Alumina-based composite fiber, its manufacturing method and product

Plasma surface modification and spatially separated atomic layer deposition are used to produce alumina-based composite fibers with a uniform alumina coating, addressing non-uniformity issues and enhancing mechanical and thermal performance.

JP7589955B2Active Publication Date: 2024-11-26HUAZHONG UNIV OF SCI & TECH +1
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023539877
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-30
Filing Date
2021-11-24
Publication Date
2024-11-26
Estimated Expiration
2041-11-24

AI Technical Summary

Technical Problem

Existing methods for producing alumina-based composite fibers result in non-uniform coating layers due to nano-alumina particle aggregation, leading to poor high-temperature antioxidant performance and mechanical properties.

Method used

A method involving plasma surface modification of polymer fibers under an external magnetic field, followed by spatially separated atomic layer deposition to uniformly deposit an alumina thin film on the fiber surface.

Benefits of technology

The method enhances the wettability and adhesiveness of the fiber surface, resulting in a more uniform alumina coating with stronger bonding, thereby improving mechanical properties and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589955000004
    Figure 0007589955000004
  • Figure 0007589955000005
    Figure 0007589955000005
  • Figure 0007589955000001
    Figure 0007589955000001
Patent Text Reader

Abstract

The present invention relates to an alumina-based composite fiber, its manufacturing method and product. The manufacturing method of the alumina-based composite fiber includes the steps of surface-modifying a polymer fiber by using plasma under the action of an external magnetic field to introduce polar groups (S10) and depositing an alumina thin film on the surface of the modified polymer fiber by using spatially resolved atomic layer deposition (S30).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to a Chinese patent application with application number 202011629302.7, filed with the State Intellectual Property Office on December 30, 2020, and entitled "Alumina-based composite fiber, its manufacturing method and product," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of composite materials, and in particular to alumina-based composite fibers, their manufacturing methods and products. [Background technology]

[0003] High molecular weight polymer fibers have excellent properties such as strength and wear resistance, and are the fastest growing and most widely produced fiber type, but high molecular weight polymer fibers usually have poor high-temperature anti-oxidation performance. Alumina has excellent high-temperature anti-oxidation performance and can be applied in high-temperature ranges up to 1400°C, and has relatively good applications in reinforced composite materials, industrial high-temperature furnaces, and environmental protection and recycling fields. In addition, the source of manufacturing raw materials is wide, the production process is simple, and the process parameters are easy to determine, so it has extremely high commercial value. Therefore, alumina-based composite fibers, which are made by combining alumina as a reinforcing material with high molecular weight polymer fibers, have better performance and can be used in a wider range of high-temperature environments.

[0004] In the prior art, the mainstream method for producing alumina-based composite fibers is the impregnation method, in which nano-alumina is prepared into a coating solution for coating polymer fibers. However, because nano-alumina particles are small, they tend to aggregate, making it impossible to form a uniform coating layer, resulting in poor quality of the resulting composite fibers, the coating layer easily falling off, and little improvement in high-temperature antioxidation performance and mechanical properties. Summary of the Invention [Problem to be solved by the invention]

[0005] Based on this, there is a need to provide an alumina-based composite fiber, a method for producing the same, and an article of manufacture thereof. [Means for solving the problem]

[0006] In one aspect of the present invention, a method for producing an alumina-based composite fiber is provided, which includes step S10 of surface-modifying a polymer fiber using plasma under the action of an external magnetic field to introduce polar groups, and step S30 of depositing an alumina thin film on the surface of the modified polymer fiber using spatially resolved atomic layer deposition technology.

[0007] In one embodiment, in step S10, the magnetic field strength of the external magnetic field is 23.5B to 118B.

[0008] In one embodiment, in step S10, the plasma processing time is 0.1 to 1 minute.

[0009] In one embodiment, the plasma is selected from one or more of an oxygen plasma, a nitrogen plasma, and an air plasma.

