Nonwoven fabric for absorbent articles and absorbent articles comprising the same
The air-through nonwoven fabric with heat-sealed portions and molten fibers addresses the adhesiveness issue, ensuring strong bonding and maintaining the integrity of absorbent articles by enhancing adhesiveness.
Patent Information
- Application Number
- JP2022503725
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-27
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-02-25
AI Technical Summary
Existing air-through nonwoven fabrics used in absorbent articles suffer from insufficient adhesiveness, which can compromise the moldability and strength of the absorbent article due to a fluffy surface that reduces adhesion to other constituent members.
An air-through nonwoven fabric with heat-sealed portions and molten fibers having melt traces is developed, ensuring a sufficient number of molten fibers on the surface to enhance adhesiveness, thereby improving bonding with other components.
The enhanced adhesiveness of the nonwoven fabric ensures better bonding with other constituents, maintaining the moldability and strength of the absorbent article.
Smart Images

Figure 0007588633000002 
Figure 0007588633000003 
Figure 0007588633000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonwoven fabric for absorbent articles and an absorbent article including the same. [Background technology]
[0002] Nonwoven fabrics are used in sheet members constituting absorbent articles such as disposable diapers. Various studies have been conducted on the configuration of nonwoven fabrics used in absorbent articles from the viewpoints of softness, texture, and other skin feel, liquid retention, and the like. For example, the present applicant has previously proposed an air-through nonwoven fabric having a first layer and a second layer having a lower density than the first layer, in which the cross section of the fibers contained in the first layer is flat and the long axis direction of the cross section is generally oriented in the planar direction of the nonwoven fabric (Patent Document 1). In such a nonwoven fabric, the average deviation of the surface roughness and the average deviation of the friction coefficient on the surface on the first layer side, as well as the linearity LC and bending rigidity of the compression characteristics are specified within a predetermined range.
[0003] In addition, Patent Document 2 describes a nonwoven fabric used in nonwoven fabric products other than absorbent articles, which contains polyethylene fibers and cellulose-based fibers and has a WC value of 0.50 gf cm / cm according to the KES compression test. 2 The nonwoven fabric is described as having only non-fixed portions at the sites where the fibers contained in the constituent fibers contact each other.
[0004] Furthermore, as a nonwoven fabric processed so that the fiber tips on the surface that comes in contact with the skin are not frayed, Patent Document 3 describes a nonwoven fabric manufactured by applying pressure with a roller to the surface that comes in contact with the skin using a known method such as an air-through method. It is said that the roller is preferably heated to 120 to 130°C, but it is also described that if the roller is heated to 130°C or higher, the thermal melting effect is large, the adhesion range between the fibers becomes wide, and the moisture permeability effect is impaired. Furthermore, Patent Document 4 describes the use of a nonwoven fabric for the outer backsheet, which is manufactured by the air-through method in which heated air is fed during the drum transport process to heat-seal the fibers at 130.5 to 135°C, and in which the engagement areas are brushed, in order to improve the engagement force of the fastening tape with the outer backsheet. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-233364 A [Patent Document 2] JP 2019-90141 A [Patent Document 3] JP 2003-265528 A [Patent Document 4] International Publication No. 2006 / 135011 Summary of the Invention
[0006] The present invention provides an air-through nonwoven fabric that contains thermoplastic fibers and has a plurality of heat-fused parts formed by heat-fusion at intersections of the fibers. The nonwoven fabric of the present invention is preferably a nonwoven fabric for absorbent articles. The nonwoven fabric of the present invention preferably contains molten fibers having melt traces in which the fibrous form has been lost due to melting and solidification of the thermoplastic fibers. The melting trace is preferably formed in a portion other than the heat-sealed portion. On at least one side of the nonwoven fabric for absorbent articles of the present invention, five observation areas of 500 μm x 400 μm are observed at a magnification of 200 times, and the molten fibers having the melt traces present in each observation area are defined as the observed molten fibers.It is preferable that the total number of the observed molten fibers is 5 or more. Other features of the invention will be apparent from the claims and the following description. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is an example of an image of one surface of the nonwoven fabric for absorbent articles of the present invention observed with a scanning electron microscope. [Diagram 2] FIG. 2 is a cross-sectional view showing one embodiment of a melting trace portion according to the present invention. [Diagram 3] FIG. 3 is another example of the observed image corresponding to FIG. [Figure 4] 4(a) to (c) are schematic diagrams illustrating a method for measuring the number of raised fibers per unit area. Detailed Description of the Invention
[0008] A typical air-through nonwoven fabric is formed by blowing gas or water vapor onto a fiber web, and therefore the surface of the nonwoven fabric tends to be fuzzy. When a nonwoven fabric having a fuzzy surface is used as a sheet member of an absorbent article, the fuzz provides a good feel to the touch, but the fuzz tends to reduce adhesion to other components of the absorbent article. If the adhesion is insufficient, the formability or strength of the absorbent article may be reduced. Patent Documents 1 to 4 do not disclose any technology for ensuring sufficient adhesion of the air-through nonwoven fabric.
[0009] The present invention relates to a nonwoven fabric for absorbent articles, which is an air-through nonwoven fabric having excellent adhesiveness, and an absorbent article including the same.
