Anti-vibration rubber composition and anti-vibration rubber
The vibration-proof rubber composition with natural and butadiene rubber, fatty acid amides, and thiuram accelerators addresses scorch and durability issues, ensuring low friction and noise reduction in stabilizer bushes.
Patent Information
- Application Number
- JP2022007656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-01-21
AI Technical Summary
Existing anti-vibration rubber compositions face issues with poor scorch resistance, heat resistance, and durability, particularly in stabilizer bushes, leading to frictional noise and wear, despite attempts to improve friction reduction and heat-setting properties.
A vibration-proof rubber composition is developed using natural rubber and butadiene rubber as main components, with specific ratios and additives like fatty acid amides, thiuram-based vulcanization accelerators, and carbon black, to enhance scorch resistance, durability, and maintain low friction over a wide temperature range.
The composition achieves excellent sliding properties, improved scorch resistance, and enhanced durability, reducing friction and preventing abnormal noise in stabilizer bushes, while maintaining productivity and resistance to wear.
Smart Images

Figure 0007588610000007 
Figure 0007588610000008 
Figure 0007588610000009
Abstract
Description
[Technical field]
[0001] The present invention relates to an anti-vibration rubber composition and an anti-vibration rubber, and more particularly to an anti-vibration rubber composition for use in, for example, automobile stabilizer bushings, which is excellent in durability and heat setting properties, can maintain excellent sliding properties, and is also excellent in productivity, and to an anti-vibration rubber made using the anti-vibration rubber composition. [Background technology]
[0002] In automotive anti-vibration rubber, for example, that is used by fitting metal parts such as stabilizer bushings into the vehicle, abnormal noise occurs at the contact points between the mounting bracket and the rubber bushing surface due to the stick-slip phenomenon when starting off, braking suddenly, or turning left or right, and a solution to this problem is required.
[0003] As a countermeasure against such noise, a self-lubricating rubber composition has been studied in which a lubricant such as a fatty acid amide is added and the self-lubricant blooms on the surface of the vulcanized rubber to reduce the coefficient of friction. As the self-lubricant, it has been proposed to add various fatty acid amides (Patent Document 1).
[0004] Furthermore, when the stabilizer bushing wears out over time, a gap forms between the stabilizer bushing and the stabilizer bar, allowing dirt and other foreign matter to get into the gap and cause noise. For this reason, it has been proposed to achieve both a low coefficient of friction and resistance to wear by incorporating specific fatty acid amides (oleic acid amide and stearic acid amide) and silicone oil (Patent Document 2). Furthermore, in order to obtain a friction reducing effect in the low temperature range, as well as heat resistance and scorch resistance (prevention of rubber burning), a self-lubricating rubber composition has been proposed that uses an unsaturated fatty acid amide and polyethylene glycol as a self-lubricant and adds a heat-resistant vulcanization accelerator and high styrene rubber (Patent Document 3).
[0005] Also, in order to maintain the friction reducing effect for a long period even in the case of severe wear, a method of incorporating a silicone acrylic copolymer has been proposed (Patent Document 4). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-234886 [Patent Document 2] Patent No. 5399169 [Patent Document 3] JP 2004-292678 A [Patent Document 4] Patent No. 6525062 Summary of the Invention [Problem to be solved by the invention]
[0007] In vibration-proof rubber compositions containing a large amount of fatty acid amide, it is possible to reduce friction, but scorch resistance tends to deteriorate. In addition, when a heat-resistant vulcanization accelerator is used to improve heat set resistance, the scorch time becomes too short, making the rubber prone to scorch. For this reason, a method is needed to delay the scorch time while improving heat set resistance.
[0008] In Patent Document 3, high styrene rubber (a mixture of high styrene resin and styrene butadiene rubber (SBR)) is added to delay scorch time while preventing rubber burning. However, high styrene rubber has a tendency to gradually deteriorate in settling resistance (compression set resistance) as the amount added increases. Therefore, it is said that various thiuram vulcanization accelerators are used in combination in an amount of 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, per 100 parts by mass of the rubber component as a heat-resistant vulcanization accelerator, but further improvement may be required to achieve both scorch resistance (prevention of rubber burning by delaying scorch time) and heat settling resistance.
[0009] In addition, in Patent Document 4, the cured product of the vibration-proof rubber composition containing the silicone acrylic graft copolymer resin in the rubber component is not intended to reduce friction by bleeding / blooming of fatty acid amide, etc., so it is possible to easily ensure scorch time even if a vulcanization system (e.g., vulcanizing agent, etc.) that imparts heat setting resistance is used. However, since the silicone acrylic graft copolymer resin is in a dispersed state in the rubber, the presence ratio of the silicone acrylic graft copolymer resin on the rubber surface is low, and there are cases where the reduction in friction, especially in the initial stage, is insufficient.
[0010] In addition, in the case of the vibration-proof rubber composition containing oleamide, stearamide, and silicone oil as in Patent Document 2, a large amount of fatty acid amides are precipitated due to the silicone oil immediately after molding of the vibration-proof rubber composition, and a solidified film may be formed on the surface of the vibration-proof rubber composition. When the surface of such a vibration-proof rubber composition is rubbed, the solidified film may peel off, and the friction reduction effect may not be obtained at all. In addition, the vibration-proof rubber composition in Patent Document 2 does not disclose anything about the use of a vulcanization system with a low sulfur content, and the effect of improving sag resistance may be insufficient.
[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an anti-vibration rubber composition for use in, for example, automobile stabilizer bushings, which is excellent in durability and heat setting resistance, can maintain excellent sliding properties, and further has excellent productivity, and to provide an anti-vibration rubber made using the anti-vibration rubber composition. [Means for solving the problem]
[0012] As a result of intensive research by the inventors to solve the above problems, they have found that an anti-vibration rubber composition having natural rubber (NR) and butadiene rubber as main rubber components, in which the main rubber components contain natural rubber / butadiene rubber in a mass ratio of 50 / 50 to 10 / 90, and when the total rubber components are 100 parts by mass, contains 10 to 50 parts by mass of fatty acid amide, 0.1 to 0.6 parts by mass of sulfur as a vulcanizing agent, and contains 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide and 0.5 to 2.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide, can be obtained that has excellent heat setting resistance and durability while maintaining a friction reducing effect, and also has excellent productivity, and have thus completed the present invention.
[0013] That is, the present invention relates to, for example, the following [1] to [5].
