Optical coating with nanolaminate for increased durability
Nanolaminate structures in optical coatings address the durability and scratch resistance issues of traditional ARCs, offering enhanced mechanical properties suitable for mass production and maintaining optical performance.
Patent Information
- Application Number
- JP2019566192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-04-02
- Filing Date
- 2018-06-01
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2038-06-01
AI Technical Summary
Existing anti-reflective coatings (ARCs) used in applications like eyeglasses, flat glass, and flat screen displays lack sufficient durability and scratch resistance, leading to visible defects and reduced functionality, especially in portable devices.
The development of optical coatings utilizing nanolaminate structures composed of alternating nanolayers of different materials with controlled refractive indices, formed through methods like sputtering, to enhance durability and scratch resistance while maintaining optical performance.
The nanolaminate structures provide improved mechanical properties, including increased corrosion, abrasion, and scratch resistance, enhancing the durability of optical coatings without compromising their optical properties, suitable for mass production at acceptable costs.
Smart Images

Figure 0007587801000001 
Figure 0007587801000002 
Figure 0007587801000003
Abstract
Description
[Technical field]
[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims priority to U.S. Provisional Patent Application No. 62 / 513,933, filed June 1, 2017, and U.S. Provisional Patent Application No. 62 / 651,617, filed April 2, 2018, the disclosures of which are incorporated herein by reference in their entireties.
[0002] [Technical field] FIELD OF THE DISCLOSURE This disclosure relates generally to the field of optical coatings, such as anti-reflective coatings, and the preparation of such optical coatings. [Background technology]
[0003] Anti-reflective coatings (ARCs) are used in many applications, such as eyeglasses, glass panes (e.g., car windshields), flat screen displays, and touch screens. For many of these applications, the requirements for ARCs include efficient anti-reflective properties at visible wavelengths, high transparency, and durability. Obviously, these properties must be obtained at a commercially acceptable cost.
[0004] Generally, there are two methods for forming ARCs on a substrate: wet and dry. Dry methods use deposition or sputtering techniques to deposit multiple thin layers of alternating high and low refractive index. This method provides excellent adhesion at the layer interfaces and very precise control of layer thickness, but requires relatively high manufacturing costs. Wet methods involve coating the substrate with a wet solution followed by drying of the solvent. This method also results in the formation of alternating layers of low and high refractive index, so the process must be repeated and results in relatively poor adhesion at the layer interfaces compared to dry methods.
[0005] Examples of wet and dry methods for forming ARCs are described, for example, in US Pat. Nos. 5,393,963, 5,496,133, 5,597,222, 5,633,362, and 5,741,623.
[0006] One problem with conventional ARCs is that most high volume, cost-competitive methods for forming ARCs do not produce coatings that are scratch or abrasion resistant enough for use in devices that are used continuously or in harsh environments. Portable devices such as cell phones are an example of an application that is not suited for conventional ARC coatings. The reason for this is that any damage to the ARC will cause the light emitted by the screen to be refracted so much that it will cause very noticeable failure of the device. This very noticeable failure will negate the anti-reflective benefit of the AR coating. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] U.S. Pat. No. 9,482,789 [Patent Document 2] U.S. Pat. No. 8,358,467 [Patent Document 3] U.S. Patent No. 6,532,112 [Patent Document 4] U.S. Pat. No. 5,106,671 Summary of the Invention [Problem to be solved by the invention]
[0008] Therefore, there is a need in the art for an improved ARC that can be used in, for example, flat panel displays and touch screens. [Means for solving the problem]
[0009] The following summary of the present disclosure is included to provide a basic understanding of some aspects and features of the present invention. This summary is not an extensive overview of the invention, and as such is not intended to particularly identify key or critical elements of the invention or to delineate the scope of the invention. Its sole purpose is to present some concepts of the invention in a simplified form as a prelude to the more detailed description that is presented below.
[0010] In the disclosed embodiments, improved optical coating structures are provided that have improved optical and mechanical properties, especially high durability and scratch resistance, and use fabrication methods that are feasible in mass production at acceptable commercial costs.
