Brazing sheet for heat exchanger and heat exchanger for air conditioning device

The brazing sheet for air conditioner heat exchangers optimizes zinc and silicon content in the sacrificial anode material to enhance both corrosion resistance and pressure resistance, addressing the higher operational demands of air conditioner heat exchangers.

JP7588324B2Active Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2019188044
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-10-11
Publication Date
2024-11-22
Estimated Expiration
2039-10-11

AI Technical Summary

Technical Problem

Brazing sheets for air conditioner heat exchangers require higher bonding strength and corrosion resistance compared to those for automobiles, as they operate under higher refrigerant pressures, and existing compositions compromise on either strength or corrosion resistance due to improper zinc and silicon content.

Method used

A brazing sheet for air conditioner heat exchangers with a core material coated on one side with an aluminum-silicon brazing filler metal and on the other side with a sacrificial anode material containing zinc and silicon, with specific thickness and silicon content optimized within the range of 15 to 25 μm, and bonding temperature between 580 to 660°C, ensuring both corrosion resistance and pressure resistance.

Benefits of technology

The optimized brazing sheet achieves both good corrosion resistance and pressure resistance, maintaining structural integrity under high refrigerant pressures by balancing zinc and silicon content in the sacrificial anode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588324000001
    Figure 0007588324000001
  • Figure 0007588324000002
    Figure 0007588324000002
  • Figure 0007588324000003
    Figure 0007588324000003
Patent Text Reader

Abstract

To provide a brazing sheet used in a heat exchanger for an air conditioner, enabling corrosion resistance and pressure resistance to be favorably compatible with each other and including a sacrificial anode material layer.SOLUTION: A brazing sheet 10 is used in a heat exchanger of an air conditioner and includes an aluminum (Al) alloy core material 11, an Al alloy brazing material layer 12 coated with one surface of the core material and containing Si, and an Al alloy sacrificial anode material layer 13 coated with the other surface of the core material and containing Zn and Si. The thickness of the sacrificial anode material layer 13 is within a range of 15-25 μm. When the temperature T of the brazing sheet 10 at the time of joining is within the range of 580-660°C, the content XSi of Si in the sacrificial anode material is equal to or smaller than a value derived from the formula (1):T=660-8×exp(0.3XSi) and also is equal to or larger than a value derived from the formula (2):T=580+55×exp(-0.5(XSi-1.7)).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a brazing sheet used in a member constituting a heat exchanger, and to a heat exchanger for an air conditioner constructed using the brazing sheet. [Background technology]

[0002] A typical heat exchanger usually comprises tubes and fins, with multiple fins attached to the outer periphery of the tubes. Copper (Cu) or its alloys (referred to as "copper materials" for convenience) have traditionally been used as the material for the tubes, but in recent years aluminum (Al) or its alloys (aluminum materials) have also been used. Aluminum materials are generally used as the material for the fins.

[0003] When manufacturing heat exchangers, brazing is generally used to attach fins to tubes. If both the tubes and fins are made of aluminum, a brazing sheet is used, in which at least one surface of an aluminum alloy core is clad with a brazing layer. Considering the corrosion resistance of the tubes and fins, a brazing sheet is used in which one surface of the core is clad with brazing and the other surface is clad with a sacrificial anode material.

[0004] The brazing filler metal is generally an aluminum-silicon (Si) alloy, which is used for brazing aluminum alloys, and the sacrificial anode material is generally an aluminum alloy with zinc (Zn) added to make its potential more base. A typical sacrificial anode material is one in which zinc is added to a general aluminum-silicon alloy brazing filler metal. This allows the sacrificial anode material to function as a brazing filler metal.

[0005] Since automotive heat exchangers may come into contact with exhaust gases, they are required to have higher corrosion resistance than heat exchangers used in building air conditioners, etc. For example, Patent Document 1 discloses an aluminum alloy brazing sheet that can be used as a fluid passage component for automotive heat exchangers. In this brazing sheet, the sacrificial anode material is an aluminum alloy containing 2.5 to 7.0 mass% Si, 1.0 to 5.5 mass% Zn, and 0.05 to 1.0 mass% Fe, with the remainder being Al and unavoidable impurities, and the cladding thickness of the sacrificial anode material is 25 to 80 μm.

[0006] Meanwhile, Patent Document 2 discloses an aluminum alloy brazing fin material for heat exchangers, used in heat exchangers for air conditioners (room air conditioners, air conditioners) or refrigerators. In this brazing fin material, the sacrificial anode material is composed of an aluminum alloy containing 7 to 15 mass% Zn, with the remainder being Al and unavoidable impurities. The cladding thickness of this sacrificial anode material is preferably 7 μm or more, and more preferably 7 to 40 μm. Furthermore, the sacrificial anode material may contain up to 8.0 mass% Si in order to suppress excessive coarsening of crystal grains and improve corrosion resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2011 / 034102 [Patent Document 2] Japanese Patent Application Laid-Open No. 2017-155308 Summary of the Invention [Problem to be solved by the invention]

[0008] As a result of intensive research by the present inventors, it became clear that brazing sheets for air conditioner heat exchangers require higher bonding strength than brazing sheets for automobiles. This is because, in general, the upper limit of the allowable refrigerant pressure (allowable internal pressure) for air conditioner heat exchangers is relatively higher than that for automobile heat exchangers. When the sacrificial anode material also serves as a brazing material, the sacrificial anode material is naturally required to have high bonding strength.

