Method for manufacturing plate-shaped body

By optimizing grinding conditions for SiC polycrystalline substrates, the wear rate of vitrified grinding wheels is reduced, addressing the high wear rate issue and enhancing manufacturing efficiency and cost-effectiveness.

JP7589508B2Active Publication Date: 2024-11-26SUMITOMO METAL MINING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020185586
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-11-26
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

The high wear rate of vitrified grinding wheels containing diamond abrasive grains during the surface grinding of silicon carbide (SiC) polycrystalline substrates poses a significant challenge, leading to increased costs due to the expense of these wheels and the need for frequent replacement.

Method used

Optimizing the grinding conditions, including spindle rotation speed, chuck table rotation speed, and machining feed rate, to reduce the wear rate of vitrified grinding wheels during the surface grinding process of SiC polycrystalline substrates.

Benefits of technology

The optimized grinding conditions significantly reduce the wear rate of vitrified grinding wheels, leading to cost savings and improved efficiency in the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589508000001
    Figure 0007589508000001
  • Figure 0007589508000002
    Figure 0007589508000002
  • Figure 0007589508000003
    Figure 0007589508000003
Patent Text Reader

Abstract

To provide a manufacturing method for a tabular compact that can reduce wear of a grindstone.SOLUTION: In a tabular compact manufacturing method comprising, to a difficult-to-cut plate-like body (silicon carbide), a lapping process in which B4C abrasive grains of No. 280 (ISO 8486 display) are applied and a surface grinding process in which a grindstone containing diamond abrasive grains of No. 7000 (same as above) is applied, surface grinding conditions of a lapped surface after lapping is set to: (a) 1800 rpm for a rotation speed of a spindle equipped with a grindstone; (b) +151 to -251 rpm for a rotation speed of a chuck table holding the plate-like body; and (c) 0.05 μm / s for a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction, and surface grinding conditions of a ground surface after surface grinding is set to: (a) 3500 rpm for a rotation speed of the spindle; (b) +51 to -251 rpm for a rotation speed of the chuck table; and (c) 0.10 μm / s for a processing feed speed.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a plate-shaped body, which includes a lapping process in which a difficult-to-cut plate-shaped body is processed to a desired thickness, and a surface grinding process in which the plate-shaped body surface after the lapping process is surface ground to process it into a highly flat and smooth surface, and in particular to a method for manufacturing a plate-shaped body that can reduce wear on the grinding wheel used in the surface grinding process. [Background technology]

[0002] Silicon carbide (SiC) has a band gap three times larger than silicon (Si) (4H-SiC: 3.8 eV, 6H-SiC: 3.1 eV, silicon: 1.1 eV) and a high thermal conductivity (5 W / cm K, silicon: 1.5 W / cm K). In recent years, SiC single crystals have begun to be used as a substrate material for power devices. For example, compared to conventional Si power devices, SiC power devices have achieved a withstand voltage 5 to 10 times larger and an operating temperature several hundred degrees higher. Furthermore, they can reduce the power loss of the element to about one-tenth, so they have been put to practical use in inverters for railway vehicles, etc.

[0003] SiC single crystals as substrate materials are usually produced by a gas phase method called sublimation recrystallization method (modified Lely process) (see, for example, Non-Patent Document 1), and are processed to the desired diameter and thickness.

[0004] The modified Lely process is a method for growing bulk SiC single crystals by heating and subliming solid SiC raw material (usually powder) at high temperatures (over 2,400°C). The sublimated Si atoms and carbon atoms are transported by diffusion through an inert gas atmosphere as vapor at 2,400°C, and become supersaturated on a seed crystal placed at a lower temperature than the raw material, causing it to recrystallize.

[0005] However, because the process temperature in the modified Lely process is very high at over 2,400°C, it is extremely difficult to control the temperature and convection during crystal growth, and to control crystal defects, and the SiC single crystal substrates produced by this method contain numerous crystal defects called micropipes and other crystal defects (stacking faults, etc.), making it extremely difficult to manufacture high-quality SiC single crystal substrates that can withstand electronic device use with a high yield. As a result, high-quality SiC single crystal substrates with few crystal defects that can be used for electronic devices are very expensive, and devices using such SiC single crystal substrates are also expensive, which has hindered the widespread use of SiC single crystal substrates.

[0006] In view of this, in recent years, a method has been proposed for producing a SiC substrate in which a SiC single crystal thin plate layer is formed on a SiC polycrystalline substrate by preparing a SiC single crystal substrate and a SiC polycrystalline substrate, performing a step of bonding the SiC single crystal substrate and the SiC polycrystalline substrate together, and then performing a step of thinning the SiC single crystal substrate (see, for example, Non-Patent Document 2).

[0007] According to this method for manufacturing a SiC substrate, the thickness of the SiC single crystal substrate can be reduced to a few tenths or even a few hundredths of that of the conventional method. Therefore, the cost of the SiC substrate can be significantly reduced compared to the conventional method in which the entire substrate is made of expensive and high-quality SiC single crystal. In addition, since elements such as power devices can be formed on a high-quality SiC single crystal layer with few crystal defects, the device performance and manufacturing yield can be significantly improved.

