Coated forming tools for improved performance and service life

The application of a Si-C-N coated forming tool, enhanced with additional layers, addresses the need for improved performance and service life in plastic and aluminum processing by providing corrosion resistance and mechanical stability.

JP7587760B2Active Publication Date: 2024-11-21OERLIKON SURFACE SOLUTIONS AG PFAFFIKON
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021570934
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-29
Filing Date
2020-05-29
Publication Date
2024-11-21
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

Existing forming tools used in plastic and aluminum processing operations face challenges in productivity, economy, and reliability, with a need for increased service life and improved performance.

Method used

A forming tool coated with a Si-C-N based layer, optionally combined with additional layers such as a nitrided layer and a hard thin film layer, is applied using PE-CVD techniques, providing improved corrosion resistance, inertness to plastic materials, and enhanced mechanical stability.

Benefits of technology

The Si-C-N coated forming tools exhibit significantly increased service life, reduced material sticking, and improved contact pressure, leading to enhanced performance and reliability in plastic and aluminum processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587760000001
    Figure 0007587760000001
  • Figure 0007587760000002
    Figure 0007587760000002
  • Figure 0007587760000003
    Figure 0007587760000003
Patent Text Reader

Abstract

A coated forming tool for processing plastic materials or aluminum or aluminum alloy materials, comprising a substrate (10) having a substrate surface (1), the substrate surface (1) being coated with a coating (2) formed of one or more layers, the coating (2) comprising Si with elements selected from the elements hydrogen, oxygen, titanium, chromium, and / or aluminum. a C b N c X d The present invention is characterized by having a Si-CN based layer (3) having an elemental composition in element % corresponding to:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated molding tool that is particularly advantageous for processing plastics or aluminum or aluminum alloys. Such processing operations may include, for example, injection molding of plastics and die casting of aluminum (or aluminum alloys). The coated molding tool of the present invention can achieve better performance and significantly increase the service life compared to coated molding tools known in the art.

[0002] The term "forming tool" in the context of the present invention should be understood to refer to any type of forming tool or part of a forming tool, including a mould or mould part, having a surface intended to come into contact with the material to be processed, e.g. with a plastic material in a plastics processing operation or with an aluminium (or aluminium alloy material) in an aluminium (or aluminium alloy) processing operation. [Background technology]

[0003] The use of coatings on forming tools to improve their performance is already known.

[0004] An article titled "Extrusion: Special Dusenoberflachen vermeiden Corrosion und Verschleiss" published in edition 6 / 2008 of the magazine "Blasformen&Extrusionswerkzeuge" reports that a chemical nickel coating on the surface of plastic extrusion nozzles offers significant advantages in terms of corrosion and wear resistance compared to other coatings.

[0005] One of the most important advantages of these chemical nickel coatings is that they can be deposited faithfully to the contours of the surface of the tool or part to be coated. They should be able to coat evenly even complex shapes, boreholes and recesses. The process temperature for depositing these coatings is up to 90°C. It has also been reported that at least twice as long a service life was achieved with chemical nickel coatings compared to coatings produced by chrome plating. Furthermore, it has been reported that the usual troubles encountered when removing polypropylene (PP) white plastic parts from blow molds can be avoided by using these types of chemical nickel coatings, especially the coating called "Chemish Nickel-PTFE".

[0006] An article by Stephane Itasse titled "New Product Review Stand for Spritzgiesswerkzeug" published on the homepage of the specialist media MaschinenMarkt on September 22, 2015, reported that a coating called Balinit A from Oerlikon Balzers was used to coat die-casting molds, and that this coating could increase the service life by ten times.

[0007] However, increasing demands on the productivity, economy and reliability of manufacturing processes require new solutions to be provided in order to meet the very high demands.

[0008] Objective of the invention The object of the present invention is to provide a solution for improving the productivity, economy and reliability of the manufacturing process in forming operations, preferably in plastics and / or aluminium processing operations, which preferably leads to a significant increase in the service life of the forming tools used in the corresponding processing operations.

[0009] Description of the invention The object of the present invention is achieved by providing a forming tool, in particular a substrate, which comprises coating a surface of the substrate with a coating comprising a Si-CN based layer, the main components of which are silicon, carbon and nitrogen.

