Compositions containing polysilazan compounds

A polysilazane compound composition with a xanthene dye and amine compound improves film visibility and curability, addressing the challenge of recognizing polysilazane films under varying conditions.

JP7590150B2Active Publication Date: 2024-11-26SHIN ETSU CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020172562
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-13
Publication Date
2024-11-26
Estimated Expiration
2040-10-13

AI Technical Summary

Technical Problem

Polysilazane-based siliceous films are difficult to visually recognize due to their colorlessness and transparency, and existing methods to enhance visibility either compromise the film composition or are ineffective under varying environmental conditions.

Method used

A polysilazane compound-containing composition incorporating a xanthene dye and an amine compound with a chain aliphatic amino group, which enhances light absorption and luminescence, allowing visibility under natural light and luminescence under irradiation, while maintaining excellent curability.

Benefits of technology

The composition enables polysilazane films to be visibly recognized under both natural light and irradiation, with improved curability and film properties such as strength and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590150000001
    Figure 0007590150000001
  • Figure 0007590150000002
    Figure 0007590150000002
  • Figure 0007590150000003
    Figure 0007590150000003
Patent Text Reader

Abstract

To provide a polysilazane compound-containing composition which improves visibility of a silica film, formed by a polysilazane compound, inherently colorless and transparent as it is, and poor in visual recognition, for giving a cured film capable of visually recognizing the existence of a siliceous film in natural light, and capable of visually recognizing the existence of the siliceous film, even in a dark place by light irradiation, and further excellent in curability.SOLUTION: A polysilazane compound-containing composition includes: (A) a polysilazane compound; (B) a rhodamine-based dye, or a xanthene-based dye; (C) an organic solvent; and (D) an amine-based compound having a linear aliphatic amino group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polysilazane compound-containing composition. [Background technology]

[0002] Polysilazane compounds form a high-quality siliceous glass film by curing, and therefore exhibit excellent gas barrier properties, heat resistance, and insulation properties. Since electronic components are required to have high reliability when used in high-temperature environments, the above-mentioned siliceous glass film is useful as a protective film that prevents moisture and corrosive gases from entering the electronic components. Patent Document 1 reports that the water vapor permeation rate of a resin sheet intended for sealing an organic EL element can be reduced by applying a polysilazane compound to the surface of the resin sheet to form a siliceous glass film. This result indicates that polysilazane compounds are useful for forming a moisture-proof coating.

[0003] Another feature of the siliceous film formed from the polysilazane compound is that it is essentially colorless and has excellent transparency. However, due to this feature, it is extremely difficult to visually confirm the presence of the protective film. For this reason, it may hinder the streamlining of product manufacturing processes, including the coating process of the polysilazane compound. In order to visually confirm such a film, it is necessary that the film has light absorption in the visible light wavelength region or emits light in the visible light wavelength region. Coloring due to light absorption is a direct and simple means for making the film visible under natural light. On the other hand, when the light reflection from the coated substrate is weak or in a dark place, coloring due to light absorption becomes meaningless for the visibility of the film. In such cases, the film becomes visible when it emits light when irradiated with light of a specific wavelength. Since the usage environment and viewing conditions of the substrate on which the film is formed vary depending on the environment in which the user is placed, it cannot be said with certainty which of the above two viewing methods is superior. Therefore, the challenge is to make it possible to apply both viewing methods to a composition of the same formulation. One solution to this problem is to add a dye compound that absorbs light in the visible light region and also emits light to a polysilazane compound-containing composition.

[0004] When the film thickness is small, the absolute amount of the dye compound that contributes to visibility is reduced. As a result, the visibility of the film is reduced. To compensate for the deficiency in the absolute amount, it is possible to increase the amount of the dye compound added to the composition, but this is not preferable because it results in a deviation from the original film composition, and the solubility of the dye compound is limited in the first place. Therefore, it is necessary to efficiently color the film with a small amount of addition.

[0005] For these reasons, there is a need for the development of technology that can efficiently color even small amounts of dye and also emit light, making the presence of a siliceous film visible from the standpoints of both coloration and light emission. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2018 / 174116 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above problems, and has an object to provide a polysilazane compound-containing composition that improves the visibility of a siliceous film formed from a polysilazane compound, which is essentially colorless and transparent and has poor visibility as it is, and that gives a cured film in which the presence of the siliceous film can be visually recognized under natural light and also in a dark place by irradiation with light, and that further has excellent curability. [Means for solving the problem]

[0008] The present invention has been made to achieve the above object, and provides a polysilazane compound-containing composition exhibiting the following characteristics.

