Polyester fiber structure, its manufacturing method, and compression inner garment
A polyester fiber structure with specific additives addresses the issue of persistent odors in work clothes and innerwear by preventing sebum accumulation and bacterial decomposition, achieving effective odor suppression and durability.
Patent Information
- Application Number
- JP2020178688
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Existing methods for imparting deodorizing properties to textiles, such as those used in work clothes with fans and compression innerwear, fail to effectively suppress odors like aldehydes and ammonia, and are not durable against washing, leading to increased sebum accumulation and bacterial decomposition, which worsens odors over time.
A polyester fiber structure containing 0.3 to 0.85% antioxidants (citric acid, malic acid, ascorbic acid, or tocopherol), 0.1 to 0.3% hydrophilic resin, and an antibacterial agent, with specific molecular weight and distribution ranges, is used to enhance odor suppression by preventing sebum accumulation and bacterial decomposition.
The polyester fiber structure effectively reduces a wide range of odors, including aldehydes and ammonia, maintains odor suppression after multiple washes, and prevents sebum stains, providing excellent comfort and hygiene in work clothes and innerwear.
Smart Images

Figure 0007589499000001 
Figure 0007589499000002 
Figure 0007589499000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester fiber structure, a method for producing the same, and a compression inner garment. [Background technology]
[0002] Techniques for imparting deodorizing and deodorizing properties to textile products have been studied. Methods proposed for imparting deodorizing and deodorizing properties include a method using a metal complex such as metal phthalocyanine (Patent Document 1), a method in which a deodorizing extract from a plant or the like is attached to a fiber (Patent Document 2), a method using a polycarboxylic acid resin and a photocatalyst (Patent Document 3), and a method in which a substance made of a hydroxy acid derivative is heated to react with the hydroxy group and carboxyl group present at the end of a polyester fiber to fix the hydroxy acid to a polyester fiber structure (Patent Document 4). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 64-20852 [Patent Document 2] Japanese Patent Application Publication No. 9-271484 [Patent Document 3] JP 2004-052208 A [Patent Document 4] Patent No. 6168093 Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, work clothes with fans attached to them have become popular as a measure against heatstroke during work in extremely hot environments. Fan-equipped work clothes cool the body by blowing outside air into the clothes and expelling the hot air inside the clothes, dramatically improving comfort when worn, but they also actively expel odorous components such as sweat odor and body odor trapped inside the clothes, which can make not only the worker but also other workers around them uncomfortable. In addition, compression innerwear, which is often worn in combination with these to reduce physical strain during work, adheres closely to the skin and absorbs sweat, causing sebum and other substances to migrate to the surface of the fabric along with sweat, and the sebum gradually accumulates on the fabric due to the fan blowing, further amplifying the odor. Analysis of these odors revealed that in addition to ammonia, acetic acid, and medium-chain fatty acids such as isovaleric acid and hexenoic acid, which are generated by the decomposition of sebum and proteins by resident bacteria, aldehyde-based odors such as nonenal and heptanal were frequently generated. These odors are not thought to be produced by the metabolism of resident bacteria, but rather by the oxidative decomposition over time of free fatty acids such as triglycerides and palmitoleic acid contained in sebum due to the effects of light and heat, and it is difficult to suppress these odors using conventional deodorizing and anti-odor processing.
[0005] The methods shown in Patent Documents 1 to 3 all have problems in that the washing durability is low, and increasing the amount of deodorant or binder used to improve the deodorizing property after washing impairs the quality of the fabric, such as the texture. In addition, even if the techniques described in these documents are directly applied, although they can deal with specific odors such as ammonia, they cannot deal with odors such as aldehydes that occur when worn, and they also have low stain resistance, so there is a problem in that the odors cannot be completely suppressed. In addition, Patent Document 4 fixes a hydroxy acid derivative such as citric acid to exhibit ammonia deodorizing properties and inhibits the oxidative decomposition of aldehyde to exhibit aldehyde deodorizing properties, but the stain resistance decreases due to the high concentration of citric acid attached to the fiber surface, so the odor derived from sebum cannot be completely suppressed.
[0006] Therefore, an objective of the present invention is to provide a polyester fiber structure that can exhibit a new odor suppression effect never before seen by comprehensively addressing the causes of unpleasant odors, which are the accumulation of sebum and protein, the decomposition of sebum and protein by resident bacteria, and the oxidative decomposition over time of sebum other than that derived from resident bacteria, as well as a production method thereof and a compression inner garment with excellent odor suppression effect. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention employs the following configuration. (1) A fiber substrate containing polyester-based fibers, At least one antioxidant selected from the group consisting of citric acid, malic acid, ascorbic acid, tocopherol, and derivatives thereof is contained in an amount of 0.3 to 0.85% by mass based on the fiber base material, The fiber substrate contains a hydrophilic resin containing a polyether component in an amount of 0.1 to 0.3% by mass, A polyester-based textile structure having an antibacterial agent. (2) The polyester fiber structure according to (1), in which the difference ΔLu in the amount of luminescence obtained in an ATP wiping evaluation test before and after a resoil recontamination prevention evaluation test represented by the following formula (1) is 1000RLu or less. ΔLu = Lu(b) - Lu(a) (1) ΔLu: Difference in Lu value before and after the recontamination prevention evaluation test (unit: R Lu) Lu(a): Lu value of polyester fiber structure before anti-redeposition evaluation test (unit: R Lu(b): Lu value of polyester fiber structure after anti-redeposition evaluation test (unit: R (3) The polyester fiber structure according to (1) or (2), wherein the antioxidant is citric acid or a derivative thereof. (4) The hydrophilic resin is a polyester-based resin, and the weight average molecular weight in terms of polyethylene glycol obtained by size exclusion chromatography of a polyether component which is a hydrophilic segment of the polyester-based resin is in the range of 1500 to 6000 g / mol; The polyester fiber structure according to any one of (1) to (3), having a molecular weight distribution (ratio of weight average molecular weight in terms of polyethylene glycol to number average molecular weight in terms of polyethylene glycol) in the range of 1.00 to 1.35. (5) The polyester fiber structure according to any one of (1) to (4), wherein the antibacterial agent is a pyridine-based antibacterial agent. (6) The polyester fiber structure according to any one of (1) to (5), wherein the fiber base material contains 1 to 30% by mass of polyurethane elastic yarn. (7) A compression inner garment comprising the polyester fiber structure according to any one of (1) to (6). (8) A method for producing a polyester fiber structure according to any one of (1) to (6), comprising a step of supporting at least one antioxidant selected from the group consisting of citric acid, malic acid, ascorbic acid, tocopherol, and derivatives thereof, a hydrophilic resin containing a polyether component as a hydrophilic segment, and an antibacterial agent on a fiber substrate containing polyester fibers. Effect of the Invention
[0008] The present invention provides a polyester fiber structure capable of exerting a new odor suppression effect that has never been seen before by comprehensively dealing with the causes of unpleasant odors, such as the accumulation of sebum and protein, the decomposition of sebum and protein by resident bacteria, and the oxidative decomposition over time of sebum other than that derived from resident bacteria. Furthermore, when the polyester fiber structure contains polyurethane elastic yarn, it exhibits good stretchability that conforms to the body, and can respond to even more types of odors, such as ammonia, generated from the body surface by utilizing the adsorption of odorous components to the polyurethane elastic yarn. Furthermore, the compression inner garment of the present invention has an excellent odor suppression effect. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below.
