Method for producing toner particles
The described method for producing toner particles addresses the challenge of achieving both low-temperature and high-temperature fixability while minimizing surfactant use and preventing abnormal images by using a polyester resin and prepolymer in an oil-in-water dispersion process.
Patent Information
- Application Number
- JP2021033289
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-03
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-03-03
AI Technical Summary
Existing toner manufacturing methods face challenges in achieving both low-temperature and high-temperature fixability while minimizing surfactant use and preventing point-like abnormal images during image formation.
A method involving dissolving or dispersing a polyester resin and a prepolymer in an organic solvent to create an oil phase, followed by phase inversion emulsification with an aqueous medium to form an oil-in-water dispersion, and then aggregating fine particles to produce toner particles.
The method produces toner particles with good low-temperature and high-temperature fixing properties, reduces surfactant use, and eliminates point-like abnormal images, thereby enhancing image quality.
Smart Images

Figure 0007589591000001 
Figure 0007589591000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing toner particles. [Background technology]
[0002] In recent years, there has been a demand for toners that have a reduced environmental impact. To meet this demand, for example, reductions in power consumption through improvements in the low-temperature fixing properties of the toner itself, and reductions in the amounts of energy and chemicals used in the toner manufacturing process are being considered.
[0003] Well-known methods for improving the low-temperature fixing property of toner include lowering the glass transition temperature or softening point of the resin, adding a crystalline resin, etc. However, since lowering the thermal properties of the toner deteriorates the fixing property at high temperatures, methods have been proposed to maintain the fixing property at high temperatures, such as adding a polymer resin or adding a prepolymer during production and polymerizing it after the toner particles are formed. In addition, pulverization was widely used as a method for producing toner, but due to the large amount of energy required for production and the trend toward smaller toner particles, chemical toner methods such as suspension polymerization have also become mainstream.
[0004] As a method for reducing the amount of chemicals used in toner production, a phase inversion emulsification method that can reduce the amount of surfactants is known. As mentioned above, as a method for maintaining the fixability at high temperatures, a method is known in which a prepolymer is added during production and polymerized after the toner particles are formed. To date, a toner manufacturing method has been known that combines these methods to produce a toner with good fixability while reducing the amount of surfactant used (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a method for producing toner particles that can produce toner particles that have good low-temperature and high-temperature fixability and suppress the occurrence of dot-like abnormal images during image formation, while reducing the amount of surfactant used. [Means for solving the problem]
[0006] The method for producing toner particles of the present invention as a means for solving the above-mentioned problems is a method for producing toner particles, comprising: a) a step of dissolving or dispersing at least a polyester resin and a prepolymer in an organic solvent to prepare an oil phase; b) a step of adding an aqueous medium to the oil phase to effect phase inversion emulsification, thereby obtaining an oil-in-water dispersion; and c) a step of aggregating fine particles in the oil-in-water dispersion. Effect of the Invention
[0007] According to the present invention, it is possible to provide a method for producing toner particles that can produce toner particles that have good low-temperature and high-temperature fixability and suppress the occurrence of dot-like abnormal images during image formation while reducing the amount of surfactant used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] (Method of manufacturing toner particles) The method for producing toner particles of the present invention is characterized by comprising: a) a step of dissolving or dispersing at least a polyester resin and a prepolymer in an organic solvent to prepare an oil phase; b) a step of adding an aqueous medium to the oil phase to effect phase inversion emulsification, thereby obtaining an oil-in-water dispersion; and c) a step of aggregating fine particles in the oil-in-water dispersion. The method for producing toner particles of the present invention includes at least an oil phase preparation step (step a), a phase inversion emulsification step (step b), and an aggregation step (step c), and further includes other steps as necessary.
[0009] The toner particle manufacturing method of the present invention is based on the finding that the toner manufacturing method described in the prior art Patent Document 1 (JP Patent Publication No. 2000-194160) is capable of manufacturing a toner with good fixing properties while reducing the amount of surfactant used, but when the toner manufactured by this method is output by electrophotography, dot-like abnormal images occur on the image. As a result of investigating the above-mentioned problems found by the present inventors, it was found that in conventional toner manufacturing methods, when a prepolymer is added to an oil phase and a toner is manufactured by phase inversion emulsification, the dispersion of the prepolymer becomes uneven, resulting in the formation of particles consisting only of resin formed by the elongated prepolymer, and these particles remain undissolved during fixing, resulting in the occurrence of dot-like abnormal images.
[0010] The present inventors have found that the method for producing toner particles of the present invention can solve the above problems of the prior art and achieve the above objects. It was found that the high-temperature fixability of the toner particles can be maintained by adding a prepolymer in the oil phase preparation step (step a), granulation can be performed with a reduced amount of surfactant used in the phase inversion emulsification step (step b), and even if particles consisting only of prepolymer are generated in the aggregation step (step c), the resulting toner particles are free of bias in polyester resin and prepolymer by aggregating these fine particles, resulting in the elimination of dot-like abnormal images on the image. In addition, because the structure has the prepolymer dispersed inside, the low-temperature fixability of the polyester resin can be secured, and the toner also has good low-temperature fixability.
[0011] <Step a: Oil phase preparation step> The oil phase preparation step is a step of preparing an oil phase by dissolving or dispersing at least a polyester resin and a prepolymer (also referred to as "a polyester resin having a group capable of reacting with an active hydrogen group-containing compound") in an organic solvent. The toner material (oil phase material) used in the oil phase preparation step contains at least a polyester resin and a prepolymer, and further contains other materials such as a colorant and a charge control agent, if necessary.
[0012] The method for dissolving or dispersing the toner materials in the organic solvent is not particularly limited and may be appropriately selected according to the purpose, and may be, for example, dissolved or dispersed using a dispersing machine such as a homomixer, a bead mill, a disk mill, etc. For example, in the case of a homomixer, it is preferable to stir at 0°C to 30°C, 6,000 rpm to 12,000 rpm, and 30 minutes to 120 minutes.
[0013] -Polyester resin- The polyester resin may be a polyester resin having only a polyester skeleton, or a block polymer of a polyester resin and a resin having another skeleton. When used as a toner for developing an electrostatic latent image in electrophotography, a resin having a polyester skeleton can provide good fixing properties. Among these, polyester resins are preferred, and amorphous polyester resins are more preferred, in terms of high uniformity in toner particles.
[0014] The weight average molecular weight of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1,000 to 30,000, more preferably 3,000 to 15,000, and even more preferably 5,000 to 12,000, in terms of molecular weight distribution by gel permeation chromatography (GPC). If the weight average molecular weight is less than 1,000, the heat resistant storage stability is deteriorated, whereas if it exceeds 30,000, the low temperature fixing property as a toner for developing an electrostatic latent image may be deteriorated.