[0011] In disclosed embodiments, optical coatings, such as ARCs, are formed using multiple superlattices, also referred to as nanolaminates, each having nanolayers of alternating refractive index to form an improved ARC structure. Each superlattice is composed of at least two nm-scale layers (i.e., one bilayer) of alternating composition and / or crystal phase, but with corresponding refractive index. Multiple superlattices are stacked with alternating effective refractive indexes. The effective refractive index of a superlattice is the average refractive index of the two nanolayers of the bilayer, weighted by the thickness of the nanolayer. In disclosed embodiments, each of the nanolayers is of a thickness of 30 nanometers or less, more specifically in the range of 2-10 nm. In some embodiments, the entire ARC structure is made from nanolayers. In other embodiments, a standard ARC layer is formed and one, typically the last optical layer, is made from multiple nanolayers to form a hard cap layer.
[0012] In a general aspect, an optical coating is provided that includes a plurality of low refractive index layers, each having a first refractive index, and a plurality of high refractive index layers, each having a second refractive index greater than the first refractive index, the low refractive index layers and the high refractive index layers interdigitated in combination to form a laminate, and at least one layer selected from the low refractive index layers and the high refractive index layers includes a nanolaminate layer made from alternating nanolayers of two different materials.
[0013] Disclosed embodiments include a method of forming an optical coating, the method including the steps of providing a transparent substrate and forming a plurality of transparent layers on the substrate by forming a first refractive index layer having a first refractive index and a second refractive index layer having a second refractive index multiple times, the forming the plurality of transparent layers including forming at least one layer by placing the transparent substrate in a sputtering chamber and operating the sputtering chamber to form at least one bilayer of two nanolayers of different materials, each of the nanolayers having a thickness of 2-10 nanometers, each of the nanolayers being formed by sputtering material from a target while simultaneously injecting oxygen ions or nitrogen ions into the nanolayer formed on the substrate. Additionally, the method can include forming a seed layer directly on the substrate prior to forming the plurality of transparent layers. Additionally, the method can include forming a diamond-like coating on the plurality of transparent layers. Additionally, the method can include forming a silicon layer on the diamond-like coating, forming a silicon oxide layer on the silicon layer, and forming an anti-fingerprint layer on the silicon oxide layer. The method may further include selecting the different materials having refractive indices n1 and n2 such that the different materials satisfy the relationship (n1-n2) / (n1+n2)≦0.07. f -n s ) / (n f +n s ) ≧0.10, f is the effective refractive index of the bilayer, and n smay include forming the plurality of transparent layers such that the refractive index is one of the first refractive index or the second refractive index.
[0014] Other aspects and features of the present invention will become apparent from the following detailed description taken in conjunction with the drawings, which should be understood to illustrate various non-limiting examples of various embodiments of the invention as defined by the appended claims.
[0015] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate embodiments of the invention and, together with the detailed description, serve to explain and illustrate the principles of the invention. The drawings are intended to show main features of exemplary embodiments in a schematic manner. The drawings are not intended to show all features of actual embodiments or the relative dimensions of the elements shown, and are not drawn to scale. [Brief description of the drawings]
[0016] [Figure 1] In FIG. 1, FIG. 1A shows a prior art ARC structure disclosed in Patent Document 3, and FIGS. 1B to 1D show a modified ARC structure in an embodiment of the present invention. [Diagram 2] In FIG. 2, FIGS. 2A-2C show a process for forming an optical coating in one embodiment. [Figure 3A] FIG. 3A shows a further embodiment of an optical coating. [Figure 3B] FIG. 3B illustrates a further embodiment of an optical coating. [Figure 3C] FIG. 3C illustrates a further embodiment of an optical coating. [Figure 3D] FIG. 3D shows an embodiment having a protective stack of DLC and an anti-fingerprint layer with an intermediate protective adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Embodiments of the inventive optical coating and its preparation will now be described with reference to the drawings. Various embodiments or combinations thereof can be used for various applications or to obtain various advantages. The various features disclosed herein can be used in part or in whole alone or in combination with other features, balancing the advantages with requirements and constraints, depending on the results to be obtained. Thus, certain advantages are emphasized in various embodiments, but are not limited to the disclosed embodiments. That is, the features disclosed herein are not limited to the embodiments in which they are described, but can be "mixed" with other features and incorporated into other embodiments.
[0018] Disclosed embodiments include methods of forming optical coatings having nanolaminate structures. In the context of this disclosure, a nanolaminate is an alternating nanolayer of different composition, each nanolayer having a thickness of 30 nm or less. Various disclosed embodiments have shown beneficial results when each nanolayer is as thin as 2-10 nm. The corrosion, wear, scratch, and hardness properties of nanolaminate structures are particularly better than those of individual or laminated films having a thickness greater than 30 nm.
