Conductive ink and manufacturing method thereof, conductive printed matter, conductor and manufacturing method thereof, and electronic device

A conductive ink with chain-shaped silver particles and controlled properties maintains stable conductivity by reducing voids and resistance changes during stretching, addressing the instability of conventional inks on flexible substrates.

JP7590618B1Active Publication Date: 2024-11-26TOKYO PRINTING INC MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024126985
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Conventional conductive inks applied to stretchable materials suffer from instability in conductivity due to expansion and contraction, leading to increased resistance values and void formation, which compromises their effectiveness in maintaining consistent electrical properties.

Method used

The development of a conductive ink comprising chain-shaped silver particles with specific crystallite sizes, tap densities, and surface areas, along with a binder resin, to ensure stable conductivity during repeated expansions and contractions.

Benefits of technology

The conductive ink maintains stable conductivity by minimizing void formation and resistance fluctuations, ensuring consistent electrical performance even under stretching conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590618000003
    Figure 0007590618000003
  • Figure 0007590618000004
    Figure 0007590618000004
  • Figure 0007590618000001
    Figure 0007590618000001
Patent Text Reader

Abstract

To provide a conductive ink which can provide good conductive stability even when stretched. [Solution] The conductive ink of the present invention contains silver particles and a resin, and is used for printing on a substrate having at least one of flexibility and stretchability, wherein the silver particles are chain-like and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive ink and a method for producing the same, a conductive printed matter, a conductor and a method for producing the same, and an electronic device. [Background technology]

[0002] Conventionally, conductive inks have been known that are made by kneading conductive particles such as silver particles or carbon particles with a binder resin, a solvent, etc. into a paste form. By printing such conductive ink on a substrate, etc., a desired circuit can be created easily and with high precision. Here, conventional conductive inks such as those disclosed in Patent Document 1 (JP 2022-99275 A) are printed on a substrate and then sintered to evaporate and dry the medium (ink solvent) in the ink coating and solidify the conductive particles.

[0003] On the other hand, the development of conductive inks that can be used in combination with stretchable substrates is attracting attention. In this case, the conductive ink is required to be able to follow the expansion and contraction of the substrate and to provide good conductivity both during expansion and contraction.

[0004] For example, Patent Document 2 (JP 2023-93906 A) describes a conductive composition comprising a block copolymer (E) mainly composed of structural units derived from an ethylenically unsaturated monomer and having a weight-average molecular weight of 20,000 or more and 500,000 or less, in order to obtain repeated stretch resistance by suppressing the occurrence of cracks in the resin during stretching, and conductive fine particles (F), wherein the content of the conductive fine particles (F) is 60 to 95 mass% with respect to the total solid content contained in the conductive composition, the content of chain-like silver powder (f1) among the conductive fine particles (F) is 20 mass% or more and less than 70 mass% with respect to the total solid content of the conductive composition, and the tap density of the chain-like silver powder (f1) is 2.0 g / cm 3 The following conductive compositions are disclosed: [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-99275 [Patent Document 2] JP 2023-93906 A Summary of the Invention [Problem to be solved by the invention]

[0006] The conductive ink disclosed in Patent Document 1 involves a sintering process, and therefore even if it is applied to a stretchable substrate, the conductive ink cannot follow the expansion and contraction and cannot maintain good conductivity.

[0007] The present inventors have focused on the development of a conductive ink for use in printing on a substrate having at least one of flexibility and stretchability. Here, the conductive ink is configured so that its conductivity is maintained by the deformation of the binder resin due to expansion and contraction, etc., within a range where the electrical chain of the conductive particles is not interrupted. However, it is known that the conductivity of the conductive ink fluctuates (resistance value changes) when it is expanded and contracted, and that the conductivity also decreases due to repeated expansion and contraction. Therefore, the technology disclosed in Patent Document 2 focuses on obtaining a conductive ink with excellent resistance to repeated stretching by comparing the initial resistance value of a test piece (stretchable conductive material) using a conductive composition with the resistance value measured in a non-stretched state after repeated stretching 1,000 times.

[0008] However, although there is a set range of allowable conductivity (resistance value) in actual electronic components in which conductive ink is used, with conventional conductive inks, sufficient consideration had not been given to the change in the difference between the resistance value when stretched and the resistance value when contracted. Therefore, the present inventors focused on a new problem of obtaining good conductive stability by suppressing the increase in the difference between the resistance value of the conductive ink when it is stretched and the resistance value when it is contracted due to repeated stretching. [Means for solving the problem]

[0009] The inventors conducted extensive research to obtain good conductive stability by minimizing the change in the resistance value of the conductive ink and the difference in the resistance value between expansion and contraction during repeated stretching, and discovered that it is effective to use chain-like silver particles and control the crystallite size obtained from powder X-ray diffraction measurement of silver microparticles, thereby completing the present invention.

[0010] According to the present invention, the following conductive ink and related techniques are provided.

