Electrical contact member, brush, and rotating machine
By integrating carbon, copper, and low ionization voltage metals in electrical contact members, the issue of zinc oxide accumulation and increased resistance is mitigated, achieving reduced electromagnetic noise and filter-free rotating machines.
Patent Information
- Application Number
- JP2023518654
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-07
- Filing Date
- 2022-04-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-04-11
AI Technical Summary
Conventional electrical contact members using zinc to reduce electromagnetic noise face challenges such as increased contact resistance and decreased motor efficiency due to zinc oxide accumulation, necessitating high zinc content.
Incorporating carbon particles, copper particles, and low ionization voltage metals with a coating or as particles in the contact surface, promoting thermal ionization of these metals before copper, thereby increasing electron density and reducing electromagnetic noise without excessive zinc use.
This configuration reduces electromagnetic noise and eliminates the need for additional noise filters, leading to smaller, lighter, and cheaper rotating machines by enhancing electron density during arc discharge.
Smart Images

Figure 0007589928000001 
Figure 0007589928000002 
Figure 0007589928000003
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application is based on Japanese Application No. 2021-079010 filed on May 7, 2021, the contents of which are incorporated herein by reference. [Technical field]
[0002] The present disclosure relates to an electrical contact member, a brush, and a rotating machine. [Background technology]
[0003] 2. Description of the Related Art Electrical contact members have been used in various fields to establish electrical connection with mating members. For example, in the field of rotating machines such as motors, brushes having a contact surface that comes into sliding contact with a commutator, which is a mating member, are known.
[0004] Specifically, for example, Patent Document 1 discloses a technology in which zinc is added to an electrical contact member as a low-boiling point material with a boiling point lower than that of copper, and the vapor density during arc discharge is increased by the zinc vapor, thereby keeping the electron velocity small and reducing electromagnetic noise. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-68653 A Summary of the Invention
[0006] The conventional technology has the following problem. That is, zinc is more difficult to thermally ionize than copper. Therefore, according to the conventional technology, a large amount of zinc needs to be added to reduce electromagnetic noise. Therefore, zinc oxide is likely to accumulate on the surface of the mating material such as a commutator, and contact resistance is likely to increase. In addition, when this electrical contact member is applied to a brush of a motor, there is a risk of problems such as a decrease in motor efficiency.
[0007] An object of the present disclosure is to provide an electrical contact member capable of reducing electromagnetic noise without adding a large amount of zinc, and a brush and a rotating machine using the electrical contact member.
[0008] One aspect of the present disclosure is It has a contact surface for facing the mating material, the portion having the contact surface includes carbon particles, copper particles, and a low ionization voltage metal having an ionization voltage lower than that of copper; The low ionization voltage metal is contained as low ionization voltage metal particles, or as a coating layer covering the surface of the copper particles. And, In the scanning electron microscope image of the contact surface, No matter where a circle with a diameter of 50 μm is placed on the scanning electron microscope image, There exists a low ionization voltage metal that falls within the circle. , Located in the electrical contact member.
[0009] Another aspect of the present disclosure is a brush having the above-described electrical contact member.
[0010] Yet another aspect of the present disclosure is a rotating machine having the above-mentioned brush.
[0011] The electrical contact member has the above configuration. Therefore, in the electrical contact member, when an arc discharge occurs between the contact surface and the mating material, the low ionization voltage metal is thermally ionized before the copper constituting the copper particles, which is the conductive material, and the electron density in the arc space increases. Therefore, according to the electrical contact member, the force that moves electrons when the same current is passed, that is, the electric field strength, can be reduced compared to when the electron density in the arc space is low. Therefore, the electrical contact member can reduce electromagnetic noise without adding a large amount of zinc.
[0012] The brush has the electrical contact member, and therefore, in the brush, when an arc discharge occurs when a sliding contact is made between a commutator, which is a mating member, and a contact surface of the electrical contact member and separation is made, thermal ionization of the low ionization voltage metal occurs, increasing the electron density in the arc space, and making it possible to reduce electromagnetic noise.
[0013] The rotating machine has the brush, and therefore it is possible to eliminate the need for a filter constituted by a coil or a capacitor, a metallic shielding case, or the like, as a measure against electromagnetic noise, and therefore it is possible to achieve a reduction in size, weight, and cost of the rotating machine.
[0014] Note that the reference characters in parentheses in the claims indicate the corresponding relationship with the specific means described in the embodiments described later, and are not intended to limit the technical scope of the present disclosure. [Brief description of the drawings]
[0015] The above and other objects, features and advantages of the present disclosure will become more apparent from the following detailed description taken in conjunction with the accompanying drawings, in which: [Figure 1] FIG. 1 is a schematic diagram showing a brush according to a first embodiment to which the electrical contact member according to the first embodiment is applied; [Diagram 2] FIG. 2 is a schematic diagram illustrating a part of a scanning electron microscope image of a contact surface of the electrical contact member according to the first embodiment; [Diagram 3] FIG. 3 is an explanatory diagram for explaining an electric contact member and a brush of a third embodiment, in which (a) is a diagram showing an example of a spherical powder of a low ionization voltage metal used in the manufacture of the electric contact member and the brush of the third embodiment, and (b) is a diagram showing an example of a foil-shaped powder of a low ionization voltage metal used in the manufacture of the electric contact member and the brush of the third embodiment, [Figure 4] FIG. 4 is an explanatory diagram for explaining an electrical contact member and a brush according to a fourth embodiment, in which (a) is a diagram that shows a schematic diagram of low ionization voltage metal particles having no missing parts in an oxide film, and (b) is a diagram that shows a schematic diagram of a state in which a missing part is generated in an oxide film and low ionization voltage metal particles are partially metallically bonded to each other at the missing part, [Diagram 5] FIG. 5 is a cross-sectional view taken along an axial direction of a shaft of a rotating machine according to a fifth embodiment; [Figure 6] FIG. 6 is a diagram illustrating a brush and a commutator in a rotating machine according to a fifth embodiment; [Figure 7] FIG. 7 is a graph showing the relationship between temperature (K) and electron density (m-3) for each of the elements Cu, Al, and Zn obtained in Experimental Example 1; [Figure 8] FIG. 8 is a diagram showing filter voltage values (dB) for the brushes of Samples 1 to 4 obtained in Experimental Example 2; [Figure 9] FIG. 9 shows scanning electron microscope images of the contact surfaces of the brushes of samples 1 to 4 obtained in Experimental Example 2, where (a) is a scanning electron microscope image of sample 1, (b) is a scanning electron microscope image of sample 2, (c) is a scanning electron microscope image of sample 3, and (d) is a scanning electron microscope image of sample 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] (Embodiment 1) The electrical contact member and brush of the first embodiment will be described with reference to Figures 1 and 2. As illustrated in Figures 1 and 2, the electrical contact member 1 of the present embodiment has a contact surface 11 for facing a mating material (not shown in Figures 1 and 2). The electrical contact member 1 contains carbon particles 12, copper particles 13, and a low ionization voltage metal 14 having a lower ionization voltage than copper.