[0010] The present invention will now be described based on preferred embodiments with reference to the drawings. The nonwoven fabric for absorbent articles of this embodiment (hereinafter, simply referred to as "nonwoven fabric") is an air-through nonwoven fabric. "Air-through nonwoven fabric" refers to a nonwoven fabric manufactured through a process (air-through process) in which a fluid having a predetermined temperature or higher, for example, hot air such as air or water vapor, is blown onto a fiber web or nonwoven fabric, which is a precursor of the nonwoven fabric. The blowing of such a fluid is performed by a so-called air-through method (penetration method) in which a fluid such as hot air penetrates the fiber web or nonwoven fabric. The air-through nonwoven fabric of the present invention includes not only nonwoven fabrics manufactured only by a heat treatment process using the air-through method, but also nonwoven fabrics manufactured by adding the heat treatment process to nonwoven fabrics manufactured by other methods, or nonwoven fabrics manufactured by carrying out some process after the air-through process.
[0011] FIG. 1 shows an electron microscope image (observation magnification: 200 times) of one surface of the nonwoven fabric of this embodiment taken in accordance with the <Method for measuring the number of observed molten fibers> described below. The nonwoven fabric of this embodiment, like a normal air-through nonwoven fabric, has a plurality of heat-sealed parts P formed by heat-sealing the intersections of thermoplastic fibers contained as constituent fibers due to its manufacturing method. The parts marked with the symbol P in Fig. 1 are the heat-sealed parts.
[0012] The nonwoven fabric of this embodiment includes molten fibers F1 having melt traces T in which the fiber form is lost due to melt solidification of the thermoplastic fibers. As shown in FIG. 1, the melt traces T are melt solidified parts formed in parts other than the heat fused parts P. That is, the molten fibers F1 have melt solidified parts and non-melted solidified parts in parts other than the heat fused parts P. The melt traces T are parts in which the original shape of the fibers is deformed due to melt solidification. The original shape of the fibers is usually produced by extruding resin from a circular nozzle when manufacturing thermoplastic fibers, so the cross-sectional shape is close to a perfect circle, and at least the cross-sectional shape has a curvature. The nonwoven fabric of this embodiment may include fibers that do not have melt traces T, in addition to the melt fibers F1.
[0013] The nonwoven fabric of this embodiment has two surfaces that are spaced apart in the thickness direction of the nonwoven fabric along a direction perpendicular to the thickness direction of the nonwoven fabric. When the nonwoven fabric of this embodiment is used as a component of an absorbent article, the surface of the nonwoven fabric is usually the surface facing the skin of the wearer of the absorbent article (skin-facing surface), or the surface facing away from the skin of the wearer (non-skin-facing surface) or the surface facing clothing such as shorts (clothing-facing surface).
[0014] For the nonwoven fabric of this embodiment, five observation regions of 500 μm × 400 μm are observed at a magnification of 200 times on at least one of the two surfaces described above. The number of molten fibers F1 (hereinafter also referred to as "observed molten fibers F1") having melt traces T present in each observation region is counted. The total number of observed molten fibers observed in the five observation regions is five or more. Hereinafter, the "total number of observed molten fibers observed in the five observation regions" is simply referred to as the "total number of observed molten fibers." The number of observed molten fibers F1 is measured by the following method.
[0015] <Method for measuring the number of observed molten fibers> For the nonwoven fabric to be measured, a sharp razor is used to cut out an area of 10 mm x 30 mm in plan view over the entire thickness direction, and this is used as the measurement sample. If a sample of this size cannot be taken out, a sample as large as possible is cut out. Three measurement samples are prepared. One side of the measurement sample is photographed at a magnification of 200 times using a scanning electron microscope (SEM, JCM-6000 product name, manufactured by JEOL Ltd., all SEMs in this specification are this type.) to photograph an area of 500 μm x 400 μm. In this SEM photographing, the focus is on the fiber located at the top of the photographed surface of the measurement sample. For one measurement sample, five different positions are photographed to obtain a total of five SEM images. Next, in each SEM image, a fiber in focus is selected, and the molten fiber having a melt trace part is counted from among these fibers. A "fiber in focus" is a fiber whose outline is not blurred within the observation area. Fibers with indistinguishable melt traces are not included in the count. When multiple melt traces T are formed on one fiber, the molten fiber F1 is counted as one. The molten fibers are counted in each SEM image, and the total of these is the total number of observed molten fibers, that is, the total number of molten fibers having melt traces T in the five observation areas. In addition, when the nonwoven fabric to be measured constitutes an absorbent article, the hot melt adhesive is solidified by cold spray or liquid nitrogen, and the nonwoven fabric is carefully peeled off to obtain the nonwoven fabric. This method is common to other measurements in this specification.
[0016] The method of counting the total number of observed molten fibers in each SEM image will be specifically described with reference to FIG. 1. First, the fiber located at the top of the SEM image and the fibers in focus in the image are selected. In FIG. 1, fiber a1 is the fiber located at the top of the SEM image, and the fibers in focus are selected together with the fiber a1. Next, fibers a1 to a6 having melt traces T are selected from the fibers in focus. In FIG. 1, there are four fibers a1, a3, a4, and a6 having one melt trace T, and two fibers a2 and a5 having two melt traces T. Specifically, fiber a2 has melt traces T1 and T2, and fiber a5 has melt traces T3 and T4. The same selection and judgment are performed for all the "fibers in focus" in the same SEM image. Therefore, the total number of observed molten fibers in FIG. 1 is six.
[0017] As described above, the nonwoven fabric of this embodiment has molten fibers F1 on one of its surfaces. The molten fibers F1 on this surface have melt traces T extending in the planar direction. Therefore, when other components of the absorbent article are adjacent to this surface, the contact area with the other components in the planar direction is larger than that of fibers without the melt traces T. As a result, on the surface on which the molten fibers F are present, the adhesion is improved by increasing the contact area between the fibers and other components due to the melt traces T. In particular, when the total number of observed molten fibers is 5 or more, the adhesion area on this surface of the nonwoven fabric can be sufficiently secured, so that this surface has excellent adhesion. When such a nonwoven fabric is used as a component of an absorbent article, the surface on which the total number of observed molten fibers is 5 or more is made to be the contact surface with other components of the absorbent article, so that the nonwoven fabric and other components are well bonded to ensure the moldability or strength of the absorbent article.
