Method for manufacturing plate-shaped body
By optimizing the processing conditions for surface grinding with a vitrified grindstone containing diamond abrasive grains, the wear rate of grinding wheels is reduced, enhancing the efficiency and cost-effectiveness of SiC polycrystalline substrate processing.
Patent Information
- Application Number
- JP2020185585
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-06
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-06
AI Technical Summary
The high wear rate of vitrified grinding wheels used in surface grinding processes for silicon carbide (SiC) polycrystalline substrates, particularly due to the material's hardness, leads to increased processing costs and inefficiencies.
Optimized processing conditions for surface grinding, including spindle rotation speed, chuck table rotation speed, and machining feed rate, are applied using a vitrified grindstone containing diamond abrasive grains to reduce the wear rate of the grinding wheel.
The optimized conditions significantly decrease the wear rate of the grinding wheel, improving the efficiency and reducing costs associated with processing SiC polycrystalline substrates.
Smart Images

Figure 0007589507000001 
Figure 0007589507000002 
Figure 0007589507000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a plate-shaped body, which includes a lapping process in which a difficult-to-cut plate-shaped body is processed to a desired thickness, and a surface grinding process in which the plate-shaped body surface after the lapping process is surface ground to process it into a highly flat and smooth surface, and in particular to a method for manufacturing a plate-shaped body that can reduce wear on the grinding wheel used in the surface grinding process. [Background technology]
[0002] Silicon carbide (SiC) has a band gap three times larger than silicon (Si) (4H-SiC: 3.8 eV, 6H-SiC: 3.1 eV, silicon: 1.1 eV) and a high thermal conductivity (5 W / cm K, silicon: 1.5 W / cm K). In recent years, SiC single crystals have begun to be used as a substrate material for power devices. For example, compared to conventional Si power devices, SiC power devices have achieved a withstand voltage 5 to 10 times larger and an operating temperature several hundred degrees higher. Furthermore, they can reduce the power loss of the element to about one-tenth, so they have been put to practical use in inverters for railway vehicles, etc.
[0003] SiC single crystals as substrate materials are usually produced by a gas phase method called sublimation recrystallization method (modified Lely process) (see, for example, Non-Patent Document 1), and are processed to the desired diameter and thickness.
[0004] The modified Lely process is a method for growing bulk SiC single crystals by heating and subliming solid SiC raw material (usually powder) at high temperatures (over 2,400°C). The sublimated Si atoms and carbon atoms are transported by diffusion through an inert gas atmosphere as vapor at 2,400°C, and become supersaturated on a seed crystal placed at a lower temperature than the raw material, causing it to recrystallize.
[0005] However, because the process temperature in the modified Lely process is very high at over 2,400°C, it is extremely difficult to control the temperature and convection during crystal growth, and to control crystal defects, and the SiC single crystal substrates produced by this method contain numerous crystal defects called micropipes and other crystal defects (stacking faults, etc.), making it extremely difficult to manufacture high-quality SiC single crystal substrates that can withstand electronic device use with a high yield. As a result, high-quality SiC single crystal substrates with few crystal defects that can be used for electronic devices are very expensive, and devices using such SiC single crystal substrates are also expensive, which has hindered the widespread use of SiC single crystal substrates.
[0006] In view of this, in recent years, a method has been proposed for producing a SiC substrate in which a SiC single crystal thin plate layer is formed on a SiC polycrystalline substrate by preparing a SiC single crystal substrate and a SiC polycrystalline substrate, performing a step of bonding the SiC single crystal substrate and the SiC polycrystalline substrate together, and then performing a step of thinning the SiC single crystal substrate (see, for example, Non-Patent Document 2).
[0007] According to this method for manufacturing a SiC substrate, the thickness of the SiC single crystal substrate can be reduced to a few tenths or even a few hundredths of that of the conventional method. Therefore, the cost of the SiC substrate can be significantly reduced compared to the conventional method in which the entire substrate is made of expensive and high-quality SiC single crystal. In addition, since elements such as power devices can be formed on a high-quality SiC single crystal layer with few crystal defects, the device performance and manufacturing yield can be significantly improved.
[0008] In the process of bonding such a SiC single crystal substrate and a SiC polycrystalline substrate, the SiC polycrystalline substrate is required to be dense and highly pure, as well as highly flat. For this reason, a chemical vapor deposition method (hereinafter, sometimes referred to as a "CVD method") is used to manufacture the SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate using the CVD method is described in Patent Document 1. The method for manufacturing a SiC polycrystalline substrate described in Patent Document 1 will be described below.