[0009] The brazing sheet disclosed in Patent Document 1 is for automobiles and must contain iron (Fe). On the other hand, the brazing fin material disclosed in Patent Document 2 is not intended for the sacrificial anode material to double as a brazing filler metal, and the inclusion of Si is intended to contribute to the sacrificial anode function.

[0010] Furthermore, Patent Document 2 states that the sacrificial anode function cannot be exerted unless the Zn content of the sacrificial anode material is 7.0 mass% or more, but the inventors' studies have shown that the Zn content can be less than 7.0 mass%. On the other hand, when the sacrificial anode material also serves as a brazing material, it is possible to increase the joint strength by increasing the Si content, but it has also become clear that if the Si content is too high, the fluidity becomes too high and the corrosion resistance of the brazing sheet is significantly reduced.

[0011] The present invention has been made to solve these problems, and aims to provide a brazing sheet having a sacrificial anode material layer that can be used in heat exchangers for air conditioning systems and that can achieve both good corrosion resistance and good pressure resistance. [Means for solving the problem]

[0012] In order to solve the above-mentioned problems, the brazing sheet according to the present invention is a brazing sheet used in a heat exchanger of an air conditioner, and comprises: an aluminum alloy core material; a brazing material layer coated on one side of the core material and made of a brazing material of an aluminum alloy containing silicon (Si); and a sacrificial anode material layer coated on the other side of the core material and made of a sacrificial anode material of an aluminum alloy containing zinc (Zn) and silicon (Si), wherein the thickness of the sacrificial anode material layer is within a range of 15 to 25 μm, and when the temperature T during joining of the brazing sheet is within a range of 580 to 660°C, the silicon content X of the sacrificial anode material is 100% or more. Si is expressed by the following equation (1): T = 660 - 8 × exp(0.3X Si ) ···(1) and the value obtained by the following formula (2) T=580+55×exp(-0.5(X Si -1.7)) (2) This is a configuration in which the value is equal to or greater than the value derived from

[0013] Alternatively, in order to solve the above-mentioned problems, the brazing sheet according to the present invention is a brazing sheet used in a heat exchanger of an air conditioner, and comprises a core material made of an aluminum alloy, and a sacrificial anode material layer made of a sacrificial anode material of an aluminum alloy containing zinc (Zn) and silicon (Si) that is coated on both surfaces of the core material, and the thickness of the sacrificial anode material layer is within a range of 15 to 25 μm, and when the temperature T during joining of the brazing sheet is within a range of 580 to 660°C, the silicon content X of the sacrificial anode material is Si is expressed by the following equation (1): T = 660 - 8 × exp(0.3X Si ) ···(1) and the value obtained by the following formula (2) T=580+55×exp(-0.5(X Si -1.7)) (2) It may be configured such that the value is equal to or greater than the value derived from

[0014] According to the above configuration, in a brazing sheet used in a heat exchanger for an air conditioner, the sacrificial anode material layer contains zinc and silicon within the above ranges. This allows the sacrificial anode material, which also serves as a brazing material, to have an optimal zinc content as well as an optimal silicon content. Therefore, even if the thickness of the sacrificial anode material layer is within the above range, it is possible to achieve both corrosion resistance and pressure resistance in the brazing sheet joint structure.

[0015] The present invention also includes a heat exchanger for an air conditioner, which is constructed using the brazing sheet having the above-described configuration. [Effects of the Invention]

[0016] With the above-described configuration, the present invention has the effect of providing a brazing sheet having a sacrificial anode material layer that can be used in a heat exchanger for an air conditioner and that can achieve both good corrosion resistance and good pressure resistance. [Brief explanation of the drawings]

[0017] [Figure 1] FIG. 1A is a schematic cross-sectional view showing the general configuration of a brazing sheet according to a representative embodiment of the present invention, and FIG. 1B is a schematic cross-sectional view showing the general configuration of the joining structure of a brazing sheet according to a representative embodiment of the present invention. [Figure 2] 2 is a schematic cross-sectional view showing an example of a header of a plate-fin stacked heat exchanger constructed using the brazing sheet shown in FIG. 1. FIG. [Figure 3] FIG. 1 is a schematic cross-sectional view showing an example of a header of a plate-fin stacked heat exchanger constructed using a brazing sheet having sacrificial anode material layers on both sides. [Figure 4] 6(A) to 6(D) are diagrams showing the results of corrosion resistance tests of the brazing sheet joint structures according to the examples and comparative examples. [Figure 5] FIG. 10 is a diagram showing the results of a corrosion resistance test of the joint structure of the brazing sheet according to another example. DETAILED DESCRIPTION OF THE INVENTION