[0009] That is, a polysilazane compound-containing composition, (A) a polysilazane compound, (B) a xanthene dye represented by the following formula (B-1) or the following formula (B-2): [ka] (In the formula, R 1 are each independently a hydrogen atom, a methyl group, or an ethyl group; R 2 are each independently a hydrogen atom or a methyl group, and X is a chloride ion or a perchlorate ion. [ka] (In the formula, R 3 are each independently a hydrogen atom or a halogen atom, and R 4 is a hydrogen atom, an amino group, a nitro group, a carboxyl group, an isothiocyanate group, a maleimide group, a semicarbazide group, or a thiosemicarbazide group. (C) an organic solvent, and (D) an amine compound having a chain aliphatic amino group, The present invention provides a polysilazane compound-containing composition comprising:

[0010] Such a polysilazane compound-containing composition is a polysilazane compound-containing composition that improves the visibility of a siliceous film formed from a polysilazane compound, which is essentially colorless and transparent and has poor visibility as it is, and gives a cured film whose presence is visible under natural light and whose presence is visible even in a dark place upon irradiation with light, and further is a polysilazane compound-containing composition with excellent curability.

[0011] In the present invention, the component (A) is preferably perhydropolysilazane.

[0012] Such a polysilazane compound-containing composition can improve the effects of the present invention.

[0013] In the present invention, the blending amount of the component (D) is preferably 1 to 10 parts by mass per 100 parts by mass of the component (A).

[0014] Such a polysilazane compound-containing composition can provide more favorable curability and more favorable visibility of the cured film.

[0015] In the present invention, the polysilazane compound-containing composition may further contain (E) an inorganic filler.

[0016] Such a polysilazane compound-containing composition can improve the properties (strength, heat resistance, insulating property, etc.) of the resulting cured film. Effect of the Invention

[0017] According to the present invention, the polysilazane compound-containing composition containing the xanthene dye having a preferred structure and the specific amine compound has excellent curability, and the polysilazane compound cured film has increased absorption in the visible light region. Furthermore, the composition can give a cured product that is visible from the viewpoints of both coloration and emission by irradiating it with light of, for example, 365 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] As described above, there has been a demand for the development of a polysilazane compound-containing composition capable of improving visibility.

[0019] In particular, in order to maximize the above-mentioned characteristics of the siliceous film, it is necessary to reduce the amount of dye added for visualization and to efficiently color and emit light. Therefore, the present inventors have come up with the idea of ​​searching for a dye to be added and a blending composition of additives that will enhance the effect of the dye in improving visibility.

[0020] As a result of intensive research into the above-mentioned problems, the present inventors have found that a polysilazane compound-containing composition containing an appropriate combination of a xanthene dye and an amine compound increases the absorption in the visible light region of a cured film of the polysilazane compound, and further emits light upon irradiation with light of, for example, 365 nm, thereby providing a cured product that is visible from the standpoints of both coloration and light emission, and further the cured film has excellent curability, thereby completing the present invention.

[0021] That is, the present invention provides a polysilazane compound-containing composition, (A) Polysilazane compound (B) A xanthene dye represented by the following formula (B-1) or the following formula (B-2): [ka] (In the formula, R 1 are each independently a hydrogen atom, a methyl group, or an ethyl group; R 2 are each independently a hydrogen atom or a methyl group, and X is a chloride ion or a perchlorate ion. [ka] (In the formula, R 3 are each independently a hydrogen atom or a halogen atom, and R 4 is a hydrogen atom, an amino group, a nitro group, a carboxyl group, an isothiocyanate group, a maleimide group, a semicarbazide group, or a thiosemicarbazide group. (C) an organic solvent, and (D) Amine compounds having a chain aliphatic amino group The polysilazane compound-containing composition is characterized by comprising:

[0022] The following describes the embodiments of the present invention, but these are presented as examples, and it goes without saying that the present invention is not limited to these and various modifications are possible.

