Method for producing toner for developing electrostatic images

By adding a flocculant and controlling viscosity and shear rates, the method addresses the issue of coarse toner contamination in electrostatic image development, achieving a more uniform particle size distribution and improved toner quality.

JP7589606B2Active Publication Date: 2024-11-26FUJIFILM BUSINESS INNOVATION CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021046473
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-19
Publication Date
2024-11-26
Estimated Expiration
2041-03-19

AI Technical Summary

Technical Problem

Existing methods for producing toner for electrostatic image development result in high contamination of coarse toner due to excessive particle growth during the agglomeration process, which is exacerbated by high viscosity in the dispersion liquid.

Method used

A method involving the addition of a flocculant to a dispersion containing binder resin particles, followed by a controlled reduction in viscosity through the addition of water or surfactants, and subsequent heating to form agglomerated particles, with specific viscosity and shear rate conditions applied to prevent excessive particle growth.

Benefits of technology

This approach reduces the amount of coarse toner contamination by maintaining optimal viscosity and shear conditions, resulting in a more uniform particle size distribution and improved toner quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589606000002
    Figure 0007589606000002
  • Figure 0007589606000001
    Figure 0007589606000001
Patent Text Reader

Abstract

To provide a method for manufacturing toner for electrostatic charge image development which reduces mixture of coarse toner.SOLUTION: A method for manufacturing toner for electrostatic charge image development includes: an aggregating agent mixing step of adding an aggregating agent to a dispersion liquid containing binder resin particles while circulating the dispersion liquid containing the binder resin particles between an agitation tank and a dispersion machine for imparting a mechanical shear force, and mixing the dispersion liquid containing the binder resin particles with the aggregation agent; an aggregation step of lowering the viscosity of the dispersion liquid through the aggregation agent mixing step, then heating the dispersion liquid to form aggregated particles; and a uniting step of heating the dispersion liquid containing the aggregated particles, fusing and uniting the aggregated particles to form toner particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a toner for developing electrostatic images, a toner for developing electrostatic images, and an electrostatic image developer. [Background technology]

[0002] In Patent Document 1, a shear rate of 10 s -1 In the flocculation step, the flocculation liquid is stirred with a multi-shaft stirring blade at a shear rate of 10 s -1 The following portion is 50% by volume or less and the shear rate is 400 s -1 A method for producing a toner in which the above-mentioned portion is 1% by volume or less is disclosed. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-008042 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present disclosure is to provide a method for producing a toner for developing electrostatic images that reduces the inclusion of coarse toner particles, compared to a production method in which a dispersion liquid that has been subjected to an aggregating agent mixing step is heated to form aggregated particles without reducing the viscosity of the dispersion liquid. [Means for solving the problem]

[0005] Means for solving the above problems include the following aspects. <1> a flocculant mixing step of adding a flocculant to the dispersion containing binder resin particles while circulating the dispersion containing binder resin particles between a stirring tank and a disperser that applies a mechanical shear force, and mixing the flocculant into the dispersion containing binder resin particles; an aggregation step of reducing the viscosity of the dispersion liquid that has been subjected to the aggregating agent mixing step and then heating the dispersion liquid to form aggregated particles; a coalescence step of heating the dispersion liquid containing the aggregated particles to fuse and coalesce the aggregated particles to form toner particles; A method for producing a toner for developing an electrostatic image comprising the steps of: <2> In the flocculation step, the viscosity of the dispersion liquid having undergone the flocculant mixing step is reduced by more than 5 Pa s and less than 50 Pa s. <1> 2. A method for producing the toner for developing electrostatic images according to claim 1 . The viscosity of the dispersion is measured at a shear rate of 1 / s using a portion of the dispersion as a sample at a sample temperature of 25°C. <3> The viscosity of the dispersion in the flocculant mixing step is 25 Pa·s or more and 85 Pa·s or less, and the peripheral speed of the rotor tip of the disperser that applies the mechanical shear force is 30 m / sec or more and 50 m / sec or less. <1> or <2> 2. A method for producing the toner for developing electrostatic images according to claim 1 . The viscosity of the dispersion is measured at a shear rate of 1 / s using a portion of the dispersion as a sample at a sample temperature of 25°C. <4> The flocculation step includes adding water to the dispersion liquid that has been subjected to the flocculant mixing step. <1> ~ <3> 13. The method for producing the toner for developing electrostatic images according to claim 12. <5> The flocculant comprises a trivalent metal salt compound; <1> ~ <4> 13. The method for producing the toner for developing electrostatic images according to claim 12. <6> the dispersion liquid containing the binder resin particles contains amorphous polyester resin particles and crystalline polyester resin particles as the binder resin particles; <1> ~ <5> 13. The method for producing the toner for developing electrostatic images according to claim 12. <7> The dispersion liquid containing the binder resin particles further contains release agent particles. <1> ~ <6> 13. The method for producing the toner for developing electrostatic images according to claim 12. <8> The dispersion liquid containing the binder resin particles further contains colorant particles. <1> ~ <7> 13. The method for producing the toner for developing electrostatic images according to claim 12. <9> the method further includes a second aggregation step of mixing a dispersion containing the aggregated particles with a dispersion containing resin particles that will become a shell layer, and aggregating the resin particles that will become the shell layer on the surfaces of the aggregated particles to form second aggregated particles, the coalescence step is a step of heating a dispersion liquid containing the second aggregated particles to fuse and coalesce the second aggregated particles to form toner particles; <1> ~ <8> 13. The method for producing the toner for developing electrostatic images according to claim 12. <10> <1> ~ <9> 13. A toner for developing electrostatic images, produced by the method for producing a toner for developing electrostatic images according to any one of claims 1 to 12. <11> <1> ~ <9> 2. An electrostatic image developer comprising a toner for developing electrostatic images produced by the method for producing a toner for developing electrostatic images according to any one of claims 1 to 11. Effect of the Invention

