Resin composition

A resin composition with specific cyanate ester compounds and a curing accelerator addresses the issues of low tensile shear adhesive strength and high water absorption in cyanate ester cured products, enhancing their performance in various applications.

JP7587740B2Active Publication Date: 2024-11-21MITSUBISHI GAS CHEM CO INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020100576
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-10
Publication Date
2024-11-21
Estimated Expiration
2040-06-10

AI Technical Summary

Technical Problem

Low-molecular-weight cyanate esters have excellent handling properties but result in cured products with low tensile shear adhesive strength and high water absorption.

Method used

A resin composition comprising a cyanate ester compound with one cyanato group and another with two or more cyanato groups, along with a curing accelerator, to enhance tensile shear adhesive strength and reduce water absorption.

Benefits of technology

The composition achieves cured products with improved tensile shear adhesive strength and lower water absorption, suitable for applications such as adhesives, insulating materials, paints, and fiber-reinforced composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587740000001
    Figure 0007587740000001
  • Figure 0007587740000002
    Figure 0007587740000002
  • Figure 0007587740000003
    Figure 0007587740000003
Patent Text Reader

Abstract

To provide a resin composition which can provide a cured product having high tensile shearing adhesion strength and a low water absorption rate, and a cured product, a sealing material, an adhesive, an insulating material, a coating material, a prepreg, a laminate and a fiber-reinforced composite material using the resin composition.SOLUTION: A resin composition is provided, containing a cyanate ester compound (A) having only one cyanate group in the molecule, and a cyanate ester compound (B) having two or more cyanate groups in the molecule.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition. [Background technology]

[0002] Cyanate esters are known as thermosetting resins that form triazine rings when cured. The cured products obtained from cyanate esters have excellent properties such as a high glass transition temperature, low dielectric constant and dielectric loss tangent, and excellent electrical insulation and flame retardancy. Therefore, cyanate esters have been widely used as raw materials for electrical and electronic materials, structural composite materials, adhesives, and various other functional polymer materials.

[0003] Under these circumstances, efforts are being made to develop cyanate esters with better properties. For example, Patent Document 1 discloses a novel bifunctional cyanatophenyl-type cyanate ester that is liquid at room temperature and can give a cured product with an excellent low thermal expansion coefficient. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] WO2012 / 057144A1 Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that low molecular weight cyanate esters such as those disclosed in Patent Document 1, although they are liquid at room temperature and easy to handle, have problems such as low tensile shear adhesive strength of the cured product and high water absorption.

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a resin composition capable of giving a cured product having high tensile shear adhesive strength and low water absorption, as well as a cured product, a sealing material, an adhesive, an insulating material, a paint, a prepreg, a laminate, and a fiber-reinforced composite material using the same. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be solved by using two specific cyanate ester compounds, thereby completing the present invention.

[0008] That is, the present invention is as follows. [1] A cyanate ester compound (A) having only one cyanato group in the molecule, and a cyanate ester compound (B) having two or more cyanate groups in the molecule, Resin composition. [2] The cyanate ester compound (A) contains a compound represented by the following formula (I): The resin composition according to [1]. [ka] (In the formula, R 1 represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, an alkenyl group having 2 to 15 carbon atoms, an alkoxy group having 1 to 15 carbon atoms, an aryl group having 6 to 20 carbon atoms, a group in which an alkyl group having 1 to 6 carbon atoms is bonded to an aryl group having 6 to 12 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms; R 1 may have a substituent other than a cyanato group. [3] The cyanate ester compound (B) contains at least one selected from the group consisting of a compound represented by the following formula (II) and a compound represented by the following formula (III): The resin composition according to [1] or [2]. [ka] (In the formula, each Ar1 independently represents an aromatic ring, Each Ra independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, and the alkyl group or aryl group in Ra may have a substituent. a represents the number of cyanato groups bonded to Ar1, and each a is independently an integer of 1 to 3, b represents the number of bonds of Ra to Ar1, and each b independently represents a number obtained by subtracting (a+2) from the number of substitutable groups of Ar1; c is an integer from 1 to 50; Each X independently represents a single bond, a divalent organic group having 1 to 50 carbon atoms, a sulfonyl group (-SO2-), a divalent sulfur atom, or a divalent oxygen atom. [ka] (In the formula, Ar2 represents an aromatic ring, each Rb independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, the alkyl group or aryl group represented by Rb optionally having a substituent; d represents the number of bonds of cyanato groups to Ar2 and is an integer of 2 to 3, and e represents the number of bonds of Rb to Ar2 and is the number obtained by subtracting (d+2) from the number of substitutable groups of Ar2. [4] In the general formula (II), each X independently represents a divalent linking group selected from the group consisting of structures represented by the following general formulas (IV) to (XV): The resin composition according to [3]. [ka] (In the formula, each Ar3 independently represents an aromatic ring, Rc, Rd, Rg, and Rh each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, and the alkyl group or aryl group in Rc, Rd, Rg, and Rh may have a substituent; Re and Rf each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, the alkyl group or aryl group in Re and Rf may have a substituent, and f represents an integer of 0 to 5. [ka] (In the formula, each Ar4 independently represents an aromatic ring, Ri and Rj each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Ri and Rj may have a substituent. g represents an integer from 0 to 5. [ka] (In the formula, h represents an integer of 4 to 7, and each Rk independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.) [5] The cyanate ester compound (B) contains at least one selected from the group consisting of a compound represented by the following formula (XVI) and a compound represented by the following formula (XVII): The resin composition according to any one of [1] to [4]. [ka] (In the formula, each Ar5 independently represents an aromatic ring, Each Rl independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rm and Rn each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rm and Rn may have a substituent. i represents the number of bonds of cyanato groups to Ar5 and is an integer of 1 to 3; j represents the number of bonds of R to Ar, and represents the number obtained by subtracting (i+2) from the number of substitutable groups of Ar; k represents the number of bonds of Rn to Ar5, which is the number of substitutable groups of Ar5 minus 2; l represents an integer of 1 or more, m represents an integer of 1 or more, and the arrangement of each repeating unit is arbitrary. [ka] (In the formula, each Ar6 independently represents an aromatic ring, Each Ro independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rp and Rq each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rp and Rq may have a substituent. n represents the number of bonds of cyanato groups to Ar6 and is an integer of 2 to 3; o represents the number of bonds of Rp to Ar6, which is the number obtained by subtracting (n+2) from the number of substitutable groups of Ar6; p represents the number of bonds of Rq to Ar6, and represents a number obtained by subtracting 2 from the number of substitutable groups of Ar6. q represents an integer of 1 or more. [6] the content of the cyanate ester compound (A) is 0.1 to 40 parts by mass relative to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B); The resin composition according to any one of [1] to [5]. [7] The cyanate ester compound (A) is allyl cyanate, nonyl cyanate or cumyl cyanate. The resin composition according to any one of [1] to [6]. [8] Further comprising a curing accelerator (C); The resin composition according to any one of [1] to [7]. [9] The curing accelerator (C) is at least one selected from the group consisting of an organic metal salt, an amine compound, a phosphinic acid compound, a phosphonic acid compound, and a urea derivative. The resin composition according to any one of [1] to [8].

[10] The content of the curing accelerator (C) is 0.001 to 5 parts by mass with respect to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B). The resin composition according to any one of [1] to [9].

[11] [1] to

[10] , obtained by curing the resin composition according to any one of the above. cured product.

[12] [1] to

[10] , comprising the resin composition according to any one of the above. Sealing material.

[13] [1] to

[10] , comprising the resin composition according to any one of the above. glue.