[0018] The brazing sheet according to the present disclosure is used in a heat exchanger of an air conditioner, and comprises: an aluminum alloy core material; a brazing material layer coated on one side of the core material and made of a brazing material of an aluminum alloy containing silicon (Si); and a sacrificial anode material layer coated on the other side of the core material and made of a sacrificial anode material of an aluminum alloy containing zinc (Zn) and silicon (Si), wherein the thickness of the sacrificial anode material layer is within a range of 15 to 25 μm, and when the temperature T during joining of the brazing sheet is within a range of 580 to 660°C, the silicon content X of the sacrificial anode material is 15 to 25 μm. Si is expressed by the following equation (1): T = 660 - 8 × exp(0.3X Si ) ···(1) and the value obtained by the following formula (2) T=580+55×exp(-0.5(X Si -1.7)) (2) This is a configuration in which the value is equal to or greater than the value derived from

[0019] Further, a brazing sheet according to the present disclosure is a brazing sheet used in a heat exchanger of an air conditioner, and comprises a core material made of an aluminum alloy, and a sacrificial anode material layer made of an aluminum alloy containing zinc (Zn) and silicon (Si) and coated on both surfaces of the core material, wherein the thickness of the sacrificial anode material layer is within a range of 15 to 25 μm, and when the temperature T during joining of the brazing sheet is within a range of 580 to 660°C, the silicon content X of the sacrificial anode material is Si is expressed by the following equation (1): T = 660 - 8 × exp(0.3X Si ) ···(1) and the value obtained by the following formula (2) T=580+55×exp(-0.5(X Si -1.7)) (2) It may be configured such that the value is equal to or greater than the value derived from

[0020] According to the above configuration, in a brazing sheet used in a heat exchanger for an air conditioner, the sacrificial anode material layer contains zinc and silicon within the above ranges. This allows the sacrificial anode material, which also serves as a brazing material, to have an optimal zinc content as well as an optimal silicon content. Therefore, even if the thickness of the sacrificial anode material layer is within the above range, it is possible to achieve both corrosion resistance and pressure resistance in the brazing sheet joint structure.

[0021] In a brazing sheet having the above configuration, the brazing sheet may have a joint portion that is joined together to form a joint, and an inclined portion adjacent to this joint portion, and the inclination angle of the inclined portion relative to the joint portion may be 40° or less.

[0022] Furthermore, in the brazing sheet having the above configuration, the core material may be any of a 3000 series, 5000 series, or 6000 series aluminum alloy, and the sacrificial anode material may be a 4000 series aluminum alloy containing zinc and silicon within the above ranges.

[0023] In the brazing sheet having the above configuration, the brazing material may be a 4000 series aluminum alloy.

[0024] The heat exchanger for an air conditioner according to the present disclosure may be configured using a brazing sheet having the above-described configuration.

[0025] The heat exchanger for an air conditioner having the above-described configuration may also be of a plate fin stack type.

[0026] Representative embodiments of the present invention will be described below with reference to the drawings. Note that the same or corresponding elements will be designated by the same reference numerals throughout the drawings, and redundant description will be omitted.

[0027] The brazing sheet according to the present disclosure is made of an aluminum alloy used in heat exchangers. Specifically, for example, as shown in Fig. 1(A), the brazing sheet 10 according to the present disclosure includes a core material 11, a brazing material layer 12, and a sacrificial anode material layer 13. The brazing material layer 12 is clad on one side of the core material 11, and the sacrificial anode material layer 13 is clad on the other side of the core material 11, i.e., the side opposite to the side on which the brazing material layer 12 is clad. The core material 11, the brazing material constituting the brazing material layer 12, and the sacrificial anode material constituting the sacrificial anode material layer 13 are all aluminum alloys.

[0028] Alternatively, although not shown, the brazing sheet 10 according to the present disclosure may have a configuration including a core material 11 and a sacrificial anode material layer 13, but not including a brazing material layer 12. In such a brazing sheet 10, the sacrificial anode material layer 13 is formed on both surfaces of the core material 11.

[0029] The brazing sheet 10 according to the present disclosure has a joining region at least on the side of the sacrificial anode material layer 13, and a joint is formed by joining the joining surfaces of this joining region to each other. The structure in which brazing sheets 10 are joined together at their joining regions is the joining structure of the brazing sheet 10 according to the present disclosure. The specific shape of the brazing sheet 10 according to the present disclosure is not particularly limited, but a representative example is a configuration having an inclined region adjacent to the joining region and inclined relative to the joining region.

[0030] Specifically, as shown in FIG. 1B, a joint structure 20 of a brazing sheet 10 according to the present disclosure is formed by joining joint portions 10a of the brazing sheet 10 together. An inclined portion 10b is adjacent to the joint portion 10a. The inclination angle θ1 of the inclined portion 10b relative to the joint portion 10a is not particularly limited. However, since the angle θ2 formed between the inclined portions 10b in the joint structure 20 is an acute angle, i.e., less than 90° (θ2<90°), the inclination angle θ1 may be less than half of that, i.e., 45°. Furthermore, as shown in FIG. 1B, a fillet 22 is formed between the inclined portions 10b. In this embodiment, this fillet 22 is defined as a solidified brazing filler metal or sacrificial anode material that flows out of the joint portion 10a during joining.

