Method for producing high pressure treated multilayer structure and method for high pressure treatment of multilayer structure
A high-pressure treatment method for multilayer structures with a highly saponified EVOH layer and thin olefin resin layer addresses the deterioration of gas barrier properties, achieving improved resistance to gas permeation by increasing crystallinity through compression.
Patent Information
- Application Number
- JP2021539269
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-09
- Filing Date
- 2020-08-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-08-07
AI Technical Summary
Existing high-pressure treatment methods for multilayer structures with an ethylene-vinyl alcohol copolymer (EVOH) layer result in moisture absorption, leading to deterioration of gas barrier properties.
A multilayer structure with an EVOH layer and an olefin resin layer, where the EVOH layer consists of a resin composition with a high degree of saponification (>99.7 mol%) and a thickness of less than 100 μm, subjected to high pressure (200 MPa or more) in an atmosphere of 20°C or higher for 3 minutes or more.
The method improves gas barrier properties by compressing the amorphous part of the EVOH layer, increasing crystallinity and regularizing the lamellar structure, thereby enhancing the multilayer structure's resistance to gas permeation.
Smart Images

Figure 0007589689000002 
Figure 0007589689000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a high-pressure treated multilayer structure, and a high-pressure treatment method for a multilayer structure having an ethylene-vinyl alcohol copolymer layer and an olefin resin layer. [Background technology]
[0002] In recent years, film packaging (multiple-layered structures) that are lighter than bottles or cans and have excellent volume reduction properties after use have come to be used as packaging for foods, etc. Such multilayered structures are required to have physical properties such as high strength and rigidity and tear resistance, as well as high gas barrier properties from the viewpoint of preventing deterioration of the contents.
[0003] On the other hand, the contents packaged in the multilayer structure usually need to be sterilized together with the multilayer structure for the sake of hygiene and storage. Known methods for the sterilization include hot water treatment such as retort treatment and boiling treatment, irradiation with ultraviolet rays or gamma rays, and high pressure treatment. Among them, the high pressure treatment is widely used because it hardly causes deterioration of the contents.
[0004] As such a high-pressure treatment method, for example, Patent Document 1 describes a method of high-pressure treatment of a multilayer structure including an ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as "EVOH") layer, the EVOH layer being made of EVOH having a saponification degree of 95 mol% or more. Also, Non-Patent Document 1 describes a method of high-pressure treatment of a multilayer structure including three layers of a polypropylene (hereinafter sometimes referred to as "PP") layer / EVOH layer / PP layer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 3-290175 [Non-patent literature]
[0006] [Non-Patent Document 1] Amparo Lopez-Rubio, Jose M. Lagaron, Pilar Hernandez-Munoz, Eva Almenar, Ramon Catala, Rafael Gavara, Melvin A. Pascall, Innovative Food Science and Emerging Technologies 6 (2005) 51-58 Summary of the Invention [Problem to be solved by the invention]
[0007] However, in the method described in Patent Document 1, although a sterilizing effect on the contents can be obtained, it was found that the EVOH layer absorbs moisture during high-pressure treatment, resulting in a problem of a decrease in the gas barrier property of the multilayer structure. Also, in the method described in Non-Patent Document 1, although a sterilizing effect on the contents can be obtained, it cannot be denied that the gas barrier property is also decreased, and there was no method in which the gas barrier property was increased by high-pressure treatment.
[0008] In view of the above background, the present invention provides a high-pressure treatment method for a multilayer structure having an olefin-based resin layer and an EVOH layer, which can be used for packaging food and the like and whose gas barrier properties can be improved by performing high-pressure treatment, and a method for producing a high-pressure-treated multilayer structure. [Means for solving the problem]
[0009] However, in view of these circumstances, the present inventors have conducted extensive research and have found that, in a multilayer structure having an EVOH layer and an olefin-based resin layer, the gas barrier property of the multilayer structure can be improved by making the EVOH layer from a resin composition mainly composed of EVOH having a high degree of saponification, making the thickness of the olefin-based resin layer less than a predetermined value, and subjecting the multilayer structure to a high-pressure treatment at a pressure of 200 MPa or more in an atmosphere at a specific temperature or higher.