[14] [1] to

[10] , comprising the resin composition according to any one of the above. Insulating material.

[15] [1] to

[10] , comprising the resin composition according to any one of the above. paint.

[16] A substrate; and the resin composition according to any one of [1] to

[10] , which is impregnated into or applied to the substrate. Prepreg.

[17]

[16] The prepreg according to the present invention is provided. Laminated plate.

[18] Reinforced fibers, The resin composition according to any one of [1] to

[10] is impregnated into or applied to the reinforcing fiber and cured. Fiber reinforced composite material. Effect of the Invention

[0009] According to the present invention, it is possible to provide a resin composition capable of giving a cured product having high tensile shear adhesive strength and low water absorption, as well as a cured product, a sealing material, an adhesive, an insulating material, a paint, a prepreg, a laminate, and a fiber-reinforced composite material using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Below, we will explain in detail the embodiment of the present invention (hereinafter referred to as the "present embodiment"). However, the present invention is not limited to this embodiment, and various modifications are possible without departing from the gist of the present invention.

[0011] [Resin composition] The resin composition of the present embodiment contains a cyanate ester compound (A) having only one cyanate group in the molecule and a cyanate ester compound (B) having two or more cyanate groups in the molecule, and may contain other components as necessary. Each component will be described in detail below.

[0012] [Cyanate ester compound (A)] The cyanate ester compound (A) is not particularly limited as long as it is a compound having only one cyanato group in the molecule, and examples thereof include compounds represented by the following formula (I): The cyanate ester compound (A) may be used alone or in combination of two or more kinds. [ka] (In the formula, R 1represents a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, an alkenyl group having 2 to 15 carbon atoms, an alkoxy group having 1 to 15 carbon atoms, an aryl group having 6 to 20 carbon atoms, a group in which an alkyl group having 1 to 6 carbon atoms is bonded to an aryl group having 6 to 12 carbon atoms, or an aryloxy group having 6 to 20 carbon atoms; R 1 may have a substituent other than a cyanato group.

[0013] In the formula, R 1 represents any one of a hydrogen atom, an alkyl group having 1 to 15 carbon atoms, an alkenyl group having 2 to 15 carbon atoms, an alkoxy group having 1 to 15 carbon atoms, an aryl group having 6 to 20 carbon atoms, and an aryloxy group having 6 to 20 carbon atoms. Among these, an alkyl group having 1 to 15 carbon atoms, an alkenyl group having 2 to 15 carbon atoms, and an aryl group having 6 to 20 carbon atoms are preferred.

[0014] The alkyl group having 1 to 15 carbon atoms is not particularly limited, and examples thereof include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, t-butyl, n-pentyl, neopentyl, n-hexyl, thexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, n-decyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cyclooctyl, cyclodecyl, and cyclododecyl. Among these, alkyl groups having 3 to 15 carbon atoms are preferred, and alkyl groups having 5 to 12 carbon atoms are more preferred. The alkyl group may be linear, branched, or cyclic.

[0015] The alkenyl group having 2 to 15 carbon atoms is not particularly limited, and examples thereof include a vinyl group, an allyl group, a butenyl group, a pentenyl group, a hexenyl group, and an octenyl group. Among these, an alkenyl group having 2 to 10 carbon atoms is preferred, and an alkenyl group having 2 to 5 carbon atoms is more preferred. The alkenyl group may be linear, branched, or cyclic.

[0016] The alkoxy group having 1 to 15 carbon atoms is not particularly limited, and examples thereof include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentyloxy group, a hexyloxy group, an octyloxy group, a decyloxy group, a dodecyloxy group, a hexadecyloxy group, and an octadecyloxy group, etc. The alkoxy group may be linear, branched, or cyclic.

[0017] The aryl group having 6 to 20 carbon atoms is not particularly limited, but examples thereof include a phenyl group and a naphthyl group.

[0018] The group in which an alkyl group having 1 to 6 carbon atoms is bonded to an aryl group having 6 to 12 carbon atoms is not particularly limited, but examples thereof include an alkylaryl group and an arylalkyl group. The alkylaryl group is not particularly limited, but examples thereof include a methylphenyl group, an ethylphenyl group, a propylphenyl group, a methylnaphthyl group, and a dimethylnaphthyl group. The arylalkyl group is not particularly limited, but examples thereof include a phenylmethyl group, a phenylethyl group, and a phenylpropyl group. Among these, an alkylaryl group and an arylalkyl group are preferred, and an arylalkyl group is more preferred.

[0019] The aryloxy group having 6 to 20 carbon atoms is not particularly limited, but examples thereof include a phenoxy group, a 2-methylphenoxy group, and a 4-t-butylphenoxy group.

[0020] Also, R 1 The substituent other than the cyanato group that may be present in the above-mentioned compound is not particularly limited, and examples thereof include a halogen atom, an alkyl group, an alkoxy group, a carbonyl group, an amino group, an imino group, a thiol group, a sulfo group, a nitro group, an acyl group, an aldehyde group, and an aryl group.

[0021] The compound represented by formula (I) is not particularly limited, but for example, allyl cyanate, nonyl cyanate, and cumyl cyanate are preferred.By using such a cyanate ester compound (A), the tensile shear adhesive strength of the obtained cured product tends to be improved and the water absorption rate tends to be reduced.Among them, allyl cyanate is preferred from the viewpoint of tensile shear adhesive strength and varnish viscosity.

[0022] The content of the cyanate ester compound (A) is preferably 0.1 to 40 parts by mass, more preferably 1 to 35 parts by mass, even more preferably 3 to 30 parts by mass, and even more preferably 4 to 15 parts by mass, relative to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B). When the content of the cyanate ester compound (A) is within the above range, the tensile shear adhesive strength of the obtained cured product tends to be further improved and the water absorption rate tends to be further reduced.

[0023] The ratio (A / B) of the cyanate group equivalent of the cyanate ester compound (A) to the cyanate group equivalent of the cyanate ester compound (B) is preferably 0.0005 to 0.75, more preferably 0.005 to 0.70, even more preferably 0.01 to 0.50, and even more preferably 0.02 to 0.20. When the ratio (A / B) is within the above range, the tensile shear adhesive strength of the obtained cured product tends to be further improved and the water absorption rate tends to be further reduced.

[0024] [Cyanate ester compound (B)] The cyanate ester compound (B) is not particularly limited as long as it is a compound having two or more cyanato groups in the molecule, and examples thereof include at least one selected from the group consisting of compounds represented by the following formula (II) and compounds represented by the following formula (III). Among these, the compound represented by formula (II) is preferred.

[0025] (Compound represented by formula (II)) The compound represented by formula (II) is shown below. [ka] (In the formula, each Ar1 independently represents an aromatic ring, Each Ra independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, and the alkyl group or aryl group in Ra may have a substituent. a represents the number of cyanato groups bonded to Ar1, and each a is independently an integer of 1 to 3, b represents the number of bonds of Ra to Ar1, and each b independently represents a number obtained by subtracting (a+2) from the number of substitutable groups of Ar1; c is an integer from 1 to 50; Each X independently represents a single bond, a divalent organic group having 1 to 50 carbon atoms, a sulfonyl group (-SO2-), a divalent sulfur atom, or a divalent oxygen atom.

[0026] In the above formula, each Ar1 independently represents an aromatic ring. The aromatic ring represented by Ar1 is not particularly limited, but examples thereof include a phenyl group and a naphthyl group. Among these, a phenyl group is preferred.

[0027] Each Ra independently represents any one of a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, and a group in which an alkyl group having 1 to 6 carbon atoms is bonded to an aryl group having 6 to 12 carbon atoms. Among these, a hydrogen atom or an alkenyl group having 2 to 6 carbon atoms is preferred.