[0006] <1> , <4> , <5> , <6> , <7> , <8> and <9> According to the present invention, there is provided a method for producing a toner for developing electrostatic images, which reduces the inclusion of coarse toner particles, compared to a production method in which a dispersion liquid that has been subjected to a coagulant mixing step is heated to form coagulated particles without reducing the viscosity of the dispersion liquid. <2> According to the present invention, there is provided a method for producing a toner for developing electrostatic images, which reduces the inclusion of coarse toner particles, compared to when the viscosity of the dispersion liquid after the aggregating agent mixing process is reduced by 5 Pa·s or less or 50 Pa·s or more. <3> According to the present invention, a method for producing a toner for developing electrostatic images is provided which reduces the inclusion of coarse toner particles compared to when the viscosity of the dispersion in the aggregating agent mixing process is less than 25 Pa·s or exceeds 85 Pa·s, or when the peripheral speed of the rotor tip of the dispersing machine is less than 30 m / sec or exceeds 50 m / sec. <10> According to the present invention, there is provided a toner for developing electrostatic images in which the amount of coarse toner particles mixed in is reduced. <11> According to the present invention, there is provided an electrostatic image developer in which the amount of coarse toner particles mixed in is reduced. [Brief description of the drawings]

[0007] [Figure 1] FIG. 2 is a schematic diagram illustrating an embodiment of a circulation type reaction tank used in the toner production method according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.

[0009] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values ​​before and after "~" as the minimum and maximum values, respectively.

[0010] In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0011] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved.

[0012] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.

[0013] In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.

[0014] In the present disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic, and "(meth)acrylate" means at least one of acrylate and methacrylate.

[0015] In this disclosure, "toner" refers to "toner for developing electrostatic images", "developer" refers to "electrostatic image developer", and "carrier" refers to "carrier for developing electrostatic images".

[0016] In the present disclosure, a method for producing toner particles by aggregating and coalescing material particles in a solvent is referred to as an EA (emulsion aggregation) method.

[0017] <Method of manufacturing toner for developing electrostatic images> The toner production method according to the present embodiment is a toner production method that includes producing toner particles by the EA method, and includes the following aggregating agent mixing step, aggregation step, and coalescence step.

[0018] Flocculant mixing process: A process in which a flocculant is added to the dispersion liquid containing binder resin particles while circulating the dispersion liquid containing binder resin particles between a stirring tank and a disperser that applies mechanical shear force, and the flocculant is mixed into the dispersion liquid containing binder resin particles. Aggregation process: A process in which the viscosity of the dispersion liquid that has been through the aggregating agent mixing process is reduced, and then the dispersion liquid is heated to form aggregated particles. Coalescence process: A process in which the dispersion liquid containing the aggregated particles is heated to fuse and coalesce the aggregated particles to form toner particles.

[0019] In the toner manufacturing method according to the present embodiment, the aggregation of the binder resin particles may start in the dispersion liquid in the aggregating agent mixing step. In this case, the aggregation step can be said to be a step of promoting the growth of the aggregates to form aggregated particles.

[0020] In the present disclosure, a reaction vessel equipped with a stirring vessel and a disperser that applies mechanical shear force and in which the contents are circulated between the stirring vessel and the disperser is referred to as a "circulation reaction vessel".

[0021] In order to make the particle size distribution of the toner particles produced by the EA method relatively narrow, it is desirable that the aggregating agent and each material particle are mixed and dispersed with high uniformity in the dispersion liquid to which the aggregating agent is added. For this purpose, a mechanical shear force is applied to the dispersion liquid by a disperser while circulating in a circulation type reaction tank, so that the aggregating agent and each material particle are mixed and dispersed. At this time, in order to efficiently apply the mechanical shear force to the dispersion liquid, it is desirable for the viscosity of the dispersion liquid to be relatively high. However, if the viscosity of the dispersion liquid is high, the mixing of the aggregated particles in the stirring tank deteriorates when the dispersion liquid is heated to form aggregated particles, and some particles grow excessively, generating aggregated particles with large diameters. As a result, coarse toner particles are mixed into the finished toner. In contrast, in the toner manufacturing method according to the present embodiment, the viscosity of the dispersion liquid is reduced before the dispersion liquid is heated to form aggregated particles. According to the toner manufacturing method according to the present embodiment, the viscosity of the dispersion liquid is not too high when the dispersion liquid is heated, so that the mixability of the aggregated particles is improved and the growth of the aggregated particles does not proceed excessively, thereby reducing the inclusion of coarse toner particles.

[0022] In this embodiment, the viscosity of the dispersion is measured using a part of the dispersion as a sample at a sample temperature of 25° C. Details of the method for measuring the viscosity of the dispersion are as follows. A rotational viscometer is used. An example of the rotational viscometer is Brookfield's R / S Plus Rheometer (spindle: CP-75-1). The rotational viscometer is placed in an environment with a temperature of 25°C and a relative humidity of 55%. During the process, samples to be measured are taken multiple times to confirm the viscosity of the dispersion during the process. The sample is 3 g of the dispersion liquid adjusted to a temperature of 25°C. The shear rate (s -1 The shear rate (s) is increased and then decreased at 0.2 increments per second, and the shear stress (Pa) is measured every 2 seconds. -1 ) is taken as the common logarithm, and the vertical axis is the shear stress (Pa) and the shear rate (s -1) is taken as a common logarithm of the viscosity (Pa s), and the viscosity is plotted against the shear rate to draw straight lines for both ascending and descending viscosity. For each of the lines ascending and descending viscosity, the viscosity (Pa s) at 1 / s is found from the common logarithm of the viscosity at 1 / s (common logarithm of shear rate = 0) (the intercept of the line) and the average of the two values ​​is calculated. The measurement is carried out three times and the average is calculated to obtain the viscosity (Pa s) at a shear rate of 1 / s.

[0023] In the aggregation step, the method for reducing the viscosity of the dispersion is not limited. Examples of the method for reducing the viscosity of the dispersion include adding water and adding a surfactant.

