Chromium alloy container and metal-supported electrochemical cell
The use of a chromium oxide adhesive layer with a metal connecting portion in chromium alloy containers addresses the issue of chromium diffusion, ensuring long-term bondability and durability by preventing composition changes in the glass seal.
Patent Information
- Application Number
- JP2024546467
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-10-05
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-10-05
AI Technical Summary
Chromium alloy containers face issues with chromium diffusion into glass seals, leading to reduced strength and bonding failure over time, affecting the longevity of the alloy members.
Incorporation of an oxide adhesive layer made of chromium-containing oxides, such as chromium oxide or chromium manganese oxide, with a metal connecting portion embedded within, to prevent chromium diffusion and enhance bonding between alloy members.
Maintains bondability between alloy members for a prolonged period by suppressing chromium diffusion and enhancing the strength and durability of the chromium alloy container.
Smart Images

Figure 0007588280000004 
Figure 0007588280000005 
Figure 0007588280000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a chromium alloy container and a metal-supported electrochemical cell. [Background technology]
[0002] Patent Document 1 discloses a chromium alloy container for housing a fuel cell. The chromium alloy container includes a first interconnector, a second interconnector, a separator, an anode frame, and a glass seal.
[0003] The first interconnector is connected to the air electrode of the fuel cell. The second interconnector is connected to the anode current collecting layer of the fuel cell. The separator is connected to the solid electrolyte of the fuel cell and separates the fuel gas and oxidant gas flow paths. The anode frame is disposed between the separator and the second interconnector. A glass seal bonds the first interconnector and the separator.
[0004] The first interconnector, the second interconnector, the separator and the fuel electrode frame are each made of a chromium alloy (for example, SUS430, SUS444, etc.) The glass seal is made of a glass material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2015-156352 Summary of the Invention [Problem to be solved by the invention]
[0006] In the chromium alloy container described in Patent Document 1, the chromium contained in the first interconnector and the separator diffuses into the glass seal, causing the composition of the glass seal to change and the strength of the glass seal to decrease. As a result, the glass seal is deformed or cracked, making it impossible to maintain the bonding between the alloy members for a long period of time. This is a problem that is common not only to containers that house fuel cells, but also to chromium alloy containers in general.
[0007] An object of the present invention is to provide a chromium alloy container and a metal-supported electrochemical cell capable of maintaining the bond between alloy members for a long period of time. [Means for solving the problem]
[0008] A chromium alloy container according to a first aspect of the present invention has an internal space. The chromium alloy container includes a first alloy member made of an alloy containing chromium, a second alloy member made of an alloy containing chromium, and an insert part interposed between the first alloy member and the second alloy member. The insert part includes an oxide bonding layer made of an oxide mainly composed of chromium, and a metal connecting part embedded in the oxide bonding layer to connect the first alloy member and the second alloy member.
[0009] A chromium alloy container according to a second aspect of the present invention is related to the first aspect, wherein the metal connection portion contains, as a main component, the same element as a main component of at least one of the first alloy member and the second alloy member.
[0010] A chromium alloy container according to a third aspect of the present invention is the chromium alloy container according to the first or second aspect, wherein the metal connecting portion contains chromium.
[0011] A chromium alloy container according to a fourth aspect of the present invention is related to any one of the first to third aspects, wherein the ratio of the minimum width of the metal connection portion in the surface direction to the thickness of the oxide adhesion layer in the thickness direction is 0.3 or more.
[0012] A chromium alloy container according to a fifth aspect of the present invention is related to any one of the first to fourth aspects, wherein the ratio of the longest distance between the metal connections in the surface direction to the thickness of the oxide adhesion layer in the thickness direction is 20 or less.
[0013] A chromium alloy container according to a sixth aspect of the present invention is related to any one of the first to fifth aspects, wherein a ratio of a thickness of the first alloy member or the second alloy member in a thickness direction to a minimum width of the metal connection portion in a surface direction is 50 or more.
[0014] A chromium alloy container according to a seventh aspect of the present invention is related to any one of the first to sixth aspects, wherein a ratio of a thickness of the first alloy member or the second alloy member in a thickness direction to a minimum width of the metal connection portion in a surface direction is 2000 or less.
[0015] The chromium alloy container according to an eighth aspect of the present invention is related to any one of the first to seventh aspects, wherein the chromium content in the metal elements in the oxide adhesion layer is 50 mol % or more.
[0016] A chromium alloy container according to a ninth aspect of the present invention is related to any one of the first to eighth aspects, wherein the oxide adhesion layer is made of at least one of chromium oxide and chromium manganese oxide.
[0017] A chromium alloy container according to a tenth aspect of the present invention is related to any one of the first to ninth aspects, in which the oxide adhesion layer is crystalline.
[0018] A chromium alloy container according to an eleventh aspect of the present invention is related to the tenth aspect, wherein the oxide adhesion layer has a spinel type or corundum type crystal structure.
[0019] A chromium alloy container according to a twelfth aspect of the present invention is related to any one of the first to eleventh aspects, wherein the insertion portion is a seal for sealing the internal space.
[0020] A chromium alloy container according to a thirteenth aspect of the present invention is the chromium alloy container according to any one of the first to twelfth aspects, wherein the second alloy member has an embossed portion in contact with the first alloy member, and the insertion portion bonds the embossed portion to the first alloy member.
[0021] A metal-supported electrochemical cell according to a fourteenth aspect of the present invention comprises a chromium alloy container according to any one of the first to thirteenth aspects, and a cell body arranged on the chromium alloy container. The first alloy member has a plurality of communication holes that communicate with the internal space. The cell body is arranged on the first alloy member so as to cover the plurality of communication holes. Effect of the Invention
[0022] According to the present invention, it is possible to provide a chromium alloy container and a metal-supported electrochemical cell capable of maintaining the bond between alloy members for a long period of time. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a plan view of the electrolysis cell according to the first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view taken along line AA of FIG. [Diagram 3] FIG. 3 is a partially enlarged view of FIG. [Figure 4] FIG. 4 is a cross-sectional view of an electrolysis cell according to a second embodiment. [Diagram 5] FIG. 5 is a partially enlarged view of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] 1. First embodiment
[0025] (Electrolysis cell 1) Fig. 1 is a plan view of an electrolysis cell 1 according to a first embodiment, and Fig. 2 is a cross-sectional view taken along line AA in Fig. 1.
[0026] The electrolysis cell 1 is an example of a "metal-supported electrochemical cell" according to the present invention.
[0027] The electrolysis cell 1 is formed in a plate shape extending in the X-axis and Y-axis directions. In this embodiment, the electrolysis cell 1 is formed in a rectangular shape extending in the Y-axis direction when viewed in a plan view from the Z-axis direction perpendicular to the X-axis and Y-axis directions. However, the planar shape of the electrolysis cell 1 is not particularly limited, and may be a polygon other than a rectangle, an ellipse, a circle, or the like.
[0028] As shown in FIGS. 1 and 2, the electrolysis cell 1 includes a cell body 2 and a chromium alloy container 3 .