[0031] For ease of explanation, the angle θ2 formed by each inclined portion 10b constituting the joint structure 20 is referred to as the "inclined portion angle." In addition, in FIG. 1(B), the inclined portion angle θ1 and the inclined portion angle θ2 are shown by dotted lines, and the reference for these angles is the midline of the thickness of the brazing sheet 10 (the line that is the midpoint in thickness (depth) from both one surface and the other surface), as shown by the dotted line in the figure. However, the reference for these angles θ1 and θ2 is not limited to the midline of the thickness, and may be any other known reference (for example, an angle based on the surface on the joining side).

[0032] As described above, the inclination angle θ1 may be less than 45°, but its upper limit is preferably less than 40°, and more preferably less than 35°. Depending on the structure of the air-conditioning heat exchanger, if the inclination angle θ1 exceeds 40°, there is a risk that partial thickness reduction will occur in the brazing sheet 10 or partial erosion will occur in the core material 11 during press working.

[0033] If the inclination angle θ1 of the inclined portion 10b relative to the joining portion 10a becomes relatively large, the brazing sheet 10 will be subjected to significant processing during press working. This will cause localized thinning of the brazing sheet 10. If the brazing sheet 10 is partially thinned, stress concentration or insufficient pressure resistance will occur in the thinned portion, which may result in breakage from that portion.

[0034] Furthermore, when large deformation is applied to the brazing sheet 10, the diffusion coefficient of silicon from the brazing material layer 12 to the core material 11 increases in the areas where the deformation has been applied, which increases the risk of erosion (melting of the core material 11). When erosion occurs, the zinc contained in the sacrificial anode material layer 13 surrounding the melted core material 11 is engulfed, and part of the core material 11 becomes a "sacrificial anode material." As a result, there is a possibility that the brazing sheet 10 will penetrate early from the area where erosion has occurred.

[0035] In contrast, if the inclination angle θ1 is 40° or less, the risk of significant processing being applied to the brazing sheet 10 is reduced. This effectively reduces the risk of localized thinning of the brazing sheet 10 or localized erosion of the core material 11. Of course, depending on the structure of the air-conditioning heat exchanger, localized thinning of the brazing sheet 10 or localized erosion of the core material 11 during press processing may be suppressed even if the inclination angle θ1 exceeds 40°, so the upper limit of the inclination angle θ1 is not necessarily 40°.

[0036] On the other hand, the lower limit of the inclination angle θ1 is not particularly limited, and a suitable lower limit may be set depending on the structure of the heat exchanger for an air conditioner. For example, in the case of a plate-fin stack-type heat exchanger described below, it is preferable that the inclination angle θ1 not be too small in order to ensure a flow path for the adjacent air (second fluid). The lower limit of the inclination angle θ1 in a plate-fin stack-type heat exchanger is preferably 15° or more, and more preferably 20° or more.

[0037] The core material 11 included in the brazing sheet 10 according to the present disclosure may be any known aluminum alloy that can achieve the physical properties required depending on various conditions such as the type or structure of the heat exchanger. In the field of heat exchangers, typical examples of aluminum alloys used as the core material 11 include, but are not limited to, 3000 series (aluminum-manganese (Al-Mn)-based alloys), 5000 series (aluminum-magnesium (Al-Mg)-based alloys), and 6000 series (aluminum-magnesium-silicon (Al-Mg-Si)-based alloys).

[0038] Alternatively, the core material 11 may contain known elements added to the aluminum alloy at a content (concentration) exceeding that of unavoidable impurities. The upper limit of the concentration of unavoidable impurities varies depending on various conditions, but may be, for example, less than 0.1 mass% of the entire aluminum alloy. Alternatively, the upper limit of the concentration of unavoidable impurities may conform to the alloy composition specified in known standards such as JIS.

[0039] In the present disclosure, the aluminum alloy used as the brazing filler metal may contain silicon (Si), i.e., may be an aluminum-silicon (Al-Si) alloy. The Si content in the brazing filler metal is not particularly limited, as long as it is within a range that allows suitable use as a brazing filler metal. Specifically, for example, the Si content (concentration) in the brazing filler metal may be within a range of 2.5 to 13 mass%, or may be within a range of 3.5 to 12 mass%. If the Si content is too low, the Al-Si alloy may not function adequately as a brazing filler metal. On the other hand, if the Si content is too high, Si may diffuse into the core material 11 or the mating material, causing the brazing sheet 10 itself to melt. Furthermore, the Al-Si alloy used as the brazing filler metal may contain elements other than Si in a content exceeding unavoidable impurities, as long as the content does not affect the function of the brazing filler metal.

[0040] The aluminum alloy used as the sacrificial anode material contains zinc (Zn) in the range of 2.5 to 6.0 mass % in order to exert the sacrificial anode function. In addition, in the present disclosure, since the sacrificial anode material also serves as a brazing filler metal as described above, it contains Si, similar to the brazing filler metal. The Si content (Si concentration) in the sacrificial anode material can be in the range of 3.0 to 6.0 mass %. Therefore, the aluminum alloy used as the sacrificial anode material may be an aluminum-silicon-zinc (Al-Si-Zn) alloy.

