Modulation of film properties by optimizing plasma coupling materials.
By employing edge rings with specific materials in substrate processing chambers, the film properties of hardmask films are modulated independently of RF power, addressing etch selectivity and deposition rate challenges in semiconductor manufacturing.
Patent Information
- Application Number
- JP2021577978
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-01
- Filing Date
- 2020-06-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-06-26
AI Technical Summary
Current hardmask materials in semiconductor manufacturing face challenges with etch selectivity and deposition rates as critical dimensions decrease, necessitating increased RF power which affects film properties like stress and modulus, leading to insufficient resist layers and pattern transfer issues.
The use of edge rings made of materials like quartz, silicone, cross-linked polystyrene, and Al2O3 in substrate processing chambers to modulate hardmask film properties without increasing RF power, allowing independent adjustment of film stress and modulus by changing the edge ring material.
This approach enables deposition of hardmask films with desired properties, such as high modulus and low stress, without altering RF power, improving pattern transfer accuracy and reducing substrate warpage.
Smart Images

Figure 0007588609000001 
Figure 0007588609000002 
Figure 0007588609000003
Abstract
Description
[Technical field]
[0001]
[0001] Embodiments of the present disclosure relate generally to apparatus and methods used in the manufacture of semiconductor devices. More specifically, embodiments of the present disclosure relate to substrate processing chambers and components thereof for forming semiconductor devices. [Background technology]
[0002]
[0002] Integrated circuits have evolved into complex devices that may contain millions of transistors, capacitors, and resistors on a single chip. Evolution in chip design is accompanied by a continual trend toward faster and denser circuits. The demand for faster and denser circuits places demands on the materials used to fabricate the integrated circuits. In particular, as the dimensions of integrated circuit components shrink to the sub-micron scale, there is a trend toward using conductive materials with low resistivity and insulating materials with low dielectric constant to obtain adequate electrical performance from the components.
[0003]
[0003] The demand for higher density of integrated circuits also places demands on the process sequences used to manufacture integrated circuit components. For example, in a process sequence using conventional photolithography techniques, a layer of energy sensitive resist is formed on a stack of material layers disposed on a substrate. The energy sensitive resist layer is exposed to an image of a pattern to form a photoresist mask. The mask pattern is then transferred to one or more material layers of the stack using an etching process. A chemical etchant used in the etching process is selected to have a higher etch selectivity for the material layers of the stack than the energy sensitive resist mask. That is, the chemical etchant etches the one or more layers of the material stack at a much faster rate than the energy sensitive resist. The higher etch selectivity for the one or more material layers of the stack compared to the resist prevents the energy sensitive resist from being consumed before the pattern transfer is complete.
[0004]
[0004] As pattern dimensions become smaller, the thickness of the energy sensitive resist becomes smaller accordingly to control the pattern resolution. However, such a thin resist layer may be insufficient to mask the underlying material layer due to the effect of chemical etchants during the pattern transfer process. Therefore, to facilitate the pattern transfer, an intermediate layer called a hard mask (such as silicon oxynitride, silicon carbide, or carbon film) is often used between the energy sensitive resist layer and the underlying material layer because it has a high resistance to chemical etchants. Hard mask materials that combine high etch selectivity with high deposition rates are often used. As the critical dimensions (CD) become smaller, current hard mask materials often do not have the desired etch selectivity to the underlying material (e.g., oxides and nitrides) and are difficult to deposit. Furthermore, modulating the properties of the hard mask requires increasing the RF power applied to the chamber, which often improves one film property, such as film modulus, while degrading another property, such as film stress.
[0005]
[0005] Accordingly, there is a need in the art for improved methods and apparatus for manufacturing semiconductor devices. Summary of the Invention
[0006]
[0006] The embodiments of the present disclosure generally relate to a substrate processing chamber for forming semiconductor devices, and components thereof. The processing chamber includes a substrate support having an edge ring disposed around the substrate support. The edge ring comprises a material selected from the group consisting of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyetheretherketone, Al2O3, and AlN. The edge ring material is selected to modulate the properties of a hardmask film deposited on a substrate in the processing chamber. Thus, a hardmask film having desired film properties can be deposited in the processing chamber without increasing the RF power to the chamber.
[0007] In one embodiment, a method of modulating properties of one or more hardmask films includes depositing a first hardmask film on a first substrate and processing the first substrate with a first RF power, measuring one or more film properties of the first hardmask film, removing the first substrate from a substrate support, replacing a first edge ring of the substrate support with a second edge ring, the second edge ring comprising a material selected from the group consisting of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyetheretherketone, Al2O3, and AlN, placing a second substrate on the substrate support, depositing a second hardmask film on the second substrate and processing the second substrate with the first RF power, and measuring one or more film properties of the second hardmask film.
[0008]
[0008] In another embodiment, a method of modulating properties of one or more hardmask films includes depositing a first hardmask film on a first substrate and treating the first substrate with a first RF power; measuring one or more film properties of the first hardmask film, the one or more film properties including elastic modulus and stress; removing the first substrate from a substrate support; and replacing a first edge ring of the substrate support with a second edge ring, the first edge ring being aligned with a second edge ring of the second edge ring. The method includes replacing a first edge ring of a substrate support with a second edge ring comprising a first material different from the first material; disposing a second substrate on the substrate support; depositing a second hardmask film on the second substrate and processing the second substrate with a first RF power, where the second material of the second edge ring is selected to adjust at least one film property of the second hardmask film based on the measured one or more film properties of the first hardmask film.