[0029] (Cell body 2) The cell body 2 is placed on a chromium alloy container 3. The cell body 2 is supported by a metal support 10 (described later) in the chromium alloy container 3. The cell body 2 has a hydrogen electrode 6 (cathode), an electrolyte 7, a reaction prevention layer 8, and an oxygen electrode 9 (anode).
[0030] The hydrogen electrode 6, electrolyte 7, reaction prevention layer 8, and oxygen electrode 9 are laminated in this order in the Z-axis direction from the chromium alloy container 3 side. The hydrogen electrode 6, electrolyte 7, and oxygen electrode 9 are essential components, while the reaction prevention layer 8 is optional.
[0031] [Hydrogen pole 6] The hydrogen electrode 6 is disposed on a first main surface 12 of the metal support 10 .
[0032] A source gas is supplied to the hydrogen electrode 6 through each supply hole 11 of the metal support 10. The source gas contains at least water vapor (H2O).
[0033] When the raw material gas contains only H2O, the hydrogen electrode 6 produces H2 from the raw material gas in accordance with the electrochemical reaction of water electrolysis shown in the following formula (1).
[0034] Hydrogen electrode 6: H2O+2e - →H2+O 2- (1)
[0035] When the raw gas contains CO in addition to H2O, the hydrogen electrode 6 converts the raw gas into H2, CO, and O2 in accordance with the electrochemical reactions of co-electrolysis shown in the following formulas (2), (3), and (4). 2- Generate.
[0036] Hydrogen electrode 6: CO2+H2O+4e - →CO+H2+2O 2- (2) Electrochemical reaction of H2O: H2O+2e - →H2+O 2- (3) Electrochemical reaction of CO2: CO2+2e - →CO+O 2- (4)
[0037] H2 generated in the hydrogen electrode 6 flows out from each supply hole 11 of the metal support 10 into an internal space 3a, which will be described later.
[0038] The hydrogen electrode 6 is a porous body having electronic conductivity. The hydrogen electrode 6 contains nickel (Ni). In the case of co-electrolysis, Ni functions as an electronic conductor and also functions as a thermal catalyst that promotes the thermal reaction between the generated H2 and the CO2 contained in the raw gas to maintain an appropriate gas composition for methanation, Fischer-Tropsch (FT) synthesis, etc. The Ni contained in the hydrogen electrode 6 is basically present in the form of metal Ni during operation of the electrolysis cell 1, but may also be partially present in the form of nickel oxide (NiO).
[0039] The hydrogen electrode 6 may contain an ion-conductive material, such as yttria-stabilized zirconia (YSZ), calcia-stabilized zirconia (CSZ), scandia-stabilized zirconia (ScSZ), gadolinium-doped ceria (GDC), samarium-doped ceria (SDC), (La,Sr)(Cr,Mn)O3, (La,Sr)TiO3, Sr2(Fe,Mo)2O6, (La,Sr)VO3, (La,Sr)FeO3, and a mixed material of two or more of these.
[0040] The thickness of the hydrogen electrode 6 is not particularly limited, but may be, for example, 1 μm or more and 100 μm or less. The thermal expansion coefficient of the hydrogen electrode 6 is not particularly limited, but may be, for example, 12×10 ―6 / ℃ or more 20×10 -6 / °C or less.
[0041] The method for forming the hydrogen electrode 6 is not particularly limited, and may be a firing method, a spray coating method (such as a thermal spray method, an aerosol deposition method, an aerosol gas deposition method, a powder jet deposition method, a particle jet deposition method, or a cold spray method), a PVD method (such as a sputtering method or a pulsed laser deposition method), or a CVD method.
[0042] [Electrolyte 7] The electrolyte 7 is formed on the hydrogen electrode 6. The electrolyte 7 is disposed between the hydrogen electrode 6 and the oxygen electrode 9. In this embodiment, the electrolyte 7 is sandwiched between the hydrogen electrode 6 and the reaction prevention layer 8 and connected to both of them.
[0043] The electrolyte 7 covers the hydrogen electrode 6 and also covers the area of the first main surface 12 of the metal support 10 that is exposed from the hydrogen electrode 6 .
[0044] The electrolyte 7 is a dense body having oxide ion conductivity. 2- is transferred to the oxygen electrode 9. The electrolyte 7 is made of an oxide ion conductive material. The electrolyte 7 can be made of, for example, YSZ, GDC, ScSZ, SDC, LSGM (lanthanum gallate), etc., with YSZ being particularly suitable.
[0045] The thickness of the electrolyte 7 is not particularly limited, but may be, for example, 1 μm or more and 100 μm or less. The thermal expansion coefficient of the electrolyte 7 is not particularly limited, but may be, for example, 10×10 ―6 / ℃ or more 12×10 ―6 / °C or less.
[0046] The method for forming the electrolyte 7 is not particularly limited, and a baking method, a spray coating method, a PVD method, a CVD method, or the like can be used.
[0047] [Reaction prevention layer 8] The reaction prevention layer 8 is disposed between the electrolyte 7 and the oxygen electrode 9. The reaction prevention layer 8 is disposed on the opposite side of the electrolyte 7 to the hydrogen electrode 6. The reaction prevention layer 8 prevents a layer with high electrical resistance from being formed due to a reaction between a constituent element of the electrolyte 7 and a constituent element of the oxygen electrode 9.
[0048] The reaction prevention layer 8 is made of an oxide ion conductive material, and may be made of GDC, SDC, or the like.
[0049] The porosity of the reaction prevention layer 8 is not particularly limited, but may be, for example, 0.1% to 50%. The thickness of the reaction prevention layer 8 is not particularly limited, but may be, for example, 1 μm to 50 μm.
[0050] The method for forming the reaction prevention layer 8 is not particularly limited, and a baking method, a spray coating method, a PVD method, a CVD method, or the like can be used.
[0051] [Oxygen pole 9] The oxygen electrode 9 is disposed on the opposite side of the hydrogen electrode 6 with respect to the electrolyte 7. In this embodiment, since the reaction prevention layer 8 is disposed between the electrolyte 7 and the oxygen electrode 9, the oxygen electrode 9 is connected to the reaction prevention layer 8. If the reaction prevention layer 8 is not disposed between the electrolyte 7 and the oxygen electrode 9, the oxygen electrode 9 is connected to the electrolyte 7.
[0052] The oxygen electrode 9 receives O transferred from the hydrogen electrode 6 through the electrolyte 7 according to the chemical reaction of the following formula (5): 2- produces O2 from
[0053] Oxygen electrode 9:2O 2- →O2+4e - (5)
[0054] The oxygen electrode 9 is a porous body having oxide ion conductivity and electron conductivity, and can be made of a composite material of one or more of (La,Sr)(Co,Fe)O3, (La,Sr)FeO3, La(Ni,Fe)O3, (La,Sr)CoO3, and (Sm,Sr)CoO3 and an oxide ion conductive material (such as GDC).