[0028] The alkyl group having 1 to 6 carbon atoms is not particularly limited, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group. The alkyl group may be linear, branched, or cyclic.

[0029] The alkenyl group having 2 to 6 carbon atoms is not particularly limited, and examples thereof include a vinyl group, an allyl group, a butenyl group, a pentenyl group, and a hexenyl group. Among these, an alkenyl group having 2 to 10 carbon atoms is preferred, and an alkenyl group having 2 to 5 carbon atoms is more preferred. The alkenyl group may be linear, branched, or cyclic.

[0030] The alkoxy group having 1 to 4 carbon atoms is not particularly limited, but examples thereof include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, etc. The alkoxy group may be linear, branched, or cyclic.

[0031] The aryl group having 6 to 20 carbon atoms is not particularly limited, but examples thereof include a phenyl group and a naphthyl group.

[0032] The group in which an alkyl group having 1 to 6 carbon atoms is bonded to an aryl group having 6 to 12 carbon atoms is not particularly limited, but examples thereof include an alkylaryl group and an arylalkyl group. The alkylaryl group is not particularly limited, but examples thereof include a methylphenyl group, an ethylphenyl group, a propylphenyl group, a methylnaphthyl group, and a dimethylnaphthyl group. The arylalkyl group is not particularly limited, but examples thereof include a phenylmethyl group, a phenylethyl group, and a phenylpropyl group.

[0033] Furthermore, the substituent that the alkyl group or aryl group in Ra may have is not particularly limited, and examples thereof include a halogen atom, an alkyl group, a cyanato group, an alkoxy group, a carbonyl group, an amino group, an imino group, a thiol group, a sulfo group, a nitro group, an acyl group, an aldehyde group, and an aryl group.

[0034] Each a represents the number of cyanato groups bonded to Ar1, and each a is independently an integer of 1 to 3, preferably an integer of 1 to 2, and more preferably 1. Each b represents the number of Ra bonds to Ar1, and each b represents independently a number obtained by subtracting (a+2) from the number of substitutable groups of Ar1. Each c represents an integer of 1 to 50, preferably an integer of 1 to 10, more preferably an integer of 1 to 5, and even more preferably 1.

[0035] Each X independently represents a single bond, a divalent organic group having 1 to 50 carbon atoms, a sulfonyl group (-SO2-), or a divalent sulfur atom or a divalent oxygen atom. The divalent organic group having 1 to 50 carbon atoms represented by X is not particularly limited, and examples thereof include a divalent organic group having 1 to 10 nitrogen atoms (-NRN- (wherein R represents an organic group)), a carbonyl group (-CO-), a carboxy group (-C(=O)O-), a carbonyl dioxide group (-OC(=O)O-), and a divalent linking group selected from the group consisting of structures represented by the following general formulas (IV) to (XV). [ka] (In the formula, each Ar3 independently represents an aromatic ring, Rc, Rd, Rg, and Rh each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, and the alkyl group or aryl group in Rc, Rd, Rg, and Rh may have a substituent; Re and Rf each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, the alkyl group or aryl group in Re and Rf may have a substituent, and f represents an integer of 0 to 5. [ka] (In the formula, each Ar4 independently represents an aromatic ring, Ri and Rj each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Ri and Rj may have a substituent. g represents an integer from 0 to 5. [ka] (In the formula, h represents an integer of 4 to 7, and each Rk independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.)

[0036] In the above formula, examples of aromatic rings represented by Ar3 and Ar4 include the same as those exemplified for Ar1. In addition, in the above formula, examples of alkyl groups having 1 to 6 carbon atoms or aryl groups having 6 to 12 carbon atoms represented by Rc, Rd, Rg, and Rh, and their substituents, and alkyl groups having 1 to 6 carbon atoms, aryl groups having 6 to 12 carbon atoms, and alkoxy groups having 1 to 4 carbon atoms, and their substituents represented by Re, Rf, Ri, and Rj, include the same as those exemplified for Ra.

[0037] Such a compound represented by formula (II) is not particularly limited, and examples thereof include bisphenol A type cyanate, bisphenol E type cyanate, diallyl bisphenol A type cyanate, etc. By using such a compound, the tensile shear adhesive strength of the obtained cured product tends to be further improved and the water absorption rate tends to be further reduced.

[0038] Moreover, as the compound represented by formula (II), a compound represented by the following formula (XVI) is preferable. [ka] (In the formula, each Ar5 independently represents an aromatic ring, Each Rl independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rm and Rn each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rm and Rn may have a substituent. i represents the number of bonds of cyanato groups to Ar5 and is an integer of 1 to 3; j represents the number of bonds of R to Ar, and represents the number obtained by subtracting (i+2) from the number of substitutable groups of Ar; k represents the number of bonds of Rn to Ar5, which is the number of substitutable groups of Ar5 minus 2; l represents an integer of 1 or more, m represents an integer of 1 or more, and the arrangement of each repeating unit is arbitrary.

[0039] In the above formula, examples of the aromatic ring represented by Ar5 include those exemplified in Ar1. In addition, examples of the alkyl group having 1 to 6 carbon atoms, the aryl group having 6 to 12 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the substituents thereof represented by Rm and Rn in the above formula include those exemplified in Ra. Furthermore, l represents an integer of 1 or more, preferably 1 to 10, and more preferably 1 to 5. Furthermore, m represents an integer of 1 or more, preferably 1 to 10, and more preferably 1 to 5.

[0040] (Compound represented by formula (III)) The compound represented by formula (III) is shown below. [ka] (In the formula, Ar2 represents an aromatic ring, each Rb independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, the alkyl group or aryl group represented by Rb optionally having a substituent; d represents the number of bonds of cyanato groups to Ar2 and is an integer of 2 to 3, and e represents the number of bonds of Rb to Ar2 and is the number obtained by subtracting (d+2) from the number of substitutable groups of Ar2.

[0041] In the above formula, examples of the aromatic ring represented by Ar2 include those exemplified as Ar1. In addition, examples of the alkyl group having 1 to 6 carbon atoms, the aryl group having 6 to 12 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the substituents thereof represented by Rb in the above formula include those exemplified as Ra.

[0042] The compound represented by formula (III) is preferably a compound represented by the following formula (XVII). [ka] (In the formula, each Ar6 independently represents an aromatic ring, Each Ro independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rp and Rq each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rp and Rq may have a substituent. n represents the number of bonds of cyanato groups to Ar6 and is an integer of 2 to 3; o represents the number of bonds of Rp to Ar6, which is the number obtained by subtracting (n+2) from the number of substitutable groups of Ar6; p represents the number of bonds of Rq to Ar6, and represents a number obtained by subtracting 2 from the number of substitutable groups of Ar6. q represents an integer of 1 or more.

[0043] In the above formula, examples of the aromatic ring represented by Ar6 include those exemplified for Ar1. In addition, examples of the alkyl group having 1 to 6 carbon atoms, the aryl group having 6 to 12 carbon atoms, the alkoxy group having 1 to 4 carbon atoms, and the substituents thereof represented by Rp and Rq in the above formula include those exemplified for Ra. In addition, q represents an integer of 1 or more, preferably 1 to 10, and more preferably 1 to 5.

[0044] The content of the cyanate ester compound (B) is preferably 60 to 99.9 parts by mass, more preferably 65 to 99 parts by mass, even more preferably 70 to 97 parts by mass, and even more preferably 85 to 96 parts by mass, relative to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B). When the content of the cyanate ester compound (B) is within the above range, the tensile shear adhesive strength of the obtained cured product tends to be further improved and the water absorption rate tends to be further reduced.