[0009]
[0009] In yet another embodiment, a non-transitory computer readable medium has instructions configured to cause a system to deposit a first hardmask film on a first substrate and process the first substrate with a first RF power, measure one or more film properties of the first hardmask film, remove the first substrate from a substrate support, replace a first edge ring of the substrate support with a second edge ring, the second edge ring comprising a material selected from the group consisting of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyether ether ketone, Al2O3, and AlN, place a second substrate on the substrate support, deposit a second hardmask film on the second substrate and process the second substrate with the first RF power, and measure one or more film properties of the second hardmask film.
[0010]
[0010] In order that the above-mentioned features of the present disclosure may be understood in detail, the present disclosure summarized above will now be more particularly described with reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings merely depict exemplary embodiments, and therefore should not be considered as limiting the scope thereof, as other equally effective embodiments may be permitted. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional side view of an exemplary processing chamber. [Diagram 2] 2 is a schematic side view of the processing chamber of FIG. 1 rotated approximately 90 degrees. [Diagram 3] 1 is a schematic cross-sectional view of a processing chamber. [Figure 4] 2 is a schematic cross-sectional view of one embodiment of a substrate support; [Diagram 5] FIG. 1 illustrates a method of using an edge ring to modulate the properties of a carbon hardmask film, according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012]
[0016] To facilitate understanding, wherever possible, the same reference numerals have been used to designate identical elements common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.
[0013]
[0017] The embodiments of the present disclosure generally relate to a substrate processing chamber and components thereof for forming semiconductor devices. The processing chamber includes a substrate support having an edge ring disposed around the substrate support. The edge ring includes a material selected from the group consisting of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyetheretherketone, Al2O3, and AlN. The edge ring material is selected to modulate the properties of a hard mask film deposited on a substrate in the processing chamber. Thus, a hard mask film having desired film properties can be deposited in the processing chamber without increasing the RF power to the chamber.
[0014]
[0018] Embodiments of the present disclosure relate to substrate processing chambers utilized for substrate processing in the manufacture of electronic devices. Substrate processing includes deposition processes, etching processes, and other low pressure, plasma, and thermal processes used to manufacture electronic devices on substrates. An example of a processing chamber and / or system that may be adapted to benefit from exemplary aspects of the present disclosure is the Producer® APF™ PECVD system available from Applied Materials, Inc., Santa Clara, Calif. It is contemplated that other processing chambers and / or processing platforms, including those from other manufacturers, may be adapted to benefit from aspects of the present disclosure.
[0015]
[0019] The embodiments of the deposition chamber disclosed herein may be used in the fabrication of memory devices, particularly in the deposition of hard masks used during the fabrication of memory devices. Current memory devices can retain stored data for very long periods of time without the application of voltage, and the read speed of such memory devices is relatively high. It is also relatively easy to erase stored data and rewrite data to memory devices. For this reason, memory devices are widely used in microcomputers, automatic control systems, and the like. To increase the bit density of memory devices and reduce the cost per bit, three-dimensional NAND (three-dimensional not AND) memory devices have been developed. In addition, memory devices such as dynamic random access memory (DRAM), expanded memory (EM), and resistive random access memory (ReRAM), as well as advanced hard mask materials for forming them, have also been developed, further promoting the development of the semiconductor industry.
[0016]
[0020] In 3D NAND technology, vertical gate 3D memory cells are being considered to reduce costs as the number of memory cell layers increases. Although stacks of oxide / silicon layers and oxide / nitride layers are useful due to their advantages in material integration, the thickness of the layers becomes a limiting factor as the number of memory cell layers increases. Therefore, attention has been focused on reducing the thickness of the memory cell layers, but issues such as oxide quality (i.e., breakdown voltage), silicon resistivity, and high aspect ratio etching cannot be solved by reducing the layer thickness.
[0017]
[0021] 1 is a schematic cross-sectional side view of an exemplary processing chamber 100 suitable for performing a deposition process. In one embodiment, the processing chamber 100 can be configured to deposit highly patterned films on a substrate, such as a hardmask film, e.g., an amorphous carbon hardmask film.
[0018]
[0022] The processing chamber 100 includes a lid assembly 105, a spacer 110 disposed on a chamber body 192, a substrate support 115, a system controller 101, and a variable pressure system 120. The lid assembly 105 includes a lid plate 125 and a heat exchanger 130. In the illustrated embodiment, the lid assembly 105 also includes a showerhead 135. However, in other embodiments, the lid assembly 105 includes a recessed or dome-shaped gas introduction plate.
[0019]
[0023] The lid assembly 105 is coupled to a process gas source 140. The process gas source 140 includes precursor gases for forming a film on a substrate 145 supported by the substrate support 115. By way of example, the process gas source 140 includes precursor gases such as a carbon-containing gas, a hydrogen-containing gas, helium, among others. In a specific example, the carbon-containing gas includes acetylene (C2H2). The process gas source 140 delivers precursor gases to a plenum 190 disposed in the lid assembly 105. The lid assembly 105 includes one or more channels for directing precursor gases from the process gas source 140 to the plenum 190. The precursor gases flow from the plenum through a showerhead 135 to the processing region 160.
[0020]
[0024] The lid assembly 105 is also coupled to an optional remote plasma source 150. The remote plasma source 150 is coupled to a cleaning gas source 155 for supplying a cleaning gas to a processing region 160 formed within the spacer 110 between the lid assembly 105 and the substrate 145. In one embodiment, the cleaning gas is supplied through a central conduit 191 formed axially through the lid assembly 105. In another embodiment, the cleaning gas is supplied through the same channels that conduct the precursor gases. Exemplary cleaning gases include oxygen-containing gases, such as oxygen and / or ozone, and fluorine-containing gases, such as NF3, or combinations thereof.