[0010] [Antioxidants] In the present invention, the antioxidant is at least one selected from the group consisting of citric acid, malic acid, ascorbic acid, tocopherol, and derivatives thereof. Among them, citric acid and its derivatives are most preferred because they cause less yellowing of the fabric during processing, are inexpensive, and are durably fixed to polyester fibers.
[0011] Among the above-mentioned antioxidants, their derivatives include those in which the chemical structure of antioxidants such as citric acid is partially changed through reactions such as self-condensation or with polymers constituting the fiber base material, to become, for example, polymers, anhydrides, esters, etc.
[0012] From the viewpoints of antifouling, deodorizing, and antioxidizing properties, the amount of antioxidant attached to the fiber substrate is 0.3 to 0.85% by mass, and preferably 0.3 to 0.75% by mass. If the amount is less than 0.3% by mass, sufficient deodorizing and antioxidizing properties may not be obtained, while if the amount is more than 0.85% by mass, the hydrophilic resin is buried by the antioxidant, reducing the antifouling properties and lowering the pH of the fabric, which is undesirable because of concerns about irritation to the skin.
[0013] [Hydrophilic resin] The hydrophilic resin used in the present invention contains a polyether component. There is no particular restriction on the structure as long as the polyester fiber structure defined in the present invention can be obtained, but a resin containing a polyether component in the polymer main chain or side chain is preferred. Specific examples of the hydrophilic resin used in the present invention include copolymer polyester resins consisting of polyester and polyether components such as polyalkylene glycol, polyether-modified silicone resins, polyether resins, etc. Among them, copolymer polyester resins consisting of polyester and polyether components such as polyalkylene glycol are preferred because they are fixed to polyester fibers and provide good washing durability.
[0014] The hydrophilic resin is present on the surface of the single fiber, and thereby improves water absorption and the ability to prevent accumulation of sebum, thereby improving quick-drying properties. From the viewpoints of water absorption, the ability to prevent accumulation of sebum components that cause unpleasant odors, and the washing durability of the performance, the amount of the hydrophilic resin added is in the range of 0.1 to 0.3% by mass relative to the fiber substrate, and more preferably in the range of 0.1 to 0.25% by mass.
[0015] In order to obtain better water absorption and sebum accumulation prevention properties, it is preferable to control the weight average molecular weight, calculated as polyethylene glycol, of the polyether component of the copolymer polyester resin used. It is preferable to use a polyether component having a relatively high molecular weight of 1500 to 6000 g / mol in terms of polyethylene glycol, more preferably 2000 to 4000 g / mol.
[0016] It is calculated from the ratio of the weight average molecular weight in terms of polyethylene glycol to the number average molecular weight in terms of polyethylene glycol (weight average molecular weight (Mw) / number average molecular weight (Mn)). Furthermore, by reducing the variation in molecular weight distribution, the ability to prevent sebum accumulation can be improved.
[0017] The molecular weight distribution is a value indicating the variation in molecular weight, and is calculated from the ratio of the weight average molecular weight converted into polyethylene glycol to the number average molecular weight converted into polyethylene glycol (weight average molecular weight (Mw) / number average molecular weight (Mn)). By reducing the variation in molecular weight distribution, the antifouling and deodorizing properties are particularly excellent. From the viewpoint of imparting better anti-soiling properties, it is preferable to use a polyether with a relatively uniform molecular weight of 1.00 to 1.35, and more preferably 1.00 to 1.25. It is even more preferable that the molecular weight is 1.00 to 1.20.
[0018] Furthermore, the weight average molecular weight of the polyether component used is preferably large in terms of antifouling and deodorizing properties, and in particular, it is preferable to use a relatively high molecular weight polyether such as 1500 to 6000 g / mol in order to provide a more excellent sebum accumulation prevention property, and more preferably 2000 to 4000 g / mol.
[0019] In the present invention, the polyether component means a polyether or a polyether group portion in a compound containing a polyether group. The polyether component refers to a compound having two or more ether bonds per molecule, or a polyether group present in the molecule. Examples of compounds that can be used to support the polyether component on the polyester fiber structure of the present invention include polyalkylene glycol, cellulose, and block copolymers consisting of polyalkylene glycol and polyester, but are not limited thereto as long as the provisions of the present invention are satisfied. Among them, a polyetherester block copolymer in which a segment A consisting of a polyalkylene glycol unit and a segment B consisting of a polymer unit copolymerizable with the polyalkylene glycol, such as polyester, are copolymerized is preferred from the viewpoint of high affinity with polyester fibers and durability such as washing resistance.
[0020] Preferred examples of the polyalkylene glycol unit constituting the above segment A include units formed from polyethylene glycol, polypropylene glycol, and polybutylene glycol, and among these, units formed from polyethylene glycol are more preferred.
[0021] As a preferred example of the polyester unit constituting the above-mentioned segment B, a polymer unit composed of terephthalic acid / or isophthalic acid and alkylene glycol is preferably exemplified.
[0022] The copolymerization ratio of polyester and polyether in these block copolymers is arbitrary, but from the viewpoint of imparting a more excellent sebum accumulation prevention property, the polyester unit:polyether unit (mass ratio) is preferably 1:1 to 1:30. More preferably, the polyester unit:polyether unit (mass ratio) is 1:1 to 1:10. Even more preferably, the polyester unit:polyether unit (mass ratio) is 1:1 to 1:3.
[0023] [Antibacterial agents] In addition, in the present invention, the antibacterial agent is preferable in that, by using it in combination with the above agent, even if contaminants such as sebum adhere to the polyester fiber structure, the performance of preventing the proliferation of bacteria that decompose these contaminants is not easily reduced by washing, and the proliferation of bacteria is suppressed for a long period of time, thereby suppressing the production of decomposition products and making it possible to suppress the generation of unpleasant odors caused by these decomposition products. The type of antibacterial agent is not limited, but examples include pyridine-based antibacterial agents and silver-based antibacterial agents, and among these, pyridine-based antibacterial agents are preferred.
[0024] The pyridine-based antibacterial agent is not particularly limited, and examples thereof include pyridine-based antibacterial agents such as 2-chloro-6-trichloromethylpyridine, 2-chloro-4-trichloromethyl-6-methoxypyridine, 2-chloro-4-trichloromethyl-6-(2-furylmethoxy)pyridine, di(4-chlorophenyl)pyridylmethanol, 2,3,5-trichloro-4-(n-propylsulfonyl)pyridine, 2-pyridylthiol-1-oxide zinc, and di(2-pyridylthiol-1-oxide). Compounds, N-trichloromethylthiophthalimide, N-1,1,2,2-tetrachloroethylthiotetrahydrophthalimide, N-trichloromethylthiotetrahydrophthalimide, N-trichloromethylthio-N-(phenyl)methylsulfamide, N-trichloromethylthio-N-(4-chlorophenyl)methylsulfamide, N-(1-fluoro-1,1,2,2-tetrachloroethylthio)-N-(phenyl)methylsulfamide, N-(1,1-difluoro-1,2,2-tetrachloroethylthio)-N-(phenyl)methylsulfamide, haloalkylthio compounds such as N,N-dichloroethylthio-N-(phenyl)methylsulfamide, N,N-dichlorofluoromethylthio-N'-phenylsulfamide, N,N-dimethyl-N'-(p-tolyl)-N'-(fluorodichloromethylthio)sulfamide, 1-diiodomethylsulfonyl-4-chlorobenzene, 3-iodo-2-propargylbutylcarbamic acid, 4-chlorophenyl-3-iodopropargylformal, 3-ethoxycarbonyloxy-1-bromo- Examples of compounds that can be used include organic iodine compounds such as 1,2-diiodo-1-propene and 2,3,3-triiodoallyl alcohol, thiazole compounds such as 4,5-dichloro-2-cyclohexyl-4-isothiazolin-3-one, 2-(4-thiocyanomethylthio)benzthiazole and 2-mercaptobenzthiazole zinc, and benzimidazole compounds such as 1H-2-thiocyanomethylthiobenzimidazole and 2-(2-chlorophenyl)-1H-benzimidazole.
