Semiconductor Optical Device

The semiconductor optical device enhances vertical optical confinement through a recessed mesa structure, addressing the issue of insufficient vertical confinement to achieve high-speed modulation and improved transmission characteristics.

JP7588722B2Active Publication Date: 2024-11-22MITSUBISHI ELECTRIC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023533022
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-09
Publication Date
2024-11-22
Estimated Expiration
2041-07-09

AI Technical Summary

Technical Problem

Existing semiconductor optical devices face challenges in achieving high-speed modulation due to insufficient vertical optical confinement, leading to relaxation oscillation frequencies that are lower than the cutoff frequency of the light-receiving side low-pass filter, which results in deteriorated transmission characteristics.

Method used

The semiconductor optical device incorporates a striped mesa structure with a recessed design that increases vertical optical confinement by reducing the thickness of the ridge upper cladding layer, allowing for higher relaxation oscillation frequencies through enhanced light confinement in the active layer.

Benefits of technology

The increased vertical optical confinement enables high-speed modulation capabilities by elevating the relaxation oscillation frequency, resulting in improved transmission characteristics and reduced loss from laser light absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588722000002
    Figure 0007588722000002
  • Figure 0007588722000003
    Figure 0007588722000003
  • Figure 0007588722000004
    Figure 0007588722000004
Patent Text Reader

Abstract

A semiconductor optical element according to the present disclosure comprises: a ridge structure (10) that includes a cladding layer (11) of a first conductivity type and an active layer (12) and is provided on a semiconductor substrate (5) of the first conductivity type; an embedding structure (20) provided on both side surfaces of the ridge structure (10); a cladding layer (30) of a second conductivity type and a contact layer (40) of the second conductivity type provided on the surface of the embedding structure (20); a ridge upper cladding layer (31) of the second conductivity type provided above the ridge structure (10); a recess (51) of which the bottom surface is the upper surface of the ridge upper cladding layer (31) and the side surfaces are the cladding layer and the contact layer of the second conductivity type; a mesa structure (50) in which both side surfaces are formed by a mesa reaching from the contact layer (40) to the semiconductor substrate (5); and an insulation film (60) covering the bottom surface and both side surfaces of the recess (51), the contact layer (40), and both side surfaces of the mesa structure (50).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to semiconductor optical devices. [Background technology]

[0002] In recent years, the amount of data traffic in mobile communication systems has been increasing rapidly. To process this huge amount of data at high speed, even higher speed operation is required for semiconductor optical elements, such as semiconductor lasers, which serve as light sources.

[0003] Patent Document 1 discloses an optical semiconductor device in which a buried region is formed covering both side surfaces of an active layer. The optical semiconductor device described in Patent Document 1 has a mesa structure in which buried regions made of, for example, an iron-doped AlInAs (aluminum indium arsenide) semiconductor are provided on both side surfaces of a ridge structure having an active layer and cladding layers provided on the upper and lower surfaces of the active layer. In such an element structure, the buried regions can confine the current injected into the active layer, and can also increase the optical confinement in the lateral direction of the active layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-286032 A Summary of the Invention [Problem to be solved by the invention]

[0005] When using a semiconductor optical element as a light source for optical communication with high-speed modulation, the relaxation oscillation frequency of the semiconductor optical element must be higher than the cutoff frequency of the low-pass filter on the light receiving side. The relaxation oscillation frequency f r Generally, there is a proportional relationship as shown in the following equation (1).

[0006]

number

[0007] In equation (1), Γ is the optical confinement factor, L is the cavity length, W is the active layer width, d is the active layer thickness, q is the elementary charge, dg / dN is the differential gain, and η i is the internal quantum efficiency, I op is the operating current, I th and represent the threshold current. As can be seen from equation (1), the larger the optical confinement factor Γ, the higher the relaxation oscillation frequency f r will be higher.

[0008] In the element structure of the optical semiconductor device described in Patent Document 1, the buried regions formed on both sides of the ridge structure increase the optical confinement in the lateral direction of the active layer, thereby increasing the relaxation oscillation frequency f r However, the optical confinement in the vertical direction of the active layer is not sufficient. r When the frequency of the relaxation oscillation is lower than the cutoff frequency of the low-pass filter on the light-receiving side, the relaxation oscillation cannot be completely cut off by the low-pass filter, resulting in a problem of deterioration of the transmission characteristics.

[0009] The present disclosure has been made to solve the above-mentioned problems, and aims to obtain a semiconductor optical element capable of high-speed modulation by increasing the optical confinement in the active layer in the vertical direction, thereby increasing the relaxation oscillation frequency. [Means for solving the problem]

[0010] The semiconductor optical device disclosed in the present application is a semiconductor substrate of a first conductivity type; a striped ridge structure including a first conductivity type cladding layer and an active layer provided on the first conductivity type semiconductor substrate; a buried structure buried so as to cover both side surfaces of the ridge structure; a ridge upper cladding layer of a second conductivity type provided on an upper portion of the ridge structure; a cladding layer of a second conductivity type and a contact layer of a second conductivity type provided on a surface of the buried structure; a stripe-shaped recess provided in the second conductivity type cladding layer and the second conductivity type contact layer, the bottom surface of which is the upper surface of the ridge upper cladding layer and the side surfaces of which are the second conductivity type cladding layer and the second conductivity type contact layer; a striped mesa structure including the ridge structure, both side surfaces of which are formed by a mesa extending from the second conductive type contact layer to the first conductive type semiconductor substrate; an insulating film covering a bottom surface and side surfaces of the recess, a surface of the second conductive type contact layer, and both side surfaces of the mesa structure; Equipped with. Effect of the Invention