[0010] In order to achieve the above object, the present invention provides the following [1] to [4]. [1] A method for producing a high-pressure-treated multilayer structure having an EVOH layer and an olefin-based resin layer, comprising: preparing a multilayer structure in which the EVOH layer is made of a resin composition mainly composed of EVOH with a saponification degree of more than 99.7 mol% and the olefin-based resin layer has a thickness of less than 100 μm; and high-pressure treating the multilayer structure at a pressure of 200 MPa or more in an atmosphere of 20° C. or more. [2] The method for producing a high-pressure treated multilayer structure according to [1], wherein the high-pressure treatment is carried out for 3 minutes or more. [3] A high-pressure treatment method for a multilayer structure having an EVOH layer and an olefin-based resin layer, comprising: making the EVOH layer from a resin composition mainly composed of EVOH having a saponification degree of more than 99.7 mol%; making the thickness of the olefin-based resin layer less than 100 μm; and high-pressure treating the multilayer structure at a pressure of 200 MPa or more in an atmosphere of 20° C. or more. [4] The method for high-pressure treatment of a multilayer structure according to [3], wherein the high-pressure treatment is carried out for 3 minutes or more. Effect of the Invention
[0011] The high-pressure treatment method for a multilayer structure of the present invention is a high-pressure treatment method for a multilayer structure having an EVOH layer and an olefin-based resin layer, in which the EVOH layer is made of a resin composition mainly composed of EVOH having a saponification degree of more than 99.7 mol %, the olefin-based resin layer has a thickness of less than 100 μm, and the multilayer structure is high-pressure treated at a pressure of 200 MPa or more in an atmosphere of 20° C. or more. Therefore, despite the high-pressure treatment, the gas barrier property of the multilayer structure can be improved. It is presumed that high-pressure treatment compresses the amorphous parts of the EVOH that make up the EVOH layer, causing the lamellar structures that form long-period arrangements in the EVOH to fold regularly, increasing the crystallinity of the EVOH and improving the gas barrier properties. In the case of EVOH with a low degree of saponification, the acetyl groups are present in a disordered manner in the polymer, and therefore steric hindrance occurs due to the molecular chains when the amorphous parts are compressed in high-pressure treatment, preventing an increase in crystallinity and making it difficult to improve the gas barrier properties. Therefore, it is speculated that the gas barrier properties are improved especially in EVOH with a high degree of saponification. In addition, the method for producing a high-pressure-treated multilayer structure of the present invention comprises producing the above-mentioned multilayer structure and high-pressure treating the multilayer structure at a pressure of 200 MPa or more in an atmosphere of 20°C or higher, thereby obtaining a multilayer structure with improved gas barrier properties. [Brief description of the drawings]
[0012] [Figure 1] 1 is a schematic diagram showing a cross section of a multilayer structure according to an embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these.
[0014] The high-pressure treatment method for a multilayer structure according to an embodiment of the present invention is performed on a multilayer structure having at least an olefin resin layer and an EVOH layer. The thickness of the olefin resin layer is less than 100 μm, the EVOH layer is made of a resin composition mainly composed of EVOH with a saponification degree exceeding 99.7 mol%, and the multilayer structure is subjected to high-pressure treatment at a pressure of 200 MPa or more in an atmosphere of 20°C or higher. Further, the method for manufacturing a high-pressure treated multilayer structure according to an embodiment of the present invention is to produce the multilayer structure and subject the multilayer structure to high-pressure treatment at a pressure of 200 MPa or more in an atmosphere of 20°C or higher to obtain a high-pressure treated multilayer structure.
[0015] First, the multilayer structure targeted by the present invention will be described, and then, as an embodiment of the present invention, the method for high-pressure treating this multilayer structure and the method for manufacturing a high-pressure treated multilayer structure will be described.