[0025] From the viewpoint of antibacterial properties and washing durability of antibacterial properties, the amount added is preferably in the range of 0.01 to 5% by mass relative to the fiber base, and more preferably in the range of 0.01 to 3% by mass.
[0026] Furthermore, when a polyester fiber structure contains polyurethane elastic yarns, particularly polyurethane fibers, the antibacterial agent is efficiently absorbed into the polyurethane elastic yarns, and therefore exhibits high antibacterial properties even at a relatively low concentration of 0.01 to 0.5% by mass.
[0027] [Fabric base material for polyester-based fiber structures] The fiber base material in the polyester fiber structure of the present invention contains 10% by mass or more of polyester fiber relative to the fiber base material excluding the processing agent, preferably 40% by mass or more, more preferably 60% by mass or more of polyester fiber in the fiber base material, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more of polyester fiber. There is no particular upper limit, and it may be 100% by mass.
[0028] The material constituting the polyester fiber may be a polymer having an ester bond, and preferably includes polyesters having a basic skeleton such as aromatic polyesters such as polyethylene terephthalate, polybutylene terephthalate, polypropylene terephthalate, and copolymers thereof, and aliphatic polyesters such as polylactic acid, among which aromatic polyesters are preferred from the viewpoint of the strength of the polyester fiber structure, and polyethylene terephthalate is even more preferred. These polyester fibers may contain additives such as hindered phenol-based, amine-based, phosphite-based, and thioester-based antioxidants, ultraviolet absorbers such as benzotriazole-based, benzophenone-based, and cyanoacrylate-based ultraviolet absorbers, infrared absorbers, organic pigments such as cyanine-based, stilbene-based, phthalocyanine-based, anthraquinone-based, verinone-based, and quinacridone-based, inorganic pigments, fluorescent whitening agents, particles such as calcium carbonate, silica, and titanium oxide, and electrostatic agents. In addition, cationic dyeable polyesters may be used in which a sulfo group or the like is introduced into the side chain of the polymer constituting the fiber so that it can be dyed with cationic dyes.
[0029] The polyester fiber structure of the present invention may be a mixed product containing fibers other than polyester fibers. Examples of the fibers other than polyester fibers include cotton, wool, rayon, cupra, nylon, and polyurethane elastic yarns, and the effect of the present invention is particularly remarkable when the fibers are cotton. These may be included in any form such as spun yarn, mixed yarn, interwoven, interknitted, and mixed cotton. From the viewpoint of a remarkable effect of preventing sebum accumulation, it is preferable that the fibers other than polyester fibers include cellulose fibers such as cotton fibers and rayon, and may be included in the fiber base material in an amount of about 1% by mass to 60% by mass.
[0030] In addition, a polyester fiber structure containing a polyurethane elastic yarn is preferred in that the effects of the present invention are particularly prominent. That is, in the present invention, when the polyurethane elastic yarn is further contained, the content in the fiber substrate is 1 to 30% by mass, more preferably 2 to 20% by mass, and even more preferably about 5 to 20% by mass, from the viewpoint of the deodorizing effect of the acidic odors such as acetic acid and isovaleric acid, which are the cause of unpleasant odors, being extremely prominent.
[0031] In addition, by incorporating polyurethane elastic yarn into a polyester fiber structure, the stretchability of the garment is improved, allowing it to conform to the body and increase the contact area between the skin and the garment, thereby more effectively suppressing unpleasant odors. From this viewpoint, the above range is also preferable.
[0032] [Polyurethane-based elastic thread] The polyurethane elastic yarn may be any polyurethane whose main components are diisocyanate and diol, and is not particularly limited. The synthesis method is also not particularly limited. The main components refer to components that constitute 50% by mass or more of the components that form polyurethane. That is, for example, polyurethane urea may be polyurethane made of polymer diol, diisocyanate, and diamino compound (low molecular weight diamine) as a chain extender, or polyurethane made of polymer diol, diisocyanate, and low molecular weight diol as a chain extender. Also, polyurethane urea may be polyurethane using a compound having a hydroxyl group and an amino group in the molecule as a chain extender. Here, a typical structural unit that constitutes the polyurethane elastic yarn used in the present invention will be described.
[0033] Next, the diisocyanate structural unit constituting the polyurethane elastic yarn used in the present invention is preferably an aromatic diisocyanate, an alicyclic diisocyanate, an aliphatic diisocyanate, etc. As the aromatic diisocyanate, for example, diphenylmethane diisocyanate (hereinafter abbreviated as MDI), tolylene diisocyanate, 1,4-diisocyanate benzene, xylylene diisocyanate, 2,6-naphthalene diisocyanate, etc. are suitable for synthesizing polyurethane having particularly high heat resistance and strength. As the alicyclic diisocyanate, for example, methylene bis(cyclohexyl isocyanate) (hereinafter abbreviated as PICM), isophorone diisocyanate, methylcyclohexane-2,4-diisocyanate, methylcyclohexane-2,6-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydroxylylene diisocyanate, hexahydrotolylene diisocyanate, octahydro-1,5-naphthalene diisocyanate, etc. are preferable. Aliphatic diisocyanates can be effectively used, particularly when suppressing yellowing of polyurethane. Among them, 4,4'-MDI is preferable. These diisocyanates may be used alone or in combination of two or more kinds.
[0034] As the polymer diol, which is a structural unit constituting the polyurethane elastic yarn, polyether glycol, polyester glycol, polycarbonate diol, etc. are preferred, and polyether glycol is preferably used from the viewpoints of deodorizing property, flexibility, and imparting high elongation when made into fibers.
[0035] Next, as the chain extender of the structural unit constituting the polyurethane-based elastic yarn, it is also preferable to use at least one or more of low molecular weight diamines and low molecular weight diols. A triamine compound capable of forming a crosslinked structure, such as diethylenetriamine, may be added to these chain extenders to an extent that the effect is not lost. Representative examples of preferred low molecular weight diols include ethylene glycol (hereinafter abbreviated as EG), 1,3-propanediol, 1,4-butanediol, bishydroxyethoxybenzene, bishydroxyethylene terephthalate, and 1-methyl-1,2-ethanediol. Particularly preferred are EG, 1,3-propanediol, and 1,4-butanediol. The use of these is preferable because they have high heat resistance as a diol-extended polyurethane.