[0011] In the semiconductor optical device disclosed in the present application, the recess provided in the mesa structure enables the layer thickness of the ridge upper cladding layer provided on the upper part of the active layer to be thinner than the cladding layers provided other than on the upper part of the active layer, thereby increasing the optical confinement in the active layer in the vertical direction and increasing the relaxation oscillation frequency, thereby obtaining a semiconductor optical device capable of high-speed modulation. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic view of a semiconductor optical device according to a first embodiment. [Diagram 2] 1 is a cross-sectional view of a semiconductor optical device according to a first embodiment taken along a direction perpendicular to a resonator. [Diagram 3] 4 is a diagram showing the dependence of the optical confinement factor on the thickness of the ridge upper cladding layer in the semiconductor optical device according to the first embodiment. FIG. [Figure 4] 2 is a cross-sectional view taken along a direction perpendicular to a resonator in a semiconductor optical device according to a first modification of the first embodiment. [Diagram 5] 11 is a cross-sectional view of a semiconductor optical device according to a second modification of the first embodiment, taken along a direction perpendicular to a resonator. FIG. [Figure 6]11 is a cross-sectional view of a semiconductor optical device according to a third modification of the first embodiment, taken along a direction perpendicular to a resonator. FIG. [Figure 7] 11 is a cross-sectional view of a semiconductor optical device according to a second embodiment taken along a direction perpendicular to a resonator. FIG. [Figure 8] 11 is a cross-sectional view of a semiconductor optical device according to a third embodiment taken along a direction perpendicular to a resonator. FIG. [Figure 9] FIG. 11 is a schematic view of a semiconductor optical device according to a fourth embodiment. [Figure 10] 11 is a cross-sectional view of a ridge structure including a recess in a semiconductor optical device according to a fourth embodiment, taken along a direction parallel to the cavity direction. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Embodiment 1 FIG. 1 is a schematic view of a semiconductor optical device 100 according to the first embodiment, and FIG. 2 is a cross-sectional view of the semiconductor optical device 100 in a direction perpendicular to a resonator. The semiconductor optical device 100 according to the first embodiment includes a striped ridge structure 10 including an n-type InP cladding layer 11 (cladding layer of a first conductivity type) and an active layer 12 which are sequentially stacked on an n-type InP (indium phosphide) substrate 5 (semiconductor substrate of a first conductivity type), a buried structure 20 including a p-type InP first buried layer 21 (first buried layer of a second conductivity type) and an n-type InP second buried layer 22 (second buried layer of a first conductivity type) which are formed so as to fill both side surfaces of the striped ridge structure 10, a p-type InP ridge upper cladding layer 31 (ridge upper cladding layer of a second conductivity type) provided on the upper portion of the ridge structure 10, a p-type InP cladding layer 30 (cladding layer of a second conductivity type) and a p-type InGaAsP (indium gallium arsenide phosphide) provided on the upper portion of the buried structure 20, and The p-type InP cladding layer 30 and the p-type InGaAsP contact layer 40 are provided with a stripe-shaped recess 51 having a bottom surface formed by the top surface of the p-type InP ridge upper cladding layer 31 and side surfaces formed by the p-type InP cladding layer 30 and the p-type InGaAsP contact layer 40, and the ridge structure 10, both side surfaces of which are formed by a mesa extending from the p-type InGaAsP contact layer 40 to the n-type InP substrate 5. The semiconductor device is composed of a striped mesa structure 50, an insulating film 60 covering the bottom and side surfaces of the recess 51, the surface of the p-type InGaAsP contact layer 40, and both side surfaces of the mesa structure 50, a striped insulating film opening 61 provided in the insulating film 60 on the p-type InGaAsP contact layer 40, a p-side electrode 70 (second conductive side electrode) in contact with the p-type InGaAsP contact layer 40 at the insulating film opening 61, and an n-side electrode 72 (first conductive side electrode) provided on the back surface side of the n-type InP substrate 5.

[0014] In the semiconductor optical device 100 of embodiment 1, the embedded structure 20 increases the optical confinement in the lateral direction of the active layer 12, i.e., in the direction parallel to the surface of the n-type InP substrate 5, and in addition, the presence of the recess 51 increases the optical confinement in the vertical direction of the active layer 12, i.e., in the direction perpendicular to the surface of the n-type InP substrate 5, thereby achieving the effect of increasing the relaxation oscillation frequency of the semiconductor optical device 100.

[0015] The semiconductor optical device 100 according to the first embodiment further has a device structure in which a p-side electrode 70 is provided on the upper surface of the striped mesa structure 50, the p-side electrode being in contact with the p-type InGaAsP contact layer 40 through the insulating film opening 61 formed laterally along the recess 51. This makes it possible to set a long distance between the active layer 12 and the p-type InGaAsP contact layer 40, thereby suppressing loss caused by absorption of the laser light emitted from the active layer 12 in the p-type InGaAsP contact layer 40.

[0016] An example of a method for manufacturing the semiconductor optical device 100 according to the first embodiment will be described below. First, the carrier concentration of the doped silicon (Si) is 4.0×10 18 cm -3 The n-type InP substrate 5 has a (001) crystal plane on its main surface, and the n-type InP substrate 5 has a carrier concentration of 4.0×10 18 cm -3 An n-type InP cladding layer 11 having a thickness of 0.5 μm and an active layer 12 made of an AlGaInAs (Aluminum Gallium Indium Arsenide)-based or InGaAsP-based semiconductor material having a thickness of 0.2 μm are sequentially grown by a crystal growth method such as Metal Organic Chemical Vapor Deposition (MOCVD) or Molecular Beam Epitaxy (MBE) (first crystal growth step).

[0017] The material of the n-type InP cladding layer 11 is not limited to InP, but may be any InP-based semiconductor material.

[0018] In the above-mentioned device structure, the active layer 12 may include a multiple quantum well structure. Also, light confinement layers made of AlGaInAs-based or InGaAsP-based semiconductor materials having a refractive index set larger than that of the n-type InP cladding layer 11 may be provided on the upper and lower surfaces of the active layer 12. Also, although an example of an InP-based semiconductor material has been given in the above description, a GaAs (Gallium Arsenide)-based or GaN (Gallium Nitride)-based semiconductor material may also be used.

[0019] After the crystal growth of each of the above layers, an insulating material such as SiO2 (silicon dioxide) is formed on the surface of the active layer 12. Examples of methods for forming the SiO2 film include vacuum deposition, CVD (Chemical Vapor Deposition), and sputtering. After the SiO2 film is formed, it is patterned into a striped SiO2 film having a desired width and extending in the resonator direction using photolithography and etching techniques. The striped SiO2 film functions as an etching mask for forming the ridge structure 10. The etching mask is not limited to a SiO2 film, and may be a SiN (silicon nitride) film.

[0020] Using an etching mask made of a SiO2 film, etching is performed to a depth reaching the n-type InP substrate 5 or the n-type InP cladding layer 11 to form a ridge structure 10 having a width of 1.2 μm (ridge structure formation process). As an etching method, dry etching is preferable, but wet etching may also be used.

[0021] After the formation of the ridge structure 10, Zn (zinc) was doped to cover both side surfaces of the ridge structure 10 to a carrier concentration of 5.0×10 17 cm -3 and a p-type InP first buried layer 21 doped with Si with a carrier concentration of 6.0×10 18 cm -3The n-type InP second burying layer 22 and the n-type InP second burying layer 23 are sequentially grown by MOCVD or the like to form the burying structure 20 (second crystal growth step).

[0022] The material of the p-type InP first buried layer 21 is not limited to InP, but may be any InP-based semiconductor material. The same is true for the n-type InP second buried layer 22.