[0010] The elemental composition of a layer according to the present invention can be expressed as follows: 50 <a+b+c≦100、0≦d<60のSi a C b N c X d , preferably 0≦d<50, and X can be one or more elements selected from the group of elements: H, O; Ti, Cr, Al. 0≦d<55 can be a preferred embodiment, 0≦d<50 can be a more preferred embodiment, 0≦d<45 can be a further preferred embodiment, and 0≦d<40 can be a still more preferred embodiment.

[0011] Preferably, X comprises hydrogen, oxygen, or hydrogen and oxygen.

[0012] Preferably, X comprises titanium, or chromium, or aluminium, or a combination of titanium, chromium, and / or aluminium.

[0013] In a preferred embodiment, the elemental composition of the layer according to the invention is as follows: Si a C b N c Y e Z f Preferably, d=e+f. Preferably, Y comprises hydrogen, oxygen, titanium, chromium, or aluminum. Preferably, Z comprises hydrogen, oxygen, titanium, chromium, or aluminum. Preferably, Si a C b N c Y e Z f contains hydrogen and oxygen.

[0014] According to a preferred embodiment, X corresponds to the elements H and O.

[0015] Furthermore, by doping the Si-C-N based layer (silicon carbonitride based layer) with metal atoms such as Ti, Cr, and / or Al, further advantages in terms of the coating properties can be obtained. These metal elements can be incorporated into the coating using typical CVD precursors such as TiCl4, AlCr3 and / or organometallic precursors.

[0016] In a preferred embodiment, an element composition of Si a C b N c X d having 60 < a + b + c ≦ 100 and 0 ≦ d < 60 is used for the Si-C-N based layer of the present invention, and particularly good results can be obtained. If 0 ≦ d < 55, it can be a preferred embodiment, if 0 ≦ d < 50, it can be a more preferred embodiment, if 0 ≦ d < 45, it can be a further preferred embodiment, and if 0 ≦ d < 40, it can be a more preferred embodiment.

[0017] To explain the present invention in more detail, some examples and preferred embodiments of the present invention will be described.

[0018] Figures 1 to 4 should be helpful for understanding some examples and preferred embodiments of the present invention.

[0019] The examples and preferred embodiments in the following description of the present invention should not be understood as limiting the present invention, but should be understood as a showcase for better understanding the present invention.

Brief Description of the Drawings

[0020] [Figure 1] The architecture of a coating system deposited on the substrate surface 1 of a substrate 10 of a forming tool according to the present invention is schematically shown. The coating 2 is deposited as a single layer on the substrate surface 1, that is, the coating 2 is formed of only one layer, and the layer is a Si-C-N based layer 3.

[0021] [Diagram 2] FIG. 1 shows a schematic architecture of a coating system in another embodiment of the present invention, deposited on a substrate surface 1 of a substrate 10 of a forming tool according to the present invention, where a coating 2 is deposited on the substrate surface 1 as a multilayer, i.e. the coating 2 is formed of two or more layers, a Si-CN based layer is deposited as the top layer and a hard thin film layer 5 is deposited between the substrate surface 1 and the Si-CN based layer 3.

[0022] [Diagram 3] FIG. 1 shows a schematic architecture of a coating system in another embodiment of the present invention deposited on a substrate surface 1 of a substrate 10 of a forming tool according to the present invention, where a coating 2 is deposited as a multilayer on the substrate surface 1, i.e. the coating 2 is formed of two or more layers, a Si-CN based layer 3 is deposited as a top layer, the substrate 10 comprises a nitride layer 4, which preferably forms the substrate surface 1, and a hard thin film layer 5 is deposited between the nitride layer 4 and the Si-CN based layer 3.

[0023] [Figure 4] Schematically shows the architecture of a coating system in another embodiment of the invention deposited on a substrate surface 1 of a substrate 10 of a forming tool according to the invention, where a coating 2 is deposited as a multilayer on an adhesion layer 6, the substrate 10 comprising a nitride layer 4, which preferably forms the substrate surface 1, an adhesion layer 6 is deposited on the nitride layer 4, which preferably comprises the substrate surface 1 as described above, a Si-CN based layer 3 is deposited as a top layer, and a hard thin film layer 5 is deposited between the adhesion layer 6 and the Si-CN based layer 3.

