Semiconductor wafer evaluation device and semiconductor wafer manufacturing method

The semiconductor wafer evaluation device uses a liquid metal Schottky electrode to non-destructively evaluate point defects on large wafers by measuring capacitance changes, addressing the limitations of existing destructive methods and enabling efficient mass production.

JP7588495B2Active Publication Date: 2024-11-22CENTRAL RESEARCH INSTITUTE OF ELECTRIC POWER INDUSTRY +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020185713
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-11-22
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

Existing methods for evaluating crystal defects in semiconductor wafers, particularly point defects, are not suitable for large-diameter wafers and are destructive, making them unsuitable for mass production.

Method used

A semiconductor wafer evaluation device using a liquid metal (mercury) Schottky electrode that compensates for parasitic inductance and capacitance, allowing non-destructive evaluation of point defects by intermittently applying voltage and measuring capacitance changes, enabling evaluation of the entire wafer surface.

Benefits of technology

Enables easy and non-destructive evaluation of crystal defects, including point defects, on large semiconductor wafers, facilitating mass production and quality control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588495000001
    Figure 0007588495000001
  • Figure 0007588495000002
    Figure 0007588495000002
  • Figure 0007588495000003
    Figure 0007588495000003
Patent Text Reader

Abstract

To directly evaluate a crystal defect in a semiconductor wafer.SOLUTION: A contactor 24 (mercury that is liquid at room temperature) is used as a shot key electrode to contact a semiconductor wafer 11, and a voltage is intermittently applied from a pulse power supply 25, the state (type, density) of a point defect is evaluated by evaluation means 27 according to the state of the capacitance of the semiconductor wafer 11, and the state (type, density) of a point defect in the plane of the large-diameter semiconductor wafer 11 is directly evaluated using a large table 22.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an apparatus for evaluating crystal defects in a semiconductor wafer, capable of accurately evaluating the state of crystal defects (point defects) within the surface of a semiconductor wafer, and a method for manufacturing a semiconductor wafer. [Background technology]

[0002] In recent years, there has been a demand for higher performance in power semiconductor elements that can withstand high voltages and control large currents, and in addition to conventional silicon (Si) single crystals, the application of new materials (e.g., silicon carbide, gallium nitride, gallium oxide, diamond) has been considered. For example, a technique for evaluating crystal defects in semiconductor elements is known that evaluates element characteristics by passing a current through the element (Patent Document 1).

[0003] Ensuring the performance and reliability of these power semiconductor elements requires inspections to ensure that the manufactured semiconductor elements function as designed, improving the quality of the semiconductor crystals that are the raw materials, detecting crystal defects within the crystals, and properly understanding their characteristics.

[0004] Conventionally, power semiconductor elements are formed using semiconductor wafers with epitaxial layers grown on single crystal substrates, and therefore, it is necessary to check the quality of the semiconductor wafer (epi-wafer) before use. Optical methods are widely used to evaluate the location, type, and density of crystal defects (extended defects) present in semiconductor wafers.

[0005] The doping concentration, which is one of the characteristics of a semiconductor wafer, can be estimated from the capacitance-voltage characteristics by forming a Schottky junction. In addition, a mercury electrode is sometimes used as a simple method that can omit the process of forming a Schottky electrode.

[0006] However, crystal defects (point defects) that affect the characteristics of semiconductor wafers are currently evaluated indirectly from the characteristics (carrier lifetime) that the defect density affects. Existing methods used to evaluate point defect density require cutting out a sample from the semiconductor wafer, depositing a Schottky electrode, and then passing a current through it to evaluate it, which is difficult to apply to large-diameter semiconductor wafers.