[0014] [1] The anti-vibration rubber composition contains natural rubber (NR) and butadiene rubber as the main rubber components and contains 10 to 50 parts by mass of fatty acid amide when the total rubber components are 100 parts by mass, characterized in that the anti-vibration rubber composition contains natural rubber (NR) and butadiene rubber (BR) in a mass ratio of natural rubber / butadiene rubber = 50 / 50 to 10 / 90, contains 0.1 to 0.6 part by mass of sulfur as a vulcanizing agent, contains 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide, and contains 0.5 to 3.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide.
[0015] [2] The anti-vibration rubber composition according to [1], characterized in that it contains 0.3 to 5 parts by mass of 2-(4'-morpholinodithio)benzothiazole and / or 4,4'-dithiodimorpholine per 100 parts by mass of the total rubber components.
[0016] [3] The anti-vibration rubber composition according to [1] or [2], further comprising 5 to 30 parts by mass of high styrene rubber (high styrene resin mixed rubber) per 100 parts by mass of the total rubber components.
[0017] [4] When the total rubber component is 100 parts by mass, the nitrogen adsorption specific surface area is 30 to 100 m 2 The anti-vibration rubber composition according to any one of [1] to [3], characterized in that it contains 40 to 80 parts by mass of carbon black having a molecular weight of 100 / g.
[0018] [5] The butadiene rubber has a cis-1,4-bond content of 90% or more and a Mooney viscosity (ML 1+4 ) is 50 to 75.
[0019] [6] An anti-vibration rubber made using the anti-vibration rubber composition according to any one of [1] to [5]. Effect of the Invention
[0020] According to the present invention, it is possible to obtain an anti-vibration rubber composition for use in the manufacture of anti-vibration rubber, which maintains excellent sliding properties, has good scorch resistance and therefore is highly productive, and has excellent resistance to settling, compared to the case where a conventional anti-vibration rubber composition having a low coefficient of friction is used. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a front view of a stabilizer bush used in the embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a stabilizer bush used in an embodiment (a cross-sectional view in the axial direction of a hollow portion 2). [Diagram 3] FIG. 2 is a perspective view illustrating the abnormal noise test method and durability test method used in the examples. [Figure 4] FIG. 2 is a front view (viewed from the axial direction of the stabilizer bar 4) for explaining the abnormal noise test method and durability test method used in the examples. [Diagram 5] FIG. 2 is a schematic diagram of a Heyden friction and wear tester for explaining a method for measuring a friction coefficient used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Matters relating to the implementation of the present invention will be described in detail below.
[0023] [Rubber component] In the anti-vibration rubber composition according to the present invention, natural rubber (NR) and butadiene rubber (BR) are the main rubber components. The term "mainly made up of natural rubber (NR) and butadiene rubber (BR)" means that 70% by mass or more of the total rubber components are made up of natural rubber (NR) and butadiene rubber (BR) (the total amount of natural rubber (NR) and butadiene rubber (BR) is 70% by mass or more of the total rubber components).
[0024] Furthermore, natural rubber (NR) and butadiene rubber (BR) are contained in a mass ratio of NR / BR=50 / 50 to 10 / 90 (hereinafter simply referred to as the rubber component category of the present invention). When NR and BR are contained in the main rubber component within the rubber component category of the present invention, the fatty acid amide in the vibration-proof rubber composition tends to come out to the surface in sequence in a wide temperature range from low to high temperatures, and the generation of abnormal noise due to stick-slip is easily suppressed, and the vibration-proof rubber composition has excellent abrasion resistance and rubber strength.
[0025] If the proportion of BR exceeds the range of the rubber component of the present invention, the strength of the vulcanized rubber will be significantly reduced, and the obtained anti-vibration rubber may be easily broken when a strong force is applied to it. If the proportion of NR exceeds the range of the rubber component of the present invention, the scorch time will tend to be shortened, and the friction coefficient of the obtained vulcanized rubber may easily become high.
[0026] The rubber component may contain rubber components other than NR and BR at a ratio of less than 30% by mass of the total rubber components. The other rubber components are not particularly limited, but high styrene rubber (high styrene resin mixed rubber) is preferably used.
[0027] In particular, when it is necessary to withstand a large load and keep the amount of settling low, it is effective to keep the amount of initial deformation low by increasing the rubber hardness, but increasing the amount of carbon black to increase hardness leads to an increase in the coefficient of friction and, further, a decrease in the fluidity of the unvulcanized rubber, which also reduces the kneading and molding processability.Adding a large amount of sulfur, which is a vulcanizing agent, is not preferred because it not only worsens the heat settling resistance of the obtained anti-vibration rubber, but also makes it brittle and prone to breakage (leading to a decrease in durability).
[0028] On the other hand, high styrene rubber usually tends to deteriorate sag resistance (increase in compression set rate) when the content is increased, but by using a vulcanizing agent and a vulcanization accelerator as in the present invention, deterioration of sag resistance can be suppressed and a vibration-proof rubber with high hardness and low friction can be obtained, so it is preferably used. The content of high styrene rubber is preferably 2 to 30 parts by mass, and more preferably 5 to 25 parts by mass, per 100 parts by mass of the total rubber component.
[0029] In the present invention, the rubber component is all high styrene rubber (high styrene resin mixed rubber). The high styrene rubber used in the present invention has a styrene content of 50% by mass or more and 75% by mass or less. For example, JSR0061 (styrene content 66% by mass) and JSR0051 (styrene content 56%) manufactured by JSR Corporation are preferably used as commercially available products, but are not limited thereto as long as they are obtained based on the above-mentioned specifications.
[0030] As the butadiene rubber (BR) used in the present invention, from the viewpoints of low-temperature properties and durability against repeated deformation, the higher the cis 1,4-bond content, the better. For example, it is preferable to use a high cis BR having a cis 1,4-bond content of 90% or more, and more preferably 93% or more.
[0031] In addition, for BR with the same chemical composition, the Mooney viscosity (ML 1+4 The higher the Mooney viscosity (ML) at 100°C, the higher the molecular weight and the better the durability. 1+4) is preferably 50 or more. On the other hand, Mooney viscosity (ML 1+4 ) increases, the flowability of rubber tends to decrease, and the Mooney viscosity (ML 1+4 If the Mooney viscosity (ML) at 100° C. is too high, the kneading processability and molding processability of the vibration-proof rubber material composition tend to deteriorate. 1+4 ) is preferably 75 or less. More preferably, the Mooney viscosity (ML 1+4 That is, in the present invention, the butadiene rubber (BR) having a Mooney viscosity of 50 or more and 65 or less is preferably used.