[0008] In the process of bonding such a SiC single crystal substrate and a SiC polycrystalline substrate, the SiC polycrystalline substrate is required to be dense and highly pure, as well as highly flat. For this reason, a chemical vapor deposition method (hereinafter, sometimes referred to as a "CVD method") is used to manufacture the SiC polycrystalline substrate, and a method for manufacturing a SiC polycrystalline substrate using the CVD method is described in Patent Document 1. The method for manufacturing a SiC polycrystalline substrate described in Patent Document 1 will be described below.

[0009] First, the inside of a growth furnace in which a carbonaceous support substrate (e.g., a graphite support substrate) 1 shown in Fig. 3(A) is placed is set to an environment of 1300°C or higher, and Si-based raw material gas such as SiH4, C-based raw material gas such as CH4, nitrogen gas as an impurity gas, and hydrogen gas as a carrier gas are introduced into the furnace, and a SiC polycrystalline film 2 shown in Fig. 3(B) is deposited on the front and back surfaces and the outer peripheral end surface of the carbonaceous support substrate 1 by thermal reaction. Then, the carbonaceous support substrate 1 on which the SiC polycrystalline film 2 is deposited is taken out of the growth furnace, and the carbonaceous support substrate 1 is beveled to expose the end surface of the carbonaceous support substrate 1 as shown in Fig. 3(C), and then only the carbonaceous support substrate 1 is burned using an electric furnace or the like, and two SiC polycrystalline substrates 3 consisting of the SiC polycrystalline film 2 formed on the front and back surfaces of the carbonaceous support substrate 1 as shown in Fig. 3(D) are obtained.

[0010] However, in this manufacturing method using the CVD method, the thickness of the formed SiC polycrystalline film 2 tends to be large near the outer edge (outer peripheral portion) of the carbonaceous support substrate 1 as shown in FIG. 3(B), and therefore the peripheral portion of the obtained SiC polycrystalline substrate 3 tends to be thicker than the central portion as shown in FIG. 3(D). Therefore, after burning and removing the carbonaceous support substrate 1, the following process was required to adjust the thickness and flatness of the SiC polycrystalline substrate 3 by grinding and polishing.

[0011] That is, as shown in Figures 4(A)-(B), a cut-out process is performed to remove the peripheral portion of the SiC polycrystalline substrate 3, a lapping process is performed to process the SiC polycrystalline substrate 3 to approximately the desired thickness as shown in Figure 4(C), a bevel process is performed to process the SiC polycrystalline substrate 3 to the desired diameter and then chamfer the end faces of the SiC polycrystalline substrate 3, a surface grinding process is performed to surface grind the surface of the SiC polycrystalline substrate 3 obtained in the lapping process to process it into a highly flat and smooth surface as shown in Figure 4(D), and a polishing process is performed to remove linear processing marks (not shown) generated in the surface grinding process by chemical mechanical polishing (mechanochemical polishing) and to make the surface of the SiC polycrystalline substrate 3 into a mirror finish as shown in Figure 4(E). Through these processes, the SiC polycrystalline substrate to be used for manufacturing SiC substrates will be in a desired state. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] Japanese Patent Application Publication No. 08-026714 [Patent Document 2] JP 2018-051646 A [Non-patent literature]

[0013] [Non-Patent Document 1] Yu.M.Tairov and VFTsvetkov: J.of Cryst.Growth 43(1978)209 [Non-Patent Document 2] Journal of the Japan Society for Precision Engineering, 2017, Vol. 83, No. 9, pp. 833-836 Summary of the Invention [Problem to be solved by the invention]

[0014] By the way, silicon carbide (SiC) is a material with very high hardness and difficult to cut, but it is possible to reduce the processing time and processing cost of SiC polycrystalline substrates by low-pressure double-sided lapping using boron carbide (B4C) abrasive grains with a grit size of about 100 (ISO 8486 designation) to 300 (ISO 8486 designation), for example, 280 (ISO 8486 designation). However, on the other hand, since steep unevenness is formed on the surface of the SiC polycrystalline substrate after the lapping process, when the SiC polycrystalline substrate is surface-ground using a vitrified grinding wheel containing diamond abrasive grains with a grit size of about 6000 (ISO 8486 designation) to 8000 (ISO 8486 designation), for example, 7000 (ISO 8486 designation), after the beveling process, there is a problem that the wear rate of the grinding wheel [(wear amount of grinding wheel / machined amount of workpiece) x 100%] becomes high. Specifically, if one side of a SiC polycrystalline substrate is surface ground by 10 μm in the first surface grinding step, and the other side of the SiC polycrystalline substrate is surface ground by 20 μm in the second surface grinding step, the wear rate of the grinding wheel in the first step is 700% to 350%, and in the second step it is 200% to 250%, which is high, and this poses a major problem because vitrified grinding wheels containing diamond abrasive grains are expensive.