[0055] The porosity of the oxygen electrode 9 is not particularly limited, but may be, for example, 20% to 60%. The thickness of the oxygen electrode 9 is not particularly limited, but may be, for example, 1 μm to 100 μm.
[0056] The method for forming the oxygen electrode 9 is not particularly limited, and a baking method, a spray coating method, a PVD method, a CVD method, or the like can be used.
[0057] (Chrome alloy container 3) The chromium alloy container 3 has an internal space 3a through which the source gas supplied to the hydrogen electrode 6 and the reducing gas (H2 in this embodiment) generated in the hydrogen electrode 6 flow.
[0058] In this embodiment, the chromium alloy container 3 includes a metal support 10, a frame 20, an interconnector 30, a first seal portion 40, and a second seal portion 50. The internal space 3a is a space surrounded by the metal support 10, the frame 20, the interconnector 30, the first seal portion 40, and the second seal portion 50.
[0059] In this embodiment, one of the metal support 10 and the frame 20 is an example of a "first alloy member" according to the present invention, and the other is an example of a "second alloy member" according to the present invention. Also, in this embodiment, one of the frame 20 and the interconnector 30 is an example of a "first alloy member" according to the present invention, and the other is an example of a "second alloy member" according to the present invention. Each of the first seal portion 40 and the second seal portion 50 is an example of an "insertion portion" according to the present invention.
[0060] [Metal support 10] The metal support 10 supports the cell body 2. In this embodiment, the metal support 10 is formed in a plate shape. The metal support 10 may be in the shape of a flat plate or a curved plate.
[0061] The metal support 10 is only required to be able to support the cell body 2, and its thickness is not particularly limited, but can be, for example, 0.1 mm or more and 2.0 mm or less.
[0062] As shown in FIG. 2, the metal support 10 has a plurality of supply holes 11, a first main surface 12 and a second main surface 13.
[0063] Each supply hole 11 penetrates the metal support 10 from the first main surface 12 to the second main surface 13. Each supply hole 11 opens to each of the first main surface 12 and the second main surface 13. Each supply hole 11 is covered by the cell body 2. Specifically, the opening of each supply hole 11 on the first main surface 12 side is covered by the hydrogen electrode 6. The opening of each supply hole 11 on the second main surface 13 side is connected to the internal space 3a.
[0064] Each supply hole 11 can be formed by mechanical processing (for example, punching), laser processing, chemical processing (for example, etching), or the like.
[0065] In this embodiment, each supply hole 11 is formed linearly along the Z-axis direction. However, each supply hole 11 may be inclined with respect to the Z-axis direction, and may not be linear. Furthermore, each supply hole 11 may be connected to another supply hole 11.
[0066] The first main surface 12 is provided on the opposite side to the second main surface 13. The cell body 2 is disposed on the first main surface 12. The frame 20 is joined to the second main surface 13 via a first seal portion 40.
[0067] The metal support 10 is made of an alloy containing Cr (chromium). Examples of such alloys include Fe-Cr alloy steel (stainless steel, etc.) and Ni-Cr alloy steel. The Cr content in the metal support 10 is not particularly limited, but may be 4% by mass or more and 30% by mass or less.
[0068] The metal support 10 may contain Ti (titanium) and / or Zr (zirconium). The Ti content in the metal support 10 is not particularly limited, but may be 0.01 mol% or more and 1.0 mol% or less. The Zr content in the metal support 10 is not particularly limited, but may be 0.01 mol% or more and 0.4 mol% or less. The metal support 10 may contain Ti as TiO2 (titania) or Zr as ZrO2 (zirconia).
[0069] [Frame 20] The frame 20 is a spacer for forming the internal space 3a. In this embodiment, the frame 20 is formed in an annular shape.
[0070] The frame 20 is joined to the metal support 10 via the first seal portion 40 , and is joined to the interconnector 30 via the second seal portion 50 .
[0071] The thickness of the frame 20 is not particularly limited, but may be, for example, 0.1 mm or more and 2.0 mm or less.
[0072] The frame 20 is made of an alloy containing Cr. Examples of such alloys include Fe-Cr alloy steel and Ni-Cr alloy steel. The Cr content in the frame 20 is not particularly limited, but may be 4% by mass or more and 30% by mass or less. The composition of the frame 20 may be the same as or different from that of the metal support 10.
[0073] [Interconnector 30] The interconnector 30 is disposed on the opposite side of the metal support 10 with respect to the frame 20. The interconnector 30 is a member for electrically connecting the electrolytic cell 1 to an external power source or another electrolytic cell.
[0074] In this embodiment, the interconnector 30 is formed in a plate shape. The interconnector 30 may be in the shape of a flat plate or a curved plate.
[0075] The interconnector 30 is joined to the frame 20 via the second seal portion 50 .
[0076] The thickness of the interconnector 30 is not particularly limited, but can be, for example, not less than 0.1 mm and not more than 2.0 mm.
[0077] The interconnector 30 is made of an alloy containing Cr. Examples of such alloys include Fe-Cr alloy steel and Ni-Cr alloy steel. The Cr content in the interconnector 30 is not particularly limited, but can be 4 mass% or more and 30 mass% or less. The composition of the interconnector 30 may be the same as or different from that of the metal support 10. The composition of the interconnector 30 may be the same as or different from that of the frame 20.
[0078] [First seal portion 40] The first seal portion 40 is disposed between the metal support body 10 and the frame body 20. The first seal portion 40 is joined to both the metal support body 10 and the frame body 20.
[0079] The first seal portion 40 is formed in an annular shape. The first seal portion 40 seals the gap between the metal support 10 and the frame 20. This prevents the source gas supplied to the hydrogen electrode 6 and the reducing gas generated in the hydrogen electrode 6 from leaking to the outside through the gap between the metal support 10 and the frame 20. A detailed configuration of the first seal portion 40 will be described later.
[0080] [Second seal portion 50] The second seal portion 50 is disposed between the frame body 20 and the interconnector 30. The second seal portion 50 is joined to each of the frame body 20 and the interconnector 30.
[0081] The second seal portion 50 is formed in an annular shape. The second seal portion 50 seals the gap between the frame 20 and the interconnector 30. This prevents the source gas supplied to the hydrogen electrode 6 and the reducing gas generated in the hydrogen electrode 6 from leaking to the outside through the gap between the frame 20 and the interconnector 30.
[0082] The configuration of the second seal portion 50 is the same as the configuration of the first seal portion 40, which will be described next, and therefore, in this embodiment, a description of the configuration of the second seal portion 50 will be omitted.
[0083] (Detailed configuration of the first seal portion 40) Fig. 3 is a partially enlarged view of Fig. 2. Fig. 3 shows a cross section of the first seal portion 40. The cross section shown in Fig. 3 is perpendicular to the first main surface 12 of the metal support 10.
[0084] The first seal portion 40 includes an oxide adhesion layer 41 and a metal connector 42 .