[0036] Although there is no particular limitation on the preferred embodiment of the polyurethane elastic yarn, it is preferred to suppress the exposure of the polyurethane elastic yarn to the fiber surface by, for example, covering the highly lipophilic polyurethane elastic yarn with other fibers to form a covered elastic yarn, thereby further enhancing the unpleasant odor suppression effect.
[0037] In addition, as the fiber substrate constituting the polyester-based fiber structure of the present invention, those in the form of fabric-like materials such as woven fabrics, knitted fabrics and nonwoven fabrics can be preferably used, and the form of the fibers constituting the polyester-based fiber structure may be either short fiber or long fiber, but is not limited thereto.
[0038] The method for producing a polyester fiber structure of the present invention includes a step of supporting the antioxidant, the hydrophilic resin, and the antibacterial agent on a fiber substrate containing polyester fibers.
[0039] Specific methods for the step of supporting the above-mentioned hydrophilic resin, antioxidant, and antibacterial agent on a polyester fiber structure include post-processing with a processing agent by bath treatment, padding, etc., as well as raw yarn modification such as using a base polymer copolymerized with a processing agent as a material constituting the fiber itself or kneading it into the fiber. In the case of raw yarn modification, however, there is a possibility that physical properties such as yarn strength may change significantly or that dirt may easily penetrate into the interior of the fiber, so post-processing treatments such as bath treatment and padding, which do not impair physical properties, are preferred.
[0040] The in-bath treatment referred to here is a method, similar to dyeing, in which the fabric is immersed in a bath containing a processing agent and heated to adhere the processing agent to the fiber structure, and is a processing method suitable for adhering hydrophilic resins and antibacterial agents to polyester fibers.
[0041] The pad method is a method in which the fabric is immersed in a bath containing a processing agent, and then pressed with a mangle roller or the like so that a certain amount of the processing agent adheres to the fabric. The processing agent is then adhered to the fabric by dry heat treatment in a dryer or wet heat treatment in saturated steam at 100°C. This is a processing method suitable for adhering antioxidants to polyester fibers.
[0042] Depending on the other required performance, a shape stabilizer, an anti-slip agent, an antistatic agent, a fixing agent, a softening agent, etc. may be used in combination.
[0043] The polyester fiber structure of the present invention has excellent stain resistance and deodorization properties, and therefore, when evaluated by the difference in luminescence amount ΔLu obtained from an ATP wiping evaluation test before and after a redeposition prevention evaluation test represented by the following formula (1), it is possible to achieve 1000RLu or less, and in a preferred embodiment, it is also possible to achieve 500 or less, and in a more preferred embodiment, 300 or less. There is no restriction on the lower limit, and the closer ΔLu is to 0, the more excellent the stain resistance and deodorization effect against sebum stains is, but in reality, it is usually about 150. ΔLu = Lu(b) - Lu(a) (1) ΔLu: Difference in Lu value before and after the recontamination prevention evaluation test (unit: R Lu) Lu(a): Lu value of polyester fiber structure before anti-redeposition evaluation test (unit: R Lu(b): Lu value of polyester fiber structure after anti-redeposition evaluation test (unit: R
[0044] The ΔLu value is the amount of light emitted from a fluorescent reaction derived from ATP (adenosine triphosphate), ADP (adenosine diphosphate), and AMP (adenosine monophosphate) remaining on the fiber surface obtained by an ATP wiping test (A3 method) before and after the anti-resoiling evaluation test. ATP, ADP, and AMP are components contained in sebum, and therefore serve as indicators of the amount of remaining sebum. The anti-resoiling evaluation test and the ATP wiping test (A3 method) are evaluation tests described below. By satisfying the above range, the polyester fiber structure of the present invention can reduce sebum stains and prevent unpleasant odors and stains caused by sebum stains.
[0045] Furthermore, the polyester fiber structure of the present invention is also excellent in durability, and is capable of maintaining its performance even after 10 washings according to JIS L0217 (1995 edition) 103 method.
[0046] That is, the difference ΔLu in the amount of luminescence obtained from the ATP wiping evaluation test before and after the anti-resoiling evaluation test represented by formula (1) after 10 washings according to the above 103 method is preferably 1000RLu or less, more preferably 800 or less, and particularly preferably 500 or less. There is no lower limit, but it is desirable that ΔLu is close to 0.
[0047] Since the polyester-based fiber structure of the present invention has durable deodorizing and anti-odor properties, it is suitable for use in clothing and bedding, specifically, sports shirts, school uniforms, nursing clothing, white coats, blouses, dress shirts, skirts, slacks, coats, blousons, windbreakers, compression inner clothing, base materials for attaching fans to fan-equipped work clothes, gloves, hats, futon coverings, futon drying covers, curtains, tents, and other clothing and non-clothing applications.
[0048] In particular, it is more suitable for use with compression innerwear and fan-equipped work clothes, which actively expel odorous components such as sweat odor and body odor trapped inside the clothing and can cause discomfort not only to the worker but also to other workers around them. Compression innerwear refers to innerwear that applies pressure to the wearer's body using highly stretchable fabric, with the aim of supporting the wearer's motor functions. By applying pressure and adhering to the skin, the vaporization heat caused by the evaporation of sweat increases the cooling effect on the body.
[0049] The fan-equipped work clothes referred to here refer to work clothes with built-in electric fans, which have been attracting attention in recent years as a way to deal with extreme heat. The purpose of these work clothes is to draw in air from outside the clothing, channel it between the body and the uniform, and cool the body with the heat of vaporization produced when sweat evaporates.
[0050] All of these devices aim to cool the body by evaporating sweat, so they are prone to problems caused by sweat, and in areas that come into close contact with the skin, they are prone to problems caused by sebum.
[0051] Furthermore, in actuality, when working, a combination of these items is often worn, such as wearing a compression inner garment to assist in tasks such as transporting heavy objects, while wearing fan-equipped work clothing to prevent heat stroke, etc. As a result, this is an application in which the decomposition by bacteria of contaminants such as sweat and sebum, and the improvement of the generation of unpleasant odors due to decomposition over time, are particularly desired, and this is also an application in which the effects of the present invention are particularly effective.
[0052] The oxidative decomposition of sebum in the present invention refers to the oxidation of free unsaturated fatty acids and their derivatives, such as triglycerides, oleic acid, linoleic acid, and linolenic acid, which are abundant in sebum components, by heat, UV light, etc., and the alkyl chain is decomposed, generating relatively low molecular weight aldehyde odors such as nonenal. These unsaturated fatty acids are mainly decomposed from the double bond of the unsaturated fatty acid and the alkyl group adjacent to it. Examples of aldehyde odors include acetaldehyde, propanal, butanal, hexanal, octanal, heptanal, decanal, and 2-nonenal.
[0053] In addition to this oxidative decomposition, triglycerides and free fatty acids contained in sebum are broken down by the metabolism of normal skin bacteria such as Moraxella, Micrococcus, and Corynebacterium, producing short-chain fatty acids such as acetic acid and medium-chain fatty acids, which produce a unique unpleasant odor.
[0054] The polyester fiber structure of the present invention can achieve an aldehyde odor of 1 ppm or less generated in an oxidative decomposition test of sebum. In a preferred embodiment, it is also possible to achieve 0.5 ppm or less. The lower limit is preferably lower, and it is preferable to achieve an amount of 0 ppm generated, but in reality, it is particularly preferable to achieve a level below the detection limit (0 ppm) in the measurement described below.
