MEMS device with reduced contact resistance
Etching ruthenium contacts with a chlorine-containing etchant and fluorine-based plasma treatment in MEMS devices addresses the sticking issue, enhancing contact resistance and reliability.
Patent Information
- Application Number
- JP2021566474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-30
- Filing Date
- 2020-05-29
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-05-29
AI Technical Summary
Ruthenium contacts in MEMS devices provide low resistance and durability but are susceptible to sticking phenomena, which is a key failure mechanism.
A method involving etching ruthenium contacts with a chlorine-containing etchant after sacrificial material removal, followed by a fluorine-based plasma treatment, to reduce contact resistance and minimize sticking.
The method achieves low contact resistance and reduces the susceptibility to sticking, improving the performance and reliability of MEMS devices.
Smart Images

Figure 0007588093000001 
Figure 0007588093000002 
Figure 0007588093000003
Abstract
Description
[Technical field]
[0001] This application claims priority to U.S. Provisional Patent Application No. 62 / 854,826, filed May 30, 2019, the disclosure of which is incorporated herein by reference in its entirety.
[0002] SUMMARY OF THE DISCLOSURE Embodiments of the present disclosure generally relate to methods for reducing contact resistance while preventing sticking in micro-electromechanical system (MEMS) devices that include one or more ruthenium contacts. [Background technology]
[0003] Contact welding or sticking is one of the main failure mechanisms in MEMS devices. Sticking is one of the key challenges in producing viable MEMS devices. Although ruthenium contacts provide a durable contact with low resistance, ruthenium contacts are susceptible to potential sticking phenomena over their operational lifetime.
[0004] It is therefore necessary to have a low resistance, durable contact that is not susceptible to sticking phenomena. Summary of the Invention
[0005] The present disclosure generally relates to a method for fabricating a MEMS device. The MEMS device has a cavity through which a beam will move to change the capacitance of the device. After the device build-up is nearly complete, the sacrificial material is removed to release the beam within the cavity of the MEMS device. The exposed ruthenium contacts are then etched back with a chlorine-containing etchant to remove the top surfaces of both the top and bottom contacts. This etch-back process can achieve a low contact resistance that is less susceptible to sticking phenomena. The sticking performance can be further improved by conditioning the ruthenium contacts in a fluorine-based plasma. The fluorine-based plasma process, or fluorine treatment, can be performed before or after the etch-back process of the ruthenium contacts.
[0006] In one embodiment, a method of manufacturing a MEMS device includes forming one or more electrical contact stacks including ruthenium contact surfaces in a cavity, forming a beam structure across the one or more electrical contact stacks in the cavity, the cavity containing a sacrificial material, removing the sacrificial material from the cavity to free the beam to move within the cavity, etching a portion of the ruthenium contact surfaces using an etchant including chlorine, and sealing the cavity.
[0007] Those skilled in the art will appreciate the scope of the present disclosure and realize additional aspects thereof from the following detailed description of the preferred embodiments, when read in conjunction with the accompanying drawings.
[0008] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate several aspects of the present disclosure and, together with the description, serve to explain the principles of the disclosure. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a schematic diagram of a MEMS device prior to removal of the sacrificial material and release of the beam. [Diagram 2]2 is a schematic diagram of the MEMS device of FIG. 1 after the sacrificial material has been removed and the beam has been released. [Figure 3A] FIG. 3 is a schematic diagram of an enlarged portion of the MEMS device of FIG. 2 after the sacrificial material has been removed. [Figure 3B] FIG. 3 is a schematic diagram of an enlarged view of the MEMS device of FIG. 2 after exposed ruthenium-containing elements of the device have been etched back. [Figure 4] FIG. 3C is a schematic diagram of the MEMS device of FIG. 3B after the MEMS device has been encapsulated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] To facilitate understanding, wherever possible, the same reference numbers have been used to designate the same elements common to the figures. It is contemplated that elements disclosed in one embodiment may be beneficially utilized in other embodiments without specific recitation.