[0015] The glass transition temperature (Tg) of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 35°C to 80°C, more preferably 40°C to 70°C, and even more preferably 45°C to 65°C. If the Tg is less than 35° C., the toner particles obtained may deform when placed in a high-temperature environment such as midsummer, or the toner particles may stick to each other and not be able to behave as intended particles. If the Tg is more than 80° C., the fixing property of the toner particles deteriorates when the toner particles are used as a toner for developing electrostatic latent images.
[0016] --Amorphous polyester resin-- The amorphous polyester resin (hereinafter sometimes referred to as "amorphous polyester", "amorphous polyester", "amorphous polyester resin", or "unmodified polyester resin") is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ring-opening polymerization products of lactones, condensation polymerization products of hydroxycarboxylic acids, polycondensation products of polyols and polycarboxylic acids, etc. Among these, polycondensation products of polyols and polycarboxylic acids are preferred from the viewpoint of freedom in design. In the present invention, the amorphous polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above, and modified polyester resins, such as the prepolymer and modified polyester resins obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, are not included in the amorphous polyester resin in the present invention, but are treated as modified polyester resins. The amorphous polyester is a polyester resin component that is soluble in tetrahydrofuran (THF).
[0017] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diols and trihydric or higher polyols. These may be used alone or in combination of two or more, but a diol alone or a mixture of a diol and a small amount of a trihydric or higher polyol is preferred.
[0018] Examples of the diol include alkylene glycols, alkylene ether glycols, alicyclic diols, alkylene oxide adducts of the alicyclic diols, 4,4'-dihydroxybiphenyls, bis(hydroxyphenyl)alkanes, bis(4-hydroxyphenyl)ethers, and alkylene oxide adducts of the bisphenols.
[0019] Examples of the alkylene glycol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol. Examples of the alkylene ether glycol include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol. Examples of the alicyclic diol include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. The 4,4'-dihydroxybiphenyls include, for example, 3,3'-difluoro-4,4'-dihydroxybiphenyl. Examples of the bis(hydroxyphenyl)alkanes include bis(hydroxyphenyl)alkanes such as bis(3-fluoro-4-hydroxyphenyl)methane, 1-phenyl-1,1-bis(3-fluoro-4-hydroxyphenyl)ethane, 2,2-bis(3-fluoro-4-hydroxyphenyl)propane, 2,2-bis(3,5-difluoro-4-hydroxyphenyl)propane (also known as tetrafluorobisphenol A), and 2,2-bis(3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane; Examples thereof include the above-mentioned bis(3-fluoro-4-hydroxyphenyl) ether. Examples of the alkylene oxide include ethylene oxide, propylene oxide, and butylene oxide.
[0020] Among these, alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols are preferred, and alkylene oxide adducts of bisphenols and combinations of these with alkylene glycols having 2 to 12 carbon atoms are more preferred.
[0021] Examples of the trihydric or higher alcohol include polyhydric trihydric or higher aliphatic alcohols, trihydric or higher phenols, and alkylene oxide adducts of the trihydric or higher phenols. Examples of the trihydric or higher polyhydric aliphatic alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. Examples of the trivalent or higher phenols include trisphenol PA, phenol novolak, and cresol novolak.
[0022] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include dicarboxylic acids and polycarboxylic acids having three or more valences. These may be used alone or in combination of two or more kinds, but a dicarboxylic acid alone or a mixture of a dicarboxylic acid and a small amount of a polycarboxylic acid having three or more valences is preferred.
[0023] Examples of the dicarboxylic acid include alkylene dicarboxylic acids (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acids (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acids (phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, etc.); 3-fluoroisophthalic acid, 2-fluoroisophthalic acid, 2-fluoroterephthalic acid, 2,4,5,6-tetrafluoroisophthalic acid, 2,3,5,6-tetrafluoroterephthalic acid, 5-trifluoromethyl ether ... ethyl isophthalic acid, 2,2-bis(4-carboxyphenyl)hexafluoropropane, 2,2-bis(3-carboxyphenyl)hexafluoropropane, 2,2'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 3,3'-bis(trifluoromethyl)-4,4'-biphenyldicarboxylic acid, 2,2'-bis(trifluoromethyl)-3,3'-biphenyldicarboxylic acid, and hexafluoroisopropylidenediphthalic anhydride. Among these, alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred.
[0024] Examples of the trivalent or higher polycarboxylic acid include aromatic polycarboxylic acids having 9 to 20 carbon atoms (eg, trimellitic acid, pyromellitic acid, etc.). As the polycarboxylic acid, anhydrides or lower alkyl esters (methyl esters, ethyl esters, isopropyl esters, etc.) of the above-mentioned polycarboxylic acids may be used.
[0025] The ratio of the polyol to the polycarboxylic acid, expressed as an equivalent ratio [OH] / [COOH] of a hydroxyl group [OH] to a carboxyl group [COOH], is preferably 2 / 1 to 1 / 2, more preferably 1.5 / 1 to 1 / 1.5, and further preferably 1.3 / 1 to 1 / 1.3.
[0026] -Prepolymer- The prepolymer is a polyester resin having a group capable of reacting with an active hydrogen group-containing compound, and may be referred to as a "polyester prepolymer" or a "reactive precursor." The prepolymer is not particularly limited and can be appropriately selected depending on the purpose. The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds. Examples of the group capable of reacting with the active hydrogen group include an isocyanate group, an epoxy group, a carboxylic acid, an acid chloride group, etc. Among these, an isocyanate group is preferred because it is capable of introducing a urethane bond or a urea bond into the amorphous polyester resin.
[0027] The polyester resin containing an isocyanate group is not particularly limited and may be appropriately selected depending on the purpose. For example, a reaction product of a polyester resin having an active hydrogen group and a polyisocyanate may be mentioned. The polyester resin having an active hydrogen group is obtained, for example, by polycondensation of a diol, a dicarboxylic acid, and at least one of a trivalent or higher polyol and a trivalent or higher carboxylic acid. The trivalent or higher polyol and the trivalent or higher carboxylic acid impart a branched structure to the polyester resin containing an isocyanate group. The prepolymer may have a branched structure imparted by at least one of a trivalent or higher polyol and a trivalent or higher carboxylic acid.
[0028] The modified polyester resin (sometimes referred to as "modified polyester") is obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, and examples thereof include a reaction product of the prepolymer and the active hydrogen group-containing compound. The modified polyester resin is a polyester resin insoluble in tetrahydrofuran (THF). The polyester resin component insoluble in tetrahydrofuran (THF) lowers Tg and melt viscosity, and ensures low-temperature fixability, while having a branched structure in the molecular skeleton and a three-dimensional network structure in the molecular chain, and thus has rubber-like properties of deforming but not flowing at low temperatures. Since the modified polyester resin has an active hydrogen group-containing compound and a site capable of reacting with the active hydrogen group-containing compound, these sites behave like pseudo-crosslinking points, and the rubber-like properties of the prepolymer are enhanced, making it possible to produce a toner having excellent heat-resistant storage stability and high-temperature offset resistance.