[0085] [Oxide adhesive layer 41] The oxide adhesive layer 41 is disposed between the metal support 10 and the frame 20. The oxide adhesive layer 41 is sandwiched between the metal support 10 and the frame 20. The oxide adhesive layer 41 is formed in a ring shape so as to surround the internal space 3a. The oxide adhesive layer 41 is exposed to the internal space 3a.
[0086] The oxide adhesive layer 41 is made of an oxide containing Cr as a main component (hereinafter, abbreviated as "Cr oxide"). This can suppress the diffusion of Cr from the metal support 10 and the frame 20 to the oxide adhesive layer 41 during the manufacture or operation of the electrolysis cell 1. Even if Cr diffuses from the metal support 10 and the frame 20 to the oxide adhesive layer 41, the effect on the composition of the oxide adhesive layer 41 is small, so that the strength of the oxide adhesive layer 41 can be suppressed from decreasing. Furthermore, since the metal support 10, the frame 20, and the oxide adhesive layer 41 all contain Cr, the mutual bonding can be improved. Therefore, the bonding between the metal support 10 and the frame 20 can be maintained for a long period of time.
[0087] In this embodiment, the term "mainly composed of Cr" means that the Cr content is the highest among the metal elements in the Cr oxide when the composition of the Cr oxide constituting the oxide adhesion layer 41 is analyzed by an energy dispersive spectroscopy (EDS) device. The Cr content is not particularly limited, but can be, for example, 20 mol% or more and 100 mol% or less.
[0088] The Cr content in the metal elements in the Cr oxide constituting the oxide adhesion layer 41 is preferably 50 mol % or more. This makes it possible to significantly suppress the diffusion of Cr contained in the metal support 10 and the frame 20 into the oxide adhesion layer 41.
[0089] The Cr oxide constituting the oxide adhesion layer 41 is preferably composed of at least one of chromium oxide and chromium manganese oxide. These oxides have the property that Cr is particularly difficult to diffuse, and therefore the durability of the oxide adhesion layer 41 can be improved.
[0090] Chromium oxides include Cr2O3, etc. Chromium manganese oxides include MnCr2O4 (spinel), Mn 1,5 Cr 1,5 O4 (spinel) and others.
[0091] The Cr oxide constituting the oxide adhesion layer 41 is preferably crystalline. This makes it possible to prevent the oxide adhesion layer 41 from being damaged due to a phase transition of the Cr oxide from amorphous to crystalline even when the electrolysis cell 1 is operated for a long period of time.
[0092] The Cr oxide constituting the oxide adhesive layer 41 preferably has a spinel or corundum crystal structure. These crystal structures are highly symmetrical, and therefore can improve the thermal stress resistance of the oxide adhesive layer 41. In addition, Cr oxides having these crystal structures have good bonding properties at the interfaces with the metal support 10 and the frame 20, both of which are made of an alloy containing Cr, and therefore can improve the bonding strength between the oxide adhesive layer 41 and the metal support 10 and the frame 20, respectively.
[0093] [Metal connection part 42] The metal connecting portion 42 is embedded in the oxide adhesive layer 41. The metal connecting portion 42 extends along a thickness direction perpendicular to the first main surface 12 of the metal support 10. The metal connecting portion 42 penetrates the oxide adhesive layer 41 in the thickness direction. When viewed three-dimensionally, the metal connecting portion 42 is columnar. The outer peripheral surface of the metal connecting portion 42 is surrounded by the oxide adhesive layer 41.
[0094] The metal connecting portion 42 connects the metal support 10 and the frame body 20. One end of the metal connecting portion 42 is connected to the metal support 10, and the other end of the metal connecting portion 42 is connected to the frame body 20. The metal connecting portion 42 may be substantially integral with at least one of the metal support 10 and the frame body 20.
[0095] By embedding the metal connecting parts 42 in the oxide adhesive layer 41, cracks occurring in the oxide adhesive layer 41 can be stopped at the metal connecting parts 42. Therefore, brittle fracture of the oxide adhesive layer 41 can be suppressed, and the bond between the metal support 10 and the frame 20 can be maintained for a longer period of time.
[0096] Although three metal connecting portions 42 are illustrated in FIG. 3, the number of metal connecting portions 42 in one cross section is not particularly limited as long as it is one or more.
[0097] 3, a metal connecting part 42 with a barrel-shaped cross section, a metal connecting part 42 with an inclined cross section, and a metal connecting part 42 with a constricted cross section are shown in that order from the left. When the cross section of the metal connecting part 42 is constricted, the interface area between the metal supporting body 10 and the metal connecting part 42 and between the metal connecting part 42 and the frame body 20 can be increased, thereby improving the interface strength between the two. When the cross section of the metal connecting part 42 is barrel-shaped or inclined, the volume of the metal connecting part 42 itself can be increased, thereby further improving the crack stopping effect.
[0098] Thus, although the cross-sectional shapes of the metal connecting parts 42 are different from one another in Fig. 3, the cross-sectional shapes of the metal connecting parts 42 may be the same. The cross-sectional shape of the metal connecting parts 42 may be a shape other than the shape shown in Fig. 3. It is preferable to set the cross-sectional shape of each metal connecting part 42 in consideration of the balance between the improvement of the interfacial strength by increasing the interfacial area between the metal supporting body 10 and the metal connecting part 42 and the frame body 20, respectively, and the improvement of the crack stopping effect by increasing the volume of the metal connecting part 42.
[0099] The metal connecting portion 42 is made of a metal. It is preferable that the metal connecting portion 42 contains as its main component the same element as the main component of at least one of the metal support 10 and the frame body 20. This makes it possible to suppress a change in the composition of the metal connecting portion 42 due to element diffusion from the metal support 10 and the frame body 20. For example, the metal connecting portion 42 can contain Cr or Fe as its main component. Incidentally, containing as the main component means that the metal connecting portion 42 shows the maximum content when subjected to elemental analysis.
[0100] Moreover, it is preferable that the metal connecting portion 42 contains Cr, which can improve the oxidation resistance of the metal connecting portion 42.
[0101] The ratio of the minimum width W1 of the metal connecting portion 42 in the planar direction to the thickness of the oxide adhesive layer 41 in the thickness direction is preferably 0.3 or more. This ensures the strength of the metal connecting portion 42, thereby preventing the metal connecting portion 42 from being damaged by cracks. The planar direction is the direction perpendicular to the thickness direction.
[0102] The thickness of the adhesive layer 41 is the arithmetic average of the thicknesses of the oxide adhesive layer 41 at three locations that divide the oxide adhesive layer 41 into four equal parts in the surface direction. However, when the location for measuring the thickness overlaps with the metal connecting portion 42, the thickness of the oxide adhesive layer 41 may be measured at any location close to the metal connecting portion 42. The thickness of the adhesive layer 41 is not particularly limited, but may be, for example, 0.3 μm or more and 30 μm or less.
[0103] Furthermore, the minimum width W1 of the metal connecting portion 42 is the minimum measurement value when the width of the metal connecting portion 42 in the surface direction is measured at 10 locations that divide the metal connecting portion 42 into 11 equal parts in the thickness direction. The value of the minimum width W1 of the metal connecting portion 42 is not particularly limited, but can be, for example, 0.05 μm or more and 5 μm or less.
