Method for producing toner for developing electrostatic images
The method addresses the issue of toner contamination by controlling stirring power and pH during aggregation and coalescence, resulting in reduced minute and coarse toner particles for improved toner production.
Patent Information
- Application Number
- JP2021046474
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-03-19
AI Technical Summary
Existing methods for producing toner for developing electrostatic images result in excessive contamination with minute and coarse toner particles due to inconsistent stirring power and pH levels during the aggregation process.
A method involving controlled aggregation and coalescence steps, including the use of alkaline solutions to adjust pH and stepwise reduction of stirring power, to form toner particles with reduced minute and coarse toner contamination.
The method effectively reduces the amount of minute and coarse toner particles, improving the quality and consistency of the toner production process.
Smart Images

Figure 0007589607000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a toner for developing electrostatic images, a toner for developing electrostatic images, and an electrostatic image developer. [Background technology]
[0002] Patent Document 1 discloses a method for producing a toner for electrophotography, which includes a step of adding a predetermined amount of aggregating agent to a dispersion of resin particles to obtain a dispersion containing resin particles and the aggregating agent, a step of aggregating resin particles in the dispersion containing the resin particles and the aggregating agent to obtain a dispersion containing aggregated particles, and a step of coalescing the aggregated particles. Patent Document 2 discloses a method for producing a toner, which includes: a mixing step of mixing an aqueous dispersion of resin particles containing a resin having an acidic polar group with an aqueous dispersion of colorant particles containing a colorant to obtain a mixed dispersion containing resin particles and colorant particles; an aggregation step of adding an aggregating agent containing a divalent or higher metal ion to the mixed dispersion to aggregate the resin particles and the colorant particles to form aggregated particles; and a fusing step of adding a chelating agent to the dispersion of aggregated particles obtained in the aggregation step, then adding a monovalent water-soluble metal salt, and heating the mixture to a temperature equal to or higher than the glass transition point of the resin to fuse the resin particles and the colorant particles in the aggregated particles. Patent Document 3 discloses a method for producing agglomerated particles, which includes the steps of mixing and stirring an aqueous dispersion of resin particles with an aggregating agent to cause the agglomerated particles to grow until the volume median particle diameter reaches a target value, and increasing the stirring power per unit mass when the volume median particle diameter of the agglomerated particles reaches the target value. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-102855 A [Patent Document 2] JP 2013-109341 A [Patent Document 3] JP 2019-111462 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a method for producing a toner for developing electrostatic images, which reduces the inclusion of fine toner particles in the aggregation stopping step, as compared to a case in which the stirring power required per unit volume is constant. [Means for solving the problem]
[0005] Means for solving the above problems include the following aspects. <1> an aggregation step of aggregating the binder resin particles in a dispersion liquid containing the binder resin particles to form aggregated particles; an aggregation stopping step of adding an alkaline aqueous solution to the dispersion liquid containing the aggregated particles to increase the pH of the dispersion liquid containing the aggregated particles and stop the growth of the aggregated particles; a coalescence step of heating the dispersion liquid containing the aggregated particles to fuse and coalesce the aggregated particles to form toner particles, the aggregation stopping step includes gradually or continuously reducing a stirring power required per unit volume while stirring the dispersion liquid containing the aggregated particles. A method for producing a toner for developing electrostatic images. <2> In the aggregation stopping step, the stirring power required per unit volume is 0.1 kW / m 3 Not less than <1> 2. A method for producing the toner for developing electrostatic images according to claim 1 . <3> In the aggregation stopping step, the required stirring power per unit volume is 3.5 kW / m 3 Not exceeding <1> or <2> 2. A method for producing the toner for developing electrostatic images according to claim 1 . <4> the pH of the dispersion liquid containing the aggregated particles does not exceed 9 in the aggregation stopping step; <1> ~ <3> 13. The method for producing the toner for developing electrostatic images according to claim 12. <5> The aggregation stopping step comprises: gradually increasing the pH of the dispersion liquid containing the aggregated particles by gradually adding the alkaline aqueous solution; and gradually decreasing the stirring power required per unit volume in accordance with the gradually increasing pH of the dispersion liquid containing the aggregated particles. <1> ~ <4> 13. The method for producing the toner for developing electrostatic images according to claim 12. <6> The alkaline aqueous solution contains at least one selected from the group consisting of an aqueous solution of an alkali metal hydroxide, an aqueous solution of an alkaline earth metal hydroxide, and an aqueous solution of a chelating agent that chelates the coagulant, <1> ~ <5> 13. The method for producing the toner for developing electrostatic images according to claim 12. <7> the dispersion liquid containing the binder resin particles further contains release agent particles, the aggregating step is a step of aggregating the release agent particles to form the aggregated particles; <1> ~ <6> 13. The method for producing the toner for developing electrostatic images according to claim 12. <8> the dispersion liquid containing the binder resin particles further contains colorant particles, the aggregating step is a step of aggregating the colorant particles to form the aggregated particles, <1> ~ <7> 13. The method for producing the toner for developing electrostatic images according to claim 12. <9> a second aggregation step, which is performed before the aggregation termination step, of mixing a dispersion liquid containing the aggregated particles with a dispersion liquid containing resin particles that will become a shell layer, and aggregating the resin particles that will become the shell layer on the surfaces of the aggregated particles to form second aggregated particles; the aggregation terminating step is a step of adding an alkaline aqueous solution to the dispersion liquid containing the second aggregated particles to increase the pH of the dispersion liquid containing the second aggregated particles and thereby terminating the growth of the second aggregated particles, the coalescence step is a step of heating a dispersion liquid containing the second aggregated particles to fuse and coalesce the second aggregated particles to form toner particles, the aggregation stopping step includes stepwise or continuously reducing a stirring power required per unit volume while stirring the dispersion liquid containing the second aggregated particles. <1> ~ <8> 13. The method for producing the toner for developing electrostatic images according to claim 12. <10> <1> ~ <9> 13. A toner for developing electrostatic images, produced by the method for producing a toner for developing electrostatic images according to any one of claims 1 to 12. <11> <1> ~ <9> 2. An electrostatic image developer comprising a toner for developing electrostatic images produced by the method for producing a toner for developing electrostatic images according to any one of claims 1 to 11. Effect of the Invention
[0006] <1> , <5> , <6> , <7> , <8> and <9> According to the present invention, there is provided a method for producing a toner for developing an electrostatic image, which reduces the inclusion of fine toner particles in the aggregation stopping step, as compared with a case in which the stirring power required per unit volume is constant. <2> According to the invention, the required stirring power per unit volume in the aggregation stopping step is 0.1 kW / m 3 The present invention provides a method for producing a toner for developing electrostatic images, which reduces the inclusion of coarse toner particles compared to when the toner particle size is less than 100%. <3> According to the invention, the required stirring power per unit volume in the aggregation stopping step is 3.5 kW / m 3 The present invention provides a method for producing a toner for developing electrostatic images, which reduces the inclusion of fine toner particles as compared with the case where the toner particles exceed the above range. <4> According to the present invention, there is provided a method for producing a toner for developing electrostatic images, which reduces the inclusion of fine toner particles as compared with a case where the pH of the dispersion liquid containing the aggregated particles exceeds 9 in the aggregation stopping step. <10> According to the present invention, there is provided a toner for developing electrostatic images in which the amount of fine toner particles mixed in is reduced. <11> According to the present invention, there is provided an electrostatic image developer in which the amount of fine toner particles mixed in is reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, embodiments of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiments, and are not intended to limit the scope of the embodiments.