[0029] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diols and trihydric or higher polyols. These may be used alone or in combination of two or more, but a diol alone or a mixture of a diol and a small amount of a trihydric or higher polyol is preferred.
[0030] Examples of the diol include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylol. Examples of such diols include diols having an oxyalkylene group such as ethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F and bisphenol S; and alkylene oxide adducts of bisphenols such as bisphenols to which alkylene oxides such as ethylene oxide, propylene oxide and butylene oxide have been added. These may be used alone or in combination of two or more. Among these, from the viewpoint of controlling the glass transition point of the prepolymer to 20° C. or lower, aliphatic diols having 3 to 10 carbon atoms, such as 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, and 1,6-hexanediol; and alkylene oxide adducts of bisphenols, such as an adduct of 2 moles of ethylene oxide of bisphenol A, are preferred, and it is more preferable to use them in an amount of 50 mol % or more of the alcohol component in the resin.
[0031] The prepolymer is preferably an amorphous polyester resin, and by providing steric hindrance to the resin chain of the prepolymer, the melt viscosity during fixing is reduced, and low-temperature fixing property is more easily achieved. For this reason, the main chain of the aliphatic diol preferably has a structure represented by the following general formula (1).
[0032] [ka] In the general formula (1), R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, n represents an odd number of 3 to 9, and in the n repeating units, R1 and R2 may be the same or different.
[0033] Here, the main chain of the aliphatic diol refers to a carbon chain that connects two hydroxyl groups of the aliphatic diol with the shortest number of carbon atoms. When the carbon number of the main chain is odd, it is preferable because the crystallinity decreases due to the odd-even ratio. In addition, when the main chain has at least one alkyl group having 1 to 3 carbon atoms in the side chain, it is more preferable because the interaction energy between the main chain molecules decreases due to the stericity.
[0034] Examples of the trihydric or higher polyols include trihydric or higher aliphatic alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol; trihydric or higher polyphenols such as trisphenol PA, phenol novolac, and cresol novolac; and alkylene oxide adducts of trihydric or higher polyphenols, such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trihydric or higher polyphenols.
[0035] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include dicarboxylic acids and polycarboxylic acids having three or more valences. These may be used alone or in combination of two or more kinds, but a dicarboxylic acid alone or a mixture of a dicarboxylic acid and a small amount of a polycarboxylic acid having three or more valences is preferred.
[0036] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid; and anhydrides, lower (carbon number 1 to 3) alkyl esters, and halides thereof. These may be used alone or in combination of two or more. Among these, from the viewpoint of controlling the Tg of the prepolymer to 20° C. or less, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred, and it is more preferred to use them in an amount of 50% by mass or more of the carboxylic acid component in the resin.
[0037] Examples of the trivalent or higher carboxylic acid include trivalent or higher aromatic carboxylic acids, their anhydrides, lower (carbon number 1 to 3) alkyl esters, halides, etc. Among these, trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms, such as trimellitic acid and pyromellitic acid, are preferred.
[0038] --Polyisocyanate-- Examples of the polyisocyanate include diisocyanates and tri- or higher valent isocyanates. The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include 1,3- and / or 1,4-phenylene diisocyanate, 2,4- and / or 2,6-tolylene diisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI), crude MDI [crude diaminophenylmethane [condensation products of formaldehyde and aromatic amine (aniline) or mixtures thereof; aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates; modified products of these isocyanates, and the like. These may be used alone or in combination of two or more. Examples of the aliphatic diisocyanate include ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate. Examples of the alicyclic diisocyanate include isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, and 2,5- and 2,6-norbornane diisocyanates. Examples of the aromatic diisocyanate include phosgenates of a mixture of diaminodiphenylmethane and a small amount (for example, 5 to 20% by mass) of a trifunctional or higher polyamine: polyallyl polyisocyanate (PAPI), 1,5-naphthylene diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanate, and the like. Examples of the araliphatic diisocyanate include m- and p-xylylene diisocyanate (XDI), and α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI). Examples of the trivalent or higher polyisocyanurates include lysine triisocyanate and diisocyanate-modified products of trivalent or higher alcohols. Examples of the modified isocyanate include modified products containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, a uretdione group, a uretoimine group, an isocyanurate group, and an oxazolidone group.
[0039] -Other toner materials (oil phase materials)- --Coloring agent-- The colorant is not particularly limited, and known dyes and pigments can be appropriately selected depending on the purpose. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, a Anthrazan Yellow BGL, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Tread F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulia Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold,Examples of the pigments include acid green lake, malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone. These pigments may be used alone or in combination of two or more.
[0040] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 part by mass to 15 parts by mass, and more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the toner.
[0041] --Charge control agent-- The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives.
[0042] Examples of commercially available charge control agents include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, and the boron complex LR-147 (all manufactured by Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone, and azo pigments; and polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.
[0043] The content of the charge control agent is not limited to a specific amount as long as the charge control agent is used in an amount that allows the agent to exhibit its performance and does not impair fixability or the like. The content of the charge control agent is preferably 0.5% by mass to 5% by mass, and more preferably 0.8% by mass to 3% by mass, based on the total amount of the toner.
[0044] - Organic solvents - The organic solvent is preferably a volatile solvent having a boiling point of less than 100° C., since this facilitates subsequent removal of the solvent. Examples of such organic solvents include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone (hereinafter sometimes abbreviated as “MEK”), and methyl isobutyl ketone. These may be used alone or in combination of two or more. Among these, when the resin to be dissolved or dispersed in the organic solvent is a polyester resin, ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate, or ketone-based solvents such as methyl ethyl ketone and methyl isobutyl ketone are preferred in terms of high solubility, and methyl acetate, ethyl acetate, and methyl ethyl ketone are more preferred in terms of high solvent removability.
[0045] <Step b: Phase inversion emulsification step> The phase inversion emulsification step is a step of adding an aqueous medium to the oil phase obtained in the oil phase preparation step to invert and emulsify the oil phase into an oil-in-water dispersion, whereby the oil phase, which is a water-in-oil type solution or dispersion, is inverted and emulsified into an oil-in-water dispersion. In addition, in order to dissociate the carboxyl groups in the resin and increase the dispersibility of the resin, it is preferable to neutralize the oil phase by adding an alkaline aqueous medium such as an aqueous ammonia solution to a neutralization rate of 100% to 700%, and then add an aqueous medium such as water to invert the phase and emulsify the mixture to obtain an oil-in-water dispersion. By the phase inversion emulsification step, an oil-in-water dispersion liquid in which fine particles of toner materials are dispersed in an aqueous medium can be obtained.
