Laser diode manufacturing method and laser diode

The manufacturing method for laser diodes with reduced dislocation density and improved carrier injection efficiency addresses the high internal loss issue in conventional ultraviolet laser diodes, enabling lower oscillation threshold currents for continuous operation.

JP7589940B2Active Publication Date: 2024-11-26ASAHI KASEI KOGYO KABUSHIKI KAISHA +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021051841
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-25
Publication Date
2024-11-26
Estimated Expiration
2041-03-25

AI Technical Summary

Technical Problem

Conventional ultraviolet laser diodes have high internal losses, making it difficult to reduce the oscillation threshold current, which is necessary for achieving continuous oscillation.

Method used

A method for manufacturing a laser diode involving the formation of a semiconductor laminated structure with a mesa structure and specific conductivity type cladding layers, followed by electrode deposition and localized heating to reduce dislocation density and improve carrier injection efficiency.

Benefits of technology

The method results in a laser diode with a significantly lower oscillation threshold current, enhancing continuous oscillation capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589940000002
    Figure 0007589940000002
  • Figure 0007589940000003
    Figure 0007589940000003
  • Figure 0007589940000004
    Figure 0007589940000004
Patent Text Reader

Abstract

To provide a laser diode of a low oscillation threshold current.SOLUTION: A laser diode comprises an Al containing nitride semiconductor substrate, and a semiconductor laminate part disposed on the nitride semiconductor substrate. The semiconductor laminate part includes: a first conductivity type clad layer disposed on the substrate and including a nitride semiconductor layer of a first conductivity type; a light-emitting layer disposed on the first conductivity type clad layer and formed from a nitride semiconductor including one or more quantum wells; and a second conductivity type clad layer disposed on the light-emitting layer and including a nitride semiconductor layer of a second conductivity type. At least a portion of the semiconductor laminate part is a mesa structure for light resonance and emission and includes a plurality of dislocation lines extending in a crystal orientation <1-100> direction of the nitride semiconductor substrate only within a first region where a distance L from a side face of the mesa structure is shorter than 15 μm, in the mesa structure including the first conductivity type clad layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a laser diode and to a laser diode. [Background technology]

[0002] Conventionally, nitride semiconductors have been used as materials for forming laser diodes. Nitride semiconductors have a direct transition recombination mode, and therefore are suitable as materials for laser diodes in that they can provide high recombination efficiency and high optical gain. As an example of a laser diode using such a nitride semiconductor, a technology for oscillating a current injection type laser diode in the ultraviolet region has been disclosed (for example, Non-Patent Document 1). [Prior art documents] [Non-patent literature]

[0003] [Non-Patent Document 1] Zhang et al., Applied Physics Express 12, 124003(2019) Summary of the Invention [Problem to be solved by the invention]

[0004] The above-mentioned ultraviolet laser diode is pulse driven, and continuous oscillation is required for practical applications. This continuous oscillation requires a reduction in the oscillation threshold current, but conventional laser diodes have large internal losses, making it difficult to reduce the oscillation threshold current.

[0005] An object of the present disclosure is to provide a manufacturing method for a laser diode having a low oscillation threshold current, and the laser diode. [Means for solving the problem]

[0006] In order to solve the above-mentioned problems, a manufacturing method of a laser diode according to an embodiment of the present disclosure includes forming a first-conductivity-type cladding layer including a first-conductivity-type nitride semiconductor layer on a nitride semiconductor substrate including Al, forming a light-emitting layer of a nitride semiconductor structure including one or more quantum wells on the first-conductivity-type cladding layer, forming a second-conductivity-type cladding layer including a second-conductivity-type nitride semiconductor layer on the light-emitting layer to form a semiconductor laminate, etching the semiconductor laminate so as to expose a portion of the first-conductivity-type cladding layer to form a mesa structure having a resonator, depositing an electrode material on each of the first-conductivity-type cladding layer and the second-conductivity-type cladding layer exposed by etching to form contact electrodes, and heat-treating the contact electrodes by an infrared lamp at a temperature of 550° C. or more and 700° C. or less for 70 seconds or less.

[0007] Furthermore, a manufacturing method of a laser diode according to another embodiment of the present disclosure includes forming a first-conductivity-type cladding layer including a first-conductivity-type nitride semiconductor layer on a nitride semiconductor substrate including Al, forming a light-emitting layer of a nitride semiconductor structure including one or more quantum wells on the first-conductivity-type cladding layer, forming a second-conductivity-type cladding layer including a second-conductivity-type nitride semiconductor layer on the light-emitting layer to form a semiconductor laminate, etching the semiconductor laminate so as to expose a portion of the first-conductivity-type cladding layer to form a mesa structure having a resonator, depositing an electrode material on each of the first-conductivity-type cladding layer and the second-conductivity-type cladding layer exposed by etching to form contact electrodes, and locally heating only the contact electrodes with a laser pulse.

[0008] Furthermore, a laser diode according to an embodiment of the present disclosure includes a nitride semiconductor substrate containing Al, and a semiconductor laminate portion disposed on the nitride semiconductor substrate, the semiconductor laminate portion having a first conductivity type cladding layer disposed on the nitride semiconductor substrate and including a first conductivity type nitride semiconductor layer, a light emitting layer formed on the first conductivity type cladding layer and having a nitride semiconductor structure including one or more quantum wells, and a second conductivity type cladding layer disposed on the light emitting layer and including a second conductivity type nitride semiconductor layer, at least a portion of the semiconductor laminate portion having a mesa structure for optical resonance and emission, and a dislocation density in the first conductivity type cladding layer, the light emitting layer, and the second conductivity type cladding layer within the mesa structure is 1 / μm or less. It should be noted that the above summary of the invention does not list all of the features of the present disclosure. Effect of the Invention

[0009] According to one aspect of the present disclosure, it is possible to provide a laser diode having a low lasing threshold current. [Brief description of the drawings]

[0010] [Figure 1] 1 is a schematic plan view illustrating a configuration example of a laser diode according to an embodiment of the present disclosure. [Diagram 2] 1 is a schematic cross-sectional view illustrating a configuration example of a laser diode according to an embodiment of the present disclosure. [Diagram 3] FIG. 11 is a cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. [Figure 4] FIG. 11 is a cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. [Diagram 5] FIG. 11 is a cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. [Figure 6] FIG. 11 is a cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. [Figure 7] 10 is a schematic plan view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. [Figure 8]10 is a schematic cross-sectional view illustrating another configuration example of a laser diode according to an embodiment of the present disclosure. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The laser diode according to the present disclosure will be described below through embodiments, but the following embodiments do not limit the invention according to the claims. Also, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.

[0012] 1. Embodiment A laser diode according to an embodiment of the present disclosure will be described. (1.1) Structure of a laser diode The laser diode according to this embodiment includes a nitride semiconductor substrate containing Al, and a semiconductor laminate disposed on the nitride semiconductor substrate, the semiconductor laminate having a first conductive type cladding layer disposed on the nitride semiconductor substrate and including a first conductive type nitride semiconductor layer, a light emitting layer formed on the first conductive type cladding layer and having a nitride semiconductor structure including one or more quantum wells, and a second conductive type cladding layer disposed on the light emitting layer and including a second conductive type nitride semiconductor layer. At least a part of the semiconductor laminate has a mesa structure for optical resonance and emission, and the dislocation density in the first conductive type cladding layer, the light emitting layer, and the second conductive type cladding layer in the mesa structure is 1 / μm or less. Each layer of the laser diode will now be described in detail.

[0013] (Nitride semiconductor substrate) The nitride semiconductor substrate (hereinafter, sometimes referred to as substrate) used in the manufacture of the laser diode according to this embodiment contains a nitride semiconductor containing Al. The nitride semiconductor containing Al is, for example, AlN. That is, the substrate is preferably an AlN single crystal substrate. The nitride semiconductor containing Al is not limited to AlN, and may be, for example, AlGaN. For example, when the substrate is a nitride semiconductor single crystal substrate such as AlN or AlGaN, the difference in lattice constant with the nitride semiconductor layer formed on the substrate becomes small, and the nitride semiconductor layer is grown in a lattice-matched system, thereby reducing threading dislocations. The threading dislocation density of the substrate is 5×10 4 cm -2 In particular, from the viewpoint of reducing the oscillation threshold current, the threading dislocation density is preferably 1×10 3 More than 1×10 4 cm -2 It is more preferable that:

[0014] Here, the wording "comprises" in the expression "comprises a nitride semiconductor" means that the layer mainly contains a nitride semiconductor, but this expression also includes cases where other elements are included. Specifically, this expression also includes cases where the composition of this layer is slightly changed by adding a small amount of an element other than the nitride semiconductor (for example, elements such as Ga (when Ga is not the main element), In, As, P, or Sb, at a few percent or less). In expressions of the composition of other layers, the wording "comprises" has a similar meaning. Also, the small amount of elements contained is not limited to the above.