[0009] First, the inside of a growth furnace in which a carbonaceous support substrate (e.g., a graphite support substrate) 1 shown in Fig. 3(A) is placed is set to an environment of 1300°C or higher, and Si-based raw material gas such as SiH4, C-based raw material gas such as CH4, nitrogen gas as an impurity gas, and hydrogen gas as a carrier gas are introduced into the furnace, and a SiC polycrystalline film 2 shown in Fig. 3(B) is deposited on the front and back surfaces and the outer peripheral end surface of the carbonaceous support substrate 1 by thermal reaction. Then, the carbonaceous support substrate 1 on which the SiC polycrystalline film 2 is deposited is taken out of the growth furnace, and the carbonaceous support substrate 1 is beveled to expose the end surface of the carbonaceous support substrate 1 as shown in Fig. 3(C), and then only the carbonaceous support substrate 1 is burned using an electric furnace or the like, and two SiC polycrystalline substrates 3 consisting of the SiC polycrystalline film 2 formed on the front and back surfaces of the carbonaceous support substrate 1 as shown in Fig. 3(D) are obtained.
[0010] However, in this manufacturing method using the CVD method, the thickness of the formed SiC polycrystalline film 2 tends to be large near the outer edge (outer peripheral portion) of the carbonaceous support substrate 1 as shown in FIG. 3(B), and therefore the peripheral portion of the obtained SiC polycrystalline substrate 3 tends to be thicker than the central portion as shown in FIG. 3(D). Therefore, after burning and removing the carbonaceous support substrate 1, the following process was required to adjust the thickness and flatness of the SiC polycrystalline substrate 3 by grinding and polishing.
[0011] That is, as shown in Figures 4(A)-(B), a cut-out process is performed to remove the peripheral portion of the SiC polycrystalline substrate 3, a lapping process is performed to process the SiC polycrystalline substrate 3 to approximately the desired thickness as shown in Figure 4(C), a bevel process is performed to process the SiC polycrystalline substrate 3 to the desired diameter and then chamfer the end faces of the SiC polycrystalline substrate 3, a surface grinding process is performed to surface grind the surface of the SiC polycrystalline substrate 3 obtained in the lapping process to process it into a highly flat and smooth surface as shown in Figure 4(D), and a polishing process is performed to remove linear processing marks (not shown) generated in the surface grinding process by chemical mechanical polishing (mechanochemical polishing) and to make the surface of the SiC polycrystalline substrate 3 into a mirror finish as shown in Figure 4(E). Through these processes, the SiC polycrystalline substrate to be used for manufacturing SiC substrates will be in a desired state. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Japanese Patent Application Publication No. 08-026714 [Patent Document 2] JP 2018-051646 A [Non-patent literature]
[0013] [Non-Patent Document 1] Yu.M.Tairov and VFTsvetkov: J.of Cryst.Growth 43(1978)209 [Non-Patent Document 2] Journal of the Japan Society for Precision Engineering, 2017, Vol. 83, No. 9, pp. 833-836 Summary of the Invention [Problem to be solved by the invention]
[0014] By the way, silicon carbide (SiC) is a material with very high hardness and difficult to cut, but it is possible to reduce the processing time and processing cost of SiC polycrystalline substrates by low-pressure double-sided lapping using boron carbide (B4C) abrasive grains with a grit size of about 100 (ISO 8486 designation) to 300 (ISO 8486 designation), for example, 280 (ISO 8486 designation). However, on the other hand, since steep unevenness is formed on the surface of the SiC polycrystalline substrate after the lapping process, when the SiC polycrystalline substrate is surface-ground using a vitrified grinding wheel containing diamond abrasive grains with a grit size of about 6000 (ISO 8486 designation) to 8000 (ISO 8486 designation), for example, 7000 (ISO 8486 designation), after the beveling process, there is a problem that the wear rate of the grinding wheel [(wear amount of grinding wheel / machined amount of workpiece) x 100%] becomes high. Specifically, if one side of a SiC polycrystalline substrate is surface ground by 10 μm in the first surface grinding step, and the other side of the SiC polycrystalline substrate is surface ground by 20 μm in the second surface grinding step, the wear rate of the grinding wheel in the first step is 700% to 350%, and in the second step is 200% to 250%, which is high, and this poses a major problem because vitrified grinding wheels containing diamond abrasive grains are expensive.
[0015] The present invention has been made with attention to these problems, and its object is to provide a method for manufacturing a plate-shaped body having a lapping process and a surface grinding process, which can reduce the wear rate of a vitrified grinding wheel (a grinding wheel containing diamond abrasive grains and a vitrified binder) used in the surface grinding process. [Means for solving the problem]
[0016] In order to solve the above problems, the present inventors conducted repeated experiments while changing the processing conditions of the grinding device (see, for example, Patent Document 2) used in the surface grinding process, specifically, the "rotation speed of the spindle" to which the vitrified grinding wheel is attached, the "rotation speed of the chuck table" that holds the plate-shaped body, and the "processing feed speed" that moves the grinding wheel and the plate-shaped body relatively in the processing feed direction, and as a result, they found appropriate conditions that reduce the wear rate of the grinding wheel.