[0017] The electrical contact member 1 can be suitably used in applications where an arc is generated between the contact surface 11 and a mating material during use. The electrical contact member 1 can also be suitably used in applications where the contact surface 11 comes into sliding contact with the mating material during use. Specifically, the electrical contact member 1 can be used as, for example, a brush (electric brush) for a rotating machine such as a motor or a generator, an arc welding rod, or the like. The contact surface 11 may be in contact with the mating material or may be separated from the mating material.
[0018] FIG. 1 shows an example in which the electrical contact member 1 is applied to a brush 10 of a rotating machine (not shown in FIG. 1). The brush 10 of this embodiment has the electrical contact member 1 of this embodiment. Specifically, the brush 10 has a contact portion 101 having the electrical contact member 1 and a lead wire 102 connected to the contact portion 101. The lead wire 102 is sometimes called a pigtail, and is a portion through which electricity supplied from the outside flows. The brush 10 supplies power through a commutator to an armature coil wound around an iron core provided in a rotor of a rotating machine. In this case, the mating member is a commutator constituting a part of the rotor in the rotating machine, and the contact surface 11 is a surface that comes into sliding contact with the mating member and is separated. The contact portion 101 may be composed of the electrical contact member 1 as exemplified in FIG. 1, or may have a configuration including the electrical contact member 1 and a separate member that is connected to the electrical contact member 1 and is different from the electrical contact member 1, although not shown. An example of the latter is a case in which the electrical contact member 1 is formed as a surface layer on the surface of a separate member.
[0019] The electrical contact member 1 includes carbon particles 12, as exemplified in Fig. 2. The carbon particles 12 are useful particles for forming a lubricating film on a mating material and preventing fusion with the mating material when sliding contact and separation occurs between the mating material and the contact surface 11. From the viewpoints of the formability of the lubricating film, electrical conductivity, cost, material procurement, and the like, graphite particles can be exemplified as a suitable carbon particle 12.
[0020] 2, the electrical contact member 1 includes copper particles 13. The copper particles 13 are base particles of the electrical contact member 1, and are important particles for imparting electrical properties, such as electrical conductivity, to the electrical contact member 1.
[0021] As illustrated in FIG. 2, the electrical contact member 1 includes a low ionization voltage metal 14. The low ionization voltage metal 14 is a metal having a lower ionization voltage than copper. The low ionization voltage metal 14 is also a metal different from copper. The ionization voltage of copper is specifically 7.73 eV. Therefore, the low ionization voltage metal 14 is selected from metals having an ionization voltage lower than 7.73 eV. The lower the ionization voltage, the less thermal energy (J) is required for thermal ionization, and the more the electron density in the arc space can be increased.
[0022] Examples of the low ionization voltage metal 14 include Al (aluminum) (ionization voltage: 5.99 eV), Cr (chromium) (ionization voltage: 6.77 eV), Mg (magnesium) (ionization voltage: 7.65 eV), Rb (rubidium) (ionization voltage: 4.18 eV), and Ce (cesium) (ionization voltage: 3.89 eV). These can be used alone or in combination of two or more. The low ionization voltage metal 14 is preferably Al, Cr, etc., from the viewpoints that the ionization voltage is sufficiently lower than that of copper, it can exist as a solid at around room temperature, and the shape of the electrical contact member 1 can be maintained. These can be used alone or in combination of two or more. More preferably, the low ionization voltage metal 14 is Al, from the viewpoints that the ionization voltage is lower, the electron density can be increased by adding a small amount, the metal vapor is thermally ionized at a temperature lower than the boiling point of copper, and the electrical contact member 1 can be solidified by sintering when the electrical contact member 1 is fired (for example, when fired at a firing temperature of about 400°C to 1000°C). The melting points and boiling points of each metal are Al (melting point: 660°C, boiling point: 2467°C), Cr (melting point: 1857°C, boiling point: 2672°C), Mg (melting point: 639°C, boiling point: 1090°C), Rb (melting point: 39°C, boiling point: 688°C), and Ce (melting point: 29°C, boiling point: 678°C). The low ionization voltage metals 14 are not limited to single elements, and the same effect can be obtained even if they are contained as compounds (including thermal separation and thermal reduction).
[0023] The low ionization voltage metal 14 can be included in the electrical contact member 1 as particles of the low ionization voltage metal 14 (hereinafter, sometimes referred to as low ionization voltage metal particles 140), for example, as illustrated in FIG. 2. According to this configuration, the electrical contact member 1 can be manufactured relatively easily by molding and firing a mixed powder containing carbon powder, copper powder, and low ionization voltage metal powder. In addition to the above, the low ionization voltage metal 14 can also be included in the electrical contact member 1 as a coating layer (not shown) that covers the surfaces of the copper particles 13. In this case, the coating layer can be formed by vapor-depositing the low ionization voltage metal 14 on the surfaces of the copper particles 13, for example.
[0024] 2 specifically shows an example in which the electrical contact member 1 includes carbon particles 12, copper particles 13, and low ionization voltage metal particles 140. More specifically, the electrical contact member 1 can be made of a sintered body including a plurality of carbon particles 12, a plurality of copper particles 13, and a plurality of low ionization voltage metal particles 140.