[0024] The inventors have found that when the Si-CN based layer 3 is deposited as the outermost layer of the coating 2, particularly good improvements in the performance and service life of forming tools, especially in plastics processing operations and aluminium processing operations, can be achieved.

[0025] The Si-CN based layer 3 of the present invention is preferably deposited so as to exhibit: - Amorphous layer structure, and / or - there are no droplets (droplets typically form in coatings deposited by physical vapor deposition (PVD) processes, especially the unfiltered arc deposition process), and / or -High corrosion resistance.

[0026] Preferably, the Si-CN based layer 3 of the present invention simultaneously exhibits all the above listed properties.

[0027] By depositing the inventive Si-CN based layer 3 as a top layer of the coating 2, it is further possible to obtain additional advantages, such as: - the material of the forming tool does not react chemically when in contact with the plastic material being processed (inert); and / or - Reduced tendency of molding tool material to stick to the molten plastic during processing.

[0028] According to a first preferred embodiment of the invention, the coating 2 consists only of one Si-CN based layer 3. In this case, the Si-CN based layer 3 may be deposited directly on the substrate surface 1, as shown in Figure 1. It may be advantageous if an adhesion layer 6 for improving the adhesion of the coating 2 to the substrate surface 1 can additionally be deposited between the substrate surface 1 and the Si-CN based layer 3 constituting the coating 2.

[0029] By providing a forming tool according to this first embodiment with a coating of the present invention (see, for example, FIG. 1), the following advantages are obtained: - inert (does not react chemically) when in contact with plastic materials, and / or - Improved corrosion resistance compared to low-alloy bulk materials (e.g. those with 5 wt. or less chromium) used in the manufacture of forming tools (e.g. tempered tool steels such as the heat-treatable cold work tool steels 1,2311 and 1,2312, hardened tool steels such as the hot work tool steels 1,2343 and 1,2344, nitrided steels such as the heat-treatable steels 1,7735, 1,8519 and 1,8550).

[0030] Preferably, the first embodiment achieves all the above listed advantages simultaneously.

[0031] According to a second further preferred embodiment of the invention, the coating 2 is deposited with a multilayer architecture comprising at least two layers, one of which is a Si-CN based layer 3 deposited as the outermost layer, preferably the top layer, as shown in Figure 2. In this case, as shown in Figure 2, the first layer 5 of the multilayer architecture can be deposited directly on the substrate surface 1. In the case shown in Figure 2, the first layer 5 is deposited between the substrate surface 1 and the Si-CN based layer 3. In this embodiment, it can be beneficial to deposit an adhesion layer 6 (not shown in Figure 2) between the substrate surface 1 and the first layer 5 of the multilayer architecture constituting the coating 2 in this embodiment, which adhesion layer 6 is used to improve the adhesion of the coating 2 to the substrate surface 1.

[0032] By providing a forming tool according to this second embodiment with a coating of the present invention (see, for example, FIG. 2), the following advantages are obtained: - inert (does not react chemically) when in contact with plastic materials, and / or - Improved corrosion resistance compared to the low-alloy bulk materials (e.g. Cr ≤ 5 wt.-%) used to manufacture the forming tools (see examples of typical forming tool materials above), and / or - the total coating hardness is increased by including a hard coating layer (e.g. a metal nitride layer) in the multi-layer structure forming coating 2, e.g. by including a PVD deposited nitride layer as the first layer 5 of coating 2, and / or -Improved contact pressure per unit area for hard particles in plastics.

[0033] Preferably, the second embodiment achieves all the above listed advantages simultaneously.

[0034] To better understand the term "improved contact pressure," the following example is provided:

[0035] For example, if the first layer 5 is thicker than 5 μm, preferably thicker than 10 μm, and harder than the top layer 3, then together with the first layer 5 a support for the top layer 3 (Si-CN-based layer 3) is provided. The plastic has, for example, hard particles. When molding the plastic with a coated molding tool, there is a risk that the hard particles of the plastic brake with the top layer 3, especially if there is no support under the top layer 3 and especially if the surface hardness of the bulk material does not exceed, for example, 550 HV. Due to the first layer 5 and preferably an additional nitride layer 4 (see FIG. 3 and / or 4 and the third preferred embodiment of the invention described below) on the substrate surface, the contact pressure per unit area can be improved, for example with respect to hard particles in plastic molding.