[0024] Fig. 1 shows an example of a circulation type reaction tank used in the flocculant mixing step, the flocculation step, and the coalescence step. The sizes of the members in the drawing are conceptual, and the relative relationship between the sizes of the members is not limited to this.

[0025] 1 includes a stirring tank 10 and a disperser 90. The stirring tank 10 and the disperser 90 are connected via a pipe 82 and a pipe 84. The stirring tank 10 includes a baffle 20 and a paddle blade 40. The baffle 20 is plate-shaped or cylindrical, and two, three, or four baffles 20 are provided at equal intervals on the inner side surface of the stirring tank 10. The paddle blades 40 are provided on the rotating shaft 60 in two stages. The dispersing machine 90 has therein a mechanism for applying mechanical shear force. Pipe 82 connects the bottom of stirring tank 10 with the inlet of disperser 90. The connection between stirring tank 10 and pipe 82 is provided with an openable and closable valve (not shown). A material inlet 86 is provided midway through the pipe 82. A flocculant, water, and a surfactant are added through the inlet 86. The pipe 84 connects the discharge port of the disperser 90 to the upper part of the stirring tank 10. The end of the pipe 84 is immersed in the dispersion liquid contained in the stirring tank 10.

[0026] In the flocculant mixing step, the dispersion containing binder resin particles is circulated between the stirring tank 10 and the disperser 90 while continuing the rotation of the paddle blades 40 and the operation of the disperser 90. The dispersion containing binder resin particles leaves the bottom of the stirring tank 10 and enters the disperser 90 through a pipe 82. The dispersion containing binder resin particles leaves the disperser 90 and enters the stirring tank 10 through a pipe 84. While the dispersion containing binder resin particles is circulating, a flocculant is added from an inlet 86, and the dispersion containing binder resin particles is continuously circulated to mix the flocculant into the dispersion containing binder resin particles. After the coagulant mixing step, the valve at the connection between the mixing tank 10 and the pipe 82 is closed. In the aggregation step, for example, water is fed from the feed port 86 while continuing to rotate the paddle blades 40. The water fed from the feed port 86 is fed into the stirring tank 10 via the disperser 90 and the pipe 84, and mixed with the dispersion contained in the stirring tank 10. Next, the dispersion contained in the stirring tank 10 is heated. In the coalescence step, the dispersion contained in the stirring tank 10 is heated while the paddle blades 40 continue to rotate.

[0027] The steps and materials of the method for producing the toner according to this embodiment will be described in detail below.

[0028] [Flocculant mixing process] The flocculant mixing step is a step of adding a flocculant to the dispersion liquid containing the binder resin particles while circulating the dispersion liquid containing the binder resin particles in a circulation reaction tank, thereby mixing the flocculant into the dispersion liquid containing the binder resin particles. The dispersion liquid to be subjected to the flocculant mixing step contains at least the binder resin particles, and may also contain at least one of release agent particles and colorant particles.

[0029] The dispersion liquid to be subjected to the flocculating agent mixing step is prepared, for example, by preparing a resin particle dispersion liquid containing binder resin particles, a release agent particle dispersion liquid containing release agent particles, and a colorant particle dispersion liquid containing colorant particles, and mixing these particle dispersion liquids. The order in which these particle dispersion liquids are mixed is not limited.

[0030] Hereinafter, the resin particle dispersion, the release agent particle dispersion, and the colorant particle dispersion will be collectively referred to as "particle dispersion" to describe what they have in common.

[0031] An example of an embodiment of a particle dispersion liquid is a dispersion liquid in which a material is dispersed in the form of particles in a dispersion medium by a surfactant.

[0032] The dispersion medium of the particle dispersion liquid is preferably an aqueous medium. Examples of the aqueous medium include water and alcohol. The water is preferably water with a reduced ion content, such as distilled water or ion-exchanged water. These aqueous media may be used alone or in combination of two or more.

[0033] The surfactant for dispersing the material in the dispersion medium may be any of anionic surfactants, cationic surfactants, and nonionic surfactants. Examples of such surfactants include anionic surfactants such as sulfate ester salts, sulfonate salts, phosphate esters, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The surfactants may be used alone or in combination of two or more. The nonionic surfactants may be used in combination with an anionic surfactant or a cationic surfactant.

[0034] Methods for dispersing a material in a particulate form in a dispersion medium include known dispersion methods using a rotary shear type homogenizer, a ball mill having media, a sand mill, a dyno mill, and the like.

[0035] The phase inversion emulsification method is a method for dispersing a resin in a dispersion medium in the form of particles. The phase inversion emulsification method involves dissolving the resin in a hydrophobic organic solvent in which the resin is soluble, adding a base to the organic continuous phase (O phase) to neutralize it, and then introducing an aqueous medium (W phase) to invert the phase from W / O to O / W, dispersing the resin in the form of particles in the aqueous medium.

[0036] The volume average particle size of the particles dispersed in the particle dispersion is preferably 30 nm or more and 300 nm or less, more preferably 50 nm or more and 250 nm or less, and even more preferably 80 nm or more and 200 nm or less. The volume average particle size of particles in a particle dispersion refers to the particle size that is 50% cumulative from the smallest diameter side in a particle size distribution measured with a laser diffraction particle size distribution measuring device (for example, LA-700 manufactured by Horiba, Ltd.).

[0037] The content of particles contained in the particle dispersion is preferably from 5% by mass to 50% by mass, more preferably from 10% by mass to 40% by mass, and even more preferably from 15% by mass to 30% by mass.

[0038] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.

[0039] The binder resin is preferably a polyester resin, for example, an amorphous polyester resin or a crystalline polyester resin.

[0040] In the present embodiment, the "crystalline" of the polyester resin refers to a state in which, in differential scanning calorimetry (DSC), the resin has a clear endothermic peak rather than a stepwise change in endothermic amount, and specifically refers to a state in which the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10°C / min. In the present embodiment, the "amorphous" polyester resin refers to a half-width exceeding 10° C., a stepwise change in endothermic heat amount being exhibited, or no clear endothermic peak being observed.