[0007] Therefore, the existing evaluation methods are not suitable for evaluation in mass production. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2016-100591 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a semiconductor wafer evaluation device capable of easily evaluating crystal defects over the entire surface of a semiconductor wafer, and a semiconductor wafer manufacturing method using this semiconductor wafer evaluation device. [Means for solving the problem]

[0010] In order to achieve the above object, the semiconductor wafer evaluation device of the present invention according to claim 1 comprises a contactor that brings a metal (Schottky electrode) that is liquid at room temperature into contact with a semiconductor wafer to be evaluated, power supply means that applies a voltage to the contactor via a means for compensating for parasitic inductance and parasitic capacitance, application control means that intermittently controls the application of voltage from the power supply means, and evaluation means that evaluates the state of point defects in the semiconductor wafer based on the state of the capacitance of the semiconductor wafer when the voltage is intermittently applied by the application control means. and a moving means for relatively reciprocating the contactor in a range of a diameter of 150 mm or more in the planar direction of the semiconductor wafer, the moving means being supported so as to be freely reciprocating in a plane and comprising a table on which the semiconductor wafer is placed, and a means for reciprocating the contactor in a direction perpendicular to the table. It is characterized by:

[0011] In the present invention according to claim 1, a contact (mercury) is brought into contact with a semiconductor wafer, a voltage is applied intermittently, and the state (type, density) of point defects is evaluated based on the state of the capacitance of the semiconductor wafer. Since a metal (mercury) that is liquid at room temperature is used as a Schottky electrode, there is no need to partially cut out the semiconductor wafer and deposit a metal electrode, and all point defects in the semiconductor wafer can be directly evaluated, making the evaluation easy. For example, as a means for compensating for parasitic inductance and parasitic capacitance, a means for utilizing offset adjustment that adjusts the error before measurement to zero can be applied. The contact can be moved to any position within the plane of the semiconductor wafer within a range of 150 mm or more in diameter, making it possible to grasp the in-plane distribution of point defects over the entire surface of the semiconductor wafer, even for large semiconductor wafers.

[0012] This makes it possible to easily evaluate crystal defects in the semiconductor wafer, and for example, to indirectly evaluate the carrier lifetime of the semiconductor wafer.

[0013] The semiconductor wafer evaluation device of the present invention according to claim 2 is characterized in that in the semiconductor wafer evaluation device according to claim 1, the metal that is liquid at room temperature is mercury.

[0014] In the present invention according to claim 2, mercury can be used as the Schottky electrode.

[0015] In addition, the semiconductor wafer evaluation device of the present invention according to claim 3 is characterized in that, in the semiconductor wafer evaluation device described in claim 2, the point defect is a defect whose signal peaks near room temperature, and the state of the point defect is the type and density of the point defect.

[0016] According to the present invention as set forth in claim 3, it is possible to evaluate the type and density of point defects whose signals reach a peak near room temperature.

[0019] Also, Claim 4 The semiconductor wafer evaluation device of the present invention relates to Claims 1 to 3In the semiconductor wafer evaluation device described in any one of claims 1 to 5, the application control means has a function of changing an applied voltage, and the evaluation means evaluates the state of point defects at a deep location in the depth direction when the applied voltage is changed.

[0020] Claim 4 In the present invention relating to the above, the state of point defects at a deep location in the depth direction of the semiconductor wafer can be evaluated by changing (increasing) the applied voltage.

[0021] Also, Claim 5 The semiconductor wafer evaluation device of the present invention relates to Claims 1 to 4 The semiconductor wafer evaluation device according to any one of claims 1 to 5, further comprising a light irradiation means for irradiating light equal to or greater than the band gap of the semiconductor wafer, and the evaluation means is characterized in that defects are evaluated by minority carrier transient spectroscopy.

[0022] Claim 5 In the present invention relating to the above, by irradiating light equal to or greater than the band gap with the light irradiating means, defects can be evaluated by minority carrier transient spectroscopy.

[0023] Also, Claim 6 The semiconductor wafer evaluation device of the present invention relates to Claims 1 to 5 In the semiconductor wafer evaluation device according to any one of claims 1 to 5, the semiconductor wafer is a SiC single crystal. Claim 7 The semiconductor wafer evaluation device of the present invention relates to Claim 6 In the semiconductor wafer evaluation device described in the above, the point defects in the SiC single crystal are caused by carbon vacancies. 1 / 2 It is characterized by being a center.