[0008] In the present disclosure, a numerical range indicated using "~" indicates a range that includes the numerical values before and after "~" as the minimum and maximum values, respectively.
[0009] In the numerical ranges described in the present disclosure in stages, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.
[0010] In the present disclosure, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved.
[0011] In the present disclosure, each component may contain multiple types of corresponding substances. When referring to the amount of each component in a composition in the present disclosure, if multiple substances corresponding to each component are present in the composition, the total amount of the multiple substances present in the composition is meant unless otherwise specified.
[0012] In the present disclosure, the particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component are present in the composition, the particle size of each component means the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.
[0013] In the present disclosure, "(meth)acrylic" means at least one of acrylic and methacrylic, and "(meth)acrylate" means at least one of acrylate and methacrylate.
[0014] In this disclosure, "toner" refers to "toner for developing electrostatic images", "developer" refers to "electrostatic image developer", and "carrier" refers to "carrier for developing electrostatic images".
[0015] In the present disclosure, a method for producing toner particles by aggregating and coalescing material particles in a solvent is referred to as an EA (emulsion aggregation) method.
[0016] <Method of manufacturing toner for developing electrostatic images> The toner production method according to the present embodiment is a toner production method including producing toner particles by the EA method, and includes the following aggregation step, aggregation termination step, and coalescence step.
[0017] Aggregation step: a step of aggregating binder resin particles in a dispersion liquid containing the binder resin particles to form aggregated particles. Aggregation stopping step: A step of adding an alkaline aqueous solution to the dispersion liquid containing the aggregated particles to increase the pH of the dispersion liquid containing the aggregated particles and stop the growth of the aggregated particles. Coalescence process: A process in which the dispersion liquid containing the aggregated particles is heated to fuse and coalesce the aggregated particles to form toner particles.
[0018] In the toner manufacturing method according to the present embodiment, the aggregation stopping step includes gradually or continuously lowering the stirring power required per unit volume while stirring the dispersion liquid containing the aggregated particles. By gradually or continuously lowering the stirring power required per unit volume, the inclusion of fine toner particles is reduced. The following mechanism is assumed to be the mechanism.
[0019] When an alkaline aqueous solution is added to a dispersion containing aggregated particles to increase the pH of the dispersion containing aggregated particles, the aggregation force of the aggregated particles tends to decrease. In this case, if the shear force acting on the aggregated particles due to stirring is too strong, the aggregated particles may split, resulting in the production of fine toner particles. Even if an alkaline aqueous solution is added to a dispersion containing aggregated particles, the splitting of the aggregated particles can be suppressed by reducing the stirring power required per unit volume, and as a result, the production of fine toner particles can be suppressed.
[0020] In the aggregation termination step, the number of stages in which the stirring power required per unit volume is gradually reduced may be any of 1, 2, 3, 4 or 5 stages, and is preferably 2, 3 or 4 stages.
[0021] The required stirring power per unit volume in the aggregation stopping step is set to 0.1 kW / m from the viewpoint of suppressing the aggregation of aggregated particles and suppressing the generation of coarse toner particles. 3 It is preferable that the power consumption does not fall below 0.14kW / m 3 It is more preferable that the value does not fall below 0.18kW / m 3 It is more preferable that the temperature is not lower than 100° C.
[0022] The required stirring power per unit volume in the aggregation stopping step is 3.5 kW / m from the viewpoint of suppressing the division of aggregated particles and suppressing the generation of fine toner particles. 3 It is preferable that the power consumption does not exceed 3.4kW / m 3 It is more preferable that it does not exceed 3.3 kW / m 3 It is more preferable that the concentration does not exceed 100%.
[0023] Mixing power required per unit volume (kW / m 3 ) is preferably controlled by varying the rotation speed of the stirring means depending on the viscosity of the dispersion containing the aggregated particles and the dimensions of the stirring means.
[0024] The steps and materials of the method for producing the toner according to this embodiment will be described in detail below.
[0025] [Aggregation step (first aggregation step)] The aggregation step is a step of aggregating at least the binder resin particles in a dispersion liquid containing at least the binder resin particles to form aggregated particles.
[0026] The dispersion liquid to be subjected to the aggregation step may also contain at least one of release agent particles and colorant particles. Therefore, the aggregation step may be a step of aggregating at least one of the release agent particles and colorant particles together with the binder resin particles.
[0027] When the toner manufacturing method according to the present embodiment includes a second aggregation step (a step for forming a shell layer) described later, the above aggregation step is referred to as a "first aggregation step." The first aggregation step is a step for forming a core in a toner having a core-shell structure.
[0028] The dispersion liquid to be subjected to the aggregation step is prepared, for example, by preparing a resin particle dispersion liquid containing binder resin particles, a release agent particle dispersion liquid containing release agent particles, and a colorant particle dispersion liquid containing colorant particles, and mixing these particle dispersion liquids. The order in which these particle dispersion liquids are mixed is not limited.
[0029] Hereinafter, the resin particle dispersion, the release agent particle dispersion, and the colorant particle dispersion will be collectively referred to as "particle dispersion" to describe what they have in common.
[0030] An example of an embodiment of a particle dispersion liquid is a dispersion liquid in which a material is dispersed in the form of particles in a dispersion medium by a surfactant.
[0031] The dispersion medium of the particle dispersion liquid is preferably an aqueous medium. Examples of the aqueous medium include water and alcohol. The water is preferably water with a reduced ion content, such as distilled water or ion-exchanged water. These aqueous media may be used alone or in combination of two or more.