[0018] From the viewpoint of further improving the adhesiveness on the adhesive surface of the nonwoven fabric, the total number of observed molten fibers is preferably 5 or more, and more preferably 10 or more. Furthermore, the total number of observed molten fibers is realistically 100 or less, or 50 or less, taking into consideration the number of fibers constituting the nonwoven fabric. The total number of observed molten fibers is preferably 5 or more and 100 or less, and more preferably 10 or more and 50 or less.
[0019] The melt trace T tends to have a flat shape compared to the non-melted and solidified portion, with the melt trace T being flattened. The outline of the cross section perpendicular to the direction in which the molten fiber extends of the melt trace T has a straight line portion a and a curved line portion b, as shown in FIG. 2, for example. This straight line portion a can be a portion extending in the planar direction. That is, the melt trace T has a straight line portion in the outline of its cross section. From the viewpoint of increasing the contact area of the fibers on the adhesive surface of the nonwoven fabric, it is preferable that in the cross-sectional contour of the melt trace portion T, the straight portion a faces outward in the thickness direction of the nonwoven fabric and the curved portion b faces inward in the thickness direction.
[0020] Fig. 3 shows another example of the nonwoven fabric of the present invention, and an image (SEM image) of the observation area of the nonwoven fabric corresponding to Fig. 1 is shown. In the SEM image shown in Fig. 3, the melt trace T in the molten fiber F1 is formed as a wide flat portion compared to the portion that has not melted and solidified. For example, the melt trace T10 in Fig. 3 has an irregular outline and extends outward from the outline of the fiber in the portion that has not melted and solidified. In such a melt trace T10, the outline of the cross section perpendicular to the extension direction of the molten fiber has the above-mentioned straight line portion a and curved portion b (not shown).
[0021] The nonwoven fabric may have a total number of observed molten fibers on either side of the nonwoven fabric of 5 or more. For example, when the total number of observed molten fibers is measured on each of both sides of the nonwoven fabric, it is sufficient that either side has 5 or more fibers. From the viewpoint of texture, it is preferable that the other surface of the nonwoven fabric has 20 or less threads.
[0022] In the nonwoven fabric of this embodiment, molten fibers F1 are present on both sides of the nonwoven fabric, and the total number of observed molten fibers is different on each side. Hereinafter, the side with the greater number of observed molten fibers will be referred to as the first side, and the side with the fewer number of observed molten fibers will be referred to as the second side. In order to have one side of the nonwoven fabric as an adhesive side and the other side softened by fluffing, the ratio of the total number of observed molten fibers on the first side to the second side (first side / second side) is preferably 1.5 times or more, and more preferably 2 times or more. There is no particular upper limit to the ratio, but when the total number of molten fibers observed on the second surface is one or more, it is preferably 10 times or less, and more preferably 5 times or less. Moreover, the ratio is preferably 1.5 times or more and 10 times or less, and more preferably 2 times or more and 5 times or less.
[0023] From the viewpoint of further improving the softness of the second surface, the total number of observed molten fibers on the second surface is preferably 50 or less, more preferably 20 or less, and most preferably 0. That is, the total number of observed molten fibers on the second surface is 0 or more.
[0024] In the nonwoven fabric of this embodiment, the first side has a greater total number of observed molten fibers than the second side, and as a result, the first side has less fuzz than the second side. The degree of fuzz can be evaluated by the number of raised fibers per unit area as follows. The fewer the number of raised fibers per unit area, the less fuzz can be evaluated. From the viewpoint of achieving a better balance between feel and texture, the number of raised fibers per unit area is preferably 20 or less. If the number of such raised fibers is 10 or less, fuzzing is less noticeable in appearance. In addition, from the viewpoint of further improving the adhesiveness, the number of raised fibers per unit area is preferably 5 or less.
[0025] <Measuring method for napped fibers per unit area> FIG. 4 is a schematic diagram showing a method for measuring the number of raised fibers among the fibers constituting a nonwoven fabric under an environment of 22°C and 65% RH. First, a 10 cm x 10 cm test piece 104 is cut out from the nonwoven fabric with a sharp razor. If a 10 cm x 10 cm test piece cannot be cut out from the nonwoven fabric, a 7 cm x 7 cm test piece is used. Next, as shown in FIG. 4(a), the test piece 104 is folded in a mountain shape and placed on an A4 size black mount (not shown). Next, as shown in FIG. 4(b), an A4 size black mount 101 with a hole 107 of 1 cm length x 1 cm width is placed on the test piece 104 on the mount. At this time, the test piece 104 is arranged so that the fold 105 of the test piece 104 is visible from the hole 107 of the upper black mount. For the mounts placed above and below the test piece 104, for example, "Kenran (black) ream weight 265 g" by Fuji Kyowa Paper Co., Ltd. can be used. In FIG. 4, the mount 101 is shown in white for ease of explanation. Next, two 50 g weights 102 are placed on the mount 101 placed on the test piece 104. At this time, the weights 102 are placed on the fold 105 of the test piece 104, at positions 5 cm outward from each of the two side edges of the hole 107 of the mount 101 placed on the test piece 104 in the direction along the fold 105. This brings the test piece 104 into a completely folded state. Next, as shown in FIG. 4(c), the inside of the hole 107 of the mount is observed at a magnification of 30 times using a microscope ("VHX-900" manufactured by Keyence Corporation). Through such observation, the number of fibers whose tips are located above an imaginary line 108 that is moved 1 mm upward in parallel from the fold 105 of the test piece 104 is counted as the number of raised fibers. As shown in Fig. 4(c), when there is a fiber 106a that crosses the virtual line 108 twice, the fiber is counted as two fibers. In the example shown in Fig. 4(c), there are four fibers that cross the virtual line 108 once and one fiber 106a that crosses the virtual line 108 twice, but since the fiber 106a that crosses the virtual line 108 twice is counted as two, the number of raised fibers is six. The number of raised fibers is counted for nine measurement pieces cut out from the nonwoven fabric, and the average (rounded to one decimal place) is calculated as the number of raised fibers per unit area (1 cm x 1 cm).