[0017] That is, the appropriate conditions for surface grinding the lapped surface of a plate-shaped body (hereinafter sometimes referred to as the "#280 surface") after the lapping process using boron carbide (B4C) abrasive grains #280 (ISO 8486 designation) using a grinding device using a vitrified grinding wheel containing diamond abrasive grains #7000 (ISO 8486 designation) are as follows: a) The above "spindle speed" is 1800 rpm, b) Set the "chuck table rotation speed" to +151 to -251 rpm. c) The above "processing feed rate" is 0.05 μm / s, It was found that, when surface grinding of "#280 surface" was performed under the above conditions, the wear rate of the vitrified grinding wheel could be reduced.
[0018] In addition, the steep unevenness formed after the lapping process is flattened by grinding the "#280 surface" by a few μm with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation). Therefore, when continuing to perform surface grinding on the ground surface (hereinafter sometimes referred to as the "#7000 surface") of the plate-shaped body flattened with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation), it is preferable to change the conditions for the "#280 surface" to those suitable for the "#7000 surface."
[0019] That is, the appropriate conditions for surface grinding the above-mentioned "♯7000 surface" using a grinding device that uses a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) are as follows: a) The above "spindle speed" is set to 3500 rpm, b) Set the "chuck table rotation speed" to +51 to -251 rpm. c) The above "processing feed rate" is 0.1 to 0.2 μm / s, It was found that, when the "#7000 surface" was surface ground under the above conditions, the wear rate of the vitrified grinding wheel could be further reduced.
[0020] The present invention has been completed based on these technical discoveries.
[0021] That is, the first invention according to the present invention is: A method for manufacturing a plate-shaped body, comprising a lapping step in which a difficult-to-cut plate-shaped body is processed to a thickness close to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface, wherein the lapping step uses B4C abrasive grains of No. 100 to No. 300 (ISO 8486 designation) and the surface grinding step uses a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation), The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The surface grinding conditions in the surface grinding process are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; The present invention is characterized in that: The second invention is In the method for producing a plate-like molded product according to the first aspect of the present invention, One surface of the plate-like body after the lapping step is surface ground under the surface grinding conditions, and then the other surface of the plate-like body is surface ground under the surface grinding conditions.
[0022] Next, the third invention according to the present invention is A method for manufacturing a plate-shaped body, comprising a lapping step in which a difficult-to-cut plate-shaped body is processed to a thickness close to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface, wherein the lapping step uses B4C abrasive grains of No. 100 to No. 300 (ISO 8486 designation) and the surface grinding step uses a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation), The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The above surface grinding process is composed of a first grinding process in the front stage and a second grinding process in the rear stage. At the same time , The conditions of the first surface grinding in the first grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; Set it to The conditions of the second surface grinding in the second grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 3500 rpm. b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.1 to 0.2 μm / s; The method is characterized in that the plate-shaped body surface is surface-ground by setting the plate-shaped body surface to the above-mentioned value. The fourth invention is In the method for producing a plate-like molded product according to the third aspect of the present invention, One surface of the plate-like body after the lapping step is surface ground under the first surface grinding conditions and the second surface grinding conditions, and then the other surface of the plate-like body is surface ground under the first surface grinding conditions and the second surface grinding conditions. do . Effect of the Invention
[0023] According to the method for producing a plate-like molded product according to the first aspect of the present invention, The conditions for surface grinding of a plate-shaped body surface after lapping process using B4C abrasive grains of No. 100 to No. 300 (ISO 8486) with a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486) are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; Since the grinding wheel is set to 0.5 mm, the wear rate of the grinding wheel can be reduced.