[0032] The surfactant for dispersing the material in the dispersion medium may be any of anionic surfactants, cationic surfactants, and nonionic surfactants. Examples of such surfactants include anionic surfactants such as sulfate ester salts, sulfonate salts, phosphate esters, and soaps; cationic surfactants such as amine salts and quaternary ammonium salts; and nonionic surfactants such as polyethylene glycols, alkylphenol ethylene oxide adducts, and polyhydric alcohols. The surfactants may be used alone or in combination of two or more. The nonionic surfactants may be used in combination with an anionic surfactant or a cationic surfactant.
[0033] Methods for dispersing a material in a particulate form in a dispersion medium include known dispersion methods using a rotary shear type homogenizer, a ball mill having media, a sand mill, a dyno mill, and the like.
[0034] The phase inversion emulsification method is a method for dispersing a resin in a dispersion medium in the form of particles. The phase inversion emulsification method involves dissolving the resin in a hydrophobic organic solvent in which the resin is soluble, adding a base to the organic continuous phase (O phase) to neutralize it, and then introducing an aqueous medium (W phase) to invert the phase from W / O to O / W, dispersing the resin in the form of particles in the aqueous medium.
[0035] The volume average particle size of the particles dispersed in the particle dispersion is preferably 30 nm or more and 300 nm or less, more preferably 50 nm or more and 250 nm or less, and even more preferably 80 nm or more and 200 nm or less. The volume average particle size of particles in a particle dispersion refers to the particle size that is 50% cumulative from the smallest diameter side in a particle size distribution measured with a laser diffraction particle size distribution measuring device (for example, LA-700 manufactured by Horiba, Ltd.).
[0036] The content of particles contained in the particle dispersion is preferably from 5% by mass to 50% by mass, more preferably from 10% by mass to 40% by mass, and even more preferably from 15% by mass to 30% by mass.
[0037] -Binding resin- Examples of the binder resin include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), (meth)acrylic acid esters (e.g., methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, 2-ethylhexyl methacrylate, etc.), ethylenically unsaturated nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), vinyl ethers (e.g., vinyl methyl ether, vinyl isobutyl ether, etc.), vinyl ketones (e.g., vinyl methyl ketone, vinyl ethyl ketone, vinyl isopropenyl ketone, etc.), and olefins (e.g., ethylene, propylene, butadiene, etc.), or copolymers of two or more of these monomers. Examples of the binder resin include non-vinyl resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin, mixtures of these with the vinyl resins, and graft polymers obtained by polymerizing vinyl monomers in the coexistence of these. These binder resins may be used alone or in combination of two or more kinds.
[0038] The binder resin is preferably a polyester resin, for example, an amorphous polyester resin or a crystalline polyester resin.
[0039] In the present embodiment, the "crystalline" of the polyester resin refers to a state in which, in differential scanning calorimetry (DSC), the resin has a clear endothermic peak rather than a stepwise change in endothermic amount, and specifically refers to a state in which the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10°C / min. In the present embodiment, the "amorphous" polyester resin refers to a half-width exceeding 10° C., a stepwise change in endothermic heat amount being exhibited, or no clear endothermic peak being observed.
[0040] -Amorphous polyester resin- The amorphous polyester resin may be a commercially available product or a synthetic product. The amorphous polyester resin may be, for example, a condensation polymer of a polycarboxylic acid and a polyhydric alcohol.
[0041] Examples of polyvalent carboxylic acids that are polymerization components of amorphous polyester resins include aliphatic dicarboxylic acids (e.g., oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, sebacic acid, etc.), alicyclic dicarboxylic acids (e.g., cyclohexanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., carbon number 1 to 5). Among these, aromatic dicarboxylic acids are preferable as polyvalent carboxylic acids. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower (e.g., carbon number 1 to 5) alkyl esters thereof. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0042] Examples of polyhydric alcohols that are polymerization components of amorphous polyester resins include aliphatic diols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, etc.), alicyclic diols (e.g., cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc.), and aromatic diols (e.g., ethylene oxide adducts of bisphenol A, propylene oxide adducts of bisphenol A, etc.). Among these, examples of polyhydric alcohols include aromatic diols and alicyclic diols, and more preferably aromatic diols. As the polyhydric alcohol which is a polymerization component of the amorphous polyester resin, a polyhydric alcohol having a crosslinked structure or a branched structure of trihydric or more may be used in combination with the diol. Examples of the polyhydric alcohol having trihydric or more include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0043] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 50°C or higher and 80°C or lower, and more preferably 50°C or higher and 65°C or lower. The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC), and more specifically, is determined from the "extrapolated glass transition onset temperature" described in the method for determining glass transition temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0044] The weight average molecular weight (Mw) of the amorphous polyester resin is preferably 5,000 or more and 1,000,000 or less, and more preferably 7,000 or more and 500,000 or less. The number average molecular weight (Mn) of the amorphous polyester resin is preferably 2,000 or more and 100,000 or less. The molecular weight distribution Mw / Mn of the amorphous polyester resin is preferably 1.5 or more and 100 or less, and more preferably 2 or more and 60 or less. The weight average molecular weight and number average molecular weight are measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC is performed using a Tosoh GPC HLC-8120GPC as the measuring device, a Tosoh TSKgel SuperHM-M (15 cm) column, and THF solvent. The weight average molecular weight and number average molecular weight are calculated from the measurement results using a molecular weight calibration curve created with a monodisperse polystyrene standard sample.
[0045] The amorphous polyester resin can be obtained by a known production method, for example, by carrying out the reaction while removing water and alcohol generated during condensation by setting the polymerization temperature to 180° C. or higher and 230° C. or lower, and reducing the pressure in the reaction system as necessary. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a solubilizing agent to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent. If a monomer with poor compatibility is present in the copolymerization reaction, it is recommended that the monomer with poor compatibility is condensed in advance with the acid or alcohol to be polycondensed, and then polycondensed with the main component.
[0046] -Crystalline polyester resin- The crystalline polyester resin may be a commercially available product or a synthetic product. Examples of the crystalline polyester resin include polycondensates of polyvalent carboxylic acids and polyhydric alcohols. The crystalline polyester resin is preferably a polycondensate of a linear aliphatic polymerizable monomer rather than a polymerizable monomer having an aromatic ring, since it easily forms a crystal structure.