[0046] The aqueous medium is not particularly limited as long as it causes phase inversion emulsification, and can be appropriately selected according to the purpose. For example, water, a solvent miscible with water, a mixture thereof, etc. can be mentioned. These can be used alone or in combination of two or more. Among these, water is preferred. The water-miscible solvent is not particularly limited as long as it causes phase inversion emulsification, and can be appropriately selected according to the purpose, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, lower ketones, etc. Examples of the alcohol include methanol, isopropanol, ethylene glycol, etc. Examples of the lower ketones include acetone, methyl ethyl ketone, etc.
[0047] The amount of the aqueous medium to be added is not particularly limited as long as phase inversion emulsification occurs, and can be appropriately selected depending on the purpose, but is preferably 150 parts by mass to 300 parts by mass relative to 100 parts by mass of the oil phase. The phase inversion emulsification of the oil phase from a water-in-oil type solution or dispersion to an oil-in-water type dispersion can be confirmed by observation with an optical microscope.
[0048] <<Solvent removal process>> The solvent removal step is a step of removing the organic solvent from the oil-in-water dispersion. The method for removing the organic solvent from the oil-in-water dispersion is not particularly limited, and a known desolvation method can be appropriately selected depending on the purpose, and examples thereof include a method in which the temperature of the oil-in-water dispersion is gradually increased while stirring the entire dispersion, and the organic solvent in the fine particles (droplets) of the toner material is completely evaporated and removed; a method in which a dispersion containing fine particles of the toner material is sprayed into a dry atmosphere while stirring, and the organic solvent in the droplets is completely removed; a method in which a dispersion containing fine particles of the toner material is depressurized while stirring, and the organic solvent is evaporated and removed; etc. The latter two methods can be used in combination with the first method.
[0049] Examples of the drying atmosphere into which the fine particles of the toner material are sprayed include air, nitrogen, carbon dioxide gas, gas obtained by heating combustion gas, etc. Among these, various air flows heated to a temperature equal to or higher than the boiling point of the organic solvent having the highest boiling point among the organic solvents used are preferable. The drying means (drying device) may be, for example, a spray dryer, a belt dryer, a rotary kiln, etc., and a dispersion of fine particles of the desired quality can be obtained by a short treatment with the drying means.
[0050] <Step c: Agglomeration step> The aggregation step is a step of aggregating the fine particles in the oil-in-water dispersion, and it is preferable to aggregate the fine particles in the oil-in-water dispersion while heating and stirring them, thereby obtaining toner particles (aggregated particles) in which the fine particles are aggregated to a desired particle size. The method for aggregating the fine particles is not particularly limited, and a known method can be appropriately selected according to the purpose, for example, a method of adding a flocculant; a method of adjusting pH, etc. When adding the flocculant, it may be added as it is, but it is preferable to add an aqueous solution of the flocculant in order to avoid localized high concentration. In addition, it is preferable to gradually add the flocculant while watching the particle size of the fine particles.
[0051] The temperature of the oil-in-water dispersion in the aggregation step is preferably from (Tg-10° C.) to (Tg+10° C.), and more preferably from (Tg-5° C.) to (Tg+5° C.), relative to the Tg of the polyester resin. If the temperature is too low, aggregation does not proceed very well, resulting in poor efficiency, whereas if the temperature is too high, the aggregation rate increases, resulting in the generation of coarse particles and a deterioration in particle size distribution. When the desired particle size is reached, the aggregation is stopped by, for example, adding a salt or a chelating agent having a low ionic valence, adjusting the pH, lowering the temperature of the dispersion, or adding a large amount of an aqueous medium to dilute the concentration.
[0052] In the aggregation step, a wax may be added as a release agent, or a crystalline polyester resin may be added for low-temperature fixability. In that case, a dispersion liquid in which a wax is dispersed in an aqueous medium or a dispersion liquid of a crystalline resin may be prepared, and mixed with an oil-in-water dispersion liquid containing fine particles made of the toner material, and then the mixture is aggregated to obtain aggregated particles in which the wax or crystalline resin is uniformly dispersed on the surface of the fine particles. The flocculant, wax, and crystalline polyester resin will be described below.
[0053] -Flocculant- The flocculant is not particularly limited, and any known flocculant can be appropriately selected depending on the purpose. Examples of the flocculant include metal salts of monovalent metals such as sodium and potassium; metal salts of divalent metals such as calcium and magnesium; and metal salts of trivalent metals such as iron and aluminum.
[0054] -wax- The wax (releasing agent) is not particularly limited and can be appropriately selected from known waxes, for example, natural waxes, synthetic waxes, etc. These may be used alone or in combination of two or more kinds.
[0055] Examples of the natural waxes include vegetable waxes such as carnauba wax, cotton wax, and wood wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. Examples of the synthetic wax include synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; fatty acid amide compounds such as esters, ketones, ethers, 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, and chlorinated hydrocarbons; low molecular weight crystalline polymer resins, such as polyacrylate homopolymers and copolymers (e.g., n-stearyl acrylate-ethyl methacrylate copolymers); and crystalline polymers having long alkyl groups in their side chains. Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.
[0056] The melting point of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 50° C. to 120° C., and more preferably 60° C. to 90° C. If the melting point is 50° C. or higher, the wax can be prevented from adversely affecting heat-resistant storage stability, and if the melting point is 120° C. or lower, the problem of cold offset occurring during fixing at low temperatures can be effectively prevented. A wax with a low melting point of 50° C. to 120° C. can effectively act as a release agent between the fixing roller and the toner interface by being dispersed in the crystalline polyester resin, thereby improving hot offset resistance even in an oil-less system (no release agent such as oil is applied to the fixing roller).
[0057] The melt viscosity of the wax is preferably 5 cps to 1,000 cps, more preferably 10 cps to 100 cps, as measured at a temperature 20° C. higher than the melting point of the wax. If the melt viscosity is 5 cps or more, the release property can be prevented from decreasing, and if it is 1,000 cps or less, the effects of hot offset resistance and low-temperature fixability can be sufficiently exhibited. The content of the wax is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0% by mass to 40% by mass, more preferably 3% by mass to 30% by mass, based on the total amount of the toner. If the content is 40% by mass or less, deterioration of the fluidity of the toner can be prevented.
[0058] -Crystalline polyester resin- The crystalline polyester resin (hereinafter also referred to as "crystalline polyester") is not particularly limited and can be appropriately selected depending on the purpose. For example, a crystalline polyester resin obtained by reacting a polyol with a polycarboxylic acid can be mentioned. In the present invention, the crystalline polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above, and modified polyester resins, such as the prepolymer and resins obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.