[0104] When multiple metal connecting parts 42 are present, the ratio of the longest distance D1 between the metal connecting parts 42 in the surface direction to the thickness of the oxide bonding layer 41 in the thickness direction is preferably 20 or less. This allows the multiple metal connecting parts 42 to be arranged in a narrow range in the surface direction, thereby preventing long cracks from occurring in the oxide bonding layer 41. As a result, peeling of the oxide bonding layer 41 from the metal support 10 and the frame 20 due to long cracks can be prevented.
[0105] The maximum distance D1 between the metal connecting parts 42 is the maximum distance between two straight lines that are parallel to the thickness direction and inscribed in the outlines of the side surfaces of the two opposing metal connecting parts 42. The value of the maximum distance D1 is not particularly limited, but can be, for example, 1 μm or more and 100 μm or less.
[0106] The ratio of the thickness of the metal support 10 or the frame body 20 in the thickness direction to the minimum width W1 of the metal connecting portion 42 in the surface direction is preferably equal to or less than 2000. This makes it possible to prevent the metal support 10 or the frame body 20 from becoming excessively thick (i.e., the metal connecting portion 42 from becoming excessively thin), thereby ensuring the strength of the metal connecting portion 42.
[0107] The ratio of the thickness of the metal support 10 or the frame body 20 in the thickness direction to the minimum width W1 of the metal connecting portion 42 in the surface direction is preferably equal to or greater than 50. This makes it possible to prevent the metal support 10 or the frame body 20 from becoming excessively thin (i.e., the metal connecting portion 42 from becoming excessively thick), thereby increasing the rigidity of the first seal portion 40.
[0108] It is preferable that the metal connecting portion 42 is away from the internal space 3a. Specifically, it is preferable that the metal connecting portion 42 is present in at least one of the central portion in the surface direction and the peripheral portion in the surface direction. This makes it possible to suppress embrittlement of the metal connecting portion 42 due to the reducing gas (H2 in this embodiment) flowing through the internal space 3a. The central portion in the surface direction is a portion located in the center when the oxide adhesive layer 41 is divided into thirds in the surface direction. The peripheral portion in the surface direction is a portion located on the external space 3b side of the central portion in the surface direction when the oxide adhesive layer 41 is divided into thirds in the surface direction.
[0109] The first seal portion 40 can be formed as follows. First, a paste containing Cr oxide and metal particles is applied onto at least one surface of the metal support 10 and the frame 20. At this time, the amount of the paste applied is adjusted so that the thickness of the applied paste is approximately the same as the average particle size of the metal particles. Next, the paste is fired to form the first seal portion 40. The metal particles are connected to the metal support 10 and the frame 20 by element diffusion between the metal support 10 and the frame 20. The firing conditions can be set appropriately, and can be, for example, 600°C to 1100°C and 0.5 hours to 24 hours.
[0110] 2. Second embodiment
[0111] (Electrolysis cell 1) 4 is a cross-sectional view of an electrolysis cell 1a according to the second embodiment. The electrolysis cell 1a is an example of the "metal-supported electrochemical cell" according to the present invention.
[0112] The electrolytic cell 1a according to the second embodiment differs from the electrolytic cell 1 according to the first embodiment in that the interconnector 30 has an embossed portion 31 and a debossed portion 32, and that the chromium alloy container 3 has a joint portion 60. The following mainly describes these differences.
[0113] In this embodiment, one of the metal support 10 and the interconnector 30 is an example of a "first alloy member" according to the present invention, and the other is an example of a "second alloy member" according to the present invention. Also, the joint portion 60 is an example of an "insertion portion" according to the present invention.
[0114] As shown in Fig. 4, the interconnector 30 has a plurality of embossed portions 31 and a plurality of debossed portions 32. Although two embossed portions 31 and three debossed portions 32 are illustrated in Fig. 4, the numbers of the embossed portions 31 and the debossed portions 32 can be changed as appropriate.
[0115] The embossed portion 31 abuts against the second main surface 13 of the metal support 10. As a result, the metal support 10 is supported by the interconnector 30, and thus bending of the metal support 10 is suppressed. Note that the embossed portion 31 only needs to abut against the metal support 10, and does not need to be fixed to the metal support 10.
[0116] The debossed portion 32 protrudes toward the side opposite to the metal support 10. The debossed portion 32 abuts against an external power source or another electrolytic cell.
[0117] The joint 60 joins the embossed portion 31 to the metal support 10. The joint 60 is disposed around the tip portion of the embossed portion 31. The tip portion of the embossed portion 31 refers to the portion of the embossed portion 31 that abuts against the metal support 10. The joint 60 is preferably formed in a ring shape so as to surround the tip portion of the embossed portion 31. This can improve the bonding between the embossed portion 31 and the metal support 10.
[0118] Here, Fig. 5 is a partially enlarged view of Fig. 4. In Fig. 5, a cross section of a joint 60 is illustrated. The cross section illustrated in Fig. 5 is perpendicular to the second main surface 13 of the metal support 10.
[0119] The joint 60 is disposed between the metal support 10 and the embossed portion 31. The joint 60 is sandwiched between the metal support 10 and the embossed portion 31. The joint 60 is disposed on the metal support 10, and is formed in an annular shape so as to surround the tip portion of the embossed portion 31.
[0120] In this embodiment, the joint 60 is embedded in a bottomed recess 80 formed between the metal support 10 and the embossed portion 31. The cross section of the bottomed recess 80 is wedge-shaped. The joint 60 is exposed to the internal space 3a.
[0121] The joint 60 comprises an oxide adhesion layer 43 and a metal interconnect 44 .
[0122] [Oxide adhesive layer 43] The oxide adhesive layer 43 is disposed between the metal support 10 and the embossed portion 31. The oxide adhesive layer 43 is sandwiched between the metal support 10 and the embossed portion 31. The oxide adhesive layer 43 is formed in a ring shape so as to surround the tip portion of the embossed portion 31. The oxide adhesive layer 43 is exposed to the internal space 3a.
[0123] The oxide adhesive layer 43 is made of Cr oxide. This can suppress the diffusion of Cr from the metal support 10 and the embossed portion 31 to the oxide adhesive layer 43 during the manufacture or operation of the electrolysis cell 1. Even if Cr diffuses from the metal support 10 and the embossed portion 31 to the oxide adhesive layer 43, the effect on the composition of the oxide adhesive layer 43 is small, so that the strength of the oxide adhesive layer 43 can be suppressed from decreasing. Furthermore, since the metal support 10, the embossed portion 31, and the oxide adhesive layer 43 all contain Cr, the mutual bonding can be improved. Therefore, the bonding between the metal support 10 and the embossed portion 31 can be maintained for a long period of time.
[0124] The Cr content in the metal elements in the Cr oxide constituting the oxide adhesion layer 43 is preferably 50 mol % or more. This makes it possible to significantly suppress the diffusion of Cr contained in the metal support 10 and the embossed portion 31 into the oxide adhesion layer 43.