[0025] The electrical contact member 1 may further include a low boiling point metal (not shown). The low boiling point metal is a metal having a boiling point lower than that of copper. According to this configuration, the low boiling point metal becomes a metal vapor at a temperature lower than the boiling point of copper, and the air in the arc space can be eliminated. Since nitrogen and oxygen contained in air are difficult to be thermally ionized, the air in the arc space is eliminated by the metal vapor of the low boiling point metal, and the thermal ionization of the low ionization voltage metal is promoted, and the electron density in the arc space can be easily increased. The boiling point of copper is specifically 2567°C. Therefore, the low boiling point metal can be selected from metals having a boiling point lower than 2567°C. The low boiling point metal is a metal different from the low ionization voltage metal 14, and as long as it has a boiling point lower than that of copper, the ionization voltage may be lower than that of nitrogen or oxygen and higher than that of copper.
[0026] Examples of low boiling point metals include Zn (zinc) (boiling point: 907°C, ionization voltage: 9.39 eV) and Mg (magnesium) (boiling point: 1090°C, ionization voltage: 7.65 eV). These can be used alone or in combination. Zn can be selected as the low boiling point metal because it has a lower boiling point and is easy to achieve the effect of removing air from the arc. Mg can be selected as the low boiling point metal because it has a lower boiling point than copper and a lower ionization voltage than copper, so that an increase in electron density due to thermal ionization can be expected.
[0027] The low boiling point metal can be contained as particles of the low boiling point metal (hereinafter, sometimes referred to as low boiling point metal particles) in the electrical contact member 1. According to this configuration, the electrical contact member 1 can be manufactured relatively easily by molding and firing a mixed powder containing carbon powder, copper powder, low ionization voltage metal powder, and low boiling point metal powder.
[0028] Although not shown, the electrical contact member 1 can specifically include, for example, carbon particles 12, copper particles 13, low ionization voltage metal particles 140, and low boiling point metal particles. In this case, more specifically, the electrical contact member 1 can be formed of a sintered body including a plurality of carbon particles 12, a plurality of copper particles 13, a plurality of low ionization voltage metal particles 140, and a plurality of low boiling point metal particles.
[0029] As illustrated in FIG. 2, the electrical contact member 1 can be configured such that, in a scanning electron microscope (hereinafter, sometimes referred to as SEM) image of the contact surface 11, the low ionization voltage metal 14 is present within the circle 3 no matter where the circle 3 having a diameter of 50 μm is placed on the SEM image. The circle 3 having a diameter of 50 μm is related to the arc bright spot diameter of the arc generated between the contact surface 11 and the mating material. The arc voltage varies depending on the material with which the arc bright spot is in contact. The above configuration promotes the reduction in particle size and uniform dispersion of the material constituting the electrical contact member 1. The above configuration is advantageous in suppressing the arc voltage fluctuation no matter where the arc is generated on the contact surface 11 or where the arc moves. In addition, the above configuration makes it easy to always have the low ionization voltage metal 14 that is within the arc bright spot diameter, regardless of the position or movement of the arc. Therefore, the above configuration can reliably cause the thermal ionization of the low ionization voltage metal 14 to occur regardless of the position or movement of the arc, and can increase the electron density in the arc space.
[0030] When the electrical contact member 1 contains a low boiling point metal, the electrical contact member 1 can be configured such that, in the SEM image of the contact surface 11, the low boiling point metal is present within the circle 3 no matter where the circle 3 is located on the SEM image. The above configuration promotes the reduction in particle size and uniform dispersion of the material constituting the electrical contact member 1. The above configuration is advantageous in suppressing the arc voltage fluctuation no matter where the arc occurs on the contact surface 11 or where the arc moves. In addition, the above configuration makes it easy to always have a low boiling point metal that is within the arc bright spot diameter, regardless of the position or movement of the arc. Therefore, the above configuration makes it possible to reliably generate metal vapor of the low boiling point metal regardless of the position or movement of the arc, and to eliminate the air in the arc space by the metal vapor of the low boiling point metal.
[0031] The above-mentioned configuration is satisfied by placing a circle 3 with a diameter of 50 μm on the SEM image of the contact surface 11, moving the circle 3 over the entire region of the SEM image, and confirming the presence of the low ionization voltage metal 14 or low boiling point metal that fits within the circle 3 at each position. When acquiring the SEM image, the contact surface 11 can be polished as necessary. The presence of the low ionization voltage metal 14 that fits within the circle 3 means the presence of the low ionization voltage metal 14 whose entire outline is within the circle 3. The presence of the low boiling point metal that fits within the circle 3 means the presence of the low boiling point metal whose entire outline is within the circle 3. In this case, the outline of the circle 3 that passes through the low ionization voltage metal 14 or the low boiling point metal (the outline of the circle 3 and the low ionization voltage metal 14 overlap, or the outline of the circle 3 and the low boiling point metal overlap) is excluded. When the low ionization voltage metal 14, low boiling point metal is contained in the electrical contact member 1 as particles, the outer contour of the low ionization voltage metal particles 140, low boiling point metal particle outer contour.
[0032] As shown in Fig. 2, the electrical contact member 1 can be configured such that, in an SEM image of the contact surface 11, no matter where a circle 3 having a diameter of 50 µm is placed, there are carbon particles 12 that fit within the circle 3. This configuration promotes the reduction in particle size and uniform dispersion of the material that constitutes the electrical contact member 1. This configuration is advantageous in suppressing arc voltage fluctuations no matter where an arc occurs on the contact surface 11 or where the arc moves.
[0033] As illustrated in FIG. 2, the electrical contact member 1 can be configured such that, in an SEM image of the contact surface 11, no matter where a circle 3 having a diameter of 50 μm is placed on the SEM image, there are copper particles 13 that fit within the circle 3. This configuration promotes the reduction in particle size and uniform dispersion of the material that constitutes the electrical contact member 1. This configuration is advantageous in suppressing arc voltage fluctuations no matter where an arc occurs on the contact surface 11 or where the arc moves. The carbon particles 12 that fit within the circle 3 and the copper particles 13 that fit within the circle 3 can be understood by applying mutatis mutandis the above explanation of the low ionization voltage metal 14 that fits within the circle 3.
