Reflective mask blank, reflective mask, and method for manufacturing semiconductor device

By using an alloy-based phase shift film with adjusted composition ratios, the reflective mask blank ensures consistent phase difference and reflectance characteristics, addressing production stability issues and enabling precise semiconductor device patterning.

JP7588176B2Active Publication Date: 2024-11-21HOYA CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023064906
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-03-03
Filing Date
2023-04-12
Publication Date
2024-11-21
Estimated Expiration
2037-05-31

AI Technical Summary

Technical Problem

Existing reflective mask blanks for EUV lithography face challenges in maintaining consistent phase difference and reflectance variations within predetermined ranges due to fluctuations in phase shift film thickness, leading to unstable production of reflective masks with desired characteristics.

Method used

The reflective mask blank is designed with a phase shift film made of an alloy containing two or more metals, where the composition ratio is adjusted to ensure that phase difference and reflectance variations remain within specific ranges despite slight thickness variations, using formulas (1) and (2) to stabilize these characteristics.

Benefits of technology

This approach allows for the stable production of reflective masks with desired phase difference and reflectance characteristics, enabling the manufacture of semiconductor devices with fine and accurate transfer patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588176000016
    Figure 0007588176000016
  • Figure 0007588176000017
    Figure 0007588176000017
  • Figure 0007588176000018
    Figure 0007588176000018
Patent Text Reader

Abstract

To provide a reflection type mask blank and a reflection type mask, having a phase shift membrane small in a phase difference and membrane thickness dependence of a reflection coefficient.SOLUTION: There is provided a reflection type mask blank, in which a reflection coefficient of a phase shift membrane surface is over 3% and 20% or less, the phase shift membrane is constituted by a material consisting of an alloy having 2 or more kinds of metals to have a phase difference of prescribed 170 degrees to 190 degrees, the alloy selects one or more kinds of metal elements from a group A and a group B, where the group A is a metal element group satisfying a refractive index n and an extinction coefficient k of k>α*n+β, and the group B is a metal element group satisfying the refractive index n and the extinction coefficient k of k<α*n+β, variation of the phase difference when a membrane thickness of the phase shift membrane varies by ±0.5% to a set membrane thickness is in a range of ±2 degrees and a composition ratio is adjusted so that variation of the reflection coefficient is in a range of ±0.2%, where α:proportional constant and β:constant.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask blank, which is an original plate for producing an exposure mask used in the manufacture of a semiconductor device, and a reflective mask, as well as a method for manufacturing a semiconductor device using the reflective mask. [Background technology]

[0002] The types of light sources of exposure equipment in the manufacture of semiconductor devices have evolved with gradually shorter wavelengths, from g-line with a wavelength of 436 nm, i-line with a wavelength of 365 nm, KrF laser with a wavelength of 248 nm, and ArF laser with a wavelength of 193 nm. In order to realize finer pattern transfer, EUV lithography using extreme ultraviolet (EUV: Extreme Ultra Violet) with a wavelength of about 13.5 nm as a light source has been proposed. In EUV lithography, a reflective mask is used because the difference in absorptivity of EUV light between materials is small. As a reflective mask, for example, a mask has been proposed in which a multilayer reflective film that reflects exposure light is formed on a substrate, and a phase shift film that absorbs exposure light is formed in a pattern on a protective film for protecting the multilayer reflective film. Light incident on a reflective mask mounted on an exposure machine (pattern transfer device) is absorbed in a portion with a phase shift film pattern, and is reflected by the multilayer reflective film in a portion without a phase shift film pattern, so that an optical image is transferred onto a semiconductor substrate through a reflective optical system. A portion of the exposure light incident on the phase shift film pattern is reflected with a phase difference of approximately 180 degrees from the light reflected by the multilayer reflective film (phase shift), thereby obtaining contrast (resolution).

[0003] Techniques relating to such reflective masks for EUV lithography and mask blanks for fabricating the same are disclosed in Patent Documents 1 to 3 and the like.

[0004] Patent Document 1 describes that in order to improve the transfer resolution by applying the principle of a halftone mask to EUV exposure, the material of a halftone film (phase shift film) made of a single layer is selected from the area enclosed by a square frame in Fig. 2, which is shown in planar coordinates with the refractive index and extinction coefficient as the coordinate axes. As a specific material for the single layer, TaMo (composition ratio 1:1) is described.

[0005] Patent Document 2 describes that in a half-tone EUV mask, in order to provide a degree of freedom in selectivity of reflectance and high cleaning resistance and to reduce the projection effect (shadowing effect), the material of the half-tone film is a compound of Ta and Ru, and its composition range is specified.

[0006] Patent Document 3 describes that in a half-tone EUV mask, in order to provide freedom in reflectance selectivity and high cleaning resistance and to improve etching processing accuracy, the material of the half-tone film contains Ta and Nb, with the Ta:Nb composition ratio in the composition range of approximately 4:1 to approximately 1:2.

[0007] Here, the shadowing effect refers to the following phenomenon. For example, in an exposure apparatus that uses a reflective mask, the light is incident on the mask at a slight angle from the perpendicular direction so that the optical axes of the incident light and the reflected light do not overlap. If the phase shift film pattern on the mask has thickness, a shadow based on the thickness of the phase shift film pattern is generated due to the inclination of the incident direction of the light. The change in the dimensions of the transferred pattern by the amount of this shadow is called the shadowing effect. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2006-228766 A [Patent Document 2] Patent No. 5233321 [Patent Document 3] Patent No. 5266988 Summary of the Invention [Problem to be solved by the invention]

[0009] In order to improve resolution through the phase shift effect, the phase shift film of a reflective mask is designed so that the reflectance of EUV light reflected from the phase shift film pattern relative to the EUV light reflected from the multilayer reflective film (including a multilayer reflective film with a protective film) in areas where there is no phase shift film pattern is 3% to 20%.

[0010] In addition, the EUV light reflected by the multilayer reflective film in a portion of the exposure light incident on the phase shift film pattern and the EUV light reflected by the multilayer reflective film in a portion where there is no phase shift film pattern are designed to have a phase difference of approximately 180 degrees with respect to the EUV light.

[0011] On the other hand, in order to maximize the phase shift effect in a reflective mask and prevent pattern errors in a transfer pattern transferred using a reflective mask, it is required that the phase difference variation of the phase shift film between multiple reflective mask blanks be within a predetermined phase difference variation range (e.g., ±2 degrees) for a predetermined phase difference (e.g., 180 degrees). In addition to the phase difference variation, it is also required that the reflectance variation be within a predetermined reflectance variation range (e.g., ±0.2%) for a predetermined reflectance (e.g., 6%).

[0012] However, it is unavoidable that the thickness of the phase shift film varies when a plurality of reflective mask blanks are manufactured, and it is difficult to stably manufacture a reflective mask blank having desired phase difference characteristics (e.g., phase difference variation in the range of ±2 degrees) for a predetermined phase difference (e.g., 180 degrees). Moreover, it is even more difficult to obtain a reflective mask blank having desired reflectance characteristics (e.g., reflectance variation in the range of ±0.2%) for a predetermined reflectance (e.g., 6%) in addition to the phase difference characteristics.

[0013] Therefore, an object of the present invention is to provide a reflective mask blank which enables the stable production of reflective masks having desired phase difference characteristics and desired reflectance characteristics, even if the film thickness of the phase shift film varies slightly from the design value when multiple reflective mask blanks are continuously produced. [Means for solving the problem]

[0014] The inventors have discovered that when continuously manufacturing a plurality of reflective mask blanks, even if the thickness of the phase shift film varies slightly from the designed value (for example, within a range of ±0.5% of the designed film thickness), the refractive index and extinction coefficient of the phase shift film constituting the reflective mask blank exist in a spot-like manner as optimal conditions for achieving desired phase difference characteristics (for example, phase difference variation between surfaces in a range of 180 degrees ±2 degrees) and desired reflectance characteristics (for example, reflectance variation between surfaces in a range of 6% ±0.2%), and have arrived at the present invention.

[0015] In order to solve the above problems, the present invention has the following features: The present invention relates to a reflective mask blank having features 1 to 10 below, a reflective mask having feature 11 below, and a method for manufacturing a semiconductor device having feature 12 below.

[0016] (Configuration 1) A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film is made of a material made of an alloy having two or more metals so that the reflectance of the surface of the phase shift film with respect to EUV light with respect to light reflected from the multilayer reflective film before the phase shift film is formed is more than 3% and less than 20%, and the phase shift film has a phase difference of 170 degrees to 190 degrees; When the refractive index at the wavelength of EUV light is n and the extinction coefficient is k, A group of metal elements satisfying the refractive index n and extinction coefficient k of the following formula (1) is defined as group A, and a group of metal elements satisfying the refractive index n and extinction coefficient k of the following formula (2) is defined as group B. The alloy is a reflective mask blank, characterized in that one or more metal elements are selected from each of Group A and Group B, and the composition ratio is adjusted so that when the thickness of the phase shift film varies by ±0.5% from the set thickness, the change in phase difference is in the range of ±2 degrees and the change in reflectance is in the range of ±0.2%. k>α*n+β Equation (1) k<α*n+β (2) (where α is a proportional constant and β is a constant.)

[0017] According to configuration 1 of the present invention, it is possible to provide a reflective mask blank which can stably produce reflective mask blanks having desired phase difference characteristics and desired reflectance characteristics even if the film thickness of the phase shift film varies slightly from the set film thickness when continuously producing a plurality of reflective mask blanks.