[0015] The substrate may be doped with a donor impurity or an acceptor impurity to be n-type or p-type, and may be a mixed crystal of a nitride semiconductor such as AlN and sapphire (Al2O3), Si, SiC, MgO, Ga2O3, ZnO, GaN, or InN.

[0016] As an example, the substrate preferably has a layer thickness of 100 μm or more and 600 μm or less. In addition, the plane orientation includes the c-plane (0001), a-plane (11-20), m-plane (10-10), etc., and the c-plane (0001) substrate is more preferable. Further, it can be formed on a plane inclined by a certain angle (for example, -4° to 4°, preferably -0.4° to 0.4°) from the normal direction of the c-plane (0001), but it is not limited thereto.

[0017] (First conductive type clad layer) The first conductive type clad layer is formed on the substrate. Here, for example, in the expression "the first conductive type clad layer is formed on the substrate", the word "on" means that the first conductive type clad layer is formed on one surface of the substrate. Also, the above expression includes the case where another layer further exists between the substrate and the first conductive type clad layer. In the relationship between other layers as well, the word "above" has the same meaning. For example, when the second conductive type clad layer is formed via an electron blocking layer on the first conductive type waveguide layer described later, it is also included in the expression "the second conductive type clad layer is formed on the first conductive type waveguide layer". In the description of the present embodiment, "the first conductive type" and "the second conductive type" each mean a semiconductor having a different conductive type. For example, when one is n-type conductivity, the other is p-type conductivity. There may be cases where the description is made on the premise that the first conductive type is n-type and the second conductive type is p-type without special explanation, but it is not limited thereto.

[0018] The first conductive type clad layer is a layer of a nitride semiconductor containing Al and Ga. The first conductive type clad layer is, for example, Al a Ga (1-a) N (0 < a < 1). Thus, when a material corresponding to the bandgap energy in the deep ultraviolet region is formed as the light-emitting layer, it becomes possible to enhance the crystallinity of the light-emitting layer and improve the light-emitting efficiency. From the viewpoint of realizing high light-emitting efficiency, the nitride semiconductor constituting the first conductive type clad layer is preferably a mixed crystal of AlN and GaN. Also, from the viewpoint of growing with complete strain with respect to the substrate, the first conductive type clad layer is Al a Ga (1-a)It is more preferably formed by N(0.6 < a ≤ 0.8).

[0019] The first conductive type clad layer may be a gradient layer in which the Al composition increases as it moves away from the substrate for the purpose of controlling the longitudinal conductivity. In this case, the above-mentioned limitation on the Al composition can be the Al composition averaged by the film thickness of the first conductive type clad layer for the Al composition at the position in the film thickness direction within the first conductive type clad layer.

[0020] When the first conductive type clad layer is an n-type conductive semiconductor layer, it may contain impurities such as group V elements other than N such as In, P, As, Sb, and impurities such as C, H, F, O, Mg, Si, etc., but the types of impurity elements are not limited to this. From the viewpoints of reducing electrical resistance and the availability of raw materials, the impurity contained in the first conductive type clad layer is preferably Si, and the impurity concentration is 5×10 18 cm -3 or more and 5×10 19 cm -3 or less is preferable.

[0021] The first conductive type clad layer preferably has a layer thickness of 200 nm or more and 800 nm or less, more preferably has a layer thickness of 300 nm or more and 750 nm or less, and still more preferably has a layer thickness of 300 nm or more and 500 nm or less, from the viewpoints of lattice relaxation and film resistance within the first conductive type clad layer.

[0022] (Light-emitting layer) The light-emitting layer is a layer of a nitride semiconductor containing Al and Ga. The nitride semiconductor contained in the light-emitting layer is preferably a mixed crystal of, for example, AlN and GaN from the viewpoint of realizing high luminous efficiency. For example, Al b Ga (1-b) N(0 < b < 1) is formed. In addition to N, the light-emitting layer may contain impurities such as group V elements other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si, etc., but it is not limited to this.

[0023] In addition, the light-emitting layer can have either a multiple quantum well structure or a single quantum well structure. Although it depends on the longitudinal conductivity of the first conductivity type clad layer and the second conductivity type clad layer, the number of quantum well structures is preferably any one of 1 to 3. Also, for the purpose of reducing the influence of crystal defects in the light-emitting layer, elements such as Si, Sb, and P may be contained in part or all of the light-emitting layer at 1×10 15 cm -3 or more.

[0024] (Waveguide layer) From the perspective of light confinement, the laser diode of this embodiment may further include a waveguide layer formed above and below the light-emitting layer so as to sandwich the light-emitting layer and having the effect of confining the light emitted from the light-emitting layer within the light-emitting layer. The waveguide layer is preferably composed of two layers, a first conductivity type waveguide layer disposed on the first conductivity type clad layer side with respect to the light-emitting layer and a second conductivity type waveguide layer disposed on the second conductivity type clad layer side with respect to the light-emitting layer. That is, the laser diode of this embodiment may include, for example, a first conductivity type waveguide layer disposed between the first conductivity type clad layer and the light-emitting layer for confining light to the light-emitting layer, and a second conductivity type waveguide layer disposed between the second conductivity type clad layer and the light-emitting layer for confining light to the light-emitting layer.

[0025] From the perspective of light confinement, the waveguide layer is preferably a nitride semiconductor containing Al and Ga having a bandgap with higher energy than that of the light-emitting layer. The waveguide layer preferably has an Al composition and a film thickness that increase the overlap of the electric field intensity distribution of the light standing in the device and the light-emitting layer. From the perspective of carrier confinement to the light-emitting layer, the light-emitting layer is Al b Ga (1-b) N(0 < b < 1), and the waveguide layer is Al c Ga (1-c)When N satisfies 0 < c < 1, it is more preferable that b < c and c ≥ b + 0.05. For example, when taking the light-emitting layer with an emission wavelength of 265 nm as an example, b = 0.52, and c is preferably 0.57 or more. Further, from the viewpoints of light confinement and sheet resistance, the total film thickness of the first conductivity type waveguide layer and the second conductivity type waveguide layer is preferably 70 nm or more and 150 nm or less.

[0026] Each of the Al compositions of the first conductivity type waveguide layer and the second conductivity type waveguide layer is preferably uniform in the film thickness direction, but this is not the only case. In order to avoid light absorption into a metal (for example, the second electrode) existing above the second conductivity type cladding layer described later, the Al composition of the second conductivity type waveguide layer may be higher than the Al composition of the first conductivity type waveguide layer. For the same purpose, the film thickness of the second conductivity type waveguide layer may be thicker than the film thickness of the first conductivity type waveguide.

[0027] For the purpose of obtaining the same conductivity type as the first conductivity type cladding layer, etc., in addition to N, group V elements other than N such as P, As, Sb, and impurities such as H, C, O, F, Mg, Si may be mixed in the first conductivity type waveguide layer, but this is not the only case.

[0028] (Second conductivity type cladding layer) The second conductivity type cladding layer is a nitride semiconductor layer containing Al and Ga having second conductivity type conductivity, which is formed on the light-emitting layer. The second conductivity type cladding layer is, for example, Al d Ga (1-d) formed by N (0 < d < 1), and preferably formed by Al d Ga 1-d N (0.1 ≤ d ≤ 1). Further, when a waveguide layer (second conductivity type waveguide layer) is provided on the light-emitting layer, the second conductivity type cladding layer is formed on the waveguide layer (second conductivity type waveguide layer). Thereby, the second conductivity type cladding layer can easily achieve lattice matching with the light-emitting layer or the waveguide layer, and it is possible to suppress the threading dislocation density.

[0029] The second-conductivity-type clad layer has conductivity sufficient to inject carriers (electrons or holes) into the light-emitting layer, and the conductivity type is not particularly limited as long as it can increase the overlap between the electric field strength distribution of the optical mode standing in the device and the light-emitting layer (i.e., increase the optical confinement). The second-conductivity-type clad layer may be, for example, p-type AlGaN doped with Mg. In addition, the second-conductivity-type clad layer may contain impurities such as group V elements other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si, etc., but the types of impurity elements are not limited to this.