[0032] Examples of such butadiene rubber include JSR BR730, JSR BR54, and JSR BR740 (all manufactured by JSR Corporation), Ubepol 390L (manufactured by Ube Industries, Ltd.), and BUNA CB21, CB22, and CB1221 (all manufactured by ARLANXEO).
[0033] In addition, masterbatches such as vulcanization accelerators and sulfur can be used as other rubber components to improve the working environment and processability, and there is no problem if the masterbatches contain small amounts of other rubber components such as EPDM.
[0034] [Fatty acid amide] In the present invention, the fatty acid amide is contained in an amount of 10 to 50 parts by mass (hereinafter, appropriately referred to as the fatty acid amide category of the present invention) when the total rubber component is taken as 100 parts by mass. In the case of this fatty acid amide category of the present invention, the fatty acid amide is appropriately precipitated (bloomed) on the rubber surface, and stable low friction is obtained. More preferably, the content of the fatty acid amide is 15 to 30 parts by mass when the total rubber component is taken as 100 parts by mass. In the case of this fatty acid amide category of the present invention, even if the fatty acid amide precipitated on the rubber surface is scraped off from the surface, the fatty acid amide precipitates stably and continuously, so that a low friction coefficient is maintained for a long period of time.
[0035] As the type of fatty acid amide to be used, various fatty acid amides can be used, but from the viewpoint of easily obtaining suitable bloom properties in the usage environment range, fatty acid amides having a melting point of 65 to 120° C. are preferably used. In order to keep the friction coefficient low in the low temperature range, it is preferable to contain 8 to 25 parts by mass of fatty acid amides having a melting point of 65 to 88° C. in the total rubber component.
[0036] Furthermore, from the viewpoint of facilitating low friction over a wider temperature range, there is no problem in mixing fatty acid amides having a melting point of 65 to 88° C. with fatty acid amides having a melting point of 90 to 120° C. Examples of fatty acid amides having a melting point of 65 to 120° C. include oleic acid amide (melting point 75° C.), erucic acid amide (melting point 81° C.), N-stearyl oleic acid amide (melting point 67° C.), N-oleyl stearic acid amide (melting point 74° C.), N-stearyl erucic acid amide (melting point 74° C.), lauric acid amide (melting point 87° C.), palmitic acid amide (melting point 100° C.), stearic acid amide (melting point 101° C.), hydroxyl amide (melting point 102° C.), hydroxyl amide (melting point 101° C.), hydroxyl amide (melting point 103° C.), hydroxyl amide (melting point 104° C.), hydroxyl amide (melting point 105° C.), hydroxyl amide (melting point 106° C.), hydroxyl amide (melting point 107° C.), hydroxyl amide (melting point 108° C.), hydroxyl amide (melting point 109° C.), hydroxyl amide (melting point 110° C.), hydroxyl amide (melting point 111° C.), hydroxyl amide (melting point 112° C.), hydroxyl amide (melting point 113° C.), hydroxyl amide (melting point 114° C.), hydroxyl amide (melting point 115° C.), hydroxyl amide (melting Examples include cystearamide (melting point 107°C), N-stearylstearamide (melting point 95°C), ethylene bisoleamide (melting point 119°C), ethylene biserucamide (melting point 120°C), hexamethylene bisoleamide (melting point 110°C), N,N'-dioleyl adipamide (melting point 118°C), and N,N'-dioleyl sebacamide (melting point 113°C).
[0037] [Vulcanization chemicals (vulcanizing agents, vulcanization accelerators, and vulcanization retarders)] Generally, vulcanizing agents and vulcanization accelerators are classified separately, but most thiurams usually classified as vulcanization accelerators are also known to be used as vulcanizing agents. Therefore, in the following, vulcanizing agents, vulcanization accelerators, and vulcanization retarders will each be simply referred to as vulcanization system chemicals, or vulcanizing agents, vulcanization accelerators, and vulcanization retarders will be collectively referred to as the vulcanization system as appropriate.
[0038] In the present invention, the vulcanizing agent contains sulfur in a ratio of 0.1 to 0.6 parts by mass (hereinafter, appropriately referred to as the sulfur range of the present invention). In the case of this sulfur range of the present invention, a vulcanized rubber composition for vibration-proof rubber having excellent heat setting resistance can be obtained.
[0039] The vulcanization system of the anti-vibration rubber composition of the present invention contains 8 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide and 0.5 to 5.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide as essential components.
[0040] In order to improve heat setting resistance, it is preferable to contain various thiurams, but if a mixture of natural rubber and butadiene rubber is used as the main rubber component and 10 to 50 parts by mass of the above fatty acid amide is contained, the vulcanization start time becomes extremely fast and scorch resistance becomes poor. By containing 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide and 0.5 to 5.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide, it is possible to achieve both scorch resistance and setting resistance.
[0041] In an anti-vibration rubber composition that does not contain a fatty acid amide, the inclusion of 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide and further the inclusion of 0.5 to 5.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide slows down the vulcanization rate and tends to lead to a deterioration in productivity, but the anti-vibration rubber composition of the present invention provides an appropriate vulcanization rate, scorch resistance, and good resistance to sagging.
[0042] Although tetrakis(2-ethylhexyl)thiuram disulfide improves sag resistance without deteriorating scorch resistance even when it is contained in a large amount, adding too much increases material costs, and therefore the content of tetrakis(2-ethylhexyl)thiuram disulfide is set, for example, to 30 parts by mass or less, preferably 7 to 20 parts by mass, and more preferably 8 to 16 parts by mass.
[0043] In this anti-vibration rubber composition, which contains a large amount of fatty acid amide, a small amount of sulfur, and a large amount of thiuram vulcanization accelerator, the well-known scorch inhibitor (retarder) CTP (N-cyclohexylthiophthalimide) does not exhibit a scorch prevention effect, whereas N-phenyl-N-(trichloromethylthio)benzenesulfonamide exhibits a sufficient scorch prevention effect even in a system such as this anti-vibration rubber composition.
[0044] If the content of N-phenyl-N-(trichloromethylthio)benzenesulfonamide is less than 0.5 parts by mass, the scorch prevention effect is small, and even if it is contained in more than 5 parts by mass, no further scorch prevention effect can be obtained. Therefore, the content of N-phenyl-N-(trichloromethylthio)benzenesulfonamide is, for example, 0.5 to 5 parts by mass, more preferably 0.5 to 3 parts by mass.