[0125] The Cr oxide constituting the oxide adhesion layer 43 is preferably composed of at least one of chromium oxide and chromium manganese oxide. These oxides have the property that Cr is particularly difficult to diffuse, and therefore the durability of the oxide adhesion layer 43 can be improved.
[0126] The Cr oxide constituting the oxide adhesion layer 43 is preferably crystalline. This makes it possible to prevent the oxide adhesion layer 43 from being damaged due to a phase transition of the Cr oxide from amorphous to crystalline even when the electrolysis cell 1 is operated for a long period of time.
[0127] The Cr oxide constituting the oxide adhesive layer 43 preferably has a spinel or corundum crystal structure. These crystal structures are highly symmetrical, and therefore can improve the thermal stress resistance of the oxide adhesive layer 43. In addition, Cr oxides having these crystal structures have good bonding properties at the interfaces with the metal support 10 and the embossed portion 31, both of which are made of an alloy containing Cr, and therefore can improve the bonding strength between the oxide adhesive layer 43 and the metal support 10 and the embossed portion 31.
[0128] [Metal connection part 44] The metal connecting portion 44 is embedded in the oxide adhesive layer 43. The metal connecting portion 44 extends along a thickness direction perpendicular to the first main surface 12 of the metal support 10. The metal connecting portion 44 penetrates the oxide adhesive layer 43 in the thickness direction. When viewed three-dimensionally, the metal connecting portion 44 is columnar. The side surfaces of the metal connecting portion 44 are surrounded by the oxide adhesive layer 43.
[0129] The metal connecting portion 44 connects the metal support 10 and the embossed portion 31. One end of the metal connecting portion 44 is connected to the metal support 10, and the other end of the metal connecting portion 44 is connected to the embossed portion 31. The metal connecting portion 44 may be substantially integral with at least one of the metal support 10 and the embossed portion 31.
[0130] By embedding the metal connecting portion 44 in the oxide adhesive layer 43, cracks occurring in the oxide adhesive layer 43 can be stopped at the metal connecting portion 44. Therefore, brittle fracture of the oxide adhesive layer 43 can be suppressed, and the bond between the metal support 10 and the embossed portion 31 can be maintained for a longer period of time.
[0131] In FIG. 5, two metal connecting portions 44 are illustrated, but the number of metal connecting portions 44 in one cross section is not particularly limited as long as it is one or more.
[0132] 5, a metal connecting portion 44 having a constricted cross section and a metal connecting portion 44 having a linear cross section are shown in order from the left. Thus, in FIG. 5, the cross-sectional shapes of the metal connecting portions 44 are different from each other, but the cross-sectional shapes of the metal connecting portions 44 may be the same. Also, the cross-sectional shape of the metal connecting portions 44 may be a shape other than the shape shown in FIG. 5.
[0133] The metal connection part 44 is made of metal. The metal connection part 44 preferably contains as its main component the same element as the main component of at least one of the metal support 10 and the embossed part 31. This makes it possible to suppress a change in composition of the metal connection part 44 due to element diffusion from the metal support 10 and the embossed part 31. For example, the metal connection part 44 can contain Cr or Fe as its main component.
[0134] Moreover, it is preferable that the metal connecting portion 44 contains Cr, which can improve the oxidation resistance of the metal connecting portion 44.
[0135] The ratio of the minimum width W2 of the metal connecting portion 44 in the planar direction to the thickness of the oxide adhesive layer 43 in the thickness direction is preferably 0.3 or more. This ensures the strength of the metal connecting portion 44, thereby preventing the metal connecting portion 44 from being damaged by cracks. The planar direction is the direction perpendicular to the thickness direction.
[0136] The thickness of the adhesive layer 43 is the arithmetic average of the thicknesses of the oxide adhesive layer 43 at three locations that divide the oxide adhesive layer 43 into four equal parts in the surface direction. However, when the location where the thickness is to be measured overlaps with the metal connecting portion 44, the thickness of the oxide adhesive layer 43 may be measured at any location close to the metal connecting portion 44. The thickness of the adhesive layer 43 is not particularly limited, but may be, for example, 0.3 μm or more and 30 μm or less.
[0137] The minimum width W2 of the metal connecting portion 44 is the minimum measurement value when the width of the metal connecting portion 44 in the planar direction is measured at 10 locations that divide the metal connecting portion 44 into 11 equal parts in the thickness direction. The value of the minimum width W2 of the metal connecting portion 44 is not particularly limited, but can be, for example, 0.05 μm or more and 5 μm or less.
[0138] When multiple metal connectors 44 are present, the ratio of the longest distance D2 between the metal connectors 44 in the planar direction to the thickness of the oxide adhesive layer 43 in the thickness direction is preferably 20 or less. This allows multiple metal connectors 44 to be arranged in a narrow range in the planar direction, thereby preventing long cracks from occurring in the oxide adhesive layer 43. As a result, peeling of the oxide adhesive layer 43 from the metal support 10 and the embossed portion 31 due to long cracks can be prevented.
[0139] The maximum distance D2 between the metal connecting parts 44 is the maximum distance between two straight lines that are parallel to the thickness direction and inscribed in the outlines of the side surfaces of the two opposing metal connecting parts 44. The value of the maximum distance D2 is not particularly limited, but can be, for example, 1 μm or more and 100 μm or less.
[0140] The ratio of the thickness of the metal support 10 or the embossed portion 31 in the thickness direction to the minimum width W2 of the metal connecting portion 44 in the surface direction is preferably equal to or less than 2000. This makes it possible to prevent the metal support 10 or the embossed portion 31 from becoming excessively thick (i.e., the metal connecting portion 44 from becoming excessively thin), thereby ensuring the strength of the metal connecting portion 44.
[0141] The ratio of the thickness of the metal support 10 or the embossed portion 31 in the thickness direction to the minimum width W2 of the metal connecting portion 44 in the surface direction is preferably equal to or greater than 50. This makes it possible to prevent the metal support 10 or the embossed portion 31 from becoming excessively thin (i.e., the metal connecting portion 44 from becoming excessively thick), thereby increasing the rigidity of the joint 60.
[0142] It is preferable that the metal connecting portion 44 is away from the internal space 3a. Specifically, it is preferable that the metal connecting portion 44 is present in at least one of the central portion in the planar direction and the inner peripheral portion in the planar direction. This can prevent the metal connecting portion 44 from being embrittled by the reducing gas (H2 in this embodiment) flowing through the internal space 3a. The central portion in the planar direction is a portion located in the center when the oxide adhesive layer 43 is divided into thirds in the planar direction. The inner peripheral portion in the planar direction is a portion located on the opposite side to the internal space 3a with respect to the central portion in the planar direction when the oxide adhesive layer 43 is divided into thirds in the planar direction.