[0041] In the Al-Si-Zn alloy used as a sacrificial anode material, if the Zn content (concentration) is less than 2.5 mass%, the sacrificial anode function will not be satisfactory. On the other hand, if the Zn content exceeds 6.0 mass%, the sacrificial anode function will proceed too quickly, causing the sacrificial anode material layer 13 to disappear prematurely from the brazing sheet 10, which may reduce the corrosion resistance of the brazing sheet 10.

[0042] Furthermore, in an Al-Si-Zn alloy as a sacrificial anode material, if the Si content is less than 3.0 mass%, the sacrificial anode material may not flow sufficiently due to the small amount of Si, and may not be able to exhibit good adhesive strength as a brazing material. On the other hand, if the Si content exceeds 6.0 mass%, although the fluidity as a sacrificial anode material is improved, the fluidity may be too high, resulting in a decrease in corrosion resistance.

[0043] In particular, in the present disclosure, the brazing sheet 10 is used in a heat exchanger for an air conditioner, and in this case, when the brazing sheet 10 is used in a joining structure 20 that forms a refrigerant flow path (such as a plate-fin laminated heat exchanger described below), an adhesive strength sufficient to withstand the upper limit of the allowable pressure of the refrigerant is required. Note that this allowable pressure differs depending on various conditions such as the type, application, and performance of the air conditioner, and therefore the adhesive strength required of the sacrificial anode material can also be set appropriately depending on the various conditions.

[0044] Here, in the present disclosure, taking into consideration the temperature (brazing temperature) when joining the brazing sheets 10 together, the important thing about the Si content is to strike a balance between adhesive strength that can achieve sufficient pressure resistance and sufficient corrosion resistance in the joining structure 20 of the brazing sheets 10. As a result of extensive research by the present inventors into this point, it has become clear that when the temperature T when joining the brazing sheets 10 is within the range of 580 to 660°C, a particularly suitable Si content in the sacrificial anode material can be defined by the following formulas (1) and (2).

[0045] Specifically, in the sacrificial anode material, when the Zn content (concentration) is within the range of 2.0 to 6.0 mass%, the Si content (concentration) is X Si Then, this Si concentration should be equal to or less than the value derived from the following formula (1) and equal to or greater than the value derived from the following formula (2). T = 660 - 8 × exp(0.3X Si ) ···(1) T=580+55×exp(-0.5(X Si -1.7)) (2) In addition, even in an Al-Si-Zn alloy used as a sacrificial anode material, elements other than Si and Zn may be contained in an amount exceeding the amount of unavoidable impurities, as long as the content does not affect the sacrificial anode function and the function as a brazing material.

[0046] The type of aluminum alloy specifically used for the brazing filler metal and the sacrificial anode material is not particularly limited, but typically, a 4000 series (aluminum-silicon (Al-Si) alloy) can be used for both. For the sacrificial anode material, a 4000 series aluminum alloy whose Si content falls within the above range can be selected, or Si can be added by a known method to adjust the Si content to fall within the above range, and Zn can also be added by a known method so that the Zn content falls within the above range.

[0047] In the brazing sheet 10 according to the present disclosure, the cladding ratio of the brazing filler metal and the sacrificial anode material is not particularly limited and may be within a general range. A general cladding ratio is, for example, within a range of 2 to 30 mass %, and may be within a range of 3 to 20 mass %.

[0048] Furthermore, the thickness of the brazing sheet 10 according to the present disclosure, and the thickness of each of the core material 11, brazing material layer 12, and sacrificial anode material layer 13 are not particularly limited and can be set appropriately depending on the configuration of the brazing sheet 10 or the type or components of the heat exchanger to be manufactured. However, in the present disclosure, the thickness of the sacrificial anode material layer 13 is within the range of 15 to 25 μm.

[0049] Because the brazing sheet 10 according to the present disclosure is used in a heat exchanger for an air conditioner, the thickness of the sacrificial anode material layer 13 can be made thinner than that for an automobile. If the thickness of the sacrificial anode material layer 13 can be made thinner, the amount of sacrificial anode material used can be reduced, making it possible to suppress increases in the manufacturing cost of the brazing sheet 10.

[0050] In particular, in this disclosure, a plate-fin stack type heat exchanger can be cited as a preferred example, as described below. In a plate-fin stack type heat exchanger, multiple plate fins are stacked to form a stack, and this stack is then pressed down with a jig and joined (brazed). Therefore, if the thickness of the sacrificial anode material layer 13 is too large, the dimensional change of the stack may become large, which may affect the joint structure 20. If the thickness of the sacrificial anode material layer 13 can be made 25 μm or less, such an effect on the joint structure 20 can be effectively suppressed.

[0051] On the other hand, if the sacrificial anode material layer 13 is less than 15 μm, the absolute amount of the sacrificial anode material relative to the brazing sheet 10 becomes too small. As a result, the sacrificial anode material layer 13 will be prematurely removed from the brazing sheet 10, and the corrosion resistance of the brazing sheet 10 may be reduced.