[0015] The present invention has been made with attention to these problems, and its object is to provide a method for manufacturing a plate-shaped body having a lapping process and a surface grinding process, which can reduce the wear rate of a vitrified grinding wheel (a grinding wheel containing diamond abrasive grains and a vitrified binder) used in the surface grinding process. [Means for solving the problem]

[0016] In order to solve the above problems, the present inventors conducted repeated experiments while changing the processing conditions of the grinding device (see, for example, Patent Document 2) used in the surface grinding process, specifically, the "rotation speed of the spindle" to which the vitrified grinding wheel is attached, the "rotation speed of the chuck table" that holds the plate-shaped body, and the "processing feed speed" that moves the grinding wheel and the plate-shaped body relatively in the processing feed direction, and as a result, they found appropriate conditions that reduce the wear rate of the grinding wheel.

[0017] That is, the appropriate conditions for surface grinding the lapped surface of a plate-shaped body (hereinafter sometimes referred to as the "#280 surface") after the lapping process using boron carbide (B4C) abrasive grains #280 (ISO 8486 designation) using a grinding device using a vitrified grinding wheel containing diamond abrasive grains #7000 (ISO 8486 designation) are as follows: a) The above "spindle speed" is 1800 rpm, b) Set the "chuck table rotation speed" to +151 to -251 rpm. c) The above "processing feed rate" is 0.05 μm / s, It was found that, when surface grinding of "#280 surface" was performed under the above conditions, the wear rate of the vitrified grinding wheel could be reduced.

[0018] In addition, when the rotation direction of the chuck table is the same as the rotation direction of the spindle, a sign "+" is added, and when the rotation direction is opposite to the rotation direction of the spindle, a sign "-" is added.

[0019] In addition, the steep unevenness formed after the lapping process is flattened by grinding the "#280 surface" by a few μm with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation), and the wear rate of the grinding wheel after grinding by 3 μm to 10 μm is almost constant. Therefore, when further surface grinding the ground surface of the plate-shaped body flattened with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) (hereinafter sometimes referred to as the "#7000 surface"), the wear rate of the grinding wheel can be reduced by changing the grinding conditions from those of the "#280 surface" to those suitable for the "#7000 surface".

[0020] The appropriate conditions for surface grinding the above-mentioned "♯7000 surface" using a grinding device that uses a vitrified grinding wheel containing diamond abrasive grains of 7000 (ISO 8486 designation) are as follows: a) The above "spindle speed" is set to 3500 rpm, b) Set the "chuck table rotation speed" to +51 to -251 rpm. c) The above "processing feed rate" is 0.1 μm / s, It was found that, when the "#7000 surface" was surface ground under the above conditions, the wear rate of the vitrified grinding wheel could be further reduced.

[0021] The present invention has been completed based on these technical discoveries.

[0022] That is, the first invention according to the present invention is: A method for manufacturing a plate-shaped body, comprising a lapping step in which a difficult-to-cut plate-shaped body is processed to a thickness close to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface, wherein the lapping step uses B4C abrasive grains of No. 100 to No. 300 (ISO 8486 designation) and the surface grinding step uses a vitrified grinding wheel having diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation), The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The above surface grinding process is composed of a first grinding process in the front stage and a second grinding process in the rear stage. At the same time , The conditions of the first surface grinding in the first grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; The plate surface is ground to a thickness of 3 μm to 10 μm. The conditions of the second surface grinding in the second grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 3500 rpm. b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.1 μm / s; and surface-grinding the plate-shaped body surface to a desired thickness.

[0023] Next, the second invention according to the present invention is In the method for producing a plate-like molded product according to the first aspect of the present invention, In the first grinding step, one surface of the plate-shaped body is surface ground to 3 μm to 10 μm under the first surface grinding conditions, and then the other surface of the plate-shaped body is surface ground to 3 μm to 10 μm under the first surface grinding conditions; a second processing step in which one surface of the plate-like body surface-ground under the first surface grinding conditions in the second grinding step is surface-ground under second surface grinding conditions, and then the other surface of the plate-like body surface-ground under the first surface grinding conditions is surface-ground under the second surface grinding conditions; The method is characterized in that a plate-shaped molded body is produced by The third invention is In the method for producing a plate-like molded product according to the second aspect of the present invention, In the second processing step, the thickness β of the other surface of the plate-like body to be surface ground under the second surface grinding conditions is set larger than the thickness α of the one surface of the plate-like body to be surface ground under the second surface grinding conditions (α<β). This is what we do. Effect of the Invention