[0021]
[0025] In addition to or as an alternative to the remote plasma source 150, the lid assembly 105 is also coupled to a first or upper radio frequency (RF) power source 165. The first RF power source 165 facilitates the maintenance or generation of a plasma, such as a plasma generated from a cleaning gas. In one embodiment, the remote plasma source 150 is omitted and the cleaning gas is ionized into a plasma in situ via the first RF power source 165. The substrate support 115 is coupled to a second or lower RF power source 170. The first RF power source 165 may be a high frequency RF power source (e.g., about 13.56 MHz or about 40 MHz) and the second RF power source 170 may be a low frequency RF power source (e.g., about 2 MHz or about 13.56 MHz). It should be noted that other frequencies are also contemplated. In some implementations, the second RF power source 170 is a mixed frequency RF power source, providing both high frequency and low frequency power. The use of a dual frequency RF power source improves film deposition, particularly the use of the second RF power source 170. When using a second RF power source 170 that provides dual frequency power, such as 13.56 MHz and 40 MHz, the 13.56 MHz frequency improves the injection of species into the deposited film, and the 40 MHz frequency increases the ionization and deposition rate of the film.
[0022]
[0026] One or both of the first RF power source 165 and the second RF power source 170 are utilized in generating or maintaining a plasma in the processing region 160. For example, the second RF power source 170 may be utilized during a deposition process and the first RF power source 165 may be utilized during a cleaning process (alone or in conjunction with the remote plasma source 150). In some deposition processes, the first RF power source 165 is used in conjunction with the second RF power source 170. During a deposition process, one or both of the first RF power source 165 and the second RF power source 170 provide power of about 4 kilowatts (kW) to about 9 kW, e.g., about 4 kW to about 6 kW, at the processing region 160 to promote ionization of the precursor gases.
[0023]
[0027] The substrate support 115 is coupled to an actuator 175 that provides its movement in the Z direction. The substrate support 115 is also coupled to an equipment cable 178 that allows vertical movement of the substrate support 115 while maintaining communication with the second RF power source 170 and other power and fluid connections. A spacer 110 is disposed in the chamber body 192. The height of the spacer 110 allows vertical movement of the substrate support 115 within the processing region 160. In one example, the substrate support 115 is movable from a first distance 180A to a second distance 180B relative to the lid assembly 105 (e.g., relative to the underside of the showerhead 135). In some embodiments, the first distance 180A is about 14 inches and the second distance is about 11.2 inches. In contrast to conventional plasma enhanced chemical vapor deposition (PECVD) processes, the spacer 110 significantly increases the distance (and therefore the volume between) between the substrate support 115 and the lid assembly 105. Increasing the distance between the substrate support 115 and the lid assembly 105 reduces the bombardment of ionized species in the process region 160, resulting in the deposition of a film with less tensile stress. Films deposited with less tensile stress promote improved flatness (e.g., less warping) of the substrate on which the film is formed. Reduced substrate warping improves the accuracy of downstream patterning steps.
[0024]
[0028] The variable pressure system 120 includes a first pump 182 and a second pump 184. The first pump 182 is a roughing pump that may be utilized during the cleaning process and / or the substrate transfer process. The roughing pump is generally configured to drive a higher volumetric flow rate and / or operate at a relatively high (albeit still sub-atmospheric) pressure. In one example, the first pump maintains a pressure in the processing chamber during the cleaning process of about 300 mtorr to about 800 mtorr, such as about 400 torr to about 6 mtorr. The utilization of the roughing pump during the cleaning process facilitates a relatively high pressure and / or volumetric flow rate of the cleaning gas (compared to the deposition process). The relatively high pressure and / or volumetric flow rate during the cleaning process improves cleaning of the chamber surfaces.
[0025]
[0029] The second pump 184 may be a turbo pump utilized during the deposition process. Turbo pumps are generally configured to operate at relatively low volumetric flow rates and / or pressures. For example, a tubular molecular pump is configured to maintain the processing region 160 of the process chamber at a pressure of less than about 10 mtorr, such as about 5 mtorr or less, during the deposition process. The reduced pressure in the processing region 160 maintained during deposition may result in reduced tensile stress and / or increased sp when depositing a carbon-based hardmask. 2 -sp 3 In this manner, the process chamber 100 is configured to utilize both relatively low pressures to improve deposition and relatively high pressures to improve cleaning.
[0026]
[0030] In some embodiments, both the first pump 182 and the second pump 184 are utilized during the deposition process. A valve 186 is utilized to control the conductance path to one or both of the first pump 182 and the second pump 184. The valve 186 also provides symmetric pumping from the processing region 160.
[0027]
[0031] The processing chamber 100 also includes a substrate transfer port 185. The substrate transfer port 185 is selectively sealed by an inner door 186A and an outer door 186B. The doors 186A and 186B are each coupled to an actuator 188. The doors 186A and 186B facilitate vacuum sealing of the processing region 160. The doors 186A and 186B also provide symmetrical RF application and / or plasma symmetry within the processing region 160. In one embodiment, at least the door 186A is formed of a material that facilitates the conduction of RF power, such as stainless steel, aluminum, or alloys thereof.