[0016] [Multilayer structure] FIG. 1 schematically shows a multilayer structure 1 targeted by an embodiment of the present invention. The multilayer structure 1 has an olefin resin layer 4 provided on both the front and back surfaces of an EVOH layer 2 via an adhesive resin layer 3, respectively, and has a five-layer structure. Such a multilayer structure 1 can be used for, for example, various packages such as general foods, seasonings such as mayonnaise and dressing, fermented foods such as miso, oil and fat foods such as salad oil, beverages, cosmetics, and pharmaceuticals. In FIG. 1, each part is schematically shown and is different from the actual thickness, size, etc.
[0017] <EVOH layer 2> The EVOH layer 2 mainly bears gas barrier properties and is made of a resin composition mainly composed of EVOH with a saponification degree exceeding 99.7 mol%. Here, the main component means a component that affects the properties of the material, and the content of that component is usually 50 mass% or more of the entire material, including those that are 100 mass% (consisting only of EVOH with a saponification degree exceeding 99.7 mol%). The saponification degree is a value obtained by measuring the vinyl ester component in EVOH according to JIS K6726 (wherein EVOH is a solution uniformly dissolved in a water / methanol solvent). In the EVOH, the saponification degree is preferably 99.8 to 100 mol%, and more preferably 99.9 to 100 mol%. If the saponification degree is too low, the gas barrier property tends to be insufficient.
[0018] The EVOH is a resin obtained by saponifying a copolymer of ethylene and a vinyl ester monomer (ethylene-vinyl ester copolymer), and is a water-insoluble thermoplastic resin. The copolymer can be produced by any known polymerization method of ethylene and a vinyl ester monomer, such as solution polymerization, suspension polymerization, or emulsion polymerization, but generally, solution polymerization using a lower alcohol such as methanol as a solvent is used. The saponification of the copolymer can also be carried out by a known method. The EVOH produced in this way mainly contains structural units derived from ethylene and vinyl alcohol structural units, and contains a small amount of vinyl ester structural units remaining without being saponified.
[0019] As the vinyl ester monomer, vinyl acetate is preferably used because of its easy availability on the market and its high efficiency in treating impurities during production. Other vinyl ester monomers include, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate, and aliphatic vinyl esters having usually 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These can be used alone or in combination of two or more kinds.
[0020] The ethylene content in the EVOH is preferably 20 to 60 mol%, more preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%, as measured in accordance with ISO 14663. If the ethylene content is too low, the gas barrier properties and melt moldability under high humidity conditions tend to decrease, whereas if the ethylene content is too high, the gas barrier properties tend to decrease.
[0021] The melt flow rate (MFR) of the EVOH (210°C, load 2,160 g) is preferably 0.5 to 100 g / 10 min, more preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, the film formability tends to decrease, and if it is too low, the melt viscosity tends to be too high, making melt extrusion difficult.
[0022] The EVOH may further contain structural units derived from the comonomers shown below, in addition to ethylene structural units and vinyl alcohol structural units (including unsaponified vinyl ester structural units). Examples of the comonomers include α-olefins such as propylene, isobutene, α-octene, α-dodecene, and α-octadecene, hydroxyl-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, and 3-buten-1,2-diol, and esters thereof; hydroxyl-containing α-olefin derivatives such as acylation products; unsaturated carboxylic acids or salts thereof, partial alkyl esters, complete alkyl esters, nitriles, amides, or anhydrides; unsaturated sulfonic acids or salts thereof; vinyl silane compounds; vinyl chloride; and styrene.
[0023] The EVOH may be an EVOH-based resin that has been "post-modified" by urethanization, acetalization, cyanoethylation, oxyalkylenation, etc. Among such modified products, EVOH in which a primary hydroxyl group has been introduced into the side chain by copolymerization is preferred in that it provides good secondary moldability in stretching treatment, vacuum / pressure molding, etc., and among these, EVOH having a 1,2-diol structure in the side chain is preferably used.
[0024] The resin composition mainly composed of EVOH may contain additives generally used in resin compositions mainly composed of EVOH, such as heat stabilizers, antioxidants, antistatic agents, colorants, ultraviolet absorbers, lubricants, plasticizers, light stabilizers, surfactants, antibacterial agents, desiccants, antiblocking agents, flame retardants, crosslinking agents, curing agents, foaming agents, crystal nucleating agents, antifogging agents, biodegradable additives, silane coupling agents, oxygen absorbers, etc., within the scope of not impairing the effects of the present invention. These may be used alone or in combination of two or more.