[0036] According to a third further preferred embodiment of the invention, the substrate surface 1 is treated such that a nitride layer 4 is formed on the surface of the substrate 10, the nitride layer 4 comprising the substrate surface 1. In this way, the coating 2 is deposited on the nitride layer 4 comprising the substrate surface 1 (as shown in FIG. 3). The coating 2 may advantageously be deposited on an adhesion layer 6 which is deposited on the nitride layer 4 comprising the substrate surface 1 (as shown in FIG. 4). The adhesion layer architecture shown in FIG. 4 appears to be useful and promising.

[0037] By providing a forming tool according to this third embodiment with a coating of the invention (see, for example, FIG. 3 or FIG. 4), the following advantages are obtained: Further improvement of the contact pressure per unit area for hard particles in the plastic (higher contact pressure compared to the embodiment shown in FIG. 2), and / or - improving the mechanical stability of the substrate-coating system by providing a better support effect of the coating on the forming tool substrate, which is usually steel with a hardness significantly lower than that of the coating (e.g. hardness of steel ≦550 HV); and / or - improved mechanical strength at high temperatures (the mechanical properties of the nitrided layer 4 are not impaired up to 500 ° C. and a high hardness is maintained even at a service temperature of 500 ° C.), and / or - Improved crack behavior / propagation (The propagation of cracks into the bulk has been improved. The cracks stop mostly in the nitrided layer 4, preferably at the end of the nitriding depth, due to the internal stresses induced with respect to the storage of nitrogen in the surface zone. The top layer 3 and the first layer 5 make the cracks flow preferably parallel to the surface and protect the substrate.)

[0038] Preferably, the third embodiment achieves all the above listed advantages simultaneously.

[0039] The inventors have found that the surprising forming tool coated or machined and coated according to any of the above-mentioned third preferred embodiments (see also Figures 3 and / or 4) can achieve a more significantly increased service life by depositing a coating 2 comprising at least one corrosion resistant layer (e.g. a hard thin film layer 5 exhibiting good corrosion resistance) deposited between the Si-CN based outermost layer 3 and the substrate surface 1 (in some cases the corrosion resistant layer 5 can be deposited, for example, between the Si-CN based outermost layer 3 and the adhesion layer 6 or between the Si-CN based layer 3 and the nitride layer 4 comprising the substrate surface 1).

[0040] The hard thin film layer 5 is preferably a metal nitride layer, a metal oxide layer, a metal oxynitride layer, a metal carboxynitride layer, or a metal carbonitride layer. The hard thin film layer 5 is preferably a metal nitride layer having the formula Me(C v N y O z ) qwhere Me is one or more elements selected from the group of elements consisting of chromium, aluminum, titanium, vanadium and molybdenum, the atomic fractions v, y and z of carbon, nitrogen and oxygen have values ​​in the ranges 0≦v≦1, 0≦y≦1, 0≦z≦1, respectively, such that v+y+z=1, and the molar concentration q of the non-metallic elements C, N and O per mole of the metallic element Me is in the range 0.76≦q≦1.2.

[0041] The corrosion-resistant layer is preferably a chromium nitride layer or a chromium nitride-based layer. In the context of the present invention, a chromium nitride-based layer is a layer containing chromium nitride, in which the sum of the chromium content and the nitrogen content in the chromium nitride-based layer constitutes more than 50% in atomic %, taking into account all elements present in the chromium nitride-based layer. The chromium nitride layer or chromium nitride-based layer used as a corrosion-resistant layer in the context of the present invention can be made to exhibit a single-layer structure or a multilayer structure. According to a preferred embodiment, the corrosion-resistant layer is made as a chromium nitride layer exhibiting a multilayer structure, the multilayer structure comprising at least two types of chromium nitride layers, preferably two different types of chromium nitride layers, for example a first type of chromium nitride layer and a second type of chromium nitride layer, one of the two types of chromium nitride layers containing more nitrogen than the other, and the different types of layers are deposited alternately with each other.

[0042] According to a preferred variant of the embodiment including a corrosion resistant layer, the Si-CN based layer 3 is deposited directly on the corrosion resistant layer.

[0043] According to a preferred variant of the embodiment comprising a corrosion-resistant layer, the latter is deposited directly on the substrate surface 1 or directly on the nitride layer 4 comprising the substrate surface 1 .