[0045] In addition, when it is desired to obtain a vibration-proof rubber having higher hardness and excellent sag resistance, it is preferable to contain 2-(4'-morpholinodithio)benzothiazole and / or 4,4'-dithiodimorpholine in a ratio of 0.3 to 5 parts by mass (hereinafter referred to as the vulcanization category of the present invention) based on 100 parts by mass of the total rubber components. In the case of this vulcanization category of the present invention, it is easy to obtain a vibration-proof rubber having moderate scorch resistance, high hardness, and heat sag resistance. By containing 0.3 to 5 parts by mass of 2-(4'-morpholinodithio)benzothiazole and / or 4,4'-dithiodimorpholine, the amount of tetrakis(2-ethylhexyl)thiuram disulfide added can be reduced in obtaining a vulcanized rubber having higher hardness and excellent C-set resistance, and the cost of rubber materials can be suppressed from increasing.
[0046] The 0.3 to 5 parts by mass of 2-(4'-morpholinodithio)benzothiazole and / or 4,4'-dithiodimorpholine means that the total amount of 2-(4'-morpholinodithio)benzothiazole and 4,4'-dithiodimorpholine is 0.3 to 5 parts by mass.
[0047] It is also preferable to further contain a thiazole-based vulcanization accelerator and / or a sulfenamide-based vulcanization accelerator. Specifically, thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and dibenzothiazyl disulfide, and sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide, N-oxydiethylene-2-benzothiazole sulfenamide, and N,N-diisopropyl-2-benzothiazole sulfenamide can be preferably used. In particular, dibenzothiazyl disulfide can be preferably used from the viewpoint of achieving both scorch resistance and sag resistance.
[0048] Furthermore, it is possible to add a small amount of guanidine vulcanization accelerators such as diphenyl guanidine, triphenyl guanidine, diorthonitrile guanidine, orthonitrile biguanide, diphenyl guanidine phthalate, etc., thiuram compounds such as tetramethyl thiuram monosulfide, tetramethyl thiuram disulfide, tetraethyl thiuram disulfide, tetrabutyl thiuram disulfide, tetrabenzyl thiuram disulfide, dipentamethylene thiuram tetrasulfide, etc., and various dithiocarbamic acid metal salt vulcanization accelerators. However, the combined use of these vulcanization accelerators tends to deteriorate scorch resistance, so the content of the vulcanization accelerator is preferably 0.3 parts by mass or less, and more preferably 0.1 parts by mass or less, when the total rubber component is 100 parts by mass.
[0049] [Carbon black] In the vibration-proof rubber composition according to the present invention, the carbon black has a nitrogen adsorption specific surface area of 30 to 100 m 2 It is preferable that the carbon black contains 40 to 80 parts by mass of carbon black having a molecular weight of 1000 to 15000 / g. The nitrogen adsorption specific surface area is an index of the particle size of carbon black, and a large nitrogen adsorption specific surface area indicates a small particle size.
[0050] As explained in the rubber component section above, the rubber component used in the present invention contains a large amount of butadiene rubber (BR). Butadiene rubber (BR) has extremely low rubber strength without a reinforcing agent such as carbon black. By including fine carbon black with a small nitrogen adsorption specific surface area (large particle size), a large reinforcing effect is obtained, and physical properties such as abrasion resistance are improved.
[0051] On the other hand, if a large amount of fine carbon black is added, gripping performance increases and friction resistance increases (slipperiness decreases). In addition, adding a large amount of fine carbon black leads to deterioration of compression set. Furthermore, the particle size and amount of carbon black added also affect the deposition of fatty acid amide on the rubber surface.
[0052] When the nitrogen adsorption specific surface area of carbon black is small (the particle size is large), it is easy to obtain a vulcanized rubber with a small friction coefficient and good reinforcement properties for compression set resistance, but the reinforcement properties are low and the durability as a vibration-proof rubber is likely to be insufficient.
[0053] 30~100m 2 By incorporating carbon black having a nitrogen adsorption specific surface area of 30 to 100 m / g in the range of 40 to 80 parts by mass per 100 parts by mass of the rubber component, it is possible to ensure sufficient rubber strength and suppress deterioration of compression set while ensuring sustained low friction. Examples of such carbon black include HAF, HAF-HS, HAF-LS, MAF, and FEF grades known as furnace blacks for rubber. In addition, there are also carbon blacks for coloring and conductive carbon blacks with a nitrogen adsorption specific surface area of 30 to 100 m. 2 / g can be preferably used.
[0054] In the vibration-proof rubber composition of the present invention, natural rubber (NR) and butadiene rubber are the main rubber components, and when the total rubber components are 100 parts by mass, the vibration-proof rubber composition contains 10 to 50 parts by mass of fatty acid amide, natural rubber (NR) and butadiene rubber (BR) in a mass ratio of natural rubber / butadiene rubber = 50 / 50 to 10 / 90, contains 0.1 to 0.6 parts by mass of sulfur as a vulcanizing agent, contains 7 to 30 parts by mass of tetrakis (2-ethylhexyl) thiuram disulfide, and contains 0.5 to 3.0 parts by mass of N-phenyl-N- (trichloromethylthio) benzenesulfonamide, and in addition to the various compounding materials described above, it is possible to appropriately contain vulcanization aids, antiaging agents, fillers, process oils, processing aids, coupling agents, etc. that are used as normal rubber compounding materials as necessary. As an example, it is possible to appropriately contain the following.
[0055] [Vulcanization aid] The anti-vibration rubber composition of the present invention is preferably used in combination with a vulcanization aid such as zinc oxide (ZnO), complex zinc oxide, stearic acid, zinc stearate, etc. These vulcanization aids may be used alone or in combination of two or more kinds.
[0056] Here, composite zinc oxide is known to have a layer of zinc oxide (zinc oxide) on the surface and contain an inorganic metal salt inside as a core component, and examples include the META-ZL series (META-Z L40, L50, L60) manufactured by Inoue Lime Industry Co., Ltd.
[0057] The content of zinc oxide or zinc oxide composite is 3 parts by mass or more and 15 parts by mass or less based on 100 parts by mass of the rubber component. The content of stearic acid or zinc stearate is preferably 0.1 parts by mass or more and 3 parts by mass or less based on 100 parts by mass of the rubber component.