[0023] Each buried layer of the buried structure 20 may be made of a semi-insulating material such as InP doped with Ru (Ruthenium) or Fe (Iron, Ferrum). The configuration of the buried structure 20 is not limited to the above-mentioned two-layer configuration, and may be semiconductor layers with different carrier concentrations or electrical conductivities, or a laminated body combining a plurality of these semiconductor layers. After the crystal growth of the buried structure 20, the striped SiO2 film is removed by dry etching or the like.

[0024] Next, the top of the ridge structure 10 and the surface of the buried structure 20 are doped with Zn to a carrier concentration of 1.0×10 18 cm -3 The p-type InP cladding layer 30 has a thickness of 2.0 μm and is doped with Zn to have a carrier concentration of 1.6×10 19 cm -3 Then, a p-type InGaAsP contact layer 40 having a thickness of 0.3 μm is successively grown by crystal growth using a method such as MOCVD (third crystal growth step).

[0025] The material of the p-type InP cladding layer 30 is not limited to InP, but may be any InP-based semiconductor material, and the material of the p-type InGaAsP contact layer 40 is not limited to InGaAsP, but may be any InGaAsP-based semiconductor material.

[0026] In the above example, the carrier concentration of the p-type InGaAsP contact layer 40 is set to 1.6×10 19 cm -3 However, the present invention is not limited to such a numerical value, and it is sufficient that the carrier concentration is higher than that of the p-type InP cladding layer 30.

[0027] Next, photolithography and etching techniques are used to form a stripe-shaped resist pattern extending in the cavity direction on the surface of the p-type InGaAsP contact layer 40. Using an etching mask made of this resist pattern, etching is performed to a depth reaching the n-type InP substrate 5 or the n-type InP cladding layer 11 to form a 10 μm-wide mesa structure 50 including the ridge structure 10 therein (mesa structure forming step). As an etching method, wet etching is preferable, but dry etching may also be used.

[0028] After the mesa structure 50 is formed, a striped resist pattern extending in the resonator direction is formed on the upper surface of the mesa structure 50 in a portion corresponding to the upper portion of the ridge structure 10 using photolithography and etching techniques. An etching mask made of this resist pattern is used to etch the portion corresponding to the upper portion of the ridge structure 10. That is, all of the p-type InGaAsP contact layer 40 and part of the p-type InP cladding layer 30 in the openings of the etching mask are removed by etching to form a recess 51 having a width of 1.2 μm (recess formation process).

[0029] The portion of p-type InP cladding layer 30 remaining on the top of ridge structure 10 due to the formation of recess 51 functions as p-type InP ridge upper cladding layer 31. The thickness of p-type InP ridge upper cladding layer 31 is controlled to within the range of 0.3 to 0.4 μm by the above-mentioned etching.

[0030] After the recess 51 is formed, an insulating film 60 is formed to a thickness of 0.4 μm and made of an insulating material such as SiO2 so as to cover the bottom and side surfaces of the recess 51, the surface of the p-type InGaAsP contact layer 40, and both side surfaces of the mesa structure 50. Examples of a method for forming the insulating film 60 include a vacuum deposition method, a CVD method, and a sputtering method.

[0031] After the insulating film 60 is formed, a striped resist pattern extending in the resonator direction is formed on the insulating film 60 using photolithography and etching techniques, and then the insulating film 60 is etched so that the surface of the p-type InGaAsP contact layer 40 is exposed, thereby forming an insulating film opening 61.

[0032] Next, a p-side electrode 70 is formed by a film formation technique such as vacuum deposition or sputtering so as to be in contact with the p-type InGaAsP contact layer 40 through the insulating film opening 61. Furthermore, an n-side electrode 72 is formed by a similar film formation method on the back surface side of the n-type InP substrate 5 (electrode formation process).

[0033] The n-side electrode 72 and the p-side electrode 70 are each composed of a single metal such as Au (gold), Pt (platinum), Zn, Ge (germanium), Ni (nickel), Ti (titanium), etc., or a combination of two or more of these metals.

[0034] The semiconductor optical device 100 has front and rear end faces formed by cleavage in the direction of the optical axis of the laser light, forming a cavity having a length of 200 μm. Through the above steps, the semiconductor optical device 100 according to the first embodiment is manufactured.

[0035] In the above description, the values ​​of the doping concentration, thickness, width, etc. of each semiconductor layer are shown as typical examples, and are not limited to the values ​​or ranges shown as examples.

[0036] Fig. 3 shows the results of a simulation performed by the Beam Propagation Method (BPM) on the change in the optical confinement factor Γ when the layer thickness h of the p-type InP ridge upper cladding layer 31 shown in the cross-sectional view of Fig. 2 is changed in the semiconductor optical device 100 according to the first embodiment. Note that in the simulation, it was assumed that the refractive index of the active layer 12 was 3.42, and that the refractive indexes of the n-type InP cladding layer 11, the p-type InP cladding layer 30, and the p-type InP ridge upper cladding layer 31 were each 3.21.

[0037] When the thickness of p-type InP ridge upper cladding layer 31 is 0.3 μm or more, the thicker the thickness h of p-type InP ridge upper cladding layer 31 is, the smaller the optical confinement factor Γ becomes, and the thinner the thickness h is, the larger the optical confinement factor Γ becomes.

[0038] However, when the thickness of p-type InP ridge upper cladding layer 31 is less than 0.3 μm, the optical confinement factor Γ decreases rapidly as the thickness h of p-type InP ridge upper cladding layer 31 becomes thinner.

[0039] From the above simulation results, it is preferable to set the thickness h of the p-type InP ridge upper cladding layer 31 in the range of 0.3 to 0.4 μm. Moreover, the optical confinement factor Γ may be further increased by adjusting not only the thickness h of the p-type InP ridge upper cladding layer 31 but also the thickness of the n-type InP cladding layer 11 or the thicknesses of the optical confinement layers formed on the upper and lower surfaces of the active layer 12.

[0040] As described above, according to the semiconductor optical device of the first embodiment, the recess provided in the mesa structure enables the layer thickness of the ridge upper cladding layer provided on the upper part of the active layer to be thinner than the cladding layers provided other than on the upper part of the active layer, thereby increasing the optical confinement in the active layer in the vertical direction and increasing the relaxation oscillation frequency, thereby providing an effect of obtaining a semiconductor optical device capable of high-speed modulation.