[0044] According to a further preferred embodiment of the present invention, a thermochemical diffusion layer having nitrogen and carbon as diffusing elements may be used as the corrosion resistant layer.

[0045] An example of a preferred embodiment using a thermochemical diffusion layer as the corrosion resistant layer and stainless steel or martensitic steel as the substrate material: For the treatment of austenitic and non-corrosive martensitic steels, the preferred variant for producing a thermochemical diffusion layer is by low-temperature nitriding or low-temperature nitrocarburizing or carburizing (low temperature in this context is, for example, a temperature in the range of 360°C to 460°C). The diffusing elements N and C produce nitrogen-expanded austenite and martensite at low temperatures, which improve pitting corrosion. By including a Si-CN based layer 3 on top of the thermochemical diffusion layer, the following improvements are achieved: o Further improving corrosion resistance, and / or o Improved contact pressure per unit area on hard particles in the plastic material (due to the high hardness of the nitrided zone, over 550HV), and / or o Improved mechanical stability by providing better support for the coating (e.g. Si-CN based layer 3) provided on the thermo-mechanical diffusion layer compared to the steel substrate, which preferably has a significantly lower hardness than the coating.

[0046] Another example of a preferred embodiment in which a thermo-mechanical diffusion layer is used as the corrosion resistant layer and a heat treatable steel, a carbon steel, a case hardened steel, a nitrided steel or a hot work steel is used as the substrate: • When treating such low alloy steels, the preferred variant for producing a thermochemical diffusion layer is nitrocarburizing with an Fe(N,C) nitride layer, preferably an epsilon nitride layer, as corrosion protection layer, or nitrocarburizing with post-oxidation with a composite epsilon nitride as corrosion protection layer. The Si-CN layer is preferably deposited directly on the epsilon nitride composite. The use of magnetite as corrosion protection layer is only optional. By including a Si-CN based layer 3 on top of the thermochemical diffusion layer, the following improvements are achieved: o Further improving corrosion resistance, and / or o Improved contact pressure per unit area on hard particles in the plastic material (due to the high hardness of the nitrided zone, over 550HV), and / or o improved mechanical stability by providing a better support for the coating (e.g., a Si-CN-based layer) provided on the thermomechanical diffusion layer compared to the steel substrate, which preferably has a significantly lower hardness than the coating, and / or o Improved mechanical strength at high temperatures, and / or o Improved crack behavior / propagation (the nitrided layer improves the propagation of cracks into the bulk material, with the advantage that the induced internal stresses generated by the nitrogen accumulated in the surface zone stop the cracking process), and / or o Reduces the tendency of mold tooling materials to adhere to molten plastics and non-ferrous metals such as aluminum and copper.

[0047] Preferably, the above-described embodiments achieve all the above-listed improvements simultaneously. The inventors have discovered that Si-CN based layers 3 deposited using Plasma Enhanced Chemical Vapor Deposition (PE-CVD) techniques (these techniques are also known as Plasma Assisted Chemical Vapor Deposition (PA-CVD) techniques) are particularly beneficial for improving tool performance and service life.

[0048] For the PE-CVD deposition of the Si-CN layer 3 of the invention, gases containing Si and C can be used. For example, hexamethyldisiloxane (HMDSO) in gaseous state can be used as a precursor and nitrogen in gaseous state can be used as a reactive gas to form the Si-CN based layer. The Si-CN layer deposited in this way exhibits a particularly low surface roughness. For example, in one example, the coating of the invention exhibits an architecture as shown in FIG. 1, where the substrate surface 1 exhibited an arithmetic mean roughness Ra=0.01 μm before coating and the arithmetic mean roughness obtained after coating was Ra=0.04 μm, where the Si-CN based layer 3 was produced with a total layer thickness of 8 μm by using PE-CVD as the method described above. In a further example, the coating of the invention exhibits an architecture as shown in FIG. 1, and the substrate surface 1 exhibits an arithmetic mean roughness Ra=0.01 μm before coating and the obtained arithmetic mean roughness after coating is Ra=0.02-0.03 μm, where the Si—CN based layer 3 was produced with a total layer thickness of 2-3 μm by using the PE-CVD method as described above.