[0058] [Anti-aging agent] It is preferable that the anti-vibration rubber composition of the present invention contains an antioxidant. The diene rubber (natural rubber, butadiene rubber) used in the present invention does not have high ozone resistance or heat resistance as a rubber component, so it is preferable to improve it with a known antioxidant. Examples of the antioxidant include carbamate-based antioxidants, phenylenediamine-based antioxidants, phenol-based antioxidants, diphenylamine-based antioxidants, quinoline-based antioxidants, imidazole-based antioxidants, waxes, etc. These are used alone or in combination of two or more kinds.
[0059] The content of the antioxidant is preferably in the range of 1 to 15 parts by mass, and more preferably in the range of 3 to 10 parts by mass, based on 100 parts by mass of the rubber component.
[0060] [Filler] The anti-vibration rubber composition of the present invention may contain a filler for the purpose of adjusting hardness and improving processability. As the filler, fillers used in ordinary rubber compositions, such as silica (wet silica, dry silica, colloidal silica, etc.), calcium carbonate, clay, talc, etc., may be used. These fillers may be used alone or in combination of two or more kinds.
[0061] [Process oil] The anti-vibration rubber composition of the present invention may contain a process oil for the purpose of adjusting hardness and improving processability. Examples of the process oil include naphthenic oil, paraffinic oil, aromatic oil, etc. These may be used alone or in combination of two or more kinds.
[0062] [Processing aids] The anti-vibration rubber composition of the present invention may contain a processing aid for the purpose of improving processability. Compounds used in normal rubber processing may be used as the processing aid. Specific examples include higher fatty acids such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid, salts of higher fatty acids such as barium stearate, zinc stearate, and calcium stearate, and esters of higher fatty acids such as ricinoleic acid, stearic acid, palmitic acid, and lauric acid. These may be used alone or in combination of two or more kinds.
[0063] [Coupling agent] In the anti-vibration rubber composition of the present invention, a coupling agent for carbon black or a silane coupling agent can be used for the purpose of adjusting vibration characteristics. Examples of the coupling agent for carbon black include hydrazide compound coupling agents, sulfide compound coupling agents, and pyrazolone compound coupling agents, and examples of the silane coupling agent include mercapto silane coupling agents, sulfide silane coupling agents, amine silane coupling agents, epoxy silane coupling agents, and vinyl silane coupling agents, and each of these can be used alone or in combination of two or more. Among these, the silane coupling agent is preferably a mercapto silane coupling agent or a sulfide silane coupling agent, and these can be used alone or in combination of two or more.
[0064] [Method for preparing anti-vibration rubber composition] The anti-vibration rubber composition of the present invention can be prepared by using a rubber component, a carbon black component, a fatty acid amide, and, if necessary, other materials listed above, and kneading these various materials using a kneading machine such as a pressure kneader, a Banbury mixer, an intermix mixer, or an open roll.
[0065] The anti-vibration rubber composition of the present invention becomes an elastic body by vulcanization, for example, at a vulcanization temperature of 145 to 170° C. for 3 to 60 minutes, although the vulcanization conditions (vulcanization temperature and vulcanization time) vary depending on the molding machine, etc. An anti-vibration rubber member having a sliding contact part made of an elastic body vulcanized from the anti-vibration rubber composition of the present invention can be suitably used as an anti-vibration rubber member that requires sliding properties, such as a stabilizer bushing used in vehicles such as automobiles.
[0066] The shape of the sliding contact portion depends on the shape of the mating member with which it slides. Therefore, for example, if the mating member is a metal shaft, the shape of the sliding contact portion may be one having an insertion hole for inserting the metal shaft. These anti-vibration rubber members can eliminate the deterioration of sliding properties caused by temperature environments and continuous use, and can effectively suppress the increase in frictional resistance between the mating member. Therefore, problems such as the generation of abnormal noise (stick-slip noise) during sliding and poor ride comfort of the vehicle can be eliminated.
[0067] 1 and 2 show an example of a stabilizer bushing 1 as an anti-vibration rubber made using the above-mentioned anti-vibration rubber composition. As shown in the figures, the stabilizer bushing 1 is configured to hold a stabilizer bar (an iron bar in the abnormal noise test described later) 4 inserted into a hollow portion 2 having a circular cross section. The main body (rubber portion) 3 of the thick-walled cylindrical stabilizer bushing 1 is held within a substantially U-shaped bracket (not shown) and is configured to be fixed to the vehicle body via the bracket.
[0068] Since such a stabilizer bush 1 is used by fitting the stabilizer bar 4, which is a metal part, a rotational force or twisting force is applied to the contact portion between the stabilizer bar 4 and the surface of the inner hole of the stabilizer bush 1 (the inner peripheral surface of the hollow portion 2) when starting, braking suddenly, turning, etc., and abnormal noise is likely to occur due to the stick-slip phenomenon. Therefore, by forming the stabilizer bush 1 from the vibration-proof rubber composition (self-lubricating rubber composition) of the present invention, the lubricating component (fatty acid amide) gradually precipitates on the rubber surface and acts as a self-lubricant, reducing the friction coefficient over a wide temperature range, thereby preventing the generation of abnormal noise. In this case, if the stabilizer bush 1 wears out over time, a gap will be generated between the stabilizer bush 1 and the stabilizer bar 4, and muddy water or the like may enter the gap, causing abnormal noise. However, the vibration-proof rubber composition of the present invention has excellent resistance to wear, so that the intrusion of muddy water can be effectively prevented. EXAMPLES
[0069] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0070] <Preparation of anti-vibration rubber composition> Anti-vibration rubber compositions were prepared by mixing and kneading various materials in the ratios shown in Tables 1 to 3. The above kneading was carried out by first kneading the materials other than the vulcanizing agent and vulcanization accelerator for 5 minutes using a Banbury mixer, and then adding the vulcanizing agent and vulcanization accelerator to the rubber kneaded in the Banbury mixer using an open roll while cooling the cooling water temperature by about 20°C, and kneading for 5 minutes to prepare anti-vibration rubber compositions (Examples 1 to 16, Comparative Examples 1 to 8).