[0041] Variation 1 of the first embodiment Fig. 4 is a cross-sectional view in a direction perpendicular to the resonator in the semiconductor optical device 200 according to the first modification of the first embodiment. Note that the n-type InP substrate 5 is omitted in Fig. 4. In Fig. 2 showing the cross-sectional view of the semiconductor optical device 100 according to the first embodiment, the cross section of the recess 51 in the direction perpendicular to the optical axis direction has a rectangular shape with an opening at the top, but in the semiconductor optical device 200 according to the first modification of the first embodiment, the bottom surface of the recess 52 has a curved surface. That is, the cross section of the recess 52 in the direction perpendicular to the optical axis direction has a U-shape.

[0042] The recess 52 is formed by wet etching using, for example, a Br-based chemical solution such as hydrogen bromide (HBr) as an etchant.

[0043] In the semiconductor optical device 200 according to the first modification of the first embodiment, similarly to the semiconductor optical device 100 according to the first embodiment, by providing the recess 52, the optical confinement in the active layer 12 in the vertical direction is increased and the relaxation oscillation frequency is increased, thereby providing an effect of obtaining a semiconductor optical device capable of high-speed modulation.

[0044] In the semiconductor optical device 200 according to the first modification of the first embodiment, the distance between the n-type InP second burying layer 22 and the recess 52 is further increased, thereby reducing the device resistance of the semiconductor optical device 200, thereby achieving the effect of reducing the operating current.

[0045] Variation 2 of embodiment 1 Fig. 5 is a cross-sectional view in a direction perpendicular to the resonator in a semiconductor optical device 300 according to a second modification of the first embodiment. Note that the n-type InP substrate 5 is omitted in Fig. 5. In Fig. 2 showing a cross-sectional view of the semiconductor optical device 100 according to the first embodiment, the insulating film opening 61 is formed only in one region of the upper surface of the mesa structure 50 divided by the recess 51.

[0046] On the other hand, in the semiconductor optical device 300 according to the second modification of the first embodiment, an insulating film opening 62 is also provided in the other region of the upper surface of the mesa structure 50, and a p-side electrode 71 is formed in the insulating film opening 62 so as to contact the surface of the p-type InGaAsP contact layer 40.

[0047] That is, on the upper surface of the mesa structure 50, an insulating film opening 61 and an insulating film opening 62 are provided at positions facing each other with a recess 51 in between, and further, a p-side electrode 70 and a p-side electrode 71 are provided in each opening so as to contact the surface of the p-type InGaAsP contact layer 40. The recess 51 may be formed into a U-shape by wet etching using a Br-based chemical solution or the like.

[0048] In the semiconductor optical device 300 according to the second modification of the first embodiment, similarly to the semiconductor optical device 100 according to the first embodiment, the provision of the recess 51 increases the optical confinement in the active layer 12 in the vertical direction and increases the relaxation oscillation frequency, thereby providing an effect of obtaining a semiconductor optical device capable of high-speed modulation.

[0049] In the semiconductor optical device 300 according to the second modification of the first embodiment, it is further possible to uniformly inject current into the active layer 12 from the two p-side electrodes 70 and 71, thereby suppressing heat generation in the semiconductor optical device and reducing power consumption.

[0050] Variation 3 of embodiment 1 Fig. 6 is a cross-sectional view in a direction perpendicular to the cavity in a semiconductor optical device 400 according to the third modification of the first embodiment. Note that the n-type InP substrate 5 is omitted in Fig. 6. In Fig. 2 showing the cross-sectional view of the semiconductor optical device 100 according to the first embodiment, the ridge structure 10 and the recess 51 are provided in the center of the mesa structure 50, but in the semiconductor optical device 400 according to the third modification of the first embodiment, the ridge structure 10 and the recess 51 are provided at a position shifted from the center of the mesa structure 50 in a direction perpendicular to the cavity direction.

[0051] That is, within the mesa structure 50, the central axes of the ridge structure 10 and the recess 51 are spaced apart at a preset interval from the central axis of the mesa structure 50 in the direction perpendicular to the surface of the n-type InP substrate 5. The recess 51 may be formed in a U-shape by wet etching using a Br-based chemical solution or the like.

[0052] In the semiconductor optical device 400 according to the third modification of the first embodiment, similarly to the semiconductor optical device 100 according to the first embodiment, the provision of the recess 51 increases the optical confinement in the active layer 12 in the vertical direction and increases the relaxation oscillation frequency, thereby providing an effect of obtaining a semiconductor optical device capable of high-speed modulation.

[0053] In the semiconductor optical device 400 according to the third modification of the first embodiment, furthermore, within the mesa structure 50, the central axes of the ridge structure 10 and the recess 51 are spaced apart from the central axis of the mesa structure 50 at a preset interval. This increases the area of ​​one side of the upper surface of the mesa structure 50, thereby making it possible to increase the opening width of the insulating film opening 61 and therefore increase the contact area between the p-type InGaAsP contact layer 40 and the p-side electrode 70. As a result, the contact resistance is reduced, and as a result, the device resistance of the semiconductor optical device is reduced, and the operating current can be reduced.

[0054] Embodiment 2 FIG. 7 is a cross-sectional view of a semiconductor optical device 500 according to the second embodiment in a direction perpendicular to the resonator. The semiconductor optical device 500 according to the second embodiment includes a striped ridge structure 13 including a p-type InP cladding layer 14 (cladding layer of a first conductivity type) and an active layer 12, which are sequentially stacked on a p-type InP substrate 6 (semiconductor substrate of a first conductivity type); a buried structure 24 including a p-type InP first buried layer 23a (first buried layer of a first conductivity type), an n-type InP second buried layer 21a (second buried layer of a second conductivity type), and a p-type InP third buried layer 22a (third buried layer of a first conductivity type) formed so as to fill both side surfaces of the striped ridge structure 13; an n-type InP ridge upper cladding layer 33 (ridge upper cladding layer of a second conductivity type) provided on the upper portion of the ridge structure 13 and having a layer thickness in the range of 0.3 to 0.4 μm; and an n-type InP cladding layer 32 (cladding layer of a second conductivity type) and an n-type InGaAsP contact layer 41 (contact layer of a second conductivity type) provided on the upper portion of the buried structure 24. the n-type InGaAsP contact layer 41 and the n-type InP cladding layer 32; a stripe-shaped recess 51 provided in the n-type InP cladding layer 32 and the n-type InGaAsP contact layer 41, the bottom surface of which is the upper surface of the n-type InP ridge upper cladding layer 33 and the side surfaces of which are made of the n-type InP cladding layer 32 and the n-type InGaAsP contact layer 41; a stripe-shaped mesa structure 53 including the ridge structure 13 and having both side surfaces formed by a mesa extending from the n-type InGaAsP contact layer 41 to the p-type InP substrate 6; an insulating film 60 covering the bottom surface and side surfaces of the recess 51, the surface of the n-type InGaAsP contact layer 41, and both side surfaces of the mesa structure 53; a stripe-shaped insulating film opening 61 provided in the insulating film 60 on the n-type InGaAsP contact layer 41;

[0055] In the semiconductor optical device 500 of the second embodiment, similarly to the semiconductor optical device 100 of the first embodiment, the embedding structure 24 increases the optical confinement in the lateral direction of the active layer 12, i.e., in the direction parallel to the surface of the p-type InP substrate 6, and in addition, the presence of the recess 51 increases the optical confinement in the vertical direction of the active layer 12, i.e., in the direction perpendicular to the surface of the p-type InP substrate 6, thereby achieving the effect of increasing the relaxation oscillation frequency of the semiconductor optical device 500.