[0024] To achieve the above objectives Claim 8 The method for producing a semiconductor wafer according to the present invention relates to Claims 1 to 7 The present invention is characterized in that a semiconductor wafer is manufactured by using the semiconductor wafer evaluation device described in any one of claims 1 to 5 and adjusting and controlling film formation conditions by a semiconductor manufacturing means based on the obtained point defect information.

[0025] Claim 8 According to the present invention, crystal defects in a semiconductor wafer can be evaluated, and the quality of the semiconductor wafer can be maintained in a desired state while manufacturing the semiconductor wafer.

[0026] Therefore, it becomes possible to easily evaluate crystal defects in a semiconductor wafer and manufacture the semiconductor wafer, and for example, it becomes possible to evaluate the carrier lifetime of a semiconductor wafer and manufacture the semiconductor wafer. Effect of the Invention

[0027] The semiconductor wafer evaluation device of the present invention makes it possible to easily and non-destructively evaluate crystal defects in a semiconductor wafer.

[0028] The method for producing a semiconductor wafer of the present invention makes it possible to easily and non-destructively evaluate crystal defects in a semiconductor wafer and produce the semiconductor wafer. Since the evaluation can be done non-destructively, the product itself can also be inspected. [Brief description of the drawings]

[0029] [Figure 1] 1 is a schematic configuration diagram of a semiconductor wafer evaluation device according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing changes in capacitance over time. [Diagram 3] 1 is a graph showing the attenuation of capacitance at a point defect peak. [Figure 4] 1 is a graph showing the relationship between signal intensity and temperature due to a point defect. [Diagram 5] 1 is a conceptual diagram of a semiconductor manufacturing system having a semiconductor wafer evaluation device according to an embodiment of the present invention. [Figure 6] 4 is a flowchart illustrating an example of a control operation of a semiconductor wafer manufacturing method according to an embodiment of the present invention. [Figure 7] 1 is a graph showing an in-plane distribution of point defect density. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] An apparatus for evaluating a semiconductor wafer according to an embodiment of the present invention will be described with reference to FIGS.

[0031] FIG. 1 shows a schematic configuration of an evaluation device 21 which is an evaluation device for a semiconductor wafer according to an embodiment of the present invention. FIG. 2 shows a graph showing the change in capacitance over time. FIG. 3 shows a point defect peak (for example, Z in a SiC single crystal). 1 / 2 Figure 4 shows a graph of the temperature sweep spectrum, which is the relationship between the signal strength and temperature due to a point defect. 1 / 2 The center is due to a carbon vacancy.

[0032] 1, the evaluation device 21 is provided with a table 22 on which the semiconductor wafer 11 to be evaluated is placed and which is supported so as to be freely movable back and forth within a plane. Also, the evaluation device 21 is provided with a probe means 23 as a contactor which comes into contact with the semiconductor wafer 11 placed on the table 22 and is provided so as to be freely movable back and forth within a plane in a direction perpendicular to the table 22.

[0033] The probe means 23 is structured so that mercury (Schottky electrode), which is liquid at room temperature, is brought into contact with the semiconductor wafer 11 as a contactor 24. The probe means 23 is freely movable to any position within the plane of the semiconductor wafer 11 by the reciprocating movement of the table 22 and itself.

[0034] The probe means 23 can move the contactor to any position within the plane of the semiconductor wafer 11, for example, within the range of the diameter of the semiconductor wafer 11 of 150 mm or more, preferably 300 mm or more. Therefore, even for a large-diameter semiconductor wafer 11, the in-plane distribution of point defects over the entire surface of the semiconductor wafer 11 can be grasped.

[0035] A pulse power supply 25 is provided as a power supply means for applying a voltage to a contact 24 (mercury) of the probe means 23 via a means 10 for compensating for parasitic inductance and parasitic capacitance, and the pulse power supply 25 has a function of intermittently applying the voltage (application control means). The evaluation device 21 is provided with a capacitance meter 26, which measures the capacitance of the semiconductor wafer 11 when a voltage is intermittently applied by the pulse power supply 25.

[0036] The change in capacitance of the semiconductor wafer 11 over time will be described with reference to FIG.