[0018] (Configuration 2) In a second aspect of the present invention, the reflectance of the surface of the phase shift film with respect to EUV light is more than 5% and not more than 10%, The reflective mask blank according to structure 1, wherein α in the formulas (1) and (2) is −0.303 and β is 0.309.

[0019] According to configuration 2 of the present invention, when continuously producing a plurality of reflective mask blanks having a phase shift film surface with a reflectance to EUV light of more than 5% and not more than 10%, even if the film thickness of the phase shift film varies somewhat from the set film thickness, a reflective mask blank having desired phase difference characteristics and desired reflectance characteristics can be stably produced.

[0020] (Configuration 3) In a third aspect of the present invention, the reflectance of the surface of the phase shift film with respect to EUV light is more than 3% and not more than 5%, The reflective mask blank according to structure 1, wherein α in the formulas (1) and (2) is −0.331 and β is 0.339.

[0021] According to configuration 3 of the present invention, when continuously producing a plurality of reflective mask blanks having a phase shift film surface with a reflectance to EUV light of more than 3% and not more than 5%, even if the film thickness of the phase shift film varies somewhat from the set film thickness, a reflective mask blank having desired phase difference characteristics and desired reflectance characteristics can be stably produced.

[0022] (Configuration 4) In a fourth aspect of the present invention, the reflectance of the surface of the phase shift film with respect to EUV light is more than 10% and not more than 20%, The reflective mask blank according to structure 1, wherein α in the formulas (1) and (2) is −0.192 and β is 0.194.

[0023] According to configuration 4 of the present invention, when continuously producing a plurality of reflective mask blanks in which the reflectance of the phase shift film surface to EUV light is more than 10% and not more than 20%, even if the film thickness of the phase shift film varies somewhat from the set film thickness, a reflective mask blank having desired phase difference characteristics and desired reflectance characteristics can be stably produced.

[0024] (Configuration 5) A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film is made of a material made of an alloy having two or more metals such that a reflectance R0 of the phase shift film surface to EUV light with respect to light reflected from the multilayer reflective film before the phase shift film is formed is 4%, 6% or 12% and a phase difference θ0 is 180 degrees; The alloy has a refractive index n and an extinction coefficient k at the wavelength of EUV light, and its composition ratio is adjusted so that the allowable range of phase difference θ when the thickness of the phase shift film varies by ±0.5% from the set thickness is θ0-5 degrees≦θ≦θ0+5 degrees, and the allowable range of reflectance R is 0.9R0≦R≦1.1R0.

[0025] According to configuration 5 of the present invention, it is possible to provide a reflective mask blank which can stably produce reflective mask blanks having desired phase difference characteristics and desired reflectance characteristics even if the film thickness of the phase shift film varies slightly from the set film thickness when continuously producing a plurality of reflective mask blanks.

[0026] (Configuration 6) A sixth aspect of the present invention is the reflective mask blank according to the fifth aspect, wherein the alloy has a refractive index falling within the range of 0.877 to 0.881 and an extinction coefficient falling within the range of 0.046 to 0.052.

[0027] (Configuration 7) A seventh aspect of the present invention is the reflective mask blank according to the fifth aspect, wherein the alloy has a refractive index falling within the range of 0.901 to 0.907 and an extinction coefficient falling within the range of 0.035 to 0.041.

[0028] The reflective mask blank of the present invention having the sixth or seventh configuration has a refractive index and an extinction coefficient within a predetermined range, and thus can easily obtain a phase shift film having a high degree of flexibility in reflectance that can accommodate a plurality of reflectances simply by changing the film thickness.

[0029] (Configuration 8) An eighth aspect of the present invention is the reflective mask blank according to any one of the first to seventh aspects, wherein the alloy is a multi-component alloy containing three or more metal elements.

[0030] In the reflective mask blank of configuration 8 of the present invention, by making the phase shift film a multi-component alloy containing three or more metal elements, it is possible to easily adjust the phase shift film to have optimal refractive index and extinction coefficient to achieve desired phase difference characteristics and desired reflectance characteristics.

[0031] (Configuration 9) A ninth aspect of the present invention is the reflective mask blank according to any one of the first to eighth aspects, wherein the phase shift film has a thickness of 25 nm or more and 70 nm or less.

[0032] In the reflective mask blank of the ninth aspect of the present invention, the thickness of the phase shift film is 25 nm or more and 70 nm or less, so that the shadowing effect can be reduced.

[0033] (Configuration 10) A tenth aspect of the present invention is the reflective mask blank according to any one of the first to ninth aspects, wherein the uppermost layer of the multilayer reflective film on the phase shift film side comprises a protective film.

[0034] In the reflective mask blank of the tenth aspect of the present invention, the uppermost layer of the multilayer reflective film on the side of the phase shift film is provided with a protective film, which can suppress damage to the surface of the multilayer reflective film when a reflective mask is manufactured using the reflective mask blank, thereby improving the reflective property of the reflective mask with respect to EUV light.

[0035] (Configuration 11) An eleventh aspect of the present invention is a reflective mask comprising a phase shift film pattern formed by patterning the phase shift film in the reflective mask blank according to any one of the first to tenth aspects.

[0036] The reflective mask of the eleventh aspect of the present invention is manufactured using the above-mentioned reflective mask blank, and therefore it is possible to obtain a reflective mask having a phase shift film pattern having desired phase difference characteristics and desired reflectance characteristics.

[0037] (Configuration 12) A method for manufacturing a semiconductor device, comprising the step of forming a pattern on a semiconductor substrate by using the reflective mask according to the eleventh aspect.

[0038] According to the manufacturing method of a semiconductor device of configuration 12 of the present invention, a reflective mask having a phase shift film pattern with desired phase difference characteristics and desired reflectance characteristics can be used, so that a semiconductor device having a fine and highly accurate transfer pattern can be manufactured. Effect of the Invention

[0039] According to the present invention, when a plurality of reflective mask blanks are continuously manufactured, even if the film thickness of the phase shift film varies slightly from the design value, it is possible to stably provide reflective mask blanks having the desired phase difference characteristics and the desired reflectance characteristics.

[0040] Furthermore, by using the reflective mask blank of the present invention, a reflective mask having a phase shift film pattern having desired phase difference characteristics and desired reflectance characteristics can be obtained.

[0041] Furthermore, the semiconductor device manufacturing method of the present invention makes it possible to use a reflective mask having a phase shift film pattern with desired phase difference characteristics and desired reflectance characteristics, thereby making it possible to manufacture a semiconductor device having a fine and highly accurate transfer pattern. [Brief description of the drawings]

[0042] [Figure 1] 1 is a cross-sectional view for explaining a schematic configuration of a reflective mask blank for EUV lithography according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing the characteristics of the refractive index n and the extinction coefficient k of a metal material in EUV light (wavelength 13.5 nm) for explaining a first embodiment of the present invention. [Diagram 3] 1 is a graph showing the characteristics of the refractive index n and the extinction coefficient k of a metal material in EUV light (wavelength 13.5 nm) for explaining a first embodiment of the present invention. [Figure 4]1 is a graph illustrating the refractive index n and extinction coefficient k characteristics of an alloy that satisfies predetermined phase difference characteristics and reflectance characteristics when the reflectance for EUV light (wavelength 13.5 nm) is 6%, for explaining a first embodiment of the present invention. [Diagram 5] 1 is a graph illustrating the refractive index n and extinction coefficient k characteristics of an alloy that satisfies predetermined phase difference characteristics and reflectance characteristics when the reflectance for EUV light (wavelength 13.5 nm) is 4%, for explaining a first embodiment of the present invention. [Figure 6] 1 is a graph illustrating the refractive index n and extinction coefficient k characteristics of an alloy that satisfies predetermined phase difference characteristics and reflectance characteristics when the reflectance for EUV light (wavelength 13.5 nm) is 20%, for explaining a first embodiment of the present invention. [Figure 7] 11 is a graph illustrating a range of refractive index n and extinction coefficient k that satisfies predetermined phase difference characteristics and reflectance characteristics when the reflectance for EUV light (wavelength 13.5 nm) is 4%, 6%, and 12%, for explaining a second embodiment of the present invention. [Figure 8] 8 is a graph showing the range of the refractive index n and the extinction coefficient k that satisfies the overlapping portion of FIG. 7, for explaining the third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the following embodiments are forms for embodying the present invention, and are not intended to limit the scope of the present invention.

[0044] [First embodiment] Fig. 1 shows a schematic cross-sectional view of a reflective mask blank 10 according to a first embodiment of the present invention. In the reflective mask blank 10 of this embodiment, a multilayer reflective film 13 and a phase shift film 15 for shifting the phase of EUV light are formed in this order on a substrate 12. Note that the reflective mask blank 10 for EUV lithography having the configuration shown in Fig. 1 can also be used in the second and third embodiments of the present invention described later.

[0045] The phase shift film 15 of the reflective mask blank 10 of the first embodiment of the present invention is made of a material consisting of an alloy containing two or more metals so that the reflectance of the surface of the phase shift film 15 to EUV light (wavelength: 13.5 nm) is more than 3% and less than 20%, and the phase shift film 15 has a phase difference of 170 degrees to 190 degrees with respect to the reflected light from the multilayer reflective film 13.