[0056] In the semiconductor optical device 500 according to the second embodiment, further, an n-side electrode 72 is provided through an insulating film opening 61 formed on the upper surface of the striped mesa structure 53 along the lateral direction of the recess 51. This enables the distance between the active layer 12 and the n-type InGaAsP contact layer 41 to be set long, thereby suppressing the loss caused by the absorption of laser light in the n-type InGaAsP contact layer 41.

[0057] An example of a method for manufacturing the semiconductor optical device 500 according to the second embodiment will be described below. First, the Zn doping carrier concentration is 1.2×10 18 cm -3 A p-type InP substrate 6 having a carrier concentration of 1.2×10 18 cm -3 A p-type InP cladding layer 14 having a thickness of 1.8 μm and an active layer 12 made of an AlGaInAs-based or InGaAsP-based semiconductor material having a thickness of 0.2 μm are sequentially grown by crystal growth methods such as MOCVD or MBE (first crystal growth step).

[0058] In the above-mentioned device structure, the active layer 12 may include a multiple quantum well structure. Also, light confinement layers made of AlGaInAs-based or InGaAsP-based semiconductor materials having a refractive index set larger than that of the p-type InP cladding layer 14 may be provided on the upper and lower surfaces of the active layer 12. Also, although the above description has given an example of an InP-based semiconductor material, GaAs-based or GaN-based semiconductor materials may also be used.

[0059] After the crystal growth of each of the above layers, an insulating material such as SiO2 is deposited on the surface of the active layer 12. Examples of methods for depositing the SiO2 film include vacuum deposition, CVD, and sputtering. After the SiO2 film is deposited, it is patterned into a striped SiO2 film having a desired width and extending in the resonator direction using photolithography and etching techniques. The striped SiO2 film functions as an etching mask for forming the ridge structure 13. The etching mask is not limited to a SiO2 film, and may be a SiN film.

[0060] Using an etching mask, etching is performed to a depth reaching the p-type InP substrate 6 or the p-type InP cladding layer 14 to form a ridge structure 13 having a width of 1.2 μm (ridge structure forming step). As an etching method, dry etching is preferable, but wet etching may also be used.

[0061] After the formation of the ridge structure 13, Zn was doped to cover both side surfaces of the ridge structure 13 to a carrier concentration of 1.0×10 17 cm -3 and a p-type InP first buried layer 23a doped with Si and having a carrier concentration of 7.0×10 18 cm -3 and an n-type InP second buried layer 21a doped with Zn and having a carrier concentration of 2.0×10 18 cm -3 The p-type InP third burying layer 22a and the p-type InP third burying layer 22b are sequentially grown by MOCVD or the like to form a burying structure 24 (second crystal growth step).

[0062] The material of the p-type InP first buried layer 23a is not limited to InP, but may be any InP-based semiconductor material, as is the case for the n-type InP second buried layer 21a and the p-type InP third buried layer 22a.

[0063] Each buried layer of the buried structure 24 may be made of a semi-insulating material such as InP doped with Ru or Fe. The configuration of the buried structure 24 is not limited to the above-mentioned three-layer configuration, and may be semiconductor layers with different carrier concentrations or electrical conductivities, or may be a laminate of a combination of a plurality of these semiconductor layers. After the crystal growth of the buried structure 24, the striped SiO2 film is removed by dry etching or the like.

[0064] Next, the upper surface of the ridge structure 13 and the surface of the buried structure 24 are doped with Si to a carrier concentration of 9.0×10 17 cm -3 , an n-type InP cladding layer 32 having a thickness of 2.0 μm, and a carrier concentration of 6.6×10 18 cm -3 Then, an n-type InGaAsP contact layer 41 having a thickness of 0.5 μm is successively grown by crystal growth using a method such as MOCVD (third crystal growth step).

[0065] The material of the n-type InP cladding layer 32 is not limited to InP, but may be any InP-based semiconductor material. The material of the n-type InGaAsP contact layer 41 is not limited to InGaAsP, but may be any InGaAsP-based semiconductor material.

[0066] In the above example, the carrier concentration of the n-type InGaAsP contact layer 41 is set to 6.6×10 18 cm -3 However, the value is not limited to this, and it is sufficient that the carrier concentration is higher than that of the n-type InP cladding layer 32.

[0067] Next, photolithography and etching techniques are used to form a stripe-shaped resist pattern extending in the cavity direction on the surface of the n-type InGaAsP contact layer 41. Using an etching mask made of this resist pattern, etching is performed to a depth reaching the p-type InP substrate 6 or the p-type InP cladding layer 14 to form a 10 μm-wide mesa structure 53 including the ridge structure 13 therein (mesa structure forming step). As an etching method, wet etching is preferable, but dry etching may also be used.

[0068] After the mesa structure 53 is formed, a striped resist pattern extending in the resonator direction is formed on the upper surface of the mesa structure 53 in a portion corresponding to the upper portion of the ridge structure 13 using photolithography and etching techniques. An etching mask made of this resist pattern is used to etch the portion corresponding to the upper portion of the ridge structure 13. That is, all of the n-type InGaAsP contact layer 41 and part of the n-type InP cladding layer 32 in the openings of the etching mask are removed by etching to form a recess 51 having a width of 1.2 μm (recess formation step).

[0069] The portion of n-type InP cladding layer 32 remaining on the upper surface of ridge structure 13 due to the formation of recess 51 functions as n-type InP ridge upper cladding layer 33. The thickness of n-type InP ridge upper cladding layer 33 is controlled to within the range of 0.3 to 0.4 μm by the above-mentioned etching.

[0070] After the recess 51 is formed, an insulating film 60 is formed to a thickness of 0.4 μm and made of an insulating material such as SiO2 so as to cover the bottom and side surfaces of the recess 51, the surface of the n-type InGaAsP contact layer 41, and both side surfaces of the mesa structure 53. Examples of a method for forming the insulating film 60 include a vacuum deposition method, a CVD method, and a sputtering method.