[0045] [Cure Accelerator (C)] The resin composition of the present embodiment may further include a curing accelerator (C). The curing accelerator (C) is not particularly limited, but examples thereof include organometallic salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octylate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and iron acetylacetonate; N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2-N-ethylanilinoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutanediamine, N-methylbutanediamine, and the like. amine compounds such as ethylpiperidine, dicyandiamide, benzyldimethylamine, and 4-methyl-N,N-dimethylbenzylamine; phosphinic acid compounds such as dimethylphosphinic acid and phenylmethylphosphinic acid; phosphonic acid compounds such as sodium phosphonate, potassium phosphonate, lithium phosphonate, potassium phosphonate, sodium phenylphosphonate, potassium phenylphosphonate, lithium phenylphosphonate, diethyl phenylphosphonate, sodium ethylphosphonate, and potassium ethylphosphonate; and urea derivatives.

[0046] Among these, at least one selected from the group consisting of organic metal salts, amine compounds, phosphinic acid compounds, phosphonic acid compounds, and urea derivatives can be used. By using such a curing accelerator (C), the tensile shear adhesive strength of the obtained cured product tends to be improved and the water absorption rate tends to be reduced.

[0047] The content of the curing accelerator (C) is preferably 0.001 to 5 parts by mass, more preferably 0.01 to 3 parts by mass, and even more preferably 0.03 to 1 part by mass, relative to 100 parts by mass of the total of the cyanate ester compound (A) and the cyanate ester compound (B). By having the content of the curing accelerator (C) within the above range, the tensile shear adhesive strength of the obtained cured product tends to be further improved and the water absorption rate tends to be further reduced.

[0048] [Other ingredients] The resin composition of the present embodiment may contain at least one selected from the group consisting of maleimide compounds, phenolic resins, epoxy resins, oxetane resins, and compounds having a polymerizable unsaturated group, as necessary. The resin composition of the present embodiment may further contain a filler, a silane coupling agent, a wetting and dispersing agent, a solvent, etc., as necessary. Each component will be described below.

[0049] (Maleimide compounds) The maleimide compound may be any known compound having one or more maleimide groups in one molecule, and the type is not particularly limited. The number of maleimide groups per molecule of the maleimide compound is 1 or more, and preferably 2 or more.

[0050] The maleimide compound is not particularly limited, but examples thereof include N-phenylmaleimide, N-hydroxyphenylmaleimide, bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5-diethyl-4-maleimidophenyl)methane, prepolymers of these maleimide compounds, and prepolymers of the above maleimide compounds and amine compounds. The maleimide compounds may be used alone or in any combination and ratio of two or more.

[0051] (Phenol Resin) The phenol resin is not particularly limited, and any known compound having two or more phenolic hydroxyl groups in one molecule can be used as appropriate.

[0052] The phenol resin is not particularly limited, and examples thereof include cresol novolac type phenol resin, biphenyl aralkyl type phenol resin, naphthol aralkyl type phenol resin, aminotriazine novolac type phenol resin, naphthalene type phenol resin, phenol novolac resin, alkylphenol novolac resin, bisphenol A type novolac resin, dicyclopentadiene type phenol resin, xylok type phenol resin, terpene modified phenol resin, polyvinylphenols, etc. The phenol resin may be used alone or in combination of two or more.

[0053] (Epoxy resin) The epoxy resin may be any known compound having one or more epoxy groups in one molecule, and the type is not particularly limited. The number of epoxy groups per molecule of the epoxy resin is 1 or more, and preferably 2 or more.

[0054] The epoxy resin is not particularly limited, and a conventionally known epoxy resin can be used. For example, biphenyl aralkyl type epoxy resin, naphthalene type epoxy resin, bisnaphthalene type epoxy resin, polyfunctional phenol type epoxy resin, naphthylene ether type epoxy resin, phenol aralkyl type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, xylene novolac type epoxy resin, naphthalene skeleton modified novolac type epoxy resin, dicyclopentadiene novolac type epoxy resin, biphenyl novolac type epoxy resin, phenol aralkyl novolac type epoxy resin, naphthol aralkyl novolac type epoxy resin, aralkyl novolac type epoxy resin, aromatic hydrocarbon formaldehyde type epoxy resin, anthraquinone type epoxy resin, Examples of the epoxy resin include anthracene type epoxy resin, naphthol aralkyl type epoxy resin, dicyclopentadiene type epoxy resin, xylok type epoxy resin, bisphenol A type epoxy resin, bisphenol E type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol A novolac type epoxy resin, phenol type epoxy resin, biphenyl type epoxy resin, aralkyl novolac type epoxy resin, triazine skeleton epoxy resin, triglycidyl isocyanurate, alicyclic epoxy resin, polyol type epoxy resin, glycidylamine, glycidyl type ester resin, butadiene and other double bond-containing compounds in which the double bonds are epoxidized, and compounds obtained by reacting hydroxyl group-containing silicone resins with epichlorohydrin. The epoxy resin may be used alone or in any combination and ratio of two or more types.

[0055] (Oxetane resin) As the oxetane resin, generally known ones can be used, and the type is not particularly limited. Specific examples thereof include alkyl oxetanes such as oxetane, 2-methyl oxetane, 2,2-dimethyl oxetane, 3-methyl oxetane, and 3,3-dimethyl oxetane, 3-methyl-3-methoxymethyl oxetane, 3,3'-di(trifluoromethyl)perfluorooxetane, 2-chloromethyl oxetane, 3,3-bis(chloromethyl)oxetane, biphenyl oxetane, OXT-101 (product name, manufactured by Toagosei Co., Ltd.), and OXT-121 (product name, manufactured by Toagosei Co., Ltd.). These oxetane resins can be used alone or in combination of two or more kinds.

[0056] (Compound having a polymerizable unsaturated group) As the compound having a polymerizable unsaturated group, any generally known compound can be used, and the type thereof is not particularly limited. Specific examples thereof include vinyl compounds such as ethylene, styrene, divinylbenzene, and divinylbiphenyl; (meth)acrylates of monohydric or polyhydric alcohols such as methyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A type epoxy (meth)acrylate and bisphenol F type epoxy (meth)acrylate; allyl compounds such as allyl chloride, allyl acetate, allyl ether, propylene, triallyl cyanurate, triallyl isocyanurate, diallyl phthalate, diallyl isophthalate, and diallyl maleate; and benzocyclobutene resins. These compounds having a polymerizable unsaturated group can be used alone or in combination of two or more.

[0057] (filling material) The filler is not particularly limited, but examples thereof include inorganic fillers and organic fillers. The fillers may be used alone or in combination of two or more.

[0058] The inorganic filler is not particularly limited, but examples thereof include silicas such as natural silica, fused silica, synthetic silica, amorphous silica, aerosil, and hollow silica; silicon compounds such as white carbon; metal oxides such as titanium white, zinc oxide, magnesium oxide, and zirconium oxide; nitrides such as boron nitride, aggregated boron nitride, silicon nitride, and aluminum nitride; metal sulfates such as barium sulfate; aluminum hydroxide; and heat-treated aluminum hydroxide (aluminum hydroxide is heat-treated to reduce some of the water of crystallization). Examples of suitable glass fibers include those having a molecular weight of 100 or more, metal hydrates such as boehmite and magnesium hydroxide; molybdenum compounds such as molybdenum oxide and zinc molybdate; zinc compounds such as zinc borate and zinc stannate; alumina, clay, kaolin, talc, calcined clay, calcined kaolin, calcined talc, mica, E glass, A glass, NE glass, C glass, L glass, D glass, S glass, M glass G20, short glass fibers (including fine glass powders such as E glass, T glass, D glass, S glass, and Q glass), hollow glass, and spherical glass.