[0010] In one embodiment, step S30 includes: Step S301: disposing the modified high molecular weight polymer fiber on a substrate of a spatially separated atomic layer deposition apparatus, the spatially separated atomic layer deposition apparatus further comprising a jetting head unit, the jetting head unit comprising a precursor A jetting head, a separation gas jetting head and a precursor B jetting head; The substrate is passed through the precursor A jetting head, the separation gas jetting head, and the precursor B jetting head in sequence; When the substrate is passed through the precursor A jetting head, the precursor A jetted from the precursor A jetting head forms a monolayer of a first reaction product on the surface of the substrate by chemical adsorption; removing unreacted precursors and reaction by-products by a separation gas ejected from the separation gas ejection head when the substrate passes through the separation gas ejection head; Step S302, when the substrate is passed through the precursor B jetting head, the precursor B jetted from the precursor B jetting head reacts with the first reaction product to obtain an alumina single layer thin film; and step S303 of relatively reciprocating the substrate and the jetting head unit to form a multi-layer thin film.

[0011] In one embodiment, the height h of the micro gap zone between the jetting head unit and the substrate is 0.3 mm to 0.8 mm.

[0012] In one embodiment, the reaction temperature of the substrate is 90°C to 150°C.

[0013] In one embodiment, the relative movement speed between the substrate and the jetting head unit is 0.05 m / s to 0.4 m / s.

[0014] In one embodiment, the flow rates of the precursor A, the precursor B, and the separation gas are between 1000 sccm and 1200 sccm.

[0015] In one embodiment, between steps S10 and S30, a step S20 of irradiating the modified polymer fiber with ultraviolet light is further included.

[0016] In one embodiment, the polymeric fibers are selected from one or more of polyethylene fibers, polypropylene fibers, polyimide fibers, polyetherimide fibers, polyaryletherketone fibers, polysulfone fibers, polyphenylene sulfide fibers, aramid, polyurethane fibers, polyester fibers, polyacrylonitrile fibers, polyamide fibers, and acrylic fibers.

[0017] In another aspect of the present invention, there is further provided an alumina-based composite fiber obtained by the above-mentioned method for producing an alumina-based composite fiber, the alumina-based composite fiber comprising a high molecular weight polymer fiber core and an alumina layer coating the surface of the high molecular weight polymer fiber core.

[0018] In yet another aspect of the present invention, there is further provided an article of manufacture comprising the above-described alumina-based composite fiber. Effect of the Invention

[0019] According to the method for producing alumina-based composite fibers provided by the present invention, under the action of an external magnetic field, polar groups are introduced into the surface of polymeric polymer fibers through surface modification by plasma to improve the wettability and adhesiveness of the fiber surface, and the introduction of an external magnetic field can effectively improve the uniformity of the plasma treatment and the stability of the fiber surface, and alumina can be deposited on the surface by combining with spatially separated atomic layer deposition technology. Alumina is easy to grow and form a film on the fiber surface uniformly, and the bonding strength between alumina and fiber is also stronger. Compared with the prior art, according to the method for producing alumina-based composite fibers of the present invention, the alumina thin film deposited on the fiber surface is more uniform, and the bonding strength between alumina and fiber is stronger, so that the mechanical properties and heat resistance of the alumina-based composite fibers can be greatly improved. The method for producing alumina-based composite fibers provided by the present invention is particularly suitable for producing an alumina thin film for covering a large area of ​​fiber surface. [Brief description of the drawings]

[0020] [Figure 1] 1 is a schematic flow diagram of a method for producing an alumina-based composite fiber of the present invention. [Diagram 2] FIG. 2 is a structural schematic diagram of spatially resolved atomic layer deposition in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In order to facilitate understanding of the present invention, the present invention will now be described in more detail with reference to the accompanying drawings. Preferred embodiments of the present invention are illustrated in the accompanying drawings. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein. On the contrary, these embodiments are provided to provide a more complete and comprehensive understanding of the present disclosure.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art of the present invention.Terms used herein in describing the present invention are only intended to describe specific embodiments and are not intended to limit the present invention.The term "and / or" used herein includes any combination of one or more of the associated listed items.

[0023] Unless indicated in the operating examples or otherwise expressly stated, all numbers used in the specification and claims expressing amounts of ingredients, physicochemical properties, and the like are understood to be modified in all cases by the term "about". For example, unless stated to the contrary, all numerical parameters recited in the foregoing specification and the appended claims are approximate, and those skilled in the art can appropriately modify these approximations to obtain desired properties using the teachings disclosed herein. Numerical ranges by endpoints include all numbers within that range and any range within that range. For example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.