[0026] From the viewpoint of more reliably ensuring adhesiveness on the first side, the number of raised fibers per unit area on the first side is preferably 10 or less, more preferably 5 or less, and most preferably 0. In other words, the number of raised fibers per unit area on the first side is 0 or more.
[0027] From the viewpoint of suppressing the appearance of fuzz on the second side and further improving the texture of the nonwoven fabric for absorbent articles, the number of raised fibers per unit area on the second side is preferably 20 or less, more preferably 10 or less, provided that the number is greater than that on the first side. Also, the number of raised fibers per unit area on the second side is more than 0.
[0028] From the standpoint of ensuring adhesiveness on the first surface more reliably, the adhesive strength of the first surface is preferably 0.13 N or more, and more preferably 0.15 N or more. Furthermore, the adhesive strength of the first surface is practically 5 N or less, or 3 N or less, and is preferably 0.13 N or more and 5 N or less, and more preferably 0.15 N or more and 3 N or less. The adhesive strength is measured by the following method.
[0029] <Method of measuring adhesive strength> A sharp razor is used to cut out two test pieces from the nonwoven fabric to be measured, each having a planar area of 10 cm x 5 cm across the entire thickness direction. Then, on one side of one of the test pieces, a 5 cm x 5 cm area at one end of the longitudinal direction of the test piece is cut to have a basis weight of 6 g / m 2A hot melt adhesive (rubber-based hot melt, manufactured by Henkel) is applied to the other test piece, and a 2 kg weight is placed on top of it and left to stand for 5 minutes, which is the measurement sample. The surfaces of the two test pieces to be bonded together are made to be the same surface of the nonwoven fabric. Next, each end of the measurement sample where the two test pieces are not bonded together is fixed between the chucks of a Tensilon universal testing machine (manufactured by A&D Co., Ltd., "RTG1310"). The distance between the chucks is 50 mm. Next, the chuck is moved at a speed of 300 mm / min along the 180° direction to peel off the two test pieces. The maximum tensile strength observed at this time is obtained. This measurement is repeated three times, and the average value is taken as the adhesive strength.
[0030] In order to ensure the strength of the nonwoven fabric, the basis weight of the nonwoven fabric is preferably 8 g / m 2 More preferably, 12 g / m 2 That's all. In addition, the basis weight of the nonwoven fabric is preferably 50 g / m 2 Less than or equal to 30 g / m 2 The following is the result. The basis weight of the nonwoven fabric is preferably 8 g / m 2 More than 50g / m 2 Less than 12 g / m, more preferably 2 More than 30g / m 2 The following is the result.
[0031] From the viewpoint of further improving the flexibility of the nonwoven fabric, the average fiber diameter of the constituent fibers of the nonwoven fabric is preferably 20 μm or less, and more preferably 15 μm or less. Furthermore, the average fiber diameter of the constituent fibers of the nonwoven fabric is practically 5 μm or more, and preferably 8 μm or more. The average fiber diameter of the fibers constituting the nonwoven fabric is preferably 5 μm or more and 20 μm or less, and more preferably 8 μm or more and 15 μm or less. The nonwoven fabric may be composed of multiple types of fibers with different fiber diameters, but from the same viewpoint as above, it is preferable that the nonwoven fabric is composed of constituent fibers with a fiber diameter of 20 μm or less. When the nonwoven fabric contains multiple types of fibers with different fiber diameters, the "average fiber diameter" is the average fiber diameter of the constituent fibers in the entire nonwoven fabric.
[0032] The fiber diameter of the constituent fibers of the nonwoven fabric is determined by the following method. The SEM image of the nonwoven fabric obtained in the above-mentioned <Method for measuring the number of observed molten fibers> is used. Ten of the above-mentioned "focused fibers" in the SEM image are arbitrarily selected. Next, for each of these 10 fibers, an arbitrary portion other than the melt trace portion T and the heat fusion portion P is selected, and a line perpendicular to the longitudinal direction of the fiber in the selected portion is drawn. The across-the-board length of the fiber along this perpendicular line is measured as the fiber diameter. This measurement is performed at a position where the across-the-board line indicating the across-the-board length, i.e., the line perpendicular to the longitudinal direction of the fiber and the line indicating the outline of the fiber are perpendicular to each other in the focused fiber. Next, the arithmetic average value of the fiber diameter is calculated for the 10 fibers for each of the total of five SEM images obtained from the measurement sample. The arithmetic average value is calculated for each of both sides of the nonwoven fabric, and the average of these is taken as the average fiber diameter. Even when fibers having different fiber diameters are included, the measurement is performed as described above.