[0023] <(A) Polysilazane compound> The polysilazane compound (A) constituting the polysilazane compound-containing composition of the present invention forms a glassy cured film by curing. The polysilazane compound is not particularly limited, but examples thereof include perhydropolysilazane, which is an inorganic polysilazane, or modified polysilazanes such as methylpolysilazane, dimethylpolysilazane, phenylpolysilazane, and vinylpolysilazane, which are organic polysilazanes; hydrocarbon compounds having reactive groups such as hydroxyl groups, vinyl groups, amino groups, and silyl groups that chemically react with polysilazane to form a crosslinked structure; cyclic saturated hydrocarbon compounds, cyclic unsaturated hydrocarbon compounds, saturated heterocyclic compounds, unsaturated heterocyclic compounds, and crosslinked polysilazanes chemically crosslinked with compounds such as silicone compounds. The polysilazane compound can be arbitrarily selected from one type alone, a mixture of polysilazanes selected from two or more types, or a polysilazane copolymer consisting of two or more types of polysilazane structures, and preferably contains at least one hydrogen atom directly bonded to a silicon atom in one molecule, and more preferably perhydropolysilazane.

[0024] From the viewpoint of solubility in the organic solvent (C) and workability during application, the polysilazane compound preferably has a weight-average molecular weight in the range of 100 to 100,000,000, preferably 1,000 to 1,000,000, and more preferably 2,000 to 500,000. A weight-average molecular weight of 100 or more is preferable because it has low volatility and there is no risk of the film quality of the coating film being deteriorated due to the volatilization of the organic solvent and the volatilization of the polysilazane compound itself during the curing process, while a weight-average molecular weight of 100,000,000 or less is preferable because it has high solubility in the organic solvent.

[0025] The weight average molecular weight referred to in this specification refers to a value obtained by gel permeation chromatography (GPC) measured under the following conditions using polystyrene as a standard substance. [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Differential refractive index detector Column: TSKguardcolumn SuperMP(HZ)-M TSKgel SuperMultipore HZ-M (4.6mmI.D.×15cm,4μm×4) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (THF solution with a concentration of 0.5% by mass)

[0026] <(B) Xanthene dye> (B) The xanthene dye is added to the polysilazane compound-containing composition of the present invention to improve the visibility of the cured film. In order to visually recognize the siliceous film obtained from the polysilazane compound, as described above, it is necessary that the film has light absorption in the visible light wavelength region or emits light in the visible light wavelength region. That is, considering that the visible light wavelength region is generally 380 to 780 nm, the xanthene dye used must have light absorption or emit light in the wavelength region of 380 to 780 nm.

[0027] Furthermore, the luminescence of these xanthene dyes is caused by absorbing light of a specific wavelength. The wavelength of the irradiated light is such that the molecules of the xanthene dye are electronically excited, and is preferably within the range of 200 to 1,000 nm.

[0028] Specific examples of the xanthene dye include rhodamine compounds such as rhodamine B, rhodamine 6G, rhodamine 110, rhodamine 123, rhodamine 590 chloride, and rhodamine 6G perchlorate; fluorescein, 2',7'-chlorofluorescein, 4',5'-dibromofluorescein, tetraiodofluorescein, 5-aminofluorescein, 6-aminofluorescein, 5-nitrofluorescein, 6-nitrofluorescein, and 5-carboxyfluorescein. Examples of fluorescein compounds include fluorescein, 6-carboxyfluorescein, fluorescein-5-isothiocyanate, fluorescein-6-isothiocyanate, fluorescein-5-maleimide, fluorescein-6-maleimide, fluorescein-5-semicarbazide, fluorescein-6-semicarbazide, fluorescein-5-thiosemicarbazide, and fluorescein-6-thiosemicarbazide. Of these, rhodamine B or fluorescein is preferable.

[0029] The xanthene dyes may be used alone or in combination of two or more kinds.

[0030] The amount of the xanthene colorant (B) added is preferably 1 to 3 parts by mass relative to 100 parts by mass of the polysilazane compound (A).

[0031] These xanthene dyes are generally in equilibrium between an open-ring structure and a lactone structure. The cases of the above formulae (B-1) and (B-2) are shown below. [ka]

[0032] As specific examples, the cases of rhodamine B and fluorescein are shown below. [ka]

[0033] In the xanthene dye, the lactone structure does not have conjugation extending over the entire molecule, but the ring-open structure has conjugation extending over the entire molecule, so that the ring-open structure absorbs and emits light in the visible light wavelength region. Even if the same amount of xanthene dye is used, it is preferable to have a higher ratio of the ring-open structure because it contributes more to improving visibility. In addition, the ratio of the ring-open structure increases by adding the component (D) described later. This enhances absorption in the visible light wavelength region and increases the amount of light emitted, so that the polysilazane compound-containing composition of the present invention provides a siliceous film with excellent visibility. That is, the siliceous film formed by the polysilazane compound is essentially colorless and transparent and has poor visibility as it is, but its presence can be visually recognized under natural light, and its presence can be visually recognized even in a dark place by light irradiation. Furthermore, as described later, the component (D) promotes the curing reaction of the component (A), so that the polysilazane compound-containing composition of the present invention also has excellent curability.