[0047] Examples of polyvalent carboxylic acids that are polymerization components of crystalline polyester resins include aliphatic dicarboxylic acids (e.g., oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid, etc.), aromatic dicarboxylic acids (e.g., dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, etc.), anhydrides thereof, and lower alkyl esters thereof (e.g., having 1 to 5 carbon atoms). The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids (e.g., 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, etc.), their anhydrides, and their lower alkyl esters (e.g., carbon number 1 to 5). As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0048] -Release agent- Examples of the release agent include hydrocarbon waxes, natural waxes such as carnauba wax, rice wax, and candelilla wax, synthetic or mineral / petroleum waxes such as montan wax, and ester waxes such as fatty acid esters and montan acid esters. The release agent is not limited to these.
[0049] The melting temperature of the release agent is preferably 50°C or higher and 110°C or lower, and more preferably 60°C or higher and 100°C or lower. The melting temperature of the release agent is determined from a DSC curve obtained by differential scanning calorimetry (DSC) in accordance with the "melting peak temperature" described in the method for determining the melting temperature in JIS K7121:1987 "Method for measuring transition temperature of plastics."
[0050] -Coloring agent- Examples of colorants include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, and Examples of the coloring agent include pigments such as rutramarine blue, chalco oil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate; dyes such as acridine, xanthene, azo, benzoquinone, azine, anthraquinone, thioindigo, dioxazine, thiazine, azomethine, indigo, phthalocyanine, aniline black, polymethine, triphenylmethane, diphenylmethane, and thiazole; etc. The coloring agent may be used alone or in combination of two or more.
[0051] The colorant may be surface-treated as necessary, and may be used in combination with a dispersant.
[0052] A dispersion liquid obtained by mixing a plurality of types of particle dispersion liquids is called a "mixed dispersion liquid."
[0053] After mixing the multiple types of particle dispersions, it is preferable to adjust the pH of the mixed dispersion to a range of 3 to 4. Examples of a means for adjusting the pH of the mixed dispersion include the addition of an acidic aqueous solution such as a nitric acid aqueous solution, a hydrochloric acid aqueous solution, or a sulfuric acid aqueous solution.
[0054] The mass ratio of the particles contained in the mixed dispersion is preferably in the following range. When the mixed dispersion contains release agent particles, the mass ratio of the binder resin particles to the release agent particles (binder resin particles:release agent particles) is preferably 100:3 to 100:30, more preferably 100:5 to 100:25, and even more preferably 100:8 to 100:20. When the mixed dispersion contains colorant particles, the mass ratio of the binder resin particles to the colorant particles (binder resin particles:colorant particles) is preferably 100:5 to 100:35, more preferably 100:7 to 100:30, and even more preferably 100:9 to 100:25.
[0055] The aggregation step may, for example, be adding a flocculant to the mixed dispersion while stirring the mixed dispersion; After adding the flocculant to the mixed dispersion, the mixed dispersion is heated while being stirred to increase the temperature of the mixed dispersion.
[0056] Examples of the flocculant include a surfactant having a polarity opposite to that of the surfactant contained in the mixed dispersion, an inorganic metal salt, and a divalent or higher metal complex. The flocculant may be used alone or in combination of two or more kinds.
[0057] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate; and inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.
[0058] The flocculant is preferably a divalent or higher metal salt compound, more preferably a trivalent metal salt compound, and even more preferably a trivalent inorganic aluminum salt compound, such as aluminum chloride, aluminum sulfate, polyaluminum chloride, and polyaluminum hydroxide.
[0059] The amount of the flocculant to be added is not limited. When a trivalent metal salt compound is used as the flocculant, the amount of the trivalent metal salt compound to be added is preferably 0.1 parts by mass or more and 2.5 parts by mass or less, more preferably 0.15 parts by mass or more and 2.0 parts by mass or less, and even more preferably 0.2 parts by mass or more and 1.5 parts by mass or less, relative to 100 parts by mass of the binder resin.
[0060] The temperature that the mixed dispersion reaches when it is heated is preferably a temperature based on the glass transition temperature (Tg) of the binder resin particles, for example, a temperature not lower than (Tg-30°C) and not higher than (Tg-10°C) of the binder resin particles. When the mixed dispersion contains a plurality of types of binder resin particles having different Tg's, the lowest temperature among the Tg's is set as the Tg in the aggregation step.
[0061] [Second flocculation step] The second aggregation step is a step for the purpose of producing a toner having a core-shell structure, and is a step performed after the first aggregation step. The second aggregation step is a step for forming a shell layer.
[0062] The second aggregation step is a step of mixing a dispersion liquid containing aggregated particles with a dispersion liquid containing resin particles that will form the shell layer, and aggregating the resin particles that will form the shell layer on the surfaces of the aggregated particles to form second aggregated particles.
[0063] As the dispersion liquid containing resin particles that will become the shell layer, at least one selected from binder resin particle dispersion liquids for forming the core is suitable, and a polyester resin particle dispersion liquid is more suitable.
[0064] The second aggregation step may, for example, adding a dispersion liquid containing resin particles to be a shell layer to the dispersion liquid containing the aggregated particles while stirring the dispersion liquid containing the aggregated particles; and heating, while stirring, the dispersion liquid containing the aggregated particles after adding the dispersion liquid containing the resin particles that will form the shell layer.
[0065] When the dispersion liquid containing the aggregated particles is heated, the temperature that the dispersion liquid containing the aggregated particles reaches is preferably a temperature based on the glass transition temperature (Tg) of the resin particles that form the shell layer, for example, a temperature that is equal to or higher than (Tg-30°C) and equal to or lower than (Tg-10°C) of the resin particles that form the shell layer.
[0066] [Agglomeration stop process] The aggregation stopping step is a step performed for the purpose of stopping the growth of the aggregated particles or the second aggregated particles after the aggregated particles or the second aggregated particles have grown to a predetermined size and before the heating in the coalescence step is performed. The form described below is common to the dispersion containing the aggregated particles and the dispersion containing the second aggregated particles.
[0067] The aggregation termination step is a step of increasing the pH of the dispersion liquid containing the aggregated particles by adding an alkaline aqueous solution to the dispersion liquid containing the aggregated particles.
[0068] The alkaline aqueous solution is preferably at least one selected from the group consisting of an aqueous solution of an alkali metal hydroxide, an aqueous solution of an alkaline earth metal hydroxide, and an aqueous solution of a chelating agent that chelates the flocculant.