[0024] Referring to FIG. 1, the present invention provides a method for producing an alumina-based composite fiber, which includes step S10 of surface-modifying a polymer fiber using plasma under the action of an external magnetic field, and step S30 of depositing an alumina thin film on the surface of the modified polymer fiber using spatially resolved atomic layer deposition technology.

[0025] According to the method for producing alumina-based composite fibers provided by the present invention, under the action of an external magnetic field, polar groups are introduced into the surface of polymeric fibers through surface modification by plasma to improve the wettability and adhesiveness of the fiber surface, and the introduction of an external magnetic field can effectively improve the uniformity of the plasma treatment and the stability of the fiber surface, and alumina can be deposited on the surface by combining with spatially separated atomic layer deposition technology. Alumina is easy to grow and form a film on the fiber surface uniformly, and the bonding strength between alumina and fiber is also strong. Compared with the prior art, according to the method for producing alumina-based composite fibers of the present invention, the alumina thin film deposited on the fiber surface is more uniform, and the bonding strength between alumina and fiber is stronger, so that the mechanical properties and heat resistance of the alumina-based composite fibers can be greatly improved. The method for producing alumina-based composite fibers provided by the present invention is particularly suitable for producing an alumina thin film for covering a large area of ​​fiber surface.

[0026] High molecular weight polymer fibers include, but are not limited to, polyethylene fibers, polypropylene fibers, polyimide fibers, polyetherimide fibers, polyaryletherketone fibers, polysulfone fibers, polyphenylene sulfide fibers, aramid, polyurethane fibers, polyester fibers, polyacrylonitrile fibers, polyamide fibers, acrylic fibers, and combinations thereof.

[0027] In step S10, the magnetic field strength of the external magnetic field can be any value between 23.5B and 118B, for example, 25B, 30B, 35B, 40B, 45B, 50B, 55B, 60B, 65B, 70B, 75B, 80B, 85B, 90B, 95B, 100B, 105B, 110B, 115B. If the magnetic field strength is too low, the surface roughness of the polymeric polymer fiber will decrease, the surface adsorption ability will decrease, the surface energy will decrease, and the contact angle will increase. If the magnetic field strength is too high, the number of polar groups will decrease. With the magnetic field strength between 23.5B and 118B, more favorable conditions for the uniform growth of alumina will be obtained.

[0028] The magnetic field may be a modulated magnetic field with a modulation frequency of 5Hz to 1Hz obtained by modulating an electric field of 300Hz to 60Hz. The electric field waveform may be a sine wave or a square wave. Magnetic field strength B*42.577=frequency.

[0029] In step S10, the plasma treatment time can be any value between 0.1 and 1 minute, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, or 0.9 minutes. When the plasma treatment time is between 0.1 and 1 minute, the oxygen atomic percentage on the polymer surface increases, and when the plasma treatment time exceeds 1 minute, the oxygen atomic percentage on the polymer surface decreases.

[0030] The plasma includes, but is not limited to, O2 plasma, CO plasma, CO2 plasma, H2O plasma, N2 plasma, NO plasma, NO2 plasma, NH3 plasma, N2-H2 mixed gas plasma, fluorine plasma, air plasma, and inert gas plasma, etc. Preferably, the plasma is selected from one or more of O2 plasma, N2 plasma, and air plasma.

[0031] The polar group may be an oxygen-containing group, such as a carbonyl group or a hydroxyl group, or a nitrogen-containing group, such as a nitrile, amine, or imine.

[0032] In some embodiments, step S30 includes: Step S301: disposing the modified high molecular weight polymer fiber on a substrate of a spatially separated atomic layer deposition apparatus, the spatially separated atomic layer deposition apparatus further comprising a jetting head unit, the jetting head unit comprising a precursor A jetting head, a separation gas jetting head and a precursor B jetting head; The substrate is passed sequentially through a precursor A jet head, a separation gas jet head, and a precursor B jet head; When the substrate is passed through the precursor A jet head, the precursor A jetted from the precursor A jet head forms a monolayer of a first reaction product on the surface of the substrate by chemical adsorption; When the substrate passes through a separation gas jet head, unreacted precursors and reaction by-products are removed by a separation gas jetted from the separation gas jet head; a step S302 in which, when the substrate is passed through the precursor B jetting head, the precursor B jetted from the precursor B jetting head chemically reacts with the first reaction product to obtain an alumina single-layer thin film; and step S303 of relatively reciprocating the substrate and the jetting head unit to form a multi-layer thin film.