[0024] According to the method for producing a plate-like molded product according to the third aspect of the present invention, The surface grinding process is composed of a first grinding process in the front stage and a second grinding process in the rear stage, The conditions of the first grinding process in which the plate surface after the lapping process using B4C abrasive grains of No. 100 to No. 300 (ISO 8486) is ground with a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486) are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; is set to The plate-shaped surface that has been surface ground under the conditions of the first grinding process is surface ground with a vitrified grinding wheel containing diamond abrasive grains of 6000 to 8000 (ISO 8486 designation) under the conditions of the second grinding process. a) The rotation speed of the spindle on which the above grinding wheel is attached is 3500 rpm. b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.1 to 0.2 μm / s; Since the grinding wheel wear rate is set to 0.05, it is possible to further reduce the wear rate of the grinding wheel. [Brief description of the drawings]
[0025] [Figure 1]Figure 1(A) is a graph showing the relationship between "spindle rotation speed rpm" and "grinding wheel wear rate (%)". On the horizontal axis, "3500#7000 surface" indicates the conditions for surface grinding a SiC substrate (#7000 surface) at a spindle rotation speed of 3500 rpm, "3500#280 surface" indicates the conditions for surface grinding a SiC substrate (#280 surface) at a spindle rotation speed of 3500 rpm, and "1800#280 surface" indicates the conditions for surface grinding a SiC substrate (#280 surface) at a spindle rotation speed of 1800 rpm. In the figure, "1st" indicates the grinding wheel wear rate when the B (Back) surface of the SiC substrate is surface ground by 10 μm, "2nd" indicates the grinding wheel wear rate when the F (Front) surface of the SiC substrate is surface ground by 20 μm, and "AVE" indicates the average value of 1st and 2nd. Moreover, Figure 1(B) is a graph showing the relationship between "feed speed μm / s" and "grinding wheel wear rate %." In the figure, "13001st" shows the grinding wheel wear rate when one side of a SiC substrate (#280 surface) is surface ground at 5 μm at a spindle rotation speed of 1300 rpm (however, there is no data for a feed speed of 0.05 μm / s), "18001st" shows the grinding wheel wear rate when one side of a SiC substrate (#280 surface) is surface ground at 5 μm at a spindle rotation speed of 1800 rpm, and "35001st" shows the grinding wheel wear rate when one side of a SiC substrate (#280 surface) is surface ground at 5 μm at a spindle rotation speed of 3500 rpm. Moreover, Figure 1 (C) is a graph showing the relationship between "CT (chuck table) rotation speed rpm" and "grinding wheel wear rate %." In the figure, "1st" is the grinding wheel wear rate when the B (Back) surface of the SiC substrate (#280 surface) is surface ground at 5 μm, "2nd" is the grinding wheel wear rate when the F (Front) surface of the SiC substrate (#280 surface) is surface ground at 5 μm, and "AVE" is the average value of 1st and 2nd. [Diagram 2]Figure 2(A) is a graph showing the relationship between "spindle rotation speed rpm" and "grinding wheel wear rate %." In the figure, "1st" is the grinding wheel wear rate when the B (Back) surface of a SiC substrate (#7000 surface) is surface ground at 10 μm, "2nd" is the grinding wheel wear rate when the F (Front) surface of a SiC substrate (#7000 surface) is surface ground at 10 μm, and "AVE" is the average value of 1st and 2nd. Moreover, Figure 2(B) is a graph showing the relationship between "feed rate μm / s" and "grinding wheel wear rate %." In the figure, "35001st" is the grinding wheel wear rate when the B (Back) surface of a SiC substrate (No. 7000 surface) was surface ground at 10 μm at a spindle rotation speed of 3500 rpm, "35002nd" is the grinding wheel wear rate when the F (Front) surface of a SiC substrate (No. 7000 surface) was surface ground at 10 μm at a spindle rotation speed of 3500 rpm, and "3500AVE" is the average value of 1st and 2nd. Moreover, Figure 2(C) is a graph showing the relationship between "CT (chuck table) rotation speed rpm" and "grinding wheel wear rate %." In the figure, "1st" is the grinding wheel wear rate when the B (Back) surface of the SiC substrate (#7000 surface) is surface ground at 5 μm, "2nd" is the grinding wheel wear rate when the F (Front) surface of the SiC substrate (#7000 surface) is surface ground at 5 μm, and "AVE" is the average value of 1st and 2nd. [Diagram 3] FIG. 1 is a process diagram illustrating a method for manufacturing a SiC polycrystalline substrate using a chemical vapor deposition method (CVD method). [Figure 4] FIG. 4 is a process explanatory diagram showing a method for producing a plate-shaped body having a lapping step and a surface grinding step. [Diagram 5] 5(A) and (B) are explanatory diagrams of the configuration of a lapping device used in the lapping process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] Hereinafter, an embodiment of the present invention will be described.
[0027] The inventors conducted repeated experiments while changing the processing conditions of the grinding machine (DFG8340 manufactured by DISCO) used for surface grinding, i.e., the "spindle rotation speed" to which the vitrified grinding wheel is attached, the "chuck table rotation speed" to hold the plate-shaped body, and the "processing feed rate" to move the grinding wheel and the plate-shaped body relatively in the processing feed direction, and discovered the appropriate conditions for reducing the wear rate of the grinding wheel as described above.
[0028] Hereinafter, the inventors will explain the experiments they conducted, and will explain the "spindle rotation speed," "CT (chuck table) rotation speed," and "processing feed rate" that reduce the wear rate of the vitrified grinding wheel.
[0029] The lapped surface of a plate-shaped body (SiC polycrystalline substrate) lapped using No. 280 (ISO 8486) boron carbide (B4C) abrasive grains is abbreviated as the "#280 surface," and the ground surface of a plate-shaped body (SiC polycrystalline substrate) plane-ground using a vitrified grinding wheel containing No. 7000 (ISO 8486) diamond abrasive grains is abbreviated as the "#7000 surface."