[0034] Advantages of using xanthene dyes include high light absorption and emission intensity, excellent light resistance, low biotoxicity, and high water solubility compared to other organic dyes.

[0035] <(C) Organic solvent> The polysilazane compound used in the present invention is diluted with an organic solvent in order to improve workability during application and storage stability. The organic solvent is not particularly limited as long as it dissolves the polysilazane compound (A) and the xanthene dye (B). For example, saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, n-nonane, isononane, n-decane, and isodecane; unsaturated aliphatic hydrocarbons such as 1-octene, 1-nonene, 1-decene, 1-dodecene, and β-myrcene; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, and decahydronaphthalene; unsaturated alicyclic hydrocarbons such as cyclohexene; terpene compounds such as p-menthane, d-limonene, l-limonene, and dipentene; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; acetone, methylbenzene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; ketone compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, ethyl acetoacetate, and ethyl caproate; alkyl ether compounds such as diethyl ether, di-n-propyl ether, di-n-butyl ether, di-n-pentyl ether, di-n-hexyl ether, and tert-butyl methyl ether; aryl ether compounds such as anisole and diphenyl ether; and glycol ether compounds such as bis(2-methoxyethyl)ether, bis(2-ethoxyethyl)ether, and bis(2-butoxyethyl)ether.

[0036] From the viewpoint of workability during application and storage stability of the polysilazane compound, the dilution ratio is preferably within the range of 100 to 100,000 parts by mass, and more preferably 400 to 10,000 parts by mass, of the (C) organic solvent per 100 parts by mass of the (A) polysilazane compound, from the viewpoint of workability during application and storage stability of the polysilazane compound.

[0037] The water content in the polysilazane compound-containing composition of the present invention is preferably 500 ppm or less, more preferably 300 ppm or less. If the water content is 500 ppm or less, polysilazane and the contained water do not react with each other, so there is no risk of heat generation, hydrogen gas or ammonia gas generation, and there is no risk of thickening or gelation. Therefore, it is preferable that the water content in the (C) organic solvent is controlled so that the water content in the polysilazane compound-containing composition of the present invention is within the above range.

[0038] <(D) Amine compounds having a chain aliphatic amino group> As mentioned above, the amine compound (D) having a chain aliphatic amino group increases the proportion of open-ring structures in the equilibrium structure of component (B), and has the effect of enhancing the absorption and emission of component (B) in the visible light wavelength range. In addition to this effect, it also has the effect of accelerating the curing reaction of component (A).

[0039] The amine compound of component (D) is not particularly limited as long as it has an amino group substituted with a chain aliphatic hydrocarbon group (chain aliphatic amino group), and the aliphatic hydrocarbon group may be linear or branched, the nitrogen atoms may be linked to each other via the aliphatic hydrocarbon group, and may be substituted with a heteroatom other than a nitrogen atom, such as an oxygen atom. When the aliphatic hydrocarbon group is monovalent, it is preferably a trialkoxysilyl-modified alkyl group, more preferably a trialkoxysilyl-modified alkyl group having 2 to 6 carbon atoms, and when it is divalent, it is preferably a linear alkylene group, more preferably a linear alkylene group having 3 to 8 carbon atoms.