[0041] -Amorphous polyester resin- The amorphous polyester resin may be a commercially available product or a synthetic product. The amorphous polyester resin may be, for example, a condensation polymer of a polycarboxylic acid and a polyhydric alcohol.

[0042] Examples of polyvalent carboxylic acids that are polymerization components of amorphous polyester resins include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., carbon number 1 to 5). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0043] Examples of polyhydric alcohols that are polymerization components of amorphous polyester resins include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol which is a polymerization component of the amorphous polyester resin, a polyhydric alcohol having a crosslinked structure or a branched structure of trihydric or more may be used in combination with the diol. Examples of the polyhydric alcohol having trihydric or more include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.

[0044] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), and more specifically, is determined from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."

[0045] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.

[0046] The amorphous polyester resin can be obtained by a known production method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present in the copolymerization reaction, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.

[0047] -Crystalline polyester resin- The crystalline polyester resin may be a commercially available product or a synthetic product. Examples of the crystalline polyester resin include polycondensates of polyvalent carboxylic acids and polyhydric alcohols. The crystalline polyester resin is preferably a polycondensate of a linear aliphatic polymerizable monomer rather than a polymerizable monomer having an aromatic ring, since it easily forms a crystal structure.

[0048] Examples of polyvalent carboxylic acids that are polymerization components of crystalline polyester resins include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.

[0049] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.

[0050] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature of the release agent is determined from a DSC curve obtained by differential scanning calorimetry (DSC) in accordance with the "melting peak temperature" described in the method for determining the melting temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."

[0051] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, and Examples of the coloring agent include pigments such as rutramarine blue, chalco oil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate; dyes such as acridine, xanthene, azo, benzoquinone, azine, anthraquinone, thioindigo, dioxazine, thiazine, azomethine, indigo, phthalocyanine, aniline black, polymethine, triphenylmethane, diphenylmethane, and thiazole; etc. The coloring agent may be used alone or in combination of two or more.

[0052] The colorant may be surface-treated as necessary, and may be used in combination with a dispersant.

[0053] A dispersion liquid obtained by mixing a plurality of types of particle dispersion liquids is called a "mixed dispersion liquid."

[0054] After mixing the multiple types of particle dispersions, it is preferable to adjust the pH of the mixed dispersion to a range of 3 to 4. Examples of a means for adjusting the pH of the mixed dispersion include the addition of an acidic aqueous solution such as a nitric acid aqueous solution, a hydrochloric acid aqueous solution, or a sulfuric acid aqueous solution.

[0055] The mass ratio of the particles contained in the mixed dispersion is preferably in the following range. When the mixed dispersion contains release agent particles, the mass ratio of the binder resin particles to the release agent particles (binder resin particles:release agent particles) is preferably 100:4 to 100:24, more preferably 100:8 to 100:22, and even more preferably 100:12 to 100:20. When the mixed dispersion contains colorant particles, the mass ratio of the binder resin particles to the colorant particles (binder resin particles:colorant particles) is preferably 100:4 to 100:24, more preferably 100:8 to 100:22, and even more preferably 100:12 to 100:20.

[0056] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant contained in the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. The flocculant may be used alone or in combination of two or more kinds.

[0057] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate; and inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.

[0058] The flocculant is preferably a divalent or higher metal salt compound, more preferably a trivalent metal salt compound, and even more preferably a trivalent inorganic aluminum salt compound, such as aluminum chloride, aluminum sulfate, polyaluminum chloride, and polyaluminum hydroxide.

[0059] The amount of the flocculant to be added is not limited. When a trivalent metal salt compound is used as the flocculant, the amount of the trivalent metal salt compound to be added is preferably 0.5 parts by mass or more and 5.0 parts by mass or less, more preferably 0.6 parts by mass or more and 4.0 parts by mass or less, and even more preferably 0.7 parts by mass or more and 3.0 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0060] The flocculant mixing step includes circulating a dispersion liquid containing at least binder resin particles through a circulation type reaction tank, thereby making the particle size distribution of the toner particles relatively narrow.

[0061] In order to efficiently apply mechanical shear force to the dispersion, it is preferable that the viscosity of the dispersion is relatively high. The viscosity of the dispersion in the flocculant mixing step is preferably from 25 Pa·s to 85 Pa·s, more preferably from 30 Pa·s to 80 Pa·s, and even more preferably from 35 Pa·s to 75 Pa·s. The viscosity of the dispersion in the flocculant mixing step may be constant or may vary throughout the flocculant mixing step. The above viscosity is measured at a shear rate of 1 / s using a part of the dispersion as a sample at a sample temperature of 25°C.

[0062] In the flocculant mixing step, it is preferable that the viscosity of the dispersion in the flocculant mixing step is in the above-mentioned range, and that the peripheral speed of the tip of the rotor of the disperser that imparts a mechanical shear force to the dispersion is 30 m / sec or more and 50 m / sec or less. By setting the viscosity of the dispersion and the peripheral speed of the rotor tip of the dispersing machine within the above ranges, a shear force is efficiently applied to the dispersion in the flocculant mixing step.

[0063] [Agglutination process] The aggregation step is a step in which the viscosity of the dispersion liquid that has been subjected to the aggregating agent mixing step is reduced, and then the dispersion liquid is heated to form aggregated particles. When the aggregation of the binder resin particles has started in the dispersion liquid in the aggregating agent mixing step, the aggregation step can be said to be a step of promoting the growth of the aggregates to form aggregated particles.

[0064] The viscosity of the dispersion liquid after the flocculant mixing step can be reduced by, for example, adding at least one of water and a surfactant to the dispersion liquid. The water is preferably water with a reduced ion content, such as distilled water or ion-exchanged water. When a surfactant is added, it is preferable to use the type of surfactant used in preparing particle dispersion liquids of various materials.

[0065] The amount of water or surfactant added is not limited. The amount of water or surfactant added is preferably an amount that reduces the viscosity of the dispersion liquid after the flocculant mixing step by more than 5 Pa s and less than 50 Pa s. The above viscosity is measured at a shear rate of 1 / s using a part of the dispersion as a sample at a sample temperature of 25°C.