[0030] From the viewpoint of more efficiently injecting carriers into the light-emitting layer, the second-conductivity-type clad layer is an Al e Ga (1-e) compositionally graded layer (second-conductivity-type vertical conduction layer) formed of N in which the Al composition e decreases in the direction away from the upper surface of the substrate, and an Al f Ga (1-f) second-conductivity-type lateral conduction layer containing N (0 < f ≦ 1). Hereinafter, the second-conductivity-type vertical conduction layer and the second-conductivity-type lateral conduction layer will be described.

[0031] (Second-conductivity-type vertical conduction layer) The second-conductivity-type vertical conduction layer is a layer that constitutes the region on the light-emitting layer side of the second-conductivity-type clad layer. The second-conductivity-type vertical conduction layer is a layer containing Al e Ga (1-e) N. The profile (gradient) of the Al composition e in the second-conductivity-type vertical conduction layer may decrease continuously or discontinuously. Here, "decrease discontinuously" means including a portion in which the Al composition e is the same (constant in the film thickness direction) in a part of the film of the second-conductivity-type vertical conduction layer. That is, the second-conductivity-type vertical conduction layer may include a portion where the Al composition e does not decrease in the direction away from the substrate, but does not include an increasing portion.

[0032] The film thickness of the second-conductivity-type vertical conduction layer is preferably 500 nm or less from the viewpoint of lattice matching. Further, the film thickness of the second-conductivity-type vertical conduction layer is more preferably 250 nm or more and 450 nm or less, and even more preferably 300 nm or more and 400 nm or less from the viewpoints of light confinement in the light-emitting layer and carrier injection.

[0033] For the purpose of suppressing impurity diffusion, etc., in the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer, impurities such as H, Mg, Be, Zn, Si, and B are not doped (not intentionally mixed in), that is, it is preferably in an undoped state. Here, "undoped" means that the above-mentioned impurities are not intentionally supplied as elements in the process of forming the target layer, but elements derived from raw materials and manufacturing equipment are, for example, 1×10 16 cm -3 If they are mixed in the following range, this is not the case. Also, the undoped region of the second-conductivity-type vertical conduction layer includes at least the boundary with the light-emitting layer (the second-conductivity-type waveguide layer when the second-conductivity-type waveguide layer is provided), but its size is not limited. For example, all regions of the second-conductivity-type vertical conduction layer may be in an undoped state. Also, as another example, 50% of the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer may be in an undoped state. Also, as another example, about 10% of the region of the second-conductivity-type vertical conduction layer close to the light-emitting layer may be in an undoped state.

[0034] (Second-conductivity-type horizontal conduction layer) The second-conductivity-type horizontal conduction layer is a layer that constitutes the region of the second-conductivity-type cladding layer on the side opposite to the light-emitting layer, and is formed on the second-conductivity-type vertical conduction layer. The second-conductivity-type horizontal conduction layer is a layer containing Al f Ga (1-f) N (0 < f ≦ 1). Here, the Al composition f on the surface of the second-conductivity-type horizontal conduction layer facing the second-conductivity-type vertical conduction layer is preferably greater than the minimum value of the Al composition e of the second-conductivity-type vertical conduction layer. The second conductive type transverse conduction layer may be intentionally doped with impurities such as H, Mg, Be, Zn, Si, and B for the purpose of controlling the longitudinal resistivity of the second conductive type transverse conduction layer. The amount of the doped impurity depends on the net electric field amount induced on the surface and inside of the second conductive type transverse conduction layer, and may be, for example, 1×10 19 cm -3 5×10 or more 21 cm -3 It may be.

[0035] The thickness of the second conductivity type lateral conduction layer is preferably 20 nm or less, more preferably 10 nm or less, and further preferably 5 nm or less, from the viewpoint of facilitating quantum transmission of carriers through the second conductivity type lateral conduction layer.

[0036] When a second-conductivity-type contact layer (described later) is provided on the second-conductivity-type lateral conduction layer, the Al composition at the interface between the second-conductivity-type lateral conduction layer and the second-conductivity-type contact layer is preferably smaller than the Al composition in the second-conductivity-type contact layer and is completely distorted with respect to the substrate. Such a second-conductivity-type lateral conduction layer can improve the lateral conductivity by guiding carriers at the interface as the net internal electric field accumulated on the surface and inside near the surface of the second-conductivity-type lateral conduction layer becomes negative.

[0037] In this way, the second conductive type vertical conductive layer generates carriers (for example, holes when the second conductive type vertical conductive layer is formed of a p-type semiconductor) by the polarization doping effect, and has the effect of efficiently injecting the carriers into the active layer in the light emitting layer. Therefore, by providing the second conductive type vertical conductive layer on the light emitting layer, the carrier injection efficiency of the laser diode can be increased and the threshold voltage can be reduced. In addition, the second-conductivity-type lateral conduction layer has the effect of spreading the carrier distribution, which is narrowed by the electric field concentrated under the electrode, in the lateral direction (within the plane of the second-conductivity-type lateral conduction layer). Due to this effect, the second-conductivity-type lateral conduction layer can increase the efficiency of carrier injection into the light-emitting layer, just like the second-conductivity-type vertical conduction layer.

[0038] (Middle class) Between the second-conductivity-type clad layer and the waveguide, that is, between the second-conductivity-type vertical conduction layer and the second-conductivity-type waveguide layer, an AlGaN (where the Al composition g increases in the direction away from the upper surface of the substrate) can be provided from the viewpoint of improving the carrier conductivity and / or from the viewpoint of forming the second-conductivity-type lateral conduction layer and the second-conductivity-type contact layer with perfect strain. g Ga (1-g) An intermediate layer composed of N (0 < g ≤ 1.0) can be provided. The intermediate layer may be a mixed crystal that is not a bandgap that does not absorb light of the desired emission wavelength, and preferably has a film thickness of 50 nm or less, and may be an undoped layer containing no impurities.

[0039] (Second-conductivity-type contact layer) The semiconductor laminate portion of the laser diode of this embodiment may further include a second-conductivity-type contact layer disposed on the second-conductivity-type clad layer. The nitride semiconductor constituting the second-conductivity-type contact layer is preferably formed of, for example, GaN, AlN, or InN and mixed crystals containing them, and more preferably a nitride semiconductor containing GaN.

[0040] In the case of the second-conductivity-type contact layer being a p-type contact layer, impurities such as group V elements other than N such as P, As, Sb, and impurities such as C, H, F, O, Mg, Si, Be may be mixed in. From the versatility of the source gas, the impurity contained in the p-type contact layer is preferably Mg. From the viewpoint of reducing contact resistance, the concentration of Mg is 8×10 19 cm -3 or more and 5×10 21 cm -3 or less, preferably 5×10 20 cm -3 or more and 5×10 21 cm -3 or less.

[0041] Also, the layer thickness of the second-conductivity-type contact layer is preferably 1 nm or more and 20 nm or less. The thinner the layer thickness of the second-conductivity-type contact layer, the higher the carrier injection efficiency of the laser diode, and the thicker the layer thickness, the lower the carrier injection efficiency.

[0042] (Electron Block Layer) The semiconductor laminate of the laser diode of this embodiment may further include an electron blocking layer above the light emitting layer, the electron blocking layer having a band gap larger than that of the second conductive type waveguide layer. The electron blocking layer may be provided, for example, inside the second conductive type waveguide layer, between the second conductive type waveguide layer and the light emitting layer, or between the second conductive type waveguide layer and the second conductive type vertical conductive layer. The thickness of the electron blocking layer is preferably 30 nm or less, more preferably 20 nm or less, and even more preferably 15 nm or less, so that carriers (holes) can easily quantum-transport through the electron blocking layer.

[0043] (Mesa structure and resonator) The mesa structure is formed to electrically separate the second conductive type layer from the first conductive type layer. The mesa structure is a structure in which a part of the semiconductor laminate is removed. Here, the "semiconductor laminate" refers to at least the first conductive type cladding layer, the light emitting layer, and the second conductive type cladding layer, and also includes the above-mentioned waveguide layers (the first conductive type waveguide layer and the second conductive type waveguide layer), the intermediate layer, and the second conductive type contact layer, if these layers are provided.

[0044] From the viewpoint of current confinement of the laser and amplification by reflection at the end facets, it is preferable that the mesa structure is rectangular in plan view having long and short sides, with the long sides extending in the <1-100> direction. This is because when obtaining the resonator mirror end faces of the laser resonator by various methods such as cleavage and etching, the atomically flat (1-100) plane is the easiest to form. In other words, the mesa structure has a resonator mirror end face of the resonator parallel to the (1-100) crystal plane of the nitride semiconductor substrate, and the laser diode of this embodiment is an edge-emitting laser diode in which the mesa structure emits light in the <1-100> direction.