[0046] The alloy constituting the phase shift film 15 is a group of metal elements satisfying the refractive index n and extinction coefficient k in the following formula (1) where n is the refractive index and k is the extinction coefficient at the wavelength of EUV light (wavelength: 13.5 nm), and the group of metal elements satisfying the refractive index n and extinction coefficient k in the following formula (2) are group A and group B, respectively, and the alloy is selected from group A and group B, and the composition ratio is adjusted so that the change in the phase difference is within a range of ±2 degrees and the change in the reflectance is within a range of ±0.2% when the film thickness of the phase shift film 15 varies by ±0.5% from the set film thickness. The change in the phase difference is within a range of ±2 degrees, where the phase difference θ is in a range of θ0-2 degrees≦θ≦θ0+2 degrees when the target phase difference is θ0. The change in the reflectance is within a range of ±0.2%, where the target reflectance is R0. In this specification, "*" is a multiplication symbol. k>α*n+β Equation (1) k<α*n+β (2) (where α is a proportional constant and β is a constant.)

[0047] FIG. 2 is a graph showing the relationship between the refractive index n and the extinction coefficient k of a metal material in EUV light (wavelength 13.5 nm).

[0048] The alloy constituting the phase shift film 15 of the present invention has α and β appropriately set according to the reflectance of the surface of the phase shift film 15 to EUV light, and one or more metal elements are selected from each of Group A and Group B, which are metal element groups satisfying the relational expressions (1) and (2) above, and the composition ratio is adjusted so that the change in phase difference is within the range of ±2 degrees and the change in reflectance is within the range of ±0.2% when the film thickness of the phase shift film 15 varies by ±0.5% from the set film thickness.

[0049] The following equation (3) is an approximate straight line passing through multiple alloy materials (Alloy A, Alloy B, Alloy C, Alloy D, Alloy E) when plotted in Figure 2, for which the phase difference of phase shift film 15 changes within a range of ±2 degrees and the reflectance changes within a range of ±0.2% when the thickness of phase shift film 15 varies by ±0.5% from the set thickness. k = α*n+β (3)

[0050] In Fig. 2, metal elements belonging to group A that satisfy formula (1) (k>α*n+β) include Pd, Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ni, Hf, Fe, Cu, Te, Zn, Mg, Ge, and Al. Metal elements belonging to group B that satisfy formula (2) (k<α*n+β) include Rh, Ru, Mo, Nb, Ti, Zr, Y, and Si.

[0051] For example, in the case of a binary alloy, alloy A can be made into a PdMo alloy (binary alloy) by selecting Pd belonging to group A and Mo belonging to group B. This PdMo alloy has a refractive index n A and the extinction coefficient k A The alloy A has a composition ratio that satisfies the above.

[0052] When the phase shift film 15 is made of a material made of a multi-element alloy containing a plurality of metal elements, a plurality of elements are selected from group A and a plurality of elements are selected from group B, and the composition ratio of the alloy containing these selected elements is adjusted to adjust the refractive index n A and the extinction coefficient k AAlloy A satisfies the refractive index n B and the extinction coefficient k B Alloy B, which satisfies the refractive index n C and the extinction coefficient k C Alloy C, or refractive index n D and the extinction coefficient k D It is possible to make alloy D satisfying the above.

[0053] 3 shows a case where the phase shift film 15 of the present invention is made of a material consisting of a ternary alloy as a multi-element alloy. When the thickness of the phase shift film 15 varies by ±0.5% from the set thickness, the phase difference of the phase shift film 15 changes within a range of ±2 degrees and the reflectance changes within a range of ±0.2%. For example, by selecting Pd and Ta belonging to group A and Mo belonging to group B, a TaPdMo alloy (ternary alloy) can be obtained. The TaPdMo alloy can be made into the above-mentioned alloy A, alloy B, alloy C, or alloy D by adjusting the composition ratio.

[0054] <Configuration of Reflective Mask Blank 10 and Its Manufacturing Method> 1 shows a schematic cross-sectional view for explaining the configuration of a reflective mask blank 10 for EUV lithography according to a first embodiment of the present invention. The reflective mask blank 10 of the present invention will be explained with reference to FIG.

[0055] As shown in FIG. 1, a reflective mask blank 10 includes a substrate 12 having a back conductive film 11 for electrostatic chuck formed on the main surface on the back side of the substrate 12, a multilayer reflective film 13 formed on the main surface of the substrate 12 (the main surface opposite to the side on which the back conductive film 11 is formed) and reflecting EUV light, which is the exposure light, a protective film 14 formed on the top layer of the multilayer reflective film 13 from a material mainly composed of ruthenium (Ru) for protecting the multilayer reflective film 13, and a phase shift film 15 formed on the protective film 14 and absorbing EUV light while reflecting a portion of the EUV light and shifting its phase.

[0056] In this specification, for example, the expression "multilayer reflective film 13 formed on the main surface of substrate 12" not only means that multilayer reflective film 13 is disposed in contact with the surface of substrate 12, but also includes the case where other films are present between substrate 12 and multilayer reflective film 13. The same applies to other films. In addition, in this specification, for example, "film A is disposed on and in contact with film B" means that film A and film B are disposed so as to be in direct contact with each other, with no other film between them.

[0057] The structure of the substrate 12 and each layer will now be described.

[0058] In order to prevent distortion of the absorber film pattern due to heat during exposure to EUV light, a material having a low thermal expansion coefficient within the range of 0±5 ppb / ° C. is preferably used as the substrate 12. Examples of materials having a low thermal expansion coefficient within this range include SiO2-TiO2 glass, multi-component glass ceramics, etc.

[0059] Of the two main surfaces of the substrate 12, the main surface on which the phase shift film 15 that becomes the transfer pattern of the reflective mask is formed is surface-processed to have a high flatness from the viewpoint of obtaining at least pattern transfer accuracy and positional accuracy. In the case of EUV exposure, the flatness is preferably 0.1 μm or less, more preferably 0.05 μm or less, and particularly preferably 0.03 μm or less in a 132 mm×132 mm area of ​​the main surface on which the transfer pattern of the substrate 12 is formed. In addition, of the two main surfaces of the substrate 12, the main surface opposite to the side on which the phase shift film 15 is formed is the surface on which the back conductive film 11 is formed for electrostatic chucking when set in an exposure device. The flatness of the surface on which the back conductive film 11 is formed is preferably 1 μm or less, more preferably 0.5 μm or less, and particularly preferably 0.3 μm or less in a 142 mm×142 mm area.

[0060] In this specification, flatness is a value that indicates the warpage (deformation amount) of the surface indicated by TIR (Total Indicated Reading). This value is the absolute value of the difference in height between the highest point on the surface of the substrate 12 above the focal plane, which is determined by the least squares method with the surface of the substrate 12 as the reference plane, and the lowest point on the surface of the substrate 12 below the focal plane.

[0061] In the case of EUV exposure, the surface smoothness required for substrate 12 is preferably 0.1 nm or less in root mean square roughness (RMS) for the main surface of substrate 12 on which phase shift film 15, which serves as a transfer pattern, is formed. The surface smoothness can be measured with an atomic force microscope (AFM).

[0062] Furthermore, the substrate 12 preferably has high rigidity to prevent deformation due to film stress of the films (such as the multilayer reflective film 13) formed thereon. In particular, the substrate 12 preferably has a high Young's modulus of 65 GPa or more.

[0063] The multilayer reflective film 13 has a function of reflecting EUV light in a reflective mask for EUV lithography. The multilayer reflective film 13 is a multilayer film in which elements having different refractive indices are periodically laminated.

[0064] Generally, a multilayer film in which a thin film (high refractive index layer) of a light element or its compound, which is a high refractive index material, and a thin film (low refractive index layer) of a heavy element or its compound, which is a low refractive index material, are alternately stacked for about 40 to 60 periods, is used as the multilayer reflective film 13. The multilayer film can have a structure in which a multilayer structure of a high refractive index layer / low refractive index layer in which a high refractive index layer and a low refractive index layer are stacked in this order from the substrate 12 side is stacked multiple times as one period. The multilayer film can also have a structure in which a multilayer structure of a low refractive index layer / high refractive index layer in which a low refractive index layer and a high refractive index layer are stacked in this order from the substrate 12 side is stacked multiple times as one period. Note that the top layer of the multilayer reflective film 13, that is, the surface layer of the multilayer reflective film 13 on the side opposite to the substrate 12, is preferably a high refractive index layer. In the above-mentioned multilayer film, when a multilayer structure of a high refractive index layer / low refractive index layer in which a high refractive index layer and a low refractive index layer are stacked in this order from the substrate 12 is stacked multiple times as one period, the top layer is a low refractive index layer. Therefore, it is preferable to form the multilayer reflective film 13 by further forming a high refractive index layer on the uppermost low refractive index layer.

[0065] In the reflective mask blank 10 of the present invention, a layer containing Si can be used as the high refractive index layer. The material containing Si may be a Si compound containing B, C, N, and / or O in addition to simple Si. By using a layer containing Si as the high refractive index layer, a reflective mask for EUV lithography having excellent reflectance of EUV light can be obtained. In the reflective mask blank 10 of the present invention, a glass substrate is preferably used as the substrate 12. Si also has excellent adhesion to a glass substrate. As the low refractive index layer, a simple metal selected from Mo, Ru, Rh, and Pt, and an alloy thereof are used. As the multilayer reflective film 13 for EUV light having a wavelength of 13 to 14 nm, for example, a Mo / Si periodic laminate film in which Mo films and Si films are alternately laminated for about 40 to 60 periods is preferably used. Note that the high refractive index layer, which is the top layer of the multilayer reflective film 13, may be formed of silicon (Si), and a silicon oxide layer containing silicon and oxygen may be formed between the top layer (Si) and the protective film 14. This can improve mask cleaning resistance (resistance to film peeling of the phase shift film pattern).