[0066] The degree of reduction in the viscosity of the dispersion liquid after the flocculant mixing step is preferably more than 5 Pa·s and less than 50 Pa·s, more preferably 8 Pa·s or more and 48 Pa·s or less, and even more preferably 10 Pa·s or more and 45 Pa·s or less, from the viewpoint of a balance between efficiently applying shear force to the dispersion liquid in the flocculant mixing step and efficiently promoting the formation of flocculant particles in the aggregation step. The above viscosity is measured at a shear rate of 1 / s using a part of the dispersion as a sample at a sample temperature of 25°C.

[0067] The temperature that the dispersion liquid reaches when it is heated in the aggregation step is preferably a temperature based on the glass transition temperature (Tg) of the binder resin particles, for example, a temperature not lower than (Tg-30°C) and not higher than (Tg-5°C) of the binder resin particles. When the dispersion contains a plurality of types of binder resin particles having different Tg's, the lowest temperature among the Tg's is set as the Tg in the aggregation step.

[0068] [Second flocculation step] The second aggregation step is a step for the purpose of producing a toner having a core-shell structure, and is a step that is performed after the aggregation step.

[0069] The second aggregation step is a step of mixing a dispersion liquid containing aggregated particles with a dispersion liquid containing resin particles that will form the shell layer, and aggregating the resin particles that will form the shell layer on the surfaces of the aggregated particles to form second aggregated particles.

[0070] As the dispersion liquid containing the resin particles that will become the shell layer, at least one selected from binder resin particle dispersion liquids for forming the core is suitable, a polyester resin particle dispersion liquid is more suitable, and an amorphous polyester resin particle dispersion liquid is even more suitable.

[0071] The second aggregation step may, for example, adding a dispersion liquid containing resin particles to be a shell layer to the dispersion liquid containing the aggregated particles while stirring the dispersion liquid containing the aggregated particles; and heating, while stirring, the dispersion liquid containing the aggregated particles after adding the dispersion liquid containing the resin particles that will form the shell layer.

[0072] When the dispersion liquid containing the aggregated particles is heated, the temperature that the dispersion liquid containing the aggregated particles reaches is preferably a temperature based on the glass transition temperature (Tg) of the resin particles that form the shell layer, for example, a temperature that is equal to or higher than (Tg-30°C) and equal to or lower than (Tg-5°C) of the resin particles that form the shell layer.

[0073] After the aggregated particles or the second aggregated particles have grown to a predetermined size, a chelating agent for the aggregating agent used in the aggregation step may be added to the dispersion containing the aggregated particles or the second aggregated particles in order to stop the growth of the aggregated particles or the second aggregated particles before the heating in the coalescence step is performed. Examples of the chelating agent include oxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid; and aminocarboxylic acids such as iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA). The amount of the chelating agent added is preferably 0.01 parts by mass or more and 5.0 parts by mass or less, and more preferably 0.1 parts by mass or more and less than 3.0 parts by mass, based on 100 parts by mass of the binder resin particles.

[0074] After the aggregated particles or the second aggregated particles have grown to a predetermined size, the pH of the dispersion containing the aggregated particles or the second aggregated particles may be increased in order to stop the growth of the aggregated particles or the second aggregated particles before the heating in the coalescence step is performed. The means for increasing the pH of the dispersion containing the aggregated particles or the second aggregated particles includes the addition of at least one selected from the group consisting of an aqueous solution of an alkali metal hydroxide and an aqueous solution of an alkaline earth metal hydroxide. The ultimate pH of the dispersion containing the aggregated particles or the second aggregated particles is preferably 8 or more and 10 or less.

[0075] [Uniting process] The coalescence step is a step in which the dispersion liquid containing the aggregated particles is heated to fuse and coalesce the aggregated particles to form toner particles.

[0076] When the second aggregation step is performed before the coalescence step, the coalescence step is a step in which the dispersion liquid containing the second aggregated particles is heated to fuse and coalesce the second aggregated particles to form toner particles. By performing the second aggregation step and the coalescence step, toner particles having a core-shell structure can be produced.

[0077] The form described below is common to the aggregated particles and the second aggregated particles.

[0078] The temperature reached by the dispersion liquid containing the aggregated particles is preferably equal to or higher than the glass transition temperature (Tg) of the binder resin, and specifically, is preferably 10° C. to 35° C. higher than the Tg of the binder resin. When the aggregated particles contain a plurality of binder resins having different Tg's, the highest temperature among the Tg's is defined as the glass transition temperature in the coalescence step.

[0079] After the coalescence step, the toner particles in the dispersion are subjected to a known washing step, solid-liquid separation step, and drying step to obtain dried toner particles. In the washing step, from the viewpoint of chargeability, it is preferable to carry out sufficient substitution washing with ion-exchanged water. In the solid-liquid separation step, it is preferable to carry out suction filtration, pressure filtration, etc., from the viewpoint of productivity. In the drying step, it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc., from the viewpoint of productivity.

[0080] [Step of adding external additives] The method for producing the toner according to the present embodiment preferably includes a step of externally adding an external additive to the toner particles. The external additive is added to the toner particles by mixing the toner particles in a dry state with the external additive. The mixing is performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.

[0081] The external additive may be, for example, inorganic particles. Examples of inorganic particles include SiO 2 , TiO 2 , Al 2 O 3 , CuO, ZnO, SnO 2 , CEO 2 , Fe 2 O 3 , MgO, BaO, CaO, K 2 O, Na 2 O, ZrO 2 , CaO SiO 2 , K 2 O (TiO 2 ) n , Al 2 O 3 2SiO 2 , CaCO 3 , MgCO 3 , BaSO 4 , MgSO 4 etc.

[0082] The surface of the inorganic particles as an external additive may be subjected to hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobic treatment agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.

[0083] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate, and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.