[0011] In the following, reference will be made to embodiments of the present disclosure. However, it should be understood that the present disclosure is not limited to the specifically described embodiments. Instead, any combination of the following features and elements, whether related to different embodiments or not, is contemplated for implementing and practicing the present disclosure. Furthermore, the embodiments of the present disclosure may achieve other possible solutions and / or advantages over the prior art, but whether a particular advantage is achieved by a given embodiment does not limit the present disclosure. Thus, the following aspects, features, embodiments, and advantages are merely illustrative and should not be considered as elements or limitations of the appended claims unless expressly recited in the claims. Similarly, references to "disclosure" should not be construed as a generalization of any inventive subject matter disclosed herein, and should not be considered as elements or limitations of the appended claims unless expressly recited in the claims.
[0012] The embodiments described below represent the necessary information to enable those skilled in the art to practice the embodiments and illustrate the best mode of practicing the embodiments. Upon reading the following description with reference to the accompanying drawings, those skilled in the art will understand the concepts of the present disclosure and recognize applications of these concepts not specifically addressed herein. It is to be understood that these concepts and applications are within the scope of the present disclosure and the appended claims.
[0013] Terms such as first, second, etc. may be used to describe various elements herein, but it should be understood that these elements should not be limited by these terms. These terms are used only to distinguish one element from another element. For example, a first element may be referred to as a second element, and similarly, a second element may be referred to as a first element, without departing from the scope of the present disclosure. As used herein, the term "and / or" includes any and all combinations of one or more of the listed items.
[0014] When an element, such as a layer, region, or substrate, is referred to as being "on" or extending "onto" another element, it is understood that it can be directly on or extending directly onto the other element, or intervening elements may be present. In contrast, when an element is referred to as being "directly on" or extending "directly onto" another element, there are no intervening elements present. Similarly, when an element, such as a layer, region, or substrate, is referred to as being "over" or extending "over" another element, it is understood that it can be directly on or extending directly onto the other element, or intervening elements may be present. In contrast, when an element is referred to as being "directly over" or extending "directly over" another element, there are no intervening elements present. When an element is referred to as being "connected" or "coupled" to another element, it should be understood that the element can be directly connected or coupled to the other element, or there may be intervening elements. In contrast, when an element is referred to as being "directly connected" or "directly coupled" to another element, there are no intervening elements present.
[0015] Relative terms such as "below" or "above" or "upper" or "lower" or "horizontal" or "vertical" may be used herein to describe the relationship of one element, layer, or region to another element, layer, or region shown in the figures. It is understood that these terms and their above discussion are intended to encompass different orientations of the device in addition to the orientation depicted in the figures.
[0016] The terms used in the specification are intended to describe only certain embodiments and are not intended to limit the disclosure. As used in the specification, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. It is further understood that the terms "comprises", "comprising", "includes" and / or "including" as used in the specification specify the presence of stated features, integers, steps, operations, elements and / or components, but do not exclude the presence of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0017] Unless otherwise defined, all terms (including technical and scientific terms) used in the specification have the same meaning as commonly understood by those skilled in the art to which this disclosure belongs. It is further understood that terms used in the specification should be interpreted to have a meaning consistent with the meaning in the context of this specification and the related art, and should not be interpreted in an idealized or overly formal sense unless expressly defined in the specification.
[0018] The present disclosure generally relates to a method for fabricating a MEMS device. The MEMS device has a cavity through which a beam will move to change the capacitance of the device. After the device build-up is nearly complete, the sacrificial material is removed to release the beam within the cavity of the MEMS device. The exposed ruthenium contacts are then etched back with a chlorine-containing etchant to remove the top surfaces of both the top and bottom contacts. This etch-back process can achieve a low contact resistance that is less susceptible to sticking phenomena. The sticking performance can be further improved by conditioning the ruthenium contacts in a fluorine-based plasma. The fluorine-based plasma process, or fluorine treatment, can be performed before or after the etch-back process of the ruthenium contacts.
[0019] 1 is a schematic diagram of a MEMS device 100 prior to removing sacrificial material and releasing the beam. The MEMS device 100 includes a substrate 102, such as a CMOS substrate that includes multiple layers for a semiconductor device. It is contemplated that the substrate 102 may simply be a semiconductor substrate containing silicon, germanium, or other suitable semiconductor material.