[0028]
[0032] The system controller 101 controls the activities and operating parameters of automated components in the processing system 100. The system controller 101 may be independently coupled to one or more components of the processing system 100, such as, for example, the actuators 175, 188, the first RF power source 165, the second RF power source 170, and the process gas source 140. The system controller 101 is a general-purpose computer used to control one or more components in the processing system 100. The system controller 101 is generally designed to facilitate the control and automation of one or more process sequences disclosed herein, and typically includes a central processing unit (CPU) (not shown), memory (not shown), and supporting circuits (or I / O) (not shown). Software instructions and data may be encoded and stored in the memory (e.g., a non-transitory computer readable medium) for instructing the CPU. Programs (or computer instructions) readable by a processing unit in the system controller determine which tasks are executable in the processing system. For example, the non-transitory computer readable medium includes a program configured to perform one or more of the methods described herein when executed by a processing unit. Preferably, the program includes code for performing tasks associated with monitoring, executing, and controlling the movement, support, and / or positioning of a substrate, as well as the various process recipe tasks being executed and the process recipe steps of the various processing modules.
[0029]
[0033] Figure 2 is a schematic side view rotated approximately 90 degrees of the processing chamber 100 of Figure 1. Figure 2 shows details of the spacer 110. The spacer 110 includes a liner 200 that surrounds the processing region 160.
[0030]
[0034] The spacer 110 also includes a number of heater elements 205 embedded in or in thermal communication with the body of the spacer 110. The heater elements 205 are utilized to maintain the temperature of the spacer 110 at or above about 80° C. Each heater element 205 may be a cartridge heater.
[0031]
[0035] The liner 200 includes an upper or first portion 210 and a lower or second portion 215. The first portion 210 has a thickness that is greater than the thickness of the second portion 215. The varied thickness provides a number of advantages. One advantage of the reduced thickness of the second portion 215 is that the space between the substrate support 115 and the inner wall of the spacer 110 is increased, thus increasing the vacuum conductance. Another advantage of the reduced thickness of the second portion 215 is a change in the thermal mass of the liner 200. Thus, the portion of the liner 200 adjacent to or at the first portion 210 is maintained at a higher temperature than the portion of the liner 200 adjacent to or at the second portion 215. The liner 200 is formed from one or more materials including aluminum, titanium, or alloys thereof. In one embodiment, the liner extends from the lid assembly 105, past the substrate support 115, and adjacent to the bottom of the processing chamber 100. In such an example, the liner 200 may not contact the bottom of the chamber 100, but instead be spaced therefrom. Additionally, while the liner 200 is shown in Figure 2 as a single piece, it is contemplated that multiple liners may be utilized to line the interior surfaces of the process chamber. For example, a first (or upper) liner may be utilized to line the spacer 110, while a second (or lower) liner may be utilized to line the interior surface of the chamber body (shown in Figure 1).
[0032]
[0036] The spacer 110 also includes a magnet assembly 220. The magnet assembly 220 includes a plurality of magnets 225 that surround the spacer 110. Each magnet 225 is coupled to an actuator 230. The actuator 230 rotates the magnets 225 around the spacer 110 outside the liner 200 about a longitudinal axis 235 of the processing chamber 100. The actuator 230 is also adapted to move the magnets 225 vertically (Z direction) along the longitudinal axis 235. Each magnet 225 may be a permanent magnet, or an electromagnet, or a combination thereof. Each magnet 225 is positioned within a cavity 240 formed in a sidewall 242 of the spacer 110. In one embodiment, the magnets are positioned below the heater element 205.
[0033]
[0037] In some embodiments, about half of the magnets 225 are oriented with their north poles facing the substrate support 115 (substantially parallel to the longitudinal axis 235). The other portion of the magnets 225 are oriented with their south poles facing the substrate support 115 (substantially parallel to the longitudinal axis 235). In one example, the magnets 225 are arranged in a circle centered on the spacer 110 (in-plane view). The magnets 225 are separated into a first portion or first semicircle and a second portion or second semicircle. The magnets 225 of the first semicircle are each oriented with their north poles facing the substrate support 115 (substantially parallel to the longitudinal axis 235). The magnets 225 of the second semicircle are each oriented with their south poles facing the substrate support 115 (substantially parallel to the longitudinal axis 235). In such examples, the magnets 225 may rotate during deposition or the magnets may remain stationary.
[0034]
[0038] The magnet assembly 220 aids in confining and / or tuning the plasma in the processing region 160. In one embodiment, the magnet assembly 220 also forms a cavity resonator 245 in the processing region 160 during the deposition process. The cavity resonator 245 provides a magnetic flux that extends the plasma sheath vertically downward (Z direction) towards the substrate (not shown in FIG. 2). The magnet assembly 220 provides a B-field in the X / Y plane as well as in the Z direction. The magnet assembly 220 also allows tuning of the plasma in the processing region 160 and / or the cavity resonator 245. The eddy currents of the plasma can be monitored to provide a metric for adjusting one or both of the position of the magnet 225 and the rotational speed of the magnet 225. Additionally or alternatively, measurements of a film previously deposited on the substrate can be performed and the results can be used to vary the position and / or rotational speed of the magnet 225. In this manner, the cavity resonator 245 and the magnet assembly 220 provide improved uniformity of the film on the substrate.
[0035]
[0039] 3 is a schematic cross-sectional view of a process chamber 100 including a cathode assembly 300 including a substrate support 115. The process chamber 100 includes an opening 285 for inserting and removing a substrate, such as a wafer, into and from the process chamber 100. The cathode assembly 300 is coupled to an actuator 305 (similar to the actuator 175 shown in FIG. 1) that moves the cathode assembly 300 vertically in the Z direction. As shown in FIG. 3, the cathode assembly 300 is at its lowest position (e.g., a first distance 180A) relative to the lid assembly 105. The position of the cathode assembly 300 can be adjusted for the deposition process to achieve optimal film quality.