[0069] Examples of the aqueous solution of an alkali metal hydroxide or an aqueous solution of an alkaline earth metal hydroxide include an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, an aqueous solution of calcium hydroxide, and an aqueous solution of barium hydroxide, and an aqueous solution of sodium hydroxide is preferred.
[0070] The chelating agent is a chemical substance that chelates the flocculant used in the flocculation step. Examples of the chelating agent include oxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid, and aminocarboxylic acids such as iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA).
[0071] In the aggregation stopping step, a chelating agent may be added to the dispersion liquid containing the aggregated particles in addition to the alkaline aqueous solution in order to stop the growth of the aggregated particles. The total amount of the chelating agent added is preferably from 0.01 to 5.0 parts by mass, and more preferably from 0.1 to less than 3.0 parts by mass, relative to 100 parts by mass of the binder resin particles.
[0072] In the aggregation stopping step, an alkaline aqueous solution is added to increase the pH of the dispersion containing the aggregated particles. From the viewpoint of maintaining the aggregation of the aggregated particles and suppressing division of the aggregated particles, it is preferable that the pH of the dispersion containing the aggregated particles does not exceed 9.
[0073] In the toner manufacturing method according to the present embodiment, the aggregation stopping step includes gradually or continuously lowering the stirring power required per unit volume while stirring the dispersion liquid containing the aggregated particles. When the stirring power required per unit volume is reduced stepwise, the number of steps may be any of 1, 2, 3, 4 or 5 steps, and is preferably 2, 3 or 4 steps.
[0074] In the coagulation stopping process, the required stirring power per unit volume is 0.1 kW / m from the viewpoint of not widening the particle size distribution of the coagulated particles. 3 More than 3.5kW / m 3 The range is preferably 0.14 kW / m 3 More than 3.4kW / m 3 More preferably, the range is 0.18 kW / m 3 More than 3.3kW / m 3 The following range is more preferable:
[0075] In the aggregation termination step, it is preferable to gradually lower the stirring power required per unit volume in accordance with the gradually increasing pH of the dispersion containing the aggregated particles. In other words, it is preferable to gradually increase the pH of the dispersion containing the aggregated particles by gradually adding the alkaline aqueous solution and gradually lower the stirring power required per unit volume in conjunction with each other. Specifically, it is preferable to add the alkaline aqueous solution and then lower the stirring power required per unit volume multiple times (e.g., 2, 3, 4, 5 times).
[0076] [Uniting process] The coalescence step is a step in which the dispersion liquid containing the aggregated particles is heated to fuse and coalesce the aggregated particles to form toner particles.
[0077] When the second aggregation step is performed before the coalescence step, the coalescence step is a step in which the dispersion liquid containing the second aggregated particles is heated to fuse and coalesce the second aggregated particles to form toner particles. By performing the second aggregation step and the coalescence step, toner particles having a core-shell structure can be produced.
[0078] The form described below is common to the aggregated particles and the second aggregated particles.
[0079] The temperature reached by the dispersion liquid containing the aggregated particles is preferably equal to or higher than the glass transition temperature (Tg) of the binder resin, and specifically, is preferably 10° C. to 30° C. higher than the Tg of the binder resin. When the aggregated particles contain a plurality of binder resins having different Tg's, the highest temperature among the Tg's is defined as the glass transition temperature in the coalescence step.
[0080] After the coalescence step, the toner particles in the dispersion are subjected to a known washing step, solid-liquid separation step, and drying step to obtain dried toner particles. In the washing step, from the viewpoint of chargeability, it is preferable to carry out sufficient substitution washing with ion-exchanged water. In the solid-liquid separation step, it is preferable to carry out suction filtration, pressure filtration, etc., from the viewpoint of productivity. In the drying step, it is preferable to carry out freeze drying, air flow drying, fluidized drying, vibration type fluidized drying, etc., from the viewpoint of productivity.
[0081] [Step of adding external additives] The method for producing the toner according to the present embodiment preferably includes a step of externally adding an external additive to the toner particles. The external additive is added to the toner particles by mixing the toner particles in a dry state with the external additive. The mixing is performed, for example, by using a V blender, a Henschel mixer, a Loedige mixer, etc. Furthermore, if necessary, coarse particles of the toner may be removed using a vibration sieve, an air sieve, etc.
[0082] The external additive may be, for example, inorganic particles. Examples of inorganic particles include SiO 2 , TiO 2 , Al 2 O 3 , CuO, ZnO, SnO2 , CEO 2 , Fe 2 O 3 , MgO, BaO, CaO, K 2 O, Na 2 O, ZrO 2 , CaO SiO 2 , K 2 O (TiO 2 ) n , Al 2 O 3 2SiO 2 , CaCO 3 , MgCO 3 , BaSO 4 , MgSO 4 etc.
[0083] The surface of the inorganic particles as an external additive may be subjected to hydrophobic treatment. The hydrophobic treatment may be performed, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, and examples thereof include silane coupling agents, silicone oils, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually, for example, 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the inorganic particles.
[0084] Examples of external additives include resin particles (resin particles such as polystyrene, polymethyl methacrylate, and melamine resin), cleaning agents (for example, metal salts of higher fatty acids such as zinc stearate, and fluorine-based polymer particles), and the like.
[0085] The amount of the external additive is preferably from 0.01% by mass to 5% by mass, and more preferably from 0.01% by mass to 2.0% by mass, based on the mass of the toner particles.
[0086] <Toner> The toner produced by the production method according to the present embodiment is preferably an externally added toner in which an external additive is added to toner particles. The form of the external additive is as described above.
[0087] The toner produced by the production method according to the present embodiment may be a toner having a single layer structure, or may be a toner having a core-shell structure having a core and a coating layer (shell layer) that coats the core. The toner having a core-shell structure has, for example, a core containing a binder resin, a release agent, and a colorant, and a coating layer containing a binder resin.
[0088] The content of the binder resin is preferably from 40% by mass to 95% by mass, more preferably from 50% by mass to 90% by mass, and even more preferably from 60% by mass to 85% by mass, based on the total mass of the toner particles.
[0089] The content of the release agent is preferably from 1% by mass to 20% by mass, and more preferably from 5% by mass to 15% by mass, based on the total mass of the toner.
[0090] When the toner contains a colorant, the content of the colorant is preferably from 1% by mass to 30% by mass, and more preferably from 3% by mass to 15% by mass, based on the total mass of the toner.