[0020] Within the substrate are one or more contact electrodes 104A, 104B. The contact electrodes 104A, 104B can be RF conductors or RF electrodes. Although two contact electrodes 104A, 104B are shown, it should be understood that a single contact electrode, or even three or more contact electrodes, are contemplated. The contact electrodes 104A, 104B can be constructed of any conductive material suitable for use in semiconductor devices, such as copper, aluminum, titanium nitride, tungsten, and combinations thereof.
[0021] Additional conductive material may be present on or above the substrate 102, as may contact electrodes 104A, 104B. For example, anchor electrodes 106A, 106B are shown in FIG. 1, as are a number of additional electrical contacts 108. The anchor electrodes 106A, 106B may be electrodes for the beam structure 114, and the electrical contacts 108 may be used as pulling electrodes. The anchor electrodes 106A, 106B and the electrical contacts 108 may be composed of any conductive material suitable for use in semiconductor devices, such as copper, aluminum, titanium nitride, tungsten, and combinations thereof.
[0022] A dielectric layer 110 resides over the substrate 102, including over the electrical contacts 108. The dielectric layer 110 is intended to include an electrically insulating material, such as silicon oxide, silicon dioxide, silicon nitride, silicon oxynitride, or a combination thereof.
[0023] A first sacrificial layer 112 resides over the dielectric layer 110. The first sacrificial layer 112 is eventually removed to release the beam structure 114. The first sacrificial layer 112 comprises a different material than the dielectric layer 110. Suitable materials for the first sacrificial layer 112 include spin-on materials, such as carbon-based materials. The first sacrificial layer 112 may include carbon, hydrogen, nitrogen, and oxygen.
[0024] A second dielectric layer 110 resides over the first sacrificial layer 112, and a bottom portion of a beam structure 114 resides over the second dielectric layer 110. The second dielectric layer 110 may comprise the same material as the first dielectric layer 110. The beam structure 114 may be composed of any conductive material suitable for use in semiconductor devices, such as copper, aluminum, titanium nitride (TiN), tungsten, titanium aluminum nitride (TiAlN), tantalum nitride (TaN), and combinations thereof. The beam structure 114 further includes a middle portion, a top portion, and a post portion. The dielectric layer 110 resides on the top and bottom surfaces of the beam portion.
[0025] Additionally, in areas where the beam structures 114 are not located, there is additional sacrificial material 112. The sacrificial material 112 may comprise the same material everywhere in the MEMS device 100. In fact, the sacrificial material 112 is present over the top portion of the beam structures 114. On and in contact with the topmost sacrificial material 112 is an additional dielectric layer 110. A pull-up electrode 116 is present over and on the additional dielectric layer 110. A dielectric roof 118 is also present over the pull-up electrode 116. A release hole 120 is present through the dielectric roof 118 and the topmost dielectric layer 110. The release hole 120 extends through the roof 118 to expose the sacrificial material 112.
[0026] The bottom of the beam structure 114 includes two beam contact portions 122 that include ruthenium. Two electrical contact stacks that include ruthenium contact surfaces 124 are across each contact electrode 104A, 104B and are aligned with the two beam contact portions 122. The ruthenium contact surfaces 124 provide a landing for the beam structure 114, as will be discussed below. The beam contact portions 122 contact the contact surfaces 124 when the beam structure 114 is released and in a pull-down state, which is a maximum capacitance state. One or more additional electrical contact stacks that include ruthenium contact surfaces 126 are disposed across a portion of the electrical contacts 108.
[0027] In order to release the beam structure 114 and move the device 100, the sacrificial material needs to be removed. Figure 2 is a schematic diagram of the MEMS device 100 of Figure 1 after the sacrificial material 112 has been removed and the beam 114 has been released. The sacrificial material 112 is removed by an etching process in which an etchant, which may be a wet etchant or a dry etchant, is introduced through the release holes 120. Once the sacrificial material 112 is removed, the location that was used for the sacrificial material is considered a cavity 202.