[0036]
[0040] The cathode assembly 300 also includes an equipment interface 310. The equipment interface 310 provides connections for RF power as well as other electrical and fluid connections. The equipment interface 310 is coupled to the substrate support 115 via an equipment cable 178. Other connections include a power supply 315, a coolant source 320, and a gas supply 325.
[0037]
[0041] The power supply 315 is utilized to provide power to the electrostatic chuck 330 that is part of the substrate support 115. The power supply 315 may be a direct current (DC) power supply. Dechucking is facilitated by a controller (not shown) that evacuates the electrostatic chuck 330. Additionally, the equipment cable 178 is coupled to the power supply 170 through an optional matching network to facilitate the process within the processing chamber 100. In one embodiment, the equipment cable 178 facilitates the transfer of RF power during the PECVD process. Due to the relatively large area provided by the spacer 110 and the pressure at which the processing chamber 100 is operated during the PECVD process, higher power levels (compared to conventional PECVD processes) are used to establish and maintain the plasma. For example, the equipment cable may carry about 4 kW to about 9 kW of power at 110 amps during the PECVD process. When utilizing the magnets 225 in a tuned configuration, it is believed that the amperage may be reduced to a range of about 78 amps to about 80 amps without degradation of film quality.
[0038]
[0042] The coolant source 320 includes a coolant that cools the substrate support 115. For example, coolant from the coolant source 320 is flowed to the substrate support 115 to maintain a temperature of the electrostatic chuck 330 (and / or a substrate positioned thereon) between about 0° C. and about −10° C. The coolant includes a heat transfer fluid, such as a heat transfer fluid sold under the trade name GALDEN®.
[0039]
[0043] A gas supply 325 supplies a fluid to the space below the electrostatic chuck 330 to prevent condensation. The fluid may be clean dry air, nitrogen (N2), helium (He), or other suitable gas. The fluid supplied to the space below the electrostatic chuck reduces condensation on the electrostatic chuck, including its underside.
[0040]
[0044] One or more of the combinations of the substrate support 115, heated spacer 110 (using heater element 205 shown in FIG. 2), and cooling of the cavity resonator 235 described herein provide many advantages. Lower substrate temperatures not only reduce substrate warping, but also increase deposition rates. Maintaining the temperature of the spacer 110 and / or liner 200 below about 100° C. promotes more efficient cleaning and / or minimizes particle deposition on the liner 200. One or more cooling channels may be formed in the spacer 110 to facilitate cooling of the liner 200.
[0041]
[0045] 3 is a support structure 335. Although only one is shown, the support structure 335 has three vacuum channels 340 formed therein. The vacuum channels 340 are coupled to the variable pressure system 120. The vacuum channels 340 facilitate symmetric pumping out of the processing region 160.
[0042]
[0046] The cathode assembly 300 is coupled to a base ring 350 and an optional mounting plate 345. Fasteners 355 extend from the base ring 350 to secure the substrate support 115 thereon.
[0043]
[0047] 4 is a schematic cross-sectional view of one embodiment of the substrate support 115. As described above, the substrate support 115 includes an electrostatic chuck 330. The electrostatic chuck 330 includes a puck 400. The puck 400 includes one or more electrodes 405 embedded therein. A first one of the one or more electrodes 405 is utilized as a chucking electrode and a second one of the one or more electrodes 405 is utilized as an RF bias electrode. The puck 400 is formed from a dielectric material, such as a ceramic material, e.g., aluminum nitride (AlN).
[0044]
[0048] The puck 400 is supported by a dielectric plate 410 and a base plate 415. The dielectric plate 410 may be formed of an electrically insulating material, such as quartz, or a thermoplastic material, such as a high performance plastic sold under the trade name REXOLITE®. The base plate 415 may be made of a metallic material, such as aluminum. During operation, the base plate 415 is tied to ground or electrically floating while the puck 400 is in an RF powered state. The ends of the facilities cables 178 are shown in openings formed in the puck 400, the dielectric plate 410, and the base plate 415. Power for the electrodes of the puck 400, as well as fluids from a gas supply 325 (shown in FIG. 3) to the substrate support 115 are provided by the facilities cables 178.
[0045]
[0049] Each of the puck 400, the dielectric plate 410, and the base plate 415 includes a respective axially aligned opening formed therein or therethrough to accommodate the equipment cable 178. The puck 400 includes an opening 495 shaped to engage the equipment cable 178. For example, the opening 495 may be configured as a female socket for receiving the equipment cable 178. The dielectric plate 410 includes an opening 496 axially aligned with the opening 495. The opening 496 includes an upper portion 496a having a diameter approximately equal to the diameter of the opening 495, a middle portion 496b having a diameter larger than the diameter of the upper portion, and a lower portion 496c having a diameter larger than the diameter of the middle portion 496b. The base plate 415 includes an opening 497 having an upper portion 497a having a first diameter and a lower portion 497b having a second diameter smaller than the first diameter. The multiple diameters of openings 496, 496, and 497 facilitate securing facility cable 178 thereto.
[0046]
[0050] The pack 400 includes a plurality of fluid channels 430 formed therein. Each fluid channel 430 is in fluid communication with an inlet channel 432. The inlet channels 432 are fluidly coupled to an inlet conduit 434. The inlet conduit 434 is coupled to the coolant source 320. Each of the fluid channels 430 and the inlet channels 432 are sealed by a cap plate 436. The cap plate 436 may be made of the same material as the pack 400 or aluminum, and may be welded or otherwise coupled to the pack 400 to seal the fluid channels 430 and the inlet conduits 434. Although not shown, an outlet conduit similar to the inlet conduit 434 is provided in the substrate support 115 to allow the cooling fluid to be recirculated therein.