[0033] The nonwoven fabric of the present embodiment is typically mainly composed of thermoplastic fibers, and the proportion of thermoplastic fibers in the total constituent fibers of the nonwoven fabric of the present embodiment is at least 50% by mass, preferably 90% by mass or more, and may be 100% by mass.
[0034] Examples of the constituent resins (thermoplastic resins) of thermoplastic fibers include polyolefins such as polyethylene (PE) and polypropylene (PP); polyesters such as polyethylene terephthalate (PET); polyamides such as nylon 6 and nylon 66; polyacrylic acid alkyl esters, polymethacrylic acid alkyl esters, polyvinyl chloride, polyvinylidene chloride, etc., and these can be used alone or in combination of two or more.
[0035] The synthetic fibers, including the thermoplastic fibers, used in the nonwoven fabric of this embodiment may be single fibers made of one type of synthetic resin or a blend polymer made by mixing two or more types of synthetic resins, or may be composite fibers. The composite fibers referred to here are synthetic fibers obtained by combining two or more types of synthetic resins with different components in a spinneret and spinning them simultaneously, and each of the components has a structure in which they are continuous in the length direction of the fiber and are mutually bonded within the single fiber. Examples of the form of the composite fiber include a core-sheath type having a core-sheath structure consisting of a core and a sheath, and a side-by-side type.
[0036] From the viewpoint of further improving the flexibility of the nonwoven fabric, the thermoplastic fibers preferably contain polyethylene as a constituent resin, more preferably contain polyethylene at least on the surface, and further preferably consist of polyethylene. For example, when the thermoplastic fiber includes a fiber having a core-sheath structure, a preferred example of the thermoplastic fiber is one in which the resin component of the core is one or more selected from the group consisting of PE and PP, and the resin component of the sheath is PE. In particular, it is preferred that the resin component of the core is PET, and the resin component of the sheath is PE.
[0037] The nonwoven fabric of the present embodiment may contain, in addition to the thermoplastic fibers, other fibers other than the thermoplastic fibers. Examples of such other fibers include natural fibers such as pulp and cotton, and cellulosic fibers such as rayon, lyocell, and tencel. These fibers may be used alone or in combination of two or more. In order to further improve the flexibility of the nonwoven fabric, the nonwoven fabric preferably contains cotton as a natural fiber. From the same viewpoint as above, the nonwoven fabric preferably contains, as the cellulosic fiber, one or more types selected from the group consisting of rayon and Tencel.
[0038] From the viewpoint of further improving the flexibility and strength of the nonwoven fabric, the contents of the other fibers and the thermoplastic fibers in the nonwoven fabric are preferably within the following ranges. The ratio of the content of the other fibers to the total content of the other fibers and the thermoplastic fibers in the nonwoven fabric is preferably 0.1% or more, and more preferably 1% or more. Moreover, the ratio is preferably 20% or less, and more preferably 10% or less. Moreover, the ratio is preferably 0.1% or more and 20% or less, and more preferably 1% or more and 10% or less. This ratio is the mass of other fibers in all the constituent fibers of the nonwoven fabric divided by the combined mass of other fibers and thermoplastic fibers in all the constituent fibers of the nonwoven fabric (mass %).
[0039] The nonwoven fabric of the present embodiment is for absorbent articles and is used as a constituent member of absorbent articles. The term "absorbent article" as used herein broadly includes articles used to absorb body fluids discharged from the human body (urine, loose stool, menstrual blood, sweat, etc.), such as disposable diapers, sanitary napkins, sanitary shorts, and incontinence pads.
[0040] An absorbent article typically comprises a liquid-permeable top sheet arranged relatively close to the wearer's skin, a liquid-impermeable or poorly liquid-permeable or water-repellent back sheet arranged relatively far from the wearer's skin, and a liquid-retentive absorbent interposed between the two sheets. The absorbent article may also comprise an exterior body forming the outer surface thereof. The nonwoven fabric of the present embodiment is preferably provided as a component of an absorbent article. From the viewpoint of more reliably ensuring the moldability or strength of the absorbent article, it is preferable that the nonwoven fabric is arranged so that the surface on which the total number of observed molten fibers is 5 or more is the adhesive surface to be bonded to other components.
[0041] The nonwoven fabric of this embodiment is also suitable as a component that can come into direct contact with the wearer's skin because the second side is more fluffy than the first side. For example, it is suitable as a back sheet or exterior body that forms the outer surface of an absorbent article. In this case, the nonwoven fabric is arranged so that the side with the total number of observed molten fibers of 5 or more, more preferably the first side, faces the non-skin facing side in the absorbent article.
[0042] In addition, an absorbent article using the nonwoven fabric of this embodiment may include the nonwoven fabric as either or both of the top sheet and the back sheet. From the viewpoint of more reliably ensuring the formability or strength of the absorbent article, it is preferable that the absorbent article includes the nonwoven fabric of this embodiment as the back sheet. In this case, from the viewpoint of more reliably ensuring the leakproofness, it is preferable that the back sheet is made of a laminated sheet of a liquid-impermeable sheet and the nonwoven fabric.
[0043] The nonwoven fabric of this embodiment basically consists of a single layer of nonwoven fabric obtained by the air-through method, but when used as a component of an absorbent article, it may be in a laminated state with other sheet materials including other nonwoven fabrics and films.
[0044] Next, a method for producing the nonwoven fabric according to the embodiment described above will be described. This method includes a heat treatment step of blowing hot air onto a fiber web containing thermoplastic fibers by an air-through method. The heat treatment step is a step of fusing intersections between constituent fibers of the fiber web to form heat-fused portions, thereby producing a nonwoven fabric.