[0025] Examples of the heat stabilizer, for the purpose of improving various physical properties such as heat stability during melt molding, include organic acids such as acetic acid, propionic acid, butyric acid, lauric acid, stearic acid, oleic acid, behenic acid, etc., or salts thereof such as alkali metal salts (sodium, potassium, etc.), alkaline earth metal salts (calcium, magnesium, etc.), zinc salts, etc.; or inorganic acids such as sulfuric acid, sulfurous acid, carbonic acid, phosphoric acid, boric acid, etc., or salts thereof such as alkali metal salts (sodium, potassium, etc.), alkaline earth metal salts (calcium, magnesium, etc.), zinc salts, etc.
[0026] The resin composition containing EVOH as a main component may use one or more types of EVOH. The two or more types of EVOH may be appropriately selected from EVOHs having different ethylene contents, different degrees of saponification, different melt flow rates (MFR) (210°C, load 2,160 g), different other copolymerization components, or different amounts of modification (for example, EVOHs having different contents of 1,2-diol structural units).
[0027] The resin composition containing EVOH as a main component preferably contains a polyamide resin, which can form a network structure through the interaction of amide bonds with at least one of the hydroxyl group and / or ester group of EVOH, thereby preventing the elution of EVOH during high-pressure treatment.
[0028] As the polyamide-based resin, known resins can be used. For example, homopolymers such as polycapramide (nylon 6), poly-ω-aminoheptanoic acid (nylon 7), poly-ω-aminononanoic acid (nylon 9), polyundecaneamide (nylon 11), and polylauryllactam (nylon 12) can be used. In addition, as copolymerized polyamide-based resins, for example, polyethylenediamineadipamide (nylon 26), polytetramethyleneadipamide (nylon 46), polyhexamethyleneadipamide (nylon 66), polyhexamethylenesebacamide (nylon 610), polyhexamethylenedodecamamide (nylon 612), polyoctamethyleneadipamide (nylon 86), polydecamethyleneadipamide (nylon 108), caprolactamamide (nylon 106), and polytetramethyleneadipamide (nylon 108) can be used. Caprolactam / lauryl lactam copolymer (nylon 6 / 12), caprolactam / ω-aminononanoic acid copolymer (nylon 6 / 9), caprolactam / hexamethylenediammonium adipate copolymer (nylon 6 / 66), lauryl lactam / hexamethylenediammonium adipate copolymer (nylon 12 / 66), ethylenediamine adipamide / hexamethylenediammonium adipate copolymer (nylon 26 / 66 ), aliphatic copolymer polyamides such as caprolactam / hexamethylene diammonium adipate / hexamethylene diammonium sebacate copolymer (nylon 66 / 610), and ethylene ammonium adipate / hexamethylene diammonium adipate / hexamethylene diammonium sebacate copolymer (nylon 6 / 66 / 610); aromatic copolymer polyamides such as polyhexamethylene isophthalamide, polyhexamethylene terephthalamide, polymetaxylylene adipamide, hexamethylene isophthalamide / terephthalamide copolymer, poly-p-phenylene terephthalamide, and poly-p-phenylene-3-4'-diphenyl ether terephthalamide; amorphous polyamides; and terminal-modified polyamides obtained by modifying the terminals of the above polyamide resins with carboxyl groups or amino groups such as methylene benzylamine and metaxylylene diamine. From the viewpoint of further improving the gas barrier property, a copolymerized polyamide resin is preferable, and an aliphatic copolymerized polyamide is particularly preferable. These can be used alone or in combination of two or more kinds.
[0029] The content of the polyamide resin in the resin composition containing EVOH as a main component is, for example, preferably 1 to 40 mass % and more preferably 5 to 35 mass % of the entire resin composition.
[0030] The thickness of the EVOH layer 2 is usually from 1 to 30 μm, preferably from 3 to 28 μm, and more preferably from 5 to 25 μm.