[0066] The reflectance of such a single multilayer reflective film 13 is, for example, 65% or more, and the upper limit is usually preferably 73%. The film thickness and number of periods of each constituent layer of the multilayer reflective film 13 are appropriately selected so as to satisfy Bragg's law according to the exposure wavelength. The multilayer reflective film 13 has a plurality of high refractive index layers and a plurality of low refractive index layers. All the high refractive index layers do not have to have the same film thickness. Also, all the low refractive index layers do not have to have the same film thickness. Also, the film thickness of the Si layer on the outermost surface of the multilayer reflective film 13 can be adjusted within a range that does not reduce the reflectance. The film thickness of the Si (high refractive index layer) on the outermost surface can be, for example, 3 to 10 nm.

[0067] The method of forming the multilayer reflective film 13 is known in the art. For example, the multilayer reflective film 13 can be formed by depositing each layer by ion beam sputtering. In the case of the above-mentioned Mo / Si periodic multilayer film, for example, a Si film having a thickness of about 4 nm is first deposited on the substrate 12 by ion beam sputtering using a Si target, and then a Mo film having a thickness of about 3 nm is deposited using a Mo target. The deposition of a Si film and a Mo film constitutes one period, and 40 to 60 periods are stacked in total to form the multilayer reflective film 13 (the uppermost layer is a Si layer).

[0068] The reflective mask blank 10 of the present invention preferably has a protective film 14 as the uppermost layer of the multilayer reflective film 13 on the phase shift film 15 side.

[0069] As shown in FIG. 1, the protective film 14 is formed on the multilayer reflective film 13 to protect the multilayer reflective film 13 from dry etching or cleaning liquid in the manufacturing process of the reflective mask described later. The protective film 14 is made of, for example, a material containing Ru (ruthenium) as a main component (main component: 50 atomic % or more). The material containing Ru as a main component can be a simple Ru metal, a Ru alloy containing metals such as Nb, Zr, Y, B, Ti, La, Mo, Co, and / or Re in Ru, or a material containing N (nitrogen) in these materials. The protective film 14 can also have a laminated structure of three or more layers, with the bottom layer and the top layer being layers made of the above-mentioned Ru-containing substance, and a metal other than Ru or an alloy being interposed between the bottom layer and the top layer.

[0070] The thickness of the protective film 14 is not particularly limited as long as it can function as the protective film 14. From the viewpoint of reflectance of EUV light, the thickness of the protective film 14 is preferably 1.5 to 8.0 nm, and more preferably 1.8 to 6.0 nm.

[0071] Any known film forming method can be used without any particular limitation as a method for forming the protective film 14. Specific examples of the method for forming the protective film 14 include a sputtering method and an ion beam sputtering method.

[0072] 1, a reflective mask blank 10 of the first embodiment of the present invention includes a phase shift film 15 on a multilayer reflective film 13. The phase shift film 15 can be formed on and in contact with the multilayer reflective film 13. Furthermore, in the case where a protective film 14 is formed on the uppermost layer of the multilayer reflective film 13, the phase shift film 15 can be formed on and in contact with the protective film 14.

[0073] The alloy constituting the phase shift film 15 of the present invention has α and β appropriately set according to the reflectivity of the surface of the phase shift film 15 to EUV light, and one or more metal elements are selected from each of Group A and Group B, which are metal element groups satisfying the above-mentioned relational expressions (1) (k>α*n+β, α: proportional constant, β: constant) and (2) (k<α*n+β, α: proportional constant, β: constant), and the composition ratio is adjusted so that the change in the phase difference is within the range of ±2 degrees when the thickness of the phase shift film 15 varies by ±0.5% from the set thickness, and the change in reflectivity is within the range of ±0.2%.

[0074] The following describes three cases in which the reflectance of the phase shift film 15 to EUV light is (i) more than 5% and not more than 10%, (ii) more than 3% and not more than 5%, and (iii) more than 10% and not more than 20%.

[0075] (i) The reflectance of the phase shift film 15 to EUV light is more than 5% and 10% or less. When the reflectance of the surface of the phase shift film 15 to EUV light is more than 5% and not more than 10%, the formulas (1) and (2) are as follows: k>-0.303*n+0.309...Equation (1) k<-0.303*n+0.309...Equation (2) As the metal elements belonging to group A that satisfy formula (1) (k>-0.303*n+0.309), Pd, Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ni, Fe, Hf, Cu, Te, Zn, Mg, Ge, and Al are listed. As the metal elements belonging to group B that satisfy formula (2) (k<-0.303*n+0.309), Rh, Ru, Mo, Nb, Ti, Zr, Y, and Si are listed. At least one metal element is selected from each of group A and group B, and the composition ratio is adjusted so that the change in the phase difference is within a range of ±2 degrees and the change in the reflectance is within a range of ±0.2% when the thickness of the phase shift film varies by ±0.5% from the set thickness.

[0076] FIG. 4 is a diagram for explaining groups A and B, which are metal element groups that satisfy the relational expressions (1) and (2) when the reflectance of the surface of the phase shift film 15 to EUV light is 6%.

[0077] As a binary alloy in which the phase difference of the phase shift film 15 changes within a range of ±2 degrees and the reflectance changes within a range of ±0.2% when the thickness of the phase shift film 15 changes by ±0.5% from the set thickness, alloy A having a refractive index of 0.883 and an extinction coefficient of 0.042 is used. 6% Examples of alloys include PdMo alloys, PdNb alloys, and PdZr alloys. Alloy B has a refractive index of 0.905 and an extinction coefficient of 0.035. 6% Examples of the alloys include RhTa alloy and RuNi alloy. The alloy C has a refractive index of 0.921 and an extinction coefficient of 0.031. 6% Examples of such alloys include TaRu alloy and CrRu alloy. The alloy D has a refractive index of 0.932 and an extinction coefficient of 0.027. 6% Examples of such alloys include MoTa alloy and WNb alloy. The alloy E has a refractive index of 0.940 and an extinction coefficient of 0.024. 6% Examples of the alloy include TaNb alloy and NiNb alloy.

[0078] As for ternary alloys, TaPdMo alloy and NiPdMo alloy are used. 6% , alloy B 6% , alloy C 6% , or Alloy D 6% It can be said that:

[0079] In addition, the above alloy A 6% , alloy B 6% , alloy C 6% , alloy D 6% , and Alloy E 6% By setting the film thicknesses to 28.2 nm, 35.0 nm, 41.5 nm, 48.2 nm, and 55.1 nm, respectively, the phase difference of the phase shift film 15 can be set to about 180 degrees, and the reflectance can be set to about 6%.

[0080] (ii) The reflectance of the phase shift film 15 to EUV light is more than 3% and 5% or less. When the reflectance of the surface of the phase shift film 15 to EUV light is more than 3% and not more than 5%, the formulas (1) and (2) are as follows: k>-0.331*n+0.339...Equation (1) k<-0.331*n+0.339...Equation (2) As the metal elements belonging to group A that satisfy formula (1) (k>-0.331*n+0.339), there are Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, Ni, Hf, Cu, Te, Zn, Mg, Ge, and Al. As the metal elements belonging to group B that satisfy formula (2) (k<-0.331*n+0.339), there are Pd, Rh, Ru, Mo, Nb, V, Ti, Zr, Y, and Si. At least one metal element is selected from each of group A and group B, and the composition ratio is adjusted so that the change in the phase difference is within a range of ±2 degrees and the change in the reflectance is within a range of ±0.2% when the thickness of the phase shift film varies by ±0.5% from the set thickness.

[0081] FIG. 5 is a diagram for explaining groups A and B, which are metal element groups that satisfy the relational expressions (1) and (2) when the reflectance of the surface of the phase shift film 15 to EUV light is 4%.

[0082] As a binary alloy in which the phase difference of the phase shift film 15 changes within a range of ±2 degrees and the reflectance changes within a range of ±0.2% when the thickness of the phase shift film 15 changes by ±0.5% from the set thickness, alloy A having a refractive index of 0.881 and an extinction coefficient of 0.047 is used. 4% Examples of alloys include RhAg alloy, PdFe alloy, and PdZn alloy. Alloy B has a refractive index of 0.905 and an extinction coefficient of 0.040. 4% Examples of such alloys include RhFe alloys and RhZn alloys. The alloy C has a refractive index of 0.921 and an extinction coefficient of 0.035. 4% Examples of alloys include CrRu alloy and RhHf alloy. The alloy D has a refractive index of 0.932 and an extinction coefficient of 0.031. 4% Examples of such alloys include NbW alloy and ZrPt alloy. The alloy E has a refractive index of 0.940 and an extinction coefficient of 0.028. 4% Examples of the alloy include a CrZr alloy, a WZr alloy, and a TaNb alloy.

[0083] In addition, the above alloy A 4% , alloy B 4% , alloy C 4% , alloy D 4% , and Alloy E4% By setting the film thicknesses to 28.4 nm, 34.9 nm, 41.4 nm, 48.1 nm, and 55.0 nm, respectively, the phase difference of the phase shift film 15 can be set to about 180 degrees, and the reflectance can be set to about 4%.