[0019] In the disclosed embodiments, the ARC layer can be formed on a variety of crystalline or non-crystalline substrates, such as glass (including treated glasses such as Gorilla Glass), sapphire, and plastic, however, in the disclosed embodiments, the layer is formed while maintaining the substrate at a temperature of 300° C. or less.
[0020] FIG. 1A shows an ARC structure disclosed in US Pat. No. 5,999,333, and FIG. 1B-D show modified ARC structures according to embodiments of the present invention. As disclosed in the prior art, the ARC layers shown in FIG. 1A are made of alternating layers of oxide materials with different refractive indices. Thus, in the example of FIG. 1A, layers 2 and 4 are made of SiO2, which has a refractive index of 1.45-1.50, while layers 3 and 5 are made of NbO, which has a refractive index of 2.1-2.3. This arrangement is capped with an ITO layer, which has a refractive index of 1.9-2.1 at 520 nm wavelength.
[0021] In the disclosed embodiment, at least one of the ARC layers is replaced with a superlattice made of alternating nanolayers of material having a refractive index similar to that of the layer it replaces, improving the performance of the ARC structure. FIG. 1B shows an example where an ITO cap layer 1 is replaced by a superlattice nanolaminate of multiple nanolayers 1′. ITO layers are reported to have a refractive index between 1.9 and 2.1. Hence, in this example, the nanolayers are selected to have similar refractive indices. In one embodiment, the ITO layer 1 is replaced by 10 alternating nanolayers of SiN and AlN, each having a thickness of 2.5 nm, for a total thickness of 25 nm. SiN has a refractive index of 2.05 at a wavelength of 520 nm. AlN has a refractive index of 2.15 at a wavelength of 520 nm. The nanolaminate layer 1′ may improve mechanical properties, making the ARC structure more durable, and has an effective refractive index of 2.10 similar to that of the ITO it replaces, as shown below.
[0022] FIG. 1C shows an embodiment in which layer 2 is replaced by nanolaminate structure 2′. Layer 2 is reported to have a refractive index of 1.45-1.50 at 520 nm wavelength. Hence, in this example, the nanolayers are selected to have similar refractive indices. In this example, nanolaminate structure 2′ is made of 16 alternating layers of SiO and Al2O3, each 2.5 nm thick, for a total of 40 nm. SiO has a reported refractive index of 1.46 at 520 nm wavelength, while Al2O3 has a reported refractive index of 1.77 at 520 nm wavelength. However, when these films are formed using sputtering, as recommended in this disclosure, SiO has a refractive index of 1.48-1.50, while Al2O3 has a refractive index of 1.65-1.67, resulting in an effective refractive index of 1.57 (see calculation below).
[0023] Although Figures 1B and 1C each show an embodiment in which only one layer is replaced with a nanolaminate, any number of layers in the disclosed embodiments can be replaced with a nanolaminate of material having a similar refractive index, and in fact, in some embodiments, all layers can be replaced, as shown in the example of Figure 1D.
[0024] In the example of FIG. 1D, ITO cap layer 1 is replaced by nanolaminate layer 1′ made of 10 alternating nanolayers of SiN and AlN, each 2.5 nm thick, for a total thickness of 25 nm. Layer 2 is replaced by nanolaminate layer 2′ made of 16 alternating layers of SiO and Al2O3, each 2.5 nm thick, for a total thickness of 40 nm. Layer 3 is replaced by nanolaminate layer 3′ made of 20 alternating nanolayers of SiN and AlN, each 3 nm thick, for a total thickness of 60 nm. Layer 4 is replaced by nanolaminate layer 4′ made of 10 alternating layers of SiO and Al2O3, each 2.5 nm thick, for a total thickness of 25 nm. Layer 5 is replaced by nanolaminate layer 5′ made of 6 alternating nanolayers of SiN and AlN, each 3 nm thick, for a total thickness of 18 nm.
[0025] The materials for each layer of the nanolaminate must be carefully selected. To function as an optical coating, the refractive index of the low AR layer nanolaminate stack must be as low as possible, and the refractive index of the high AR layer nanolaminate stack must be as high as possible. However, refractive index is not the only important property. For a robust nanolaminate stack, the hardness, shear modulus, and stress of the individual nanolayers are also important. High index nanolayers can be made from a combination of ZrO, Y-ZrO, AlN, SiN, ZrN, TiO, CrO, CrN, CrTiO, and CrTiN (stoichiometric and non-stoichiometric) optical films. Low index nanolayers can be made from a combination of SiO, AlO, SiON, and SiAlO films.