[0049] However, the deposition of the Si-CN layer of the present invention is not limited to the above-mentioned method. The Si-CN layer of the present invention can also be deposited by any PVD or reactive PVD method, such as the following method: - a method of sputtering a target containing silicon, carbon and nitrogen in an atmosphere containing argon or in an atmosphere containing nitrogen-argon, or - A method of sputtering or arc-evaporating a target containing silicon and carbon in a nitrogen-containing atmosphere.

[0050] However, it should be understood that all of the above methods are exemplary and are not intended to limit the methods that may be used to deposit the Si-CN layers of the present invention.

[0051] In order to achieve better performance of the forming tool, the coated or treated and coated forming tool according to the invention can preferably be post-treated to achieve the desired surface quality. Some suitable post-treatments in this regard are, for example: - Polishing with abrasives of 1200 grit or higher, and / or -Glass bead blasting, and / or - Polishing with diamond paste.

[0052] The choice of architecture and elemental composition of the coating system used to improve the performance and service life of the forming tools according to the present invention may be selected depending on: -Type of plastic processing operation and / or type of plastic material being processed or -Type of aluminium processing operation and / or type of aluminium alloy being processed.

[0053] Example 1 of the present invention:

[0054] As a substrate, a wet calibration caliber for extrusion of window profiles was used.

[0055] The substrates used were hot work tool steels 1.2311 and 1.2316.

[0056] The substrate was introduced inside the coating chamber of a vacuum coating device for carrying out the coating process according to the invention. A coating was deposited on the substrate comprising two layers: a first layer 5 of chromium nitride and a second layer, a Si-CN based layer 3. The first layer 5 was deposited directly on the surface of the caliber intended to be in contact with the material to be processed. The contact material in contact with the Si-CN based layer 3 was polyvinyl chloride (PVC).

[0057] The chromium nitride layer (hereinafter also referred to as CrN layer) was deposited using a physical vapor deposition (PVD) technique, preferably of the reactive cathodic arc deposition type. The coating of the hard material (chromium nitride) is preferably carried out in a PVD system (arc PVD or magnetron PVD system). For the deposition of the first layer 5, a chromium target was evaporated in a nitrogen-containing atmosphere and a bias voltage was applied to the calibre, preferably a bias voltage of at least 50 V, preferably a bias voltage of up to 300 volts, preferably a bias voltage of 50-300 V.

[0058] Before and during the deposition of the first layer 5 (in this example: a chromium nitride layer deposited by reactive cathodic arc PVD), the following process steps were carried out.

[0059] 1. Pump to high vacuum 2. Heating by thermal radiation up to 400℃ 3. Sputter cleaning by argon ion / metal ion bombardment 4. In a reactive cathodic arc deposition process, a chromium target acts as the cathode and a nitrogen-argon gas mixture flow is used as the process / reactive gas during this step, and a bias voltage is applied to the substrate.

[0060] The second layer 3 was deposited as the outermost layer using PE-CVD. The deposition of the second layer 3 is preferably carried out in a plasma nitridation system. For the deposition of the second layer, HMDSO in gaseous state was used as a precursor, nitrogen gas was introduced into the coating chamber, and the deposition temperature (temperature of the substrate surface to be coated during the deposition process) was maintained at a value between 360°C, preferably 380°C and 450°C, preferably 480°C.

[0061] After the deposition of the first layer 5, the second layer (in this example: during deposition of a Si-CN based layer deposited by PE-CVD 3) was subjected to the following process steps:

[0062] 5. Switch off the chrome target, stop the flow of gas into the coating chamber, and apply a vacuum to the coating chamber.

[0063] 6. Introduction of a mixed gas flow of hydrogen, nitrogen, and argon (mixed gas flow of H2, N2, Ar) into the coating chamber.

[0064] 7. Increase the substrate bias voltage to a value in the range of 500 V-600 V to initiate a glow discharge directly on the substrate (sample or forming tool).

[0065] 8. Start the HMDSO vaporizer and add 5% HMDSO to the mixed gas stream of H2, N2, and Ar.