[0028] The beam structure 114 is free to move within the cavity 202 once the sacrificial material 112 is removed. The beam structure 114 may be moved back and forth as desired from a first position (shown in FIG. 2) spaced from both the pull-up electrode 116 and the electrical contact stack containing the ruthenium contact surface 124, to a second position in contact with the contact surface 124, and to a third position disposed adjacent the pull-up electrode 116 and spaced a greater distance from the contact surface 124 than the first position. The terms "first position," "second position," and "third position" are not intended to be limiting, and the beam structure 114 may be moved to and from any of the three positions in any order.
[0029] As mentioned above, the sacrificial material 112 is removed, but everything else in the device 100 remains. Thus, the contact surfaces 124, 126 are exposed, as is the contact portion 122 containing ruthenium. Additionally, as mentioned above, ruthenium is a low resistance, durable contact, but the ruthenium contacts are susceptible to potential sticking phenomena over their operational life. Thus, it has been surprisingly found that additional processing of ruthenium results in less sticking, further lowering the contact resistance of the device.
[0030] The ruthenium-containing elements of the device 100 (i.e., the beam contact portion 122 and the contact surfaces 124, 126) may be treated with a fluorine-based treatment. For example, a plasma containing fluorine and oxygen may optionally be introduced into the cavity 202 through the release hole 120. In one embodiment, the plasma is formed from O2 and CF4. It is contemplated that other fluorine-based gases such as NF3, SF6, and CHF3 may be used. In one embodiment, a fluorocarbon-based self-assembled monolayer (SAM) may be utilized. Thus, the present disclosure is not limited to CF4. Excess amounts of C formed during the introduction of the fluorine-based treatment may be reduced by 100%. x F y Polymer formation can increase contact resistance to unacceptable levels. Excessive fluorine doping of ruthenium can increase contact resistance to unacceptable levels. Therefore, to maintain low contact resistance, as little polymer formation as possible is desired.
[0031] Figure 3A is a schematic diagram of an enlarged portion of the MEMS device 100 of Figure 2 after the sacrificial material 112 has been removed and / or after an optional fluorine-based treatment. As shown in Figure 3A, an interstitial layer 330 or layer of residue may be disposed on the top surface 332 of the contact surface 124. The interstitial layer 330 or layer of residue may be formed on the contact surfaces 124, 126 during various formation operations of the MEMS device 100, for example, during fabrication or construction, during removal of the sacrificial material 112, or during optional fluorine-based treatment.
[0032] After the optional fluorine-based treatment, a chlorine (Cl) etching process is performed. In one embodiment, the chlorine etching process is performed before the optional fluorine-based treatment. Thus, the optional fluorine-based treatment may occur before or after the chlorine etching process. The chlorine etching process may occur after the removal of the sacrificial material 112. A chlorine-containing etchant, such as hydrochloric acid (HCl), boron trichloride (BCl3), or chlorine gas (Cl2), is introduced into the cavity 202 through the release holes 120. The chlorine etch-back process may be a "wet" or "dry" process. In addition to chlorine, the dry etch-back process may include oxygen and / or a combination of oxygen and fluorine. The chlorine-containing etchant has a high etch selectivity such that it etches only the ruthenium-containing elements of the device 100 and residues such as the interstitial layer 330. Thus, the chlorine-containing etchant etches a portion of the contact electrode surfaces 124, 126 and / or a bottom portion of the beam contact surface 122 without etching the beam structure 114 or the dielectric layer 110. The chlorine-containing etch-back process has very high selectivity (20:1) to the dielectric, titanium, titanium nitride, and titanium aluminum nitride, which allows the etch-back process to selectively etch back the contact electrode surfaces 124, 126 without adversely affecting other components within the cavity.
[0033] Figure 3B is a schematic diagram of an enlarged view of the MEMS device 100 of Figure 2 after the exposed ruthenium-containing elements of the device 100 (i.e., the beam contacting portion 122 and the contact surfaces 124, 126) have been etched. In Figure 3B, the top portions or surfaces 332 of the contact surfaces 124, 126 and the bottom portion or surface 334 of the beam contacting portion 122 have been partially removed through a chlorine etching process. Although Figure 3B shows the removal of ruthenium from both the contact surfaces 124, 126 and the beam contacting portion 122, removal may occur only on the contact surfaces 124, 126, only on the beam contacting portion 122, or on both the contact surfaces 124, 126 and the beam contacting portion 122.