[0033] The spatially separated atomic layer deposition apparatus is a common apparatus in the art, and can be obtained by purchase or self-assembly. Referring to FIG. 2, the present invention provides a spatially separated atomic layer deposition apparatus, which includes a separation gas and precursor supply system 100, a deposition system 200, and a driving system 300. The deposition system includes a jetting head unit and a reaction unit, the reaction unit includes a substrate 21 and a heating device 22 disposed below the substrate, and the jetting head unit includes a plurality of jetting heads 11, including a precursor A jetting head, a separation gas jetting head, and a precursor B jetting head. The driving system 300 is electrically connected to the substrate 21 or the jetting head unit, and the driving system 300 is used to control the movement of the substrate 21 or the jetting head unit.

[0034] The precursor A jetting head is used to jet precursor A gas, the separation gas jetting head is used to jet separation gas, and the precursor B jetting head is used to jet precursor B. The separation gas jetting head is disposed between the precursor A jetting head and the precursor B jetting head.

[0035] 2, a microgap zone exists between the jet head 11 and the substrate 21, and the height of the microgap zone is h. The precursor A jet head, the separation gas jet head and the precursor B jet head are fixed as a whole on a support frame, and the height h of the microgap zone between each jet head and the substrate is the same.

[0036] The precursor A jet head, separation gas jet head, and precursor B jet head may be of the same or different construction, all of which are known in the art.

[0037] The separation gas can be any inert gas, such as N2, Ar, He, etc., and the separation gas is continuously injected to separate precursor A and precursor B.

[0038] In some embodiments, the height h of the micro-gap zone between the jetting head 11 and the substrate 21 can be any value between 0.3 mm and 0.8 mm, such as 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm. The larger the height h of the micro-gap zone, the lower the separation effect of the isolation gas, and the easier it is for precursor A and precursor B to mix and form a CVD deposit, which leads to unstable growth of alumina and non-uniform thickness of the coated alumina thin film.

[0039] In some embodiments, the reaction temperature of the substrate 21 may be any value between 90° C. and 120° C., such as 95° C., 100° C., 105° C., 110° C., or 115° C. The temperature of the reaction substrate affects the chemisorption ability of the substrate, so that a reaction temperature between 100° C. and 150° C. will make the substrate's chemisorption ability stronger, and will also remove moisture present in the gas, ensuring the stability of the deposition.

[0040] In step S302, the substrate 21 is driven by the driving system 300 to pass through the precursor A jetting head, the isolation gas jetting head, and the precursor B jetting head in sequence at a predetermined moving speed.

[0041] In some embodiments, the relative movement speed between the substrate 21 and the jetting head unit can be any value between 0.05 m / s and 0.4 m / s, for example, 0.06 m / s, 0.07 m / s, 0.08 m / s, 0.09 m / s, 0.1 m / s, 0.15 m / s, 0.2 m / s, 0.25 m / s, 0.3 m / s, and 0.35 m / s. The lower the relative movement speed between the substrate 21 and the jetting head unit, the longer the substrate is exposed under the jetting head, and the higher the adsorption rate for precursor A and precursor B, but the lower relative movement speed reduces the deposition efficiency. The relative movement speed between the substrate 21 and the jetting head unit is 0.05 m / s to 0.1 m / s, which can improve the deposition efficiency and ensure high-quality deposition effect, and does not waste raw materials.

[0042] In one embodiment, as shown in FIG. 2, a drive system 300 is electrically connected to the substrate 21 , and the drive system 300 controls the movement of the substrate 21 .

[0043] The flow rates of precursor A, precursor B, and the separation gas are any value between 1000 sccm and 1200 sccm.

[0044] The flow rates of precursor A, precursor B and the separation gas may be the same or different, but are preferably the same.

[0045] Alumina is obtained by reacting precursor A with precursor B. In one embodiment, precursor A is Al(CH3)3 (TMA) and precursor B is HO. In one embodiment, the separation gas is nitrogen. In some embodiments, nitrogen can be used as a carrier gas for precursor A and precursor B.