[0026] It should be understood that in this context, the terms low index and high index are not used as quantitative measurements, but rather as relative descriptors that allow for distinction between alternating layers. What is important in the context of ARC is not the particular value of the refractive index, but that the low index layers have a refractive index value sufficiently lower than that of the high index to provide the required optical effect.
[0027] It is also important that the refractive index of the nanolayers is appropriate for their purpose in the optical stack. For each of the high and low nanolayers, the closer the refractive index of the materials in the two alternating nanolayers, the better the optical performance. In fact, if the refractive index of the two nanolayers in a nanolaminate is equal, there will be no photodegradation since the amount of light reflected at the optical interface is proportional to (n1-n2) / (n1+n2). The result of (n1-n2) / (n1+n2) should preferably be less than 0.07 for the nanolayers within the nanolaminate layer and greater than 0.1 between the high and low nanolaminate stacks.
[0028] Looking at the example of FIG. 1D, the difference in refractive index of the high index nanolaminate (e.g., layers 1′, 3′, and 5′) is (n1-n2) / (n1+n2)=(2.15-2.05) / (2.15+2.05)=0.02. The difference in refractive index of the low index nanolaminate using the reported values is (n1-n2) / (n1+n2)=(1.77-1.46) / (1.77+1.46)=0.09, which exceeds the required 0.07. It is therefore advantageous to form the layers by sputtering, as described herein. Using the sputtering values, we obtain (n1-n2) / (n1+n2)=(1.67-1.48) / (1.67+1.48)=0.06, which is within the required 0.07. The difference between the high and low index is calculated taking into account the thickness ratio of the two layers. Nanolaminate 1' has an effective refractive index of [(t1×n1)+(t2×n2)] / (t1+t2), where t=thickness, i.e. [(2.5×2.05)+(2.5×2.15)] / 5=2.10. The effective refractive index of layer 2' is [(2.5×1.48)+(2.5×1.67)] / 5=1.57. Hence the difference between these two layers is (n1-n2) / (n1+n2)=(2.10-1.57) / (2.10+1.57)=0.14.
[0029] Incidentally, in the example of Figures 1B-1D, all the nanolayers in the nanolaminate have the same thickness, but this is not necessarily the case. As an example, the effective refractive index of layer 1' can be increased by making the AlN nanolayer thicker than the SiN nanolayer. As an example, the AlN can be set to 6 nm and the SiN to 3 nm, in which case the effective refractive index is [(3 x 2.05) + (6 x 2.15)] / 9 = 2.12. Similarly, to decrease the effective refractive index of layer 2', it can be set to [(5.5 x 1.46) + (2.0 x 1.67)] / 7.5 = 1.52.
[0030] As can be seen from the above disclosure, each nanolaminate comprises multiple nanolayers of two different materials with similar refractive indexes, which are stacked one on top of the other.Therefore, it can be said to be a bilayer, and each bilayer is a stack of two nanolayers of different materials but with similar refractive indexes.In this context, similar refractive index means that the refractive index value of one layer in a bilayer of a nanolaminate is closer to the refractive index value of the other nanolayer in the bilayer than the refractive index of a nanolayer in a different nanolaminate.That is, the two materials in the bilayer of a low refractive index nanolaminate have refractive index values closer to each other than the refractive index of any bilayer of a high refractive index nanolaminate.
[0031] Typically, the bilayer is made of nanolayers, each having a thickness of 2-10 nanometers, to improve the corrosion resistance, wear resistance, scratch resistance, and hardness of the coating. The bilayer is used to form multiple nanolaminates with alternating refractive index to obtain the desired optical effect. In some embodiments, a reflective coating is formed. The reflective coating can be formed, for example, on the back side of the mobile device. In this case, the optical stack is designed to reflect the desired color so that the mobile device appears colored. The reflective coating is designed in a half-wave (1 / 2λ) stack. Meanwhile, the anti-reflective coating is formed on the display side of the mobile device to eliminate or reduce light reflection from the screen. The anti-reflective coating is designed in a quarter-wave stack (1 / 4λ). The wavelength is the wavelength that the stack is intended to reflect. Therefore, multiple nanolaminates need to be formed with various thicknesses to form an effective ARC that reflects a wide range of wavelengths.