[0034] Specifically, FIG. 2 shows an example in which the electrical contact member 1 includes carbon particles 12 that fit within the circle 3, copper particles 13 that fit within the circle 3, and low ionization voltage metal particles 140 that fit within the circle 3, regardless of the position of the circle 3 on the SEM image of the contact surface 11. Although not shown, the electrical contact member 1 may further include low boiling point metal particles that fit within the circle 3. In these cases, the particle sizes of the materials constituting the electrical contact member 1 (carbon particles 12, copper particles 13, low ionization voltage metal particles 140, low boiling point metal particles, etc.) are reduced and uniformly dispersed. When the electrical contact member 1 is applied to a brush, for example, when the contact surface 11 of the electrical contact member 1 is in sliding contact with a mating material, the contact surface 11 is worn by the sliding contact, and the arc generation position is likely to be in a different position. Therefore, in the above case, even when the contact surface 11 is in sliding contact with the mating material, the arc voltage fluctuation can be suppressed regardless of the position and movement of the arc.
[0035] In the electrical contact member 1, the size of the low ionization voltage metal 14 can be equal to or less than half the diameter of the circle 3. Furthermore, when the electrical contact member 1 contains a low boiling point metal, the size of the low boiling point metal can be equal to or less than half the diameter of the circle 3. With these configurations, it becomes easier to suppress arc voltage fluctuations regardless of the position and movement of the arc.
[0036] The size of the low ionization voltage metal 14 and the low boiling point metal can be preferably, from the viewpoint of ensuring the above-mentioned action effects, not more than 2 / 5 of the diameter of the circle 3, more preferably not more than 3 / 10 of the diameter of the circle 3, even more preferably not more than 1 / 5 of the diameter of the circle 3, and even more preferably not more than 1 / 10 of the diameter of the circle 3.
[0037] The above-mentioned configuration is satisfied by placing a size confirmation circle (not shown) having a predetermined diameter on the SEM image of the contact surface 11 relative to the circle 3 having a diameter of 50 μm, moving the size confirmation circle over the entire region of the SEM image, and confirming that the low ionization voltage metal 14 and the low boiling point metal are contained within the size confirmation circle at each position. The low ionization voltage metal 14 being contained within the size confirmation circle means that the entire outline of each low ionization voltage metal 14 is contained within the size confirmation circle. The low boiling point metal being contained within the size confirmation circle means that the entire outline of each low boiling point metal is contained within the size confirmation circle. In this case, the outline of the size confirmation circle that passes over the low ionization voltage metal 14 or the low boiling point metal (the outline of the size confirmation circle and the low ionization voltage metal 14 overlap, or the outline of the size confirmation circle and the low boiling point metal overlap) is excluded. When the low ionization voltage metal 14, low boiling point metal is contained in the electrical contact member 1 as particles, the size of the low ionization voltage metal particle 140, low boiling point metal particle is the particle size of the low ionization voltage metal particle 140, low boiling point metal particle.
[0038] In FIG. 2, specifically, the particle diameter of each of the carbon particles 12, the copper particles 13, and the low ionization voltage metal particles 140 can be set to 1 / 2 or less of the diameter of the circle 3. Although not shown, when the electrical contact member 1 further includes low boiling point metal particles that fit within the circle 3, the particle diameter of the low boiling point metal particles can be set to 1 / 2 or less of the diameter of the circle 3. In addition, from the viewpoint of ensuring the above-mentioned action and effect, each particle diameter of the carbon particles 12, the copper particles 13, the low ionization voltage metal particles 140, and the low boiling point metal particles can be preferably set to 2 / 5 or less of the diameter of the circle 3, more preferably 3 / 10 or less of the diameter of the circle 3, even more preferably 1 / 5 or less of the diameter of the circle 3, and even more preferably 1 / 10 or less of the diameter of the circle 3, from the viewpoint of ensuring the above-mentioned action and effect. In addition, the particle diameter of the carbon particles 12 and the copper particles 13 can be understood by applying mutatis mutandis the explanation of the size of the low ionization voltage metal 14 and the low boiling point metal.
[0039] In the electrical contact member 1, the content of the carbon particles 12 can be selected from the range of 25% by mass to 85% by mass from the viewpoint of effectively suppressing fusion between the contact surface 11 and the mating material when the contact surface 11 is brought into sliding contact with the mating material. The content of the copper particles 13 can be selected from the range of 15% by mass to 75% by mass from the viewpoint of electrical properties such as electrical conductivity of the electrical contact member 1. The content of the low ionization voltage metal 14 can be selected from the range of 2% by mass to 75% by mass from the viewpoint of ensuring the effect of the addition, suppressing the deterioration of electrical and mechanical bonds, and raw material costs. The content of the low boiling point metal can be selected from the range of 2% by mass to 30% by mass from the viewpoint of ensuring the effect of the addition, suppressing the increase of an insulating oxide film, and the like. The above mass % is selected so that the total is 100% by mass.
[0040] In the electrical contact member 1 of this embodiment, when an arc discharge occurs between the contact surface 11 and the mating material, the low ionization voltage metal 14 is thermally ionized prior to the copper constituting the copper particles 13, which is a conductive material, and the electron density in the arc space increases. Therefore, according to the electrical contact member 1 of this embodiment, the force that moves electrons when the same current is passed, that is, the electric field strength, can be reduced compared to when the electron density in the arc space is low. Therefore, the electrical contact member 1 of this embodiment can reduce electromagnetic noise without adding a large amount of zinc.
[0041] The brush 10 of this embodiment has the electrical contact member 1 of this embodiment. Therefore, in the brush 10 of this embodiment, during arc discharge when sliding contact and separation occur between a commutator, which is a mating material, and the contact surface 11 of the electrical contact member 1, thermal ionization of the low ionization voltage metal 14 occurs, increasing the electron density in the arc space, and making it possible to reduce electromagnetic noise.
[0042] (Embodiment 2) A description will be given of an electrical contact member and a brush according to embodiment 2. Of the symbols used in embodiment 2 and onwards, the same symbols as those used in the previous embodiments represent the same components, etc. as those in the previous embodiments, unless otherwise specified.
[0043] In the electrical contact member 1 of the present embodiment, some or all of the copper particles 13 are replaced with replacement particles (not shown) made of a metal other than copper. That is, in the electrical contact member 1 of the present embodiment, at least some of the copper particles 13 are replaced with replacement particles.
[0044] Examples of the replacement particles include Al particles and Cr particles. When the replacement particles are Al particles, they have the advantages of being lightweight, low cost, easy to procure materials, and low risk of depletion. When the replacement particles are Cr particles, they have the advantages of increased mechanical strength and improved wear resistance.