[0045] From the viewpoint of lowering the oscillation threshold current, the mesa structure including the first-conductivity-type cladding layer preferably has a number of dislocation lines per unit length of 1 / μm or less, and the mesa structure not including the first-conductivity-type cladding layer preferably has a number of dislocation lines per unit length of 1 / μm or less. The mesa structure can be formed by etching the semiconductor laminate using inductively coupled plasma (ICP) or the like.

[0046] Since the mesa structure includes a resonator, the presence of dislocation lines causes a deterioration in the oscillation threshold current. Therefore, the number of dislocation lines per unit length is preferably 1 / μm or less. In this case, the regions in the mesa structure that include dislocation lines are the first-conductivity-type cladding layer, the light-emitting layer, and the second-conductivity-type cladding layer, and no reduction in the oscillation threshold current is observed in the other regions due to the presence or absence of dislocation lines. As an example, if there are dislocation lines in the second-conductivity-type contact layer, there is no effect on the oscillation threshold current. Generally, dislocation density is often expressed as the number of dislocations contained per unit area, but in this embodiment, the number of dislocation lines contained per unit length is defined as the dislocation density. That is, threading dislocations from inside the substrate (dislocations extending in the thickness direction of the substrate) are excluded, and only dislocations formed in a direction parallel to the substrate surface are considered to be dislocations in this embodiment. This is because, in the structure of the laser diode according to this embodiment, the density of threading dislocations from inside the substrate is low, so that the influence of the presence of threading dislocations from inside the substrate on the oscillation threshold current is minor, and dislocations formed in a direction parallel to the substrate surface mainly contribute to the deterioration of the oscillation threshold current.

[0047] (electrode) The laser diode can be formed by a second electrode disposed on the second conductivity type cladding layer and a first electrode disposed on the first conductivity type cladding layer, where the first electrode is formed in electrical contact with the first conductivity type cladding layer and the second electrode is formed in electrical contact with the second conductivity type cladding layer. The first electrode can be disposed, for example, on the back side of the substrate, and is disposed on the first conductive clad layer exposed by removing layers (e.g., one or more layers near the second conductive contact layer) above the first conductive clad layer of the semiconductor laminate by, for example, chemical etching or dry etching.

[0048] When the first conductive type cladding layer is an n-type cladding layer, the first electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the first conductive type cladding layer is a p-type cladding layer, the first electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.

[0049] When the second conductive type cladding layer is an n-type cladding layer, the second electrode is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3. When the second conductive type cladding layer is a p-type cladding layer, the second electrode is formed of a metal such as Ni, Au, Pt, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, or a mixed crystal of these metals, or a conductive oxide such as ITO or Ga2O3.

[0050] The arrangement area and shape of the first electrode and the second electrode are not limited as long as they are in electrical contact with the first conductivity type cladding layer and the second conductivity type cladding layer (the second conductivity type contact layer if a second conductivity type contact layer is provided). Since carriers are captured and preferentially consumed in areas with many dislocations, resulting in worsening internal loss, it is preferable that the second electrode is arranged in an area 5 μm or more away from the side surface of the mesa structure on the second conductivity type cladding layer in a plan view.

[0051] (Buffer layer) The buffer layer is formed between the substrate and the first-conductivity-type cladding layer, and is preferably formed on the entire surface of the substrate. By providing the buffer layer, a nitride semiconductor layer having a small lattice constant difference and a small thermal expansion coefficient difference and a small number of defects is formed on the buffer layer. Furthermore, by providing the buffer layer, the first-conductivity-type cladding layer can be grown under compressive stress, and the occurrence of cracks in the first-conductivity-type cladding layer can be suppressed. Therefore, even if the substrate is formed of a nitride semiconductor such as AlN or AlGaN, a nitride semiconductor layer having a small number of defects can be formed above the buffer layer.

[0052] The buffer layer is formed of a nitride semiconductor such as AlN or AlGaN, etc. The buffer layer may contain impurities such as C, Si, Fe, Mg, etc.

[0053] The buffer layer has a thickness of, for example, several μm. Specifically, the thickness of the buffer layer is preferably thicker than 10 nm and thinner than 10 μm. When the thickness of the buffer layer is thicker than 10 nm, the crystallinity of the nitride semiconductor such as AlN is high. When the thickness of the buffer layer is thinner than 10 μm, cracks are less likely to occur in the buffer layer formed by crystal growth on the entire surface of the wafer. Moreover, the buffer layer is more preferably thicker than 50 nm and thinner than 5 μm. When the thickness of the buffer layer is thicker than 50 nm, a layer with high crystallinity can be formed. When the thickness of the buffer layer is thinner than 5 μm, cracks are less likely to occur in the buffer layer.

[0054] (1.2) Manufacturing method of ultraviolet light emitting element The laser diode of this embodiment is manufactured through a process of forming each layer on a substrate.

[0055] (Formation of the substrate) The substrate is formed by a general substrate growth method such as a vapor phase growth method, such as a sublimation method or a hydride vapor phase epitaxy (HVPE) method, or a liquid phase growth method.

[0056] (Formation of semiconductor laminate) Each layer of the semiconductor laminate formed on the substrate can be formed by, for example, molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), or metal organic chemical vapor deposition (MOCVD).

[0057] Here, among the layers formed on the substrate, the nitride semiconductor layer can be formed using, for example, an Al source containing trimethylaluminum (TMAl), a Ga source containing trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing ammonia (NH3).

[0058] Laser diodes are manufactured through a process of removing unnecessary portions of each layer of a semiconductor laminate formed on a substrate by etching. The unnecessary portions of each layer of the semiconductor laminate can be removed by, for example, inductively coupled plasma (ICP) etching.

[0059] (Electrode formation) The laser diode may also be manufactured through a process of forming electrodes. The electrodes, such as the first electrode and the second electrode, may be formed by, for example, resistance heating deposition, electron gun deposition, or sputtering, but are not limited to these methods. Each electrode may be formed as a single layer, or may be formed by laminating multiple layers. Each electrode may also be heat-treated in an oxygen, nitrogen, or air atmosphere after the layers are formed.

[0060] The formed electrode can be alloyed by heating with a rapid thermal annealing (RTA) device, which is a heating process using an infrared lamp, or by laser annealing, which is a heating process using a laser pulse, to obtain contact with the nitride semiconductor layer. In this case, the method of alloying is not particularly limited as long as sufficient contact with the nitride semiconductor layer is obtained and dislocations are not introduced into the mesa structure. From the viewpoint of easiness of the electrode formation process and reduction of contact resistance, it is preferable to perform heating by RTA or laser annealing.

[0061] When heating the electrodes by RTA, it is preferable to anneal at a temperature of 550° C. or more and 700° C. or less. This is because as the annealing temperature increases, dislocations are introduced to the end of the mesa structure, and the oscillation threshold current significantly deteriorates. In addition, it is more preferable to perform RTA for a short time of 70 seconds or less, preferably 60 seconds or less, because this makes it possible to suppress the introduction of dislocations and to achieve contact at the same time. In addition, when performing laser annealing, there are no particular limitations on the type of laser or the irradiation conditions as long as contact with the nitride semiconductor layer can be obtained. As an example, a CW laser having a wavelength of 532 nm is focused by a lens to anneal only the electrode, thereby suppressing the temperature rise in the nitride semiconductor layer and achieving both suppression of dislocation introduction in the nitride semiconductor layer and contact. Specifically, a 20 mW laser is focused to 40 μm, held for 4 seconds per point, and scanned over the electrode. This allows both suppression of dislocation introduction into the nitride semiconductor layer and contact. Finally, the substrate on which the layers have been formed through the above-mentioned steps is divided into individual pieces by dicing to manufacture the laser diodes.

[0062] 2. Measurement methods for the physical properties of ultraviolet light-emitting devices The physical properties of the laser diode described above can be measured as follows.

[0063] (Measurement of impurity and doping concentrations) The concentrations of dopants and impurities contained in the substrate and each layer of the semiconductor laminate that constitutes the laser diode can be measured by secondary ion mass spectrometry (SIMS). When measuring the concentration of dopants and impurities in each layer of the semiconductor laminate by SIMS after processing into a device, the measurement can be performed after removing the electrodes by chemical etching or physical polishing. The concentration of dopants and impurities in each layer of the semiconductor laminate can also be measured by sputtering from the substrate side where no electrodes are formed. Specifically, SIMS measurements are performed under the measurement conditions provided by Evans Analytical Group (EAG), Inc. A cesium (Cs) ion beam with an energy of 14.5 keV is used to sputter the sample during the measurements.