[0059] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diols and trihydric or higher alcohols. These may be used alone or in combination of two or more kinds.
[0060] The diol includes, for example, saturated aliphatic diols. The saturated aliphatic diol may be a linear saturated aliphatic diol or a branched saturated aliphatic diol. These may be used alone or in combination of two or more. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having a carbon number of 2 to 12 are more preferred, because they can improve crystallinity and prevent a decrease in melting point.
[0061] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanediol. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred because the crystalline polyester resin has high crystallinity and excellent sharp melting properties.
[0062] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0063] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids. These may be used alone or in combination of two or more kinds.
[0064] Examples of the dicarboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and further, anhydrides of these acids and lower (carbon number: 1 to 3) alkyl esters of these acids.
[0065] Examples of the trivalent or higher polycarboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and anhydrides and lower (carbon number 1 to 3) alkyl esters of these.
[0066] The polycarboxylic acid may contain a dicarboxylic acid having a sulfonic acid group in addition to the saturated aliphatic dicarboxylic acid or aromatic dicarboxylic acid. Furthermore, the polycarboxylic acid may contain a dicarboxylic acid having a double bond in addition to the saturated aliphatic dicarboxylic acid or aromatic dicarboxylic acid. These may be used alone or in combination of two or more.
[0067] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms, which provides high crystallinity and excellent sharp melting properties, thereby enabling the toner to exhibit excellent low-temperature fixing properties. In addition, as a method for controlling the crystallinity and softening point of a crystalline polyester resin, there can be mentioned a method of designing and using a non-linear polyester obtained by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component during polyester synthesis, or a trivalent or higher polycarboxylic acid such as trimellitic anhydride to the acid component and carrying out condensation polymerization.
[0068] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc., but it can be easily confirmed by infrared absorption spectrum at 965±10 cm -1 Or 990±10cm -1 One method is to detect a crystalline polyester resin that has absorption based on the δCH (out-of-plane bending vibration) of olefin.
[0069] As for the molecular weight of the crystalline polyester resin, from the viewpoint that a low molecular weight with a sharp molecular weight distribution provides excellent low-temperature fixability, and that a large amount of low molecular weight components deteriorates heat-resistant storage stability, it has been found through extensive investigation that, in a molecular weight distribution diagram of the o-dichlorobenzene soluble portion measured by gel permeation chromatography (GPC), the horizontal axis is log(M) and the vertical axis is weight %, the peak position is in the range of 3.5 to 4.0, the half-width of the peak is 1.5 or less, the weight average molecular weight (Mw) is 3,000 to 30,000, the number average molecular weight (Mn) is 1,000 to 10,000, and Mw / Mn is 1 to 10. It is more preferable that the weight average molecular weight (Mw) is 5,000 to 15,000, the number average molecular weight (Mn) is 2,000 to 10,000, and the Mw / Mn is 1 to 5.
[0070] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of affinity between paper and resin, in order to achieve the desired low-temperature fixability, it is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, while in order to improve high-temperature offset resistance, it is preferably 45 mgKOH / g or less.
[0071] The hydroxyl value of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose. In order to achieve the desired low-temperature fixability and good charging characteristics, the hydroxyl value is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 50 mgKOH / g.
[0072] The melting point of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 60° C. to 80° C. If the melting point is 60° C. or higher, the crystalline polyester resin is easily melted at low temperatures, and the problem of the heat-resistant storage stability of the toner decreasing can be prevented, whereas if the melting point is 80° C. or lower, the crystalline polyester resin is not sufficiently melted by heating during fixing, and the problem of the low-temperature fixability decreasing can be prevented.
[0073] The content of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 4% by mass to 30% by mass, more preferably 5% by mass to 25% by mass, based on the total amount of the toner. If the content is 4% by mass or more, the problem of poor low-temperature fixability due to insufficient sharp melting by the crystalline polyester resin can be prevented. Also, if the content is 30% by mass or less, the problem of poor cohesion and adhesion at high temperatures can be prevented.
[0074] <Other processes> Examples of the other steps include the above-mentioned desolvation step, fusion step, washing and drying step, annealing step, and external addition step.
[0075] <<Fusing process>> The fusion step is a step of fusing the aggregated particles obtained in the aggregation step by heat treatment, and it is preferable to heat the dispersion of the aggregated particles while stirring, thereby obtaining fused particles having reduced surface irregularities of the aggregated particles. The temperature at which the aggregated particles are heat-treated is preferably near a temperature exceeding the Tg of the polyester resin (higher than Tg and not higher than Tg+15° C.). The average circularity of the fused particles is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 0.940 to 0.985, and more preferably 0.950 to 0.975.
[0076] <<Cleaning and drying process>> The washing and drying step is a step of washing and drying the aggregated particles obtained in the aggregation step and the fused particles obtained in the fusion step to obtain toner particles. The dispersion of fine particles obtained by the above method contains sub-materials such as coagulated salts in addition to the fine particles made of the toner materials. Therefore, it is preferable to carry out washing and drying in order to extract only the toner particles from the dispersion.
[0077] The washing method is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include centrifugation, reduced pressure filtration, and filter press. Any of the methods can obtain a cake of toner particles, but if the toner particles cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the process of extracting the toner particles by any of the above methods may be repeated. When washing is performed by reduced pressure filtration or filter press, a method may be adopted in which the aqueous solvent is passed through the cake to wash out the secondary materials contained in the toner particles. The aqueous solvent used for the washing may be, for example, water or a mixed solvent obtained by mixing water with an alcohol such as methanol or ethanol. Among these, water is preferred in view of costs and environmental loads due to wastewater treatment.
[0078] The toner particles obtained by the washing contain a large amount of the aqueous medium, so that only the toner particles can be obtained by removing the aqueous medium through drying. The drying method is not particularly limited and can be appropriately selected depending on the purpose. Examples of the drying method include drying methods using a dryer such as a spray dryer, a vacuum freeze dryer, a reduced pressure dryer, a stationary shelf dryer, a mobile shelf dryer, a fluidized bed dryer, a rotary dryer, or an agitator dryer. The drying is preferably carried out until the moisture content in the dried toner particles is finally reduced to less than 1%. In addition, if the toner particles after drying are softly aggregated and cause inconvenience during use, the soft aggregates may be broken down by using a device such as a jet mill, a Henschel mixer, a super mixer, a coffee mill, an Oster blender, or a food processor.