[0084] The amount of the external additive is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the mass of the toner particles.

[0085] <Toner> The toner produced by the production method according to the present embodiment is preferably an externally added toner in which an external additive is added to toner particles. The form of the external additive is as described above.

[0086] The toner produced by the production method according to the present embodiment may be a toner having a single layer structure, or may be a toner having a core-shell structure having a core and a coating layer (shell layer) that coats the core. The toner having a core-shell structure has, for example, a core containing a binder resin, a release agent, and a colorant, and a coating layer containing a binder resin.

[0087] The content of the binder resin is preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total mass of the toner particles.

[0088] The content of the release agent is preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total mass of the toner.

[0089] When the toner contains a colorant, the content of the colorant is preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner.

[0090] The volume average particle diameter of the toner is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm. The method for measuring the volume average particle diameter of the toner is as follows. The particle size distribution of the toner is measured using a Coulter Multisizer II (manufactured by Beckman Coulter) and an electrolyte ISOTON-II (manufactured by Beckman Coulter). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% by mass aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant. This is added to 100 ml to 150 ml of electrolyte. The electrolyte in which the sample is suspended is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture of 100 μm diameter. The number of particles sampled is 50,000. The particle size distribution is plotted from the small diameter side, and the particle size at which the cumulative 50% is reached is taken as the volume average particle size D50v.

[0091] The average circularity of the toner is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less. The average circularity of the toner is calculated by dividing the perimeter of a circle having the same area as the projected image of a particle by the perimeter of the projected image of a particle. It is determined by sampling 3,500 particles using a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation).

[0092] <Developer> The toner produced by the production method according to the present embodiment may be used as a one-component developer, or may be mixed with a carrier and used as a two-component developer.

[0093] The carrier is not particularly limited, and may be any known carrier. Examples of the carrier include a coated carrier in which the surface of a core material made of magnetic powder is coated with a resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, and a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier or the resin-impregnated type carrier may be a carrier in which the constituent particles of the carrier serve as a core material, and the surface of the core material is coated with a resin.

[0094] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt; magnetic oxides such as ferrite and magnetite; and the like.

[0095] Examples of the resin and matrix resin for coating include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin or its modified product containing organosiloxane bonds, fluororesin, polyester, polycarbonate, phenolic resin, epoxy resin, etc. The resin and matrix resin for coating may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, potassium titanate, etc.

[0096] To coat the surface of the core material with a resin, a method of coating with a coating layer forming solution in which the coating resin and various additives (used as necessary) are dissolved in a suitable solvent can be mentioned. The solvent is not particularly limited and may be selected taking into consideration the type of resin used, suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer; a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material; a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air; and a kneader coater method in which the carrier core material and the solution for forming a coating layer are mixed in a kneader coater and then the solvent is removed.

[0097] The mixture ratio (mass ratio) of the toner and the carrier in the two-component developer is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100. EXAMPLES

[0098] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are by mass. Synthesis, processing, preparation, etc. were carried out at room temperature (25°C ± 3°C) unless otherwise noted.

[0099] <Preparation of particle dispersion> [Preparation of amorphous polyester resin particle dispersion (A)] Terephthalic acid: 690 parts Fumaric acid: 310 parts Ethylene glycol: 400 parts 1,5-Pentanediol: 450 parts The above materials were placed in a reaction tank equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under nitrogen gas flow, and 10 parts of titanium tetraethoxide was added for a total of 1000 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (A) with a weight average molecular weight of 96000 and a glass transition temperature of 59°C was obtained.

[0100] In a tank equipped with a temperature control means and a nitrogen substitution means, 550 parts of ethyl acetate and 250 parts of 2-butanol were added to prepare a mixed solvent, and then 1000 parts of amorphous polyester resin (A) were gradually added and dissolved, and a 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the reaction vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 4000 parts of ion-exchanged water was dropped into the mixed liquid while stirring, to perform emulsification. After the dropwise addition, the emulsion was returned to 25°C, and the solvent was removed under reduced pressure to obtain a resin particle dispersion in which resin particles with a volume average particle size of 160 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (A) was obtained.

[0101] [Preparation of amorphous polyester resin particle dispersion (B)] Terephthalic acid: 690 parts Trimellitic acid: 310 parts Ethylene glycol: 400 parts 1,5-Pentanediol: 450 parts The above materials were placed in a reaction tank equipped with a stirrer, nitrogen inlet tube, temperature sensor, and distillation column, and the temperature was raised to 220°C over 1 hour under nitrogen gas flow, and 10 parts of titanium tetraethoxide was added for a total of 1000 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (B) with a weight average molecular weight of 127000 and a glass transition temperature of 59°C was obtained.

[0102] A resin particle dispersion in which resin particles having a volume average particle size of 160 nm were dispersed was obtained in the same manner as in the case of the amorphous polyester resin dispersion (A), except that 1000 parts of the amorphous polyester resin (A) was replaced with 1000 parts of the amorphous polyester resin (B). Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, thereby obtaining an amorphous polyester resin particle dispersion (B).

[0103] [Preparation of crystalline polyester resin particle dispersion (C)] 1,10-Decanedicarboxylic acid: 2600 parts 1,6-Hexanediol: 1670 parts Dibutyltin oxide (catalyst): 3 parts The above materials were placed in a heated and dried reactor, the air in the reactor was replaced with nitrogen gas to create an inert atmosphere, and the mixture was stirred and refluxed at 180°C for 5 hours using mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and the mixture was stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Thus, a crystalline polyester resin with a weight average molecular weight of 12600 and a melting temperature of 73°C was obtained. 900 parts of crystalline polyester resin, 18 parts of anionic surfactant (TaycaPower, manufactured by Tayca Corporation) and 2100 parts of ion-exchanged water were mixed, heated to 120°C, dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA Corporation), and then dispersed for 1 hour using a pressure discharge type Gaulin homogenizer to obtain a resin particle dispersion in which resin particles with a volume average particle size of 160 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a crystalline polyester resin particle dispersion (C) was obtained.