[0071] [Table 1]
[0072] [Table 2]
[0073] [Table 3]
[0074] The materials listed in Tables 1 to 3 are as follows. Natural rubber: SVR CV60 Butadiene rubber-1: cis 1,4-bond content 94%, Mooney viscosity (ML 1+4 )55, JSR Corporation "BR-730" Butadiene rubber-2: cis 1,4-bond content 96%, Mooney viscosity (ML 1+4 )44, JSR Corporation "BR-01" High styrene rubber: Product name "JSR 0061", manufactured by JSR Corporation, bound styrene content 66% by mass Zinc oxide: Sakai Chemical Industry Co., Ltd. "Zinc oxide type 2" Stearic acid: "Camellia stearate" manufactured by Nippon Oil & Fats Co., Ltd. Anti-aging agent 1: (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine), "Vulkanox 4020" manufactured by LANXESS · Anti-aging agent-2: (2-mercaptobenzimidazole) "Nocrac MB" manufactured by Ouchi Shinko Co., Ltd. · Anti-aging agent-3: (wax) Nippon Seiro Co., Ltd. "Ozoace 0100" Carbon black-1: Nitrogen adsorption specific surface area 47m 2 / g (MAF grade), "Niteron #10" manufactured by Nippon Steel Carbon Co., Ltd. Carbon black-2: Nitrogen adsorption specific surface area 39m 2 / g (FEF grade), "HTC#100" manufactured by Nippon Steel Carbon Co., Ltd. Carbon black-3: Nitrogen adsorption specific surface area 76m 2 / g (HAF grade), "VULCAN3D" manufactured by Cabot Japan Co., Ltd. Carbon black-4: Nitrogen adsorption specific surface area 108 m 2 / g (ISAF class), Cabot Japan Co., Ltd. "VULCAN6J" Carbon black-5: Nitrogen adsorption specific surface area 26m 2 / g (GPF grade), "Niteron 55S" manufactured by Nippon Steel Carbon Co., Ltd. Fatty acid amide-1: Erucic acid amide, melting point 81°C, "Diamid L-200" manufactured by Mitsubishi Chemical Corporation Fatty acid amide-2: Palmitic acid amide, melting point 100°C, "Diamid KP" manufactured by Mitsubishi Chemical Corporation Oil: ENEOS Corporation "Crisef Oil H56" Vulcanization system 1 (sulfur): Tsurumi Chemical Industry Co., Ltd. "Kinkajirushi Micro Powder Sulfur 200Mesh" Vulcanization system-2 Tetrakis(2-ethylhexyl)thiuram disulfide: "Noccela TOT-N" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization system-3 N-phenyl-N-(trichloromethylthio)benzenesulfonamide: LANXESS "Bulcurrent E / C" Vulcanization system 4 (4,4'-dithiodimorpholine): "Actor R" manufactured by Kawaguchi Chemical Co., Ltd. Vulcanization system-5 (2-(4'-morpholinodithio)benzothiazole): "Noccela MDB-P" manufactured by Ouchi Koh Chemical Co., Ltd. Vulcanization system 6 Di-2-benzothiazolyl disulfide: "Noccela DM" manufactured by Ouchi Shinko Chemical Co., Ltd. Vulcanization system 7 (N-oxydiethylene-2-benzothiazolyl sulfenamide: "Accel NS" manufactured by Kawaguchi Chemical Co., Ltd.) Vulcanization system-8: Tetrabutylthiuram disulfide: "Accel TBT" manufactured by Kawaguchi Chemical Co., Ltd. Vulcanization system-9 Tetramethylthiuram disulfide: "Noccela TT-P" manufactured by Ouchi Shinko Chemical Co., Ltd. Vulcanization system - 10 N-cyclohexylthiophthalimide: "Retarder CTP" manufactured by Toray Industries, Inc. The evaluation methods and sample preparation methods for the anti-vibration rubber compositions (Examples 1 to 16, Comparative Examples 1 to 8) shown in Tables 1 to 3, and the judging criteria for each item are as follows. The evaluation results and judging results are shown in Tables 4, 5, and 6 below.
[0075] <<Vulcanization characteristic test - Measurement of vulcanization speed (unvulcanized test)>> In accordance with JIS K6300-2, a V-type curing meter was used to draw a vulcanization curve for 20 minutes at a measurement temperature of 150°C, an amplitude angle of ±1°, and a frequency of 100 cpm, and the tC(10) and tC(90) values were calculated from the vulcanization curve.
[0076] In terms of evaluation, those with a tC(10) of less than 2 minutes were rated as × because the vulcanization start time was short and they were prone to scorching (rubber burning) during molding processing; those with a tC(10) of 2 to 3 minutes were rated as △ because care must be taken against scorching; and those with a tC(10) of 3 minutes or more were rated as ◯.
[0077] <Moony Scorch Time> For each of the vibration-proof rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8, a Mooney viscometer was used in accordance with JIS 6300-1 using an L-type rotor to measure the minimum Mooney viscosity at a measurement temperature of 125°C, Vm, and the time t5 required for the viscosity to rise by 5M from Vm was measured, and t5 was defined as the Mooney scorch time.
[0078] In terms of evaluation, those with a Mooney scorch time of less than 10 minutes were rated as × since they are prone to scorching, those with a Mooney scorch time of 10 to 15 minutes were rated as △ since there are restrictions on the storage period of unvulcanized rubber and the method of molding anti-vibration rubber, and those with a Mooney scorch time of 15 minutes or more were rated as ◯.
[0079] <Creating evaluation samples (vulcanized rubber)> Preparation of 2 mm thick vulcanized rubber sheet: For each of the vibration-proof rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8, vulcanization molding was carried out by compression molding using a 2 mm sheet mold with a cavity that would result in a rubber thickness of 2 mm, at 150°C for a vulcanization time of (tC(90)+5) to obtain a 2 mm thick vulcanized rubber sheet (hereinafter simply referred to as the evaluation rubber sheet).
[0080] Preparation of vulcanized rubber test pieces for compression set tests: For each of the vibration-proof rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8, a cylindrical test piece preparation mold having a diameter of 29.0 mm and a height of 12.5 mm was used to carry out vulcanization molding at 150°C for a vulcanization time of (tC(90)+10) to obtain cylindrical vulcanized rubber test pieces for compression set tests having a diameter of 29.0 mm and a height of 12.5 mm (hereinafter simply referred to as rubber test pieces).
[0081] Molding of anti-vibration rubber: For each of the anti-vibration rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8, an injection molding machine with a clamping force of 50 tons was used to vulcanize and mold the composition at 150°C for 8 minutes into a shape similar to that of stabilizer bushing 1 shown in FIG. 1 to mold anti-vibration rubber (stabilizer bushing; hereinafter, simply referred to as anti-vibration rubber for evaluation).