[0037] When a steady-state voltage (3) is applied to the semiconductor wafer 11 (1), electrons are captured in the n-type semiconductor and holes are captured in the p-type semiconductor at the trap level of the point defects. That is, the capacitance of the semiconductor wafer 11 changes from C1 to C2. When the voltage application is stopped, the captured electrons or holes are released and become positively or negatively charged, and the depletion layer expands to cancel the charge (2). Finally, the capacitance of the semiconductor wafer 11 changes to C1 at the steady-state voltage (3).

[0038] By applying a pulse voltage, the capacitance changes over time from C2 (1) through the process of (2) to C1 (3). Based on this change in capacitance over time (the value of the capacitance after a certain time has passed), the trap level and density of point defects can be confirmed. Specifically, when a voltage is applied (1), the density of captured electrons or holes corresponds to the density of point defects, so the change in capacitance is approximately proportional to the density of point defects.

[0039] Therefore, in the above-mentioned evaluation device 21, it becomes possible to easily evaluate the density of point defects, which are crystal defects, of the semiconductor wafer 11.

[0040] As shown in Fig. 3, in a silicon carbide semiconductor wafer, the attenuation state of the capacitance of the point defect (carbon vacancy defect) peak has been confirmed. That is, when the point defect (carbon vacancy defect) is large (shown by a solid line), the signal strength for detecting the capacitance decreases over time, and when the point defect (carbon vacancy defect) is small (shown by a dashed line), the absolute value of the signal strength is lower than when the point defect is large, and the signal strength for detecting the capacitance decreases (attenuation) over time.

[0041] Returning to FIG. 1, the state of the capacitance measured by the capacitance meter 26 is sent to the evaluation means 27. In the evaluation means 27, the state (type, density, etc.) of the point defects of the semiconductor wafer 11 is evaluated based on the state of the capacitance of the semiconductor wafer 11. As an example of the implementation, the amount of change in the signal intensity is obtained by approximating the decay curve of the capacitance with an exponential function (with the Napier number as the base), and the defect density can be calculated using a predetermined doping density value. In addition, the time constant is calculated from the exponent of the exponential function, and the energy depth of the defects in the band gap is evaluated. Specifically, when the trap density is Nt and the doping density is N, Nt is approximately calculated by 2N×|C2-C1|÷C1. It should be noted that Nt may be multiplied by a correction term for correcting an error due to the non-ionized region at the tip of the depletion layer.

[0042] In addition, a point defect is a defect whose signal peaks near room temperature, and as a specific measurement method, a correlation function (correlator) method can be used to apply to defects that can be adjusted to obtain an electrical signal peak near room temperature. For example, the correlation function described in the literature Y. Tokuda, N. Shimizu, and A. Usami, Jpn. J. Appl. Phys. 18, 309 (1979) can be used.

[0043] As shown in Figure 4, for example, when a Ni Schottky electrode is used, by adjusting the measurement conditions (period of the correlation function), it is possible to observe point defects at a peak near room temperature (solid line) rather than at a peak higher than room temperature (dashed line). An example of a point defect near room temperature is the Z 1 / 2 There is a center defect.

[0044] The period of the correlation function that gives the maximum signal strength is determined by evaluating the signal strength while changing the period of the correlation function in advance. Since the optimal value of the period of the correlation function depends on the type of defect (energy depth of the defect), in order to evaluate multiple defects, it is necessary to use appropriate values ​​for each.

[0045] Furthermore, even if the signal intensity deviates slightly from the peak value near room temperature, it is possible to use the relative value to evaluate the uniformity of defect density within the wafer surface, but this will result in underestimating the defect density and may be below the detection limit in areas with low defect density.

[0046] Generally, in comparison with an evaluation method in which temperature sweep is used for the purpose of evaluating unknown defects, the present invention does not require a heavy cooling device or high-temperature heating device for adjusting the wafer temperature; it is sufficient to provide a heater that adjusts the temperature to room temperature or close to room temperature, thereby reducing the cost of the equipment.