[0034] Etching the bottom portion or surface 334 of the beam contact portion 122 recesses the beam contact portion 122 into the beam structure 114, and etching the top portion or surface 332 of the contact surfaces 124, 126 reduces the overall height of the contact electrodes. As shown in FIG. 3B, the exposed ruthenium-containing elements etched during the chlorine etching process (i.e., the top surface 332 of the contact surfaces 124, 126 and / or the bottom surface 334 of the beam contact portion 122) may have a surface with elevated roughness. In other words, the top surface 332 of the contact surfaces 124, 126 and / or the bottom surface 334 of the beam contact portion 122 have a surface roughness due to being etched with an etchant containing chlorine. In one embodiment, the top surface 332 and the bottom surface 334 each have a root mean square roughness of about 1 nm to about 10 nm, e.g., about 2 nm to about 5 nm. Surface roughness may increase with extended exposure of surfaces 332, 334 to chlorine-containing etchants. Additionally, following the chlorine etching process, any residue or interstitial layer 330 that may have formed during formation of device 100 is removed from the exposed ruthenium-containing elements by pumping an inert gas, such as argon, into the cavity.
[0035] The chlorine-containing etchant has a ruthenium etch rate of about 2 nm / min to about 10 nm / min, e.g., about 4 nm / min, and an etching selectivity of ruthenium to surrounding exposed materials, such as oxide, TiAlN, and TiN, of about 20:1 to about 25:1 (i.e., the chlorine-containing etchant may etch ruthenium 20-25 times faster than the chlorine-containing etchant etches oxide, TiAlN, TiN). The chlorine-containing etchant may be present in the cavity 202 for about 1 minute to 5 minutes, e.g., about 2.5 minutes to 3 minutes. The chlorine etching process may remove about 5 nm to 15 nm of ruthenium from each of the contact surfaces 124, 126 and the beam contact portion 122. By etching the ruthenium from the contact surfaces 124, 126 and the beam contact portion 122, the contact resistance of the MEMS device 100 is effectively reduced. In one embodiment, the chlorine etch process reduces the contact resistance of device 100 by approximately two times compared to conventional MEMS devices.
[0036] Etching a portion of the contact surfaces 124, 126 from each of the electrical contact stacks and / or a portion of each beam contact portion 122 cleans the ruthenium surface that was in contact with the sacrificial material 112. The chlorine etch process further removes residues, interstitial layers, or interstitial impurities that may have formed on the surface while forming the MEMS device 100, such as during fabrication or construction, during removal of the sacrificial material 112, or during the optional fluorine-containing plasma treatment. For example, the chlorine etch process removes any C ions that may have formed during the optional fluorine-containing plasma treatment. x F y Polymer formation may be eliminated.
[0037] Once the sacrificial material 112 has been removed and the exposed ruthenium has been treated, the device 100 is ready to be encapsulated. Figure 4 is a schematic diagram of the MEMS device 100 of Figure 3B after it has been encapsulated. As shown in Figure 4, an encapsulation portion 402 is formed to encapsulate the release hole 120. The encapsulation portion 402 extends downward to contact the topmost dielectric layer 110 disposed on the beam structure 114. The encapsulation portion 402 may include a dielectric material such as silicon oxide, silicon dioxide, silicon nitride, silicon oxynitride, or a combination thereof.
[0038] By treating the exposed ruthenium surface after the sacrificial material is removed, the resulting MEMS device has contact surfaces that are low-resistance, durable, and less susceptible to sticking phenomena.
[0039] In one embodiment, a method of manufacturing a MEMS device includes forming one or more electrical contact stacks including ruthenium contact surfaces in a cavity, forming a beam structure across the one or more electrical contact stacks in the cavity, the cavity containing a sacrificial material, removing the sacrificial material from the cavity to free the beam to move within the cavity, etching a portion of the ruthenium contact surfaces using an etchant including chlorine, and sealing the cavity.