[0059] In addition, the organic filler is not particularly limited, but examples thereof include rubber powders such as styrene type powder, butadiene type powder, and acrylic type powder; core-shell type rubber powder; silicone resin powder; silicone rubber powder; and silicone composite powder.

[0060] (Silane coupling agent) The silane coupling agent is not particularly limited as long as it is a silane coupling agent generally used for surface treatment of inorganic substances, but examples thereof include aminosilane compounds such as γ-aminopropyltriethoxysilane and N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane; epoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane; acrylicsilane compounds such as γ-acryloxypropyltrimethoxysilane; cationic silane compounds such as N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride; and phenylsilane compounds. The silane coupling agents may be used alone or in combination of two or more.

[0061] (Wetting and dispersing agent) The wetting and dispersing agent is not particularly limited, but examples thereof include DISPER-110, 111, 118, 180, 161, BYK-W996, W9010, and W903 manufactured by BYK-Chemie Japan Co., Ltd.

[0062] (solvent) The solvent is not particularly limited as long as it can dissolve a part or all of the resin components in the resin composition, and examples thereof include ketones such as acetone and methyl ethyl ketone, aromatic hydrocarbons such as toluene and xylene, amides such as dimethylformamide, methyl cellosolve, propylene glycol monomethyl ether and its acetate, etc. The solvent may be used alone or in combination of two or more kinds.

[0063] [Application] The resin composition of the present embodiment can be suitably used as a cured product, a prepreg, a metal foil-clad laminate, a laminated resin sheet, a resin sheet, a printed wiring board, a sealing material, an adhesive, an insulating material, a paint, or a fiber-reinforced composite material. These will be described below.

[0064] [Cured product] The cured product of this embodiment is obtained by curing the resin composition. The method for producing the cured product is not particularly limited, but for example, the resin composition is melted or dissolved in a solvent, poured into a mold, and cured under normal conditions using heat, light, or the like. In the case of heat curing, the curing temperature is not particularly limited, but is preferably within the range of 120°C to 300°C from the viewpoint of efficient curing and preventing deterioration of the obtained cured product. In the case of photocuring, the wavelength region of light is not particularly limited, but it is preferable to cure in the range of 100nm to 500nm, where curing efficiently proceeds by a photopolymerization initiator, etc.

[0065] [Prepreg] The prepreg of this embodiment has a base material and the above-mentioned resin composition impregnated or applied to the base material. The manufacturing method of the prepreg can be performed according to a conventional method and is not particularly limited. For example, the prepreg of this embodiment can be produced by impregnating or applying the resin component of this embodiment to the base material, and then semi-curing (B-stage) by heating in a dryer at 100 to 200°C for 1 to 30 minutes.

[0066] The content of the resin composition (including the filler) is preferably 30 to 90 mass % relative to the total amount of the prepreg, more preferably 35 to 85 mass %, and further preferably 40 to 80 mass %. When the content of the resin composition is within the above range, moldability tends to be further improved.

[0067] The substrate is not particularly limited, and known materials used in various printed wiring board materials can be appropriately selected and used depending on the intended use and performance. Specific examples of fibers constituting the substrate are not particularly limited, and include glass fibers such as E glass, D glass, S glass, Q glass, spherical glass, NE glass, L glass, and T glass; inorganic fibers other than glass such as quartz; wholly aromatic polyamides such as polyparaphenylene terephthalamide (Kevlar (registered trademark), manufactured by DuPont Co., Ltd.) and copolyparaphenylene-3,4'-oxydiphenylene-terephthalamide (Technora (registered trademark), manufactured by Teijin Techno Products Co., Ltd.); polyesters such as 2,6-hydroxynaphthoic acid-parahydroxybenzoic acid (Vectran (registered trademark), manufactured by Kuraray Co., Ltd.) and Zexion (registered trademark, manufactured by KB Seiren); organic fibers such as polyparaphenylene benzoxazole (Zylon (registered trademark), manufactured by Toyobo Co., Ltd.) and polyimide. Among these, at least one selected from the group consisting of E glass cloth, T glass cloth, S glass cloth, Q glass cloth, and organic fiber is preferable. These substrates may be used alone or in combination of two or more.

[0068] The shape of the substrate is not particularly limited, but examples thereof include woven fabric, nonwoven fabric, roving, chopped strand mat, surfacing mat, etc. The weaving method of the woven fabric is not particularly limited, but examples thereof include plain weave, sash weave, twill weave, etc., and these known weaves can be appropriately selected and used depending on the intended use and performance. In addition, glass woven fabrics that have been subjected to fiber opening treatment or surface treatment with a silane coupling agent or the like are preferably used. The thickness and mass of the substrate are not particularly limited, but typically, those of about 0.01 to 0.3 mm are preferably used. In particular, from the viewpoint of strength and water absorbency, the substrate should have a thickness of 200 μm or less and a mass of 250 g / m 2 The following glass woven fabrics are preferred, and glass woven fabrics made of E-glass, S-glass, and T-glass glass fibers are more preferred.

[0069] [Laminated resin sheet] The laminated resin sheet of the present embodiment has a support and the above-mentioned resin composition disposed on the support. The laminated resin sheet is used as one means for thinning a sheet, and can be produced, for example, by directly applying the resin composition to a support such as a metal foil or a film, and drying the applied resin composition.

[0070] The support is not particularly limited, but may be any known material used in various printed wiring board materials. For example, organic film substrates such as polyimide film, polyamide film, polyester film, polyethylene terephthalate (PET) film, polybutylene terephthalate (PBT) film, polypropylene (PP) film, polyethylene (PE) film, polycarbonate film, ethylene tetrafluoroethylene copolymer film, and release film obtained by applying a release agent to the surface of these films, conductive foils such as aluminum foil, copper foil, and gold foil, and plate-shaped inorganic films such as glass plate, SUS plate, and FPR, etc. are preferred. Among these, electrolytic copper foil and PET film are preferred.

[0071] Examples of the application method include a method in which a solution in which the resin composition of the present embodiment is dissolved in a solvent is applied onto a support using a bar coater, a die coater, a doctor blade, a baker applicator, or the like.

[0072] The laminated resin sheet is preferably a laminated resin sheet obtained by applying the resin composition to a support and then semi-curing (B-stage). Specifically, for example, the resin composition is applied to a support such as copper foil, and then semi-cured by heating in a dryer at 100 to 200° C. for 1 to 60 minutes to produce a laminated resin sheet. The amount of the resin composition attached to the support is preferably in the range of 1 to 300 μm in terms of the resin thickness of the laminated resin sheet.

[0073] [Single-layer resin sheet] The single-layer resin sheet of the present embodiment includes a resin composition. The single-layer resin sheet is formed by molding the resin composition into a sheet. The manufacturing method of the resin sheet can be performed according to a conventional method and is not particularly limited. For example, the resin sheet can be obtained by peeling or etching the support from the laminated resin sheet. In addition, a single-layer resin sheet can also be obtained without using a sheet substrate by supplying a solution in which the resin composition of the present embodiment is dissolved in a solvent into a mold having a sheet-shaped cavity and drying it to form it into a sheet.

[0074] [Laminated Plate] The laminate of the present embodiment includes the above prepreg. The laminate may be a metal foil-clad laminate further including a metal foil disposed on one or both sides of the prepreg.

[0075] The metal foil can be a metal foil such as copper or aluminum. The metal foil used here is not particularly limited as long as it is used as a printed wiring board material, but is preferably a known copper foil such as rolled copper foil or electrolytic copper foil. The thickness of the conductor layer is not particularly limited, but is preferably 1 to 70 μm, more preferably 1.5 to 35 μm.