[0064] (Layer thickness measurement method) The thickness of each layer constituting the laser diode can be measured by cutting out a predetermined cross section perpendicular to the substrate, observing this cross section with a transmission electron microscope (TEM), and using the length measurement function of the TEM. As a measurement method, first, a cross section perpendicular to the main surface of the substrate of the laser diode is observed using a TEM. Specifically, for example, in a TEM image showing a cross section perpendicular to the main surface of the substrate of the laser diode, a range of 2 μm or more in a direction parallel to the main surface of the substrate is set as the observation width. Since contrast is observed at the interface between two layers with different compositions within this observation width, the thickness up to this interface is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of each layer included in this 200 nm wide observation region can be calculated from five points arbitrarily extracted from the above-mentioned observation width of 2 μm or more, thereby obtaining the layer thickness of each layer.

[0065] (Method of measuring relaxation) The presence or absence of relaxation can be obtained from the lattice constant calculated from the TEM lattice diffraction image. Distortion can be expressed as the amount by which the lattice constant in the in-plane direction of the a-axis of each layer of the laser diode has changed from the original lattice constant. If the lattice constant is the same as that of the substrate, it is strained, and if there is a difference, it can be said to be relaxed. Here, relaxation calculated from calculations is defined as 20% or more. The difference in lattice constant can be measured by automatic mapping measurement of the lattice diffraction image at each spot, and displayed as a mapping using analysis software. Specifically, the measurement can be performed using analysis software (ASTER, manufactured by NanoMEGAS).

[0066] (Method of measuring atomic concentration of each layer) One method for measuring the atomic concentration in each layer that constitutes a laser diode is reciprocal space mapping (RSM) using the X-ray diffraction (XRD) method. Specifically, the lattice relaxation rate and Al composition relative to the substrate can be obtained by analyzing reciprocal space mapping data in the vicinity of the diffraction peak obtained using an asymmetric plane as the diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (20-24) plane. In addition, layers and regions that do not provide sufficient reflection intensity by XRD, such as the light-emitting layer, the gradient layer, and hillocks formed in each layer, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS).

[0067] In EELS, the composition of a sample is analyzed by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, the energy loss spectrum of the intensity of the transmitted electron beam is measured and analyzed for a thin-sectioned sample used in TEM observation. The position of the peak that appears around 20 eV of energy loss changes depending on the composition of each layer, and the composition can be determined from the peak position. In the same manner as in the method for calculating layer thickness by TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.

[0068] In EDX, characteristic X-rays generated by an electron beam in a thin-sectioned sample used in the above-mentioned TEM observation, etc. are measured and analyzed. In the same manner as the method for calculating layer thickness using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.

[0069] In XPS, the evaluation of the depth direction is possible by performing XPS measurement while performing sputter etching using an ion beam. Although Ar+ is generally used as the ion beam, other ion species such as Ar cluster ions can be used as long as they can be irradiated with the etching ion gun mounted on the XPS device. The XPS peak intensities of Al, Ga, and N are measured and analyzed to obtain the depth direction distribution of the Al composition of each layer. Instead of sputter etching, the laser diode may be polished obliquely so that the cross section perpendicular to the main surface of the substrate is enlarged and exposed, and the exposed cross section may be measured by XPS.

[0070] The composition of each layer can be measured not only by XPS but also by Auger Electron Spectroscopy (AES). In this case, the composition can be measured by Auger Electron Spectroscopy on a cross section exposed by sputter etching or oblique polishing. The composition of each layer can also be measured by SEM-EDX measurement of a cross section exposed by oblique polishing.

[0071] (Measuring method for dislocation lines in mesa structures) The dislocation lines formed in the mesa structure can be measured by cutting out a predetermined cross section parallel to the surface of the substrate as a sample and observing it with a transmission electron microscope (TEM). As a measurement method, if the sample has electrodes, they are peeled off with aqua regia or the like. Alternatively, the electrodes present on the upper part may be removed by polishing or the like.

[0072] Dislocations are counted using TEM images observed at a magnification of 10k to 20k with an applied voltage of 200kV. An arbitrary point in the mesa structure is determined, and the observation area is moved from the edge of the mesa structure to the inside, observing all areas in the mesa width direction. Specifically, if the mesa width is 40μm, the entire 40μm wide area is observed. The mesa length direction can be observed at any three points. At this time, threading dislocations from the substrate are observed as points or short lines in a plan view. Therefore, dislocations that are observed to be interrupted midway within the observation field are treated as dislocations extending perpendicular to the substrate, and are not counted here.

[0073] When a dislocation extending in a certain direction intersects with a dislocation extending in another direction, each consecutive dislocation is counted as one. The number of dislocations per unit length is calculated assuming that the dislocations are lined up on the same plane in the planar TEM image. In other words, even if the dislocations are not at the same height in the cross section, they are calculated assuming that they exist on the same plane. Specifically, if there are five dislocation lines parallel to the <1-100> direction per μm in the TEM image in the observation range, the dislocation density is 5 / μm. Information on the dislocations in the mesa structure can be obtained by calculating the average dislocation density obtained from these measurements.

[0074] (Applications of ultraviolet light emitting devices) The laser diode according to the present disclosure can be applied to devices in, for example, the medical and life science fields, the environmental field, the industrial and manufacturing fields, the lifestyle and home appliances field, the agricultural field, and other fields. The laser diode can be applied to a drug or chemical synthesis and decomposition device, a liquid, gas, and solid (container, food, medical equipment, etc.) sterilization device, a semiconductor cleaning device, etc., a surface modification device for film, glass, metal, etc., an exposure device for manufacturing semiconductors, FPD (Flat Panel Display), PCB (Printed Wiring Board), and other electronic products, a printing and coating device, an adhesive and sealing device, a transfer and molding device for film, pattern, mockup, etc., and a measurement and inspection device for banknotes, wounds, blood, chemical substances, etc.

[0075] Examples of liquid sterilization equipment include, but are not limited to, automatic ice makers, ice trays and ice storage containers in refrigerators, water tanks for ice makers, freezers, ice makers, humidifiers, dehumidifiers, cold water tanks, hot water tanks and flow piping for water servers, freezer-type water purifiers, portable water purifiers, water supply units, hot water heaters, wastewater treatment equipment, garbage disposers, toilet drain traps, washing machines, water sterilization modules for dialysis, connector sterilizers for peritoneal dialysis, and disaster water storage systems.

[0076] Examples of gas sterilization devices include, but are not limited to, air purifiers, air conditioners, ceiling fans, floor or bedding vacuum cleaners, futon dryers, shoe dryers, washing machines, clothes dryers, indoor germicidal lamps, storage ventilation systems, shoe boxes, chests of drawers, etc. Examples of solid sterilization equipment (including surface sterilization equipment) include, but are not limited to, vacuum packing machines, belt conveyors, hand tool sterilization equipment for medical, dental, barber, and beauty salon use, toothbrushes, toothbrush holders, chopstick cases, cosmetic pouches, drain covers, toilet spot cleaners, and toilet lids.

[0077] 3. Examples of UV light-emitting elements The laser diode of this embodiment will be described in more detail below with reference to Figures 1 to 8. The detailed configuration of each layer in each of the following embodiments is as described above.

[0078] (3.1) First embodiment 1 and 2 are schematic diagrams for explaining a laser diode 1 according to a first embodiment. Fig. 1 is a schematic plan view of the laser diode 1, and Fig. 2 is a schematic cross-sectional view of the laser diode 1. In Fig. 1, <1-100><11-20> <0001> indicates the crystal orientation. 2, the laser diode 1 includes a substrate 10, a semiconductor laminate 20 disposed on the substrate 10, a first electrode 31, and a second electrode 32. The semiconductor laminate 20 includes a first conductive type cladding layer 21, a light emitting layer 22, and a second conductive type cladding layer 23. A part of the semiconductor laminate 20 has a mesa structure 201. An end surface ES (see FIG. 1) of the mesa structure 201 is a resonator structure for optical resonance and emission, and laser light is emitted in a direction perpendicular to the end surface ES (the direction of the arrow in FIG. 1). In the laser diode 1, the number of dislocation lines per unit length (dislocation density) in the mesa structure 201 (particularly in the first conductivity type cladding layer, the light emitting layer, and the second conductivity type cladding layer) is 1 line / μm or less.