[0143] The joint 60 can be formed as follows. First, a paste containing Cr oxide and metal particles is applied onto at least one surface of the metal support 10 and the embossed portion 31. At this time, the amount of the paste applied is adjusted so that the thickness of the applied paste is approximately the same as the average particle size of the metal particles. Next, the paste is fired to form the joint 60. The metal particles are connected to the metal support 10 and the embossed portion 31 by element diffusion between the metal support 10 and the embossed portion 31. The firing conditions can be set appropriately, and can be, for example, 600°C to 1100°C and 0.5 hours to 24 hours.
[0144] (Modification of the embodiment) Although the embodiments of the present invention have been described above, the present invention is not limited to these, and various modifications are possible without departing from the spirit of the present invention.
[0145] [Variation 1] In the above first and second embodiments, the frame 20 and the interconnector 30 are separate members, but the frame 20 and the interconnector 30 may be an integral member. In this case, the chromium alloy container 3 does not include the second seal portion 50.
[0146] [Variation 2] In the first and second embodiments, the metal support 10 and the frame 20 are separate members, but the metal support 10 and the frame 20 may be an integral member. In this case, the chromium alloy container 3 does not include the first seal portion 40.
[0147] [Variation 3] In the first and second embodiments, the oxide adhesion layer 41 has a single-layer structure, but is not limited to this. The oxide adhesion layer 41 may have a multi-layer structure of two or more layers each composed of Cr oxides having different compositions.
[0148] [Variation 4] In the second embodiment, the oxide adhesion layer 43 has a single-layer structure, but is not limited to this. The oxide adhesion layer 43 may have a multi-layer structure of two or more layers each composed of Cr oxides having different compositions.
[0149] [Variation 5] In the first embodiment, the metal support 10 and the frame 20 may be partially welded or brazed. In this case, the first seal portion 40 may be divided in the planar direction by welding or brazing the metal support 10 and the frame 20.
[0150] In the first embodiment, the frame 20 and the interconnector 30 may be partially welded or brazed. In this case, the second seal portion 50 may be divided in the planar direction by welding or brazing the frame 20 and the interconnector 30.
[0151] In the second embodiment, the metal support 10 and the embossed portion 31 may be partially welded or brazed. In this case, the joint 60 may be divided in the planar direction by the welding or brazing of the metal support 10 and the embossed portion 31.
[0152] [Variation 6] In the above embodiment, an electrolytic cell has been described as an example of an electrochemical cell, but the electrochemical cell is not limited to an electrolytic cell. An electrochemical cell is a general term for an element in which a pair of electrodes are arranged so that an electromotive force is generated from an overall oxidation-reduction reaction in order to convert electrical energy into chemical energy, and an element for converting chemical energy into electrical energy. Therefore, the electrochemical cell includes, for example, a fuel cell that uses oxide ions or protons as a carrier.
[0153] [Variation 7] In the above embodiment, the chromium alloy container according to the present invention is applied to an electrochemical cell, but the chromium alloy container can be used for various purposes. For example, the chromium alloy container can be used as a methanation reactor for synthesizing methane from hydrogen and carbon dioxide. EXAMPLES
[0154] The following describes examples of the chromium alloy container according to the present invention, but the present invention is not limited to the following examples.
[0155] (Sample No. 1-5) Chromium alloy containers 3 (see FIG. 3) according to Samples No. 1 to 5 were fabricated as follows.
[0156] First, a paste containing Cr2O3 and metal particles (specifically, SUS430 particles) was applied to the outer periphery of the second main surface 13 of the metal support 10, and then the frame 20 was placed on the paste to produce a laminate. At this time, the minimum width W1 of the metal connecting portion 42 was changed by changing the particle size of the metal particles.
[0157] Next, the laminate was subjected to a heat treatment (1000°C, 1 hour) to form the first seal portion 40 from the paste, which was composed of the oxide adhesive layer 41 and the metal connecting portion 42. In this way, the chromium alloy container 3 equipped with the first seal portion 40 was completed.
[0158] Next, the chromium alloy container 3 was subjected to a thermal cycle test in which a process of heating from room temperature to 800° C. at a heating / cooling rate of 200° C. / hr and then cooling from 800° C. to room temperature at a cooling rate of 200° C. / hr was repeated 10 times.
[0159] Next, the chromium alloy container 3 was cut along the thickness direction to expose a cross section of the first seal portion 40 along the thickness direction.
[0160] Next, as described in the above embodiment, the cross section of the first seal portion 40 was observed with an SEM (5000x) to measure the ratio of the minimum width W1 of the metal connecting portion 42 to the thickness of the oxide adhesive layer 41. The measurement results of this ratio are shown in Table 1.
[0161] Next, the cross section of the first seal portion 40 was observed with an SEM (5000x) to check for the presence or absence of cracks at the joints between the metal support 10 and the metal connecting portion 42 and between the metal support 10 and the frame 20 and between the metal connecting portion 42 and the frame 20. The results of the cracking are shown in Table 1.
[0162] [Table 1]
[0163] As shown in Table 1, in samples Nos. 1 to 4 in which the ratio of the minimum width W1 of the metal connecting portion 42 to the thickness of the oxide adhesive layer 41 was 0.3 or more, it was possible to suppress the occurrence of cracks at the joints between the metal supporting body 10 and the metal connecting portion 42 and between the metal supporting body 10 and the frame body 20 and between the metal connecting portion 42 and the thickness of the oxide adhesive layer 41 being 0.3 or more. This shows that the strength of the metal connecting portion 42 can be ensured by setting the ratio of the minimum width W1 of the metal connecting portion 42 to the thickness of the oxide adhesive layer 41 to be 0.3 or more.
[0164] Although not shown in Table 1, the same results as those of the first seal portion 40 were obtained for the second seal portion 50.
[0165] (Sample No. 6-10) Chromium alloy containers 3 (see FIG. 3) according to Samples No. 6 to 10 were fabricated as follows.
[0166] First, a paste containing Cr2O3 and metal particles (specifically, SUS430 particles) was applied to the outer periphery of the second main surface 13 of the metal support 10, and then the frame 20 was placed on the paste to produce a laminate. At this time, the maximum distance D1 between the metal connecting parts 42 was changed by changing the amount of metal particles added.
[0167] Next, the laminate was subjected to a heat treatment (1000°C, 1 hour) to form the first seal portion 40 from the paste, which was composed of the oxide adhesive layer 41 and the metal connecting portion 42. In this way, the chromium alloy container 3 equipped with the first seal portion 40 was completed.
[0168] Next, the chromium alloy container 3 was subjected to a thermal cycle test in which a process of heating from room temperature to 800° C. at a heating / cooling rate of 200° C. / hr and then cooling from 800° C. to room temperature at a cooling rate of 200° C. / hr was repeated 10 times.
[0169] Next, the chromium alloy container 3 was cut along the thickness direction to expose a cross section of the first seal portion 40 along the thickness direction.
[0170] Next, as described in the above embodiment, the cross section of the first seal portion 40 was observed with an SEM (5000x) to measure the ratio of the longest distance D1 between the metal connectors 42 to the thickness of the oxide adhesive layer 41. The measurement results of this ratio are shown in Table 2.