[0045] In addition, when the replacement particles are Al particles, or the metal constituting the replacement particles can function as a low ionization voltage metal, the electrical contact member 1 can be configured to include, for example, carbon particles 12, copper particles 13, and replacement particles, or to include carbon particles 12 and replacement particles.
[0046] Moreover, the brush 10 of this embodiment has the electrical contact member 1 of this embodiment.
[0047] The description of the copper particles in the first embodiment can be applied mutatis mutandis to the description of the replacement particles. Other configurations and effects are the same as those in the first embodiment.
[0048] (Embodiment 3) The electrical contact member and the brush of the third embodiment will be described with reference to Fig. 3. In the electrical contact member 1 of the third embodiment, the low ionization voltage metal 14 is composed of spherical particles or foil-like particles. Fig. 3(a) is a diagram showing an example of a spherical powder of the low ionization voltage metal 14 used in the manufacture of the electrical contact member 1 and the brush 10 (described later) of the third embodiment, and Fig. 3(b) is a diagram showing an example of a foil-like powder of the low ionization voltage metal 14 used in the manufacture of the electrical contact member 1 and the brush 10 (described later) of the third embodiment. The material of the spherical powder and the foil-like powder of the low ionization voltage metal 14 exemplified in Fig. 3 is specifically Al.
[0049] When the low ionization voltage metal 14 is composed of spherical particles, a mixed powder containing carbon powder for containing the carbon particles 12 and spherical powder of the low ionization voltage metal 14 for containing the low ionization voltage metal 14 composed of spherical particles is prepared during the manufacture of the electrical contact member 1. Since the spherical powder of the low ionization voltage metal 14 has excellent uniform dispersibility with the carbon powder, the above configuration provides an electrical contact member 1 having excellent uniform dispersibility of the carbon particles 12 and the low ionization voltage metal 14 composed of spherical particles. The spherical powder of the low ionization voltage metal 14 can be prepared, for example, by using an atomization method.
[0050] On the other hand, when the low ionization voltage metal 14 is made of foil-like particles, there are the following advantages. As described above, when the low ionization voltage metal 14 is made of spherical particles, the spherical particles have less contact with each other and the surfaces of the spherical particles are smoother than when the low ionization voltage metal 14 is made of foil-like particles, so that the mechanical and electrical bonding forces are small, and the spherical particles may fall off during sliding, which may increase the electrical resistance of the electrical contact member 1. On the other hand, when the low ionization voltage metal 14 is made of foil-like particles, the foil particles are easily entangled with each other, so that the mechanical and electrical bonding forces are improved, and the foil particles are less likely to fall off during sliding, making it possible to suppress an increase in the electrical resistance of the electrical contact member 1. As the foil-like powder of the low ionization voltage metal 14 used in manufacturing the electrical contact member 1, for example, a powder obtained by pulverizing the foil of the low ionization voltage metal 14 (foil pulverized powder) can be suitably used.
[0051] The shape of the low ionization voltage metal 14 contained in the electrical contact member 1 can be identified by observing the cross-sectional cut surface of the electrical contact member 1 using an SEM or the like. The spherical particles have a perfectly circular or elliptical outer shape. On the other hand, the corners of the foil-like particles do not have a perfectly circular or elliptical outer shape. Therefore, the two types of particles can be relatively easily distinguished from each other. The other configurations and effects are the same as those of the electrical contact members 1 of the first and second embodiments.
[0052] The brush 10 of this embodiment has the electrical contact member 1 of this embodiment. Therefore, when the electrical contact member 1 has the low ionization voltage metal 14 composed of spherical particles, the brush 10 has excellent uniform dispersion of the carbon particles 12 and the low ionization voltage metal 14 composed of spherical particles. Also, when the electrical contact member 1 has the low ionization voltage metal 14 composed of foil-like particles, the foil-like particles are less likely to fall off during sliding, and the brush 10 can be obtained in which an increase in electrical resistance due to this is suppressed. The other configurations and effects are the same as those of the brush 10 of the first and second embodiments.
[0053] (Embodiment 4) The electrical contact member and brush of the fourth embodiment will be described with reference to Fig. 4. As illustrated in Fig. 4, in the electrical contact member 1 of the fourth embodiment, the low ionization voltage metal 14 is contained in the electrical contact member 1 as particles of the low ionization voltage metal 14 (low ionization voltage metal particles 140). In the electrical contact member 1 including the low ionization voltage metal particles 140, the microstructure of the low ionization voltage metal particles 140 can be at least one of the microstructures illustrated in Fig. 4(a) and Fig. 4(b). A specific description will be given below.
[0054] In Fig. 4(a), the entire surface of the low ionization voltage metal particle 140 is covered with an oxide film 141. No missing portion 141a is formed in the oxide film 141, and no partial metallic bonding occurs between the low ionization voltage metal particles 140. The electrical contact member 1 having the microstructure exemplified in Fig. 4(a) can be manufactured, for example, by firing the electrical contact member 1 at a temperature not exceeding the melting point of the low ionization voltage metal 14 (at which deformation does not occur) during firing. When the low ionization voltage metal 14 is, for example, Al, the melting point of Al is about 660°C.
[0055] On the other hand, in FIG. 4(b), for example, the low ionization voltage metal 14 is sintered at a temperature exceeding the melting point thereof, causing deformation of the particles due to melting. The surface of the low ionization voltage metal particle 140 is covered with an oxide film 141. However, the oxide film 141 has a partial defect 141a, and the low ionization voltage metal particles 140 are partially metal-bonded to each other at the defect 141a. Specifically, the metal bond may be, for example, fusion bonding. As illustrated in FIG. 4(b), the low ionization voltage metal particle 140 may include an oxide film 141 having no defect 141a. The electrical contact member 1 having the microstructure illustrated in FIG. 4(b) may be manufactured, for example, by sintering the electrical contact member 1 at a temperature equal to or higher than the melting point of the low ionization voltage metal 14. In the electrical contact member 1 having the microstructure as exemplified in FIG. 4(b), the mechanical and electrical bonding forces are improved due to partial metal bonding between the low ionization voltage metal particles 140, and the low ionization voltage metal particles 140 are less likely to fall off during sliding, making it possible to suppress an increase in the electrical resistance of the electrical contact member 1. In particular, when the material of the low ionization voltage metal particles 140 is Al, a thin oxide film 141 (for example, about 5 nm) is likely to be formed on the surface of the low ionization voltage metal particles 140 during firing. The oxide film 141 reduces the mechanical bonding force between the particles and is insulating, leading to an increase in the electrical resistance. Therefore, according to the electrical contact member 1 having the microstructure as exemplified in FIG. 4(b), it is possible to fully exert the effect of partial metal bonding between the low ionization voltage metal particles 140 at the missing parts 141a of the oxide film 141. The density of the partial metal joint may vary, for example, in the depth direction of the electrical contact member 1. This is because, during manufacturing, the firing temperature may vary in the depth direction of the electrical contact member 1.