[0055] The method for the oxidative decomposition test of sebum and the method for measuring aldehyde odor are as described below. EXAMPLES
[0056] [Evaluation method] (Method for measuring weight-average molecular weight in terms of polyethylene glycol) The weight average molecular weight calculated as polyethylene glycol was measured under the following conditions. Apparatus: Gel permeation chromatograph GPC (Shimadzu Corporation LC-20AD) Detector: Differential refractive index detector RI (Waters RI-8020 type, sensitivity 32x) Column: TSKgel G3000PW XL (Manufactured by Tosoh) Solvent: 0.1M sodium chloride solution Flow rate: 0.8 mL / min Column temperature: 23℃ Injection volume: 0.1 mL Standard samples: polyethylene glycol, polyethylene oxide Data processing: Shimadzu Prominence GPC system
[0057] The sample preparation method is shown below. 1. Take 5 g of polyester fiber from the polyester fiber structure, add this to a test tube with 30 mL of ammonia water, and seal tightly. 2.Heat at 120℃ for 5 hours and allow to cool. 3. Open the cap and add 30 mL of purified water, then add 6 M hydrochloric acid until a precipitate derived from terephthalic acid appears, and centrifuge. 4. Collect the supernatant and adjust the hydrochloric acid concentration to 0.1M. 5. The mixture was filtered through a 0.45 μm filter and used for molecular weight measurement.
[0058] When polyethylene terephthalate fibers are used and the polyether component is a polyethylene glycol component, the above measurement may detect ethylene glycol components derived from polyethylene terephthalate. In this case, taking into account the purpose of the measurement, the polyethylene glycol component is the subject of evaluation.
[0059] (NMR measurement) The same operations as in Sample Preparation Methods 1 to 3 for the measurement of the weight average molecular weight in terms of polyethylene glycol were carried out, and 5 mL of the resulting supernatant was dried and then dissolved in 1 mL of 50% deuterated chloroform / deuterated hexafluoro-2-propanol, which was then placed in an NMR tube and measured using the following measurement method. 1 H-NMR measurements were performed.
[0060] When the peak derived from the internal standard tetramethylsilane is set at 0 ppm in the NMR spectrum chart, a strong peak is detected at 3.7 to 3.8 ppm, indicating the presence of a polyethylene glycol component. ( 1 H-NMR measurement method) [conditions] Device name: ECA400 (manufactured by JEOL) Measurement nucleus: 1H Observation frequency: 399.78 MHz Solvent: Deuterated chloroform + deuterated hexafluoro-2-propanol (1 / 1 v / v) Internal standard: Tetramethylsilane (TMS) [detail] Measurement method: Single pulse Spectral width: 8000 Hz Pulse width: 6.45 μs (45° pulse) Pulse waiting time: 15.0 s Data points: 32768
[0061] (Re-soiling prevention evaluation test method) 150ml of the soiled solution containing the following components and 10 stainless steel balls with a diameter of 6.4mm are placed in a 450ml test bottle attached to a laundermeter type washing tester and preheated to 40±2℃. Three test pieces cut to 5cm x 10cm are placed in the test bottle, the lid is put on, and the tester is adjusted to 40±2℃ and rotated for 20 minutes. After completion, the test pieces are removed, washed with running water and air-dried. This is repeated 20 times to evaluate re-soiling prevention.
[0062] (Creating contaminated liquid) Weigh out 17.5 g of HEAL'S ECE FORMULATION NON PHOSPHATE REFERENCE DETERGENT (A), 2.8 g of oily contaminant, and 0.95 g of dry contaminant. Grind the detergent in a mortar to knead the contaminants, then add water little by little and knead until the total volume is 1 L.
[0063] The components of the oily and dry staining agents used above are shown in Tables 1 and 2.
[0064] [Table 1]
[0065] [Table 2]
[0066] (ATP Wipe Evaluation Test Method) Remove the "Lucipack (registered trademark)" A3 Surface manufactured by Kikkoman Biochemifa Corporation from the cotton swab holder and moisten the cotton swab with pure water. Press the cotton swab of the "Lucipack (registered trademark)" A3 Surface, which has been moistened with pure water, against the contaminant-attached part of the test piece before and after the recontamination prevention evaluation test, and wipe 5 cm in the vertical and horizontal directions of the woven and knitted fabrics 10 times. Return the "Lucipack (registered trademark)" A3 Surface to the cotton swab holder, press it in until it reacts with the reagent built into the cotton swab and the tip of the holder, and shake it up and down 10 times. Set the "Lucipack (registered trademark)" A3 Surface in an ATP swabbing test device (Lumitester PD-30 manufactured by Kikkoman Biochemifa Corporation) and measure the amount of luminescence derived from ATP, ADP, and AMP caused by beef tallow contained in the contaminant. The Lu value before the anti-soiling re-evaluation test was designated as Lu(a), and the Lu value after the anti-soiling re-evaluation test was designated as Lu(b), and the difference in Lu values, ΔLu, was evaluated using the following formula. ΔLu = Lu(b) - Lu(a) (1) ΔLu: Difference in Lu value before and after the recontamination prevention evaluation test (unit: R Lu) Lu(a): Lu value of polyester fiber structure before anti-redeposition evaluation test (unit: R Lu(b): Lu value of polyester fiber structure after anti-redeposition evaluation test (unit: R The smaller ΔLu is, the more the accumulation of sebum and the like is suppressed.
[0067] (Washing instructions) JIS L0217 (2012 edition) 103 method was used. Specifically, a household electric washing machine (Panasonic NA-F50B9) with a centrifugal spin-drying device specified in JIS C9606 (2007 edition) was used, and water with a liquid temperature of 40°C was added up to the water level line indicating the standard water volume, and 20 g of synthetic laundry detergent (Kao Attack Highly Active Bio EX) was added and dissolved in the ratio corresponding to the standard usage to make the washing liquid. The sample and load cloth were added to this washing liquid so that the liquor ratio was 1:30, and the operation was started.
[0068] After 5 minutes of treatment, the machine was stopped, the sample and the loaded fabric were dehydrated in a spin dryer, and then the washing liquid was replaced with fresh water at 30°C or less and rinsed for 2 minutes at the same bath ratio. After rinsing for 2 minutes, the machine was stopped, the sample and the loaded fabric were dehydrated, rinsed again for 2 minutes, dehydrated, and hung to dry without being exposed to direct sunlight.
[0069] (Ammonia deodorizing properties) A 500ml container was filled with ammonia gas so that the initial concentration was 300ppm, cut into a 10cm x 5cm sample, and then sealed. After leaving it for 30 minutes, the residual ammonia concentration was measured using a gas detector. The same procedure was performed without the sample, and the residual ammonia concentration was measured as the blank test concentration, and the deodorization rate (%) was calculated according to the following formula. Ammonia deodorization rate (%) = (1-(gas detector tube measured concentration) / (blank test concentration)) x 100 The larger the value, the better the deodorizing properties.