[0171] Next, the cross section of the first seal portion 40 was observed with an SEM (5000x) to check whether the oxide adhesive layer 41 had locally peeled off from the metal support 10 and the frame 20 near the crack that had occurred in the oxide adhesive layer 41. The peeling confirmation results are shown in Table 2.
[0172] [Table 2]
[0173] As shown in Table 2, in samples Nos. 6 to 9 in which the ratio of the longest distance D1 between the metal connections 42 to the thickness of the oxide bonding layer 41 was set to 20 or less, peeling of the oxide bonding layer 41 was suppressed. This shows that by setting the ratio of the longest distance D1 between the metal connections 42 to the thickness of the oxide bonding layer 41 to 20 or less, local peeling due to cracks in the oxide bonding layer 43 can be suppressed.
[0174] Although not shown in Table 2, the same results as those of the first seal portion 40 were obtained for the second seal portion 50.
[0175] (Sample No. 11-18) Chromium alloy containers 3 (see FIG. 3) according to Samples No. 11 to 18 were fabricated as follows.
[0176] First, a paste containing Cr2O3 and metal particles (specifically, SUS430 particles) was applied to the outer periphery of the second main surface 13 of the metal support 10, and then the frame 20 was placed on the paste to produce a laminate. At this time, the minimum width W1 of the metal connecting portion 42 was changed by changing the particle size of the metal particles.
[0177] Next, the laminate was subjected to a heat treatment (1000°C, 1 hour) to form the first seal portion 40 from the paste, which was composed of the oxide adhesive layer 41 and the metal connecting portion 42. In this way, the chromium alloy container 3 equipped with the first seal portion 40 was completed.
[0178] Next, the chromium alloy container 3 was subjected to a thermal cycle test in which a process of heating from room temperature to 800° C. at a heating / cooling rate of 200° C. / hr and then cooling from 800° C. to room temperature at a cooling rate of 200° C. / hr was repeated 10 times.
[0179] Next, the chromium alloy container 3 was cut along the thickness direction to expose a cross section of the first seal portion 40 along the thickness direction.
[0180] Next, as explained in the above embodiment, the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 was measured. Table 3 shows the measurement results of this ratio.
[0181] Next, the cross section of the first seal portion 40 was observed with an SEM (5000x) to check for the presence or absence of cracks at the joints between the metal support 10 and the metal connecting portion 42 and between the frame 20 and the metal connecting portion 42. The crack confirmation results are shown in Table 3.
[0182] Next, a three-dimensional shape measuring device was used to measure the amount of deflection of the first seal portion 40. The measurement results of the amount of deflection are shown in Table 3.
[0183] [Table 3]
[0184] As shown in Table 3, in samples Nos. 11 to 17 in which the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 was set to 2000 or less, it was possible to suppress the occurrence of cracks at the joints between the metal support 10 and the metal connecting portion 42 and between the metal support 10 and the frame 20 and between the metal connecting portion 42 and the minimum width W1 of the metal connecting portion 42 and the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 was set to 2000 or less. This shows that the strength of the metal connecting portion 42 can be ensured by setting the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 to 2000 or less.
[0185] Furthermore, as shown in Table 3, in samples Nos. 12 to 18 in which the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 was set to 50 or more, it was possible to suppress the amount of deflection of the first seal portion 40. This shows that the rigidity of the first seal portion 40 can be increased by setting the ratio of the thickness of the metal support 10 to the minimum width W1 of the metal connecting portion 42 to 50 or more.
[0186] Although not shown in Table 3, the same results as those of the first seal portion 40 were obtained for the second seal portion 50. [Explanation of symbols]
[0187] 1,1a Electrolysis cell 2 Cell body 3. Chromium alloy container 3a Interior space 6 Hydrogen electrode 7 Electrolytes 8. Reaction prevention layer 9 Oxygen electrode 10 Metal support 11 Supply hole 12 First main surface 13 Second main surface 20 Frame 30 Interconnector 31 Embossed section 40 First seal part 41,43 Oxide adhesive layer 42,44 Metal connections 50 Second seal part 60 Joint
Claims
1. A chromium alloy container having an internal space, A first alloy member made of an alloy containing chromium; A second alloy member made of an alloy containing chromium; an insertion portion interposed between the first alloy member and the second alloy member; Equipped with The insertion portion is an oxide adhesion layer composed of an oxide mainly composed of chromium; a metal connector embedded in the oxide adhesive layer and connecting the first alloy member and the second alloy member; having Chromium alloy container.
2. The metal connection portion contains, as a main component, the same element as a main component of at least one of the first alloy member and the second alloy member.
2. The chromium alloy container according to claim 1.
3. The metal connection portion contains chromium.
3. The chromium alloy container according to claim 1 or 2.
4. The ratio of the minimum width of the metal connection portion in the surface direction to the thickness of the oxide adhesion layer in the thickness direction is 0.3 or more.
2. The chromium alloy container according to claim 1.
5. The ratio of the maximum distance between the metal connections in the surface direction to the thickness of the oxide adhesive layer in the thickness direction is 20 or less.
2. The chromium alloy container according to claim 1.
6. The ratio of the thickness of the first alloy member or the second alloy member in the thickness direction to the minimum width of the metal connection portion in the surface direction is 50 or more.
2. The chromium alloy container according to claim 1.
7. The ratio of the thickness of the first alloy member or the second alloy member in the thickness direction to the minimum width of the metal connection portion in the surface direction is 2000 or less.
2. The chromium alloy container according to claim 1.
8. The chromium content of the metal elements in the oxide adhesion layer is 50 mol % or more.
2. The chromium alloy container according to claim 1.
9. The oxide adhesion layer is composed of at least one of chromium oxide and chromium manganese oxide.
2. The chromium alloy container according to claim 1.
10. the oxide adhesion layer is crystalline; 2. The chromium alloy container according to claim 1.
11. The oxide adhesion layer has a spinel or corundum type crystal structure; The chromium alloy container according to claim 10.
12. The insertion portion is a seal for sealing the internal space.
2. The chromium alloy container according to claim 1.
13. The second alloy member has an embossed portion in contact with the first alloy member, The insertion portion bonds the embossed portion to the first alloy member.
2. The chromium alloy container according to claim 1.
14. The chromium alloy container according to claim 1 ; a cell body disposed on the chromium alloy vessel; Equipped with the first alloy member has a plurality of communicating holes that communicate with the internal space, the cell main body is disposed on the first alloy member so as to cover the plurality of communication holes; Metal-supported electrochemical cells.
Citation Information
Patent Citations
Joining material of solid electrolyte fuel cell stack and its joining method
JP1996130022A
Inorganic adhesive, semiconductor device using the same and its production
JP1997217039A
Solid electrolyte fuel cell
JP1998106596A
Sealing material for low-temperature operation solid oxide fuel cell
JP2004039573A
Metal support solid oxide fuel cell and manufacturing method therefor
JP2016207630A