[0045] A fibrous web is typically produced by opening raw fibers such as thermoplastic fibers with a fiber opening machine and forming the opened raw fibers into a web with a carding machine. The raw fibers, i.e., the constituent fibers of the fibrous web, are preferably the same as the constituent fibers of the nonwoven fabric described above. The basis weight of the fibrous web is preferably within the basis weight range of the nonwoven fabric described above. The fiber web may be formed by laminating or mixing a plurality of types of fibers having different fiber diameters.
[0046] The obtained fiber web is placed on, for example, a resin mesh belt, a metal edgeless net made of wire mesh, a metal plate with air holes, or a metal plate without air holes, and hot air or steam is blown onto the fiber web side to thermally fuse the intersections of the fibers. As a result, the obtained nonwoven fabric has two surfaces: a surface facing the plate or net (hereinafter also referred to as the non-blowing surface) and a surface onto which hot air is blown (hereinafter also referred to as the blowing surface). Of these two surfaces of the nonwoven fabric, a large amount of molten fibers F1 is formed on one surface, which becomes the first surface, and the other surface becomes the second surface. Typically, the blowing surface becomes the first surface, and the non-blowing surface becomes the second surface.
[0047] The temperature of the hot air in a typical air-through process is set to a range of about 10°C higher than the lowest melting point of the constituent fibers in the fiber web (for example, the melting point of the sheath portion of a core-sheath composite fiber), but from the viewpoint of more easily forming the melt trace portion T, the temperature difference between the hot air temperature and the lowest melting point of the constituent fibers is preferably 5°C or more, more preferably 10°C or more. Furthermore, the temperature difference between the hot air temperature and the lowest melting point of the constituent fibers is preferably 70° C. or less, more preferably 50° C. or less, in practice. The temperature difference between the hot air temperature and the minimum melting point of the constituent fibers is preferably 5°C or more and 70°C or less, more preferably 10°C or more and 50°C or less. In addition, the lowest melting point of the constituent fibers refers to the melting point of the resin with the lowest melting point when the fiber contains multiple types of resins, such as core-sheath type composite fibers. In the case of a resin that does not have a clear melting point, it refers to the softening point.
[0048] From the viewpoint of more easily forming a nonwoven fabric having the molten fibers F1, the wind speed of the hot air blown onto the fiber web in the heat treatment step is preferably within the following range. The speed of the hot air blown onto the fiber web in the heat treatment step is preferably 0.3 m / sec or more, more preferably 0.5 m / sec or more, and even more preferably 0.8 m / sec or more. The speed of the hot air is preferably 10 m / sec or less, more preferably 5 m / sec or less, and further preferably 3 m / sec or less.
[0049] In the heat treatment step, the time for blowing hot air onto the fiber web (heat treatment time) may be similar to that in the conventional manufacturing method of air-through nonwoven fabrics, but from the same viewpoint as above, the heat treatment time is preferably 1 second or more, more preferably 3 seconds or more. From the viewpoint of increasing the production speed as much as possible and reducing the production costs, the heat treatment time is preferably 60 seconds or less, and more preferably 30 seconds or less. The heat treatment time is preferably from 1 to 60 seconds, more preferably from 3 to 30 seconds.
[0050] In the heat treatment step, instead of blowing hot air onto the fiber web, a treatment may be performed in which only one side of the fiber web is heated to a high temperature and pressure is applied from the other side. For example, such a treatment method may be a method in which the fiber web is placed on a hot plate and pressure is applied from the side opposite to the hot plate. Such a treatment method may employ a configuration similar to that of the high-temperature pressurization step described later.
[0051] The nonwoven fabric obtained by the heat treatment step may further be subjected to a high-temperature pressurizing step in which it is heated and pressed in its thickness direction. With such a configuration, the melt traces T can be easily formed. The high-temperature pressurizing step may be performed, for example, by pressing the nonwoven fabric between two heated metal plates. In this case, the nonwoven fabric may be subjected to a pressure load from both of the two plates, or from only one of the plates.
[0052] From the same viewpoint as above, the high-temperature pressurization step is preferably carried out under the following conditions. The heating temperature of the nonwoven fabric in the high-temperature pressurizing step is preferably 120°C or higher, more preferably 130°C or higher, even more preferably 135°C or higher, still more preferably 136°C or higher, and even more preferably 140°C or higher. The heating temperature of the nonwoven fabric is preferably 180° C. or lower, and more preferably 160° C. or lower. The heating temperature of the nonwoven fabric is preferably 120°C or higher and 180°C or lower, more preferably 130°C or higher and 160°C or lower, even more preferably 135°C or higher and 160°C or lower, still more preferably 136°C or higher and 160°C or lower, and even more preferably 140°C or higher and 160°C or lower. The heating temperature is set to the temperature of, for example, one of two metal plates that applies a pressure load to the nonwoven fabric.
[0053] The pressure load applied to the nonwoven fabric in the high-temperature pressing step is preferably 15 N / cm 2 More preferably, 30N / cm 2 That's all. The pressure load is preferably 200 N / cm 2 Less than or equal to 100N / cm 2 The following is the result. The pressure load is preferably 15 N / cm 2 More than 200N / cm 2 Less than or equal to 30N / cm 2 More than 100N / cm 2 The following is the result. The treatment time for which the nonwoven fabric is heated and pressed in the high-temperature pressurizing step is preferably 2 seconds or more, and more preferably 3 seconds or more. Moreover, the treatment time is preferably 10 seconds or less, and more preferably 8 seconds or less. The treatment time is preferably from 2 to 10 seconds, more preferably from 3 to 8 seconds.