[0030] 1. Conditions for "spindle rotation speed" when a vitrified grinding wheel is installed (1) Test method (1-1) Equipment conditions Precision surface grinding machine: DISCO DFG8340 Grindstone: Vitrified grindstone containing diamond grits #7000 (ISO 8486 designation) Grinding fluid: Pure water
[0031] (1-2) Equipment fixing conditions: "Processing feed rate": 0.20μm / s "CT (chuck table) rotation speed": +151 rpm
[0032] (2) Materials used (♯280 surface): A polycrystalline SiC substrate that has been lapped on both sides with low pressure using boron carbide (B4C) abrasive grains of #280 (ISO 8486 designation) [SiC substrate (♯280 surface)] (2-1) "Spindle speed" conditions (2-1-1) "3500#280 side" The B (Back) surface of the SiC substrate (#280 surface) was surface ground 10 μm (1st) at a spindle rotation speed of 3,500 rpm, and then the F (Front) surface of the SiC substrate (#280 surface) was surface ground 20 μm (2nd). At the same time, 200 SiC substrates (#280 surface) were ground and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0033] The results are shown in Figure 1(A). When the spindle rotation speed was 3,500 rpm in surface grinding of a SiC substrate (#280 surface), the "grinding wheel wear rate" (average value) was confirmed to be high, over 500% in the 1st stage, around 200% in the 2nd stage, and 350% for the average of the 1st and 2nd stages.
[0034] (2-1-2) "1800#280 side" The B (Back) surface of the SiC substrate (#280 surface) was surface ground 10 μm (1st) at a spindle rotation speed of 1800 rpm, and then the F (Front) surface of the SiC substrate (#280 surface) was surface ground 20 μm (2nd). At the same time, 200 SiC substrates (#280 surface) were ground and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0035] The results are also shown in Figure 1(A). In surface grinding of a SiC substrate (#280 surface), when the spindle rotation speed is 1800 rpm, the "grinding wheel wear rate" (average value) is improved to about 400% in the 1st, about 200% in the 2nd, and the average of the 1st and 2nd is improved to about 300%.
[0036] (2-1-3) "3500#7000 sides" The B (Back) surface of the SiC substrate (No. 7000 surface) was surface ground 10 μm (1st) at a spindle rotation speed of 3500 rpm, and then the F (Front) surface of the SiC substrate (No. 7000 surface) was surface ground 10 μm (2nd). The "grinding wheel wear rate" (average value) of the 1st and 2nd grinding of two SiC substrates (No. 7000 surfaces) is shown below for reference.
[0037] The results are also shown in Figure 1(A). When the spindle rotation speed is 3500 rpm in surface grinding of a SiC substrate (#7000 surface), it can be confirmed that the "grinding wheel wear rate" (average value) is approximately 45% in the 1st, approximately 25% in the 2nd, and the average value of the 1st and 2nd is approximately 40%, which is a significant improvement.
[0038] (2-2) Spindle rotation speed on SiC substrate (♯280 surface) From the graph in FIG. 1(A), it was confirmed that in surface grinding of a SiC substrate (#280 surface), it is advisable to set the spindle rotation speed to 1800 rpm.
[0039] (2-3) Why is the wheel wear rate so different between the B side (1st) and the F side (2nd)? As can be seen from the "Grindstone Wear Rate %" of the "3500 #280 surface" and "1800 #280 surface" in Figure 1(A), the grindstone wear rate is significantly different when grinding the B (Back) surface (1st) of the SiC substrate (#280 surface) and when grinding the F (Front) surface (2nd).
[0040] The present inventors speculate that the reason for this is as follows.
[0041] Before surface grinding, both sides of the SiC substrate (#280 surface) have steeply uneven surfaces. When the F surface of the substrate is attached to the CT (chuck table) and the B surface of the SiC substrate (#280 surface) is ground, the adhesion of the SiC substrate (#280 surface) to the CT (chuck table) is weak due to the steeply uneven surface (#280 surface), and the holding of the SiC substrate (#280 surface) becomes unstable, resulting in a high rate of wear of the grinding wheel.
[0042] On the other hand, when grinding the F side of a SiC substrate (#280 surface), the B side of the SiC substrate has been surface-ground to a flat surface (#7000 surface), so the adhesion force of the SiC substrate (#7000 surface) to the CT (chuck table) becomes stronger, and it is presumed that the holding of the SiC substrate (#7000 surface) becomes more stable and the wear rate of the grinding wheel becomes lower.
[0043] (3) Materials used (♯7000 surface): A polycrystalline SiC substrate [SiC substrate (♯7000 surface)] that has been surface ground with a vitrified grinding wheel containing diamond abrasive grains of 7000 (ISO 8486 designation).
[0044] (3-1) "Spindle speed" conditions As shown in FIG. 2(A), tests were performed while changing the "spindle rotation speed" to 1800 rpm, 2000 rpm, 2200 rpm, 2400 rpm, 2600 rpm, 2800 rpm, 3000 rpm, 3200 rpm, and 3500 rpm.