[0076] The molding method and molding conditions for the metal foil-clad laminate are not particularly limited, and general methods and conditions for laminates and multilayer boards for printed wiring boards can be applied. For example, a multi-stage press machine, a multi-stage vacuum press machine, a continuous molding machine, an autoclave molding machine, etc. can be used when molding the metal foil-clad laminate. In addition, the temperature in molding the metal foil-clad laminate is 100 to 350°C, and the pressure is a surface pressure of 2 to 100 kgf / cm. 2 The heating time is generally in the range of 0.05 to 5 hours. If necessary, post-curing can be performed at a temperature of 150 to 350° C. Also, it is possible to form a multilayer board by combining the above-mentioned prepreg with a separately prepared wiring board for an inner layer and laminating and molding it.

[0077] [Printed Wiring Board] The printed wiring board of this embodiment includes an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer includes the above-mentioned resin composition. The above-mentioned metal foil-clad laminate can be suitably used as a printed wiring board by forming a predetermined wiring pattern. The above-mentioned metal foil-clad laminate has good moldability and chemical resistance, and can be particularly effectively used as a printed wiring board for semiconductor packages that require such performance.

[0078] Specifically, the printed wiring board of the present embodiment can be manufactured, for example, by the following method. First, the above-mentioned metal foil-clad laminate (copper-clad laminate, etc.) is prepared. The surface of the metal foil-clad laminate is etched to form an inner layer circuit, and an inner layer substrate is manufactured. The inner layer circuit surface of this inner layer substrate is subjected to a surface treatment for increasing adhesive strength as necessary, and then a required number of the above-mentioned prepregs are stacked on the inner layer circuit surface, and a metal foil for an outer layer circuit is further stacked on the outside thereof, and heated and pressed to form an integral mold. In this way, a multilayer laminate is manufactured in which an insulating layer made of a base material and a cured product of a resin composition is formed between the inner layer circuit and the metal foil for the outer layer circuit. Next, the multilayer laminate is subjected to a hole punching process for through holes and via holes, and then a desmear process is performed to remove smears, which are resin residues derived from the resin components contained in the cured product layer. A plated metal film is then formed on the wall surface of this hole to provide electrical continuity between the inner layer circuit and the metal foil for the outer layer circuit, and the metal foil for the outer layer circuit is then etched to form the outer layer circuit, thereby producing a printed wiring board.

[0079] The printed wiring board obtained in the above manufacturing example has an insulating layer and a conductor layer formed on the surface of this insulating layer, and the insulating layer contains the resin composition of the present embodiment described above. In other words, the above prepreg (substrate and the above resin composition attached thereto) and the resin composition layer of the metal foil-clad laminate (layer made of the above resin composition) constitute the insulating layer containing the above resin composition.

[0080] In addition, when a metal foil-clad laminate is not used, a printed wiring board may be produced by forming a conductor layer to be a circuit on the prepreg, the laminated resin sheet, or the resin composition. In this case, the conductor layer may be formed by electroless plating.

[0081] The printed wiring board of this embodiment can be particularly effectively used as a printed wiring board for semiconductor packages, since the insulating layer has excellent properties such as plating peel strength, bending strength, dielectric constant, and thermal weight loss rate.

[0082] [Sealing material] The sealing material of the present embodiment includes the resin composition of the present embodiment. The method for producing the sealing material can be appropriately applied by a generally known method, and is not particularly limited. For example, the above-mentioned resin composition and various known additives or solvents generally used in sealing material applications can be mixed using a known mixer to produce a sealing material. In addition, the method for adding each component during mixing can be appropriately applied by a generally known method, and is not particularly limited.

[0083] 〔glue〕 The adhesive of the present embodiment includes the resin composition of the present embodiment. The manufacturing method of the adhesive can be appropriately applied by a generally known method, and is not particularly limited. For example, the adhesive can be manufactured by mixing the above-mentioned resin composition with various known additives or solvents generally used in adhesive applications using a known mixer. In addition, the method of adding each component during mixing can be appropriately applied by a generally known method, and is not particularly limited.

[0084] [Insulating materials] The insulating material of the present embodiment includes the resin composition of the present embodiment. The method for producing the insulating material can be appropriately applied by a generally known method, and is not particularly limited. For example, the adhesive can be produced by mixing the above-mentioned resin composition with various known additives or solvents that are generally used in adhesive applications using a known mixer. In addition, the method for adding each component during mixing can be appropriately applied by a generally known method, and is not particularly limited.

[0085] 〔paint〕 The coating material of the present embodiment includes the resin composition of the present embodiment. The coating material can be produced by a method that is generally known and is not particularly limited. For example, the coating material can be produced by mixing the above-mentioned resin composition with various known additives or solvents that are generally used in adhesive applications using a known mixer. The method of adding each component during mixing can be appropriately applied using a method that is generally known and is not particularly limited.

[0086] [Fiber-reinforced composite materials] The fiber-reinforced composite material of the present embodiment has reinforcing fibers and a resin composition that has been impregnated into or applied to the reinforcing fibers and cured.

[0087] As the reinforcing fiber, generally known ones can be used, and are not particularly limited. Specific examples thereof include glass fibers such as E glass, D glass, L glass, S glass, T glass, Q glass, UN glass, NE glass, and spherical glass, carbon fibers, aramid fibers, boron fibers, PBO fibers, high-strength polyethylene fibers, alumina fibers, and silicon carbide fibers. The form and arrangement of the reinforcing fiber are not particularly limited, and can be appropriately selected from woven fabrics, nonwoven fabrics, mats, knits, braided cords, unidirectional strands, rovings, chopped fibers, and the like. In addition, as the form of the reinforcing fiber, a preform (a laminate of woven fabric base fabrics made of reinforcing fibers, or a laminate of the laminate sewn together with a stitch thread, or a fiber structure such as a three-dimensional woven fabric or a braided fabric) can also be applied.

[0088] The manufacturing method of these fiber-reinforced composite materials can be appropriately applied by a generally known method, and is not particularly limited. Specific examples include the liquid composite molding method, the resin film infusion method, the filament winding method, the hand lay-up method, the pultrusion method, etc. Among these, the resin transfer molding method, which is one of the liquid composite molding methods, can be used for various applications because materials other than the preform, such as metal plates, foam cores, honeycomb cores, etc., can be set in the mold in advance, and is therefore preferably used when mass-producing composite materials with relatively complex shapes in a short period of time. EXAMPLES

[0089] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0090] Synthesis Example 1: Synthesis of a compound represented by the following formula (1) (allylphenol cyanate ester compound, hereinafter abbreviated as "ACN") [ka] Solution A was prepared by dissolving 30.0 g (224 mmol) of allylphenol (manufactured by Tokyo Chemical Industry Co., Ltd.) and 17.14 g (169 mmol) of triethylamine (0.75 mol per mol of hydroxyl group) in 150.0 g of dichloromethane.

[0091] 22.44g (365mol) of cyanogen chloride (1.6mol per 1mol of hydroxyl group), 50.86g of dichloromethane, 36.91g (364mmol) of 36% hydrochloric acid (1.6mol per 1mol of hydroxyl group), and 228.8g of water were poured into the flask over 20 minutes while stirring and maintaining the liquid temperature at -2 to -0.5°C. After the end of the pouring of solution A, the mixture was stirred at the same temperature for 30 minutes, and then a solution (solution B) in which 30.86g of triethylamine (304mmol) (1.35mol per 1mol of hydroxyl group) was dissolved in 30.86g of dichloromethane was poured into the flask over 15 minutes. After the end of the pouring of solution B, the mixture was stirred at the same temperature for 30 minutes to complete the reaction.