[0070] (Isovaleric acid deodorizing properties) In a 500ml container, a sample cut to 10cm x 5cm was placed in the same way as for ammonia, and isovaleric acid gas was added to make the initial concentration 300ppm, then the container was sealed, and after leaving it for 30 minutes, the residual isovaleric acid concentration was measured using a gas detector tube. At this time, the same operation was performed without the sample, and the residual isovaleric acid concentration was measured, which was used as the blank test concentration, and the deodorization rate (%) was calculated according to the following formula. Isovaleric acid deodorization rate (%) = (1-(gas detector tube measured concentration) / (blank test concentration)) x 100 The larger the value, the better the deodorizing properties.
[0071] (Antibacterial activity evaluation method) The measurements were performed according to the bacterial liquid absorption method of JIS L1902 (2015 edition). Details are as follows. 1. Place 0.4g of the test piece in a vial, drip 0.2ml of the test bacteria liquid, and then close the vial. 2. Incubate the vial at 37°C for 24 hours. 3. Add 20 ml of washing solution to wash out the test bacteria from the test piece, and measure the number of live bacteria in the washing solution using the pour plate culture method. 4. Calculate the antibacterial activity value according to the formula below. Antibacterial activity value = {log (control sample, viable bacteria count after incubation) - log (control sample, viable bacteria immediately after inoculation) log(test sample · viable bacteria count after incubation)-log(test sample · viable bacteria count immediately after inoculation)} A standard cloth (cotton) was used as a control sample. When the antibacterial activity value is greater than the growth value (antibacterial activity value of the target sample), this is preferable because it means that the bacteria are not growing but are rather decreasing. As the target bacterial species, Corynebacterium, which is the cause of body odor, was selected.
[0072] (ΔL * Evaluation method) After wearing and washing the garment 10 times, the fabric around the neck, which is particularly prone to darkening, was cut into 5cm x 10cm pieces and measured by brightness (L * The L value was measured using a multi-light source spectrophotometer (CM-3700D) manufactured by Konica Minolta, Inc., folded in three, using the total reflection method. * Value L * (a) L after recontamination prevention evaluation test * Value L * (b) and L in the following formula * Difference in value ΔL * was evaluated. ΔL * =L * (a)-L * (b) (1) ΔL *:L before and after repeated wearing * Difference in values L * (a): L of polyester fiber structure before repeated wearing * value L * (b): L of polyester fiber structure after repeated wearing * value L * (b) The larger the value, the better the cleaning property and the better the stain resistance. * The smaller the value, the more the dark spots caused by sebum accumulation are suppressed.
[0073] (Sebum oxidation decomposition test / aldehyde odor measurement) A 0.1 g sample of a model sebum component, a mixture of squalene (reagent manufactured by Wako Pure Chemical Industries, Ltd.) and linoleic acid (reagent manufactured by Wako Pure Chemical Industries, Ltd.) in a mass ratio (squalene:linoleic acid) of 2:8, was dropped onto a test piece of cloth cut to 2.5 cm x 2.5 cm, and the sample was placed into a polystyrene container with a screw cap (PS Screw Bottle SS-50 manufactured by AS ONE). The opening was sealed with Parafilm M (manufactured by Bemis Flexible Packaging), and the sample was then sealed with the screw cap and left to stand for 4 days in a constant temperature and humidity chamber adjusted to a temperature of 40°C and a humidity of 60%RH. The sample was then left to stand for 20 minutes in a room adjusted to a temperature of 20°C and a humidity of 65%RH with the container sealed. The screw cap was then opened and both ends of an acetaldehyde odor detection tube (Gastec N-92L) were removed using the chip breaker attached to the gas sampler (Gastec GV-100) and then inserted into the inlet rubber of the gas sampler. A hole was made in the parafilm and 100 mL was drawn in. After leaving it to stand for 2 minutes, the concentration of aldehyde odor in the container was measured.
[0074] (Odor sensory evaluation after wearing test) The fiber structures of the Examples and Comparative Examples were used as the base material for compression innerwear worn inside fan-equipped workwear, or as the base material for fan-equipped workwear, and a wear test was conducted. After 10 repeated cycles of wearing and washing at home, the odor of the fabric was evaluated sensorily. When an aldehyde-based odor is generated, a unique irritating odor is observed. Based on the results of the sensory evaluation, the odor suppression level was evaluated on a four-level scale of A, B, C, and D. A: There was almost no unpleasant odor when wearing the product, and no unpleasant odor was noticed even after repeated use. B: The unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use. C: The unpleasant odor was reduced when worn, but the unpleasant odor gradually increased with repeated use. D: An unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use. E: An unpleasant odor was felt when worn, and the unpleasant odor significantly increased with repeated use.
[0075] (Pickup rate) The pick-up rate is the ratio of the difference in mass between the processed fabric before immersion in the processing liquid and the fabric after immersion in the processing liquid and squeezing, and is expressed by the following formula (2). Pick-up rate (%) = (mass of processed fabric after soaking and squeezing - mass of processed fabric before soaking) / mass of processed fabric before soaking × 100 ... (2).
[0076] (Amount of each processing agent applied) Bath treatment In the bath treatment, the amount of the processing agent attached to the fiber was measured by the following method. Approximately 300 g of untreated fabric was completely dried at 100°C for 60 minutes, then the fabric was left to stand in a desiccator containing silica gel as a desiccant for about 20 minutes, and immediately after cooling, the fabric mass was measured using a precision balance. The fabric mass was also measured in the same manner after bath treatment using the method described in the Examples, and the amount of adhesion was measured. Amount of adhesion in bath treatment (%) = (mass of fabric after bath treatment - mass of untreated fabric) / Fabric mass after bath treatment × 100…(3) When two or more types of processing agents were used in combination, the adhesion amount was measured when each processing agent was used alone under the same conditions, and was considered as the adhesion amount for each processing agent. It was confirmed that the values were not contradictory to the measurement results of the total adhesion amount when two or more types of processing agents were used in combination.
[0077] Pad Method Based on the above pickup rate measurement, the amount of adhesion to the fabric after processing by the pad method was calculated using the following formula (4). Amount of adhesion in the pad method (%) = Pick-up rate (%) / 100 × concentration of processing agent (g / L) / 10…(4) In the bath treatment and pad method, if any of the antioxidants, hydrophilic resins, or antibacterial agents were already attached to the fabric before each treatment, the amounts of these agents attached were subtracted from the results and the calculations were corrected to reflect the amounts relative to the fiber base.
[0078] (Production of polyester resin containing polyether component) A polyester resin was obtained by mixing a polyester component of terephthalic acid and ethylene glycol as a hard segment made of polyester, and a polyethylene glycol component as a soft segment made of a polyether component in an arbitrary ratio and simultaneously carrying out a condensation reaction.
[0079] [Example 1] A polyester knitted fabric made of 90% by mass of polyethylene terephthalate fiber having a fineness of 66T-96F / 10% by mass of 22T-2F polyurethane elastic yarn (core yarn: polyurethane elastic yarn, covering yarn: polyethylene terephthalate) was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., block copolymer consisting of polyester units and polyalkylene glycol units consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1 "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 1 are shown in Table 3. The polyester fiber structure obtained in Example 1 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, almost no unpleasant odor was felt when worn, and no unpleasant odor was felt even after repeated use, so that the odor prevention property when worn is rated A.