[0047]
[0051] A portion of the inlet conduit 434 is formed by a tubular member 438. The tubular member 438 is formed from a dielectric material, such as a ceramic material. Seals 440 are provided at the ends of the tubular member 438 adjacent the cap plate 436 and the base plate 415. The tubular member 438 prevents arcing that may be caused by the cooling fluid flowing therethrough. The tubular member 438 may also thermally insulate the dielectric plate 410 from the relatively cool cooling fluid flowing therethrough to prevent cracking of the dielectric plate 410.
[0048]
[0052] The substrate support 115 also includes a number of lift pins 442 (only one shown). Each lift pin 442 is movably disposed in a dielectric bushing 444. Each lift pin 442 may be formed of a ceramic material such as AlN, sapphire, quartz, etc. A dielectric bushing 444 is disposed in or through each of the puck 400, the dielectric plate 410, and the base plate 415. The dielectric bushing 444 is made of a polymer material such as a polytetrafluoroethylene (PTFE) material. The dielectric bushing 444 includes an opening 446 along its length through which the lift pin 442 is guided. The opening 446 is sized slightly larger than the size (diameter) of the lift pin 442 so that a conductance path is formed in the dielectric bushing 444. For example, the opening 446 is coupled to the variable pressure system 120 so that a vacuum conductance is provided between the processing region 160 and the variable pressure system 120 through the dielectric bushing 444. The conductance path provided by the openings 446 prevents arcing of the lift pins. The dielectric bushing 444 includes a number of variable diameter steps 448. The steps 448 reduce arcing between the puck 400 and the base plate 415 by increasing the length of the path through which electricity can travel and by introducing angled turns along the path.
[0049]
[0053] The substrate support 115 also includes a plurality of fastener devices 450 (only one shown). The fastener devices 450 are utilized to attach the puck 400 to the dielectric plate 410. Each fastener device 450 includes a fastener 452, a metal washer 454, and a fastener cap 456. When the fastener 456 is tightened, the washer 454 presses against a surface 458 of an opening 460 formed in the dielectric plate 410. The washer 454 and the fastener 452 are made of a metallic material, such as stainless steel. The washer 454 includes rounded top corners. The rounded top corners prevent cracking of the material of the dielectric plate 410 when the fastener 452 is tightened.
[0050]
[0054] A fastener cap 456 is utilized to fill the remainder of the opening 460 in the dielectric plate 410. The fastener cap 456 includes a pocket 464 sized to receive the head of the fastener 452. The fastener cap 456 is formed from a dielectric material, such as a polymer, for example, polyetheretherketone (PEEK). The exterior surface of the fastener cap 456 includes a step that reduces arcing between the puck 400 and the base plate 415 by increasing the length of the path through which electricity can travel.
[0051]
[0055] The substrate support 115 also includes a number of gaps between its layers. A first gap 470 is provided between the puck 400 and the dielectric plate 410. A second gap 472 is provided between the dielectric plate 410 and the base plate 415. The first gap 470 and the second gap 472 are in fluid communication with the gas supply 325 shown and described in Figures 3A and 3B. Fluid from the gas supply 325 is channeled through the first gap 470 and the second gap 472 to prevent condensation between adjacent layers. The fluid in the first gap 470 and the second gap 472 is sealed to the edge of the substrate support 115 by an insulator ring 420. The insulator ring 420 may be sized to control leakage of fluid from the first gap 470 and the second gap 472. The insulator ring 420 may include an insulating material such as silicon oxide.
[0052]
[0056] At least the puck 400 and the dielectric plate 410 are surrounded by an insulator ring 420. The base plate 415 and a portion of the insulator ring 420 are surrounded by a ground ring 425 made of aluminum or other conductive material. The insulator ring 420 may include further extensions (not shown) that reduce the "line of sight" of RF current flow by inducing square turns. By including square turns with the cross-sectional shape shown, arcing of RF current is reduced. The insulator ring 420 prevents or minimizes arcing between the puck 400 and the base plate 415 during processing.
[0053]
[0057] Disposed adjacent the inner periphery of the insulator ring 420 is an edge ring 422. The edge ring 422 may comprise a dielectric material such as quartz, silicon, cross-linked polystyrene and divinylbenzene (e.g., Rexolite®), PEEK, Al2O3, AIN, among others. Utilizing an edge ring 422 comprising such dielectric materials helps to modulate the plasma coupling and allows the voltage on the substrate support (V dc ) to improve the properties of the hardmask film deposited on the substrate. By modulating the RF coupling to the wafer or substrate through the edge ring 422 material, the film's elastic modulus can be decoupled from the film's stress. In this way, the hardmask's stress can be reduced without affecting its elastic modulus or the hardmask's elastic modulus can be improved without affecting its stress by increasing the RF power without modulating the ion energy.
[0054]
[0058] Traditionally, tuning of the elastic modulus or stress of a film has been accomplished by adjusting the RF power utilized to ignite or sustain a plasma in a processing chamber. By varying the RF power, the elastic modulus or stress of the film can be changed. However, varying the RF power simultaneously affects both the elastic modulus of the film and the stress of the film. Thus, traditionally, intentionally changing the elastic modulus of a film may unintentionally change the stress of the film, or vice versa.