[0045] (3-2) Test conditions The B (back) surface of a SiC substrate (#7000 surface) was surface ground 10 μm (1st), and then the F (front) surface of the SiC substrate (#7000 surface) was surface ground 10 μm (2nd). At the same time, two SiC substrates (#7000 surfaces) were ground and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0046] (3-3) Evaluation From the results shown in Figure 2(A), it can be confirmed that in surface grinding of a SiC substrate (#7000 surface), when the spindle rotation speed is 3500 rpm, the "grinding wheel wear rate" (average value) is approximately 50% in the 1st, approximately 22% in the 2nd, and the average value of the 1st and 2nd is approximately 36%, which is a significant improvement.
[0047] (3-4) Spindle rotation speed on SiC substrate (♯7000 surface) From the graphs of FIG. 2(A) and FIG. 1(A), it was confirmed that in surface grinding of a SiC substrate (#7000 surface), it is advisable to set the spindle rotation speed at 3500 rpm.
[0048] 2. "Machining feed rate" conditions (1) Test method (1-1) Equipment conditions Precision surface grinding machine: DISCO DFG8340 Grindstone: Vitrified grindstone containing diamond grits #7000 (ISO 8486 designation) Grinding fluid: Pure water
[0049] (1-2) Equipment fixing conditions: "CT (chuck table) rotation speed": +151 rpm
[0050] (2) Materials used (♯280 surface): One SiC polycrystalline substrate [SiC substrate (♯280 surface)] that had been lapped on both sides at low pressure using boron carbide (B4C) abrasive grains no. 280 (ISO 8486) was used for each.
[0051] (2-1) "Spindle speed" conditions As shown in FIG. 1(B), the test was performed while changing the "spindle rotation speed" to 1300 rpm, 1800 rpm, and 3500 rpm.
[0052] (2-2) "Machining feed rate" conditions As shown in FIG. 1(B), the test was conducted while changing the "processing feed rate" to 0.05 μm / s, 0.10 μm / s, 0.15 μm / s, and 0.20 μm / s.
[0053] (2-3) Test conditions Using one SiC polycrystalline substrate [SiC substrate (♯280 surface)], the "spindle rotation speed" was set to three levels, 1300 rpm, 1800 rpm, and 3500 rpm, and the "processing feed rate" was set to four levels, 0.05 μm / s, 0.10 μm / s, 0.15 μm / s, and 0.20 μm / s. One side of each SiC polycrystalline substrate [SiC substrate (♯280 surface)] was surface ground by 5 μm, and the "grinding wheel wear rate" was measured.
[0054] In addition, the conditions of "spindle rotation speed" of 1300 rpm and "processing feed rate" of 0.05 μm / s were excluded.
[0055] (2-4) Evaluation From the results shown in Figure 1(B), it was confirmed that the optimal conditions for surface grinding of a SiC substrate (#280 surface) were a "spindle rotation speed" of 1800 rpm and a "processing feed rate" of 0.05 μm / s, and the "grinding wheel wear rate" was 242%.
[0056] (3) Materials used (♯7000 surface): Two pieces of SiC polycrystalline substrates [SiC substrates (♯7000 surface)] that had been surface ground with a vitrified grinding wheel containing diamond abrasive grains of 7000 (ISO 8486 designation) were used.
[0057] (3-1) "Spindle speed" conditions As shown in FIG. 2(B), the "spindle rotation speed" was set to 3500 rpm.
[0058] (3-2) "Machining feed rate" conditions As shown in FIG. 2(B), the test was performed while changing the "processing feed rate" to 0.05 μm / s, 0.10 μm / s, 0.15 μm / s, and 0.20 μm / s.
[0059] (3-3) Test conditions Two SiC polycrystalline substrates [SiC substrates (♯7000 surface)] were used, and the "spindle rotation speed" was set to one of 3500 rpm, and the "processing feed rate" was set to one of four types: 0.05 μm / s, 0.10 μm / s, 0.15 μm / s, and 0.20 μm / s. The B (Back) surface of each SiC polycrystalline substrate [SiC substrates (♯7000 surface)] was surface ground 10 μm (1st), and then the F (Front) surface of the SiC substrates (♯7000 surface) was surface ground 10 μm (2nd), and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0060] (4-4) Evaluation From the results shown in Figure 2(B), it was confirmed that the optimum condition for the "processing feed rate" in surface grinding of a SiC substrate (♯7000 surface) was 0.10μm / s to 0.20μm / s, excluding 0.05μm / s, and the average "grinding wheel wear rate" was about 40%.
[0061] 3. Conditions for "CT (chuck table) rotation speed" (1) Test method (1-1) Equipment conditions Precision surface grinding machine: DISCO DFG8340 Grindstone: Vitrified grindstone containing diamond grits #7000 (ISO 8486 designation) Grinding fluid: Pure water
[0062] (1-2) Equipment fixing conditions: "Spindle speed": 3500 rpm "Processing feed rate": 0.10μm / s
[0063] (2) Materials used (♯280 surface): One SiC polycrystalline substrate [SiC substrate (♯280 surface)] that had been lapped on both sides at low pressure using boron carbide (B4C) abrasive grains no. 280 (ISO 8486) was used for each.