[0024] According to the method for producing a plate-like molded product according to the first aspect of the present invention, Regarding the conditions for surface grinding of a plate-shaped surface after the lapping process using B4C abrasive grains of No. 100 to No. 300 (ISO 8486 designation) with a vitrified grinding wheel containing diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation), The method is composed of a first grinding step in the front stage and a second grinding step in the rear stage, The conditions of the first surface grinding in the first grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 1800 rpm. b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) a processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.05 μm / s; The plate surface is surface ground to a depth of 3 μm to 10 μm under the appropriate conditions. The conditions of the second surface grinding in the second grinding step are as follows: a) The rotation speed of the spindle on which the above grinding wheel is attached is 3500 rpm. b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) A processing feed speed for relatively moving the grindstone and the plate-like body in a processing feed direction is 0.1 μm / s Because the appropriate conditions are set as follows, It is possible to reduce the wear rate of the vitrified grinding wheel. [Brief description of the drawings]

[0025] [Figure 1]This is a graph showing the relationship between the polishing conditions of the SiC substrate and the grindstone wear rate %. On the horizontal axis, "♯280REF" (1st) is the grindstone wear rate % when the B (Back) surface, which is the lapped surface (♯280 surface) of the SiC substrate, is ground at 5 μm under the comparison conditions [spindle rotation speed: 1800 rpm, CT (chuck table) rotation speed: +151 rpm, processing feed rate: 0.2 μm / s], and "♯280REF" (2nd) is the grindstone wear rate % when the F (Front) surface, which is the lapped surface (♯280 surface) of the SiC substrate, is ground at 5 μm under the comparison conditions [spindle rotation speed: 1800 rpm, CT (chuck table) rotation speed: +151 rpm, processing feed rate: 0.2 μm / s]. The graph shows the percent wheel wear rate when 5μm surface grinding was performed under the conditions shown in Fig. 1. Also, "♯280 Optimal" (1st) shows the percent wheel wear rate when 5μm surface grinding was performed on the B (Back) surface, which is the lapped surface (♯280 surface) of the SiC substrate, under the optimal conditions [spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, processing feed rate: 0.05μm / s], and "♯280 Optimal" (2nd) shows the percent wheel wear rate when 5μm surface grinding was performed on the F (Front) surface, which is the lapped surface (♯280 surface) of the SiC substrate, under the above optimal conditions. The wear rate % is shown, and "♯7000REF" (1st) shows the grinding wheel wear rate % when the B (Back) surface, which is the ground surface (♯7000 surface) of the SiC substrate, is surface ground at 5 μm under the comparison conditions [spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, processing feed rate: 0.2 μm / s]. "♯7000REF" (2nd) shows the grinding wheel wear rate % when the F (Front) surface, which is the ground surface (♯7000 surface) of the SiC substrate, is surface ground at 15 μm under the above comparison conditions. "♯ "#7000 Optimal" (1st) indicates the wheel wear rate % when the B (Back) surface, which is the grinding surface (#7000 surface) of the SiC substrate, is surface ground at 5 μm under optimal conditions [spindle rotation speed: 3500 rpm, CT rotation speed: -51 rpm, processing feed rate: 0.10 μm / s], "#7000 Optimal" (2nd) indicates the wheel wear rate % when the F (Front) surface, which is the grinding surface (#7000 surface) of the SiC substrate, is surface ground at 15 μm under the above optimal conditions, and "AVE" indicates the average value of 1st and 2nd. [Diagram 2]This is a graph showing the relationship between the polishing conditions for SiC substrates and the percent wheel wear rate. On the horizontal axis, "total REF" (1st) is the average value obtained by summing the percent wheel wear rate of the above "♯280REF" (1st) and "♯7000REF" (1st), "total REF" (2nd) is the average value obtained by summing the percent wheel wear rate of the above "♯280REF" (2nd) and "♯7000REF" (2nd), "total optimum" (1st) is the average value obtained by summing the percent wheel wear rate of the above "♯280 optimum" (1st) and "♯7000 optimum" (1st), "total optimum" (2nd) is the average value obtained by summing the percent wheel wear rate of the above "♯280 optimum" (2nd) and "♯7000 optimum" (2nd), and "AVE" is the average value of 1st and 2nd. [Diagram 3] FIG. 1 is a process diagram illustrating a method for manufacturing a SiC polycrystalline substrate using a chemical vapor deposition method (CVD method). [Figure 4] FIG. 4 is a process explanatory diagram showing a method for producing a plate-shaped body having a lapping step and a surface grinding step. [Diagram 5] 5(A) and (B) are explanatory diagrams of the configuration of a lapping device used in the lapping process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Hereinafter, an embodiment of the present invention will be described.

[0027] The inventors conducted repeated experiments while changing the processing conditions of the grinding machine (DFG8340 manufactured by DISCO) used for surface grinding, i.e., the "spindle rotation speed" to which the vitrified grinding wheel is attached, the "chuck table rotation speed" to hold the plate-shaped body, and the "processing feed rate" to move the grinding wheel and the plate-shaped body relatively in the processing feed direction, and discovered the appropriate conditions for reducing the wear rate of the grinding wheel as described above.

[0028] Hereinafter, the inventors' experiments will be described, and the "spindle rotation speed", "CT (chuck table) rotation speed", and "processing feed rate" that reduce the wear rate of the vitrified grinding wheel will be described.