[0055]
[0059] In contrast, it has been unexpectedly discovered that changing the edge ring material can change the film modulus without affecting the film stress, and vice versa. Without being bound by theory, it is believed that this is a result of changing the properties of the edge ring formed from a different material, which changes the RF coupling to the substrate. Furthermore, by varying the RF coupling to the substrate without changing the RF power applied to generate / sustain the plasma, it is possible to tune one property (e.g., modulus or stress) without significantly affecting the other property (e.g., modulus or stress).
[0056]
[0060] Typically, only one RF source is used during deposition, V dc By increasing the plasma power (or pressure) to increase the V dc This increases both the ion density (i.e., more ionization at higher power) and the ion energy. Therefore, the stress and elastic modulus cannot be independently adjusted or modified. However, by changing the material of the edge ring 422, the V dc is increased without affecting plasma ionization. In this manner, properties such as stress and elastic modulus can be independently tuned or modified. For example, comparing a first edge ring comprising Al2O3 with a second edge ring comprising quartz, both the Al2O3 edge ring and the quartz edge ring result in a film having the same elastic modulus, but the quartz edge ring results in a film having significantly less stress than the Al2O3 edge ring.
[0057]
[0061] By utilizing an edge ring 422 with a low dielectric constant placed between the plasma and ground, which acts as a conductor at the plasma potential, the capacitance between the plasma and ground can be modulated. This reduces the electric field between the plasma and ground and modulates the ion flux to the ground. The edge ring 422 with a lower dielectric constant and the modulated ion flux to the ground enhances or strengthens the electric field, resulting in a V dcBoth the V and ion energy are increased. In this way, the ion energy on the substrate is increased without requiring any increase in ion and neutral density that occurs when the RF power is increased. dc By increasing the ion energy, it becomes possible to independently tune the stress and elastic modulus of the substrate.
[0058]
[0062] 5 illustrates a method 500 of using an edge ring to modulate a hardmask film property according to one embodiment. The method 500 may be utilized with the process chamber 100 of FIGS. 1-3, including the system controller 101, and the substrate support 115 of FIG.
[0059]
[0063] In step 502, a first substrate is placed in a process chamber, a first hard mask film is deposited on the first substrate, and the first substrate is processed with a first RF power. In step 504, one or more film properties of the first hard mask film are measured. The one or more film properties include at least film stress and film modulus. In step 506, the first substrate is removed from the substrate support and the processing chamber.
[0060]
[0064] In step 508, the first edge ring of the substrate support is replaced with a second edge ring comprising a dielectric material such as quartz, silicon, cross-linked polystyrene and divinylbenzene (e.g., Rexolite®), PEEK, Al2O3, or AlN. The second edge ring may be edge ring 422 of FIG. 4. The second edge ring may have a lower dielectric constant than the first edge ring. Alternatively, the second edge ring may have a higher dielectric constant than the first edge ring. The second edge ring comprising the dielectric material helps to modulate plasma coupling, modulating plasma properties without changing plasma power, improving properties of the hardmask film deposited on the substrate. In one example, the second edge ring is selected to adjust properties such as elastic modulus or stress as a result of measurements of the first hardmask film. For example, if it is determined that the modulus of the first hardmask film is not within the predetermined range (but the stress is within the predetermined range), then the second edge ring is selected to adjust the modulus of the subsequently deposited film to be within the predetermined range, while also maintaining the stress within the previously determined range.
[0061]
[0065] A second substrate is then placed on the substrate support in step 510. A second hard mask film is deposited on the second substrate and the second substrate is processed at the first RF power in step 512. In this manner, both the first substrate and the second substrate are processed in the same processing chamber at the same RF power.
[0062]
[0066] In step 514, one or more film properties of the second hardmask film are measured. The one or more film properties include at least film stress and film modulus. The film properties of the second hardmask film are then compared to the film properties of the first hardmask film to confirm that a desired amount of coordination between the first hardmask film and the second hardmask film has been achieved. The second hardmask film may have a modulus change different from the first hardmask film by at least about 20%. The second hardmask film may have a stress change different from the first hardmask film by less than about 5%. Alternatively, the second hardmask film may have a stress change different from the first hardmask film by at least about 20% and the second hardmask film may have a modulus change different from the first hardmask film by less than about 5%. In this manner, even though the first and second substrates are processed at the same RF power, the change in edge ring material results in a second hard mask film disposed on the second substrate that is of better quality than the first hard mask film disposed on the first substrate, without any other changes to the process recipe / parameters.
[0063]
[0067] By modulating the RF coupling to the substrate through the edge ring material, the inverse relationship between modulus and stress can be broken (i.e., modulus can be decoupled from stress). Thus, the stress of the hardmask can be reduced without affecting the modulus, or the modulus of the hardmask can be increased without affecting the stress. Furthermore, the film properties of the hardmask can be improved by increasing the RF power without modulating the ion energy.
[0064]
[0068] The use of an edge ring comprising a dielectric material such as quartz, silicon, cross-linked polystyrene and divinylbenzene (e.g., Rexolite®), PEEK, Al2O3, or AIN allows the deposited hardmask film to have both a high modulus and low stress. The use of an edge ring deposits a hardmask film having a high modulus and low stress, which prevents other components of the system from having to handle increased loads from increased RF currents and voltages, thereby extending the life of the components by preventing component failure.
[0065]
[0069] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, as determined by the following claims.
