Aspect 27] 1. An electrochemical device comprising an anode, a cathode, and an electrolyte disposed between the anode and the cathode, The electrochemical device, wherein the anode comprises an active electrode material according to any of aspects 1-25, and optionally the electrochemical device is a lithium ion battery or a sodium ion battery. [Aspect 28] a lithium ion battery having a reversible anode active material specific capacity of greater than 190 mAh / g at 20 mA / g; 28. The electrochemical device of embodiment 27, wherein the battery can be charged and discharged at a current density for the anode active material of 200 mA / g or more, or 1000 mA / g or more, or 2000 mA / g or more, or 4000 mA / g or more, while retaining 70% or more of the initial cell capacity at 20 mA / g. [Aspect 29] A method for producing a niobium mixed oxide as defined in any one of aspects 1 to 23, comprising the steps of: obtaining one or more precursor materials; mixing the precursor materials to form a precursor material mixture; and heat treating the precursor mixture at a temperature range of 400°C to 1350°C or 800°C to 1250°C to obtain the niobium mixed oxide; The method comprising: [Aspect 30] mixing said niobium mixed oxide with a precursor comprising element Q to obtain a further precursor material mixture; and heat treating said further precursor mixture, optionally under reducing conditions, in the temperature range of 300-1200°C or 800-1200°C to obtain said niobium mixed oxide containing element Q. 30. The method of embodiment 29, further comprising: [Aspect 31] 31. The method according to embodiment 29 or 30, comprising the further step of heat treating the niobium mixed oxide or the niobium mixed oxide comprising element Q under reducing conditions in the temperature range of 400 to 1350 °C or 800 to 1250 °C to induce oxygen vacancies in the niobium mixed oxide. [Aspect 32] The niobium mixed oxide or the niobium mixed oxide containing the element Q is subjected to a polyaromatic sp 2 combining with a carbon precursor comprising carbon to form an intermediate material; and heating the intermediate under reducing conditions to pyrolyze the carbon precursor to form a carbon coating on the niobium mixed oxide and induce oxygen vacancies in the niobium mixed oxide. 32. The method of any of embodiments 29 to 31, further comprising:
Claims
1. An active electrode material comprising a niobium mixed oxide, said niobium mixed oxide having the composition M1 a M2 2-a M3 b Nb 34-b O87-c, wherein M1 is selected from Cr, Al, Ge, and mixtures thereof; M2 is Zn or Cu; M3 is selected from Ti, Zr, Fe, and mixtures thereof; 0<a<1.0, 0<b≦1.5, and −0.5≦c≦4.35, The crystal structure of the niobium mixed oxide, as determined by X-ray diffraction, is 2 Nb 34 O 87 and Cu 2 Nb 34 O 87 and The niobium mixed oxide has a D of at least 0.05 μm. 10 and D of 200 μm or less 90 The active electrode material has a particle size of
2. 2. The active electrode material of claim 1 , wherein 0<a≦0.
6.
3. 3. The active electrode material of claim 1 or 2, wherein c≠0.
4. 3. The active electrode material of claim 1 or 2, wherein 0≦c≦4.
35.
5. 3. The active electrode material of claim 1 or 2, wherein 0<c≦4.
35.
6. 6. The active electrode material of claim 1, wherein M2 is Zn.
7. M1 is Cr; M2 is Zn; M3 is selected from Ti, Zr, and mixtures thereof; 0.01<a<1.0, 0.01<b<1.0, 7. The active electrode material according to claim 1, wherein −0.5≦c≦2.
8. 8. The active electrode material according to any one of claims 1 to 7, wherein the niobium mixed oxide is oxygen deficient.
9. 9. An active electrode material according to any one of claims 1 to 8, wherein the niobium mixed oxide is coated with carbon.
10. The carbon coating is a polyaromatic sp 2 10. The active electrode material of claim 9 comprising carbon.
11. 11. The active electrode material according to any one of claims 1 to 10, wherein the niobium mixed oxide further comprises Li and / or Na.
12. The crystal structure of the niobium mixed oxide, as determined by X-ray diffraction, is 2 Nb 34 O 87 12. The active electrode material according to claim 1 , which corresponds to a crystal structure of
13. 13. The active electrode material according to any one of claims 1 to 12, comprising the niobium mixed oxide and at least one other component, the at least one other component being selected from a binder, a solvent, a conductive additive, a different active electrode material, and mixtures thereof.
14. 14. An electrode comprising the active electrode material of any one of claims 1 to 13 in electrical contact with a current collector.
15. 1. An electrochemical device comprising an anode, a cathode, and an electrolyte disposed between the anode and the cathode, 14. The electrochemical device, wherein the anode comprises the active electrode material of any one of claims 1 to 13, and the electrochemical device is a lithium ion battery or a sodium ion battery.
16. a lithium ion battery having a reversible anode active material specific capacity of greater than 190 mAh / g at 20 mA / g; 16. The electrochemical device of claim 15, wherein the battery can be charged and discharged at current densities for the anode active material of 200 mA / g or greater while retaining 70% or more of the initial cell capacity at 20 mA / g.
17. A method for producing a niobium mixed oxide as defined in any one of claims 1 to 12, said method comprising the steps of: Obtaining one or more precursor materials; mixing the precursor materials to form a precursor material mixture; and heat treating the precursor mixture at a temperature in the range of 400° C. to 1350° C. to obtain the niobium mixed oxide; The method comprising:
Citation Information
Patent Citations
Titanium oxide-based compound for electrode and lithium secondary battery using the same
JP2011173761A
Method for forming semiconductor structure
US20200013618A1
Anode Material of Lithium Ion Battery And Non-aqueous Electrolyte Battery
US20200112018A1
Recombinant virus with codon-pair deoptimized region and uses thereof for the treatment of cancer