[0046] In step S303, the movement of the substrate 21 from the precursor A jetting head to the precursor B jetting head, or from the precursor B jetting head to the precursor A jetting head, is one cycle movement period.

[0047] In some embodiments, between steps S10 and S30, a step S20 of irradiating the modified polymer fiber with ultraviolet light is further included. In addition, ultraviolet light irradiation can cause chemical changes on the fiber surface, improving the wettability and adhesion of the fiber surface, and further ensuring the uniformity of the alumina deposition.

[0048] The duration of ultraviolet irradiation can be any value between 1 and 2 minutes, for example, 1.1 minutes, 1.2 minutes, 1.3 minutes, 1.4 minutes, 1.5 minutes, 1.6 minutes, 1.7 minutes, 1.8 minutes, or 1.9 minutes.

[0049] In some embodiments, the method further includes a step of pretreating the polymer fiber before step S10. The pretreatment step includes washing and drying the surface of the polymer fiber. The washing step may use an organic solvent such as anhydrous ethanol or acetone as a cleaning solution. In addition, cleaning with a plasma cleaning agent may also be used. In the drying step, nitrogen may be used to blow dry the fiber.

[0050] The present invention further provides an alumina-based composite fiber obtained by the above-mentioned method for producing an alumina-based composite fiber. The alumina-based composite fiber includes a polymer fiber core and an alumina layer covering the surface of the polymer fiber core.

[0051] In some embodiments, the alumina layer has a thickness between 20 nm and 100 nm.

[0052] The present invention further provides a product made of the above alumina-based composite fiber. EXAMPLES

[0053] Specific examples are given below. These specific examples are intended to explain the present invention in detail so that those skilled in the art and researchers can further understand the present invention, and the relevant technical conditions, etc. do not limit the present invention. Any modifications made within the scope of the claims of the present invention are within the scope of protection of the claims of the present invention.

[0054] <Example 1> 1. Plasma modification of polyester fibers (1) Pretreatment of polyester fiber surface The polyester fibers were immersed in absolute ethanol, washed in a plasma cleaner, wiped dry with a dust-free cloth or dust-free paper, and dried with a nitrogen gas gun.

[0055] (2) Plasma surface modification The pretreated polyester fiber was stored in a glove box to keep the surface clean and dry. It was then transferred to a plasma surface activation chamber. The plasma surface activation chamber was filled with oxygen, and a modulated magnetic field (magnetic field strength was 23.5 B) with a square waveform and a modulation frequency of 1 Hz was obtained using a signal generator with an AC discharge of 60 Hz. The polyester fiber was treated for 1 minute.

[0056] (3) Ultraviolet light irradiation The chamber was cleaned by blowing N2 into it, kept in a N2 atmosphere, and irradiated with ultraviolet light for 1 minute.

[0057] (4) Spatial separation atomic layer deposition Alumina thin films were deposited using a spatially resolved atomic layer deposition system as shown in Figure 2. The process parameters were set on the PC side. The flow rates of carrier gas (N2), separation gas (N2), precursor A (TMA), and precursor B (H2O) are all 1000sccm, the substrate temperature is 120°C, the height h of the micro-gap zone is 0.5mm, and the substrate moving speed is 0.1m / s. The specific procedure is as follows: 1) In order to reduce the influence of environmental factors in the reaction region, the nitrogen flow path was opened and purging was performed for 20 minutes. 2) The TMA and HO flow paths were opened and purged for 10 minutes to remove impurities from the pipeline. 3) The polyester fibers treated in step (3) were straightened and clamped to a reaction substrate. 4) The substrate was moved into the reaction area and purged for 2 minutes. 5) The substrate was moved back and forth for 100 cycles to obtain alumina-based composite fibers.

[0058] <Example 2> The manufacturing method of Example 2 was basically the same as that of Example 1, except that the height h of the microgap zone was set to 0.3 mm.

[0059] <Example 3> The manufacturing method of Example 3 was basically the same as that of Example 1, except that the height h of the microgap zone was set to 0.8 mm.

[0060] <Example 4> The manufacturing method of Example 4 was basically the same as that of Example 1, except that the substrate temperature was set to 100°C.