[0029] The lapped surface of a plate-shaped body (SiC polycrystalline substrate) lapped using No. 280 (ISO 8486) boron carbide (B4C) abrasive grains is abbreviated as the "#280 surface," and the ground surface of a plate-shaped body (SiC polycrystalline substrate) plane-ground using a vitrified grinding wheel containing No. 7000 (ISO 8486) diamond abrasive grains is abbreviated as the "#7000 surface."

[0030] 1. Conditions for surface grinding on lapped surface (♯280 surface) (1) Test method (1-1) Equipment conditions Precision surface grinding machine: DISCO DFG8340 Grindstone: Vitrified grindstone containing diamond grits #7000 (ISO 8486 designation) Grinding fluid: Pure water

[0031] (1-2) Equipment fixing conditions: "Spindle speed": 1800 rpm "CT (chuck table) rotation speed": +151 rpm

[0032] (2) Board used (#280 side): A polycrystalline SiC substrate that has been lapped on both sides at low pressure using boron carbide (B4C) abrasive grains of #280 (ISO 8486 designation) [SiC substrate (♯280 surface)] (2-1) "Machining feed rate" conditions (2-1-1) "♯280REF" "Processing feed rate": Under the condition of 0.2 μm / s, the B (Back) surface of the SiC substrate (No. 280 surface) was surface ground to 5 μm (1st), and then the F (Front) surface of the SiC substrate (No. 280 surface) was surface ground to 5 μm (2nd). At the same time, four SiC substrates (No. 280 surfaces) were surface ground and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.

[0033] The results are shown in Figure 1 for "♯280REF" (1st) (2nd). In surface grinding of a SiC substrate (♯280 surface), when the spindle rotation speed was set to 1800 rpm, the CT rotation speed to +151 rpm, and the processing feed rate to 0.2 μm / s, it was confirmed that the "grinding wheel wear rate" (average value) was extremely high, at approximately 890% for the 1st, approximately 490% for the 2nd, and the average value of the 1st and 2nd was approximately 690%.

[0034] (2-1-2) "No. 280 Optimal" "Processing feed rate": Under the condition of 0.05 μm / s, the B (Back) surface of the SiC substrate (No. 280 surface) was surface ground to 5 μm (1st), and then the F (Front) surface of the SiC substrate (No. 280 surface) was surface ground to 5 μm (2nd). At the same time, four SiC substrates (No. 280 surfaces) were surface ground and the "grinding wheel wear rate" (average value) of the 1st and 2nd were measured.

[0035] The results are shown in "Optimal #280" (1st) (2nd) in Figure 1. In surface grinding of a SiC substrate (#280 surface), when the spindle rotation speed was set to 1800 rpm, the CT rotation speed to +151 rpm, and the processing feed rate to 0.05 μm / s, it was confirmed that the "grinding wheel wear rate" (average value) improved to approximately 290% in 1st, approximately 210% in 2nd, and approximately 250% for the average of the 1st and 2nd.

[0036] 2. Conditions for surface grinding on the grinding surface (♯7000 surface) (1) Test method (1-1) Equipment conditions Precision surface grinding machine: DISCO DFG8340 Grindstone: Vitrified grindstone containing diamond grits #7000 (ISO 8486 designation) Grinding fluid: Pure water

[0037] (2) Substrate used (#7000 side): A SiC polycrystalline substrate [SiC substrate (♯7000 surface)] in which the B (back) and F (front) surfaces of the SiC polycrystalline substrate [SiC substrate (♯280 surface)] have been surface ground under the above-mentioned "♯280REF" conditions using a vitrified grinding wheel containing diamond abrasive grains of 7000 (ISO 8486 designation), and a SiC polycrystalline substrate [SiC substrate (♯7000 surface)] in which the B (back) and F (front) surfaces of the SiC polycrystalline substrate [SiC substrate (♯280 surface)] have been surface ground under the above-mentioned "♯280 optimal" conditions.

[0038] (2-1) Surface grinding conditions (2-1-1) "♯7000REF" The B (Back) surface of the SiC polycrystalline substrate [SiC substrate (#7000 surface)] that had been surface ground under the above-mentioned "#280REF" conditions was subjected to 5 μm surface grinding (1st) under conditions of spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, and processing feed rate: 0.2 μm / s. Subsequently, the F (Front) surface of the above-mentioned SiC substrate (#7000 surface) was surface ground 15 μm (2nd), and four SiC substrates (#7000 surfaces) were also surface ground to measure the "grinding wheel wear rate" (average value) of the 1st and 2nd.

[0039] The results are shown in Figure 1 for "♯7000REF" (1st) (2nd). In surface grinding of a SiC substrate (♯7000 surface), when the spindle rotation speed was set to 1800 rpm, the CT rotation speed to +151 rpm, and the processing feed rate to 0.2 μm / s, it was confirmed that the "grinding wheel wear rate" (average value) was high, at approximately 190% for the 1st, approximately 120% for the 2nd, and approximately 155% for the average value of the 1st and 2nd.