[0031] <Adhesive resin layer 3> The adhesive resin layer 3 is provided to increase the adhesive strength between the EVOH layer 2 and the olefin resin layer 4 described later, and is made of a resin composition containing an adhesive resin. The adhesive resin may be a known one, and may be appropriately selected according to the type of resin used in the EVOH layer 2 and the olefin resin layer 4. A representative example is a modified polyolefin polymer containing a carboxyl group obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin by addition reaction, graft reaction, or the like. Examples of such modified polyolefins include maleic anhydride grafted polyethylene, maleic anhydride grafted polypropylene, maleic anhydride grafted ethylene-propylene (block and random) copolymer, maleic anhydride grafted ethylene-ethyl acrylate copolymer, maleic anhydride grafted ethylene-vinyl acetate copolymer, maleic anhydride modified polycyclic olefin resin, maleic anhydride grafted polyolefin resin, etc. Among them, from the viewpoint of improving the water resistance of the multilayer structure 1, it is preferable to use an adhesive resin with excellent hydrophobicity, and in particular, it is preferable to use a polycyclic olefin resin. These can be used alone or in combination of two or more kinds.
[0032] The polycyclic olefin resin has a lower moisture permeability than linear aliphatic polyolefins such as polyethylene, polypropylene, etc. Therefore, when a polycyclic olefin resin is used for the adhesive resin layer 3, the amount of moisture mixed in from the outside due to humidity or hot water sterilization treatment, etc., can be reduced, and the oxygen permeability of the multilayer structure 1 after high pressure treatment can be maintained at a good level.
[0033] The resin composition containing the adhesive resin may be composed of only the adhesive resin, but may also contain conventionally known plasticizers, fillers, clays (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, ultraviolet absorbers, waxes, etc.
[0034] The thickness of the adhesive resin layer 3 is usually 1 to 30 μm, preferably 2 to 20 μm, and more preferably 3 to 10 μm.
[0035] <Olefin-based resin layer 4> The olefin resin layer 4 is provided to further increase the strength and gas barrier properties, and is made of a resin composition containing an olefin resin. The olefin resin may be one that melts by heat and can be fused to other layers. Examples of the olefin resin include polypropylene resin, polyethylene resin, polycyclic olefin resin, and unsaturated carboxylic acid modified polyolefin resins thereof. Among them, it is preferable to use a polypropylene resin because of its excellent heat resistance, moisture absorption, and solvent resistance. These can be used alone or in combination of two or more kinds.
[0036] Examples of the polypropylene-based resin include propylene homopolymer, ethylene-propylene random copolymer, ethylene-propylene block copolymer, copolymer of propylene and a small amount (1 to 10 mass%) of other α-olefins (e.g., 1-butene, 1-hexene, 4-methyl-1-pentene, etc.), propylene and ethylene propylene, etc. Propylene homopolymer is preferred in terms of excellent recyclability and heat sealability, low cost, etc. In addition, it is desirable that the melting point is 130°C or higher in terms of being usable in hot water sterilization treatment under stricter conditions.
[0037] The resin composition containing the olefin-based resin may be composed only of the olefin-based resin, but may also contain conventionally known plasticizers, fillers, clays (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, ultraviolet absorbers, waxes, etc.
[0038] The thickness of the olefin-based resin layer 4 is less than 100 μm, preferably 10 to 90 μm, more preferably 20 to 80 μm, and further preferably 30 to 70 μm in order to further improve the gas barrier property of the multilayer structure 1. When there are a plurality of the olefin-based resin layers, it is sufficient that at least one of the layers has a thickness of less than 100 μm.
[0039] The multilayer structure 1 (see FIG. 1) having these layers can be manufactured by, for example, melt molding, wet lamination, dry lamination, solventless lamination, extrusion lamination, co-extrusion lamination, inflation, etc. Among them, the melt molding is preferably used from the environmental aspect of not using a solvent and from the cost aspect of not needing lamination in a separate process. As the melt molding method, a known method can be adopted, for example, an extrusion molding method (T-die extrusion, tubular film extrusion, blow molding, melt spinning, irregular extrusion, etc.), an injection molding method, etc. The melt molding temperature is usually appropriately selected from the range of 150 to 300°C.