[0071] After forming the insulating film 60, a striped resist pattern extending in the cavity direction is formed using photolithography and etching techniques, and then the insulating film 60 is etched so that the surface of the n-type InGaAsP contact layer 41 is exposed, thereby forming an insulating film opening 61.

[0072] Next, an n-side electrode 72 is formed by a film formation technique such as vacuum deposition or sputtering so as to be in contact with the n-type InGaAsP contact layer 41 through the insulating film opening 61. Furthermore, a p-side electrode 70 is formed by a similar film formation method on the back surface side of the p-type InP substrate 6 (electrode formation process).

[0073] The n-side electrode 72 and the p-side electrode 70 are each made of a single metal such as Au, Pt, Zn, Ge, Ni, or Ti, or a combination of two or more of these metals.

[0074] The semiconductor optical device 500 has front and rear end faces formed by cleavage in the direction of the optical axis of the laser light, forming a cavity having a length of 200 μm. Through the above steps, the semiconductor optical device 500 according to the second embodiment is manufactured.

[0075] In the above description, the values ​​of the doping concentration, thickness, width, etc. of each semiconductor layer are shown as typical examples, and are not limited to the values ​​or ranges shown as examples.

[0076] As a modification of the second embodiment, the recess 51 may be formed in a U-shape by wet etching using a Br-based chemical solution or the like. Even in such a modification, the recess 51 can provide the effect of increasing the optical confinement in the vertical direction of the active layer 12. In addition, since the distance between the p-type InP third buried layer 22a and the recess 51 is increased, the device resistance is reduced, and therefore, an effect of reducing the operating current is achieved.

[0077] In the semiconductor optical device 500 according to the second embodiment, the insulating film opening 61 is formed only on one side of the upper surface of the mesa structure 53 in the lateral direction of the recess 51, but an insulating film opening may also be provided on the other upper surface of the mesa structure 53 to form a second n-side electrode. In this case, it becomes possible to flow current evenly from the active layer 12 to the two n-side electrodes, which has the effect of suppressing heat generation in the semiconductor optical device and reducing power consumption.

[0078] As another modification of the second embodiment, the ridge structure 13 and the recess 51 may be provided at a position shifted in the direction perpendicular to the cavity direction from the center of the mesa structure 53. Even in such a modification, the recess 51 exerts the effect of increasing the optical confinement in the vertical direction of the active layer 12.

[0079] As described above, in the semiconductor optical device according to the second embodiment, even if a semiconductor substrate and layer structure of the opposite conductivity type to those of the semiconductor optical device according to the first embodiment are adopted, the recess provided in the mesa structure enables the layer thickness of the ridge upper cladding layer provided on the upper part of the active layer to be thinner than the cladding layers provided other than on the upper part of the active layer, thereby increasing the optical confinement in the active layer in the vertical direction and increasing the relaxation oscillation frequency, thereby providing an effect of obtaining a semiconductor optical device capable of high-speed modulation.

[0080] Embodiment 3 Fig. 8 is a cross-sectional view in a direction perpendicular to the resonator of a semiconductor optical device 600 according to embodiment 3. Note that the n-type InP substrate 5 is omitted in Fig. 8. The semiconductor optical device 600 according to the third embodiment includes a striped ridge structure 10 including an n-type InP cladding layer 11 (cladding layer of a first conductivity type) and an active layer 12 which are sequentially stacked on an n-type InP substrate 5 (semiconductor substrate of a first conductivity type), a buried structure 20 including a p-type InP first burying layer 21 (first burying layer of a second conductivity type) and an n-type InP second burying layer 22 (second burying layer of a first conductivity type) which are formed so as to fill both side surfaces of the striped ridge structure 10, and A p-type InP ridge upper cladding layer 31 (second conductivity type ridge upper cladding layer) having a thickness in the range of 0.3 to 0.4 μm is provided on the upper part of the ridge structure 10, a p-type InP first cladding layer 30a (second conductivity type first cladding layer) and a p-type InGaAsP contact layer 40 (second conductivity type contact layer) are provided on the surface of the buried structure 20 on one side of the ridge structure 10, and a p-type InP ridge upper cladding layer 30b (second conductivity type first cladding layer) and a p-type InGaAsP contact layer 40 (second conductivity type contact layer) are provided on the surface of the buried structure 20 on the other side of the ridge structure 10. a p-type InP second cladding layer 30b (second conductive type second cladding layer) that is flush with the p-type InP ridge upper cladding layer 31, a step portion 54 that is made up of the upper surfaces of the p-type InP second cladding layer 30b and the p-type InP ridge upper cladding layer 31 and the side surfaces of the p-type InP first cladding layer 30a and the p-type InGaAsP contact layer 40, and a mesa that includes a ridge structure 10 and has one side extending from the p-type InGaAsP contact layer 40 to the n-type InP substrate 5 and the other side extending from the step portion 54 to the n-type InP substrate 5. the p-type InGaAsP contact layer 40, and both side surfaces of the mesa structure 50; an insulating film 60 covering the step portion 54, the p-type InGaAsP contact layer 40, and both side surfaces of the mesa structure 50; a stripe-shaped insulating film opening 61 provided in the insulating film 60 on the p-type InGaAsP contact layer 40; a p-side electrode 70 (second conductive side electrode) in contact with the p-type InGaAsP contact layer 40 at the insulating film opening 61; and an n-side electrode 72 (first conductive side electrode) provided on the back surface side of the n-type InP substrate 5.

[0081] In the semiconductor optical device 600 according to the third embodiment, the embedding structure 20 increases the optical confinement in the lateral direction of the active layer 12, and the step portion 54 increases the optical confinement in the vertical direction of the active layer 12, thereby achieving the effect of increasing the relaxation oscillation frequency of the semiconductor optical device 600.

[0082] The semiconductor optical device 600 according to the third embodiment further has a device structure in which a p-side electrode 70 is provided in contact with the p-type InGaAsP contact layer 40 through an insulating film opening 61 formed on the upper surface of the striped mesa structure 50 opposite the step portion 54. This makes it possible to set a long distance between the active layer 12 and the p-type InGaAsP contact layer 40, thereby suppressing loss caused by absorption of the laser light emitted from the active layer 12 in the p-type InGaAsP contact layer 40.