[0080] [Example 2] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber having a fineness of 66T-96F / 10% by mass of 22T-2F polyurethane elastic yarn was immersed in a processing solution containing water as a solvent, Silverdur (a silver-based antibacterial agent manufactured by Dow Chemical), 1.5% owf, TM-SS21 (a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, manufactured by Matsumoto Yushi Seiyaku Co., Ltd., solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 2 are shown in Table 3. The polyester fiber structure obtained in Example 2 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0081] [Example 3] A polyester resin P-1 was produced using MR-T100 (manufactured by Osaka Kasei Co., Ltd., pyridine-based antibacterial agent, solid content 19%); 1% owf and a polyethylene glycol with a weight average molecular weight of 1700 g / mol based on the manufacturing method of the polyester resin containing the above polyether component, with a mass ratio of the polyester component and the polyethylene glycol component being 1:3; 0.5% owf and acetic acid were added to the processing solution containing 0.5 g / L. A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber with a fineness of 66T-96F / 10% by mass of 22T-2F polyurethane elastic yarn was immersed in the processing solution, sealed, and then subjected to a heat treatment in a bath at 130°C for 60 minutes, followed by rinsing with running water for 1 minute and drying to complete the bath treatment, and then a treatment by padding was performed. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1 "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 3 are shown in Table 3. The polyester fiber structure obtained in Example 3 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0082] [Example 4] Based on the manufacturing method of polyester resin containing MR-T100 (Osaka Kasei Co., Ltd., pyridine-based antibacterial agent, solid content 19%); 1% owf and the above-mentioned polyether component, polyester resin P-2 was manufactured using polyethylene glycol with a weight average molecular weight of 5800 g / mol, with a mass ratio of polyester component to polyethylene glycol component of 1:3; 0.5% owf and acetic acid 0.5 g / L. A polyester knitted fabric knitted with a blended yarn of 90% by mass of polyethylene terephthalate fiber with a fineness of 66T-96F / 10% by mass of 22T-2F polyurethane elastic yarn was immersed in the processing solution containing 0.5% owf and acetic acid, and then sealed. After that, it was subjected to a heat treatment in a bath at 130°C for 60 minutes, followed by rinsing with running water for 1 minute and drying to complete the bath treatment, and then a treatment by the pad method was performed. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1 "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 4 are shown in Table 3. The polyester fiber structure obtained in Example 4 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0083] [Example 5] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber with a fineness of 66T-96F / 10% by mass of 22T-2F polyurethane elastic yarn was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TO-SR-1 (manufactured by Takamatsu Oil Co., Ltd., block copolymer consisting of terephthalic acid and / or isophthalic acid and alkylene glycol and / or polyalkylene glycol, solid content 10%), 3% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 5 are shown in Table 3. The polyester fiber structure obtained in Example 5 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, although the unpleasant odor when worn was reduced, the unpleasant odor gradually increased with repeated use, so the odor prevention when worn was rated C.
[0084] [Example 6] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the above processed fabric was immersed in a processing solution containing 7.5 g / L of DL-malic acid (Nacalai Tess Nacalai standard Grade 1) using water as a solvent, and the pickup rate was reduced to 80%, followed by heat treatment at 130°C for 2 minutes and then heat treatment at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 6 are shown in Table 3. The polyester fiber structure obtained in Example 6 was used to sew a compression inner to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so the odor prevention when worn was rated B.
[0085] [Example 7] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of L(+)-ascorbic acid (manufactured by Nacalai Tesque, Inc., JIS special grade reagent); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 7 are shown in Table 3. The polyester fiber structure obtained in Example 7 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0086] [Example 8] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of DL-α-tocopherol (Nacalai Tesque, Inc., Nacalai standard special grade), and the pickup rate was reduced to 80%, followed by heat treatment at 130°C for 2 minutes and then heat treatment at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 8 are shown in Table 4. The polyester fiber structure obtained in Example 8 was used to sew a compression inner to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0087] [Example 9] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, acetic acid 0.5 g / L, and TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), and 5% owf, and then sealed and subjected to heat treatment in a bath at 130°C for 60 minutes, followed by rinsing with running water for 1 minute and drying to complete the bath treatment, and then treatment by the pad method was performed. That is, the above processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 9 are shown in Table 4. The polyester fiber structure obtained in Example 9 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor was reduced when worn repeatedly, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0088] [Example 10] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the above processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of DL-malic acid (Nacalai Tesque, Inc., Nacalai standard grade 1); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 10 are shown in Table 4. The polyester fiber structure obtained in Example 10 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0089] [Example 11] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the above processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of L(+)-ascorbic acid (manufactured by Nacalai Tesque, Inc., JIS special grade reagent); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 11 are shown in Table 4. The polyester fiber structure obtained in Example 11 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0090] [Example 12] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the above processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of DL-α-tocopherol (Nacalai Tesque, Inc., Nacalai standard special grade), and after squeezing the pickup rate to 80%, it was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 12 are shown in Table 4. The polyester fiber structure obtained in Example 12 was used to sew a compression inner to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0091] [Example 13] A polyester fabric woven using polyethylene terephthalate fibers with a fineness of 84T-72F as warp and weft yarns was immersed in a processing solution containing water as the solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., block copolymer consisting of polyester units and polyalkylene glycol units consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, followed by rinsing with running water for 1 minute and drying to complete the bath treatment, and then treatment by the pad method was performed. That is, the above processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Example 13 are shown in Table 4. The polyester fiber structure obtained in Example 13 was used to sew fan-equipped work clothes and a wearing test was conducted. As a result, the unpleasant odor when worn was reduced, and the odor was also reduced even with repeated use, so that the odor prevention when worn was rated B.
[0092] [Comparative Example 1] A polyester fiber structure was obtained without processing the knitted fabric described in Example 1. The measurement results of the polyester fiber structure obtained in Comparative Example 1 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 1 was used to sew an inner layer of fan-equipped workwear, and a wearing test was conducted. As a result, an unpleasant odor was felt when worn, and the unpleasant odor significantly increased with repeated use, so the odor prevention property when worn was rated E.
[0093] [Comparative Example 2] A polyester fiber structure was obtained without processing the knitted fabric described in Example 9. The measurement results of the polyester fiber structure obtained in Comparative Example 2 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 2 was used to sew an inner layer of a fan-equipped work suit, and a wearing test was conducted. As a result, an unpleasant odor was felt when worn, and the unpleasant odor significantly increased with repeated use, so that the odor prevention property when worn was rated E.
[0094] [Comparative Example 3] A polyester fiber structure was obtained without processing the woven fabric described in Example 13. The measurement results of the polyester fiber structure obtained in Comparative Example 3 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 3 was used to sew fan-equipped work clothes, and a wearing test was conducted. As a result, an unpleasant odor was felt when worn, and the unpleasant odor significantly increased with repeated use, so the odor prevention property when worn was rated E.
[0095] [Comparative Example 4] A polyester knitted fabric made of a 90% by mass polyethylene terephthalate fiber / 10% by mass 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent and 0.5 g / L of acetic acid, sealed, and then heat-treated in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried to complete the bath treatment, and then treated by padding. That is, the above-mentioned processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was squeezed to 80%, and then heat-treated at 130°C for 2 minutes and then heat-treated at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 4 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 4 was used to sew a compression inner garment to be worn inside a fan-equipped work suit. A wearing test was conducted, and an unpleasant odor was felt when the garment was worn, and the unpleasant odor increased with repeated use. Therefore, the odor prevention property when worn was rated D.