[0052] In the present disclosure, multiple brazing sheets 10 are stacked with their joining portions 10a facing each other, and then brazed by melting a brazing filler metal and a sacrificial anode material at a high temperature (580°C or higher), thereby joining the brazing sheets 10 together. In a joining structure 20 of the brazing sheet 10 manufactured in this manner, as shown in Fig. 1(B) , in a portion adjacent to the joining portion 10a (joint 21) between the inclined portions 10b, the sacrificial anode material that has flowed out from the sacrificial anode material layer 13 of the joining portion 10a solidifies, forming a fillet 22.

[0053] In the present disclosure, from the viewpoint of evaluating the corrosion resistance of the brazing sheet 10, the potential of the joint 21 (including the fillet 22), the sacrificial anode material layer 13, etc. may be evaluated (measured) by a known method. A typical method for evaluating the potential is to connect a sample for potential measurement (for example, the brazing sheet 10, or the core material 11, the brazing material, the sacrificial anode material, the fillet 22, or the joint 21, or an alloy having a composition simulating these), a counter electrode, and a reference electrode (for example, a silver / silver chloride (Ag / AgCl) electrode) to a potentiostat / galvanostat, immerse the sample in an electrolyte (for example, a 5 wt % sodium chloride (NaCl) solution), and measure the potential difference between the sample and the reference electrode.

[0054] The method for manufacturing the brazing sheet 10 according to the present disclosure is not particularly limited, and known manufacturing methods can be suitably used. Specifically, for example, an aluminum alloy of a desired composition is formed into a plate shape by a known method to form the core material 11, one side of the core material 11 is clad with a brazing filler metal made of an aluminum alloy containing Si by a known method, and the other side of the core material 11 is clad with a sacrificial anode material made of an aluminum alloy containing 2.0 to 6.0 mass% Zn and 3.0 to 6.0 mass% Si by a known method. In the present disclosure, the manufacturing conditions for the brazing sheet 10 can be set appropriately depending on the configuration of the brazing sheet 10 or the type or part of the air-conditioning heat exchanger to be manufactured.

[0055] As described above, the brazing sheet 10 according to the present disclosure can be particularly suitably used in the manufacture of heat exchangers for air conditioning systems. The joining structure 20 formed when the brazing sheet 10 according to the present disclosure is applied to a heat exchanger has a structure as exemplified in Fig. 1(B) as described above, but more specific examples include a plate-fin stacked heat exchanger having a structure as shown in Fig. 2, or a stacked heat exchanger for an air-to-water heat pump having a structure as shown in Figs. 4(A) and (B).

[0056] Although not shown, a plate fin stack heat exchanger is a plate fin stack having flow paths through which a first fluid (refrigerant) flows, and a second fluid (air) flows between the plate fin stacks to exchange heat between the first and second fluids. The plate fins of this heat exchanger have a flow path region having multiple first fluid flow paths through which the first fluid flows in parallel, and a header region having header flow paths that communicate with each of the first fluid flow paths in this flow path region.

[0057] In a plate fin stack heat exchanger, end plates having approximately the same shape as the plate fins in a plan view are provided on both sides of the plate fin stack in the stacking direction, and these paired end plates and the multiple plate fins interposed between them are joined together by brazing while stacked. Figure 2 shows a partial cross section of the schematic structure of the header portion of this plate fin stack 30, with multiple plate fins 32 stacked on an end plate 31 located at the top of the figure.

[0058] The end plates 31 and the plate fins 32 each have an opening, and these plates are stacked to form the plate fin stack 30, thereby forming the header opening 33. In the configuration shown in FIG. 2, a refrigerant, which is a first fluid, flows in from the outside of the header opening 33 in the direction indicated by the block arrow in the figure, and then flows between the plate fins 32. As described above, each plate fin 32 is provided with a first fluid flow path, so the refrigerant that flows between the plate fins 32 flows through the first fluid flow path. In addition, air, which is a second fluid, flows through the spaces formed between the plate fins 32 in a direction that intersects the flow direction of the refrigerant (the direction of the first fluid flow path). This causes the air to be cooled by the refrigerant.

[0059] Specific configuration examples of such plate fin stacked heat exchangers are described in, for example, JP 2017-180856 A, JP 2018-066531 A, JP 2018-066532 A, JP 2018-066533 A, JP 2018-066534 A, JP 2018-066535 A, JP 2018-066536 A, etc., and the contents of these publications are incorporated herein by reference as part of the description of this specification.

[0060] As shown in Fig. 3, the plate fin stack 34 constituting the stack-type heat exchanger for an air-to-water heat pump has a basic configuration similar to that of the plate fin stack 30 of the general plate fin stack-type heat exchanger shown in Fig. 2. However, the plate fins 35 (brazing sheets 10 according to the present disclosure) constituting the plate fin stack 34 have sacrificial anode layers 13 on both sides. Therefore, as shown in Fig. 3, fillets 22 are formed not only at the joints 21 located on the header opening 33 side (inside) but also at the joints 21 located on the opposite side from the header opening 33 side (outside). Note that the configuration shown in Fig. 3 is the same as the configuration shown in Fig. 2 except for the positions of the plate fins 35 and fillets 22, and therefore a description thereof will be omitted.