[0040] (2-1-2) "♯7000 Optimal" The B (Back) surface of the SiC polycrystalline substrate [SiC substrate (#7000 surface)] that had been surface ground under the above-mentioned "#280 optimal" conditions was subjected to 5 μm surface grinding (1st) under conditions of spindle rotation speed: 3500 rpm, CT rotation speed: -51 rpm, and processing feed rate: 0.10 μm / s. Subsequently, the F (Front) surface of the above-mentioned SiC substrate (#7000 surface) was surface ground 15 μm (2nd), and four SiC substrates (#7000 surfaces) were also surface ground to measure the "grinding wheel wear rate" (average value) of the 1st and 2nd.

[0041] The results are shown in "Optimal #7000" (1st) (2nd) in Figure 1. In surface grinding of a SiC substrate (#7000 surface), when the spindle rotation speed was set to 3500 rpm, the CT rotation speed to -51 rpm, and the processing feed rate to 0.10 μm / s, it was confirmed that the "grinding wheel wear rate" (average value) improved significantly to about 80% in 1st, about 20% in 2nd, and about 50% for the average value of 1st and 2nd.

[0042] Meanwhile, the grinding amount of the B (Back) surface of the SiC substrate (#7000 surface) is set to 5 μm, whereas the grinding amount of the F (Front) surface is set to 15 μm, which is large. The reason for this is that when the surface-ground SiC substrate is used as a SiC polycrystalline substrate to be bonded to a SiC single crystal substrate, the F (Front) surface, which has a larger amount of grinding, is made flatter and better bonded to the SiC single crystal substrate.

[0043] 3. Overall evaluation of lapped surface (#280 surface) and ground surface (#7000 surface) (1) In Figure 2, the “total REF” (1st) is the average value (approximately 540%) obtained by adding up the grinding wheel wear rates of the above-mentioned “♯280REF” (1st) (approximately 890%) and “♯7000REF” (1st) (approximately 190%), while the “total REF” (2nd) is the average value (approximately 305%) obtained by adding up the grinding wheel wear rates of the above-mentioned “♯280REF” (2nd) (approximately 490%) and “♯7000REF” (2nd) (approximately 120%). The average value of the “total REF” obtained by adding up the average values ​​of 1st and 2nd was approximately 420%.

[0044] In other words, when the B (Back) and F (Front) surfaces of a SiC substrate (#280 surface) are surface ground under the above comparative conditions [spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, and processing feed rate: 0.2 μm / s], and when the B (Back) and F (Front) surfaces of a SiC substrate (#7000 surface) are also surface ground under the above comparative conditions [spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, and processing feed rate: 0.2 μm / s], it is confirmed that the overall grinding wheel wear rate is high at approximately 420%.

[0045] (2) On the other hand, the “overall optimum” (1st) in Figure 2 is the average value (approximately 180%) obtained by adding up the grinding wheel wear rate of the above “♯280 optimum” (1st) (approximately 290%) and the grinding wheel wear rate of the “♯7000 optimum” (1st) (approximately 80%), while the “overall optimum” (2nd) is the average value (approximately 120%) obtained by adding up the grinding wheel wear rate of the above “♯280 optimum” (2nd) (approximately 210%) and the grinding wheel wear rate of the “♯7000 optimum” (2nd) (approximately 20%). The average value of the “overall optimum”, obtained by adding up the average values ​​of the 1st and 2nd, was approximately 150%.

[0046] In other words, when the B (Back) and F (Front) surfaces of a SiC substrate (#280 surface) are surface ground under the above-mentioned optimal conditions [spindle rotation speed: 1800 rpm, CT rotation speed: +151 rpm, and processing feed rate: 0.05 μm / s], and the B (Back) and F (Front) surfaces of a SiC substrate (#7000 surface) are surface ground under the above-mentioned optimal conditions [spindle rotation speed: 3500 rpm, CT rotation speed: -51 rpm, processing feed rate: 0.10 μm / s], it is confirmed that the overall grinding wheel wear rate is significantly improved by approximately 150%.

[0047] (3) Why the wear rate of the grinding wheel is so different between 1st and 2nd For example, as can be seen from a comparison of the grinding wheel wear rate of "♯280REF" (1st) (approximately 890%) and the grinding wheel wear rate of "♯280REF" (2nd) (approximately 490%) shown in Figure 1, there is a large difference in the grinding wheel wear rate between the 1st and 2nd grinding wheels.

[0048] The present inventors speculate that the reason for this is as follows.

[0049] Before surface grinding, both the B (Back) and F (Front) surfaces of the SiC substrate (#280 surface) have steeply uneven surfaces. When the F (Front) surface of the SiC substrate is attached to the CT (Chuck Table) and the B (Back) surface of the SiC substrate (#280 surface) is ground (1st step), the adhesion of the SiC substrate (#280 surface) to the CT (Chuck Table) is weak due to the steeply uneven surface (#280 surface), and the holding of the SiC substrate (#280 surface) becomes unstable, resulting in a high wear rate of the grinding wheel in the 1st step.