[0079] (3.2) Second embodiment Fig. 3 is a schematic diagram for explaining a laser diode 2 according to the second embodiment. Fig. 3 is a schematic cross-sectional view of the laser diode 2. The laser diode 2 differs from the laser diode 1 according to the first embodiment in that the laser diode 2 has a semiconductor laminate 20A further including a first conductive type waveguide layer 24 and a second conductive type waveguide layer 25. A part of the semiconductor laminate 20A has a mesa structure 201. In such a laser diode 2, the effect of confining light in the light emitting layer 22 is improved, and the emission intensity of the laser diode 2 is improved.

[0080] (3.3) Third embodiment Fig. 4 is a schematic diagram for explaining a laser diode 3 according to the third embodiment. Fig. 4 is a schematic cross-sectional view of the laser diode 3. The laser diode 3 differs from the laser diode 2 according to the second embodiment in that the laser diode 3 has a semiconductor laminate 20B including a second-conductivity-type contact layer 26 disposed on a second-conductivity-type cladding layer 23. A part of the semiconductor laminate 20B has a mesa structure 201. In such a laser diode 3, the efficiency of carrier injection into the light emitting layer 22 is improved, and the light emission efficiency of the laser diode 3 is improved.

[0081] The second conductive type contact layer 26 may be combined with, for example, the laser diode 2 according to the second embodiment. That is, the laser diode may have the second conductive type contact layer 26 disposed on the second conductive type cladding layer 23 of the laser diode 2 (not shown).

[0082] (3.4) Fourth embodiment Fig. 5 is a schematic diagram for explaining a laser diode 4 according to the fourth embodiment. Fig. 5 is a schematic cross-sectional view of the laser diode 4. The laser diode 4 differs from the laser diode 1 according to the first embodiment in that it has a semiconductor laminate 20C including a second-conductivity-type cladding layer 23 composed of a second-conductivity-type vertical conductive layer 23A and a second-conductivity-type lateral conductive layer 23B, and a second-conductivity-type contact layer 26. A part of the semiconductor laminate 20C has a mesa structure 201. In such a laser diode 4, the efficiency of carrier injection into the light emitting layer 22 is improved, and the light emission efficiency of the laser diode 4 is improved.

[0083] (3.5) Fifth embodiment Fig. 6 is a schematic diagram for explaining a laser diode 5 according to the fifth embodiment. Fig. 6 is a schematic cross-sectional view of the laser diode 5. The laser diode 5 differs from the laser diode 1 according to the first embodiment in that it has a semiconductor laminate 20D including a first-conductivity-type waveguide layer 24, a second-conductivity-type waveguide layer 25, a second-conductivity-type cladding layer composed of a second-conductivity-type vertical conductive layer 23A and a second-conductivity-type lateral conductive layer 23B, and an intermediate layer 27 provided between the second-conductivity-type vertical conductive layer 23A and the second-conductivity-type waveguide layer 25. A part of the semiconductor laminate 20D has a mesa structure 201. In the laser diode 5, the carrier conductivity in the intermediate layer 27 is improved, and the second conductive type lateral conduction layer 23B and the second conductive type contact layer 26 are formed with perfect strain, thereby improving the carrier lateral conduction.

[0084] (3.6) Sixth embodiment Fig. 7 and Fig. 8 are schematic diagrams for explaining a laser diode 6 according to the sixth embodiment. Fig. 7 is a schematic plan view of the laser diode 6, and Fig. 8 is a schematic cross-sectional view of the laser diode 6. The laser diode 6 further includes a first-conductivity-type waveguide layer 24, a second-conductivity-type waveguide layer 25, and a second-conductivity-type contact layer 26. The mesa structure of the laser diode 6 is a two-stage structure, and the laser diode 6 differs from the laser diode 1 according to the first embodiment in that it includes a semiconductor laminate 20E including a mesa structure 201 including a first-conductivity-type cladding layer 21 and a mesa structure 203 not including a first-conductivity-type cladding layer 21. A part of the semiconductor laminate 20E includes the mesa structure 201 and the mesa structure 203. At this time, the mesa structure 201 including the first-conductivity-type cladding layer 21 includes a plurality of dislocation lines extending in the crystal orientation <1-100> of the substrate 10. From the viewpoint of reducing the oscillation threshold current, it is preferable that the mesa structure 203 not including the first-conductivity-type cladding layer 21 does not include dislocation lines extending in the crystal orientation <1-100> of the substrate 10.

[0085] 4.Effects The above-mentioned laser diode has the following advantages. (1) A laser diode is formed by forming a semiconductor laminate section by sequentially forming a nitride semiconductor substrate, a first conductivity type cladding layer, a light emitting layer, and a second conductivity type cladding layer, etching the semiconductor laminate section so as to expose a portion of the first conductivity type cladding layer to form a mesa structure having a resonator, depositing an electrode material on each of the first conductivity type cladding layer and the second conductivity type cladding layer exposed by etching to form contact electrodes, and heat-treating the contact electrodes using an infrared lamp at a temperature of 550°C to 700°C for 70 seconds or less. This makes it possible to suppress the rise in annealing temperature and the introduction of dislocations into the mesa structure end, thereby suppressing a significant deterioration in the oscillation threshold current. In addition, since the electrodes are heated in a short time, it is possible to achieve both the suppression of dislocation introduction and contact.

[0086] (2) The laser diode is formed by depositing an electrode material on each of the first conductivity type cladding layer and the second conductivity type cladding layer exposed by etching as described above to form contact electrodes, and then locally heating only the contact electrodes with a laser pulse. This makes it possible to suppress a rise in temperature in the nitride semiconductor layer, and to simultaneously suppress the introduction of dislocations in the nitride semiconductor layer and establish contact.

[0087] (3) In the laser diode, at least a portion of the semiconductor laminate disposed on the substrate has a mesa structure for optical resonance and emission, and the dislocation density in the first conductivity type cladding layer, the light emitting layer, and the second conductivity type cladding layer within the mesa structure is 1 / μm or less. This makes it possible to suppress the deterioration of internal loss caused by dislocations capturing and preferentially consuming carriers in the mesa structure of the laser diode, thereby lowering the oscillation threshold current. (4) The mesa structure of the laser diode has a resonator that emits light, and the ratio of the distance between the resonator mirror end faces in a plan view to the distance between the side faces of the mesa structure is preferably 5:1 to 500:1. As a result, it is possible to appropriately adjust the distance between the sides of the mesa structure that correlates with the threshold voltage and the oscillation threshold current, thereby reducing the threshold voltage and the oscillation threshold current.

[0088] (5) The laser diode is preferably an end-face emission type laser diode in which the resonant mirror end face of the resonator is a plane parallel to the crystal plane (1-100) based on the crystal orientation of the nitride semiconductor substrate, and light is emitted in the <1-100> direction of the crystal orientation of the nitride semiconductor substrate. As a result, a resonant mirror end face can be formed on the atomically flat (1-100) plane, and the resonant mirror end face of the laser resonator can be easily formed. (6) The nitride semiconductor substrate is preferably an AlN single crystal substrate. As a result, the lattice constant difference between the substrate and the nitride semiconductor layer formed on the upper side of the substrate is reduced, and threading dislocations can be reduced by growing the nitride semiconductor layer in a lattice-matched system, and a highly stable nitride semiconductor layer can be formed. (7) The laser diode preferably includes a first conductivity type waveguide layer disposed between the first conductivity type clad layer and the light emitting layer, and a second conductivity type waveguide layer disposed between the second conductivity type clad layer and the light emitting layer. As a result, the effect of confining light in the light emitting layer is improved, and the light emitting efficiency is improved.

[0089] (8) The laser diode preferably includes a second conductivity type contact layer disposed on the second conductivity type clad layer and formed of a nitride semiconductor containing GaN. At this time, the second conductivity type clad layer preferably has a second conductivity type vertical conduction layer containing Al e Ga 1-e N (0.1 ≦ e ≦ 1) and having a composition gradient in which the Al composition e decreases as it moves away from the nitride semiconductor substrate and a film thickness of less than 0.5 μm, and a second conductivity type horizontal conduction layer containing Al f Ga 1-f N (0 < f ≦ 1). As a result, carriers can be more efficiently injected into the light emitting layer, and the light emitting efficiency can be improved. (9) The laser diode is disposed between the second-conductivity-type vertical conduction layer and the second-conductivity-type waveguide layer, and preferably includes an intermediate layer formed of Al g Ga 1-g N (0 < g ≦ 1.0). Thereby, the second-conductivity-type lateral conduction layer and the second-conductivity-type contact layer can be formed with complete strain to improve the conductivity of carriers.