[0032] In the disclosed embodiments, the nanolayers are made of metal oxides, nitrides, or oxynitrides. Some examples are YsZ, Al x O y , AlN, Si x N y, AlSiO, and SiON. In some embodiments, an adhesion or seed layer is deposited first, which may be of materials such as ITO, SnxOy, and WOx. Also, in a preferred embodiment, the various layers are formed using ion beam assisted deposition (IBAD) such that the target material is made of the metal to be deposited and oxygen or nitrogen is ion-implanted during deposition. Thus, the sputtering process is performed in metal mode (also called meta mode), where the target is typically sputtered as a (non-oxidized) metal by argon ions, and a very thin film (typically about 1 nm) formed on the substrate is converted to an oxide or nitride by bombarding the deposited metal with an O2 or N2 ion beam. As an example, the sputtering target may be made of pure silicon or aluminum, while the ion beam contains O2 or N2, with or without argon, to form layers such as SiO, SiN, AlO, etc. Also, in a preferred embodiment, the ratio ion current to atom arrival rate is less than 0.5 and the ions have a potential energy of 600 eV or less.
[0033] In some embodiments, the refractive index of any layer can be modified by alloying the materials. As an example, MgO can be used to alloy a high refractive index material such as ZrOx or a low refractive index material such as AlOx. Alloying can be done by adding about 8-10% MgO, which will lower the crystallization temperature of the layer. In another example, about 10-12% chromium can be alloyed with titanium to improve toughness. Anatase, one of the three mineral forms of titanium dioxide, has a high refractive index of 2.4 but low hardness, making it a good candidate for alloying. Titanium itself can be used as an alloying agent to modify the refractive index. Tantalum can be an alloying agent to modify the properties of high refractive index materials, while boron can be an alloying agent to modify the properties of low refractive index materials.
[0034] 2A-2C illustrate a process for forming an optical coating in one embodiment. In FIG. 2A, the process can begin with treating a surface of a substrate 200, for example, using plasma or ion bombardment. The plasma or ion bombardment can include argon or hydrogen species. In FIG. 2B, a seed layer 205 is formed on the surface of the substrate 200 to set the crystal growth pattern and / or improve adhesion. The seed layer 205 can be of materials such as ITO, SnxOy, and WOx, and is formed using ion beam assisted deposition. In FIG. 2C, a nanolaminate layer 210 is formed on the seed layer 205.
[0035] Turning now to FIG. 3A, an optical coating, in this example ARC, is shown, which is made partially from standard layers and partially from nanolaminates. In this example, the substrate 300 can be glass, such as the front glass of a mobile phone or other cellular device or touch screen. When applied to the glass of a display, ARC can increase battery life and improve the visibility of the display in bright light. However, scratches in the coating can cause areas of the device that are difficult to see. This cosmetic damage is very visible, making the use of these films undesirable in high wear and high use applications. Also, the stresses in the films used in the prior art optical stacks can be very large. If the device is dropped or impacted against the glass surface, this can result in increased breakage. Breakage is a significant cause of warranty returns for mobile device manufacturers, and the risk of increased breakage makes the use of the films undesirable for manufacturers. Thus, the embodiment of FIG. 3A is provided to increase the durability of coatings and can be used in display devices.
[0036] The coating of FIG. 3A includes multiple layers of alternating high and low refractive indices. The first layer is a thin, high refractive index conventional layer 305 having a thickness of 10 nm. This layer, and all remaining high n layers, are made of Si3N4, which has a refractive index of 2.02. The second layer 310 is a 40 nm low refractive index conventional layer, in this case made of SiO2, which has a refractive index of 1.48. This is followed by a 30 nm high n layer 315, a 25 nm low n layer 320, a 100 nm high n layer 325, a 10 nm low n layer 330, and a 50 nm high n layer 335. All high n layers are made of Si3N4 and all low n layers are made of SiO2. Traditionally, the last layer is a low n layer, for example a 100 nm SiO2 layer. 3A embodiment, however, the top layer is made from a nanolaminate of ten bilayers, each bilayer made from a 5 nm nanolayer of SiO2 and a 5 nm nanolayer of a material having a refractive index closer to that of SiO2 than to that of Si3N4, in this example Al2O3, which has a refractive index of 1.67 when formed by sputtering. That is, the effective refractive index of top layer 340 is [(5×1.48)+(5×1.67)] / 10=1.57, which is closer to the low index of SiO2 than to the high index of Si3N4.