[0082] Using the vulcanized rubbers (evaluation rubber sheets, rubber test pieces, evaluation anti-vibration rubbers) of the vibration-proof rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8 thus obtained, evaluation of each property was carried out according to the following criteria. The results are shown in Tables 4 to 6 below. The evaluation methods for each evaluation item are as follows.
[0083] <Tensile properties> The rubber sheets for evaluation obtained from each of the anti-vibration rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8 were punched out with a JIS No. 3 dumbbell, and the breaking strength (TB) and breaking elongation (EB) were measured in accordance with JIS K 6251, and the rubber hardness (HA: JIS A) was measured in accordance with JIS K 6253-3. The evaluation was judged as follows: those with a breaking strength (TB) of 10 MPa or more were rated as ◯, and those with a breaking strength of less than 10 MPa were rated as △, since the strength was low and some anti-vibration rubbers may be difficult to use.
[0084] <<Resistance to settling – Compression set rate>> The rubber test pieces obtained in each of the vibration-proof rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8 were compressed in the height direction by 25.0% (height 9.38 mm) using a jig in accordance with JIS K6262 (compression set) and left in a thermostatic chamber at an atmospheric temperature of 100°C for the following time, and then the jig was removed and the rubber test pieces were quickly released. After this release, the rubber test pieces were left on a wooden stand in an atmosphere of 23°C for 30 minutes, and the height of the rubber test pieces was measured to calculate the compression set CS (%). Four types of leaving time in the 100°C thermostatic chamber were performed: 22 hours, 72 hours, 150 hours, and 500 hours. The smaller the compression set, the better the settling resistance. Therefore, in the evaluation judgment, those with the above compression set CS (%)-500 hours of less than 40% were marked as ◯, those with 40% to less than 50% were marked as △, and those with more than 50% were marked as x.
[0085] <Friction coefficient> [Method of measuring friction coefficient] The rubber sheets for evaluation obtained from each of the anti-vibration rubber compositions of Examples 1 to 16 and Comparative Examples 1 to 8 were prepared and then left at 23°C for 24 hours, after which samples S were cut to 50 mm x 10 mm, and the friction coefficients were immediately measured using a Hayden friction and wear tester 6 shown in Fig. 5 in an atmosphere of 23°C. That is, the sample S, 50 mm in the moving direction, 10 mm in width, and 2 mm in thickness, was attached to a movable table 61 that can move on a fixed table 60 as shown in Fig. 5, and when the movable table 61 was moved 16.7 mm in the surface direction (direction of the black arrow in the figure) at a speed of 16.7 mm per second, the force (F) applied to the counter member 63 that was fixed to the load cell 62 and could not be moved was measured by the load cell 62. Reference numeral 64 denotes an operating lever that adjusts the position of the counter member 63 with the fulcrum between the load cell 62 and the counter member 63, and reference numeral 65 denotes a balancer that is attached between the load cell 62 and the fulcrum.
[0086] Here, the counter member 63 used was made of stainless steel with a contact surface of 10 mm x 10 mm and a surface roughness (Rmax) of 5 to 10 μm. A load (weight) W of 100 g was placed on the counter member 63. The friction coefficient μ is a μ value calculated by the formula F = μM. The peak of the friction coefficient obtained first after the movable base 61 started to move was defined as the static friction coefficient (μs), and the average value of the friction coefficient obtained during the subsequent movement of 16.7 mm was defined as the dynamic friction coefficient (μd).
[0087] [Determination of friction coefficient] In assessing the above friction tests, a static friction coefficient of less than 0.8 was rated as "good", a coefficient between 0.8 and 1.0 was rated as "△" as it may be usable, and a coefficient of 1.0 or more was rated as "×". A dynamic friction coefficient of less than 0.6 was rated as "good", a coefficient between 0.6 and 1.0 was rated as "△", and a coefficient of 1.0 or more was rated as "×". If there was an "×" in the static and dynamic friction coefficient ratings of "good", "△", or "×", then the friction coefficient test rating was "×". If there was no "×" and any rating was "△", then it was rated as "△". If all were "good", then they were rated as "good".
[0088] <Anti-vibration rubber evaluation - Stabilizer bush evaluation> As shown in Figures 1 and 2, for a stabilizer bush 1 (outer dimension 42 mm) having a hollow section 2 (diameter 20 mm), the presence or absence of cracks and the amount of sag (sag resistance judgment) were measured based on the following items [abnormal noise test], [heat resistance endurance test - crack occurrence], and [heat resistance endurance test - sag].
[0089] [Abnormal noise test] First, as shown in Figures 3 and 4, an iron bar 4 having a diameter of 21.0 mm and a surface that has been electrochemically painted (cationic coating) was inserted into a hollow portion 2 having a diameter of 20 mm provided in the main body 3 of the stabilizer bush 1, and then the stabilizer bush 1 was fixed to a fixed base 50 in a compressed state using an approximately U-shaped bracket 5 so that the radial dimension of the hollow portion 2 (the vertical height in Figure 4) was 37 mm.
[0090] Next, the iron bar 4 was rotated (input) axially in the twisting direction (the twisting direction indicated by the arrow in Fig. 4) by ±10° at a frequency of 1 Hz. This axial rotation was performed for 10 minutes at ambient temperatures of -30°C and 100°C, and the presence or absence of abnormal noise was measured. The evaluation was made as follows: if no abnormal noise was generated within 10 minutes of the start of the axial rotation, it was marked as ◯; if abnormal noise was generated, it was marked as ×.
[0091] [Heat resistance durability test] First, in the same manner as in the previous item [Noise test], the stabilizer bush 1 with an iron bar 4 inserted therethrough was compressed by an approximately U-shaped bracket 5 and fixed to a fixed base 50. This was left at 100°C for 500 hours, and then left in a room temperature (23°C) atmosphere for a further 24 hours before a durability test was conducted.
[0092] The durability test method involved applying ±8000N to the stabilizer bushing 1 in the direction perpendicular to the axis (upward in Figure 4), while performing a biaxial durability test with an axial rotation (frequency: 1Hz) of ±5° in the torsional direction, 100,000 times at room temperature (23°C).
[0093] [Heat resistance durability test - crack generation] After the heat resistance durability test was completed, the stabilizer bushing 1 was checked for cracks. The evaluation was judged as ◯ when no cracks were generated, and × when cracks were generated.