[0090] (10) The film thickness of the second-conductivity-type vertical conduction layer is preferably 250 nm or more and 450 nm or less. Thereby, the light confinement effect on the light-emitting layer is improved, the carrier injection effect is improved, and the light-emitting efficiency of the laser diode is improved. (11) Preferably, a part or all of the regions of the second-conductivity-type vertical conduction layer including the interface with the second-conductivity-type waveguide layer are regions not doped with impurities. Thereby, diffusion of impurities can be suppressed, carriers can be efficiently injected into the light-emitting layer, and the oscillation efficiency can be increased.

[0091] (12) The first-conductivity-type clad layer is formed of Al a Ga 1-a N (0.6 < a ≦ 0.8), and preferably, the second-conductivity-type vertical conduction layer and the second-conductivity-type lateral conduction layer are formed with complete strain with respect to the substrate. By forming the first-conductivity-type clad layer with Al a Ga 1-a N (0.6 < a ≦ 0.8), the second-conductivity-type vertical conduction layer and the second-conductivity-type lateral conduction layer can be formed with complete strain with respect to the substrate to improve the conductivity of carriers. (13) Preferably, the Al composition f on the surface of the second-conductivity-type lateral conduction layer facing the second-conductivity-type vertical conduction layer is larger than the minimum value of the Al composition e of the second-conductivity-type vertical conduction layer. Thereby, carriers can be diffused in the lateral direction, and the injection efficiency of carriers can be increased.

[0092] (14) The laser diode preferably includes a second electrode provided on the second conductivity type cladding layer in a region 5 μm or more away from a side surface of the mesa structure in a plan view. This prevents internal loss in the laser diode, and improves the light emission efficiency. (15) It is preferable that the mesa structure of the laser diode is rectangular in plan view having long and short sides, with the long sides being arranged parallel to the <1-100> direction. This allows the resonator mirror end faces of the laser resonator to be formed into atomically flat (1-100) faces, which makes it easy to form the resonator mirror end faces. EXAMPLES

[0093] Examples and comparative examples of the present disclosure will be described below.

[0094] [Example 1] A 550μm thick (0001) AlN single crystal substrate was used as the substrate, and annealing was performed on this substrate using a metal organic chemical vapor deposition (MOCVD) device. The annealing process was performed in two sets of annealing at 1300℃, one set being annealing for 5 minutes in an NH3 atmosphere and the other being annealing for 5 minutes in an H2 atmosphere.

[0095] Next, an AlN layer, which is a homoepitaxial layer, was formed on the substrate as a buffer layer. The AlN layer was formed to a thickness of 500 nm in an environment at 1200°C. At this time, the ratio (V / III ratio) of the supply rate of the group III element source gas to the supply rate of the nitrogen source gas was set to 50. The degree of vacuum of the chamber in which the annealing was performed was set to 50 mbar. The growth rate of the AlN layer at this time was 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al source, and ammonia (NH3) was used as the N source.

[0096] A first conductive cladding layer was formed on the AlN layer formed as described above. The first conductive cladding layer was an n-type AlGaN layer (Al: 70%, i.e., Al0.70 Ga 0.30 The first conductive type cladding layer was formed to a thickness of 350 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the first conductive type cladding layer was 0.4 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material. Ammonia (NH3) was used as the N raw material. Monosilane (SiH4) was used as the Si raw material.

[0097] Next, an n-type waveguide layer, which is a first conductive type waveguide layer, was formed on the first conductive type cladding layer. The n-type waveguide layer was an n-type AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 The n-type waveguide layer was formed to a thickness of 60 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the n-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, triethylgallium (TEGa) was used as the Ga raw material, and ammonia (NH3) was used as the N raw material.

[0098] Next, a light emitting layer was formed on the n-type waveguide layer. The light emitting layer was formed to have a multiple quantum well structure in which quantum well layers and barrier layers were stacked three times. Here, the quantum well layer was an AlGaN layer (Al: 52%, i.e., Al 0.52 Ga 0.48 The barrier layer having a thickness of 6.0 nm was an AlGaN layer (Al: 63%, i.e., Al 0.63 Ga 0.37 N layer). The light-emitting layer was formed under conditions of a vacuum degree of 50 mbar and a V / III ratio of 4000. The growth rate of the quantum well layer was 0.18 μm / hr, and the growth rate of the barrier layer was 0.15 μm / hr.

[0099] Next, a p-type waveguide layer, which is a second conductive type waveguide layer, was formed on the light emitting layer. The p-type waveguide layer was an AlGaN layer containing no dopant (Al: 63%, i.e., Al 0.63 Ga 0.37 The p-type waveguide layer was formed to a thickness of 60 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the p-type waveguide layer was 0.35 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material, and triethylgallium (TEGa) was used as the Ga raw material.

[0100] Next, a second conductive cladding layer was formed on the p-type waveguide layer. The second conductive cladding layer has a laminated structure including a second conductive vertical conductive layer and a second conductive horizontal conductive layer, and is a graded layer with a gradient Al composition ratio. The second conductive vertical conductive layer was an AlGaN layer with a thickness of 320 nm, in which the Al composition was distributed in the direction away from the substrate, varying from Al=1.0 to 0.7. The second conductive horizontal conductive layer was a p-type AlGaN layer with Al=0.9 and a thickness of 2 nm. The second conductive cladding layer was formed under the conditions of a temperature of 1080° C., a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the second conductive cladding layer at this time was 0.3 to 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material.

[0101] Next, a p-type contact layer, which is a second conductive type contact layer, was formed on the second conductive type cladding layer. Here, the p-type contact layer was formed of an AlGaN layer and a GaN layer. The AlGaN layer was a p-type nitride semiconductor layer with a layer thickness of 30 nm, using Mg as a dopant impurity and with an Al composition distribution in the direction away from the substrate, varying from Al=0.7 to 0.4. The GaN layer was formed of GaN (i.e. Al:0%) with a thickness of 10 nm.

[0102] The second conductive type contact layer was formed under the conditions of a temperature of 950° C., a degree of vacuum of 150 mbar, and a V / III ratio of 3650. The growth rate of the second conductive type contact layer at this time was 0.2 μm / hr.

[0103] In this manner, a semiconductor laminate was formed on an AlN substrate. When reciprocal lattice mapping measurement was performed on this semiconductor laminate by XRD, it was found that the semiconductor laminate had grown pseudomorphically without relaxation up to the second conductivity type contact layer.

[0104] The semiconductor laminate formed as described above was annealed in an N2 atmosphere at 700°C for 10 minutes or more to further reduce the resistance of the second conductive contact layer. The first conductive clad layer was exposed by dry etching using a gas containing Cl2 using an ICP. The first conductive clad layer was formed in a rectangular region long in the <1-100> direction in a plan view. The ICP conditions were: antenna power 320W, bias power 30W, automatic pressure regulation (APC: Adaptive Pressure Control valve) 2Pa, process pressure 600Pa, and gas flow rate of Cl2 gas 20sccm. The formed mesa structure had a length of 700 μm in the <1-100> direction and a length of 40 μm in the <11-20> direction, where the length of the mesa structure in the <1-100> direction is the distance between the end faces of the cavity mirror in a plan view, and the length in the <11-20> direction is the distance between the side faces of the mesa structure.

[0105] On the second conductive contact layer of the mesa structure, Ni and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as p-type second electrodes. At this time, the width of the second electrode was 5 μm and the length was 700 μm. In addition, in the region where the n-type cladding layer of the mesa structure was exposed, V, Al, Ni, Ti, and Au were sequentially deposited in a rectangular shape elongated in the <1-100> direction to form multiple electrode metal regions as n-type first electrodes. The first and second electrodes were annealed at 550°C for 60 seconds in a nitrogen atmosphere using an RTA device. Furthermore, the substrate was divided into stripes by cleaving multiple times parallel to the <11-20> direction within the electrode metal region to form individual laser diodes. The length of the mesa structure in the <1-100> direction after division was 600 μm.

[0106] The laser diode thus obtained was subjected to current injection and edge emission intensity measurements. The threshold voltage was 12 V and the oscillation threshold current was 10 kA / cm. 2 It was. Planar TEM measurement of this laser diode revealed that the total number of dislocation lines in the mesa structure was zero in the first cladding layer, the light-emitting layer, and the second cladding layer, and the number of dislocation lines per unit length (dislocation density) was zero / μm.

[0107] [Example 2] A laser diode of Example 2 was formed in the same manner as in Example 1, except that the annealing temperature when the first electrode and the second electrode were annealed by the RTA apparatus was set to 630°C. When the current-facet emission intensity of the obtained laser diode was measured by current injection, the threshold voltage was 11 V and the oscillation threshold current was 10.5 kA / cm 2 It was. When a planar TEM measurement was performed on the mesa structure of this laser diode, the total number of dislocation lines in the mesa structure was 8, and the number of dislocation lines per unit length (dislocation density) was 0.2 / μm.