[0092] The reaction solution was then left to stand to separate the organic and aqueous phases. The resulting organic phase was washed with 300 g of 0.1N hydrochloric acid, and then washed four times with 150 g of water. The electrical conductivity of the wastewater from the fourth water wash was 17 μS / cm, confirming that the ionic compounds were sufficiently removed by washing with water.

[0093] The organic phase after washing with water was concentrated under reduced pressure, and finally concentrated to dryness at 50° C. for 1 hour to obtain 33.3 g of the target cyanate ester compound ACN. The structure of the obtained cyanate ester compound ACN was identified by NMR. 1H-NMR: (500MHz, chloroform-d, internal standard TMS) δ(ppm)=3.41(d,2H), 5.05(m,1H), 5.11(m,1H), 5.87-5.95(m,1H), 7.23-7.45(m,4H)

[0094] Synthesis Example 2: Synthesis of a compound represented by the following formula (2) (nonylphenol cyanate ester compound, hereinafter abbreviated as "NPCN") [ka] Solution A was prepared by dissolving 35.0 g (159 mmol) of 4-nonylphenol (Tokyo Chemical Industry Co., Ltd.) and 12.18 g (120 mmol) of triethylamine (0.75 mol per mol of hydroxyl group) in 175.0 g of dichloromethane.

[0095] 15.94g (259mol) of cyanogen chloride (1.6mol per 1mol of hydroxyl group), 36.13g of dichloromethane, 26.22g (259mmol) of 36% hydrochloric acid (1.6mol per 1mol of hydroxyl group), and 162.6g of water were poured into the flask over 20 minutes while stirring and maintaining the liquid temperature at -2 to -0.5°C. After the end of the pouring of solution A, the mixture was stirred at the same temperature for 30 minutes, and then a solution (solution B) in which 33.28g (329mmol) of triethylamine (2.05mol per 1mol of hydroxyl group) was dissolved in 33.28g of dichloromethane was poured into the flask over 20 minutes. After the end of the pouring of solution B, the mixture was stirred at the same temperature for 30 minutes to complete the reaction.

[0096] The reaction solution was then left to stand to separate the organic and aqueous phases. The resulting organic phase was washed with 300 g of 0.1N hydrochloric acid, and then washed five times with 180 g of water. The electrical conductivity of the wastewater from the fifth water wash was 29 μS / cm, confirming that the ionic compounds were sufficiently removed by washing with water.

[0097] The organic phase after washing with water was concentrated under reduced pressure, and finally concentrated to dryness at 50°C for 1 hour to obtain 36.4 g of the target cyanate ester compound NPCN. The IR spectrum of NPCN showed an absorption at 2263 cm-1 (cyanate ester group) and no absorption of the hydroxyl group.

[0098] Synthesis Example 3: Synthesis of a compound represented by the following formula (3) (cumylphenol cyanate ester compound, hereinafter abbreviated as "CPCN") [ka] 20.0 g (94 mmol) of cumylphenol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 7.22 g (71 mmol) of triethylamine (0.75 mol per mol of hydroxyl group) were dissolved in 100.0 g of dichloromethane to prepare solution A.

[0099] 9.46g (154mol) of cyanogen chloride (1.6mol per 1mol of hydroxyl group), 21.43g of dichloromethane, 15.55g (154mmol) of 36% hydrochloric acid (1.6mol per 1mol of hydroxyl group), and 96.4g of water were poured in over 10 minutes while stirring and keeping the liquid temperature at -2 to -0.5°C. After the end of pouring in solution A, the mixture was stirred at the same temperature for 30 minutes, and then a solution (solution B) in which 19.74g (195mmol) of triethylamine (2.05mol per 1mol of hydroxyl group) was dissolved in 19.74g of dichloromethane was poured in over 15 minutes. After the end of pouring in solution B, the mixture was stirred at the same temperature for 30 minutes to complete the reaction.

[0100] The reaction solution was then left to stand to separate the organic and aqueous phases. The resulting organic phase was washed with 200 g of 0.1N hydrochloric acid, and then washed six times with 100 g of water. The electrical conductivity of the wastewater from the sixth wash was 26 μS / cm, confirming that the ionic compounds were sufficiently removed by washing with water.

[0101] The organic phase after washing with water was concentrated under reduced pressure, and finally concentrated to dryness at 50° C. for 1 hour to obtain 19.0 g of the target cyanate ester compound CPCN. The structure of the obtained cyanate ester compound CPCN was identified by NMR. 1H-NMR: (500MHz, chloroform-d, internal standard TMS) δ(ppm)=1.68(s,6H), 7.18-7.31(m,9H)

[0102] Example 1 A resin composition was obtained by mixing 5 parts by mass of allyl cyanate (Synthesis Example 1, ACN), 95 parts by mass of bisphenol E type cyanate (P-201, manufactured by Mitsubishi Gas Chemical Company, Inc.), and 0.05 parts by mass of zinc octylate.

[0103] [Examples 2 to 3] A resin composition was obtained in the same manner as in Example 1, except that the mass ratio of allyl cyanate (ACN) and bisphenol E type cyanate (P-201) was changed as shown in Table 1 below.

[0104] Example 4 A resin composition was obtained by mixing 1 part by mass of nonyl cyanate (Synthesis Example 2, NPCN), 99 parts by mass of bisphenol E type cyanate (P-201), and 0.05 parts by mass of zinc octylate.

[0105] [Examples 5 to 7] A resin composition was obtained in the same manner as in Example 4, except that the mass ratio of nonyl cyanate (NPCN) and bisphenol E type cyanate (P-201) was changed as shown in Table 1 below.

[0106] Example 8 A resin composition was obtained by mixing 10 parts by mass of cumyl cyanate (Synthesis Example 3, CPCN), 90 parts by mass of bisphenol E type cyanate (P-201), and 0.05 parts by mass of zinc octylate.

[0107] Example 9 A resin composition was obtained in the same manner as in Example 8, except that the mass ratio of cumyl cyanate (CPCN) and bisphenol E type cyanate (P-201) was changed as shown in Table 1 below.

[0108] Comparative Example 1 A resin composition was obtained by mixing 100 parts by mass of bisphenol E cyanate (P-201) and 0.05 parts by mass of zinc octylate.

[0109] Example 10 A resin composition was obtained by mixing 5 parts by mass of nonyl cyanate (NPCN), 95 parts by mass of bisphenol A cyanate (TA, manufactured by Mitsubishi Gas Chemical Company, Inc.), and 0.05 parts by mass of zinc octylate.

[0110] Comparative Example 2 A resin composition was obtained by mixing 100 parts by mass of bisphenol A cyanate (TA) and 0.05 parts by mass of zinc octylate.

[0111] Example 11 A resin composition was obtained by mixing 1 part by mass of allyl cyanate (ACN), 99 parts by mass of diallyl bisphenol A cyanate (A-211, manufactured by Mitsubishi Gas Chemical Company, Inc.), and 0.05 parts by mass of zinc octylate.

[0112] [Examples 12 to 13] A resin composition was obtained in the same manner as in Example 11, except that the mass ratio of allyl cyanate (ACN) and diallyl bisphenol A cyanate (A-211) was changed as shown in Table 2 below.

[0113] Comparative Example 2 A resin composition was obtained by mixing 100 parts by mass of diallyl bisphenol A cyanate (A-211) and 0.05 parts by mass of zinc octylate.