[0091] The volume average particle diameter of the toner is preferably from 2 μm to 10 μm, and more preferably from 4 μm to 8 μm. The method for measuring the volume average particle diameter of the toner is as follows. The particle size distribution of the toner is measured using a Coulter Multisizer II (manufactured by Beckman Coulter) and an electrolyte ISOTON-II (manufactured by Beckman Coulter). For the measurement, 0.5 mg to 50 mg of the measurement sample is added to 2 ml of a 5% by mass aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant. This is added to 100 ml to 150 ml of electrolyte. The electrolyte in which the sample is suspended is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with diameters in the range of 2 μm to 60 μm is measured using a Coulter Multisizer II with an aperture of 100 μm diameter. The number of particles sampled is 50,000. The particle size distribution is plotted from the small diameter side, and the particle size at which the cumulative 50% is reached is taken as the volume average particle size D50v.
[0092] The average circularity of the toner is preferably 0.94 or more and 1.00 or less, and more preferably 0.95 or more and 0.98 or less. The average circularity of the toner is calculated by dividing the perimeter of a circle having the same area as the projected image of a particle by the perimeter of the projected image of a particle. It is determined by sampling 3,500 particles using a flow-type particle image analyzer (FPIA-3000 manufactured by Sysmex Corporation).
[0093] <Developer> The toner produced by the production method according to the present embodiment may be used as a one-component developer, or may be mixed with a carrier and used as a two-component developer.
[0094] The carrier is not particularly limited, and may be any known carrier. Examples of the carrier include a coated carrier in which the surface of a core material made of magnetic powder is coated with a resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, and a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier or the resin-impregnated type carrier may be a carrier in which the constituent particles of the carrier serve as a core material, and the surface of the core material is coated with a resin.
[0095] Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt; magnetic oxides such as ferrite and magnetite; and the like.
[0096] Examples of the resin and matrix resin for coating include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid ester copolymer, straight silicone resin or its modified product containing organosiloxane bonds, fluororesin, polyester, polycarbonate, phenolic resin, epoxy resin, etc. The resin and matrix resin for coating may contain other additives such as conductive particles. Examples of the conductive particles include particles of metals such as gold, silver, copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, potassium titanate, etc.
[0097] To coat the surface of the core material with a resin, a method of coating with a coating layer forming solution in which the coating resin and various additives (used as necessary) are dissolved in a suitable solvent can be mentioned. The solvent is not particularly limited and may be selected taking into consideration the type of resin used, suitability for application, etc. Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer; a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material; a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air; and a kneader coater method in which the carrier core material and the solution for forming a coating layer are mixed in a kneader coater and then the solvent is removed.
[0098] The mixture ratio (mass ratio) of the toner and the carrier in the two-component developer is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100. EXAMPLES
[0099] Hereinafter, the embodiments of the present invention will be described in detail with reference to examples, but the embodiments of the present invention are not limited to these examples. In the following description, unless otherwise specified, "parts" and "%" are by mass. Synthesis, processing, preparation, etc. were carried out at room temperature (25°C ± 3°C) unless otherwise noted.
[0100] <Preparation of particle dispersion> [Preparation of amorphous polyester resin particle dispersion (A)] Terephthalic acid: 690 parts Fumaric acid: 310 parts Ethylene glycol: 400 parts 1,5-Pentanediol: 450 parts The above materials were placed in a reaction tank equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under nitrogen gas flow, and 10 parts of titanium tetraethoxide was added for a total of 1000 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (A) with a weight average molecular weight of 96000 and a glass transition temperature of 59°C was obtained.
[0101] In a tank equipped with a temperature control means and a nitrogen substitution means, 550 parts of ethyl acetate and 250 parts of 2-butanol were added to prepare a mixed solvent, and then 1000 parts of amorphous polyester resin (A) were gradually added and dissolved, and a 10% aqueous ammonia solution (equivalent to 3 times the amount by mole relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the reaction vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 4000 parts of ion-exchanged water was dropped into the mixed liquid while stirring, to perform emulsification. After the dropwise addition, the emulsion was returned to 25°C, and the solvent was removed under reduced pressure to obtain a resin particle dispersion in which resin particles with a volume average particle size of 160 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (A) was obtained.
[0102] [Preparation of amorphous polyester resin particle dispersion (B)] Terephthalic acid: 690 parts Trimellitic acid: 310 parts Ethylene glycol: 400 parts 1,5-Pentanediol: 450 parts The above materials were placed in a flask equipped with a stirrer, a nitrogen inlet tube, a temperature sensor, and a distillation column, and the temperature was raised to 220°C over 1 hour under a nitrogen gas flow, and 10 parts of titanium tetraethoxide was added for a total of 1000 parts of the above materials. The temperature was raised to 240°C over 0.5 hours while distilling off the generated water, and the dehydration condensation reaction was continued at 240°C for 1 hour, after which the reaction product was cooled. In this way, an amorphous polyester resin (B) with a weight average molecular weight of 127000 and a glass transition temperature of 59°C was obtained.
[0103] In a tank equipped with a temperature control means and a nitrogen substitution means, 700 parts of ethyl acetate and 500 parts of 2-butanol were added to prepare a mixed solvent, and then 1000 parts of amorphous polyester resin (B) were gradually added and dissolved, and a 10% aqueous ammonia solution (equivalent to 4 times the amount by molar ratio relative to the acid value of the resin) was added thereto and stirred for 30 minutes. Next, the inside of the reaction vessel was substituted with dry nitrogen, the temperature was kept at 40°C, and 4000 parts of ion-exchanged water was dropped into the mixed liquid while stirring, to perform emulsification. After the dropwise addition, the emulsion was returned to 25°C, and the solvent was removed under reduced pressure to obtain a resin particle dispersion in which resin particles with a volume average particle size of 80 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and an amorphous polyester resin particle dispersion (B) was obtained.
[0104] [Preparation of crystalline polyester resin particle dispersion (C)] 1,10-Decanedicarboxylic acid: 2600 parts 1,6-Hexanediol: 1670 parts Dibutyltin oxide (catalyst): 3 parts The above materials were placed in a heated and dried reactor, the air in the reactor was replaced with nitrogen gas to create an inert atmosphere, and the mixture was stirred and refluxed at 180°C for 5 hours using mechanical stirring. The temperature was then gradually increased to 230°C under reduced pressure and the mixture was stirred for 2 hours, and when the mixture became viscous, it was air-cooled to stop the reaction. Thus, a crystalline polyester resin with a weight average molecular weight of 12600 and a melting temperature of 73°C was obtained. 900 parts of crystalline polyester resin, 18 parts of anionic surfactant (TaycaPower, manufactured by Tayca Corporation) and 2100 parts of ion-exchanged water were mixed, heated to 120°C, dispersed using a homogenizer (Ultra Turrax T50 manufactured by IKA Corporation), and then dispersed for 1 hour using a pressure discharge type Gaulin homogenizer to obtain a resin particle dispersion in which resin particles with a volume average particle size of 160 nm were dispersed. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a crystalline polyester resin particle dispersion (C) was obtained.