[0054] Although the present invention has been described above based on the preferred embodiment, the present invention is not limited to the above embodiment and can be modified as appropriate. The above-described embodiments may also be combined. For example, in the nonwoven fabric in the above-described embodiment, the molten fibers F1 are present on both sides thereof, but the molten fibers F1 may be present on only one side thereof.
[0055] In the present specification, when an upper limit or lower limit or upper and lower limits of a numerical value are specified, the upper limit and lower limit values themselves are included. In addition, even if not specifically stated, it is understood that all numerical values or numerical ranges below the upper limit or above the lower limit, or within the range of the upper and lower limits, are described. As used herein, "a" and "an" and the like are intended to mean one or more. In light of the above disclosure in this specification, it is understood that various modifications and variations of the present invention are possible. Therefore, it should be understood that the present invention can be practiced in embodiments not expressly described in this specification within the technical scope based on the description of the claims. The contents of the above-mentioned patent documents are incorporated herein in their entirety as part of the content of this specification. EXAMPLES
[0056] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to such examples.
[0057] Example 1 As the raw fiber, a thermoplastic fiber of 2.0 dtex was used, which was a concentric core-sheath type composite fiber (core-sheath ratio 50% by mass:50% by mass) with a core component of PET and a sheath component of PE. Such raw fiber had a minimum melting point of 120°C. Using this raw fiber, a fiber web was produced in a conventional manner using a known carding machine, and the fiber web was placed on a metal plate previously heated to 136°C, and a heat treatment step was performed in which hot air was blown onto the fiber web using an air-through method to produce an air-through nonwoven fabric. The heat treatment conditions in the heat treatment step (air-through treatment) were as shown in Table 1.
[0058] Example 2 An air-through nonwoven fabric was produced on a resin mesh belt using the same fibers as in Example 1. Then, a high-temperature pressurizing step was carried out. The processing conditions for the high-temperature pressurizing step were as shown in Table 1. In the high-temperature pressurizing step, the nonwoven fabric was placed on a metal plate heated to 150°C with the sprayed surface facing down, and then a metal weight was placed on top of the nonwoven fabric and a pressure of 30 cN / cm was applied. 2 Pressure was applied for 5 seconds.
[0059] Example 3 An air-through nonwoven fabric was produced by carrying out a high-temperature pressurizing step after the heat treatment step in the same manner as in Example 2, except that raw fibers having different finenesses were used.
[0060] Example 4 An air-through nonwoven fabric was produced by carrying out a high-temperature pressurizing step after the heat treatment step in the same manner as in Example 2, except that the speed and temperature of the hot air were changed.
[0061] Example 5 A fiber web (hereinafter referred to as "1.2 dtex fiber web") formed of 1.2 dtex thermoplastic fiber consisting of concentric core-sheath composite fibers (core-sheath ratio 50% by mass:50% by mass) with a core component being PET and a sheath component being PE, and a fiber web (hereinafter referred to as "2.0 dtex fiber web") formed of 2.0 dtex thermoplastic fiber consisting of concentric core-sheath composite fibers (core-sheath ratio 50% by mass:50% by mass) with a core component being PET and a sheath component being PE were prepared, and laminated in a mass ratio of 1.2 dtex fiber web:2.0 dtex fiber web = 2:3 to produce a laminated web. The fiber diameter of the raw fiber of the 1.2 dtex fiber web was 11.9 μm, and the fiber diameter of the raw fiber of the 2.0 dtex fiber web was 15.2 μm. Except for using this laminated web, an air-through nonwoven fabric was produced by carrying out a high-temperature pressurizing step after the heat treatment step in the same manner as in Example 4. In the heat treatment step, the heat treatment was carried out so that the 2.0 dtex fiber web side of the laminated web became the blown surface.
[0062] Example 6 An air-through nonwoven fabric was produced in the same manner as in Example 4, except that raw fibers having different finenesses were used.
[0063] Example 7 A fiber web was produced using the same fibers as in Example 3, and further blending cotton manufactured by Marusan Sangyo Co., Ltd. at 1 / 12 of the mass of the core-sheath composite fiber. Then, in the same manner as in Example 4, a heat treatment process and a high-temperature pressurization process were carried out to produce an air-through nonwoven fabric.
[0064] Example 8 A fiber web was produced using the same fibers as in Example 1, and further mixed with Marusan Sangyo cotton at 1 / 12 of the mass of the core-sheath composite fiber. Then, in the same manner as in Example 4, a heat treatment process and a high-temperature pressurization process were carried out to produce an air-through nonwoven fabric.
[0065] Comparative Example 1 In Comparative Example 1, except that raw fibers having different fineness were used, an air-through nonwoven fabric was produced in the same manner as in Example 1. The fiber diameter of the raw fibers in Comparative Example 1 was 15.5 μm.
[0066] [Comparative Examples 2 and 3] In Comparative Example 2, an air-through nonwoven fabric was produced in the same manner as in Example 4, except that the high-temperature pressurization step was not performed. In Comparative Example 3, an air-through nonwoven fabric was produced in the same manner as in Example 6.
[0067] Comparative Example 4 An air-through nonwoven fabric was produced in the same manner as in Comparative Example 2, except that the same laminated web as in Example 5 was used.
[0068] Comparative Examples 5 and 6 In Comparative Example 5, an air-through nonwoven fabric was produced in the same manner as in Example 6, except that the high-temperature pressurization process was not performed. In Comparative Example 6, an air-through nonwoven fabric was produced in the same manner as in Example 4, but with a reduced basis weight.