[0104] [Preparation of styrene acrylic resin particle dispersion (S)] Styrene: 3,750 parts n-Butyl acrylate: 250 parts Acrylic acid: 20 parts Dodecanethiol: 240 parts Carbon tetrabromide: 40 parts A surfactant aqueous solution was prepared by dissolving 60 parts of a nonionic surfactant (Sanyo Chemical Industries, Nonipol 400) and 100 parts of an anionic surfactant (TaycaPower, Tayca Co., Ltd.) in 5500 parts of ion-exchanged water. The mixture obtained by mixing and dissolving the above-mentioned polymerization materials was dispersed and emulsified in the surfactant aqueous solution. Next, an aqueous solution obtained by dissolving 40 parts of ammonium persulfate in 500 parts of ion-exchanged water was added to the reaction vessel over a period of 20 minutes while stirring the inside of the reaction vessel. Next, after nitrogen replacement, the reaction vessel was heated in an oil bath while stirring the inside of the reaction vessel until the contents reached 70°C, and the temperature was maintained at 70°C for 5 hours to continue emulsion polymerization. In this way, a resin particle dispersion in which resin particles having a volume average particle size of 160 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a styrene acrylic resin particle dispersion (S) was obtained.

[0105] [Preparation of release agent particle dispersion (W)] Paraffin wax (manufactured by Nippon Seiro Co., Ltd., FNP92, melting temperature 92°C): 1,000 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 10 parts Ion-exchanged water: 3,500 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 220 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W).

[0106] [Preparation of colorant particle dispersion (C)] Cyan pigment (Pigment Blue 15:3, Dainichi Seika Chemicals): 500 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 50 parts Ion-exchanged water: 1930 parts The above materials were mixed and dispersed for 10 minutes at 240 MPa using an Ultimizer (manufactured by Sugino Machine Co., Ltd.) to obtain a colorant particle dispersion (C) with a solid content of 20%.

[0107] <Example 1> [Preparation of circulating reactor] A jacketed stirring tank was prepared. The bottom of the stirring tank was connected to a disperser (Cavitron CD1010, manufactured by Pacific Machinery Co., Ltd.) via a conduit and a circulation pump, and the conduit from the disperser's outlet was immersed in the tank from above to create a circulation type reaction tank. A material inlet was provided in the conduit connecting the bottom of the stirring tank and the disperser.

[0108] [Flocculant mixing process] Ion-exchanged water: 3,500 parts Amorphous polyester resin particle dispersion (A): 2630 parts Amorphous polyester resin particle dispersion (B): 2630 parts Crystalline polyester resin particle dispersion (C): 1,500 parts Styrene acrylic resin particle dispersion (S): 750 parts Release agent particle dispersion (W): 1,500 parts Colorant particle dispersion (C): 1,500 parts The above materials were placed in a circulating reactor and the pH was adjusted to 3.8 by adding 0.1N nitric acid. An aqueous solution of aluminum sulfate was prepared by dissolving 25 parts of aluminum sulfate in 1500 parts of ion-exchanged water. While the contents were circulated in the circulating reaction tank for stirring and dispersion, an aqueous aluminum sulfate solution was added from the inlet. The contents were then circulated for 10 minutes while maintaining the temperature at 30° C., for stirring and dispersion. The peripheral speed of the rotor tip of the dispersing machine equipped in the circulating reaction tank is shown in Table 1. Table 1 also shows the viscosity of the dispersion measured by taking a sample at the middle point during the 10-minute circulation, and the viscosity of the dispersion measured by taking a sample at the end of the 10-minute circulation (referred to as "viscosity A").

[0109] [Agglutination process] The disperser was stopped, the bottom valve at the bottom of the stirring tank was closed, and 1500 parts of ion-exchanged water was charged from the inlet, and then charged into the stirring tank through the disperser and the conduit, and mixed into the dispersion. The viscosity of the dispersion (referred to as "viscosity B") measured by taking a sample after stirring and mixing 1500 parts of ion-exchanged water is shown in Table 1. Next, the contents were heated to 45° C. in the jacket while continuing to stir, and maintained at that temperature until the volume average particle size of the aggregated particles reached 4.0 μm.

[0110] [Second flocculation step] A mixture of 2250 parts of the amorphous polyester resin particle dispersion (A) and 2250 parts of the amorphous polyester resin particle dispersion (B) was added to the dispersion containing the aggregated particles, and the mixture was held for 30 minutes to form second aggregated particles. Then, the pH was adjusted to 9.0 using a 1N aqueous sodium hydroxide solution.

[0111] [Uniting process] While continuing stirring in the stirring tank, the mixture was heated to 85°C at a heating rate of 0.5°C / min, held at 85°C for 3 hours, and then cooled to 30°C at 15°C / min (first cooling). Next, the mixture was heated to 55°C at a heating rate of 0.2°C / min (reheating), held for 30 minutes, and then cooled to 30°C at 15°C / min (second cooling). Next, the solid content was filtered, washed with ion-exchanged water, and dried to obtain toner particles (1) having a volume average particle size of 5.0 μm.

[0112] [Addition of external additives] 100 parts of toner particles (1) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with an opening of 45 μm to obtain toner (1). The volume average particle diameter of toner (1) was 5.0 μm.

[0113] [Creating the carrier] After 500 parts of spherical magnetite powder particles (volume average particle diameter 0.55 μm) were stirred with a Henschel mixer, 5 parts of a titanate-based coupling agent were added, and the mixture was heated to 100 ° C and stirred for 30 minutes. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of magnetite particles treated with a titanate-based coupling agent, 6.25 parts of 25% ammonia water, and 425 parts of water were added to a four-neck flask and stirred, and reacted at 85 ° C for 120 minutes while stirring. Next, the mixture was cooled to 25 ° C, 500 parts of water were added, and the supernatant liquid was removed and the precipitate was washed with water. The washed precipitate was heated and dried under reduced pressure to obtain a carrier (CA) with an average particle size of 35 μm.