[0037] Thus, in general, the embodiment of FIG. 3A provides an optical coating comprising a plurality of first layers having a first refractive index and a plurality of second layers having a second refractive index different from the first refractive index, the plurality of first layers and the plurality of second layers being alternately formed to be combined on a substrate, terminating in a layer from the plurality of second layers, on which a top layer is formed comprising a nanolaminate having a plurality of bilayers, each bilayer comprising two nanolayers of different materials such that the effective refractive index of the top layer has a value closer to the first refractive index than to the second refractive index. The two different materials are selected to satisfy the formula (n1-n2) / (n1+n2)≦0.07, where n1 and n2 are the refractive indices of the two different materials. The resulting effective refractive index of the top layer, n eff is the formula |(n eff -n s ) / (n eff +n s )|≧0.10, where ns is preferably the second refractive index.
[0038] FIG. 3B shows another embodiment of an optical coating that can replace the structure of FIG. 3A. The embodiment of FIG. 3B can not only increase durability but also change the effective refractive index of the low index layer. Specifically, in FIG. 3B, all high n layers are standard layers, while all low n layers are nanolaminates. Layer 311 is made of four bilayers, each bilayer having a 5 nm nanolayer of SiO2 and a 5 nm nanolayer of Al2O3 for a total of 40 nm. Layer 321 is made of three 5 nm nanolayers of SiO2 combined with two 5 nm nanolayers of Al2O3 for a total of 25 nm. Layer 331 is made of one bilayer having a 5 nm nanolayer of SiO2 and a 5 nm nanolayer of Al2O3 for a total of 10 nm. Layer 340 is made of ten bilayers, each bilayer having a 5 nm nanolayer of SiO2 and a 5 nm nanolayer of Al2O3 for a total of 100 nm. That is, when using the standard ARC layer, high n was 2.02 and low n was 1.48, whereas in the embodiment of FIG. 3B, high n is still 2.02 but low n is 1.57.
[0039] Alternatively, to keep the low index close to that of SiO2, the bilayer can be made of SiO2 and SiON. SiON is formed by adding a nitrogen-containing gas flow such as N2O. Depending on the N2O flow during formation, the index of refraction of SiON can be adjusted from 1.46 to 1.56. Thus, even at the high end, we obtain (1.56-1.46) / (1.56+1.46)=0.03, which is well within the required 0.07. Similarly, the bilayer can be made of SiO2 and SiAlO. Since SiAlO has a refractive index of about 1.50, we obtain (1.50-1.46) / (1.50+1.46)=0.01, which is well within the required 0.07.
[0040] Thus, in general, the embodiment of FIG. 3B provides an optical coating that includes a plurality of first layers having a first refractive index, n1, and a plurality of second layers having a second refractive index, n2, different from the first refractive index, the plurality of first layers and the plurality of second layers being alternately formed to be assembled on a substrate, each of the plurality of second layers including a nanolaminate having at least one bilayer, each bilayer being arranged such that the effective refractive index of each nanolaminate is equal to the second refractive index, i.e., n eff = n2. In this regard, the effective refractive index is given by the formula |(n eff -n1) / (n eff + n1)|≧0.10. The effective refractive index is the weighted average of the refractive indices of the nanolayers, n eff = [(t3×n3)+(t4×n4)] / (t3+t4), where t3 and t4 are the thicknesses of each nanolayer, and the first and second nanolayers are selected to satisfy the formula (n3-n4) / (n3+n4)≦0.07.
[0041] Further examples of optical coatings are shown in FIG. 3C. In the embodiment of FIG. 3C, all layers are nanolaminates. The low-n laminates are similar to those described with respect to FIG. 2B, but the high-n layers are also replaced with nanolaminates. In this example, the first layer 306 is a bilayer of one 5 nm AlN nanolayer and one 5 nm Si3N4 nanolayer. Layer 316 is a nanolaminate of three bilayers, each bilayer made of one 5 nm AlN nanolayer and one 5 nm Si3N4 nanolayer. Layer 326 is a nanolaminate of ten bilayers, each bilayer made of one 5 nm AlN nanolayer and one 5 nm Si3N4 nanolayer. Layer 336 is a nanolaminate of five bilayers, each bilayer made of one 5 nm AlN nanolayer and one 5 nm Si3N4 nanolayer, so the effective refractive index of the high-n laminate is [(5×2.02)+(5×2.15)] / 10=2.085.
[0042] Thus, in general, the embodiment of FIG. 3C provides an optical coating including a plurality of first layers having a first refractive index and a plurality of second layers having a second refractive index different from the first refractive index, the plurality of first layers and the plurality of second layers being alternately formed to be combined on a substrate, each of the plurality of first layers including a first nanolaminate having at least one bilayer made from two nanolayers of different materials, and configured such that the effective refractive index of the first nanolaminate is equal to the first refractive index, and each of the plurality of second layers including a second nanolaminate having at least one bilayer, each bilayer including two nanolayers of different materials, and configured such that the effective refractive index of the second nanolaminate is equal to the second refractive index.