[0094] [Heat resistance durability test - settling] After the heat resistance durability test, the iron bar 4 and the approximately U-shaped bracket 5 were removed, and the outer dimensions of the stabilizer bushing 1 after the heat resistance durability test and the outer diameter of the hollow portion 2 with an initial diameter (20 mm) provided in the main body 3 were measured, and the difference between the outer dimensions of the stabilizer bushing 1 and the outer diameter of the hollow portion 2 was taken as the rubber thickness after the heat resistance durability test. The initial rubber thickness of the stabilizer bushing 1 (before the heat resistance durability test) was approximately 22 mm (outer dimension approximately 42 mm - outer diameter of the hollow portion approximately 20 mm). On the other hand, the rubber thickness when the iron bar 4 was inserted and the approximately U-shaped bracket 5 was assembled was 37 mm - 21 mm = 16 mm. The difference between this initial rubber thickness and the rubber thickness after the heat resistance durability test was obtained, and this value was taken as the amount of sag. That is, if there is no difference in rubber thickness before and after the heat resistance durability test, the amount of sag is 0mm (0%), and if there is no recovery at all even when the iron bar 4 and the approximately U-shaped bracket 5 are removed after the heat resistance durability test is completed, the amount of sag is 22mm-16mm=6mm (100%). The evaluation was carried out with an amount of sag between 0mm and 2.5mm or less as ◯, with an amount of sag over 2.5mm and 4mm or less as △, and with an amount of sag over 4mm as ×.
[0095] <Overall Judgment> Products that received a score of 〇 for all of the above evaluation items were given an overall rating of 〇; products that received three or less △ ratings but the rest were 〇 were given an overall rating of 〇△ since they may be usable; products that received an × rating for even one rating were given an overall rating of ×.
[0096] [Table 4]
[0097] [Table 5]
[0098] [Table 6]
[0099] As shown in Tables 4 to 6, in the vibration-proof rubber composition containing natural rubber (NR) and butadiene rubber as the main rubber components and containing 10 to 50 parts by mass of fatty acid amide when the total rubber components are 100 parts by mass, the vibration-proof rubber composition containing natural rubber (NR) and butadiene rubber (BR) in a mass ratio of natural rubber / butadiene rubber = 50 / 50 to 10 / 90, containing 0.1 to 0.6 parts by mass of sulfur as a vulcanizing agent, containing 7 to 30 parts by mass of tetrakis (2-ethylhexyl) thiuram disulfide and containing 0.5 to 3.0 parts by mass of N-phenyl-N- (trichloromethylthio) benzenesulfonamide was all rated as fair or fair in the overall judgment (Examples 1 to 16). On the other hand, those in which the mass ratio of natural rubber (NR) and butadiene rubber (BR) was outside the range of 50 / 50 to 10 / 90 natural rubber / butadiene rubber, and those that contained 0.1 to 0.6 parts by mass of sulfur as a vulcanizing agent, 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide, and did not contain 0.5 to 3.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide were given an "X" in the overall assessment.
[0100] [Effects of the Anti-Vibration Rubber Composition of the Present Invention] As described above, the vibration-proof rubber composition of the present invention contains natural rubber (NR) and butadiene rubber as the main rubber components, and contains 10 to 50 parts by mass of fatty acid amide when the total rubber components are 100 parts by mass, and contains natural rubber (NR) and butadiene rubber (BR) in a mass ratio of natural rubber / butadiene rubber = 50 / 50 to 10 / 90, contains 0.1 to 0.6 parts by mass of sulfur as a vulcanizing agent, contains 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide, and contains 0.5 to 3.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide, thereby fully exerting the effect of reducing the friction coefficient, has excellent scorch resistance and therefore good productivity, and has excellent compression set and therefore excellent resistance to sagging, and can obtain a vibration-proof rubber composition with stable rubber strength, and a vibration-proof rubber using the same.
[0101] Although the present invention has been described in detail above only with respect to the specific examples, it will be apparent to those skilled in the art that various modifications are possible within the scope of the technical concept of the present invention, and it is natural that such modifications fall within the scope of the claims. [Industrial Applicability]
[0102] The anti-vibration rubber composition according to the present invention can be suitably used as an anti-vibration rubber such as a stabilizer bushing. [Explanation of symbols]
[0103] 1...Stabilizer bush 2...Hollow part 3…Main body (rubber part) 4…Stabilizer bar 5…Bracket
Claims
1. An anti-vibration rubber composition having natural rubber (NR) and butadiene rubber as main rubber components and containing 10 to 50 parts by mass of a fatty acid amide when the total rubber components are 100 parts by mass, the anti-vibration rubber composition containing natural rubber (NR) and butadiene rubber (BR) in a mass ratio of natural rubber / butadiene rubber = 50 / 50 to 10 / 90, containing 0.1 to 0.6 part by mass of sulfur as a vulcanizing agent, containing 7 to 30 parts by mass of tetrakis(2-ethylhexyl)thiuram disulfide, and containing 0.5 to 3.0 parts by mass of N-phenyl-N-(trichloromethylthio)benzenesulfonamide.
2. 2. The anti-vibration rubber composition according to claim 1, further comprising 0.3 to 5 parts by mass of 2-(4'-morpholinodithio)benzothiazole and / or 4,4'-dithiodimorpholine per 100 parts by mass of the total rubber component.
3. 3. The anti-vibration rubber composition according to claim 1, further comprising 5 to 30 parts by mass of high styrene rubber per 100 parts by mass of the total rubber components.
4. When the total rubber component is 100 parts by mass, the nitrogen adsorption specific surface area is 30 to 100 m 2 4. The anti-vibration rubber composition according to claim 1, further comprising 40 to 80 parts by mass of carbon black having a molecular weight of 1 / g.
5. The butadiene rubber has a cis 1,4-bond content of 90% or more and a Mooney viscosity at 100° C. (ML 1+4 5. The anti-vibration rubber composition according to claim 1, wherein the molecular weight of the polymer is 50 to 75.
6. A vibration-proof rubber obtained by using the vibration-proof rubber composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Reel driving device
JP1978099169A
Vibration-damping rubber composition and vibration-damping rubber using the same
JP1994234886A
Vibrationproof rubber composition and vibrationproof rubber
JP1997302148A
Vibro-isolating device for automobile
JP2000026658A
Rubber vibration insulator composition and rubber vibration insulator obtained from the same
JP2004292678A