[0084] (iii) The phase shift film 15 has a logarithmic reflectance of more than 10% and less than 20% for EUV light. When the reflectance of the surface of the phase shift film 15 to EUV light is more than 10% and not more than 20%, the formulas (1) and (2) are as follows: k>-0.192*n+0.194...Equation (1) k<-0.192*n+0.194...Equation (2) As the metal elements belonging to group A that satisfy formula (1) (k>-0.192*n+0.194), Rh, Pd, Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ni, Ti, Hf, Cu, Te, Zn, Mg, Ge, and Al are listed. As the metal elements belonging to group B that satisfy formula (2) (k<-0.192*n+0.194), Ru, Mo, Nb, Zr, Y, and Si are listed. At least one metal element is selected from each of group A and group B, and the composition ratio is adjusted so that the change in the phase difference is within a range of ±2 degrees and the change in the reflectance is within a range of ±0.2% when the thickness of the phase shift film varies by ±0.5% from the set thickness.

[0085] As a binary alloy in which the phase difference of the phase shift film 15 changes within a range of ±2 degrees and the reflectance changes within a range of ±0.2% when the thickness of the phase shift film 15 changes by ±0.5% from the set thickness, alloy A having a refractive index of 0.885 and an extinction coefficient of 0.025 is used. 20% Examples of such alloys include PdRu alloys, with a refractive index of 0.907 and an extinction coefficient of 0.021. 20% Examples of such alloys include PdMo alloys and RuGe alloys. The alloy C has a refractive index of 0.922 and an extinction coefficient of 0.018. 20% The MoCo alloy has a refractive index of 0.932 and an extinction coefficient of 0.016. 20% Examples of such alloys include WNb alloy and MoHf alloy, and the alloy E has a refractive index of 0.940 and an extinction coefficient of 0.014.20% Examples of the alloy include HfNb alloy and ZnNb alloy.

[0086] In addition, the above alloy A 20% , alloy B 20% , alloy C 20% , alloy D 20% , and Alloy E 20% By setting the film thicknesses to 28.2 nm, 35.0 nm, 41.7 nm, 48.6 nm, and 55.4 nm, respectively, the phase difference of the phase shift film 15 can be set to about 180 degrees, and the reflectance can be set to about 20%.

[0087] The phase shift film 15 of the present invention may contain at least one element selected from oxygen, nitrogen, carbon, and boron within the scope of the invention.

[0088] The thickness of the phase shift film 15 is appropriately set so that the phase difference with respect to EUV light is 170 degrees to 190 degrees and the reflectance is more than 3% and not more than 20%. From the viewpoint of reducing the shadowing effect, the thickness of the phase shift film 15 is preferably 25 nm to 70 nm, more preferably 25 nm to 50 nm, and even more preferably 25 nm to 40 nm.

[0089] If the surface of the phase shift film 15 is not smooth, the edge roughness of the phase shift film pattern may become large, resulting in poor dimensional accuracy of the pattern. For this reason, the surface roughness of the phase shift film 15 after deposition is preferably 0.5 nm or less, more preferably 0.4 nm or less, and even more preferably 0.3 nm or less, in root mean square roughness (RMS).

[0090] In the reflective mask blank of the present invention, an etching mask film (not shown) can be further formed on the phase shift film 15. The etching mask film is made of a material that has etching selectivity with respect to the uppermost layer of the multilayer reflective film 13 and can be etched (has no etching selectivity) with an etching gas for the phase shift film 15. The etching mask film can be formed by a known method such as a DC sputtering method or an RF sputtering method.

[0091] The thickness of the etching mask film is preferably 5 nm or more from the viewpoint of ensuring the function as a hard mask. In consideration of the thickness of the phase shift film 15, the thickness of the etching mask film is desirably 5 nm or more and 20 nm or less, more preferably 5 nm or more and 15 nm or less.

[0092] As shown in FIG. 1, a back conductive film 11 for electrostatic chuck is formed on the back side of the substrate 12 (opposite to the surface on which the multilayer reflective film 13 is formed). The electrical characteristic required for the back conductive film 11 for electrostatic chuck is usually a sheet resistance of 100 Ω / sq or less. The back conductive film 11 can be formed by magnetron sputtering or ion beam sputtering using a target of a metal such as chromium or tantalum, or an alloy thereof. When the back conductive film 11 is formed of CrN, for example, it can be formed by the above-mentioned sputtering method using a Cr target in a gas atmosphere containing N such as nitrogen gas. The thickness of the back conductive film 11 is not particularly limited as long as it satisfies the function for electrostatic chuck, but is usually 10 to 200 nm.

[0093] The reflective mask blank 10 of the present invention is not limited to the above-mentioned embodiment. For example, the reflective mask blank 10 of the present invention can have a resist film that functions as an etching mask on the phase shift film 15. The reflective mask blank 10 of the present invention can have a phase shift film 15 on and in contact with the multilayer reflective film 13 without having a protective film 14 on the multilayer reflective film 13.

[0094] <Reflection mask and its manufacturing method> The present invention is a reflective mask having a phase shift film pattern formed by patterning the phase shift film 15 in the above-mentioned reflective mask blank 10 of the present invention. The above-mentioned reflective mask blank 10 of the present invention can be used to produce the reflective mask of the present invention. For the manufacture of a reflective mask for EUV lithography, electron beam lithography, which can perform high-definition patterning, is most suitable.

[0095] In this embodiment, a method for manufacturing a reflective mask using photolithography will be described by taking as an example a case in which a reflective mask blank 10 shown in FIG. 1 is used.

[0096] First, a resist film (not shown) is formed on the outermost surface (phase shift film 15) of the reflective mask blank 10 shown in Fig. 1. The thickness of the resist film may be, for example, 100 nm. Next, a desired pattern is drawn (exposed) on the resist film, and the resist film is developed and rinsed to form a predetermined resist pattern (not shown).

[0097] Next, using a resist pattern (not shown) as a mask, the phase shift film 15 is dry-etched with an etching gas containing a fluorine-based gas such as SF6 or a chlorine-based gas such as Cl2 depending on the material of the phase shift film 15, thereby forming a phase shift film pattern (not shown). In this process, the resist pattern (not shown) is removed.

[0098] Here, the etching rate of the phase shift film 15 depends on the material from which the phase shift film 15 is formed, the etching gas, and other conditions.

[0099] The above steps form a phase shift film pattern. Next, wet cleaning is performed using an acidic or alkaline aqueous solution to obtain a reflective mask for EUV lithography that achieves high reflectance.

[0100] In addition, the etching gas may be a fluorine-based gas such as SF6, CHF3, CF4, C2F6, C3F6, C4F6, C4F8, CH2F2, CH3F, C3F8, and F, or a mixed gas containing these fluorine gases and O2 at a predetermined ratio. In addition, other etching gases may be, for example, chlorine-based gases such as Cl2, SiCl4, CHCl3, CCl4, and BCl3, or a mixed gas thereof, a mixed gas containing a chlorine-based gas and He at a predetermined ratio, a mixed gas containing a chlorine-based gas and Ar at a predetermined ratio, a halogen gas containing at least one selected from fluorine gas, chlorine gas, bromine gas, and iodine gas, and at least one or more selected from the group consisting of hydrogen halide gas, and further, a mixed gas containing these gases and oxygen gas, etc. may be used.

[0101] Since the above-mentioned reflective mask blank 10 is used to manufacture the reflective mask of the present invention, it is possible to obtain a reflective mask having a phase shift film pattern with desired phase difference characteristics and reflectance characteristics.

[0102] <Manufacturing of semiconductor devices> The present invention is a method for manufacturing a semiconductor device, which includes a pattern forming step of forming a pattern on a semiconductor substrate using the above-mentioned reflective mask of the present invention.

[0103] Using the above-mentioned reflective mask of the present invention, a transfer pattern based on the phase shift film pattern of the reflective mask can be formed on a semiconductor substrate by EUV lithography. After that, by going through various other processes, a semiconductor device in which various patterns and the like are formed on the semiconductor substrate can be manufactured. A known pattern transfer device can be used to form the transfer pattern.

[0104] According to the semiconductor device manufacturing method of the present invention, a reflective mask having a phase shift film pattern in which the phase difference and reflectance have a small film thickness dependency can be used, so that a semiconductor device having a fine and highly accurate transfer pattern can be manufactured.

[0105] [Second embodiment] The phase shift film 15 of the reflective mask blank 10 in the second embodiment of the present invention has a wider allowable range for phase difference variation and reflectance variation than in the first embodiment.

[0106] The phase shift film 15 is made of a material made of an alloy containing two or more metals so that the reflectance R0 of the EUV light on the surface of the phase shift film for the light reflected from the multilayer reflective film before the formation of the phase shift film 15 is 4%, 6% or 12% and the phase difference θ0 is 180 degrees. This alloy has a refractive index n and an extinction coefficient k at the wavelength of EUV light, and its composition ratio is adjusted so that the allowable range of the phase difference θ when the film thickness of the phase shift film 15 varies by ±0.5% from the set film thickness is ±5 degrees (θ0-5 degrees≦θ≦θ0+5 degrees), and the allowable range of the reflectance R is 0.9R0≦R≦1.1R0.

[0107] FIG. 7 is a graph showing the range of the refractive index n and the extinction coefficient k that satisfy predetermined phase difference characteristics and reflectance characteristics when the reflectance for EUV light (wavelength 13.5 nm) is 4%, 6%, and 12%.