[0061] <Example 5> The manufacturing method of Example 5 was basically the same as that of Example 1, except that the moving speed of the substrate was set to 0.05 m / s.

[0062] <Example 6> The manufacturing method of Example 6 was basically the same as that of Example 1, except that the plasma treatment time in the plasma modification step of the polyester fiber was 0.1 minutes.

[0063] <Example 7> The manufacturing method of Example 7 is basically the same as that of Example 1, except that the magnetic field strength is 118 B in the plasma modification step of the polyester fiber.

[0064] <Example 8> The manufacturing method of Example 8 is basically the same as that of Example 1, except that the polyester fiber fabric is not irradiated with ultraviolet light.

[0065] <Comparative Example 1> The manufacturing method of Comparative Example 1 was basically the same as that of Example 1, except that the height h of the microgap zone was set to 1 mm.

[0066] <Comparative Example 2> The manufacturing method of Comparative Example 2 was basically the same as that of Example 1, except that the substrate temperature was 80°C.

[0067] <Comparative Example 3> The manufacturing method of Comparative Example 3 was basically the same as that of Example 1, except that the moving speed of the substrate was set to 0.5 m / s.

[0068] <Comparative Example 4> The manufacturing method of Comparative Example 4 was basically the same as that of Example 1, except that in the plasma modification step of the polyester fiber, the plasma treatment time was set to 2 minutes.

[0069] <Comparative Example 5> The manufacturing method of Comparative Example 5 was basically the same as that of Example 1, except that in the plasma modification step of the polyester fiber, the plasma treatment time was set to 5 minutes.

[0070] <Comparative Example 6> The manufacturing method of Comparative Example 6 was basically the same as that of Example 1, except that in the plasma modification step of the polyester fiber, the plasma treatment time was set to 10 minutes.

[0071] <Comparative Example 7> The manufacturing method of Comparative Example 7 was basically the same as that of Example 1, except that the polyester fibers were not modified by plasma treatment or irradiated with ultraviolet light, and alumina was directly deposited on the substrate.

[0072] <Comparative Example 8> The manufacturing method of Comparative Example 8 was basically the same as that of Example 1, except that no external magnetic field was applied in the plasma modification step of the polyester fiber.

[0073] The process parameters in the manufacturing methods of Examples 1 to 8 and Comparative Examples 1 to 8 are listed in Table 1 below.

[0074] [Table 1]

[0075] Using the alumina-based composite fibers produced in Examples 1 to 8 and Comparative Examples 1 to 8 as samples, thickness measurements were taken at five different points (points A, B, C, D, and E) for each fiber sample, and the positions of the five points taken for each sample were consistent, and the results are shown in Table 2. Here, the relative difference is the difference between the maximum value and the minimum value.

[0076] [Table 2]

[0077] From Table 1, it can be seen that the alumina-based composite fibers produced in the comparative examples had a large relative difference, and the alumina deposition was uneven or the alumina deposition layer was thin, resulting in waste of raw material, but the alumina coating film of the alumina-based composite fibers produced in Examples 1 to 8 was of appropriate and uniform thickness, resulting in a high utilization rate of raw material.

[0078] The alumina-based composite fibers produced in Example 1 and Comparative Example 1 were tested for heat resistance and tensile strength, and the results are shown in Table 3 below.

[0079] The test conditions or test standards for various performance test items were as follows:

[0080] Thermogravimetric analysis (TGA) test: Samples were weighed and tested in nitrogen or air atmosphere using a 1100SF standard thermogravimetric analyzer (Mettler Toledo, Switzerland). The temperature was raised from room temperature to the measurement temperature, and the heating rate was 10.0 K / min. The weight change of the sample with increasing temperature was observed, and if the weight loss reached 50%, it was deemed to have failed, and the test temperature at this time was the maximum heat-resistant temperature. The higher the maximum heat-resistant temperature value, the higher the temperature at which the sample can be safely used, and if the heat-resistant temperature exceeds 1000°C, the sample can be used in special environments such as high-temperature work, space technology, etc.

[0081] Tensile strength: The tensile strength of the fiber was measured using a XQ-1C type high strength high modulus fiber tensile tester. Measurement parameters: clamp distance 8mm, tensile speed 5mm / min, modulus start point 0.1%, modulus end point 0.7%, tension clamp load 0.2cN.