[0050] On the other hand, when grinding (2nd) the F (Front) surface of a SiC substrate (#280 surface), the B (Back) surface of the SiC substrate has been surface-ground to a flat surface (#7000 surface), so the adhesion force of the SiC substrate (#7000 surface) to the CT (chuck table) becomes stronger, and it is presumed that the holding of the SiC substrate (#7000 surface) becomes more stable, resulting in a lower wear rate of the 2nd grinding wheel.

[0051] 4. Optimal conditions for surface grinding to reduce the wear rate of the grinding wheel From the above experimental results, the following optimum conditions are found.

[0052] That is, (1) The appropriate conditions for surface grinding of the lapped surface (#280 surface) of a plate-shaped body after the lapping process using boron carbide (B4C) grains #280 (ISO 8486 designation) using a grinding device that uses a vitrified grinding wheel containing diamond grains #7000 (ISO 8486 designation) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the plate is +151 to -251 rpm; c) The feed rate at which the grinding wheel and the plate-shaped body are moved relative to each other in the feed direction is 0.05 μm / s. and (2) The appropriate conditions for surface grinding of a plate-shaped body (#7000 surface) flattened with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) using a grinding device that uses a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 3500 rpm. b) The rotation speed of the chuck table that holds the plate is +51 to -251 rpm; c) The feed rate at which the grinding wheel and the plate-shaped body are moved relative to each other in the feed direction is 0.1 μm / s. It is found that:

[0053] In addition, the plate-shaped body is difficult to cut. Materials that make up In addition to silicon carbide (SiC), boron carbide, titanium carbide, alumina or boron nitride are also used. The raw Illustrated. EXAMPLES

[0054] Examples of the present invention will be specifically described below with reference to comparative examples, but the present invention is not limited to the following examples.

[0055] [Example 1] A SiC polycrystalline substrate (wafer) was placed between the upper and lower plates of the lapping device shown in Figures 5(A) and (B), and low-pressure double-sided lapping was performed while supplying a polishing solution containing boron carbide (B4C) abrasive grains No. 280 (ISO 8486 designation) between the upper and lower plates.

[0056] Next, the B (Back) side of the wafer (#280 surface) was subjected to 5 μm surface grinding (1st) using a grinding machine (DISCO Corp., DFG8340) with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation), and then the F (Front) side of the wafer (#280 surface) was subjected to 5 μm surface grinding (2nd) using a grinding machine (DISCO Corp., DFG8340) with a vitrified grinding wheel containing diamond abrasive grains of #7000 (ISO 8486 designation).

[0057] The grinding conditions for the above wafer (#280 surface) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.05 μm / s; was set to.

[0058] Then, the wear rate of the grinding wheel when grinding a wafer (No. 280 surface) was investigated, and it was found to be about 290% in the 1st process [see "No. 280 Optimal" (1st) in Figure 1] and about 210% in the 2nd process [see "No. 280 Optimal" (2nd) in Figure 1].

[0059] Next, the B (Back) side of the surface-ground wafer (#7000 surface) was surface-ground to 5 μm (1st) using the above-mentioned grinding machine (DFG8340 manufactured by DISCO) using a vitrified grinding wheel containing #7000 (ISO 8486) diamond abrasive grains, and further, the F (Front) side of the wafer (#7000 surface) was surface-ground to 15 μm (2nd) using a grinding machine (DFG8340 manufactured by DISCO) using a vitrified grinding wheel containing #7000 (ISO 8486) diamond abrasive grains to produce a plate-shaped molded body according to Example 1.

[0060] The grinding conditions for the above wafer (#7000 surface) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 3500 rpm. b) The rotation speed of the chuck table holding the wafer is -51 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.10 μm / s; was set to.

[0061] Similarly, when the wear rate of the grinding wheel when grinding a wafer (#7000 surface) was investigated, it was about 80% in the 1st process [see "#7000 Optimal" (1st) in Figure 1] and about 20% in the 2nd process [see "#7000 Optimal" (2nd) in Figure 1].

[0062] [Comparative Example 1] The grinding conditions for the above wafer (#280 surface) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.20 μm / s; and The grinding conditions for the above wafer (#7000 surface) are as follows: a) The rotation speed of the spindle with the grinding wheel attached is 1800 rpm. b) The rotation speed of the chuck table that holds the wafer is +151 rpm. c) The processing feed speed for moving the grindstone and the wafer relatively in the processing feed direction is 0.20 μm / s; A plate-shaped molded product according to Comparative Example 1 was obtained in the same manner as in Example 1, except that the temperature was set to 100° C.

[0063] Then, the wear rate of the grinding wheel when grinding a wafer (#280 surface) was investigated, and it was found to be approximately 890% in the 1st process [see "#280REF" (1st) in Figure 1] and approximately 490% in the 2nd process [see "#280REF" (2nd) in Figure 1].