[0108] Spiral H in Figure 7 6% is a set of plots of refractive indexes and extinction coefficients in which the allowable range of phase difference θ is ±5 degrees (θ0-5 degrees≦θ≦θ0+5 degrees) when the thickness of the phase shift film 15 varies by ±0.5% from the set thickness, and the allowable range of reflectance R is 0.9R0≦R≦1.1R0, when the phase difference θ with respect to EUV light is 180 degrees and the reflectance R is 6%. Here, the allowable range of phase difference θ is 175 degrees to 185 degrees, and the allowable range of reflectance R is 5.4% to 6.6%.

[0109] Similarly, the spiral H in Fig. 7 4% In the case where the phase difference θ0 with respect to the EUV light is 180 degrees and the reflectance R0 is 4%, the allowable range of the phase difference θ is 175 degrees to 185 degrees and the allowable range of the reflectance R is 3.6% to 4.4%. 12%In this case, the phase difference θ0 with respect to the EUV light is 180 degrees and the reflectance R0 is 12%, and the allowable range of the phase difference θ is 175 degrees to 185 degrees, and the allowable range of the reflectance R is 10.8% to 13.2%.

[0110] The alloy is, as in the first embodiment, 4% , spiral H 6% Or Spiral H 12% The helical structure can be obtained by dividing the helical structure into groups A' and B', and selecting one or more metal elements from each of groups A' and B'. 6% When the elements contained in are group A', for example, metal elements belonging to group A' include Ag, Pt, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ni, Hf, Fe, Cu, Te, Zn, Mg, Ge, and Al. Metal elements belonging to group B' include Au, Pd, Rh, Ru, Mo, Nb, Ti, Zr, and Y.

[0111] In the second embodiment of the present invention, a reflective mask blank 10 and a reflective mask can be manufactured in the same manner as in the first embodiment of the present invention, except that the material of the phase shift film 15 is configured as described above.

[0112] [Third embodiment] The phase shift film 15 of the reflective mask blank 10 in the third embodiment of the present invention will be described. When manufacturing a plurality of reflective mask blanks, reflective mask blanks each having a different reflectance may be manufactured, but it is difficult to obtain a phase shift film that has the desired phase difference characteristics and reflectance characteristics and can accommodate a plurality of reflectances without changing the material (and further the composition ratio). The phase shift film 15 in the third embodiment of the present invention is made of a material made of an alloy that can accommodate a plurality of reflectances simply by changing the set film thickness.

[0113] The phase shift film 15 is made of a material made of an alloy containing two or more metals so that the reflectance R0 of the EUV light on the surface of the phase shift film for the light reflected from the multilayer reflective film before the formation of the phase shift film 15 is 4%, 6% or 12% and the phase difference θ0 is 180 degrees. This alloy has a refractive index n and an extinction coefficient k at the wavelength of EUV light, and its composition ratio is adjusted so that the allowable range of the phase difference θ when the film thickness of the phase shift film 15 varies by ±0.5% from the set film thickness is ±5 degrees (θ0-5 degrees≦θ≦θ0+5 degrees) and the allowable range of the reflectance R is 0.9R0≦R≦1.1R0.

[0114] (i) When the reflectance R0 is set to 4%, 6%, and 12%, the reflectance can be increased to three values. FIG. 8 is a graph showing the range of the refractive index n and the extinction coefficient k that satisfy the overlapping portion of FIG. 7. 3A and Spot S 3B is a set of plots of refractive indexes and extinction coefficients that correspond to three reflectances R0 of 4%, 6%, and 12%. That is, the spot S 3A and Spot S 3B is the spiral H in Figure 7. 4% , spiral H 6% and Spiral H 12% This is the overlapping part.

[0115] Spot S 3A The refractive index is in the range of 0.877 to 0.881, and the extinction coefficient is in the range of 0.046 to 0.052. 3B The refractive index is in the range of 0.901 to 0.904, and the extinction coefficient is in the range of 0.039 to 0.041.

[0116] The alloy is, as in the first embodiment, Spot S 3A and Spot S 3BThe metal elements can be obtained by dividing the metal elements into Group A' and Group B' on either side of an approximate straight line connecting the metal elements A and B, and selecting one or more metal elements from each of Group A' and Group B'. For example, metal elements belonging to Group A' include Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ti, Ni, Hf, Fe, Cu, Te, Zn, Mg, Ge, Al, and Si. Metal elements belonging to Group B' include Pd, Rh, Ru, Mo, Nb, Zr, and Y.

[0117] Examples of binary alloys include AgPd alloys, PtPd alloys, AuPd alloys, IrPd alloys, CoPd alloys, SnPd alloys, NiPd alloys, TePd alloys, CuPd alloys, FePd alloys, WPd alloys, CrPd alloys, TaPd alloys, ZnPd alloys, HfPd alloys, GePd alloys, AlPd alloys, MgPd alloys, AgRh alloys, CuRh alloys, FeRh alloys, and IrRu alloys. For example, the composition ratio of the PtPd alloy is preferably 0.10:0.90 to 0.25:0.75.

[0118] (ii) When the reflectance R0 is set to 6% and 12%, the reflectance R0 can be adjusted to accommodate two reflectances. Spot S in Figure 8 2A , Spot S 2B , Spot S 2C , Spot S 2D and Spot S 2E is a set of plots of refractive indexes and extinction coefficients that can satisfy two reflectances R0 of 6% and 12%. That is, the spot S 2A , Spot S 2B , Spot S 2C , Spot S 2D and Spot S 2E is the spiral H in Figure 7. 6% and Spiral H 12% This is the overlapping area.

[0119] Spot S 2A is the above spot S 3A In addition to the range of the refractive index and extinction coefficient of spot S, the refractive index is in the range of 0.880 to 0.888 and the extinction coefficient is in the range of 0.041 to 0.046.2B is the above spot S 3B In addition to the range of the refractive index and extinction coefficient of 0.901 to 0.907, the refractive index is in the range of 0.035 to 0.041. 2C The refractive index is in the range of 0.917 to 0.921, and the extinction coefficient is in the range of 0.030 to 0.034. 2D The refractive index is in the range of 0.929 to 0.931, and the extinction coefficient is in the range of 0.027 to 0.028. 2E The refractive index is in the range of 0.938 to 0.939, and the extinction coefficient is in the range of 0.024.

[0120] The alloy is, as in the first embodiment, Spot S 2A (Spot S 3A (including Spot S) 2B (Spot S 3B (including Spot S) 2C , Spot S 2D and Spot S 2E The metal elements can be obtained by dividing the metal elements into Group A' and Group B' on either side of an approximate straight line connecting the metal elements A and B, and selecting one or more metal elements from each of Group A' and Group B'. For example, metal elements belonging to Group A' include Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ni, Hf, Fe, Cu, Te, Zn, Mg, Ge, Al, and Si. Metal elements belonging to Group B' include Pd, Rh, Ru, Mo, Nb, Ti, Zr, and Y.

[0121] Examples of binary alloys include, in addition to the alloys described in (i) above, PtMo alloys, AuMo alloys, NiMo alloys, FeMo alloys, ZnMo alloys, MnMo alloys, AgNb alloys, NiNb alloys, WNb alloys, TaNb alloys, MnPd alloys, VPd alloys, TiPd alloys, PtRh alloys, AuRh alloys, WRa alloys, CrRh alloys, TaRh alloys, ZnRh alloys, MnRh alloys, HfRh alloys, GeRh alloys, AlRh alloys, MgRh alloys, CoRu alloys, SnRu alloys, NiRu alloys, WRu alloys, CrRu alloys, TaRu alloys, ZnRu alloys, HfRu alloys, GeRu alloys, VRu alloys, IrY alloys, PtZr alloys, and AuZr alloys. For example, the composition ratio of the PtMo alloy is preferably 0.60:0.40 to 0.55:0.45.

[0122] In the third embodiment of the present invention, a reflective mask blank 10 and a reflective mask can be manufactured in the same manner as in the first embodiment of the present invention, except that the material of the phase shift film 15 is configured as described above. EXAMPLES

[0123] The present invention will be described below with reference to examples.

[0124] Example 1 <Preparation of Reflective Mask Blank 10> A reflective mask blank 10 of Example 1 having a phase shift film 15 with a reflectance of 6% was produced by the method described below. The reflective mask blank 10 of Example 1 has a structure in which a Mo / Si multilayer reflective film 13, a Ru protective film 14, and a phase shift film 15 are laminated on a substrate 12, and a CrN conductive film is formed on the rear surface of the substrate 12.

[0125] First, a SiO2-TiO2 glass substrate 12 was prepared.

[0126] A back surface conductive film 11 made of CrN was formed on the back surface of this substrate 12 by magnetron sputtering under the following conditions: Using a Cr target, the back surface conductive film 11 was formed to a thickness of 20 nm in an Ar+N2 gas atmosphere (Ar:N2=90%:N:10%).

[0127] Next, a multilayer reflective film 13 was formed on the main surface of the substrate 12 opposite to the side on which the back conductive film 11 was formed. A Mo / Si periodic multilayer reflective film 13 suitable for 13.5 nm EUV light was adopted as the multilayer reflective film 13 formed on the substrate 12. The multilayer reflective film 13 was formed by alternately laminating Mo layers and Si layers on the substrate 12 by ion beam sputtering (Ar gas atmosphere) using a Mo target and a Si target. First, a Si film was formed to a thickness of 4.2 nm, and then a Mo film was formed to a thickness of 2.8 nm. This constitutes one cycle, and 40 cycles were laminated in the same manner, and finally a Si film was formed to a thickness of 4.0 nm to form the multilayer reflective film 13 (total thickness: 284 nm).