[0040] Alternatively, a multilayer material having any layer such as the olefin resin layer 4 and the EVOH layer 2 is prepared in advance, and the multilayer material is laminated to another multilayer material or any layer. In terms of reducing the cost required for lamination, it is preferable to manufacture the multilayer material by a method that requires fewer laminations.
[0041] The multilayer structure 1 thus obtained may be reheated and may be uniaxially or biaxially stretched, for example, by a thermoforming method such as squeeze molding, a roll stretching method, a pantograph stretching method, an inflation stretching method, a blow molding method, or the like, to obtain a stretched molded product.
[0042] The thickness of the multilayer structure 1 is usually 10 to 600 μm, preferably 50 to 300 μm, more preferably 70 to 280 μm, and even more preferably 80 to 260 μm. If the thickness of the multilayer structure 1 is too thin, it tends to be easily broken due to insufficient strength, and if it is too thick, it tends to have reduced flexibility. When the multilayer structure 1 is reheated (stretched, etc.), the above thickness is the value for the molded product after reheating (stretching, etc.) (the same applies below).
[0043] In the multilayer structure 1, the thickness ratio of the olefin resin layer 4 to the EVOH layer 2 (olefin resin layer 4 / EVOH layer 2), expressed as the ratio between the thinnest layers when there are multiple layers of each type, is usually 0.25 / 1 to 10 / 1, preferably 1 / 1 to 8 / 1, and more preferably 2 / 1 to 6 / 1.
[0044] In the multilayer structure 1, the thickness ratio of the adhesive resin layer 3 to the EVOH layer 2 (adhesive resin layer 3 / EVOH layer 2), expressed as the ratio between the thinnest layers when there are multiple layers, is usually 0.1 / 1 to 10 / 1, preferably 0.25 / 1 to 5 / 1, and more preferably 0.5 / 1 to 2 / 1.
[0045] In this embodiment, the multilayer structure 1 is a laminate of five layers in the order of olefin resin layer 4 / adhesive resin layer 3 / EVOH layer 2 / adhesive resin layer 3 / olefin resin layer 4 (see FIG. 1), but the present invention is not limited to this embodiment as long as it has at least two layers, olefin resin layer 4 and EVOH layer 2. The multilayer structure 1 used in the present invention may have any number of layers as long as it has at least the above two layers and does not impair the effects of the present invention, and may have other layers or may not have the adhesive resin layer 3. However, as in this embodiment, the structure in which the EVOH layer 2 is in contact with the olefin resin layer 4 via the adhesive resin layer 3 can further increase the adhesion between the EVOH layer 2 and the olefin resin layer 4, and can achieve higher gas barrier properties. From this point of view, it is preferable to provide the adhesive resin layer 3 between the EVOH layer 2 and the olefin resin layer 4.
[0046] Examples of the resin constituting the other layer include polyester resins such as polyethylene terephthalate and polyethylene naphthalate, polyamide resins such as various nylon resins, polyaramid resins, polypropylene resins, polyethylene resins, polycarbonate resins, polyacetal resins, and fluorine resins. A base film may be used as the other layer. The thickness of the other resin layer is preferably 1 to 100 μm per layer, more preferably 5 to 90 μm, and particularly preferably 10 to 80 μm.
[0047] In this embodiment, the multilayer structure 1 has two olefin-based resin layers 4, which are made of the same resin composition and have the same thickness, but they may be made of different resin compositions and have different thicknesses. The same applies to the adhesive resin layer 3.
[0048] [Method of manufacturing high-pressure treated multilayer structure] The high pressure treatment in the present invention may, for example, be a sterilization treatment of the multilayer structure 1 itself or the contents (hereinafter sometimes referred to as "contents") packaged in the multilayer structure 1 by placing the multilayer structure 1 under high pressure conditions using water as a medium. Compared with the commonly used retort sterilization treatment, the high pressure treatment has the advantage that it is possible to perform treatment at a low temperature for a short time, and therefore does not impair the color, aroma, or nutrients of the contents. In addition, by performing the high pressure treatment on the multilayer structure, a high pressure treated multilayer structure of the present invention can be obtained.