[0079] <<Annealing process>> The annealing step is a step performed after the drying step when a crystalline polyester resin is added in the aggregation step, and is a step of storing the toner particles at a temperature near the glass transition temperature (Tg) of the polyester resin for 10 hours or more, whereby the amorphous polyester resin and the crystalline polyester resin are phase-separated, improving fixability. The temperature near the glass transition temperature (Tg) of the polyester resin is preferably (Tg-15°C) to (Tg+5°C).
[0080] <<External addition process>> The external addition step is a step of adding and mixing an external additive to the toner particles. By adding and mixing the external additive to the toner particles, the resulting toner particles can be endowed with properties such as fluidity, chargeability, and cleanability. The method of mixing is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a method of applying an impact force to the mixture by a blade rotating at high speed, a method of introducing the mixture into a high-speed air current, accelerating the mixture, and causing the particles to collide with each other or the composite particles to collide with an appropriate collision plate, and the like. Examples of the mixing means include an Angmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) with reduced grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar.
[0081] -External additives- Examples of the external additive include inorganic fine particles, polymer fine particles, and cleaning assistants. --Inorganic fine particles-- Examples of the inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride. The primary particle diameter of the inorganic fine particles is preferably from 5 nm to 2 μm, and more preferably from 5 nm to 500 nm. The specific surface area of the inorganic fine particles according to the BET method is 20 m 2 / g~500m 2 / g is preferred. The content of the inorganic fine particles is preferably 0.01% by mass to 5% by mass with respect to the total amount of the toner.
[0082] --Polymer-based fine particles-- Examples of the polymeric fine particles include polystyrene obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization, methacrylic acid ester or acrylic acid ester copolymers, polycondensation systems such as silicone, benzoguanamine, and nylon, and polymer particles made of thermosetting resins.
[0083] --Flow improver-- The flowability improver is not particularly limited as long as it is capable of performing a surface treatment to increase hydrophobicity and prevent deterioration of flowability and charging properties even under high humidity conditions, and can be appropriately selected depending on the purpose. Examples of the flowability improver include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils. It is particularly preferable that the silica and titanium oxide are surface-treated with such a flowability improving agent and used as hydrophobic silica and hydrophobic titanium oxide.
[0084] --Cleaning improver-- The cleaning property improver is not particularly limited as long as it is added to the toner in order to remove the developer remaining on the photoconductor or the primary transfer medium after transfer, and may be appropriately selected depending on the purpose. Examples of the cleaning property improver include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization, such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution, and the volume average particle size is preferably 0.01 μm to 1 μm. EXAMPLES
[0085] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0086] <Preparation of polyester resin 1> In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 2 mol ethylene oxide adduct of bisphenol A / 3 mol propylene oxide adduct of bisphenol A (molar ratio 40 / 60) as a diol component, terephthalic acid / adipic acid (molar ratio 85 / 15) as a dicarboxylic acid component, and 3.5 mol% trimethylolpropane based on the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2. Furthermore, 1,000 ppm of tetrabutyl orthotitanate based on the total monomer amount was added as a condensation catalyst, and the temperature was raised to 230°C over 2 hours under a nitrogen stream, and the reaction was carried out for 5 hours while distilling off the generated water. After that, the mixture was reacted for 4 hours under a reduced pressure of 5 mmHg to 15 mmHg, and then cooled to 180°C. After that, 1.0 mol% of trimellitic anhydride based on the total monomer amount and 200 ppm of tetrabutyl orthotitanate based on the total monomer amount were added, and the mixture was reacted for 1 hour at normal pressure at 180°C. After that, the mixture was reacted for another 3 hours under a reduced pressure of 5 mmHg to 20 mmHg, to obtain [Polyester Resin 1] having a glass transition point (Tg) of 57°C and a weight average molecular weight of 7,700, as determined from the DSC curve of the first heating cycle by DSC.
[0087] <Preparation of prepolymer 1> In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 3-methyl-1,5-pentanediol as a diol component, terephthalic acid / adipic acid (molar ratio 55 / 45) as a dicarboxylic acid component, 1.0 mol% trimethylolpropane with respect to the total monomer amount, and 0.5 mol% trimellitic anhydride with respect to the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.5. Furthermore, 1,000 ppm of tetrabutyl orthotitanate with respect to the total monomer amount was added as a condensation catalyst, and the temperature was raised to 200°C over 2 hours under a nitrogen stream, and the temperature was further raised to 230°C over 2 hours, and the reaction was carried out for 3 hours while distilling off the generated water. After that, the reaction was carried out for 5 hours under a reduced pressure of 5 mmHg to 15 mmHg to obtain [intermediate polyester 1] with a weight average molecular weight of 18,000.
[0088] Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester 1] and isophorone diisocyanate (IPDI) were placed in amounts such that the molar ratio (NCO / OH) between the isocyanate groups of IPDI and the hydroxyl groups of [intermediate polyester 1] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. The mixture was then heated to 80°C under a nitrogen stream and reacted for 5 hours to obtain an ethyl acetate solution of [prepolymer 1]. The glass transition temperature of the obtained amine-extended product of [Prepolymer 1] was −37° C. as determined from the DSC curve of the first heating run by DSC.
[0089] The amine-extended product of [Prepolymer 1] was obtained by the following procedure: First, ethyl acetate was added to [Prepolymer 1] so that it became a 20% ethyl acetate solution, and while stirring, a 20% ethyl acetate solution of isophoronediamine (IPDA) was added dropwise in an amount such that the molar ratio (NH2 / NCO) of the isocyanate groups of [Prepolymer 1] to the amino groups of IPDA became 1.1, and the mixture was thoroughly stirred. The obtained ethyl acetate solution of the amine extension product of [prepolymer 1] was cast onto a Teflon (registered trademark) petri dish and dried in an environment of 80°C for 10 hours, and further dried under reduced pressure in an environment of 120°C and 10 kPa or less to thoroughly remove the solvent, thereby obtaining an amine extension product of [prepolymer 1].
[0090] <Preparation of prepolymer 2> In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 1,6-hexanediol as a diol component, terephthalic acid / adipic acid (molar ratio 55 / 45) as a dicarboxylic acid component, 1.0 mol% trimethylolpropane relative to the total monomer amount, and 0.5 mol% trimellitic anhydride relative to the total monomer amount were added so that the molar ratio of hydroxyl groups to carboxylic acids (OH / COOH) was 1.5. Furthermore, 1,000 ppm of tetrabutyl orthotitanate relative to the total monomer amount was added as a condensation catalyst, and the temperature was raised to 200°C over 2 hours under a nitrogen stream, and then to 230°C over another 2 hours, and the reaction was carried out for 3 hours while distilling off the water produced. After that, the reaction was carried out for 5 hours under a reduced pressure of 5 mmHg to 15 mmHg to obtain [intermediate polyester 2] with a weight average molecular weight of 18,000.