[0047] The pulse power supply 25 has a function of changing the applied voltage. By increasing the applied voltage from the pulse power supply 25 (for example, to 100 V), the evaluation means 27 evaluates the state (type, density, etc.) of point defects at a deep location in the depth direction of the semiconductor wafer 11. By performing measurements while changing the applied voltage, a depth profile of the defect state can be obtained.

[0048] The evaluation device 21 may be configured to include a light irradiation means 29 that irradiates light equal to or greater than the band gap of the semiconductor wafer 11. By irradiating light equal to or greater than the band gap from the light irradiation means 29, the evaluation means 27 evaluates defects by minority carrier transient spectroscopy.

[0049] In the case of no light irradiation, the method is applicable to defects that form defect levels in the band gap near the conduction band in n-type semiconductors, and to defects that form defect levels in the band gap near the valence band in p-type semiconductors. On the other hand, in the case of light irradiation, the method is applicable to defects that form defect levels in the band gap near the valence band in n-type semiconductors, and to defects that form defect levels in the band gap near the conduction band in p-type semiconductors.

[0050] For example, it is possible to evaluate the status of B-related defects in n-type SiC crystals at the same time. B defects are formed by B impurities unintentionally introduced during the crystal growth of SiC, and affect the doping density of n-type SiC crystals. Evaluating the density of B-related defects can be applied to wafer quality control. As an example, it can be applied to the density evaluation of point defects called D centers, which are complex defects of B defects and carbon vacancies. It can also be applied to the density evaluation of defects caused not only by B impurities but also by unintentionally introduced transition metal elements.

[0051] The evaluation device 21 configured as described above can bring the contactor 24 (mercury) into contact with the semiconductor wafer 11 to apply a voltage intermittently and evaluate the state of point defects (type, density, etc.: for example, carbon vacancy density in SiC crystal, etc.) based on the state of the capacitance of the semiconductor wafer 11. Because a metal (mercury) that is liquid at room temperature can be used as a Schottky electrode, it is not necessary to cut out a portion of the semiconductor wafer 11 and deposit a metal electrode for evaluation, and it becomes possible to directly evaluate the point defects of all the semiconductor wafers.

[0052] By moving the contact 24 (mercury) to any position relatively within the surface of the semiconductor wafer 11 and applying a voltage intermittently, the distribution of point defects (e.g., distribution of density, etc.) within the surface of the semiconductor wafer 11 can be evaluated.

[0053] An outline of a semiconductor manufacturing system and a specific flow of evaluation of the carrier lifetime of the semiconductor wafer 11 (manufacturing method) will be described with reference to FIGS.

[0054] In the following examples, an example is shown in which a silicon carbide semiconductor is applied as the semiconductor wafer 11, and in this case, the density of carbon vacancies (carbon vacancy density) can be evaluated as the point defects.

[0055] FIG. 5 shows a conceptual configuration of a semiconductor manufacturing system having a semiconductor wafer evaluation device according to one embodiment of the present invention, and FIG. 6 shows a flow chart for explaining an example of a control operation in the control means 12. In FIG.

[0056] 5, a silicon carbide single crystal manufacturing apparatus 1, which is a semiconductor manufacturing means, epitaxially grows a silicon carbide single crystal (SiC single crystal) by, for example, chemical vapor deposition. The silicon carbide single crystal manufacturing apparatus 1 is an apparatus equipped with a source gas supply device, a temperature adjustment device, etc. A seed substrate is placed on a susceptor, and a source gas is supplied to obtain a semiconductor wafer 11 in which a SiC single crystal is grown on the seed substrate.

[0057] In the silicon carbide single crystal manufacturing apparatus 1, the pressure of the manufacturing apparatus, the composition of the raw material gas supplied from the raw material gas supply apparatus (C / Si ratio, the addition ratio of additives such as N2, Al, B, etc.), the gas supply amount, the supply position (supply angle) of the raw material gas, etc. are controlled by the control means 12. The state of the susceptor (rotation speed, position of the rotation axis, etc.) is also adjusted by the control means 12. Furthermore, the control means 12 controls the temperature adjustment means to adjust the temperature to a predetermined high temperature state.