[0040] Examples of the amine compounds used in the present invention include methylamine, dimethylamine, trimethylamine, ethylamine, diethylamine, triethylamine, n-propylamine, isopropylamine, di-n-propylamine, diisopropylamine, tri-n-propylamine, triisopropylamine, n-butylamine, sec-butylamine, isobutylamine, tert-butylamine, di-n-butylamine, di-sec-butylamine, diisobutylamine, di-tert-butylamine, tri-n-butylamine, tri-sec -butylamine, triisobutylamine, tri-tert-butylamine, n-pentylamine, 2-pentylamine, 3-pentylamine, isopentylamine, neopentylamine, di-n-pentylamine, diisopentylamine, dineopentylamine, tri-n-pentylamine, triisopentylamine, trimeopentylamine, n-hexylamine, di-n-hexylamine, tri-n-hexylamine, n-octylamine, di-n-octylamine, tri-n-octylamine, 1,2-diaminoethane, N,N'-dimethyl- 1,2-diaminoethane, N,N,N',N'-1,2-tetramethyldiaminoethane, 1,3-diaminopropane, N,N'-dimethyl-1,3-diaminopropane, N,N,N',N'-1,3-tetramethyldiaminopropane, 1,4-diaminobutane, N,N'-dimethyl-1,4-diaminobutane, N,N,N',N'-1,4-tetramethyldiaminobutane, 1,5-diaminopentane, N,N'-dimethyl-1,5-diaminopentane, N,N,N',N'-1,5-tetramethyldiaminopentane, 1,6-diaminohexane, N ,N'-Dimethyl-1,6-diaminohexane, N,N,N',N'-Tetramethyl-1,6-diaminohexane, N,N-Bis(3-aminopropyl)amine, N,N-Bis[3-(methylamino)propyl]amine, N,N-Bis[3-(dimethylamino)propyl]amine, N-Methyl-N,N-bis(3-aminopropyl)amine, N-Methyl-N,N-bis[3-(methylamino)propyl]amine, N-Methyl-N,N-bis[3-(dimethylamino)propyl]amine, N,N'-Bis(3-aminopropyl)ethylenediamine, N,aliphatic amines such as N'-bis[3-(methylamino)propyl]ethyleneamine and N,N'-bis[3-(dimethylamino)propyl]ethyleneamine; alkoxysilyl group-containing aliphatic amines such as 3-aminopropyltriethoxysilane and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane; aliphatic amino alcohols such as ethanolamine, N-methylethanolamine, N,N-dimethylethanolamine, N-ethylethanolamine, N,N-diethylethanolamine, N-methyl-N-ethylethanolamine, N-benzylethanolamine, N,N-dibenzylethanolamine, and diethylene glycolamine; 2-methoxyethylamine, 2-ethoxyethylamine, 2-n-propoxyethylamine, 2-isopropoxyethylamine, 2-n-butoxyethylamine, 2-methoxypropylamine, 2-ethoxypropylamine, 2-n-propoxypropylamine, 2-isopropoxypropyl Amines, 2-n-butoxypropylamine, 3-methoxypropylamine, 3-ethoxypropylamine, 3-n-propoxypropylamine, 3-isopropoxypropylamine, 3-n-butoxypropylamine, 2-methoxybutylamine, 2-ethoxybutylamine, 2-n-propoxybutylamine, 2-isopropoxybutylamine, 2-n-butoxybutylamine, 3-methoxybutylamine, 3-ethoxybutylamine, 3-n-propoxybutylamine, 3 -isopropoxybutylamine, 3-n-butoxybutylamine, 4-methoxybutylamine, 4-ethoxybutylamine, 4-n-propoxybutylamine, 4-isopropoxybutylamine, 4-n-butoxybutylamine, bis(2-aminoethyl)ether, bis(3-aminopropyl)ether, bis(4-aminobutyl)ether, 1,4-butanediol bis(2-aminoethyl)ether, 1,4-butanediol bis(3-aminopropyl)ether, 1,Examples of the amino ethers include aliphatic amino ethers such as 4-butanediol bis(4-aminobutyl) ether, bis[2-(2-aminoethoxy)ethyl] ether, bis[2-(3-aminopropoxy)ethyl] ether, bis[2-(4-aminobutoxy)ethyl] ether, triethylene glycol bis(2-aminoethyl) ether, triethylene glycol bis(3-aminopropyl) ether, and triethylene glycol bis(4-aminobutyl) ether.

[0041] The amount of the amine compound (D) added is preferably 1 to 10 parts by mass, and more preferably 5 to 10 parts by mass, per 100 parts by mass of the polysilazane compound (A).

[0042] <(E) Inorganic filler> The polysilazane compound-containing composition of the present invention may contain an inorganic filler, which is not particularly limited, but may include, for example, fumed silica, fused silica, alumina, zirconium oxide, calcium carbonate, calcium silicate, titanium dioxide, ferric oxide, zinc oxide, etc.

[0043] The addition of such inorganic fillers improves the properties (strength, heat resistance, insulating properties, etc.) of the resulting cured film.