[0049] In the present invention, the pressure employed in the high-pressure treatment is 200 MPa or more, preferably 200 to 800 MPa, and more preferably 500 to 700 MPa. That is, if the pressure is too low, the improvement in gas barrier properties tends to be insufficient, whereas if the pressure is too high, the load on the apparatus tends to be large.
[0050] The temperature employed in the high pressure treatment is 20° C. or higher, preferably 20 to 90° C., and more preferably 50 to 80° C. That is, if the temperature is too low, the amount of heat required to control the molecular motion of EVOH is insufficient, and it tends to be difficult to improve the barrier properties. On the other hand, if the temperature is too high, bumping occurs when water is used as the pressure medium, and the load on the device tends to be large.
[0051] The high pressure treatment is preferably carried out for 3 minutes or more, more preferably 5 to 60 minutes. That is, if the treatment time is too short, the improvement of the gas barrier property tends to be insufficient, whereas if the treatment time is too long, the inside of the apparatus remains in a pressurized state for a long period of time, which increases the load on the apparatus and tends to increase the frequency of replacing packing and the like.
[0052] The high-pressure treatment method of the present invention is useful for the multilayer structure 1 used for various packages of general foods, as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, medicines, etc. That is, according to the high-pressure treatment method of the present invention, the multilayer structure 1 has excellent gas barrier properties after high-pressure treatment, and further has the advantage of minimizing deterioration of the contents. Furthermore, according to the manufacturing method of the high-pressure-treated multilayer structure of the present invention, it is possible to obtain a high-pressure-treated multilayer structure with improved gas barrier properties, and therefore when used for packaging containing general foods as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc., the deterioration of the contents can be minimized. EXAMPLES
[0053] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.
[0054] First, the following materials were prepared as materials for each layer constituting the multilayer structure. [EVOH layer] No.1: EVOH with an ethylene structural unit content of 29 mol%, a saponification degree of 99.8 mol%, and an MFR of 4.0 g / 10 min (210°C, load 2,160 g). No. 2: EVOH with an ethylene structural unit content of 44 mol%, a saponification degree of 99.8 mol%, and an MFR of 4.0 g / 10 min (210°C, load 2,160 g). No. 3: EVOH with an ethylene structural unit content of 44 mol%, a saponification degree of 98.5 mol%, and an MFR of 4.0 g / 10 min (210°C, load 2,160 g). [Olefin resin layer] Homopolypropylene (Novatec EA7AD, manufactured by Japan Polypropylene Corporation). [Adhesive resin layer] Polypropylene adhesive resin (Plexor PX6002, manufactured by LyondellBasell).
[0055] <Examples 1 to 8 and Comparative Examples 1 to 6> Using the materials for each of the above layers, a film was formed by extrusion molding (T-die extrusion) to produce a multilayer structure 1 (see Figure 1) having five layers: olefin-based resin layer 4 / adhesive resin layer 3 / EVOH layer 2 / adhesive resin layer 3 / olefin-based resin layer 4, with the type of resin in the EVOH layer and the thickness of each layer shown in Table 1 below.
[0056] Next, each of the obtained multilayer structures 1 was subjected to high-pressure treatment under hydrostatic pressure using a high-pressure treatment device (Dr. Chef, manufactured by Kobe Steel Works, Ltd.) under the conditions shown in Table 1, with water as a solvent.