[0056] The microstructure of the low ionization voltage metal particles 140 in the electrical contact member 1 can be understood by subjecting a cross-sectional cut surface of the electrical contact member 1 to EPMA (X-ray element mapping) analysis and checking for the presence or absence of missing parts 141a in the oxide film 141 that the low ionization voltage metal particles 140 have on their surfaces. If missing parts 141a are present in the oxide film 141, it can be said that metallic bonding has occurred between the low ionization voltage metal particles 140. The other configurations and effects are the same as those of the electrical contact members 1 in the first and second embodiments.
[0057] The brush 10 of this embodiment has the electrical contact member 1 of this embodiment. In particular, in the electrical contact member 1, when a missing portion 141a occurs in the oxide film 141 on the surface of the low ionization voltage metal particles 140 and the low ionization voltage metal particles 140 are partially metallically bonded to each other at the missing portion 141a, the low ionization voltage metal particles 140 are unlikely to fall off each other during sliding, and thus a brush 10 is obtained that can suppress an increase in electrical resistance due to this. The other configurations and effects are the same as those of the brush 10 of the first and second embodiments.
[0058] (Embodiment 5) A rotating machine of the fifth embodiment will be described with reference to Figs. 5 and 6. As illustrated in Figs. 5 and 6, the rotating machine 2 of this embodiment has the brush 10 of the first embodiment. Specifically, the rotating machine 2 is a rotating electric machine, and more specifically, is configured as a brushed DC motor. The rotating machine 2 can be used as a driving motor for various devices, such as a driving motor for an in-vehicle device, a driving motor for a household electric appliance, and a driving motor for a general industrial machine. The rotating machine 2 may be configured as an electric motor, or as a motor generator having both the functions of an electric motor and a generator.
[0059] In this embodiment, unless otherwise specified, the axial direction of the shaft 20 constituting the rotating machine 2 is indicated by an arrow X, and the radial direction of the shaft 20 is indicated by an arrow Y. Moreover, the rotation direction, which is one of the circumferential directions of the shaft 20, is indicated by an arrow Za.
[0060] The rotating machine 2 includes a cylindrical shaft 20 that is a rotating shaft, and is configured so that the shaft 20 is rotationally driven by power supplied from a power source E. The rotating machine 2 includes a housing 22 that is composed of a case 23 and a cover 24, and a plurality of components for rotationally driving the shaft 20, and these plurality of components are accommodated within the housing 22. The plurality of components include a plurality of support parts 25 that rotatably support the shaft 20, a rotor 220 as a rotor, a commutator 231, two brushes 10, 10, and a magnet 240 as a stator.
[0061] Rotor 220 is fixed to shaft 20. Rotor 220 has an iron core 221 formed by laminating a plurality of electromagnetic steel plates, and an armature coil 222, and armature coil 222 is wound around iron core 221.
[0062] Magnet 240 is fixed to the inner surface of case 23 constituting housing 22 with a gap between it and rotor 220. Magnet 240 has a function of providing a field magnet to armature coil 222, and is configured as a permanent magnet for the field magnet having mutually different polarities (south pole and north pole).
[0063] The commutator 231 has a plurality of commutator segments 232 and is electrically connected to the armature coils 222. As shown in Fig. 6, in the commutator 231, the plurality of commutator segments 232 are arranged side by side in the circumferential direction of the shaft 20. Adjacent commutator segments 232 are spaced apart from each other in the circumferential direction and are electrically connected to each other by the armature coils 222.
[0064] Both brushes 10 are rectangular brushes that are electrically connected to a power source E and come into sliding contact with a plurality of commutator segments 232 as the commutator 231 rotates. One of the brushes, the first brush 10, is electrically connected to the positive terminal of the power source E. The other brush, the second brush 10, is electrically connected to the negative terminal of the power source E and is configured to be paired with the first brush 10. The two brushes 10 are disposed at positions shifted by 180° in the circumferential direction. For this reason, the first brush 10 can also be called the "positive brush" and the second brush 10 can also be called the "negative brush."
[0065] The first brush 10 is capable of sliding contact with and separation from the multiple commutator segments 232, and when the first brush 10 makes sliding contact with or separates from the multiple commutator segments 232, its potential becomes higher relative to the multiple commutator segments 232. The second brush 10 is capable of sliding contact with and separation from the multiple commutator segments 232, and when the first brush 10 makes sliding contact with or separates from the multiple commutator segments 232, its potential becomes lower relative to the multiple commutator segments 232. In this manner, each of the multiple commutator segments 232 can be on the high potential side or the low potential side depending on the sliding contact relationship with the two brushes 10. In this embodiment, both of the two brushes 10 are configured using the electrical contact member 1.
[0066] The rotating machine 2 of this embodiment has the brush 10 of the first embodiment. Therefore, the rotating machine 2 of this embodiment can eliminate the need for a filter constituted by a coil, a capacitor, etc., a metallic shielding case, etc., as a measure against electromagnetic noise. Therefore, according to the rotating machine 2 of this embodiment, it is possible to reduce the size, weight, and cost of the rotating machine 2.
[0067] In this embodiment, the input power of the rotating machine 2 is not particularly limited, but may be, for example, 10 W or more and 800 W or less. In this case, the effect of the above-mentioned electrical contact member 1 can be fully exhibited in relation to the size of the arc bright spot diameter of the arc formed between the electrical contact member 1 of the brush and the commutator 231.
[0068] In this embodiment, the rotating machine 2 has the brush 10 of the first embodiment. However, the rotating machine 2 may have the brush 10 having the electrical contact member 1 of the second to fourth embodiments.