[0108] [Example 3] A laser diode of Example 3 was formed in the same manner as in Example 1, except that the annealing temperature when the first electrode and the second electrode were annealed by the RTA apparatus was set to 700°C. When the current-facet emission intensity of the obtained laser diode was measured by current injection, the threshold voltage was 10 V and the oscillation threshold current was 11 kA / cm 2 It was. Plane TEM measurements were performed on the mesa structure of this laser diode, and it was found that there were a total of 16 dislocation lines in the mesa structure, and the number of dislocation lines per unit length (dislocation density) was 0.4 lines / μm.

[0109] [Example 4] The laser diode of Example 4 was formed in the same manner as in Example 1, except that the first electrode and the second electrode were annealed using a laser annealing method in which a CW laser (output 20 mW) having a wavelength of 532 nm was focused to 40 μm using a lens, the laser was held for 4 seconds per point, and only the first electrode and the second electrode were scanned. When the current-facet emission intensity of the obtained laser diode was measured by current injection, the threshold voltage was 9.5 V and the oscillation threshold current was 10 kA / cm 2 It was. When a planar TEM measurement was performed on the mesa structure of this laser diode, the total number of dislocation lines in the mesa structure was found to be zero, and the number of dislocation lines per unit length (dislocation density) was found to be zero / μm.

[0110] [Comparative Example 1] A laser diode of Comparative Example 1 was formed in the same manner as in Example 1, except that the annealing temperature when the first electrode and the second electrode were annealed by the RTA apparatus was set to 750°C. When the current-facet emission intensity of the obtained laser diode was measured by current injection, the threshold voltage was 9 V and the oscillation threshold current was 25 kA / cm 2 It was. When a planar TEM measurement was performed on the mesa structure of this laser diode, the total number of dislocation lines in the mesa structure was 80, and the number of dislocation lines per unit length (dislocation density) was 6.0 lines / μm.

[0111] Table 1 below shows the evaluation results of each of the examples and comparative examples.

[0112] [Table 1]

[0113] As shown in Table 1, the laser diodes of each embodiment, in which the number of dislocation lines per unit length in the mesa structure (dislocation density) is 1 line / μm or less, exhibited a significantly lower oscillation threshold without deteriorating the threshold voltage, compared to the laser diode of the comparative example, in which the number of dislocation lines per unit length in the corresponding region (dislocation density) is 6.0. From the above, it was found that it is necessary to appropriately set the number of dislocation lines formed per unit length in the mesa structure (dislocation density).

[0114] Although the embodiments of the present disclosure have been described above, the technical scope of the present disclosure is not limited to the technical scope described in the above-mentioned embodiments. Various modifications or improvements can be made to the above-mentioned embodiments, and it is clear from the claims that the forms to which such modifications or improvements are made are also included in the technical scope of the present disclosure. [Explanation of symbols]

[0115] 10 Substrate 20 Semiconductor laminate 21 First conductive type cladding layer 22 Light-emitting layer 23 Second conductive type cladding layer 23A Second conductive type vertical conductive layer 23B Second conductive type lateral conductive layer 24 First conductive type waveguide layer 25 Second conductive type waveguide layer 26 Second conductive type contact layer 27 Middle Class 31 1st electrode 32 2nd electrode 201 Mesa structure including first conductive type cladding layer 203 Mesa structure (ridge portion) that does not include the first conductive type cladding layer Side of SS mesa structure End face of ES mesa structure

Claims

1. forming a first conductive type clad layer including a first conductive type nitride semiconductor layer on a nitride semiconductor substrate including Al; forming a light emitting layer having a nitride semiconductor structure including one or more quantum wells on the first conductive type clad layer; and forming a second conductive type clad layer including a second conductive type nitride semiconductor layer on the light emitting layer to form a semiconductor laminate; The semiconductor laminate is etched so that a portion of the first conductive type cladding layer is exposed to form a mesa structure having a resonator; depositing an electrode material on each of the first conductive type cladding layer and the second conductive type cladding layer exposed by etching to form contact electrodes; The contact electrodes are heat-treated by an infrared lamp at a temperature of 550° C. to 700° C. for 70 seconds or less. A method for manufacturing a laser diode.

2. a nitride semiconductor substrate containing Al; a semiconductor laminate portion disposed on the nitride semiconductor substrate; Equipped with The semiconductor laminate portion is a first conductivity type cladding layer disposed on the nitride semiconductor substrate and including a first conductivity type nitride semiconductor layer; a light emitting layer having a nitride semiconductor structure including one or more quantum wells formed on the first conductive type cladding layer; a second conductivity type cladding layer disposed on the light emitting layer and including a second conductivity type nitride semiconductor layer; At least a part of the semiconductor laminate has a mesa structure for optical resonance and emission, The dislocation density in the first conductive type cladding layer, the light emitting layer, and the second conductive type cladding layer in the mesa structure is 1 / μm or less. Laser diode.

3. the mesa structure has a resonator that emits light, In a plan view, the ratio of the distance between the end faces of the resonator to the distance between the side faces of the mesa structure is 5:1 to 500:

1.

3. The laser diode of claim 2.

4. a resonator mirror end face of the resonator is a surface parallel to a crystal plane (1-100) based on the crystal orientation of the nitride semiconductor substrate, The laser diode is an edge-emitting type laser diode that emits light in the crystal orientation <1-100> of the nitride semiconductor substrate.

4. The laser diode of claim 3.

5. The nitride semiconductor substrate is an AlN single crystal substrate.

5. The laser diode according to claim 2, wherein the first and second electrodes are arranged in a first direction.

6. The semiconductor laminate portion is a first conductivity type waveguide layer disposed between the first conductivity type cladding layer and the light emitting layer to confine light to the light emitting layer; a second conductive type waveguide layer disposed between the second conductive type cladding layer and the light emitting layer to confine light to the light emitting layer; 6. The laser diode according to claim 2,

7. a second conductive type contact layer disposed on the second conductive type cladding layer and formed of a nitride semiconductor containing GaN; The second conductive type cladding layer is made of Al e G 1-e a second conductivity type vertical conduction layer having a thickness of less than 0.5 μm, the second conductivity type vertical conduction layer including N (0.1≦e≦1), the Al composition e of which decreases with increasing distance from the nitride semiconductor substrate; f G 1-f N (0<f≦1), 7. The laser diode of claim 6.

8. A second conductive type vertical conduction layer is disposed between the second conductive type vertical conduction layer and the second conductive type waveguide layer. g G 1-g An intermediate layer formed of N (0<g≦1.0); 8. The laser diode of claim 7.

9. The thickness of the second conductive type vertical conductive layer is 250 nm or more and 450 nm or less.

9. The laser diode according to claim 7 or 8.

10. a part or all of a region of the second conductive type vertical conduction layer including an interface with the second conductive type waveguide layer is a region that is not doped with impurities; 10. The laser diode according to claim 7.

11. The first conductive type cladding layer is made of Al a G 1-a N (0.6<a≦0.8), the second conductive type vertical conduction layer and the second conductive type lateral conduction layer are formed with complete strain with respect to the nitride semiconductor substrate; 11. The laser diode according to claim 7.

12. the Al composition f of the second conductive type lateral conduction layer at a surface facing the second conductive type vertical conduction layer is greater than a minimum value of the Al composition e of the second conductive type vertical conduction layer; 12. A laser diode according to any one of claims 7 to 11.

13. a second electrode provided on the second conductive type cladding layer in a region that is 5 μm or more away from a side surface of the mesa structure in a plan view; Equipped 13. A laser diode according to any one of claims 2 to 12.

14. The mesa structure has a rectangular shape having long and short sides in a plan view, and the long sides are parallel to the <1-100> direction.

14. A laser diode according to any one of claims 2 to 13.

Citation Information

Patent Citations

  • Production process of ii-vi compd. semiconductor device

    JP1995335985A

  • Group iii nitride semiconductor element, manufacturing method thereof and group iii nitride semiconductor substrate

    JP2004071657A

  • Gallium nitride-based semiconductor light-emitting element, method of producing the same, gallium nitride-based light-emitting diode, epitaxial wafer, and method of producing the same diode

    JP2010114418A

  • Relief of strain in group III nitride heterostructures due to substrate and epitaxial layer patterning

    JP2013544027A

  • Hybrid heterostructure light-emitting device

    JP2017531327A