Claims
1. 1. A method of modulating properties of one or more hardmask films, comprising: depositing a first hard mask film on a first substrate and treating the first substrate with a first RF power; Measuring one or both of an elastic modulus and a stress of the first hard mask film; Removing the first substrate from a substrate support; replacing a first edge ring of the substrate support with a second edge ring, the second edge ring being made of any of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyetheretherketone, Al; 2 O 3 replacing a first edge ring of the substrate support with a second edge ring comprising a material selected from the group consisting of: AIN; placing a second substrate on the substrate support; depositing a second hard mask film on the second substrate and treating the second substrate with the first RF power; Measuring one or both of the elastic modulus and the stress of the second hard mask film; The method includes:
2. 2. The method of claim 1 , wherein the second hardmask film has a different change in elastic modulus than the first hardmask film by at least about 20%, and the second hardmask film has a different change in stress than the first hardmask film by less than about 5%.
3. 2. The method of claim 1 , wherein the second hardmask film has a change in stress that differs from the first hardmask film by at least about 20%, and the second hardmask film has a change in elastic modulus that differs from the first hardmask film by less than about 5%.
4. 2. The method of claim 1, wherein the first edge ring comprises a different material than the second edge ring, and a first hard mask material is the same as a second hard mask material.
5. The method of claim 1 , wherein the second edge ring has a lower dielectric constant than the first edge ring.
6. 10. The method of claim 1, wherein the material of the second edge ring increases the voltage and ion energy on the second substrate when the first RF power is applied.
7. The method of claim 1, wherein the material of the second edge ring is selected to adjust one of the elastic modulus or stress of the second hard mask film independently from the other of the elastic modulus or stress of the second hard mask film.
8. 1. A method of modulating properties of one or more hardmask films, comprising: depositing a first hard mask film on a first substrate and treating the first substrate with a first RF power; Measuring a plurality of film properties of the first hardmask film, the plurality of film properties including elastic modulus and stress; Removing the first substrate from a substrate support; replacing a first edge ring of the substrate support with a second edge ring, the first edge ring comprising a first material different from a second material of the second edge ring; placing a second substrate on the substrate support; depositing a second hardmask film on the second substrate and processing the second substrate with the first RF power, wherein the second material of the second edge ring is selected to adjust at least one film property of the second hardmask film based on the measured film properties of the first hardmask film; depositing a second hardmask film on the second substrate and processing the second substrate with the first RF power, wherein the second material of the second edge ring is selected to adjust at least one film property of the second hardmask film based on the measured film properties of the first hardmask film; The method includes:
9. The dielectric material of the second edge ring is selected from the group consisting of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyether ether ketone, and Al. 2 O 3 9. The method of claim 8, wherein the AIN is selected from the group consisting of:
10. 9. The method of claim 8, wherein the second hardmask film has a different change in elastic modulus than the first hardmask film by at least about 20%, and the second hardmask film has a different change in stress than the first hardmask film by less than about 5%.
11. 9. The method of claim 8, wherein the second hardmask film has a change in stress that differs from the first hardmask film by at least about 20%, and the second hardmask film has a change in elastic modulus that differs from the first hardmask film by less than about 5%.
12. The method of claim 8 , wherein the second edge ring has a higher dielectric constant than the first edge ring.
13. 10. The method of claim 8, wherein the material of the second edge ring increases the voltage and ion energy on the second substrate when the first RF power is applied.
14. 9. The method of claim 8, wherein a second material of the second edge ring is selected to adjust one of a modulus or a stress of the second hardmask film independently from the other of a modulus or a stress of the second hardmask film.
15. A non-transitory computer readable medium for a system, comprising: depositing a first hard mask film on a first substrate and treating the first substrate with a first RF power; Measuring one or both of an elastic modulus and a stress of the first hard mask film; Removing the first substrate from a substrate support; replacing a first edge ring of the substrate support with a second edge ring, the second edge ring being made of any of quartz, silicon, cross-linked polystyrene and divinylbenzene, polyetheretherketone, Al; 2 O 3 replacing a first edge ring of the substrate support with a second edge ring comprising a material selected from the group consisting of: AIN; placing a second substrate on the substrate support; depositing a second hard mask film on the second substrate and treating the second substrate with the first RF power; Measuring one or both of the elastic modulus and the stress of the second hard mask film; 16. A non-transitory computer readable medium having instructions configured to cause a
16. 16. The non-transitory computer-readable medium of claim 15, wherein the second hardmask film has a different change in elastic modulus than the first hardmask film by at least about 20%, and the second hardmask film has a different change in stress than the first hardmask film by less than about 5%.
17. 16. The non-transitory computer-readable medium of claim 15, wherein the second hardmask film has a change in stress that differs from the first hardmask film by at least about 20%, and the second hardmask film has a change in elastic modulus that differs from the first hardmask film by less than about 5%.
18. The non-transitory computer-readable medium of claim 15, wherein the material of the second edge ring is selected to adjust one of the elastic modulus or stress of the second hard mask film independently from the other of the elastic modulus or stress of the second hard mask film.
19. 16. The non-transitory computer-readable medium of claim 15, wherein the second edge ring has a lower dielectric constant than the first edge ring.
20. 20. The non-transitory computer readable medium of claim 15, wherein a material of the second edge ring increases a voltage and ion energy on the second substrate when the first RF power is applied.
Citation Information
Patent Citations
Amorphous carbon film, semiconductor device, film forming method, film forming device and storage medium
JP2008141009A
Method of manufacturing amorphous carbon film used in semiconductor device and method of manufacturing the semiconductor device
JP2012212706A
Methods of forming an amorphous carbon layer and methods of forming a pattern using the same
US20100258526A1
Amorphous carbon deposition process using dual RF bias frequency applications
US20150371851A1
Ultra-high modulus and etch selectivity boron-carbon hardmask films
US20190122889A1