[0061] Thus, the brazing sheet according to the present disclosure is used in a heat exchanger of an air conditioning unit and comprises an aluminum alloy core material, a brazing material layer of an aluminum alloy containing silicon (Si) coated on one side of the core material, and a sacrificial anode material layer of an aluminum alloy containing zinc (Zn) and silicon (Si) coated on the other side of the core material, or a core material coated with a sacrificial anode material layer on both sides.

[0062] Furthermore, in the brazing sheet according to the present disclosure, when the thickness of the sacrificial anode material layer is within the range of 15 to 25 μm and the temperature T during joining of the brazing sheet is within the range of 580 to 660° C., the silicon content X of the sacrificial anode material is Si is equal to or less than the value derived from formula (1) and equal to or greater than the value derived from formula (2). This allows the sacrificial anode material, which also serves as a brazing filler metal, to have an optimum content of not only zinc but also silicon. Therefore, even if the thickness of the sacrificial anode material layer is within the above range, it is possible to achieve both corrosion resistance and pressure resistance in the brazing sheet joint structure. [Example]

[0063] The present invention will be described in more detail based on examples and comparative examples, but the present invention is not limited thereto. Those skilled in the art can make various changes, modifications, and alterations without departing from the scope of the present invention. The corrosion resistance tests in the following examples and comparative examples were carried out as follows.

[0064] [Corrosion resistance test] The corrosion resistance of the brazing sheet joint structure was evaluated based on the SWAAT test (Sea Water Acidified Test) specified in ASTM G85-A3.

[0065] (Comparative Example 1) The brazing sheet used in Comparative Example 1 had a core material made of 3003 aluminum alloy, a brazing material layer made of 4343 aluminum alloy, and a sacrificial anode material layer made of an aluminum alloy (Al-2.5%Si-4.0%Zn) consisting of 2.5 mass% silicon (Si), 4.0 mass% zinc (Zn), and the remainder aluminum (Al). The inclination angle θ1 of the inclined portion of the brazing sheet was approximately 30°.

[0066] These brazing sheets were brazed together at their joint locations to form a joint. The joint surface of the joint was a sacrificial anode material layer. The brazing temperature was 610°C, and the Si content (concentration) in the sacrificial anode material at this time was within the range of approximately 2.9 to 6.1 mass% based on the above formulas (1) and (2). Visual inspection of the joint confirmed that the joint was insufficient.

[0067] The corrosion resistance of the joints between the brazing sheets was evaluated using the corrosion test described above. As a result, as shown in the cross-sectional photograph in Figure 4(A), the sacrificial anode function of the sacrificial anode material layer was confirmed, but corrosion of the core material was not observed.

[0068] Example 1 In Example 1, the brazing sheets were brazed together to form a joint in the same manner as in Comparative Example 1, except that the sacrificial anode material layer was an aluminum alloy (Al-2.8%Si-4.0%Zn) containing 2.8% silicon (Si) by mass, 4.0% zinc (Zn), and the remainder aluminum (Al). The brazing temperature was 620°C, and the Si content (concentration) in the sacrificial anode material at this time was within the range of approximately 2.3 to 5.3% by mass, based on the formulas (1) and (2). Visual inspection of the joint confirmed good bonding.

[0069] The corrosion resistance of the joints between the brazing sheets was also evaluated using the corrosion test described above. As a result, as shown in the cross-sectional photograph in Figure 4(B), the sacrificial anode function of the sacrificial anode material layer was confirmed, but corrosion of the core material was not observed.

[0070] Example 2 In Example 2, a brazing sheet was used in which the sacrificial anode material layer was an aluminum alloy (Al-4.4%Si-4.0%Zn) of 4.4% silicon (Si) by mass, 4.0% zinc (Zn) by mass, and the remainder aluminum (Al). The brazing sheets were brazed together to form a joint in the same manner as in Comparative Example 1. The brazing temperature was set to 620°C, and the Si content (concentration) in the sacrificial anode material at this time was within the range of approximately 2.3 to 5.3% by mass, based on the formulas (1) and (2). Visual inspection of the joint confirmed a good bond.

[0071] The corrosion resistance of the joints between the brazing sheets was evaluated using the corrosion test described above. As a result, as shown in the cross-sectional photograph in Figure 4(C), the sacrificial anode function of the sacrificial anode material layer was confirmed, but corrosion of the core material was not observed.

[0072] (Comparative Example 2) In Comparative Example 2, a brazing sheet was used in which the sacrificial anode material layer was an aluminum alloy (Al-4.4%Si-4.0%Zn) of 7.0% by mass of silicon (Si), 4.0% by mass of zinc (Zn), and the remainder aluminum (Al). The brazing sheets were brazed together to form a joint in the same manner as in Comparative Example 1. The brazing temperature was 610°C, and the Si content (concentration) in the sacrificial anode material at this time was within the range of approximately 2.9 to 6.1% by mass, based on the formulas (1) and (2). Visual inspection of the joint confirmed a good bond.