[0043] Also in general, the embodiment of FIG. 3C provides an optical coating including a plurality of first layers having a first refractive index and a plurality of second layers having a second refractive index different from the first refractive index, the plurality of first layers and the plurality of second layers being alternately formed to be combined on a substrate, each of the plurality of first layers including an oxide nanolaminate having at least one oxide bilayer made from a first oxide nanolayer and a second oxide nanolayer of a material different from the first oxide nanolayer, and configured such that the effective refractive index of the oxide nanolaminate is equal to the first refractive index, and each of the plurality of second layers including a nitride nanolaminate having at least one nitride bilayer made from a first nitride nanolayer and a second nitride nanolayer of a material different from the first nitride nanolayer, and configured such that the effective refractive index of the nitride nanolaminate is equal to the second refractive index.
[0044] The nanolayers require control of their material properties (stress, hardness, stoichiometry). For this purpose, reactive sputtering ion-assisted deposition is the preferred technique. Reactive sputtering allows for rapid deposition of stoichiometric films, and the ion-assisted portion allows for atomic level heating that helps control the stress, density, and hardness of the deposited films. Also, by controlling the sputtering parameters and gas flows during nanolayer formation, the product of (n1-n2) / (n1+n2) is less than 0.07 for both nanolayers in the bilayer nanolaminate, and the effective ratio of (n 1eff -n 2eff ) / (n 1eff +n 2eff The refractive index can be adjusted so that the result of ) is greater than 0.1.
[0045] The optical film may have a high coefficient of friction, meaning that it is very hard, but may be damaged by repeated rubbing contact. To protect the optical coating from wear, it may be coated with a lubricating film. This is shown by the dotted layer labeled DLC in Figures 3A-3C. In this example, the diamond-like coating (DLC) film is a highly hydrogenated DLC containing at least 20% hydrogen.
[0046] Furthermore, in consumer display products, fingerprints reduce the visibility of the display. The final surface of these types of products needs to have an anti-smudge or anti-fingerprint (AF) coating. It is very difficult to adhere DLC to fluorocarbon materials that are typically used for anti-fingerprint applications. To improve adhesion, a bilayer is used between the DLC and the AF coating. A thin silicon film is deposited on the DLC to protect it from oxygen, which is used to form a second SiO2 layer. The resulting stack is shown in FIG. 3D, but similar DLC, Si, SiO2, and AF cap layers can be formed on any of the embodiments of FIGS. 3A-3C.
[0047] It should be understood that the processes and techniques described herein are not inherently related to any particular apparatus, but may be practiced by any suitable combination of components. Moreover, various types of general purpose devices may be used in accordance with the description herein. The present invention has been described with reference to specific embodiments, which are intended in all respects to be illustrative and not restrictive. Those skilled in the art will recognize that a variety of combinations are suitable for practicing the present invention.
[0048] Additionally, other aspects of the invention will be apparent to those skilled in the art from consideration of the specification and practice of the invention disclosed herein. Various aspects and / or components of the described embodiments may be used alone or in any combination. It is intended that the specification and examples be considered as exemplary only, with a true scope and spirit of the invention being indicated by the following claims.
Claims
1. a plurality of low refractive index layers each having a first refractive index; a plurality of high refractive index layers each having a second refractive index greater than the first refractive index; the low refractive index layers and the high refractive index layers are arranged alternately in combination to form a laminate; At least one layer selected from the low refractive index layer and the high refractive index layer comprises a superlattice nanolaminate layer made from a plurality of alternating nanolayers of two different materials having refractive indices different from the first refractive index and the second refractive index; when the at least one layer is selected from the low refractive index layers, each of the two different materials is an oxide material; When said at least one layer is selected from said high refractive index layers, each of said two different materials comprises a nitride material.
2. The optical coating of claim 1 , wherein each of the nano-layers has a thickness between 2 nm and 10 nm.
3. When the at least one layer is selected from the low refractive index layers, each of the two different materials is selected to have a refractive index having a value closer to the first refractive index than to the second refractive index; 2. The optical coating of claim 1, wherein when the at least one layer is selected from the high refractive index layers, each of the two different materials is selected to have a refractive index having a value closer to the second refractive index than to the first refractive index.