[0091] Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester 2] and isophorone diisocyanate (IPDI) were placed in amounts such that the molar ratio (NCO / OH) of the isocyanate groups of IPDI to the hydroxyl groups of [intermediate polyester 2] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. The temperature was then raised to 80°C under a nitrogen stream and the reaction was carried out for 5 hours, yielding an ethyl acetate solution of [prepolymer 2]. The obtained ethyl acetate solution of the amine-extended product of [prepolymer 2] was cast onto a Teflon (registered trademark) petri dish, dried in an environment of 80°C for 10 hours, and further dried under reduced pressure in an environment of 120°C and 10 kPa or less to thoroughly remove the solvent, thereby obtaining an amine-extended product of [prepolymer 2]. The glass transition temperature of the obtained amine-extended product of [prepolymer 2] was −5° C. as determined from the DSC curve of the first heating run by DSC.
[0092] <Preparation of prepolymer 3> In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 3-methyl-1,5-pentanediol / bisphenol A 2-mol ethylene oxide adduct (molar ratio 20 / 80) as a diol component, isophthalic acid / adipic acid (molar ratio 60 / 40) as a dicarboxylic acid component, and 0.5 mol% trimellitic anhydride relative to the total monomer amount were added so that the molar ratio of hydroxyl group to carboxylic acid (OH / COOH) was 1.2. Furthermore, 1,000 ppm of tetrabutyl orthotitanate relative to the total monomer amount was added as a condensation catalyst, and the temperature was raised to 200°C over 2 hours under a nitrogen stream, and then to 230°C over another 2 hours, and the reaction was carried out for 3 hours while distilling off the water produced. After that, the reaction was carried out for 5 hours under a reduced pressure of 5 mmHg to 15 mmHg to obtain [intermediate polyester 3] with a weight average molecular weight of 18,000.
[0093] Next, in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, [intermediate polyester 2] and isophorone diisocyanate (IPDI) were placed in amounts such that the molar ratio (NCO / OH) of the isocyanate groups of IPDI to the hydroxyl groups of [intermediate polyester 3] was 2.0, and ethyl acetate was added to dissolve so as to obtain a 50% ethyl acetate solution. The mixture was then heated to 80°C under a nitrogen stream and reacted for 5 hours to obtain an ethyl acetate solution of [prepolymer 3]. The obtained ethyl acetate solution of the amine-extended product of [prepolymer 3] was cast onto a Teflon (registered trademark) petri dish and dried in an environment of 80°C for 10 hours, and further dried under reduced pressure in an environment of 120°C and 10 kPa or less to thoroughly remove the solvent, thereby obtaining an amine-extended product of [prepolymer 3]. The glass transition temperature of the obtained amine-extended product of [prepolymer 3] was 5°C as determined from the DSC curve of the first heating run by DSC.
[0094] <Preparation of Crystalline Polyester Resin Dispersion C-1a> <<Synthesis of crystalline polyester resin C-1>> Into a 5 L four-necked flask equipped with a nitrogen inlet tube, a dehydrating tube, a stirrer, and a heat transfer pair, 1,6-hexanediol and sebacic acid were charged so that the ratio of OH groups to COOH groups (OH / COOH) was 1.1. While flowing out water together with 500 ppm of titanium tetraisopropoxide with respect to the mass of the charged raw materials, the reaction was carried out, and finally the temperature was raised to 235 °C and the reaction was carried out for 1 hour. Then, the reaction was carried out for 6 hours under a reduced pressure of 10 mmHg or less. Then, the temperature was set to 185 °C, and trimellitic anhydride was added so that the molar ratio to the COOH group was 0.053, and the reaction was carried out for 2 hours with stirring to obtain [crystalline polyester resin C-1].
[0095] To the four-necked flask, [crystalline polyester resin C-1] (55 parts by mass), methyl ethyl ketone (35 parts by mass), and 2-propyl alcohol (10 parts by mass) were added. Then, while heating at the melting point temperature of [crystalline polyester resin C-1], stirring was carried out to dissolve the above crystalline polyester resin. Then, a 28% by mass aqueous ammonia solution was added so that the neutralization rate became 200%. The neutralization rate was calculated from the acid value of the crystalline polyester resin. Further, ion-exchanged water (130 parts by mass) was gradually added, phase inversion emulsification was carried out, and then solvent removal was carried out. Then, ion-exchanged water was added to adjust the solid content concentration (concentration of the crystalline polyester resin) to 25% by mass, and [dispersion liquid C-1a of the crystalline polyester resin], which is a binder resin dispersion for toner, was obtained. The particle size of the crystalline polyester resin in [dispersion liquid C-1a of the crystalline polyester resin] was 250 nm, and the melting point was 65 °C.
[0096] <Preparation of WAX Emulsion 1> To 100 parts by mass of ion-exchanged water, 28 parts by mass of paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.) as a wax and Sanisol B50 as a surfactant were added. This was dispersed with a homogenizer while heating to 90 °C to obtain [WAX Emulsion 1]. The solid content concentration was 30% by mass.
[0097] (Example 1) <Preparation of Toner> <<Oil Phase Preparation Step, Phase Inversion Emulsification Step>> A four-neck flask was charged with 100 parts by mass of [polyester resin 1], 10 parts by mass of [prepolymer 1], 10 parts by mass of carbon black (REGAL 400R, manufactured by Cabot Corporation), and 120 parts by mass of ethyl acetate, and the mixture was stirred at 10°C, 8,000 rpm, and 60 minutes using a homomixer (manufactured by Primix Corporation) to dissolve and disperse the mixture, thereby preparing an oil phase. Then, 28% by mass of ammonia aqueous solution was added while stirring to neutralize the oil phase to a neutralization rate of 400%. Furthermore, 340 parts by mass of ion-exchanged water was gradually added to carry out phase inversion emulsification. After that, the solvent was removed to obtain [Slurry 1]. The particle size of [Slurry 1] was measured to be 0.50 μm. The solid content concentration was also measured to be 23.0% by mass.
[0098] <<Agglomeration process, fusion process>> 100 parts by mass of [Slurry 1], 6.0 parts by mass of [Crystalline polyester resin dispersion C-1a], 5.0 parts by mass of [WAX emulsion 1], and 300 parts by mass of ion-exchanged water were placed in a container and stirred for 1 minute. Next, 100 parts by mass of 3% by mass magnesium chloride solution was dropped and stirred for another 5 minutes, and then the temperature was raised to 60°C. After that, when the particle size became 5.0 μm, 50 parts by mass of sodium chloride was added to terminate the aggregation process, and aggregated slurry 1 was obtained. The aggregated slurry 1 was heated to 70° C. while stirring to fuse the fine particles, and when the desired circularity of 0.957 was reached, the slurry was cooled to obtain [toner dispersion 1].