[0114] [Preparation of developer] The toner (1) and the carrier (CA) were placed in a V blender in a ratio of toner (1):carrier (CA)=5:95 (mass ratio) and stirred for 20 minutes to obtain a developer (1).

[0115] <Examples 2 to 7 and Comparative Examples 1 to 2> Toner particles were obtained in the same manner as in Example 1, except that the production conditions of the toner particles were changed to the specifications shown in Table 1. Next, in the same manner as in Example 1, external additives were added to the toner particles, and the toner particles were mixed with a carrier to obtain a developer.

[0116] <Performance evaluation> [Amount of coarse particles, amount of fine particles] 2 ml of a 5% aqueous solution of a surfactant (sodium dodecylbenzenesulfonate) and 0.5 mg of toner were added to 100 ml of ISOTON-II (manufactured by Beckman Coulter), and the mixture was dispersed for about 3 minutes using an ultrasonic disperser to prepare a measurement sample. The particle size of the measurement sample was measured using a Coulter Multisizer II (manufactured by Beckman Coulter) with an aperture diameter of 100 μm. Particles with a particle size of 10.5 μm or more were defined as coarse particles, and their volume percentage was calculated and classified as follows: Particles with a particle size of 2.5 μm or less were defined as fine particles, and the percentage of these particles was calculated and classified as follows:

[0117] - Coarse particles - A: Coarse particles are less than 0.5% by volume B: Coarse particles are 0.5% by volume or more and less than 2.5% by volume C: Coarse particles are 2.5% or more by volume

[0118] -Small particles- A: Microparticles are less than 3.0% by number B: Fine particles are 3.0% or more and less than 8.0% by number C: Microparticles are 8.0% or more by number

[0119] [White space] The developer was placed in a developing device of a modified image forming apparatus ApeosPortIV C5575 manufactured by Fuji Xerox Co., Ltd. After leaving this image forming apparatus for one day in an environment of a temperature of 25°C and a relative humidity of 15%, 100 sheets of halftone images with an image density of 5% were outputted on the entire surface of P paper manufactured by Fuji Xerox Co., Ltd. Next, one sheet of an image with an image density of 100% was outputted on the entire surface of P paper manufactured by Fuji Xerox Co., Ltd., and the presence or absence of dot-like image defects (so-called white spots) was confirmed.

[0120] A: No white spots are observed visually or with a magnifying glass. B: No white spots were observed with the naked eye, but slight white spots were observed with a magnifying glass. C: White spots were visually observed.

[0121] [Table 1] [Explanation of symbols]

[0122] 100 Circulating Reactor 10 Stirring tank 20 Baffle 40 Paddle wing 60 Rotational Axis 82,84 tube 86 Inlet 90 Dispersing machine

Claims

1. a flocculant mixing step of adding a flocculant to the dispersion containing binder resin particles while circulating the dispersion containing binder resin particles between a stirring tank and a disperser that applies a mechanical shear force, and mixing the flocculant into the dispersion containing binder resin particles; an aggregation step of reducing the viscosity of the dispersion liquid that has been subjected to the aggregating agent mixing step and then heating the dispersion liquid to form aggregated particles; a coalescence step of heating the dispersion liquid containing the aggregated particles to fuse and coalesce the aggregated particles to form toner particles; A method for producing a toner for developing an electrostatic image comprising the steps of:

2. 2. The method for producing a toner for developing an electrostatic image according to claim 1, wherein in the aggregating step, the viscosity of the dispersion liquid having been subjected to the aggregating agent mixing step is reduced by a degree of more than 5 Pa.s and less than 50 Pa.s. The viscosity of the dispersion is measured at a shear rate of 1 / s using a part of the dispersion as a sample at a sample temperature of 25°C.

3. The viscosity of the dispersion in the flocculant mixing step is 25 Pa·s or more and 85 Pa·s or less, 3. The method for producing a toner for developing electrostatic images according to claim 1, wherein the peripheral speed of a rotor tip of the dispersing machine for applying the mechanical shearing force is 30 m / sec or more and 50 m / sec or less. The viscosity of the dispersion is measured at a shear rate of 1 / s using a part of the dispersion as a sample at a sample temperature of 25°C.

4. 4. The method for producing a toner for developing an electrostatic image according to claim 1, wherein the aggregating step includes adding water to the dispersion liquid that has been subjected to the aggregating agent mixing step.

5. The method for producing a toner for developing an electrostatic image according to any one of claims 1 to 4, wherein the coagulant contains a trivalent metal salt compound.

6. 6. The method for producing a toner for developing an electrostatic image according to claim 1, wherein the dispersion liquid containing the binder resin particles contains, as the binder resin particles, amorphous polyester resin particles and crystalline polyester resin particles.

7. 7. The method for producing a toner for developing an electrostatic image according to claim 1, wherein the dispersion liquid containing the binder resin particles further contains releasing agent particles.

8. The method for producing a toner for developing an electrostatic image according to any one of claims 1 to 7, wherein the dispersion liquid containing the binder resin particles further contains colorant particles.

9. the method further includes a second aggregation step of mixing a dispersion containing the aggregated particles with a dispersion containing resin particles that will become a shell layer, and aggregating the resin particles that will become the shell layer on the surfaces of the aggregated particles to form second aggregated particles, the coalescence step is a step of heating a dispersion liquid containing the second aggregated particles to fuse and coalesce the second aggregated particles to form toner particles; The method for producing the toner for developing electrostatic images according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for manufacturing toner for electrostatic charge image development

    JP2004093586A

  • Magenta toner for electrostatic image development, developer for electrostatic image development, method for manufacturing toner and image forming method

    JP2006065107A

  • Toner for electrostatic charge development, developer for electrostatic charge development, image forming apparatus, and manufacturing device for toner for electrostatic charge development

    JP2008225120A

  • Device for manufacturing electrophotographic toner and method for manufacturing electrophotographic toner

    JP2014048364A

  • Manufacturing method of toner by emulsion agglomeration method

    JP2019008042A