[0114] [Tensile shear adhesive strength] The resin composition obtained as described above was applied to one of the two adherends, and the two adherends were bonded together via the resin composition. The resin composition was then cured to obtain a test piece. The tensile shear adhesive strength (MPa) was then measured in accordance with JIS K 6850 (1999). A precision universal testing machine (Shimadzu Corporation, Autograph Model "AG-X plus") was used as the measuring device.

[0115] [Water absorption rate] The resin composition was cured at 150°C for 3 hours, 180°C for 5 hours, and 250°C for 3 hours to obtain test pieces of 10 mm x 35 mm x 4 mm. The test pieces were used to measure the water absorption rate after treatment at 121°C and 2 atm for 14 days in a pressure cooker tester (Hirayama Seisakusho, PC-3 type) in accordance with JIS C648.

[0116] [Varnish Viscosity] The viscosity (mPa s) of the resin composition at 25°C was measured using a dynamic viscoelasticity measuring device (Model "DHR-2" manufactured by TA Instruments Japan, Inc.). Note that the viscosity measurement was performed for resin compositions that were liquid at 25°C, and for resin compositions that were solid at 25°C, this is noted in Tables 1 and 2.

[0117] The measured values ​​of each Example for the tensile shear adhesive strength, water absorption, and varnish viscosity were evaluated relative to the measured values ​​of the Comparative Examples, which were set to 100. Specifically, Examples 1 to 9 were evaluated relative to the measured value of Comparative Example 1, Example 10 was evaluated relative to the measured value of Comparative Example 2, which was set to 100, and Examples 11 to 13 were evaluated relative to the measured value of Comparative Example 3, which was set to 100. The results are shown in Tables 1 and 2 below.

[0118] [Table 1]

[0119] [Table 2] [Industrial Applicability]

[0120] INDUSTRIAL APPLICABILITY The resin composition of the present invention has industrial applicability as a resin component used in cured products, sealing materials, adhesives, insulating materials, paints, prepregs, laminates, fiber-reinforced composite materials, and the like.

Claims

1. A cyanate ester compound (A) having only one cyanato group in the molecule and represented by the following formula (I), and a cyanate ester compound (B) having two or more cyanate groups in the molecule and being at least one selected from the group consisting of a compound represented by the following formula (II) and a compound represented by the following formula (III), The content of the cyanate ester compound (A) is 0.1 to 40 parts by mass relative to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B). 【Chemistry 1】 (In the formula, R1 represents any one of alkenyl groups having 2 to 15 carbon atoms.) 【Chemistry 2】 (In the formula, Ar 1 each independently represents an aromatic ring; Each Ra independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, and the alkyl group or aryl group represented by Ra may have a substituent. a is Ar 1 each independently represents an integer of 1 to 3, b is Ar 1 represents the number of bonds of Ra to Ar, 1 represents the number obtained by subtracting (a+2) from the substitutable base of c is an integer from 1 to 50; Each X independently represents a single bond, a divalent organic group having 1 to 50 carbon atoms, a sulfonyl group (-SO2-), a divalent sulfur atom, or a divalent oxygen atom. 【Chemistry 3】 (In the formula, Ar 2 represents an aromatic ring, each Rb independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, or a group in which an alkyl group having 1 to 6 carbon atoms and an aryl group having 6 to 12 carbon atoms are bonded, the alkyl group or aryl group represented by Rb optionally having a substituent; d is Ar 2 represents the number of bonds of cyanato groups to Ar, and is an integer of 2 to 3; 2 represents the number of bonds of Rb to Ar 2 It represents the number obtained by subtracting (d+2) from the substitutable base number of . Resin composition.

2. In the general formula (II), each X independently represents a divalent linking group selected from the group consisting of structures represented by the following general formulas (IV) to (XV): The resin composition according to claim 1. 【Chemistry 4】 (In the formula, Ar 3 each independently represents an aromatic ring; Rc, Rd, Rg, and Rh each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 12 carbon atoms, and the alkyl group or aryl group in Rc, Rd, Rg, and Rh may have a substituent; Re and Rf each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, the alkyl group or aryl group in Re and Rf may have a substituent, and f represents an integer of 0 to 5. 【Chemistry 5】 (In the formula, Ar 4 each independently represents an aromatic ring; Ri and Rj each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Ri and Rj may have a substituent. g represents an integer of 0 to 5. 【Chemistry 6】 (In the formula, h represents an integer of 4 to 7, and each Rk independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms.)

3. The cyanate ester compound (B) contains at least one selected from the group consisting of a compound represented by the following formula (XVI) and a compound represented by the following formula (XVII): The resin composition according to any one of claims 1 to 2. 【Chemistry 7】 (In the formula, Ar 5 each independently represents an aromatic ring; Each R independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rm and Rn each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rm and Rn may have a substituent. i is Ar 5 represents the number of cyanato groups bonded to j is Ar 5 represents the number of bonds of Rm to Ar 5 represents the number obtained by subtracting (i+2) from the substitutable base of k is Ar 5 represents the number of bonds of R to Ar 5 represents the substitutable base of minus 2, l represents an integer of 1 or more, m represents an integer of 1 or more, and the arrangement of each repeating unit is arbitrary. 【Chemistry 8】 (In the formula, Ar 6 each independently represents an aromatic ring; Each Ro independently represents a methylene group, a methyleneoxy group, a methyleneoxymethylene group, an oxymethylene group, or a group formed by linking these groups; Rp and Rq each independently represent a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms, and the alkyl group or aryl group in Rp and Rq may have a substituent. n is Ar 6 represents the number of cyanato groups bonded to o is Ar 6 represents the number of bonds of Rp to Ar 6 represents the number obtained by subtracting (n+2) from the substitutable base of p is Ar 6 represents the number of bonds of Rq to Ar 6 It represents the substitutable base of minus 2. q represents an integer of 1 or more.

4. The cyanate ester compound (A) is allyl phenyl cyanate. The resin composition according to any one of claims 1 to 3.

5. Further comprising a curing accelerator (C); The resin composition according to any one of claims 1 to 4.

6. The curing accelerator (C) is at least one selected from the group consisting of an organic metal salt, an amine compound, a phosphinic acid compound, a phosphonic acid compound, and a urea derivative. The resin composition according to claim 5.

7. The content of the curing accelerator (C) is 0.001 to 5 parts by mass relative to 100 parts by mass in total of the cyanate ester compound (A) and the cyanate ester compound (B). The resin composition according to claim 5 or 6.

8. A cured resin composition according to any one of claims 1 to 7. cured product.

9. The resin composition according to any one of claims 1 to 7 is included. Sealing material.

10. The resin composition according to any one of claims 1 to 7 is included. glue.

11. The resin composition according to any one of claims 1 to 7 is included. Insulating material.

12. The resin composition according to any one of claims 1 to 7 is included. paint.

13. A substrate; The resin composition according to any one of claims 1 to 7, which is impregnated or applied to the substrate. Prepreg.

14. The prepreg according to claim 13 is provided. Laminated plate.

15. Reinforced fibers, The resin composition according to any one of claims 1 to 7, which is impregnated or applied to the reinforcing fiber and cured. Fiber reinforced composite material.

Citation Information

Patent Citations

  • The comonomer composition derived from aromatic and / [porishianeto[porishianeto][monoshianeto[monoshianeto] polytriazines

    JP1990503003A

  • Prepreg and laminate for electricity

    JP1994049238A

  • Triazine polymer and its use

    JP1994228308A

  • Resin composition having excellent dielectric characteristic, varnish, prepreg and metal-clad laminate made by using the same

    JP2001261958A

  • Cyanate ester compound, curable resin composition containing cyanate ester compound, and cured product thereof

    WO2012057144A1