[0099] <<Cleaning and drying process, annealing process>> [Toner dispersion liquid 1] was stored at 45° C. for 10 hours, filtered under reduced pressure, and washed and dried as follows. (1) 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (2): 900 parts of ion-exchanged water was added to the filter cake of (1), and ultrasonic vibration was applied and mixed with a TK homomixer (rotation speed 12,000 rpm for 30 minutes), and then the mixture was filtered under reduced pressure. This operation was repeated until the electrical conductivity of the reslurry liquid became 10 μC / cm or less, and then the mixture was filtered to obtain [Filter cake 1]. [Filter cake 1] was dried in a circulating air dryer at 45° C. for 48 hours, sieved through a 75 μm mesh, and annealed at 45° C. for 10 hours to obtain [colored resin particles 1].
[0100] <<External addition process>> To 100 parts by mass of [colored resin particles 1], 2.5 parts by mass of inorganic fine particles, fumed silica (CAB-O-SIL (registered trademark) TS-530, manufactured by Cabot Corporation), was added, and mixed in a Henschel mixer at 40 m / s for 10 minutes to obtain the toner of Example 1.
[0101] Example 2 A toner of Example 2 was obtained in the same manner as in Example 1, except that in the oil phase preparation step and the transfer emulsification step, the organic solvent used was changed from ethyl acetate to methyl ethyl ketone (MEK).
[0102] Example 3 A toner of Example 3 was obtained in the same manner as in Example 1, except that the [Prepolymer 1] used in Example 1 was changed to [Prepolymer 2].
[0103] Example 4 A toner of Example 4 was obtained in the same manner as in Example 1, except that the [Prepolymer 1] used in Example 1 was changed to [Prepolymer 3].
[0104] Comparative Example 1 A toner of Comparative Example 1 was obtained in the same manner as in Example 1, except that the prepolymer was not added.
[0105] Comparative Example 2 A toner of Comparative Example 2 was obtained in the same manner as in Example 1, except that the amount of organic solvent added and the stirring conditions were adjusted so that the particle size of the slurry obtained after phase inversion emulsification was 5.0 μm, and the aggregation process was not performed. When the dot-shaped abnormal images were evaluated (described later), many dot-shaped abnormal images were found. Unmelted particles were present in the center of the abnormal image areas, and analysis of these particles with an IR microscope confirmed that they were composed of elongated prepolymers.
[0106] Comparative Example 3 The toner of Comparative Example 3 was obtained in the same manner as in Example 2, except that the amount of organic solvent added and the stirring conditions were adjusted so that the particle size of the slurry obtained after phase inversion emulsification was 5.0 μm, and the aggregation process was not performed. When the dot-shaped abnormal images were evaluated (described later), many dot-shaped abnormal images were found. Unmelted particles were present in the center of the abnormal image areas, and analysis of these particles with an IR microscope confirmed that they were composed of elongated prepolymers.
[0107] <Evaluation> The toners prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were evaluated as follows. The results are shown in Table 1.
[0108] <<Image of dot-like abnormalities>> Using a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), 100 solid images were printed at 23° C. and 50% RH. The image was visually inspected for the presence of dot-like abnormal images (black spots), and evaluated according to the following evaluation criteria. [Evaluation Criteria] ◎: 0 dot-shaped abnormal images out of 100 images ○: 5 or less dot-shaped abnormal images out of 100 images ×: 6 or more dot-shaped abnormal images out of 100 images
[0109] <<High temperature fixability>> Using the fixing unit of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), a 0.6 mg / cm2 ink was applied to plain paper. 2 The temperature at which hot offset occurs was measured and rated on a three-level scale. [Evaluation Criteria] ◎: Hot offset occurs at temperatures of 190°C or higher ○: The temperature at which hot offset occurs is 170℃ or higher and less than 190℃. ×: The temperature at which hot offset occurs is less than 170°C.
[0110] <<Low temperature fixability>> Using the fixing unit of a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.), a 0.6 mg / cm2 ink was applied to plain paper. 2 The temperature at which cold offset occurs is measured and rated on a three-level scale. [Evaluation Criteria] ◎: Cold offset occurs at temperatures below 120℃ ○: The temperature at which cold offset occurs is 120℃ or higher and less than 130℃. ×: The temperature at which cold offset occurs is 130°C or higher.
[0111] [Table 1]
[0112] For example, aspects of the present invention are as follows. <1> a) dissolving or dispersing at least a polyester resin and a prepolymer in an organic solvent to prepare an oil phase; b) adding an aqueous medium to the oil phase to effect phase inversion emulsification to obtain an oil-in-water dispersion; and c) aggregating fine particles in the oil-in-water dispersion. <2> The organic solvent is ethyl acetate. <1> The present invention relates to a method for producing toner particles. <3> The organic solvent is methyl ethyl ketone. <1> The present invention relates to a method for producing toner particles. <4> The prepolymer has a Tg of 0° C. or less. <1> from <3> 2. The method for producing the toner particles according to claim 1,
[0113] The above <1> from <4> The method for producing toner particles according to any one of the above items can solve the above-mentioned problems in the prior art and achieve the object of the present invention. [Prior art documents] [Patent documents]
[0114] [Patent Document 1] JP 2000-194160 A
Claims
1. a) dissolving or dispersing at least a polyester resin and a prepolymer in an organic solvent to prepare an oil phase; b) adding an aqueous medium to the oil phase to effect phase inversion emulsification to obtain an oil-in-water dispersion; c) agglomerating the fine particles in the oil-in-water dispersion, The method for producing toner particles, wherein the prepolymer has a Tg of 0° C. or lower.
2. 2. The method for producing toner particles according to claim 1, wherein the organic solvent is ethyl acetate.
3. a) dissolving or dispersing at least a polyester resin and a prepolymer in an organic solvent to prepare an oil phase; b) adding an aqueous medium to the oil phase to effect phase inversion emulsification to obtain an oil-in-water dispersion; c) agglomerating the fine particles in the oil-in-water dispersion, The method for producing toner particles, wherein the organic solvent is methyl ethyl ketone.
4. The method for producing toner particles according to claim 3, wherein the prepolymer has a Tg of 0° C. or lower.
Citation Information
Patent Citations
Toner and its manufacture
JP2000194160A
Toner for electrostatic latent image development, image forming method, process cartridge, toner container and method for manufacturing toner
JP2007192952A
Toner for electrostatic latent image development, method for manufacturing the same, electrostatic latent image developer using the toner, toner container, image forming apparatus and process cartridge
JP2008070829A
Toner, developer, and color toner set
JP2013225096A
Toner and manufacturing method of the same
JP2017076124A