[0096] [Comparative Example 5] A polyester knitted fabric made of a 90% by mass polyethylene terephthalate fiber / 10% by mass 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as the solvent, MR-T100 (manufactured by Osaka Kasei Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, and 0.5 g / L of acetic acid, sealed, and then heat-treated in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried to complete the bath treatment, and then treated by the pad method. That is, the above-mentioned processed fabric was immersed in a processing solution containing water as the solvent and 7.5 g / L of citric acid (manufactured by Nacalai Tesque Co., Ltd., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was squeezed to 80%, and then heat-treated at 130°C for 2 minutes and then heat-treated at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 5 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 5 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so the odor prevention property when worn was rated D.
[0097] [Comparative Example 6] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units formed of terephthalic acid and / or isophthalic acid and alkylene glycol, and polyalkylene glycol units, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by the pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 6 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 6 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0098] [Comparative Example 7] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 2.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 7 are shown in Table 5. The polyester fiber structure obtained in Comparative Example 7 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0099] [Comparative Example 8] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 15 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 8 are shown in Table 6. The polyester fiber structure obtained in Comparative Example 8 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was conducted. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0100] [Comparative Example 9] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 0.8% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 9 are shown in Table 6. The polyester fiber structure obtained in Comparative Example 9 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0101] [Comparative Example 10] A polyester knitted fabric made of a blended yarn of 90% by mass of polyethylene terephthalate fiber and 10% by mass of 22T-2F polyurethane elastic yarn with a fineness of 66T-96F was immersed in a processing solution containing water as a solvent, MR-T100 (manufactured by Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 30% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then a treatment was performed by a pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 10 are shown in Table 6. The polyester fiber structure obtained in Comparative Example 10 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0102] [Comparative Example 11] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 2.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester-based fiber structure. The measurement results of the fiber structure obtained in Comparative Example 11 are shown in Table 6. The fiber structure obtained in Comparative Example 11 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0103] [Comparative Example 12] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 5% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and the bath treatment was completed, and then the fabric was treated by the pad method. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 15 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 12 are shown in Table 6. The polyester fiber structure obtained in Comparative Example 12 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0104] [Comparative Example 13] A polyester knitted fabric made of polyethylene terephthalate fibers with a fineness of 84T-72F was immersed in a processing solution containing water as a solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 0.8% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, followed by rinsing with running water for 1 minute and drying to complete the bath treatment, and then treatment by the pad method was performed. That is, the processed fabric was immersed in a processing solution containing water as a solvent and 7.5 g / L of citric acid (Nacalai Tesque, Inc., Nacalai standard Class 1, "citric acid (anhydrous)"); the pickup rate was reduced to 80%, and the fabric was heat-treated at 130°C for 2 minutes and then at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 13 are shown in Table 6. The polyester fiber structure obtained in Comparative Example 13 was used to sew a compression inner garment to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, an unpleasant odor was felt when worn, and the unpleasant odor increased with repeated use, so that the odor prevention property when worn was rated D.
[0105] [Comparative Example 14] A polyester knitted fabric made of a polyethylene terephthalate fiber having a fineness of 84T-72F was immersed in a processing solution containing water as the solvent, MR-T100 (Osaka Chemical Industry Co., Ltd., pyridine-based antibacterial agent, solid content 19%), 1% owf, TM-SS21 (Matsumoto Yushi Seiyaku Co., Ltd., a block copolymer consisting of polyester units and polyalkylene glycol units, consisting of terephthalic acid and / or isophthalic acid and alkylene glycol, solid content 10%), 30% owf, and 0.5 g / L of acetic acid, and then sealed. The fabric was subjected to a heat treatment in a bath at 130°C for 60 minutes, rinsed with running water for 1 minute, dried, and then treated with water as the solvent and citric acid (Nacalai Tesque, Inc., The processed fabric was immersed in a processing solution containing 7.5 g / L of "citric acid (anhydrous)" (Nacalai Class 1 standard), and the pickup rate was reduced to 80%, followed by heat treatment at 130°C for 2 minutes and then heat treatment at 170°C for 1 minute to obtain a polyester fiber structure. The measurement results of the polyester fiber structure obtained in Comparative Example 14 are shown in Table 7. The polyester fiber structure obtained in Comparative Example 14 was used to sew a compression inner to be worn inside a fan-equipped work suit, and a wearing test was performed. As a result, although the unpleasant odor when worn was reduced, the unpleasant odor gradually increased with repeated use, so the odor prevention when worn was rated C.
[0106] [Table 3]
[0107] [Table 4]
[0108] [Table 5]
[0109] [Table 6]
Claims
1. The fiber substrate includes a polyester fiber. At least one antioxidant selected from the group consisting of citric acid, malic acid, ascorbic acid, tocopherol, and derivatives thereof is present on a surface of the fiber substrate in an amount of 0.3 to 0.85% by mass relative to the fiber substrate; A hydrophilic resin containing a polyether component is present on a surface of the fiber substrate in an amount of 0.1 to 0.3% by mass relative to the fiber substrate, A polyester-based fiber structure having an antibacterial agent on the surface of the fiber substrate.
2. 2. The polyester fiber structure according to claim 1, wherein the difference ΔLu in the amount of luminescence obtained from an ATP wiping evaluation test before and after a redeposition prevention evaluation test represented by the following formula (1) is 1000 RLu or less. ΔLu=Lu(b)-Lu(a) (1) ΔLu: Difference in Lu value before and after the resoiling prevention evaluation test (unit: RLu) Lu(a): Lu value of the polyester fiber structure before the anti-resoiling evaluation test (unit: RLu) Lu(b): Lu value of the polyester fiber structure after the anti-redeposition evaluation test (unit: RLu)
3. 3. The polyester fiber structure according to claim 1 or 2, wherein the antioxidant is citric acid and its derivatives.
4. the hydrophilic resin is a polyester resin, the weight average molecular weight, calculated as polyethylene glycol, of the polyether component which is the hydrophilic segment of the polyester resin is in the range of 1500 to 6000 g / mol, which is obtained by size exclusion chromatography; The polyester fiber structure according to any one of claims 1 to 3, wherein the molecular weight distribution (ratio of weight average molecular weight in terms of polyethylene glycol to number average molecular weight in terms of polyethylene glycol) is in the range of 1.00 to 1.
35.
5. The polyester fiber structure according to any one of claims 1 to 4, wherein the antibacterial agent is a pyridine-based antibacterial agent.
6. 6. The polyester fiber structure according to claim 1, wherein the polyurethane elastic yarn is contained in the fiber substrate in an amount of 1 to 30% by mass.
7. A compression inner garment comprising the polyester fiber structure according to any one of claims 1 to 6.
8. 7. A method for producing a polyester fiber structure according to claim 1, comprising a step of supporting at least one antioxidant selected from the group consisting of citric acid, malic acid, ascorbic acid, tocopherol and derivatives thereof, a hydrophilic resin containing a polyether component as a hydrophilic segment, and an antibacterial agent on a fiber substrate containing polyester fibers.
Citation Information
Patent Citations
Dehydration washing machine
JP1986068093A
deodorant
JP1989020852A
Method for using paper diaper
JP1997271484A
Deodorizing textile product
JP2004052208A
Deodorant fiber structure
JP2013067918A