[0069] The fiber diameters of the nonwoven fabrics of the Examples and Comparative Examples, measured according to the above-mentioned method, are shown in Table 1. For Examples (e.g., Examples 1 and 2) and Comparative Examples using the same raw fibers, the fiber diameters in Table 1 may differ slightly, but this is due to slight deviations in the actual measured values. The total number of observed molten fibers was measured by the above-mentioned method for both sides of the air-through nonwoven fabric of the examples and comparative examples, that is, the non-sprayed side and the sprayed side. In addition, for the total number of observed molten fibers in Example 1, Comparative Example 2, Comparative Example 5, and Comparative Example 6, the number of times the non-sprayed side was compared to the sprayed side was calculated as the ratio of the number of molten fibers. In Examples 2 to 8, Comparative Example 1, Comparative Example 3, and Comparative Example 4, the number of times the sprayed side was compared to the non-sprayed side was calculated as the ratio of the number of molten fibers. Furthermore, the non-sprayed side was used as the adhesive side in Example 1, and the sprayed side was used as the adhesive side in the other examples, and the adhesive strength was measured by the above-mentioned method. These measurement results are shown in Table 1.
[0070] The number of raised fibers per unit area was measured using the method described above for the sprayed and non-sprayed surfaces of the air-through nonwoven fabrics of the Examples and Comparative Examples. The results are shown in Table 1.
[0071] [Table 1]
[0072] As shown in Table 1, the air-through nonwoven fabric of each Example had a total number of observed molten fibers of 5 or more on either the sprayed or non-sprayed surface, resulting in a small number of raised fibers per unit area on the sprayed surface. On the other hand, the air-through nonwoven fabric of each Comparative Example had a total number of observed molten fibers of less than 5 on either the sprayed or non-sprayed surface. Furthermore, in the Examples having a surface with a total number of observed molten fibers of 5 or more, the adhesive strength of the adhesive surface was higher than that of the Comparative Examples. These results show that the nonwoven fabrics in the Examples have a surface with excellent adhesiveness. [Industrial Applicability]
[0073] According to the present invention, it is possible to provide a nonwoven fabric for absorbent articles, which is an air-through nonwoven fabric having excellent adhesiveness, and an absorbent article including the same.
Claims
1. An absorbent article comprising, as a constituent member, a nonwoven fabric for absorbent articles, the nonwoven fabric being made of an air-through nonwoven fabric containing thermoplastic fibers and having a plurality of heat-fused portions formed by heat-fusion at intersections of the fibers, The nonwoven fabric for absorbent articles is The thermoplastic fiber includes molten fibers having melt traces that have lost their fiber shape due to melting and solidification of the thermoplastic fiber, The melt trace portion of the molten fiber is formed in a portion other than the heat-sealed portion, five observation regions of 500 μm×400 μm are observed at a magnification of 200 times on each of the first and second surfaces of the nonwoven fabric for absorbent articles, and the molten fibers having the melt traces present in each observation region are regarded as observed molten fibers. The observed molten fibers are present on each of the first and second surfaces, The total number of the observed molten fibers on the first surface is 5 or more, and is 1.5 times or more and 10 times or less than that on the second surface; An absorbent article, wherein the first surface is arranged to be an adhesive surface for bonding to other components.
2. The absorbent article according to claim 1 , wherein the melt trace has a cross-sectional profile perpendicular to the direction in which the molten fiber extends, the cross-sectional profile having straight and curved portions.
3. The absorbent article according to claim 2 , wherein the straight portions face outward in a thickness direction of the nonwoven fabric for absorbent articles, and the curved portions face inward in the thickness direction.
4. The absorbent article according to any one of claims 1 to 3, wherein the average fiber diameter of the constituent fibers is 5 µm or more and 20 µm or less.
5. The absorbent article according to any one of claims 1 to 4, wherein the thermoplastic fibers include core-sheath type composite fibers having a core-sheath structure consisting of a core and a sheath.
6. 6. The absorbent article according to claim 5, wherein the resin component of the core is polyethylene terephthalate, and the resin component of the sheath is polyethylene.
7. The absorbent article according to any one of claims 1 to 6, further comprising fibers other than the thermoplastic fibers, the other fibers being cellulosic fibers or natural fibers.
8. The absorbent article according to claim 7 , wherein a ratio of a content of the other fibers to a total content of the other fibers and the thermoplastic fibers is 0.1% or more and 20% or less.
9. The absorbent article according to any one of claims 1 to 8, wherein the first surface has an adhesive strength of 0.13 N or more and 5 N or less.
10. An absorbent article described in any one of claims 1 to 9, wherein the first side has less fuzz than the second side.
11. The absorbent article according to any one of claims 1 to 10, comprising the nonwoven fabric for absorbent articles as an exterior body forming the outer surface of the absorbent article, and the first surface is arranged to face the non-skin facing surface.
12. The device comprises a top sheet, a back sheet, and an absorbent disposed between the top sheet and the back sheet, The absorbent article according to any one of claims 1 to 11, comprising the nonwoven fabric for absorbent articles as either or both of the top sheet and the back sheet.
13. The absorbent article according to claim 12, comprising the nonwoven fabric for absorbent articles as the back sheet.
14. The absorbent article according to claim 13, wherein the back sheet is a laminated sheet of a liquid-impermeable sheet and the nonwoven fabric for absorbent articles.
Citation Information
Patent Citations
Disposable paper diaper
JP2003265528A
Nonwoven fabric
JP2006233364A
Non-woven fabric and face mask made of the non-woven fabric
JP2019090141A
Disposable diaper
WO2006135011A1