[0057] [Gas barrier improvement rate] Regarding the multilayer structure 1, the oxygen permeability (cc / m 2 The oxygen permeability (MPa) was measured under the following conditions using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 21). The obtained values were then used in the following formula to calculate the gas barrier improvement rate (%). These are shown in Table 1 below. <Measurement conditions> ·Temperature: 23℃ Humidity on the water vapor supply side: 90% RH Humidity on carrier gas side: 50% RH <Gas barrier improvement rate (%)> Gas barrier improvement rate (%) = (oxygen permeability before high pressure treatment - oxygen permeability after high pressure treatment) / oxygen permeability before high pressure treatment
[0058] [Table 1]
[0059] From the above results, it was found that by forming a multilayer structure in which the olefin resin layer has a specific thickness and the EVOH layer is made of a resin composition having a specific EVOH as a main component, and by subjecting the multilayer structure to high pressure treatment under specific conditions, the gas barrier properties of the multilayer structure were improved (improved) (Examples 1 to 8). In contrast, in Comparative Examples 1 to 6 which did not satisfy at least one of the above conditions, no improvement in the gas barrier properties of the multilayer structure was observed. Therefore, it is evident that the high-pressure treatment method for a multi-layer structure of the present invention is extremely useful as a method for sterilization when the multi-layer structure is used in various packages. Furthermore, the method for producing a high-pressure-treated multilayer structure of the present invention can produce a high-pressure-treated multilayer structure having improved gas barrier properties by subjecting the multilayer structure to the high-pressure treatment.
[0060] In the above embodiment, specific embodiments of the present invention are shown, but the above embodiment is merely illustrative and should not be interpreted as being limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention. [Industrial Applicability]
[0061] The high-pressure treatment method for a multilayer structure of the present invention can improve the gas barrier properties of the multilayer structure after high-pressure treatment, and can therefore be suitably used when the multilayer structure is used as a packaging material for food and beverages, etc., and the contents (food and beverages, etc.) are sterilized together with the packaging material. [Explanation of symbols]
[0062] 1 Multilayer structure 2 EVOH layer 3 Adhesive resin layer 4 Olefin resin layer
Claims
1. A method for producing a high-pressure treated multilayer structure having an ethylene-vinyl alcohol-based copolymer layer and an olefin-based resin layer, comprising the steps of: a multilayer structure is produced in which the ethylene-vinyl alcohol copolymer layer is made of a resin composition containing as a main component an ethylene-vinyl alcohol copolymer with a saponification degree of more than 99.7 mol %, an olefin resin layer is provided on both the front and back surfaces of the ethylene-vinyl alcohol copolymer layer via another layer, the other layer being made of a resin composition containing a modified polyolefin polymer containing a carboxyl group, and the olefin resin layer has a thickness of less than 100 μm; A method for producing a high-pressure treated multilayer structure, comprising subjecting the multilayer structure to a high-pressure treatment at a pressure of 200 MPa or more.
2. 2. The method for producing a high-pressure treated multi-layer structure according to claim 1, wherein the high-pressure treatment is carried out for 3 minutes or more.
3. A method for producing a high-pressure treated multilayer structure according to claim 1 or 2, characterized in that the high-pressure treatment is carried out in an atmosphere of 50 to 90°C.
4. A high-pressure treatment method for a multilayer structure having an ethylene-vinyl alcohol-based copolymer layer and an olefin-based resin layer, comprising: the ethylene-vinyl alcohol copolymer layer is made of a resin composition mainly containing an ethylene-vinyl alcohol copolymer with a saponification degree of more than 99.7 mol %, an olefin resin layer is provided on both the front and back sides of the ethylene-vinyl alcohol copolymer layer via another layer, the other layer being made of a resin composition containing a modified polyolefin polymer containing a carboxyl group, and the thickness of the olefin resin layer is less than 100 μm, A method for high-pressure treatment of a multilayer structure, comprising subjecting the multilayer structure to a high-pressure treatment at a pressure of 200 MPa or more.
5. 5. The method for high pressure treatment of a multi-layer structure according to claim 4, wherein the high pressure treatment is carried out for 3 minutes or more.
6. The method for high pressure treatment of a multilayer structure according to claim 4 or 5, wherein the high pressure treatment is carried out in an atmosphere of 50 to 90°C.
Citation Information
Patent Citations
High-temperature sterilization
JP1991290175A
Multilayer food and its preparation
JP1992148653A
Multilayered structure for ultrahigh pressure treatment, package for ultrahigh pressure treatment and treatment method therefor
JP2018058298A