[0044] The amount of the (E) inorganic filler added is not particularly limited, but is preferably 0.1 to 400 parts by mass, and more preferably 1 to 100 parts by mass, per 100 parts by mass of the (A) component.

[0045] <Method of producing polysilazane compound-containing composition> The polysilazane compound-containing composition of the present invention is not limited in its manufacturing method, and can be obtained, for example, by adding the (B) and (D) components, and optionally the (E) component to a solution obtained by mixing the (A) and (C) components, and stirring the mixture while applying ultrasonic waves. In this way, a polysilazane compound-containing composition in which the xanthene colorant is suitably dispersed can be obtained. In addition, additives other than those mentioned above can be added to the composition of the present invention depending on the purpose.

[0046] <Method of forming a cured film> The method for forming a cured film using the polysilazane compound-containing composition of the present invention is not particularly limited, and examples thereof include a method including a coating step of coating the polysilazane compound-containing composition on a substrate, a solvent volatilization step of volatilizing and removing the organic solvent from the coating film coated on the substrate, and a curing step of curing the xanthene dye-containing polysilazane compound.

[0047] (Coating process) Examples of methods for applying the polysilazane compound-containing composition of the present invention to a substrate include roll coating methods using a direct gravure coater, a chamber doctor coater, an offset gravure coater, a reverse kiss coater, a reverse roll coater, a slot die, a lip coater, an air doctor coater, a single roll kiss coater, a positive rotation roll coater, a blade coater, an impregnation coater, an MB coater, an MB reverse coater, a knife coater, a bar coater, etc., spin coating methods, dispensing methods, dipping methods, spraying methods, transfer methods, slit coating methods, etc.

[0048] The thickness of the coating film varies depending on the purpose of the cured film, but the cured film thickness is preferably 10 to 100,000 nm, and more preferably 100 to 10,000 nm.

[0049] Before applying the polysilazane compound-containing composition, the substrate may be subjected to a surface modification treatment. The surface modification treatment is mainly performed for the purpose of improving the adhesion between the substrate and the polysilazane compound, and is realized by decomposing and removing organic matter attached to the substrate surface, or by forming chemical reaction points on the substrate surface. Examples of the surface modification treatment method include argon plasma treatment, oxygen plasma treatment, ozone treatment, UV irradiation treatment, and xenon excimer light irradiation treatment, and are used depending on the type of substrate.

[0050] (Solvent evaporation process) Following the coating step, the process proceeds to a solvent evaporation step in which the organic solvent is evaporated from the coating film formed on the substrate. The solvent evaporation step is preferably performed at 20 to 300°C, more preferably 25 to 200°C. Within this range, the organic solvent evaporates quickly and the process proceeds to the curing step. If the temperature of the solvent evaporation step is 300°C or lower, there is no risk of the luminescent substance (xanthene dye) decomposing or the evaporated solvent igniting, which is preferable. In addition, if the boiling point of the organic solvent is sufficiently lower than the temperature at which polysilazane is cured, the temperature of the solvent evaporation step is appropriately set, so that the curing reaction of polysilazane does not occur at the same time, and the organic solvent does not remain in the cured film, which does not cause discoloration.

[0051] For the above reasons, the boiling point of the organic solvent (C) used in the present invention under atmospheric pressure (1013 hPa) is preferably 25 to 300° C., and more preferably 25 to 150° C. If it is within this range, the organic solvent will not remain in the cured film, and handling properties will be good.

[0052] (hardening process) After the solvent evaporation process, the process proceeds to the curing process of the xanthene dye-containing polysilazane compound. The curing process of the xanthene dye-containing polysilazane compound is not particularly limited as long as the curing reaction proceeds, but it is necessary to select a method that does not deteriorate the substrate. Examples of the curing process method include heat treatment, steam heat treatment, atmospheric pressure plasma treatment, low temperature plasma treatment, UV treatment, and excimer light treatment. EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The weight average molecular weight is a value measured by GPC under the above conditions.