[0105] [Preparation of styrene acrylic resin particle dispersion (S)] Styrene: 3,750 parts n-Butyl acrylate: 250 parts Acrylic acid: 20 parts Dodecanethiol: 240 parts Carbon tetrabromide: 40 parts A surfactant aqueous solution was prepared by dissolving 60 parts of a nonionic surfactant (Sanyo Chemical Industries, Nonipol 400) and 100 parts of an anionic surfactant (TaycaPower, Tayca Co., Ltd.) in 5500 parts of ion-exchanged water. The mixture obtained by mixing and dissolving the above-mentioned polymerization materials was dispersed and emulsified in the surfactant aqueous solution. Next, an aqueous solution obtained by dissolving 40 parts of ammonium persulfate in 500 parts of ion-exchanged water was added to the reaction vessel over a period of 20 minutes while stirring the inside of the reaction vessel. Next, after nitrogen replacement, the reaction vessel was heated in an oil bath while stirring the inside of the reaction vessel until the contents reached 70°C, and the temperature was maintained at 70°C for 5 hours to continue emulsion polymerization. In this way, a resin particle dispersion in which resin particles having a volume average particle size of 160 nm were dispersed was obtained. Ion-exchanged water was added to this resin particle dispersion to adjust the solid content to 20%, and a styrene acrylic resin particle dispersion (S) was obtained.
[0106] [Preparation of release agent particle dispersion (W)] Paraffin wax (manufactured by Nippon Seiro Co., Ltd., FNP92, melting temperature 92°C): 1,000 parts Anionic surfactant (TaycaPower, manufactured by Tayca Corporation): 10 parts Ion-exchanged water: 3,500 parts The above materials were mixed and heated to 100°C, dispersed using a homogenizer (IKA Ultra Turrax T50), and then dispersed using a pressure discharge Gaulin homogenizer to obtain a release agent particle dispersion in which release agent particles with a volume average particle size of 220 nm were dispersed. Ion-exchanged water was added to this release agent particle dispersion to adjust the solid content to 20%, and this was used as release agent particle dispersion (W).
[0107] [Preparation of colorant particle dispersion (K)] Carbon black (Cabot, Regal 330): 500 parts Anionic surfactant (Daiichi Kogyo Seiyaku Co., Ltd., Neogen RK): 50 parts Ion-exchanged water: 1930 parts The above materials were mixed and dispersed for 10 minutes at 240 MPa using an Ultimizer (manufactured by Sugino Machine Co., Ltd.) to obtain a colorant particle dispersion (K) with a solid content concentration of 20%.
[0108] <Example 1> [Preparing the reaction vessel] A jacketed stirring tank was prepared. The bottom of the stirring tank was connected to a disperser (Cavitron CD1010, manufactured by Pacific Machinery Co., Ltd.) via a conduit and a circulation pump, and the conduit from the disperser's outlet was immersed in the tank from above to create a circulation type reaction tank. A material inlet was provided in the conduit connecting the bottom of the stirring tank and the disperser.
[0109] [First flocculation step] Ion-exchanged water: 5,000 parts Amorphous polyester resin particle dispersion (A): 2630 parts Amorphous polyester resin particle dispersion (B): 2630 parts Crystalline polyester resin particle dispersion (C): 1,500 parts Styrene acrylic resin particle dispersion (S): 750 parts Release agent particle dispersion (W): 1,500 parts Colorant particle dispersion (K): 1,500 parts The above materials were placed in a circulating reactor and the pH was adjusted to 3.8 by adding 0.1N nitric acid. An aqueous aluminum sulfate solution was prepared by dissolving 15 parts of aluminum sulfate in 1000 parts of ion-exchanged water. While the contents were circulated in the circulation reaction tank for stirring and dispersion, the aqueous aluminum sulfate solution was added from the inlet. Next, the contents were circulated for 10 minutes while maintaining the temperature at 30°C, and stirred and dispersed. Next, the disperser was stopped, the bottom valve at the bottom of the stirring tank was closed, and 3,000 parts of ion-exchanged water was charged from the charging port, and then charged into the stirring tank via the disperser and conduit, and mixed with the dispersion by stirring. Next, the contents were heated to 45° C. in the jacket while continuing to stir, and maintained at that temperature until the volume average particle size of the aggregated particles reached 4.0 μm.
[0110] [Second flocculation step] A mixture of 2250 parts of the amorphous polyester resin particle dispersion (A) and 2250 parts of the amorphous polyester resin particle dispersion (B) was added to the stirring vessel and held for 30 minutes to obtain a dispersion containing second aggregated particles.
[0111] [Agglomeration stop process] 200 parts of EDTA (ethylenediaminetetraacetic acid) was added to the dispersion liquid containing the second aggregated particles, and then the pH was adjusted and the stirring power required per unit volume was varied in three stages as described below. (1) Add 1N sodium hydroxide solution to adjust the pH to 5, and reduce the stirring power required per unit volume to 3.2 kW / m 3 to 2.8kW / m 3 and held for 5 minutes. (2) Next, a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 7, and the stirring power required per unit volume was adjusted to 2.8 kW / m 3 to 1.4kW / m 3 and held for 3 minutes. (3) Next, a 1N aqueous solution of sodium hydroxide was added to adjust the pH to 9, and the stirring power required per unit volume was adjusted to 1.4 kW / m 3 to 0.3kW / m 3 and held for 5 minutes.
[0112] [Uniting process] While continuing stirring in the stirring layer, the mixture was heated to 85°C at a heating rate of 0.5°C / min, held at 85°C for 3 hours, and then cooled to 30°C at 15°C / min (first cooling). Next, the mixture was heated to 55°C at a heating rate of 0.2°C / min (reheating), held for 30 minutes, and then cooled to 30°C at 0.5°C / min (second cooling). Next, the solid content was filtered, washed with ion-exchanged water, and dried to obtain toner particles (1) having a volume average particle size of 5.0 μm.