[0040] The etchant may further include oxygen or a fluorine-based gas. The etchant may be present in the cavity for a period of about 2.5 minutes to about 3 minutes. About 5 nm to about 15 nm of the ruthenium contact surface may be removed through etching. The beam structure may include at least one contact portion including ruthenium. Etching the portion of the ruthenium contact surface using an etchant including chlorine may further include etching a bottom portion of the at least one contact portion including ruthenium. Etching the portion of the at least one contact portion including ruthenium may recess the at least one contact portion including ruthenium into the beam structure. The MEMS device may include at least one contact electrode. At least one of the one or more electrical contact stacks including the ruthenium contact surface may be formed over the at least one contact electrode.
[0041] The method may further include introducing a plasma containing fluorine and oxygen into the cavity prior to etching the portion of the ruthenium interface using a chlorine-containing etchant. The chlorine-containing etchant may include hydrochloric acid, boron trichloride, or chlorine gas. Etching the portion of the ruthenium interface using a chlorine-containing etchant may further remove any residue or interstitial layer from the ruthenium interface. The chlorine-containing etchant may have an etch rate of about 4 nanometers per minute to about 6 nanometers per minute. The chlorine-containing etchant may have a selectivity ratio of about 20:1 for etching ruthenium over oxide or titanium aluminum nitride.
[0042] Those skilled in the art will recognize improvements and modifications to the preferred embodiments of the present disclosure, and all such improvements and modifications are considered within the scope of the concepts disclosed herein and the following claims.
Claims
1. 1. A method of manufacturing a MEMS device, comprising: forming one or more electrical contact stacks including a contact surface of ruthenium, such that at least one of the one or more electrical contact stacks is formed across at least one contact electrode; depositing a sacrificial material over the one or more electrical contact stacks; forming a beam structure across the one or more electrical contact stacks such that the one or more electrical contact stacks are formed within the cavity filled with the sacrificial material; removing a sacrificial material to release the beam structure to move within the cavity, such that at least one contact portion of the beam structure can contact a contact surface of the at least one contact electrode; Etching a portion of the contact surface of the ruthenium in the cavity using an etchant comprising chlorine; and sealing the cavity.
2. The method of claim 1 , wherein the etchant further comprises oxygen or a fluorine-based gas.
3. The method of claim 1, wherein the etching agent is present in the cavity for a period of about 2.5 minutes to 3 minutes.
4. The method of claim 1 , wherein about 5 nm to about 15 nm of said contact surface of ruthenium is removed during said etching.
5. The method of claim 1 , wherein the beam structure includes at least one contact portion comprising ruthenium.
6. 6. The method of claim 5, wherein said etching said portion of said contact surface of ruthenium using said etchant comprising chlorine further comprises etching a bottom portion of said at least one contact portion comprising ruthenium.
7. The method of claim 6 , wherein etching the bottom portion of the at least one contact portion comprising ruthenium recesses the at least one contact portion into the beam structure.
8. 2. The method of claim 1, further comprising introducing a plasma containing fluorine and oxygen into the cavity prior to etching the portion of the contact surface of ruthenium using the etchant containing chlorine.
9. 2. The method of claim 1, wherein the chlorine-containing etchant comprises hydrochloric acid, boron trichloride, or chlorine gas.
10. 2. The method of claim 1, wherein said etching said portion of said contact surface of ruthenium using said etchant comprising chlorine further removes any residue or interstitial layers from said contact surface of ruthenium.
11. 10. The method of claim 1, wherein the etchant comprising chlorine has an etch rate of between about 4 nanometers per minute and about 6 nanometers per minute.
12. 2. The method of claim 1, wherein the etchant containing chlorine has a selectivity ratio for etching ruthenium over oxide or titanium aluminum nitride of about 20:1.
Citation Information
Patent Citations
mems switch contact system
JP2009510707A
Method for forming pore in crystal substrate, and functional device having wiring and piping in crystal substrate
JP2014045030A
Piezoelectric actuator and manufacturing method of the same, liquid cartridge, and image forming apparatus
JP2016062984A
Method of preparing electrical contacts used in switches
US20020088112A1
Encapsulated micro-electromechanical system switch and method of manufacturing the same
US20120175715A1