[0054] (A) Polysilazane compound (Synthesis example) Synthesis of polysilazane compound (A) Dehydrated pyridine (4,500 g) was cooled to -10°C under a nitrogen atmosphere, and dichlorosilane (64 L) was blown in, followed by stirring at -10°C for 1 hour. Ammonia (216 L) was blown in, and the mixture was stirred for 12 hours while returning to 25°C. The resulting solid was filtered off, and n-dibutyl ether (1,000 g) was added to the filtrate. The pyridine in the liquid was distilled off under reduced pressure while azeotroping with n-dibutyl ether, and when the distillate reached 4,500 g, n-dibutyl ether (1,000 g) was further added. Next, pyridine was distilled off under reduced pressure while azeotroping with n-dibutyl ether to obtain an n-dibutyl ether solution of perhydropolysilazane. The weight-average molecular weight of this perhydropolysilazane was 6,100. Then, n-dibutyl ether was added so that the polysilazane compound was 20 parts by mass when the entire solution was 100 parts by mass. In the following Examples and Comparative Examples, this solution was used assuming that it contained 20 parts by mass of perhydropolysilazane as the component (A) and 80 parts by mass of n-dibutyl ether as the component (C-1).

[0055] (B) Xanthene dyes (B-1) Rhodamine B (Alfa Aesar) (B-2) Fluorescein (Fujifilm Wako Pure Chemical Industries, Ltd.) (Comparative dye) (B-3) Tetraphenylethylene (Tokyo Chemical Industry Co., Ltd.) (B-4) 1,1,2,3,4,5-Hexaphenyl-1H-silole (manufactured by SIGMA-ALDRICH)

[0056] (C) Organic solvent (C-1) Di-n-butyl ether (Kanto Chemical) (C-2) Acetone (Fujifilm Wako Pure Chemical Industries, Ltd.)

[0057] (D) Amine compounds (D-1) 3-Aminopropyltriethoxysilane (KBE-903, manufactured by Shin-Etsu Chemical Co., Ltd.) (D-2) N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (KBM-603, manufactured by Shin-Etsu Chemical Co., Ltd.) (D-3) N,N,N',N'-Tetramethyl-1,6-diaminohexane (Tokyo Chemical Industry Co., Ltd.) (Comparative amine compounds) (D-4) 1,8-diazabicyclo[5.4.0]-7-undecene (Tokyo Chemical Industry Co., Ltd.)

[0058] (E) Inorganic filler Fused silica (Tokuyama Excelica SE-8)

[0059] [Examples 1 to 18, Comparative Examples 1 to 13] (1) Evaluation of coatability The polysilazane compound-containing compositions were prepared by adding the components (B) and (D), and optionally the components (C-2) and (E) to a solution prepared by mixing the components (A) and (C-1) prepared in the above synthesis example in the ratios shown in Tables 1 and 2, and stirring the mixture for 5 minutes while applying ultrasonic waves (38 kHz) using an ultrasonic cleaner. Each of the obtained polysilazane compound-containing compositions was spin-coated (rotation speed 500 rpm, rotation time 30 seconds) onto a polycarbonate substrate. Tables 1 and 2 show that a uniform film could be produced by this process, with an ◯, and that the composition gelled during the process and a uniform film could not be produced.

[0060] (2) Evaluation of luminescence Solvent evaporation process Of the polysilazane compound-containing compositions coated above, those with coatability of ◯ were left to stand at 25° C. for 15 minutes to volatilize the solvent.

[0061] Curing process The xanthene dye-containing polysilazane compound from which the solvent had been evaporated as described above was heated in a dryer at 120° C. for 1 hour to form a cured film on the surface of the polycarbonate substrate.

[0062] The cured film formed above was irradiated with a 365 nm UV LED (manufactured by Eye Graphics) in a dark place with a peak intensity of 130 mW / cm 2The appearance was visually compared under fluorescent light with that of a comparative example not containing component (D). The change in appearance from Comparative Example 1, that is, the appearance of luminescence was observed, was marked with an O, and the appearance of no luminescence was marked with an X, as shown in Tables 1 and 2.

[0063] (3) Evaluation of colorability The UV-visible absorption spectrum of the cured film prepared in the evaluation of (2) was measured using a spectrophotometer (Hitachi High-Tech). The absorbance at the selected wavelength was taken as A value, and the film thickness (unit: nm) measured using a microspectrophotometer (Otsuka Electronics) was taken as B value. The value obtained by dividing A value by B value is shown in Tables 1 and 2 as a numerical value indicating colorability. However, the wavelengths selected at this time were 558 nm when (B-1) was used, 491 nm when (B-2) was used, and 390 nm when (B-3) or (B-4) was used. The higher the colorability value in Tables 1 and 2, the more improved the visibility.