[0113] [Addition of external additives] 100 parts of toner particles (1) and 1.5 parts of hydrophobic silica (RY50, manufactured by Nippon Aerosil Co., Ltd.) were mixed and mixed for 30 seconds at a rotation speed of 10,000 rpm using a sample mill. The mixture was sieved using a vibrating sieve with an opening of 45 μm to obtain toner (1). The volume average particle diameter of toner (1) was 5.0 μm.
[0114] [Creating the carrier] After 500 parts of spherical magnetite powder particles (volume average particle diameter 0.55 μm) were stirred with a Henschel mixer, 5 parts of a titanate-based coupling agent were added, and the mixture was heated to 100 ° C and stirred for 30 minutes. Next, 6.25 parts of phenol, 9.25 parts of 35% formalin, 500 parts of magnetite particles treated with a titanate-based coupling agent, 6.25 parts of 25% ammonia water, and 425 parts of water were added to a four-neck flask and stirred, and reacted at 85 ° C for 120 minutes while stirring. Next, the mixture was cooled to 25 ° C, 500 parts of water were added, and the supernatant liquid was removed and the precipitate was washed with water. The washed precipitate was heated and dried under reduced pressure to obtain a carrier (CA) with an average particle size of 35 μm.
[0115] [Preparation of developer] The toner (1) and the carrier (CA) were placed in a V blender in a ratio of toner (1):carrier (CA)=5:95 (mass ratio) and stirred for 20 minutes to obtain a developer (1).
[0116] <Examples 2 to 6, Comparative Examples 1 to 2> Toner particles were obtained in the same manner as in Example 1, except that the production conditions of the toner particles were changed to the specifications shown in Table 1. Next, in the same manner as in Example 1, external additives were added to the toner particles, and the toner particles were mixed with a carrier to obtain a developer.
[0117] <Performance evaluation> The toner particles before the external addition were used as a sample and the following evaluations were carried out.
[0118] [Particle size distribution index] The particle size distribution of the toner particles was measured using the measurement method for the volume average particle size of the toner described above. The cumulative volume distribution was plotted from the small diameter side, and the particle size D16v at the cumulative 16% and the particle size D50v at the cumulative 50% were obtained. The particle size distribution index on the small diameter side was calculated by dividing D50v by D16v. The results are shown in Table 1. The closer the value of D50v / D16v is to 1, the better.
[0119] [Fine particle ratio] Toner particles with a particle size of 3 μm or less were defined as fine particles, and the percentage of toner particles with a particle size of 3 μm or more (number %) was calculated in the particle size distribution obtained above. The results are shown in Table 1.
[0120] [Ratio of coarse particles] Toner particles having a particle size of 15 μm or more were defined as coarse particles, and the volume ratio (volume %) of toner particles having a particle size of 15 μm or more was calculated in the particle size distribution obtained above. The results are shown in Table 1.
[0121] [Table 1]
Claims
1. an aggregation step of aggregating the binder resin particles in a dispersion liquid containing the binder resin particles to form aggregated particles; an aggregation stopping step of adding an alkaline aqueous solution to the dispersion liquid containing the aggregated particles to increase the pH of the dispersion liquid containing the aggregated particles and stop the growth of the aggregated particles; a coalescence step of heating the dispersion liquid containing the aggregated particles to fuse and coalesce the aggregated particles to form toner particles, The aggregation stopping step includes: gradually increasing the pH of the dispersion liquid containing the aggregated particles by gradually adding the alkaline aqueous solution; and gradually decreasing the stirring power required per unit volume in accordance with the gradually increasing pH of the dispersion liquid containing the aggregated particles. A method for producing a toner for developing electrostatic images.
2. In the aggregation stopping step, the stirring power required per unit volume is 0.1 kW / m 3 The method for producing a toner for developing electrostatic images according to claim 1, wherein the toner content is not less than
3. In the aggregation stopping step, the required stirring power per unit volume is 3.5 kW / m 3 The method for producing a toner for developing an electrostatic image according to claim 1 or 2, wherein the toner has a molecular weight of 1:1 or more.
4. 4. The method for producing a toner for developing an electrostatic image according to claim 1, wherein the pH of the dispersion liquid containing the aggregated particles does not exceed 9 in the aggregation stopping step.
5. The method for producing a toner for developing an electrostatic image according to any one of claims 1 to 4, wherein the alkaline aqueous solution contains at least one selected from the group consisting of an aqueous solution of an alkali metal hydroxide, an aqueous solution of an alkaline earth metal hydroxide, and an aqueous solution of a chelating agent that chelates the coagulant.
6. the dispersion liquid containing the binder resin particles further contains release agent particles, the aggregating step is a step of aggregating the release agent particles to form the aggregated particles; The method for producing the toner for developing electrostatic images according to any one of claims 1 to 5.
7. the dispersion liquid containing the binder resin particles further contains colorant particles, the aggregating step is a step of aggregating the colorant particles to form the aggregated particles, The method for producing the toner for developing electrostatic images according to any one of claims 1 to 6.
8. a second aggregation step, which is performed before the aggregation termination step, of mixing a dispersion liquid containing the aggregated particles with a dispersion liquid containing resin particles that will become a shell layer, and aggregating the resin particles that will become the shell layer on surfaces of the aggregated particles to form second aggregated particles; the aggregation terminating step is a step of adding an alkaline aqueous solution to the dispersion liquid containing the second aggregated particles to increase the pH of the dispersion liquid containing the second aggregated particles and thereby terminating the growth of the second aggregated particles, the coalescence step is a step of heating a dispersion liquid containing the second aggregated particles to fuse and coalesce the second aggregated particles to form toner particles, The aggregation stopping step includes stirring the dispersion liquid containing the second aggregated particles, gradually increasing the pH of the dispersion liquid containing the second aggregated particles by gradually adding the alkaline aqueous solution; and gradually decreasing the stirring power required per unit volume in accordance with the gradually increasing pH of the dispersion liquid containing the second agglomerated particles. The method for producing the toner for developing electrostatic images according to any one of claims 1 to 7.
Citation Information
Patent Citations
Electrostatic image developing toner, and developing agent for electrostatic image developing, developing agent cartridge for electrostatic image developing process cartridge and image forming apparatus using the same
JP2010060896A
Method for producing electrophotographic toner
JP2011102855A
Method for manufacturing toner with a narrow particle size distribution
JP2012514232A
Method of manufacturing toner
JP2013109341A
Agitation device, agitation method, and method for manufacturing electrical static charge image developing toner