[0058] In silicon carbide single crystal manufacturing apparatus 1, the conditions for growing SiC single crystal are adjusted in accordance with information from evaluation apparatus 21, which is an evaluation apparatus for semiconductor wafers of the present invention. Evaluation apparatus 21 determines the state of point defects (type and density of point defects) in the epitaxial film of semiconductor wafer 11. Then, control means 12 adjusts and controls the conditions for growing SiC single crystal by silicon carbide single crystal manufacturing apparatus 1 (distribution of point defects, etc.) in accordance with the evaluation results in evaluation apparatus 21.

[0059] Furthermore, in the unlikely event that the desired performance is not obtained (the desired conditions are not met) even after adjusting and controlling the conditions for growing the SiC single crystal, control means 12 can determine a malfunction of silicon carbide single crystal manufacturing apparatus 1. This makes it possible to manage the maintenance of silicon carbide single crystal manufacturing apparatus 1, and by identifying malfunctions on the equipment side, it is possible to avoid continuing to manufacture products that do not provide the desired performance.

[0060] Therefore, it becomes possible to evaluate the state of point defects (type and density of point defects) in the epitaxial film of the semiconductor wafer 11 and maintain the quality of the semiconductor wafer 11 in a desired state.

[0061] The control means 12, for example, determines the carbon vacancy density, and controls the composition of the raw material gas so that the determined carbon vacancy density is in a desired state. This makes it possible to control the carbon vacancy density to be maintained in a desired state. Furthermore, when the carbon vacancy density does not reach the desired state even after performing control to maintain the carbon vacancy density in the desired state, the control means 12 can determine that there is a problem with the silicon carbide single crystal manufacturing apparatus 1, and can take necessary measures.

[0062] In addition, the control means 12 determines, for example, point defects related to additives (impurity-related) and controls the flow rate of the source gas (doping gas) so that the determined point defect density becomes a desired state. This makes it possible to maintain the state of the impurity-related point defects in a desired state.

[0063] As described above (see paragraph number

[0047] ), by increasing the applied voltage from the pulse power supply 25 and changing the measurement voltage, the state (type, density, etc.) of point defects at a deep location in the depth direction of the semiconductor wafer 11 is evaluated, and therefore, by linking with the control means, it is possible to control the characteristics of the epitaxial wafer in the depth direction. Also, by devising the process, it is possible to fabricate a multi-layer epitaxial wafer whose characteristics change in the depth direction, and the state in the depth direction can be confirmed in the evaluation device 21.

[0064] An example of a specific control (manufacturing method) will be described with reference to FIG.

[0065] In step S1, point defects (type and density of point defects: point defect density A) in the epitaxial film based on the change in capacitance are read. In step S2, it is determined whether the read point defect density A is equal to or less than a target value B (threshold value). If it is determined in step S2 that the point defect density A is equal to or less than B, it is determined that the point defect density is in a desired state, and the process ends, and the production of the semiconductor wafer 11 continues.

[0066] If it is determined in step S2 that the point defect density A exceeds the target value B, it is determined in step S3 whether the point defect density A is equal to or less than a value C that is higher than the target value B. If it is determined in step S3 that the point defect density A is equal to or less than the value C, the raw material gas supply device is controlled, and in step S4, for example, the amount of raw material gas is changed, and the C / Si ratio of the raw material gas is changed, so that the point defect density A becomes a desired state (equal to or less than the target value B, which is a threshold value).

[0067] On the other hand, if it is determined in step S3 that the point defect density A exceeds the value C, the temperature adjustment means is controlled, and in step S5, for example, the temperature inside the processing chamber is adjusted (temperature change) so that the point defect density A becomes a desired state (below the target value B, which is a threshold value). Note that in step S5, it is also possible to change the gas supply amount, supply angle, etc.

[0068] After the supply state of the source gas is changed in step S4, it is determined in step S6 whether the point defect density A is equal to or lower than the target value B (threshold value). That is, it is determined whether the point defect density A has reached a desired state by changing the supply state of the source gas.