[0064] (4) Evaluation of hardening properties The FT-IR spectrum (ATR method) of the cured film formed in the evaluation of (2) was measured using a Fourier transform infrared spectrophotometer (Shimadzu Corporation). -1 The absorbance of the peaks is shown in Tables 1 and 2. The more Si-H bonds are consumed in the crosslinking, the smaller the peak intensity derived from the Si-H bonds becomes. Therefore, the smaller the value of curability in Tables 1 and 2, the better the curability.

[0065] [Table 1]

[0066] [Table 2]

[0067] In Comparative Examples 10 to 13, which used the component (B-3) or (B-4) that is not a xanthene dye of the present invention, the luminescence was rated as "good", but the coloring value was smaller than that of Examples 1 to 18, and therefore the effect of improving visibility under natural light was inferior. When the (B-1) component was used, the composition was unstable in Comparative Example 5, in which the (D-4) component was used as the (D) component, which was not an amine-based compound having a chain aliphatic amino group, and a uniform film could not be produced. Comparative Examples 3 and 4, in which the (D-4) component was used as the (D) component, which was not an amine-based compound having a chain aliphatic amino group, had good coatability and luminescence, but at least one of the colorability and curability was inferior compared to Examples 1 to 15. Comparative Examples 1 and 2, which did not contain the (D) component, had good coatability and luminescence, but at least one of the colorability and curability was inferior compared to Examples 1 to 15. When the (B-2) component was used, the composition had low stability in Comparative Example 9, in which the (D-4) component was used, which was not an amine-based compound having a chain aliphatic amino group, and a uniform film could not be produced. In Comparative Example 6, in which the (D) component was not included, the luminescence was ×, and the visibility of the cured film was not improved. In Comparative Examples 7 and 8, in which the (D-4) component was used, which was not an amine-based compound having a chain aliphatic amino group, the coating property and luminescence property were good, but both the coloring property and curing property were inferior compared to Examples 16 to 18.

[0068] [Industrial Applicability] The polysilazane-containing composition of the present invention has excellent curability, and can form a siliceous film that appears colored to the naked eye and emits light when irradiated with light of, for example, 365 nm, and is therefore useful for easily judging whether a substrate is appropriately coated with a siliceous film.

[0069] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.

Claims

1. A polysilazane compound-containing composition, (A) a polysilazane compound, (B) a xanthene dye represented by the following formula (B-1) or the following formula (B-2): [Case 1] (In the formula, R 1 are each independently a hydrogen atom, a methyl group, or an ethyl group; R 2 are each independently a hydrogen atom or a methyl group, and X is a chloride ion or a perchlorate ion. [Case 2] (In the formula, R 3 are each independently a hydrogen atom or a halogen atom; R 4 is a hydrogen atom, an amino group, a nitro group, a carboxyl group, an isothiocyanate group, a maleimide group, a semicarbazide group, or a thiosemicarbazide group. (C) an organic solvent, and (D) Amine compounds having a chain aliphatic amino group The chain aliphatic amino group is an amino group substituted with a monovalent or divalent chain aliphatic hydrocarbon group, the amino group substituted with a monovalent chain aliphatic hydrocarbon group is an amino group substituted with a trialkoxysilyl-modified alkyl group having 2 to 6 carbon atoms; A polysilazane compound-containing composition, wherein the amino group substituted with a divalent chain aliphatic hydrocarbon group is two amino groups linked by a linear alkylene group having 3 to 8 carbon atoms.

2. 2. The polysilazane compound-containing composition according to claim 1, wherein the component (A) is a perhydropolysilazane.

3. 3. The polysilazane compound-containing composition according to claim 1, wherein the blending amount of the component (D) is 1 to 10 parts by mass per 100 parts by mass of the component (A).

4. The polysilazane compound-containing composition according to any one of claims 1 to 3, further comprising (E) an inorganic filler.

Citation Information

Patent Citations

  • Coating liquid for silica-based film formation, its production, silica-based film and semiconductor device

    JP1996176511A

  • Polymerizable fluorescent sealant and method for gap filling for building

    JP2000219869A

  • Multiphoton polymerizable preceramic polymer composition

    JP2008525626A

  • Single-photon polymerizable preceramic polymer compositions and multiphoton polymerizable preceramic polymer compositions

    JP2008525627A

  • Coating composition containing polysilazane and wavelength conversion agent and wavelength conversion sheet using the same

    JP2015155525A