[0083] The step portion 54 of the semiconductor optical device 600 according to the third embodiment can be fabricated, for example, as follows. First, a stripe-shaped etching mask extending in the resonator direction is formed on the upper surface of the mesa structure 50 using an insulating material such as SiO2. Using the etching mask, the p-type InP first cladding layer 30a and the p-type InGaAsP contact layer 40 from one side surface of the mesa structure 50 to the top of the ridge structure 10 are etched and removed to form the p-type InP ridge upper cladding layer 31 having a layer thickness in the range of 0.3 to 0.4 μm and the step portion 54. At this time, the p-type InP second cladding layer 30b, which is flush with the p-type InP ridge upper cladding layer 31, is also formed at the same time. The other configurations of the semiconductor optical device 600 are the same as those of the semiconductor optical device 100 according to the first embodiment, and therefore the semiconductor optical device 600 can be fabricated by the same manufacturing method as that of the semiconductor optical device 100 according to the first embodiment described above.

[0084] As described above, in the semiconductor optical device of the third embodiment, the step portion provided in the mesa structure enables the thickness of the ridge upper cladding layer provided on the upper part of the active layer to be made thinner than the cladding layers provided other than on the upper part of the active layer. This not only increases the optical confinement in the active layer in the vertical direction, but also enables the distance between the active layer and the p-type InGaAsP contact layer to be set long, thereby suppressing the loss caused by the absorption of laser light emitted from the active layer in the p-type InGaAsP contact layer.

[0085] Embodiment 4 Fig. 9 is a schematic view of a semiconductor optical device 700 according to the fourth embodiment, and Fig. 10 is a cross-sectional view of the semiconductor optical device 700 taken along line AA in Fig. 9, i.e., a cross-sectional view in a direction parallel to the cavity direction in the ridge structure 10 including the recess 55. Note that the n-type InP substrate 5 is omitted in Figs. 9 and 10.

[0086] The semiconductor optical device 700 according to the fourth embodiment includes a striped ridge structure 10 including an n-type InP cladding layer 11 (cladding layer of a first conductivity type) and an active layer 12 which are sequentially stacked on an n-type InP substrate 5 (semiconductor substrate of a first conductivity type), a buried structure 20 including a p-type InP first buried layer 21 (first buried layer of a second conductivity type) and an n-type InP second buried layer 22 (second buried layer of a first conductivity type) which are formed so as to fill both side surfaces of the striped ridge structure 10, a p-type InP ridge upper cladding layer 31 (ridge upper cladding layer of a second conductivity type) which is provided on the upper portion of the ridge structure 10 and has a layer thickness in the range of 0.3 to 0.4 μm and which is formed in an area excluding both ends in the cavity direction, a p-type InP cladding layer 30 (cladding layer of a second conductivity type) and a p-type InGaAsP contact layer 40 (contact layer of a second conductivity type) which are provided on the surface of the buried structure 20, and a p-type InP cladding layer 30 and a p-type InGaAsP contact layer 40. the p-type InGaAsP contact layer 40; a striped recess 55 formed in the p-type InP ridge upper cladding layer 31 except for both ends in the resonator direction so as to correspond to the shape of the p-type InP ridge upper cladding layer 31; a striped mesa structure 50 including the ridge structure 10 and having both side surfaces formed by a mesa extending from the p-type InGaAsP contact layer 40 to the n-type InP substrate 5; an insulating film 60 covering the bottom and side surfaces of the recess 55, the surface of the p-type InGaAsP contact layer 40, and both side surfaces of the mesa structure 50; a striped insulating film opening 61 provided in the insulating film 60 on the p-type InGaAsP contact layer 40; a p-side electrode 70 (second conductive side electrode) in contact with the p-type InGaAsP contact layer 40 at the insulating film opening 61;

[0087] In the semiconductor optical device 700 of embodiment 4, the embedding structure 20 increases the optical confinement in the lateral direction of the active layer 12, and in addition, the presence of the recess 55 increases the optical confinement in the vertical direction of the active layer 12, thereby achieving the effect of increasing the relaxation oscillation frequency of the semiconductor optical device 700.

[0088] Furthermore, in the semiconductor optical device 700 according to the fourth embodiment, a device structure is adopted in which the p-side electrode 70 is provided on the upper surface of the striped mesa structure 50 through the insulating film opening 61 formed along the lateral direction of the recess 55. This makes it possible to set a long distance between the active layer 12 and the p-type InGaAsP contact layer 40, thereby suppressing loss caused by absorption of the laser light emitted from the active layer 12 in the p-type InGaAsP contact layer 40.

[0089] In the semiconductor optical device 700 according to the fourth embodiment, the recess 55 is further formed in a region excluding both end portions in the resonator direction of the semiconductor optical device 700. In other words, the p-type InP ridge upper cladding layer 31 and the recess 55 are not provided in a region preset from both end faces in the resonator direction.

[0090] By adopting such an element structure, the optical confinement of the active layer 12 in the regions near both end faces of the semiconductor optical element 700 is relatively smaller than the optical confinement in the region where the recesses 55 are provided. This suppresses the occurrence of end face damage due to an increase in optical density that occurs when the optical confinement is set large in the semiconductor optical element, thereby enabling high-output operation and providing a highly reliable semiconductor optical element.

[0091] The recess 55 of the semiconductor optical device 700 according to the fourth embodiment can be fabricated, for example, as follows. First, an etching mask is formed on the upper surface of the mesa structure 50 using an insulating material such as SiO2. Next, a resist is patterned on the upper portion of the ridge structure 10 so that the region excluding both ends in the cavity direction can be etched. After forming the resist mask, the p-type InP cladding layer 30 and the p-type InGaAsP contact layer 40 are etched to form the p-type InP ridge upper cladding layer 31 having a layer thickness of 0.3 to 0.4 μm and the recess 55.

[0092] When forming the recess 55, as shown in the cross-sectional view along the resonator direction in Fig. 10, it is desirable to set the distance a between the front end face of the semiconductor optical element 700 and the recess 55 and the distance b between the rear end face and the recess 55 to about 10 µm in consideration of misalignment during cleavage. However, the distances a and b are not limited to these values. The other configurations of the semiconductor optical element 700 are the same as those of the semiconductor optical element 100 according to the first embodiment, and therefore the semiconductor optical element 700 can be manufactured by the same manufacturing method as that of the semiconductor optical element 100 according to the first embodiment described above.

[0093] As described above, in the semiconductor optical device according to the fourth embodiment, the recess provided in the mesa structure enables the thickness of the ridge upper cladding layer provided on the upper part of the active layer to be thinner than the cladding layers provided other than on the upper part of the active layer. This increases the optical confinement in the active layer in the vertical direction, and increases the relaxation oscillation frequency. In addition, the optical confinement in the active layer in the regions near both end facets of the semiconductor optical device is made smaller than the optical confinement in the regions where the recess is provided. This suppresses the occurrence of end face damage due to an increase in optical density, thereby enabling high-output operation and providing a highly reliable semiconductor optical device.