[0064] (2-1) Conditions for "CT (chuck table) rotation speed" As shown in Figure 1(C), the test was conducted by changing the "CT (chuck table) rotation speed" to -251 rpm, -151 rpm, -51 rpm, +51 rpm, +151 rpm, and +251 rpm. Note that the sign "+" is added when the rotation direction of the chuck table is the same as the rotation direction of the spindle, and the sign "-" is added when it is opposite to the rotation direction of the spindle.
[0065] (2-2) Test conditions Using one SiC polycrystalline substrate [SiC substrate (#280 surface)], the "CT (chuck table) rotation speed" was set to -251 rpm, -151 rpm, -51 rpm, +51 rpm, +151 rpm, and +251 rpm. The B (Back) surface of each SiC polycrystalline substrate [SiC substrate (#280 surface)] was surface ground to 5 μm (1st), and then the F (Front) surface of the SiC substrate (#280 surface) was surface ground to 5 μm (2nd), and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0066] (2-3) Evaluation From the results shown in Fig. 1(C), it was confirmed that the optimum condition for the "CT (chuck table) rotation speed" in surface grinding of the SiC substrate (#280 surface) was +151 to -251 rpm, excluding +251 rpm, and the average "grinding wheel wear rate" was approximately 260%.
[0067] (3) Materials used (♯7000 surface): One SiC polycrystalline substrate [SiC substrate (♯7000 surface)] that had been surface ground with a vitrified grinding wheel containing diamond abrasive grains of 7000 (ISO 8486 designation) was used for each.
[0068] (3-1) Conditions for "CT (chuck table) rotation speed" As shown in Figure 2(C), the test was conducted while changing the "CT (chuck table) rotation speed" to -251 rpm, -151 rpm, -51 rpm, +51 rpm, +151 rpm, and +251 rpm.
[0069] (3-2) Test conditions Using one SiC polycrystalline substrate [SiC substrate (♯7000 surface)], the "CT (chuck table) rotation speed" was set to -251 rpm, -151 rpm, -51 rpm, +51 rpm, +151 rpm, and +251 rpm. The B (Back) surface of each SiC polycrystalline substrate [SiC substrate (♯7000 surface)] was surface ground to 5 μm (1st), and then the F (Front) surface of the SiC substrate (♯7000 surface) was surface ground to 5 μm (2nd), and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.
[0070] (3-3) Evaluation From the results shown in Fig. 2(C), it was confirmed that the optimum condition for the "CT (chuck table) rotation speed" in surface grinding of the SiC substrate (♯7000 surface) was +51 rpm to -251 rpm, excluding +151 rpm and +251 rpm, and the average "grinding wheel wear rate" was about 25%, and when the "CT (chuck table) rotation speed" was +51 rpm, the 2nd "grinding wheel wear rate" was 0%.
[0071] 4. Optimal conditions for surface grinding to reduce wheel wear rate From the above experimental results, the following optimum conditions are found.
[0072] That is, (1) The appropriate conditions for surface grinding of the lapped surface (#280 surface) of a plate-shaped body after the lapping process using boron carbide (B4C) grains #280 (ISO 8486 designation) using a grinding device that uses a vitrified grinding wheel containing diamond grains #7000 (ISO 8486 designation) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the plate is +151 to -251 rpm; c) The feed rate at which the grinding wheel and the plate-shaped body are moved relative to each other in the feed direction is 0.05 μm / s. and (2) The appropriate conditions for surface grinding of a plate-shaped body (#7000 surface) flattened with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) using a grinding device that uses a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 3500 rpm. b) The rotation speed of the chuck table that holds the plate is +51 to -251 rpm; c) The feed rate at which the grinding wheel and the plate-shaped body are moved relative to each other in the feed direction is 0.1 to 0.2 μm / s; It is found that:
[0073] In addition, the plate-shaped body is difficult to cut. Materials that make up In addition to silicon carbide (SiC), boron carbide, titanium carbide, alumina or boron nitride are also used. The raw Illustrated. EXAMPLES
[0074] Examples of the present invention will be specifically described below with reference to comparative examples, but the present invention is not limited to the following examples.
[0075] [Example 1] A SiC polycrystalline substrate (wafer) was placed between the upper and lower plates of the lapping device shown in Figures 5(A) and (B), and low-pressure double-sided lapping was performed while supplying a polishing solution containing boron carbide (B4C) abrasive grains No. 280 (ISO 8486 designation) between the upper and lower plates.
[0076] Next, surface B (#280 surface) of the wafer was subjected to 10 μm surface grinding (1st stage) using a grinding machine (DFG8340 manufactured by DISCO) using a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation), and surface F (#280 surface) of the wafer was also subjected to 20 μm surface grinding (2nd stage) using the same grinding machine to obtain a plate-shaped molded body according to Example 1.