[0066] The second layer thus deposited is Si a C b N c X d type Si-CN based layer 3, where X is the element of hydrogen (H) and oxygen (O), and the coefficient d corresponds to the sum of the H content and the O content in the Si-CN based layer 3 expressed in atomic %. Therefore, the elemental composition of this type of Si-CN based layer 3 can be expressed as follows:

[0067] S a C b N c H d1 O d2 , where d1+d2=d

[0068] In the test of this embodiment, the composition of the obtained Si-CN-based layer is specifically as follows: S 28 C 29 N 12 H 19 O 12

[0069] The CrN layer in this example has a multilayer structure Cr / CrN / Cr / CrN... and is deposited with a multilayer layer thickness of 6-8 μm or with a multilayer layer thickness of 8-10 μm (preferred thickness range of such a CrN layer or other type of first layer is: 1-10 μm).

[0070] Preferably, layers with a thickness of more than about 8 μm with very good adhesive strength can be deposited on the substrate 10 of the forming tool (see FIG. 1), preferably at about 480° C. The hardness of these layers is preferably of the order of 5000 HV0.1.

[0071] The corrosion resistance of the approximately 2 μm thick layer is preferably 144-188 h in a salt spray test. The tested architecture of this preferred embodiment is depicted in Figure 1. The corrosion resistance of the thicker layer is believed to be at least as good as the 2 μm thick layer, preferably it is more corrosion resistant, but is currently under testing.

[0072] According to a preferred embodiment of the CrN layer having a multi-layer structure, the stacking of layers preferably always starts with Cr, followed by CrN, and then stacking these stacks, for example 5. The ratio of Cr to CrN is preferably 1 / 5.

[0073] In this embodiment, the Si-CN based layer 3 is deposited to a thickness of 1 to 2 μm, but the preferred thickness range of such a Si-CN based layer is 1 to 10 μm.

[0074] The coated caliber showed no signs of corrosion even after 48 hours of use.

[0075] The description and claims of priority application US62 / 853,969 filed on May 29, 2019, on which this application is based, preferably form an integral part of this application.

[0076] As described in this description, one main objective is to deposit a layer on tools used in the plastic and aluminum processing industries. Specifically, heretofore, it has been studied to qualify the "Si-C-N based layer directly on the nitride layer" in the application temperature range of 360 °C to 480 °C. PE-CVD or PA-CVD can be a preferred technique for the deposition of the Si-C-N layer. It may be preferable to treat the layer with glass beads or diamond paste. As described in one of the foregoing embodiments, it is preferable to first perform the deposition process in two different plants, for example, deposit a coating of a hard material (chromium nitride) with a PVD system (arc PVD or magnetron PVD system), and then perform the deposition of Si-C-N with a plasma nitriding system. The above-described architecture of the adhesion layer shown in FIG. 4 can be useful and promising.

[0077] Regardless of the claims, protection is also sought for the following items.

[0078] A coated forming tool for processing plastic materials or aluminum or aluminum alloy materials, comprising a substrate 10 having a substrate surface 1, the substrate surface 1 being coated with a coating 2 formed of one or more layers, the coating having 50 < a + b + c ≦ 100, 0 ≦ d < 50, preferably 0 ≦ d < 50 of Si

[0079] C a C b N c X d% according to the present invention, characterized in that X is one or more elements selected from the group of elements constituted by the non-metallic elements hydrogen and oxygen, and the metallic elements titanium, chromium and aluminum.

[0080] A coated forming tool according to the preceding paragraph, characterized in that the coating is formed in several layers, the Si-CN based layer 3 being deposited as the outermost layer.

[0081] A coated forming tool according to any one of the preceding paragraphs, characterised in that the substrate surface 1 comprises a nitride layer 4 on which the coating 2 is deposited.

[0082] A coated forming tool according to any one of the preceding paragraphs, characterized in that the coating 2 comprises a hard thin film layer 5 deposited between the substrate surface 1 and the silicon carbonitride layer 3.

[0083] The hard thin film layer 5 is a metal nitride layer, or a metal oxide layer, or a metal oxynitride layer, or a metal carboxynitride layer, or a metal carbonitride layer, the layer having the formula Me(C v N y O z ) q where Me is one or more elements selected from the group of elements formed by chromium, aluminum, titanium, vanadium and molybdenum, the atomic fractions v, y and z of carbon, nitrogen and oxygen have values ​​in the ranges 0≦v≦1, 0≦y≦1, 0≦z≦1, respectively, such that v+y+z=1, and the molar concentration q of the non-metallic elements C, N and O per mole of the metallic element Me is in the range 0.76≦q≦1.2.