[0073] The corrosion resistance of the joints between the brazing sheets was evaluated using the corrosion test described above. As a result, not only was the sacrificial anode function of the sacrificial anode material layer confirmed, but also the progression of intergranular corrosion in the core material, as shown in the cross-sectional photograph in Figure 4(D).

[0074] Example 3 The brazing sheets according to Example 3 were provided with sacrificial anode material layers having the same composition as in Example 1 on both sides of the core material, and no brazing material layers were used. Except for this, the brazing sheets were brazed together to form a joint in the same manner as in Comparative Example 1. Visual inspection of the joint confirmed good bonding.

[0075] The corrosion resistance of the joints between the brazing sheets was also evaluated using the corrosion test described above. As a result, as shown in the cross-sectional photograph in Figure 5, the sacrificial anode function of the sacrificial anode material layer was confirmed, but corrosion of the core material was not observed.

[0076] The present invention is not limited to the description of the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments or multiple modified examples are also included in the technical scope of the present invention. [Industrial Applicability]

[0077] The present invention can be suitably used not only in the field of brazing sheets used in heat exchangers for air conditioners having a sacrificial anode material layer, but also in a wide range of fields in which the brazing sheets are used for heat exchangers for air conditioners. [Explanation of symbols]

[0078] 10: Brazing sheet 10a:Joint site 10b: Inclined part 11: Heartwood 12: Brazing material layer 13: Sacrificial anode material layer 20: Brazing sheet joint structure 21: Joint 22: Fillet 30: Plate fin laminate 31: End plate 32: Plate fin 33: Header opening 34: Plate fin laminate 35: Plate fin

Claims

1. A brazing sheet used in a heat exchanger of an air conditioning device, comprising a brazing sheet joint structure having a joint portion that is joined together to form a joint and an inclined portion adjacent to the joint portion, the inclination angle of the inclined portion relative to the joint portion being 40° or less, and a temperature during joining of the brazing sheet is set within a range of 580 to 660° C., An aluminum alloy core; a brazing material layer formed of an aluminum alloy brazing material containing silicon (Si) and covering one surface of the core material; A sacrificial anode material layer is coated on the other surface of the core material, and is made of a sacrificial anode material of an aluminum alloy containing zinc (Zn) and silicon (Si), forming the joint portion; Equipped with The content of the zinc in the sacrificial anode material is within a range of 2.5 to 6.0 mass %, The thickness of the sacrificial anode material layer is within the range of 15 to 25 μm; The silicon content X in the sacrificial anode material Si is expressed by the following formula (1), where T is the temperature at the time of bonding. T=660-8×exp(0.3X Si ) ・・・(1) and the value is equal to or less than the value derived from the following formula (2): T=580+55×exp(-0.5(X Si -1.7)) ・・・(2) is adjusted to be equal to or greater than a value derived from Blazing sheet.

2. A brazing sheet used in a heat exchanger of an air conditioning device, comprising a brazing sheet joint structure having a joint portion that is joined together to form a joint and an inclined portion adjacent to the joint portion, the inclination angle of the inclined portion relative to the joint portion being 40° or less, and a temperature during joining of the brazing sheet set within a range of 580 to 660° C., An aluminum alloy core; A sacrificial anode material layer is coated on both surfaces of the core material and is made of an aluminum alloy sacrificial anode material containing zinc (Zn) and silicon (Si), at least one of which forms the joining portion; Equipped with The zinc content in the sacrificial anode material is within the range of 2.5 to 6.0 mass %, The thickness of the sacrificial anode material layer is within the range of 15 to 25 μm; The silicon content X in the sacrificial anode material Si is expressed by the following formula (1), where T is the temperature at the time of bonding. T=660-8×exp(0.3X Si ) ・・・(1) and the value is equal to or less than the value derived from the following formula (2): T=580+55×exp(-0.5(X Si -1.7)) ・・・(2) is adjusted to be equal to or greater than a value derived from Blazing sheet.

3. The temperature T is in the range of 610 to 620° C. The brazing sheet according to claim 1 or 2.

4. The core material is an aluminum alloy of any one of 3000 series, 5000 series, and 6000 series; The sacrificial anode material is a 4000 series aluminum alloy and contains zinc and silicon within the above ranges. The brazing sheet according to claim 1 or 2.

5. The brazing material is a 4000 series aluminum alloy. The brazing sheet according to claim 1 .

6. A heat exchanger for an air conditioner, comprising the brazing sheet according to any one of claims 1 to 5.

7. Characterized in that it is a plate fin laminated type. The heat exchanger for an air conditioner according to claim 6.

Citation Information

Patent Citations

  • Multilayer type aluminum heat exchanger with good corrosion resistance

    JP1996303988A

  • Aluminum alloy composite material for heat exchanger

    JP1999199957A

  • Aluminum alloy-made brazing sheet

    JP2009155673A

  • Aluminum alloy cladding material

    JP2009155679A

  • Aluminum alloy heat exchanger and aluminum alloy heat exchanger manufacturing method