[0082] [Table 3]

[0083] From Table 2 above, it can be seen that, compared with the alumina-based composite fiber produced in Comparative Example 1, the alumina-based composite fiber produced in Example 1 is superior in heat resistance and tensile strength.

[0084] Although the technical features of the above embodiments may be combined in any manner, for the sake of brevity, not all possible combinations of the technical features of the above embodiments are described, but combinations of these technical features should be considered to be within the scope described herein unless there is a contradiction.

[0085] The above embodiments only represent some embodiments of the present invention, and the description is relatively specific and detailed, but should not be construed as limiting the patent scope of the present invention. It should be noted that those skilled in the art can make some modifications and improvements without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention should be based on the attached claims.

Claims

1. Step S10 of surface-modifying the polymer fiber using plasma under the action of an external magnetic field to introduce polar groups; and (S30) depositing an alumina thin film on the surface of the modified polymer fiber using spatially resolved atomic layer deposition technology.

2. 2. The method for producing an alumina-based composite fiber according to claim 1, wherein in step S10, the magnetic field strength of the external magnetic field is 23.5B to 118B.

3. 2. The method for producing an alumina-based composite fiber according to claim 1, wherein in step S10, the plasma treatment time is 0.1 to 1 minute.

4. 2. The method of claim 1, wherein the plasma is selected from one or more of an oxygen plasma, a nitrogen plasma, and an air plasma.

5. Step S30 Step S301, the modified high molecular weight polymer fiber is disposed on a substrate of a spatially separated atomic layer deposition apparatus, the spatially separated atomic layer deposition apparatus further includes a jetting head unit, the jetting head unit includes a precursor A jetting head, a separation gas jetting head, and a precursor B jetting head; passing the substrate sequentially through the precursor A jetting head, the separation gas jetting head, and the precursor B jetting head; When the substrate is passed through the precursor A jetting head, the precursor A jetted from the precursor A jetting head forms a monolayer of a first reaction product on the surface of the substrate by chemical adsorption; removing unreacted precursors and reaction by-products by a separation gas ejected from the separation gas ejection head when the substrate passes through the separation gas ejection head; Step S302: when the substrate is passed through the precursor B jetting head, the precursor B jetted from the precursor B jetting head reacts with the first reaction product to obtain an alumina single layer thin film; and (S303) moving the substrate and the ejection head unit back and forth relative to each other to form a multi-layered thin film.

6. 6. The method for producing an alumina-based composite fiber according to claim 5, wherein the height h of the micro-gap zone between the ejection head unit and the substrate is 0.3 mm to 0.8 mm.

7. The method for producing an alumina-based composite fiber according to claim 5, characterized in that the reaction temperature of the substrate is 90°C to 120°C.

8. 6. The method for producing an alumina-based composite fiber according to claim 5, wherein the relative movement speed between the substrate and the ejection head unit is 0.05 m / s to 0.4 m / s.

9. 6. The method for producing an alumina-based composite fiber according to claim 5, wherein the flow rates of the precursor A, the precursor B and the separation gas are 1000 sccm to 1200 sccm.

10. The method for producing an alumina-based composite fiber according to any one of claims 1 to 9, further comprising a step S20 between steps S10 and S30, of irradiating the modified polymer fiber with ultraviolet light.

11. The method for producing an alumina-based composite fiber according to any one of claims 1 to 9, characterized in that the high molecular weight polymer fibers are selected from one or more of polyethylene fibers, polypropylene fibers, polyimide fibers, polyetherimide fibers, polyaryletherketone fibers, polysulfone fibers, polyphenylene sulfide fibers, aramid, polyurethane fibers, polyester fibers, polyacrylonitrile fibers, polyamide fibers, and acrylic fibers.

Citation Information

Patent Citations

  • Device and method for depositing ultrathin alumina film by atomic layer

    CN101921994A

  • Preparation method of alumina-tin oxide composite nanotube

    CN103105419A

  • Preparation method of oxide ceramic coating layer on surface of silicon carbide fiber

    CN104213099A

  • Oriented carbon nano tube and aluminum oxide hybrid fiber and preparation method thereof

    CN105420689A

  • Preparation method of quantum dot film

    CN105779968A