[0069] (Experimental Example 1) For each element of Cu (ionization voltage: 7.72 eV), Al (ionization voltage: 5.99 eV), and Zn (ionization voltage: 9.39 eV), the temperature and the 1 m 3 The relationship between the temperature (K) and the electron density (defined as the number of thermally ionized electrons per unit mass) was determined by simulation. In this simulation, it was assumed that the elements Cu, Al, and Zn were all gasified (vaporized) at atmospheric pressure, regardless of temperature. In this case, each element was assumed to be in a 100% metallic gas state, with no air (N2, O2) mixed in. Furthermore, the electron density was determined by calculating the number of electrons ionized from the thermal ionization energy for each element. Figure 7 shows the relationship between temperature (K) and electron density (m -3 In this experimental example, a small brushed DC motor with an input power of about 50 W was assumed, and the arc discharge temperature was set to 4000 K (Kelvin).
[0070] According to FIG. 7, the following can be seen. Each of the elements Cu, Al, and Zn is almost 100% ionized (electron density is saturated) at temperatures above 10,000 K (9,727 °C). Zn has a higher ionization voltage than Cu. On the other hand, Al has a lower ionization voltage than Cu. At an arc discharge temperature of about 4,000 K, Al can increase the electron density in the arc space compared to Zn. From this, it can be said that by using Al instead of Zn in an electrical contact member containing copper particles, that is, by using a low ionization voltage metal such as Al, which has a lower ionization voltage than Cu, when an arc discharge occurs between the contact surface and the mating material, thermal ionization of the low ionization voltage metal occurs prior to copper constituting the copper particles, which is a conductive material, and it is possible to increase the electron density in the arc space. Therefore, according to such an electrical contact member, compared to a case where the electron density in the arc space is low, the force that moves electrons when the same current flows, that is, the electric field strength, can be reduced, and it can be said that it is possible to reduce electromagnetic noise without adding a large amount of zinc.
[0071] (Experimental Example 2) Cu (copper) powder with an average particle size of 50 μm and C (graphite) powder with an average particle size of 5 μm were blended in a mass ratio of 50:50 (volume ratio of about 20:80), and stirred and mixed. The mixed powder obtained was then compression molded in a mold. The compression molded body obtained was then sintered in a deoxidized atmosphere at a temperature at which the components would not be thermally changed, and baked to harden it. In this way, the brush of sample 1 was produced. The average particle size of the raw material powder refers to the particle size at which the volume integrated value in the particle size distribution obtained by the laser diffraction / scattering method is 50% (the same applies below).
[0072] A brush of Sample 2 was prepared in the same manner as in the preparation of the brush of Sample 1, except that the ingredients were stirred and mixed so as to improve uniform dispersion.
[0073] The brush of sample 3 was produced in the same manner as in producing the brush of sample 1, except that Cu powder with an average particle size of 20 μm and C powder with an average particle size of 5 μm were mixed in a mass ratio of 50:50 (volume ratio of approximately 20:80).
[0074] The brush of sample 4 was produced in the same manner as in producing the brush of sample 1, except that Cu powder with an average particle size of 2 μm and C powder with an average particle size of 5 μm were mixed in a mass ratio of 50:50 (volume ratio of approximately 20:80).
[0075] The voltage waveform between the electrical contacts was captured in a sliding electrical contact circuit equivalent to an actual motor using each brush, and the filtered voltage value (magnitude of the voltage waveform) after a 250 MHz bandpass filter was measured. The magnitude of the filtered voltage value varies depending on the contact state, so there is a range. Therefore, data measurement was repeated with the same settings to determine the upper limit, lower limit, and average value of the filtered voltage value. For each sample, two samples were taken and four repetitions were taken, so n=8. Figure 8 shows the filtered voltage values (dB) for the brushes of Samples 1 to 4. Figure 9 shows SEM images of the contact surfaces of the brushes of Samples 1 to 4. In Figure 9, the white parts are Cu and the gray parts are C.
[0076] 8 and 9, the following can be seen. As shown in FIG. 8 and FIG. 9, in the brush of sample 1, when a circle with a diameter of 50 μm is placed on the SEM image, the material particles (here, Cu particles and C particles) constituting the electrical contact member are not present within the circle. Therefore, the width of the filter voltage value of the brush of sample 1 is large. Therefore, it can be said that the brush of sample 1 cannot suppress the arc voltage fluctuation regardless of the position and movement of the arc. The same is true for the brush of sample 2. Note that the brush of sample 2 has the same raw material particle size as the brush of sample 1, but only the dispersibility is improved. In contrast, in the brushes of sample 3 and sample 4, when a circle with a diameter of 50 μm is placed at any position on the SEM image, the material particles constituting the electrical contact member are present within the circle. Therefore, the brushes of sample 3 and sample 4 have a narrower width of the filter voltage value due to the small particle size and uniform dispersion of the material particles. From this result, it can be said that the brushes of sample 3 and sample 4 can suppress the arc voltage fluctuation regardless of the position and movement of the arc. Also, comparing the brushes of Samples 1 to 4, it can be seen that the smaller the particle size of the material is and the more uniformly dispersed it is, the smaller the range of the filter voltage value becomes, and the easier it is to suppress the arc voltage fluctuation. It can also be seen that by making the particle size of the material particles 1 / 2 or less of the diameter of the circle, it becomes easier to ensure that the material particles are contained within the circle.
[0077] (Experimental Example 3) Cu (copper) powder with an average particle size of 5 μm, C (graphite) powder with an average particle size of 10 μm, and Al (aluminum) powder with an average particle size of 5 μm were mixed in a mass ratio of 50:45:5, and stirred and mixed using a ball mill. The mixed powder obtained was then compression molded in a mold. The compression molded body obtained was then sintered in a deoxidized atmosphere at a temperature at which the components would not change due to heat, and baked to harden it. In this way, the brush of Sample 6 was obtained. The brush of Sample 6 contains Al particles as low ionization voltage metal particles.
[0078] Cu (copper) powder with an average particle size of 5 μm, C (graphite) powder with an average particle size of 10 μm, Al (aluminum) powder with an average particle size of 5 μm, and Zn (zinc) powder with an average particle size of 5 μm were blended in a mass ratio of 50:40:5:5, and stirred and mixed using a ball mill. The mixed powder obtained was then compression molded in a mold. The compression molded body obtained was then fired in a deoxidized atmosphere at a temperature at which the components do not change due to heat, and baked to harden. This resulted in the brush of Sample 7. The brush of Sample 7 contains Al particles as low ionization voltage metal particles and Zn particles as low boiling point particles.