[0077] The grinding conditions of the grinding device are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.05 μm / s; was set to.
[0078] Then, the wear rate of the vitrified grinding wheel in the 1st and 2nd processes was investigated, and it was 230% in the 1st process [see the 0.05 μm / s column in Figure 1(B)] and 127% in the 2nd process [see the 0.05 μm / s column in Figure 1(B) and the "1800♯280 surface" column in Figure 1(A)].
[0079] [Comparative Example 1] The grinding conditions of the grinding device are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 3500 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.20 μm / s; A plate-shaped molded product according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the temperature was set to 100° C.
[0080] Then, the wear rate of the vitrified grinding wheel in the 1st and 2nd processes was investigated, and it was 520% in the 1st process [see the "3500#280 surface" column in Figure 1(A)] and 190% in the 2nd process [see the "3500#280 surface" column in Figure 1(A)].
[0081] [Example 2] The B and F faces (#7000 faces) of the plate-like molded product according to Example 1 were subjected to surface grinding using a grinding device equipped with a vitrified grinding wheel containing diamond abrasive grains of No. 7000 (ISO 8486 designation).
[0082] The grinding conditions of the grinding device are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 3500 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.20 μm / s; was set to.
[0083] Then, the wear rate of the vitrified grinding wheel in the 1st and 2nd processes was investigated, and it was found to be 53% in the 1st process [see the 3500 rpm column in Figure 2(A)] and 22% in the 2nd process [see the 3500 rpm column in Figure 2(A)].
[0084] [Comparative Example 2] The grinding conditions of the grinding device are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.20 μm / s; A plate-shaped molded product according to Comparative Example 2 was obtained in the same manner as in Example 2, except that the temperature was set to 100° C.
[0085] Then, the wear rate of the vitrified grinding wheel in the 1st and 2nd processes was investigated, and it was 105% in the 1st process [see the 1800 rpm column in Figure 2(A)] and 108% in the 2nd process [see the 1800 rpm column in Figure 2(A)]. [Industrial Applicability]
[0086] INDUSTRIAL APPLICABILITY The method of the present invention can reduce the wear rate of the grindstone used in the surface grinding process, and therefore has industrial applicability for use in the manufacture of silicon carbide (SiC) polycrystalline substrates. [Explanation of symbols]
[0087] 1 Carbonaceous support substrate (graphite support substrate) 2 SiC polycrystalline film 3 SiC polycrystalline substrate
Claims
1. The process includes a lapping step in which a plate-shaped body that is difficult to cut is processed to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface. In the lapping step, B 4 In a method for manufacturing a plate-shaped compact, a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation) is used in a surface grinding process, The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The surface grinding conditions in the surface grinding process are as follows: a) The rotation speed of the spindle on which the grinding wheel is attached is 1800 rpm; b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) the grindstone and the plate-like body are moved relatively in the processing feed direction at a processing feed speed of 0.05 μm / s; A method for producing a plate-like molded product, characterized in that:
2. The method for manufacturing a plate-shaped body according to claim 1, characterized in that one surface of the plate-shaped body after the lapping process is surface ground under the surface grinding conditions, and then the other surface of the plate-shaped body is surface ground under the surface grinding conditions.
3. The process includes a lapping step in which a plate-shaped body that is difficult to cut is processed to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface. In the lapping step, B 4 In a method for manufacturing a plate-shaped compact, a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation) is used in a surface grinding process, The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The surface grinding process is composed of a first grinding process in the front stage and a second grinding process in the rear stage, The conditions of the first surface grinding in the first grinding step are as follows: a) The rotation speed of the spindle on which the grinding wheel is attached is 1800 rpm; b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) the grindstone and the plate-like body are moved relatively in the processing feed direction at a processing feed speed of 0.05 μm / s; Set it to The conditions of the second surface grinding in the second grinding step are as follows: a) The rotation speed of the spindle on which the grinding wheel is mounted is 3,500 rpm; b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) the grinding wheel and the plate-like body are moved relatively in the processing feed direction at a processing feed speed of 0.1 to 0.2 μm / s; and subjecting the plate-shaped body surface to surface grinding in the same manner as above.
4. The method for manufacturing a plate-shaped molded body according to claim 3, characterized in that one surface of the plate-shaped body after the lapping process is surface ground under the first surface grinding conditions and the second surface grinding conditions, and then the other surface of the plate-shaped body is surface ground under the first surface grinding conditions and the second surface grinding conditions.
Citation Information
Patent Citations
Thinning method of silicon carbide wafer
CN109664172A
Production of silicon carbide formed body
JP1996026714A
Method of processing semiconductor wafer
JP2008084930A
Semiconductor wafer manufacturing method
JP2011129569A
Planarization grinding process of silicon carbide substrate
JP2013197425A