[0064] Similarly, when the wear rate of the grinding wheel when grinding a wafer (#7000 surface) was investigated, it was approximately 190% in the 1st process [see "#7000REF" (1st) in Figure 1] and approximately 120% in the 2nd process [see "#7000REF" (2nd) in Figure 1].

[0065] [comprehensive evaluation] (1) Example 1 The average wheel wear rate (1st) calculated by adding up the wheel wear rate of the "♯280 surface" (1st) (approximately 290%) and the wheel wear rate of the "♯7000 surface" (1st) (approximately 80%) was approximately 180%, and the average wheel wear rate (2nd) calculated by adding up the wheel wear rate of the "♯280 surface" (2nd) (approximately 210%) and the wheel wear rate of the "♯7000 surface" (2nd) (approximately 20%) was approximately 120%, meaning that the average wheel wear rate for the entire process (1st and 2nd) was approximately 150%.

[0066] (2) Comparative Example 1 The average wheel wear rate (1st) calculated by adding up the wheel wear rate of the "♯280 surface" (1st) (approximately 890%) and the wheel wear rate of the "♯7000 surface" (1st) (approximately 190%) was approximately 540%, and the average wheel wear rate (2nd) calculated by adding up the wheel wear rate of the "♯280 surface" (2nd) (approximately 490%) and the wheel wear rate of the "♯7000 surface" (2nd) (approximately 120%) was approximately 305%, meaning that the average wheel wear rate for the entire process (1st and 2nd) was approximately 420%.

[0067] (3) The average wear rate of the grinding wheel in all processes (1st and 2nd) was approximately 150% in Example 1 and approximately 420% in Comparative Example 1. This confirms that the wear rate of the grinding wheel can be significantly reduced by adopting the grinding conditions in Example 1. [Industrial Applicability]

[0068] INDUSTRIAL APPLICABILITY The method of the present invention can reduce the wear rate of the grindstone used in the surface grinding process, and therefore has industrial applicability for use in the manufacture of silicon carbide (SiC) polycrystalline substrates. [Explanation of symbols]

[0069] 1 Carbonaceous support substrate (graphite support substrate) 2 SiC polycrystalline film 3 SiC polycrystalline substrate

Claims

1. The process includes a lapping step in which a plate-shaped body that is difficult to cut is processed to a desired thickness, and a surface grinding step in which the plate-shaped body surface after the lapping step is surface ground to a highly flat and smooth surface. In the lapping step, B 4 A method for manufacturing a plate-shaped compact, in which a vitrified grinding wheel having diamond abrasive grains of No. 6000 to No. 8000 (ISO 8486 designation) is used in a surface grinding process, The hard-to-cut plate-shaped body is made of any material selected from silicon carbide, boron carbide, titanium carbide, alumina, and boron nitride, and The surface grinding process is composed of a first grinding process in the front stage and a second grinding process in the rear stage, The conditions of the first surface grinding in the first grinding step are as follows: a) The rotation speed of the spindle on which the grinding wheel is attached is 1800 rpm; b) the rotation speed of the chuck table holding the plate-like body is +151 to -251 rpm; c) the grinding wheel and the plate-like body are moved relatively in the processing feed direction at a processing feed speed of 0.05 μm / s; The plate surface is ground to a thickness of 3 μm to 10 μm. The conditions of the second surface grinding in the second grinding step are as follows: a) The rotation speed of the spindle on which the grinding wheel is mounted is 3,500 rpm; b) the rotation speed of the chuck table holding the plate-like body is +51 to -251 rpm; c) the grinding wheel and the plate-like body are moved relatively in the processing feed direction at a processing feed speed of 0.1 μm / s; and surface-grinding the plate-shaped body surface to a desired thickness.

2. In the first grinding step, one surface of the plate-shaped body is surface ground to 3 μm to 10 μm under the first surface grinding conditions, and then the other surface of the plate-shaped body is surface ground to 3 μm to 10 μm under the first surface grinding conditions; a second processing step in which one surface of the plate-like body surface-ground under the first surface grinding conditions in the second grinding step is surface-ground under second surface grinding conditions, and then the other surface of the plate-like body surface-ground under the first surface grinding conditions is surface-ground under the second surface grinding conditions; 2. The method for producing a plate-like molded product according to claim 1, further comprising the steps of:

3. The method for manufacturing a plate-shaped molded body as described in claim 2, characterized in that in the second processing step, the thickness β to which one surface of the plate-shaped body is surface ground under the second surface grinding conditions is set to be larger than the thickness α to which one surface of the plate-shaped body is surface ground under the second surface grinding conditions (α < β).

Citation Information

Patent Citations

  • Production of silicon carbide formed body

    JP1996026714A

  • Method of processing semiconductor wafer

    JP2008084930A

  • Semiconductor wafer manufacturing method

    JP2011129569A

  • Planarization grinding process of silicon carbide substrate

    JP2013197425A

  • Method for determining physical property of monocrystalline silicon carbide substrate and method for manufacturing monocrystalline silicon carbide substrate

    JP2017208432A