[0079] The present disclosure is not limited to the above-mentioned embodiments and experimental examples, and various modifications are possible within the scope of the gist of the disclosure. That is, although the present disclosure has been described in accordance with the embodiments, it is understood that the present disclosure is not limited to the embodiments, structures, etc. The present disclosure also includes various modifications and modifications within the equivalent range. In addition, various combinations and forms, and further other combinations and forms including only one element, more than one element, or less than one element, are also within the scope and concept of the present disclosure. In addition, the configurations and effects shown in each embodiment, each experimental example, and the following reference form can be arbitrarily combined with each other.
[0080] An example of the first embodiment is given below. [1] It has a contact surface (11) for facing a mating material, Carbon particles (12); Copper particles (13); A low ionization voltage metal (14) that has a lower ionization voltage than copper; An electrical contact member (1). [2] In the scanning electron microscope image of the contact surface, No matter where the 50 μm diameter circle (3) is placed on the scanning electron microscope image, The electrical contact member according to [1], wherein the low ionization voltage metal is present within the circle. [3] The electrical contact member according to [2], wherein the size of the low ionization voltage metal is equal to or less than half the diameter of the circle. [4] The electrical contact member according to any one of [1] to [3], wherein the low ionization voltage metal is at least one metal selected from the group consisting of Al and Cr. [5] The electrical contact member according to any one of [1] to [4], further comprising a low-boiling point metal having a boiling point lower than that of copper. [6] The electrical contact member according to [5], wherein the low boiling point metal is at least one metal selected from the group consisting of Zn and Mg. [7] A part or all of the copper particles are replaced with replacement particles composed of a metal other than copper. An electrical contact member according to any one of [1] to [6]. [8] A brush (10) having an electrical contact member according to any one of [1] to [7]. [9] A rotating machine (2) having a brush according to [8]. Also, Below Second An example of the reference form is given below. [Section 1] An electrical contact member having a contact surface for facing a mating member, In the scanning electron microscope image of the contact surface, No matter where a circle with a diameter of 50 μm is placed on the scanning electron microscope image, The material particles constituting the electrical contact member are present within the circle. Electrical contact components. According to the electrical contact member of the above item 1, the material particles constituting the electrical contact member 1 can be made small and uniformly dispersed. Therefore, according to the electrical contact member of the above item 1, the problem of suppressing the arc voltage fluctuation can be solved even if an arc occurs at any position on the contact surface or the arc moves. [Section 2] Item 2. The electrical contact member according to item 1, wherein the particle size of the material particles is equal to or less than half the diameter of the circle. According to the electrical contact member of item 2 above, it is possible to reliably ensure that the material particles constituting the electrical contact member are contained within the circle. [Section 3] the material particles include copper particles; Item 3. The electrical contact member according to item 1 or 2, wherein the copper particles have a particle size of ½ or less of the diameter of the circle. [Section 4] The material particles include low ionization voltage metal particles having a lower ionization voltage than copper, 4. The electrical contact member according to any one of items 1 to 3, wherein the particle size of the low ionization voltage metal particles is equal to or less than half the diameter of the circle. [Section 5] Item 5. The electrical contact member according to item 4, wherein the metal constituting the low ionization voltage metal particles is at least one metal selected from the group consisting of Al and Cr. [Section 6] The material particles include low-boiling point metal particles having a boiling point lower than that of copper, 6. The electrical contact member according to any one of items 1 to 5, wherein the particle diameter of the low-boiling point metal particles is equal to or less than half the diameter of the circle. [Section 7] Item 7. The electrical contact member according to item 6, wherein the metal constituting the low-boiling point metal particles is at least one metal selected from the group consisting of Zn and Mg. [Section 8] the material particles include carbon particles, 8. The electrical contact member according to any one of items 1 to 7, wherein the carbon particles have a particle size of ½ or less than a diameter of the circle. [Section 9] A part or all of the copper particles are replaced with replacement particles composed of a metal other than copper. Item 4. An electrical contact member according to item 3. [Section 10] Item 10. A brush having the electrical contact member according to any one of items 1 to 9. According to the brush of item 10, a brush capable of suppressing arc voltage fluctuations regardless of the position or movement of the arc can be obtained. [Section 11] Item 11. A rotating machine having the brush according to item 10. According to the rotating machine of item 11, a rotating machine having a brush capable of suppressing arc voltage fluctuations regardless of the position or movement of the arc can be obtained.
Claims
1. It has a contact surface (11) for facing a mating material, The portion having the contact surface includes carbon particles (12), copper particles (13), and a low ionization voltage metal (14) having an ionization voltage lower than that of copper, The low ionization voltage metal is contained as low ionization voltage metal particles, or as a coating layer covering the surfaces of the copper particles, In the scanning electron microscope image of the contact surface, No matter where the 50 μm diameter circle (3) is placed on the scanning electron microscope image, There is a low ionization voltage metal that falls within the circle. An electrical contact member (1).
2. 2. The electrical contact member according to claim 1, wherein the size of the low ionization voltage metal is equal to or smaller than half the diameter of the circle.
3. 3. The electrical contact member according to claim 1, wherein the low ionization voltage metal is at least one metal selected from the group consisting of Al and Cr.
4. 3. The electrical contact member according to claim 1, further comprising a low-boiling point metal having a boiling point lower than that of copper.
5. 5. The electrical contact member according to claim 4, wherein the low boiling point metal is at least one metal selected from the group consisting of Zn and Mg.
6. A part or all of the copper particles are replaced with replacement particles composed of a metal other than copper. The electrical contact member according to claim 1 or 2.
7. A brush (10) having an electrical contact member according to claim 1 or 2.
8. A rotating machine (2) comprising a brush according to claim 7.
Citation Information
Patent Citations
Preparation method of composite contact material for high-breaking-capacity low-voltage electric appliance
CN111575527A
TFT equipment
JP1988081860A
Sintered composite material for electric contact and sintered pad using the same
JP1988293132A
Copper paste
JP1996031229A
Copper-carbon brush and its manufacturing method
JP2001327127A