[0128] Subsequently, a protective film 14 containing Ru was formed to a thickness of 2.5 nm on the uppermost Si film of the multilayer reflective film 13 by ion beam sputtering (in an Ar gas atmosphere) using a Ru target.

[0129] Next, a phase shift film 15 was formed on the protective film 14 by the following method. That is, sputtering was performed using a PdMo target (Pd:Mo=0.86:0.14) in an Ar gas atmosphere to form a phase shift film 15 made of a PdMo alloy with a set thickness of 28.2 nm, thereby obtaining a reflective mask blank 10. The composition ratio of the PdMo alloy in this phase shift film 15 is the same as that of the target.

[0130] Ten reflective mask blanks 10 were produced by the above-mentioned method, and the refractive index and extinction coefficient of the phase shift film 15 were measured using EUV light (wavelength 13.5 nm) for each reflective mask blank 10. As a result, the phase shift film 15 formed on the reflective mask blank 10 had a refractive index of 0.883 and an extinction coefficient of 0.042.

[0131] Therefore, in the phase shift film 15 of the obtained reflective mask blank 10, the phase difference variation was 180 degrees±1.3 degrees and the reflectance variation was 6%±0.1% according to simulation.

[0132] <Making a reflective mask> Next, ten reflective mask blanks 10 of the above-mentioned Example 1 were produced. A resist film was formed to a thickness of 100 nm on the phase shift film 15 of each of the ten produced reflective mask blanks, and a resist pattern was formed by drawing and developing. Then, using this resist pattern as a mask, the phase shift film 15 was dry-etched using fluorine-based SF6 gas to form a phase shift film pattern. Then, the resist pattern was removed to produce ten reflective masks.

[0133] For the ten reflective masks thus obtained, the phase difference and reflectance due to the reflected light from the phase shift film pattern surface and the reflected light from the multilayer reflective film surface were measured using EUV light. The phase difference variation was 180 degrees ±1.8 degrees, and the reflectance variation was 6% ±0.1%, both of which were small values.

[0134] <Manufacturing of semiconductor devices> The reflective mask obtained in Example 1 was set on an EUV scanner, and a wafer having a processed film and a resist film formed on a semiconductor substrate 12 was exposed to EUV light. The exposed resist film was developed, so that the processed film formed a resist pattern on the semiconductor substrate 12.

[0135] The reflective mask of Example 1 is a reflective mask on which a phase shift film pattern having the desired phase difference characteristics (phase difference variation of 180 degrees ±1.3 degrees) and reflectance characteristics (reflectance variation of 6% ±0.1%) is formed, and therefore a semiconductor device having a fine and highly accurate transfer pattern can be manufactured.

[0136] Furthermore, this resist pattern is transferred to the film to be processed by etching, and by going through various processes such as forming an insulating film or a conductive film, introducing a dopant, or annealing, it is possible to manufacture semiconductor devices with the desired characteristics with a high yield.

[0137] Example 2 A reflective mask blank and a reflective mask were produced in the same manner as in Example 1 above, except that phase shift film 15 was a TaPdMo alloy (Ta:Pd:Mo=0.015:0.869:0.116, set film thickness=28.2 nm).

[0138] As a result, the phase shift film 15 formed on the reflective mask blank 10 had a refractive index of 0.883 and an extinction coefficient of 0.042, and the phase difference variation obtained by simulation was 180 degrees ±1.3 degrees and the reflectance variation was 6% ±0.1%. The phase difference variation of the reflective mask was also small, being 180 degrees ±1.3 degrees and 6% ±0.1%, respectively.

[0139] (Examples 3 to 8) A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the material (alloy, composition ratio) and set film thickness of the phase shift film 15 in the above-mentioned Example 1 were changed to those shown in the following Table 1. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film 15 measured in the same manner as in Example 1 were as shown in Table 2.

[0140] [Table 1]

[0141] [Table 2]

[0142] In the above-mentioned Examples 3 to 8, the material of protective film 14 was appropriately selected from materials having etching resistance to the dry etching gas used when phase shift film 15 was patterned.

[0143] As the above results show, also in Examples 3 to 8, the phase difference variation and reflectance variation of the reflective mask blank and the reflective mask were small.

[0144] (Examples 9 to 10) In Example 9, a reflective mask blank 10 was produced in which the phase shift film 15 had a reflectance of 4%, and in Example 10, a reflective mask blank 10 was produced in which the phase shift film 15 had a reflectance of 20%. The rear surface conductive film 11, the multilayer reflective film 13, and the protective film 14 were the same as in Example 1.

[0145] A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the material (alloy, composition ratio) and set film thickness of the phase shift film 15 in the above-mentioned Example 1 were changed to those shown in the following Table 3. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film 15 measured in the same manner as in Example 1 were as shown in Table 4.

[0146] [Table 3]

[0147] [Table 4]

[0148] As the above results show, in Examples 9 and 10, the phase difference variations and reflectance variations of the reflective mask blanks and reflective masks were small.

[0149] The reflective masks of Examples 3 to 10 are reflective masks on which phase shift film patterns having desired phase difference characteristics (phase difference variation of 180 degrees ±2 degrees) and desired reflectance characteristics (reflectance variations of 6% ±0.1%, 4% ±0.1%, 20% ±0.1%) are formed, and therefore semiconductor devices having fine and high-precision transfer patterns can be manufactured.

[0150] Furthermore, this resist pattern is transferred to the film to be processed by etching, and by going through various processes such as forming an insulating film or a conductive film, introducing a dopant, or annealing, it is possible to manufacture semiconductor devices with the desired characteristics with a high yield.

[0151] (Examples 11 to 15) A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the material (alloy, composition ratio) and set film thickness of the phase shift film 15 in the above-mentioned Example 1 were changed to those shown in the following Table 5. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film 15 measured in the same manner as in Example 1 were as shown in Tables 6-1 and 6-2.

[0152] [Table 5]

[0153] [Table 6-1]

[0154] [Table 6-2]

[0155] In the above-mentioned Examples 11 to 15, the material of protective film 14 was appropriately selected from materials having etching resistance to the dry etching gas used when phase shift film 15 was patterned.

[0156] As the above results show, in Examples 11 to 15, the phase difference variation and reflectance variation of the reflective mask blank and the reflective mask were larger than those of Examples 1 to 10 at reflectances of 4%, 6% and 12%, but were within the allowable range. Moreover, by changing the film thickness without changing the material and composition ratio of the phase shift film, a phase shift film that satisfied the desired phase difference characteristics (phase difference variation of 180 degrees ±5 degrees) and the desired reflectance characteristics (0.9R0≦R≦1.1R0) could be obtained at reflectances of 4%, 6% and 12%, respectively.

[0157] The reflective masks of Examples 11 to 15 were reflective masks on which phase shift film patterns having desired phase difference characteristics (phase difference variation of 180 degrees ±5 degrees) and desired reflectance characteristics (0.9R0≦R≦1.1R0) were formed, and therefore semiconductor devices having fine and highly accurate transfer patterns could be manufactured.

[0158] (Examples 16 to 22) A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the material (alloy, composition ratio) and set film thickness of the phase shift film 15 in the above-mentioned Example 1 were changed to those shown in the following Table 7. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film 15 measured in the same manner as in Example 1 were as shown in Tables 8-1 and 8-2.

[0159] [Table 7]

[0160] [Table 8-1]

[0161] [Table 8-2]

[0162] In the above-mentioned Examples 16 to 22, the material of protective film 14 was appropriately selected from materials having etching resistance to the dry etching gas used when phase shift film 15 was patterned.

[0163] As the above results show, in Examples 16 to 22, the phase difference variation and reflectance variation of the reflective mask blank and the reflective mask were larger than those of Examples 1 to 10 at both reflectances of 6% and 12%, but were within the allowable range. Moreover, by changing the film thickness without changing the material and composition ratio of the phase shift film, a phase shift film that satisfied the desired phase difference characteristics (phase difference variation of 180 degrees ±5 degrees) and the desired reflectance characteristics (0.9R0≦R≦1.1R0) could be obtained at both reflectances of 6% and 12%, respectively.

[0164] The reflective masks of Examples 16 to 22 were reflective masks on which phase shift film patterns having the desired phase difference characteristics (phase difference variation of 180 degrees ±5 degrees) and the desired reflectance characteristics (0.9R0≦R≦1.1R0) were formed, making it possible to manufacture semiconductor devices having fine and highly accurate transfer patterns.

[0165] (Comparative Examples 1 to 3) As Comparative Example 1, a reflective mask blank was prepared in which the phase shift film had a reflectance of 6%. As Comparative Example 2, a reflective mask blank was prepared in which the phase shift film had a reflectance of 4%. As Comparative Example 3, a reflective mask blank was prepared in which the phase shift film had a reflectance of 12%.

[0166] A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the phase shift film was changed to the material (alloy, composition ratio) and set film thickness shown in Table 9 below. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film measured in the same manner as in Example 1 were as shown in Table 10.

[0167] [Table 9]

[0168] [Table 10]

[0169] As the above results show, in Comparative Examples 1 to 3, the reflectance variations of the reflective mask blanks and reflective masks were within the range of 0.9R0≦R≦1.1R0, but the phase difference variations exceeded the range of ±5 degrees.