[0069] If it is determined in step S6 that the point defect density A has become equal to or less than the target value B, the point defect density is deemed to be in a desired state, the process ends, and the manufacturing of the semiconductor wafer 11 continues. Therefore, by evaluating the point defect density (e.g., carbon vacancy density) of the semiconductor wafer 11 with the evaluation device 21 and controlling the state of the point defect density with the control means 12, it is possible to manufacture a semiconductor wafer 11 that maintains the desired performance.

[0070] If it is determined in step S6 that the point defect density A exceeds the target value B, it is determined that the point defect density A will not decrease (the desired point defect density will not be obtained) even if the supply conditions of the raw material gas are changed, and the process proceeds to step S7, where it is determined that there is a malfunction in the silicon carbide single crystal manufacturing apparatus 1, and the process ends.

[0071] In other words, if it is determined that the desired point defect density (desired defect state) is not achieved even when the supply conditions of the raw material gas are changed, it is determined that the reason the point defect density is not improved lies not in the conditions but in the silicon carbide single crystal manufacturing apparatus 1 itself. If it is determined in step S7 that there is a malfunction in the silicon carbide single crystal manufacturing apparatus 1, the apparatus can be stopped to interrupt the production of semiconductor wafers 11, and maintenance of the silicon carbide single crystal manufacturing apparatus 1 can be performed. Here, maintenance of the silicon carbide single crystal manufacturing apparatus 1 includes replacement of members constituting the silicon carbide single crystal manufacturing apparatus 1, adjusting the positions of the members, cleaning the silicon carbide single crystal manufacturing apparatus 1, and the like.

[0072] As a result, even if the control means 12 controls the point defect density so as to obtain the desired performance, in the unlikely event that the desired performance is not obtained, it is possible to determine whether there is a problem with the silicon carbide single crystal manufacturing apparatus 1 itself, and to perform maintenance management, etc. of the silicon carbide single crystal manufacturing apparatus 1. Therefore, it is possible to grasp the problem on the silicon carbide single crystal manufacturing apparatus 1 side, and to prevent the continued manufacturing of semiconductor wafers 11 (products) that do not provide the desired performance.

[0073] The semiconductor wafer manufacturing system having the above configuration can maintain the quality of the semiconductor wafer 11 in a desired state, that is, in a desired point defect state (a state in which a desired carrier life can be obtained). Then, the conditions of the silicon carbide single crystal manufacturing apparatus 1 can be controlled so that the semiconductor wafer 11 in the desired point defect state can be manufactured, and the semiconductor wafer 11 can be manufactured in a stable state. Furthermore, it is possible to grasp any defects on the silicon carbide single crystal manufacturing apparatus 1 side, and to avoid continuing to manufacture semiconductor wafers 11 (products) that do not provide the desired performance.

[0074] The distribution of point defect density can be evaluated to evaluate point defects in semiconductor wafers. Figure 7 shows the in-plane distribution of point defect density.

[0075] By checking the density within the plane of the semiconductor wafer 11 (in the horizontal direction: indicated by → in the figure), as shown in Fig. 7, as one example, it is possible to evaluate the relative value (%) of the density of point defects within the plane of the semiconductor wafer 11. That is, it is possible to evaluate the variation of point defects within the plane of the semiconductor wafer 11. In the example shown in Fig. 7, it can be confirmed that the relative value (%) of the density of point defects within the plane of the semiconductor wafer 11 falls within the range of ±S1.

[0076] In addition to controlling the absolute amount by setting a defect density threshold value, the variation in point defects within the surface of the semiconductor wafer 11 can be evaluated to control the variation in defect density within the surface of the semiconductor wafer 11.

[0077] The above-mentioned evaluation device 21 evaluates the in-plane point defect density of the semiconductor wafer 11 to judge the malfunction of the silicon carbide single crystal production apparatus 1, but it is also possible to evaluate the in-plane distribution of point defects to judge the malfunction of the silicon carbide single crystal production apparatus 1. In this case, if the in-plane variation of point defects in the semiconductor wafer 11 does not fall within a threshold range, the gas supply angle can be adjusted or a maintenance decision can be made to bring the in-plane variation of point defects in the semiconductor wafer 11 within the threshold range.