[0084] A coated forming tool according to any one of the preceding paragraphs, characterized in that an adhesive layer 6 is deposited between the substrate surface 1 and the coating 2.

[0085] 10. Coated forming tool according to claim 1, characterized in that the Si-CN based layer 3 contains, in addition to silicon, carbon and nitrogen, hydrogen and oxygen.

[0086] 13. A method for manufacturing a coated forming tool according to any one of the preceding paragraphs, characterized in that the silicon carbonitride layer is deposited by means of a PE-CVD technique, using a Si-containing gas as precursor.

[0087] The method of the preceding paragraph, wherein the Si-containing gas is hexamethyldisiloxane (HMDSO).

[0088] A method according to any one of the two preceding paragraphs, characterized in that prior to the deposition of the silicon carbonitride layer 3, the substrate 10 to be coated is subjected to a plasma nitridation process to form a nitride layer 4 comprising the substrate surface 1 on which the coating 2 is deposited.

[0089] 20. Use of a coated forming tool according to any one of the preceding paragraphs in plastics processing operations.

[0090] 2. Use according to the preceding paragraph, characterized in that the plastic processing operation is plastic injection molding.

[0091] 2. Use of a coated forming tool according to any one of the preceding paragraphs in aluminium or aluminium alloy processing operations.

[0092] 2. Use according to the preceding paragraph, characterized in that the plastic processing operation is aluminium die casting or aluminium alloy die casting.

Claims

1. A coated forming tool for processing plastic materials or aluminum or aluminum alloy materials, the forming tool comprising a substrate (10) having a substrate surface (1) and used for plastic injection molding or aluminum or aluminum alloy die casting, the substrate surface (1) being coated with a coating (2) formed of one or more layers, the coating (2) being a Si(II) having a content of 50<a+b+c≦100, 0≦d<60, preferably 0≦d<50. a C b N c X d wherein X comprises hydrogen and oxygen; The coating (2) includes a hard thin film layer (5) deposited between the substrate surface (1) and the Si-C-N based layer (3); The hard thin-film layer (5) is a metal nitride layer, or a metal oxide layer, or a metal oxynitride layer, or a metal carboxynitride layer, or a metal carbonitride layer, the hard thin-film layer (5) having a chemical composition in atomic % corresponding to the formula Me(CvNyOz)q, where Me is aluminum, the atomic fractions v, y, and z of carbon, nitrogen, and oxygen have values ​​in the ranges 0≦v≦1, 0≦y≦1, 0≦z≦1, respectively, v+y+z=1, and the molar concentration q of the non-metallic elements C, N, and O relative to 1 mol of the metallic element Me is in the range 0.76≦q≦1.

2.

2. 2. The coated forming tool of claim 1, wherein X comprises titanium, or chromium, or aluminum, or a combination of titanium, chromium and / or aluminum.

3. 3. The coated forming tool of claim 1, wherein X is one or more elements selected from the group of elements formed by the nonmetallic elements hydrogen and oxygen, and the metallic elements titanium, chromium, and aluminum.

4. A coated forming tool according to any one of claims 1 to 3, characterized in that the coating (2) is formed in several layers, a Si-C-N based layer (3) being deposited as the outermost layer.

5. A coated forming tool according to any one of claims 1 to 4, characterised in that the substrate surface (1) comprises a nitride layer (4) on which the coating (2) is deposited.

6. A coated forming tool according to any one of claims 1 to 5, characterised in that an adhesion layer (6) is deposited between the substrate surface (1) and the coating (2).

7. 7. Method for manufacturing a coated forming tool according to any one of claims 1 to 6, characterized in that the Si-C-N based layer (3) is deposited by means of a PE-CVD technique, using a Si-containing gas as precursor.

8. 8. The method of claim 7, wherein the Si-containing gas is hexamethyldisiloxane (HMDSO).

9. 9. A method according to claim 7 or 8, characterized in that, prior to the deposition of a silicon carbonitride layer (3), the substrate (10) to be coated is subjected to a plasma nitridation process for forming a nitride layer (4) comprising the substrate surface (1) on which the coating (2) is deposited.

Citation Information

Patent Citations

  • Member coated with diamond-like carbon film

    JP2000178738A

  • Thin film for molding mold, and mold

    JP2001277251A

  • Advanced high-speed steel tool

    JP2004283995A

  • Member for casting