[0170] The reflective masks of Comparative Examples 1 to 3 were reflective masks in which phase shift film patterns were formed that did not satisfy the desired phase difference characteristics (phase difference variation in the range of 180 degrees ±5 degrees) and the desired reflectance characteristics (reflectance variation of 0.9R0≦R≦1.1R0), and therefore it was not possible to manufacture a semiconductor device having a fine and high-precision transfer pattern.

[0171] Furthermore, this resist pattern is transferred to the film to be processed by etching, and various processes such as forming an insulating film or a conductive film, introducing a dopant, or annealing are performed, so it was not possible to manufacture a semiconductor device having the desired characteristics with a high yield.

[0172] (Reference examples 1 and 2) A reflective mask blank and a reflective mask were produced in the same manner as in Example 1, except that the material (alloy, composition ratio) and set film thickness of the phase shift film 15 in the above-mentioned Example 1 were changed to those shown in the following Table 11. The refractive index, extinction coefficient, phase difference variation, and reflectance variation of the phase shift film 15 measured in the same manner as in Example 1 were as shown in Tables 12-1 and 12-2.

[0173] [Table 11]

[0174] [Table 12-1]

[0175] [Table 12-2]

[0176] As shown by the above results, in Reference Example 1, the reflectance variation of the reflective mask blank and the reflective mask was within the range of 0.9R0≦R≦1.1R0, and the phase difference variation was within the range of ±5 degrees when the reflectance was 6%, but exceeded the range of ±5 degrees when the reflectance was 4% and 12%. In Reference Example 2, the reflectance variation was within the range of 0.9R0≦R≦1.1R0, and the phase difference variation was within the range of ±5 degrees when the reflectance was 4%, but exceeded the range of ±5 degrees when the reflectance was 6% and 12%. Therefore, by changing only the film thickness without changing the material and composition ratio of the phase shift film, it was not possible to obtain a phase shift film that satisfies the desired phase difference characteristic (phase difference variation of 180 degrees ±5 degrees) and the desired reflectance characteristic (0.9R0≦R≦1.1R0) in any of the cases of the reflectance of 4%, 6%, and 12%. [Explanation of symbols]

[0177] 10 Reflective mask blanks 11 Back conductive film 12 Substrate 13 Multilayer reflective film 14 Protective film 15 Phase shift film

Claims

1. A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film comprises an alloy containing two or more metals; When the metal element group is group A and group B, Group A metal elements are Pd, Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Fe and Hf; Group B metal elements are Rh, Ru, Mo, Nb, Ti, Zr, Y and Si; The alloy contains one or more metal elements from group A and one or more metal elements from group B, The phase shift film has a predetermined phase difference of θ with respect to a wavelength of 13.5 nm when the film thickness of the phase shift film varies by ±0.5% from the set film thickness. 0 When the phase difference θ is 0 -2 degrees≦θ≦θ 0 +2 degrees and a predetermined reflectance for a wavelength of 13.5 nm is R 0 When the reflectance R is R 0 −0.2%≦R≦R 0 The composition ratio is adjusted to be in the range of +0.2%, a reflective mask blank, wherein the phase difference and the reflectance are those of a phase difference and a reflectance of a surface of the phase shift film with respect to light reflected from the multilayer reflective film before the phase shift film is formed;

2. A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film comprises an alloy containing two or more metals; When the metal element group is group A and group B, Group A metal elements are Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, Fe and Hf; Group B metal elements are Pd, Rh, Ru, Mo, Nb, V, Ti, Zr, Y and Si; The alloy contains one or more metal elements from group A and one or more metal elements from group B, The phase shift film has a predetermined phase difference of θ with respect to a wavelength of 13.5 nm when the film thickness of the phase shift film varies by ±0.5% from the set film thickness. 0 When the phase difference θ is 0 -2 degrees≦θ≦θ 0 +2 degrees and a predetermined reflectance for a wavelength of 13.5 nm is R 0 When the reflectance R is R 0 −0.2%≦R≦R 0 The composition ratio is adjusted to be in the range of +0.2%, a reflective mask blank, wherein the phase difference and the reflectance are those of a phase difference and a reflectance of a surface of the phase shift film with respect to light reflected from the multilayer reflective film before the phase shift film is formed;

3. A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film comprises an alloy containing two or more metals; When the metal element group is group A and group B, Group A metal elements are Rh, Pd, Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ti, Fe and Hf; Group B metal elements are Ru, Mo, Nb, Zr, Y and Si; The alloy contains one or more metal elements from group A and one or more metal elements from group B, The phase shift film has a predetermined phase difference of θ with respect to a wavelength of 13.5 nm when the film thickness of the phase shift film varies by ±0.5% from the set film thickness. 0 When the phase difference θ is 0 -2 degrees≦θ≦θ 0 +2 degrees and a predetermined reflectance for a wavelength of 13.5 nm is R 0 When the reflectance R is R 0 −0.2%≦R≦R 0 The composition ratio is adjusted to be in the range of +0.2%, a reflective mask blank, wherein the phase difference and the reflectance are those of a phase difference and a reflectance of a surface of the phase shift film with respect to light reflected from the multilayer reflective film before the phase shift film is formed;

4. A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film comprises an alloy containing two or more metals; When the metal element group is group A and group B, Group A metal elements are Ag, Pt, Ir, W, Cr, Co, Mn, Sn, Ta, V, Fe and Hf; Group B metal elements are Au, Pd, Rh, Ru, Mo, Nb, Ti, Zr, Y and Si; The alloy contains one or more metal elements from group A and one or more metal elements from group B, The phase shift film has a predetermined phase difference of θ with respect to a wavelength of 13.5 nm when the film thickness of the phase shift film varies by ±0.5% from the set film thickness. 0 When the phase difference θ is 0 -5 degrees ≤ θ ≤ θ 0 +5 degrees and a predetermined reflectance for a wavelength of 13.5 nm is R 0 When the reflectance R is 0.9R 0 ≦R≦1.1R 0 and the refractive index and extinction coefficient are in the range a reflective mask blank, wherein the phase difference and the reflectance are those of a phase difference and a reflectance of a surface of the phase shift film with respect to light reflected from the multilayer reflective film before the phase shift film is formed;

5. A reflective mask blank comprising a multilayer reflective film formed on a substrate and a phase shift film formed on the multilayer reflective film, the phase shift film comprises an alloy containing two or more metals; When the metal element group is group A and group B, Group A metal elements are Ag, Pt, Au, Ir, W, Cr, Co, Mn, Sn, Ta, V, Ti, Fe, Hf and Si; Group B metal elements are Pd, Rh, Ru, Mo, Nb, Zr, and Y; The alloy contains one or more metal elements from group A and one or more metal elements from group B, The phase shift film has a predetermined phase difference of θ with respect to a wavelength of 13.5 nm when the film thickness of the phase shift film varies by ±0.5% from the set film thickness. 0 When the phase difference θ is 0 -5 degrees ≤ θ ≤ θ 0 +5 degrees and a predetermined reflectance for a wavelength of 13.5 nm is R 0 When the reflectance R is 0.9R 0 ≦R≦1.1R 0 and the refractive index and extinction coefficient are in the range a reflective mask blank, wherein the phase difference and the reflectance are those of a phase difference and a reflectance of a surface of the phase shift film with respect to light reflected from the multilayer reflective film before the phase shift film is formed;

6. The metal elements of group A are Pd, Ag, Pt, Au, Ir, W, Cr, Mn, Sn, Ta, V, Fe, and Hf; 2. The reflective mask blank according to claim 1, wherein the metal elements of group B are Rh, Ru, Mo, Nb, Zr and Y.

7. The metal elements of group A are Ag, Pt, Ir, W, Cr, Mn, Sn, Ta, Fe, and Hf; 6. The reflective mask blank according to claim 2, wherein the metal elements of group B are Rh, Ru, Mo, Nb, Zr and Y.

8. The metal elements of group A are Rh, Pd, Ag, Pt, Au, Ir, W, Cr, Mn, Sn, Ta, V, Fe, and Hf; 4. The reflective mask blank according to claim 3, wherein the metal elements of group B are Ru, Mo, Nb, Zr and Y.

9. 9. The reflective mask blank according to claim 1, wherein the phase shift film contains an alloy containing three or more metals.

10. The reflective mask blank according to claim 1 , wherein the phase shift film further contains at least one element selected from the group consisting of oxygen, nitrogen, carbon, and boron.

11. 11. The reflective mask blank according to claim 1, wherein the phase shift film has a reflectance at a wavelength of 13.5 nm of more than 3% and not more than 20%.

12. 12. The reflective mask blank according to claim 1, wherein the phase shift film has a thickness of 25 nm or more and 70 nm or less.

13. 13. The reflective mask blank according to claim 1, wherein the uppermost layer of the multilayer reflective film on the phase shift film side is provided with a protective film.

14. A reflective mask having a phase shift film pattern formed by patterning the phase shift film in the reflective mask blank according to claim 1 .

15. 15. A method for manufacturing a semiconductor device, comprising the step of forming a pattern on a semiconductor substrate by using the reflective mask according to claim 14.

Citation Information

Patent Citations

  • Particle board for backing

    JP1977033321A

  • Manufacturing of symmetric type voltage nonnlinear resistor

    JP1977066988A

  • High tension cold rolled thin steel plate having excellent deep drawing property

    JP1982016146A

  • Mask for extreme ultraviolet ray exposure, mask blank, and exposure method

    JP2006228766A

  • Reflective mask blank, method of manufacturing reflective mask blank, and method of manufacturing reflective mask

    JP2015142083A