[0078] The semiconductor wafer evaluation device (evaluation device 21) of the present invention described above brings a contactor 24 (mercury) into contact with the semiconductor wafer 11, applies a voltage intermittently, and evaluates the state (type, density) of point defects based on the state of the capacitance of the semiconductor wafer 11, thereby making it possible to use a metal (mercury) that is liquid at room temperature as a Schottky electrode.

[0079] Therefore, it is possible to directly evaluate point defects in all semiconductor wafers without the need to cut out a part of the semiconductor wafer 11 and deposit metal electrodes for evaluation. Therefore, it is possible to easily evaluate crystal defects in semiconductor wafers and manufacture semiconductor wafers. [Industrial Applicability]

[0080] The present invention can be utilized in industrial fields such as semiconductor wafer evaluation devices and semiconductor wafer manufacturing methods. [Explanation of symbols]

[0081] 1. Silicon carbide single crystal manufacturing equipment 10 Means for compensating for parasitic inductance and capacitance 11 Semiconductor wafers 12 Control Means 21 Evaluation equipment 22 Tables 23 Probe means 24 Contact 25 Pulse power supply 26 Capacity meter 27 Evaluation methods 29 Light irradiation means

Claims

1. A contactor that brings a metal (Schottky electrode) that is liquid at room temperature into contact with a semiconductor wafer to be evaluated; power supply means for applying a voltage to the contacts via means for compensating for parasitic inductance and parasitic capacitance; an application control means for intermittently controlling the application of a voltage from the power supply means; An evaluation means for evaluating a state of point defects in the semiconductor wafer based on a state of the capacitance of the semiconductor wafer when a voltage is intermittently applied by the application control means; a moving means for relatively reciprocating the contactor in a range of a diameter of 150 mm or more in a planar direction of the semiconductor wafer, The moving means is a table supported so as to be freely reciprocable within a plane and on which the semiconductor wafer is placed; and a means for reciprocating the contact in a direction perpendicular to the table. A semiconductor wafer evaluation device comprising:

2. The semiconductor wafer evaluation device according to claim 1, The metal that is liquid at room temperature is mercury. A semiconductor wafer evaluation device comprising:

3. The semiconductor wafer evaluation device according to claim 2, Point defects are defects whose signal peaks around room temperature. The state of point defects is determined by the type and density of the point defects. A semiconductor wafer evaluation device comprising:

4. In the semiconductor wafer evaluation device according to any one of claims 1 to 3, The application control means has a function of changing an applied voltage, The evaluation means includes: When the applied voltage is increased, the state of point defects at deep locations in the depth direction is evaluated. A semiconductor wafer evaluation device comprising:

5. A semiconductor wafer evaluation device according to any one of claims 1 to 4, A light irradiation means is provided for irradiating the semiconductor wafer with light having a band gap or greater, In the evaluation means, Defects characterized by minority carrier transient spectroscopy A semiconductor wafer evaluation device comprising:

6. The semiconductor wafer evaluation device according to any one of claims 1 to 5, The semiconductor wafer is a SiC single crystal. A semiconductor wafer evaluation device comprising:

7. The semiconductor wafer evaluation device according to claim 6, The point defects in the SiC single crystal are caused by carbon vacancies. 1/2 Center A semiconductor wafer evaluation device comprising:

8. A method for manufacturing a semiconductor wafer, characterized in that a semiconductor wafer is manufactured by using a semiconductor wafer evaluation device described in any one of claims 1 to 7, and adjusting and controlling the conditions of film formation by a semiconductor manufacturing means based on the obtained point defect information.

Citation Information

Patent Citations

  • Start position controller in transfer type electrophotographic copier

    JP1979015751A

  • Manufacturing method of silicon carbide semiconductor element

    JP2007318031A

  • Method for manufacturing silicon carbide semiconductor epitaxial substrate

    JP2008053343A

  • Band gap electronic physical property measuring method of wide gap semiconductor and band gap electronic physical property measuring apparatus for wide gap semiconductor

    JP2014027193A

  • Method for manufacturing silicon carbide epitaxial substrate, silicon carbide epitaxial substrate and silicon carbide semiconductor device

    JP2016063190A