4. A plurality of low refractive index layers, each of which has a first refractive index; a plurality of high refractive index layers each having a second refractive index greater than the first refractive index; the low refractive index layers and the high refractive index layers are arranged alternately in combination to form a laminate; An optical coating, wherein each of the plurality of low refractive index layers and each of the plurality of high refractive index layers comprises a nanolaminate layer made from alternating nanolayers of two different materials.
5. In the low refractive index layer, each of the two different materials is an oxide material; The optical coating of claim 4 , wherein in the high refractive index layer, each of the two different materials comprises a nitride material.
6. each of the plurality of low refractive index layers comprises a nanolaminate layer made of alternating nanolayers of two different materials having refractive index values closer to the first refractive index than to the second refractive index; 5. The optical coating of claim 4, wherein each of the plurality of high refractive index layers comprises a nanolaminate layer made from alternating nanolayers of two different materials having refractive index values closer to the second refractive index than to the first refractive index.
7. In the superlattice nanolaminate layer, the two different materials are represented by the formula (n 1 -n 2 ) / (n 1 +n 2 )≦0.07, 1 and n 2 The optical coating of claim 1 , wherein:
8. Each of the plurality of low refractive index layers has a refractive index n 1 and n 2 and each of the formula (n 1 -n 2 ) / (n 1 +n 2 ) ≦0.07, Each of the plurality of high refractive index layers has a refractive index n i and n j and each of the formula (n i -n j ) / (n i +n j 5. The optical coating of claim 4, comprising a nanolaminate layer made of alternating nanolayers of two different materials, wherein the nanolaminate layer has a refractive index of 0.1 to 0.5, and the refractive index of the two materials is 0.1 to 0.
5.
9. Formula (n f -n s ) / (n f +n s ) ≧0.10, wherein n f is equal to the first refractive index, and n s The optical coating of claim 8 , wherein:
10. The two different materials are ZrO 2 , ZrN, AlN, Si 3 N 4 , TiO 2 , Nb 2 O 5 , Ta 2 O 5 , CrO 2 , W.O. 3 The optical coating of claim 1 , comprising two or more of:
11. The two different materials are SiO 2 , Al 2 O 3 , SiO x N y , Si x A y O z The optical coating of claim 1 , comprising two or more of:
12. The optical coating of claim 1 further comprising a diamond-like coating (DLC) formed on the stack.
13. a silicon layer formed on the DLC; SiO formed on the silicon layer 2 Layers, The SiO 2 13. The optical coating of claim 12, further comprising an anti-fingerprint (AF) layer formed on the layer.
14. a plurality of first layers having a first refractive index; a plurality of second layers having a second refractive index different from the first refractive index; the first layers and the second layers are alternately formed on a substrate so as to be combined therewith, terminating with one layer from the second layers; a top layer formed on the one layer, the top layer comprising a nanolaminate having a plurality of bilayers, each bilayer comprising two nanolayers of different materials; An optical coating, wherein each of the different materials is different from the materials of the first and second layers such that the effective refractive index of the upper layer has a value closer to the first refractive index than to the second refractive index.
15. The different materials are represented by the formula (n 1 -n 2 ) / (n 1 +n 2 )≦0.07, 1 and n 2 The optical coating of claim 14 , wherein:
16. The effective refractive index n of the upper layer eff is the formula |(n eff -n s ) / (n eff +n s )|≧0.10, wherein n s The optical coating of claim 15 , wherein:
17. The different material is ZrO 2 , ZrN, AlN, Si 3 N 4 , TiO 2 , Nb 2 O 5 , Ta 2 O 5 , CrO 2 , W.O. 3 17. The optical coating of claim 16, comprising two or more of:
18. The different material is SiO 2 , Al 2 O 3 , SiO x N y , Si xAlyO z 17. The optical coating of claim 16, comprising two or more of:
19. The optical coating of claim 16 further comprising a diamond-like coating (DLC) formed on the top layer.
20. a silicon layer formed on the DLC; SiO formed on the silicon layer 2 Layers, The SiO 2 20. The optical coating of claim 19, further comprising an anti-fingerprint (AF) layer formed on the layer.
Citation Information
Patent Citations
Semiconductor device, surface emitting semiconductor laser, and edge emitting semiconductor laser
JP2000349393A
Nitride semiconductor element
JP2005294306A
Nitride semiconductor laser element, and nitride semiconductor element
JP2008098664A
Thin film and optical interference filter incorporating high-index titanium dioxide and method for making them
US20090311521A1
Object with reflection-reducing coating and method for the production thereof
US20140233106A1