[0094] Although the present disclosure describes various exemplary embodiments and examples, the various features, aspects, and functions described in one or more embodiments are not limited to application to a particular embodiment, but may be applied to the embodiments alone or in various combinations.

[0095] Therefore, countless modifications not exemplified are assumed within the scope of the technology disclosed in the present specification, including, for example, modifying, adding, or omitting at least one component, and further, extracting at least one component and combining it with a component of another embodiment. [Explanation of symbols]

[0096] 5 n-type InP substrate (semiconductor substrate of first conductivity type), 6 p-type InP substrate (semiconductor substrate of first conductivity type), 10, 13 ridge structure, 11 n-type InP cladding layer (cladding layer of first conductivity type), 12 active layer, 14 p-type InP cladding layer (cladding layer of first conductivity type), 20, 24 buried structure, 21 p-type InP first buried layer (first buried layer of second conductivity type), 21a n-type InP second buried layer (second buried layer of second conductivity type), 22 n-type InP second buried layer (second buried layer of first conductivity type), 22a p-type InP third buried layer (third buried layer of first conductivity type), 23a p-type InP first buried layer (first buried layer of first conductivity type), 30 p-type InP cladding layer (cladding layer of second conductivity type), 30a p-type InP first cladding layer (second conductive type first cladding layer), 30b p-type InP second cladding layer (second conductive type second cladding layer), 31 p-type InP ridge upper cladding layer (second conductive type ridge upper cladding layer), 32 n-type InP cladding layer (second conductive type cladding layer), 33 n-type InP ridge upper cladding layer (second conductive type ridge upper cladding layer), 40 p-type InGaAsP contact layer (second conductive type contact layer), 41 n-type InGaAsP contact layer (second conductive type contact layer), 50, 53 mesa structure, 51, 52, 55 recess, 54 step portion, 60 insulating film, 61, 62 insulating film opening, 70, 71 p-side electrode (second conductive side electrode), 72 n-side electrode (first conductive side electrode), 100, 200, 300, 400, 500, 600, 700 Semiconductor Optical Device

Claims

1. a semiconductor substrate of a first conductivity type; a stripe-shaped ridge structure including a first conductivity type cladding layer and an active layer provided on the first conductivity type semiconductor substrate; a buried structure buried so as to cover both side surfaces of the ridge structure; a ridge upper cladding layer of a second conductivity type provided on an upper portion of the ridge structure; a cladding layer of a second conductivity type and a contact layer of a second conductivity type provided on a surface of the buried structure; a stripe-shaped recess provided in the second conductivity type cladding layer and the second conductivity type contact layer, the bottom surface of which is the upper surface of the ridge upper cladding layer and the side surfaces of which are the second conductivity type cladding layer and the second conductivity type contact layer; a striped mesa structure including the ridge structure, both side surfaces of which are formed by a mesa extending from the second conductivity type contact layer to the first conductivity type semiconductor substrate; an insulating film covering a bottom surface and side surfaces of the recess, a surface of the second conductive type contact layer, and both side surfaces of the mesa structure; A semiconductor optical element comprising:

2. a stripe-shaped insulating film opening provided in the insulating film on the second conductive type contact layer; a second conductive side electrode in contact with the second conductive type contact layer in the insulating film opening; The semiconductor optical device according to claim 1 , further comprising:

3. 3. The semiconductor optical device according to claim 2, wherein the insulating film opening is provided in one region and the other region of the upper surface of the mesa structure that are divided by the recess.

4. 3. The semiconductor optical device according to claim 1, wherein the central axes of the ridge structure and the recess are spaced a predetermined distance from the central axis of the mesa structure in a direction perpendicular to the surface of the first conductivity type semiconductor substrate.

5. 5. The semiconductor optical device according to claim 1, wherein a cross section of the recess in a direction perpendicular to the resonator is U-shaped.

6. 6. The semiconductor optical device according to claim 1, wherein the second conductivity type ridge upper cladding layer and the recess are not provided in a predetermined region from both end faces in the resonator direction.

7. a semiconductor substrate of a first conductivity type; a stripe-shaped ridge structure including a first conductivity type cladding layer and an active layer provided on the first conductivity type semiconductor substrate; a buried structure buried so as to cover both side surfaces of the ridge structure; a first cladding layer of a second conductivity type and a contact layer of a second conductivity type provided on a surface of the buried structure on one side of the ridge structure; a ridge upper cladding layer of a second conductivity type provided on an upper portion of the ridge structure; a second cladding layer of a second conductivity type provided on a surface of the buried structure on the other side of the ridge structure and coplanar with an upper surface of the ridge upper cladding layer; a step portion formed by upper surfaces of the second cladding layer of the second conductivity type and the ridge upper cladding layer of the second conductivity type, and side surfaces of the first cladding layer of the second conductivity type and the contact layer of the second conductivity type; a striped mesa structure including the ridge structure, one side of which is formed by a mesa that extends from the contact layer of the second conductivity type to the semiconductor substrate of the first conductivity type and the other side of which is formed by a mesa that extends from the step portion to the semiconductor substrate of the first conductivity type; an insulating film covering the step portion, the second conductive type contact layer, and both side surfaces of the mesa structure; a stripe-shaped insulating film opening provided in the insulating film on the second conductive type contact layer; a second conductive side electrode in contact with the second conductive type contact layer in the insulating film opening; A semiconductor optical element comprising:

8. 8. The semiconductor optical device according to claim 1, wherein the second conductivity type ridge upper cladding layer has a thickness of 0.3 μm or more and 0.4 μm or less.

9. 9. The semiconductor optical device according to claim 1, wherein the buried structure comprises at least a first buried layer of the second conductivity type and a second buried layer of the first conductivity type.

10. 9. The semiconductor optical device according to claim 1, wherein the buried structure comprises a first buried layer of a first conductivity type, a second buried layer of a second conductivity type, and a third buried layer of the first conductivity type.

11. 11. The semiconductor optical device according to claim 1, wherein the first conductivity type is n-type, and the second conductivity type is p-type.

12. 11. The semiconductor optical device according to claim 1, wherein the first conductivity type is p-type, and the second conductivity type is n-type.

Citation Information

Patent Citations

  • Semiconductor laser and manufacture thereof

    JP1986032587A

  • Semiconductor laser and its manufacture

    JP1994097603A

  • Semiconductor laser and manufacture thereof

    JP1994291416A

  • Semiconductor optical element and manufacture thereof

    JP1996111565A

  • Semiconductor laser element and its manufacturing method

    JP2003264342A