[0011] [1] A conductive ink containing silver particles and a resin, the ink being used for printing on a substrate having at least one of flexibility and stretchability, A conductive ink, wherein the silver particles are chain-like and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement. [2] The conductive ink according to [1], The silver particles have a tap density of 1.3 g / cm 3 More than 1.6g / cm 3 The following is a conductive ink. [3] The conductive ink according to [1] or [2], The specific surface area of ​​the silver particles (BET method) is 3.5 m 2 / g or more, 5.5m 2 / g or less. [4] The conductive ink according to any one of [1] to [3], The conductive ink has a particle size (average particle size D50) corresponding to a cumulative 50% of the volume-based integrated fraction of the silver particles as determined by a laser diffraction method of 4.5 μm or more and 6.5 μm or less. [5] The conductive ink according to any one of [1] to [4], A conductive ink, in which the ratio of the particle size (average particle size D50; μm) corresponding to a cumulative 50% of the volume-based integrated fraction of the silver particles measured by a laser diffraction method to the crystallite size (nm) of the silver particles is 0.12 or more and 0.30 or less. [6] The conductive ink according to any one of [1] to [5], The resin is a conductive ink containing one or more resins selected from the group consisting of polyurethane resin, polystyrene resin, acrylic resin, polycarbonate resin, polyamide resin, polyamideimide resin, and thermoplastic elastomer. [7] The conductive ink according to any one of [1] to [6], The silver particles are a mixture containing silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less, and silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less. [8] The conductive ink according to any one of [1] to [7], The silver particles have a specific surface area (BET method) of 4 m 2 / g, 6m 2 / g or less and a specific surface area (BET method) of 2m 2 / g or more, 4m 2 and silver particles (B2) having an average particle size of 100 nm or less. [9] The conductive ink according to any one of [1] to [8], A conductive ink, wherein the content of the silver particles is 70 mass % or more and 90 mass % or less with respect to the total amount (solid content) of the conductive ink.

[10] The conductive ink according to any one of [1] to [9], Conductive ink used in screen printing.

[11] A conductive printed matter using the conductive ink described in any one of [1] to

[10] .

[12] A conductor comprising a substrate having at least one of flexibility and stretchability, and a conductive ink according to any one of [1] to

[10] printed on the substrate.

[13] An electronic device comprising the conductor described in

[12] .

[14] A method for producing a conductive ink that contains silver particles and a resin and is used for printing on a substrate having at least one of flexibility and stretchability, comprising: The method includes a step of mixing the silver particles with the resin, A method for producing a conductive ink, wherein the silver particles are chain-like and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement.

[15] A method for producing the conductive ink according to

[14] , comprising the steps of: In the mixing step, The method for producing a conductive ink includes mixing the silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less, the silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less, and the resin.

[16] A method for producing a conductor, comprising: A step of printing the conductive ink according to any one of [1] to

[10] on a substrate having at least one of flexibility and stretchability; A step of drying the printed film obtained by the printing to obtain a conductive film; A method for producing a conductor, comprising:

[17] A method for producing the electric conductor according to

[16] , comprising the steps of: A method for producing an electric conductor, wherein a screen printing method is used in the step of printing the conductive ink. Effect of the Invention

[0012] According to the present invention, it is possible to provide a conductive ink that exhibits good conductivity stability even when stretched or expanded. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a graph showing the resistance values ​​measured in the non-stretched and stretched cycles of a tensile test in the evaluation of the electrical conductivity stability of Example 1. [Diagram 2] FIG. 13 is a graph showing the resistance values ​​measured in the non-stretched and stretched cycles of a tensile test in the evaluation of the electrical conductivity stability of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In this specification, the expression "a to b" in the description of a numerical range means from a to b, unless otherwise specified. For example, "1 to 5 mass%" means "1 mass% to 5 mass%". Furthermore, the lower limit and upper limit of a numerical range can be arbitrarily combined with the lower limit and upper limit of another numerical range.

[0015] Unless otherwise specified, each of the components and materials exemplified in this specification may be used alone or in combination of two or more kinds.

[0016] In this specification, the term "(meth)acrylic" refers to a concept that includes both acrylic and methacrylic. The same applies to similar terms such as "(meth)acrylate."

[0017] In this specification, the crystallite size of silver particles is defined as a value calculated by determining the half-value width β (rad) of the peak of the plane with plane index (1,1,1) from measurement by powder X-ray diffraction method using CuKα radiation as a radiation source, and using the following Scherrer formula (1). D=Kλ / (βcosθ) (1) (where K is the Scherrer constant and λ is the wavelength of the X-rays used) D: Crystallite size K: Scherrer constant = 0.94 λ: wavelength of X-ray used, CuKα 0.154nm θ: Bragg angle (rad)

[0018] In this specification, the specific surface area of ​​silver particles is a value measured by the BET method.

[0019] In this specification, the average particle size D50 of silver particles refers to the particle size equivalent to 50% of the cumulative volume-based integrated fraction measured by the particle laser diffraction scattering method in accordance with JIS R 1629: 1997. Distilled water is used as the solvent, and the powder is ultrasonically dispersed in a sample circulator that is a standard accessory to the device, after which the particle size is measured.

[0020] In this specification, the tap density of silver particles is defined as the tap density of a volume of 20 cm 3The value is measured from the bulk (volume) when 15 g of silver powder is put into the cell container, the tap stroke is 10 mm, and the number of taps is 1500. The equipment used is a functional powder property measuring instrument, Multitester MT-1000 (manufactured by Seishin Enterprise Co., Ltd.).

[0021] Hereinafter, an embodiment of the present invention will be described in detail.

[0022] <Conductive ink> The conductive ink of this embodiment contains silver particles and a resin, and is used for printing on a substrate having at least one of flexibility and stretchability, and the silver particles are chain-like and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement. This allows a conductive printed product using the conductive ink of this embodiment to have good conductivity both when stretched and when contracted.

[0023] Although the details of the reason for this are not clear, it is speculated as follows. First, the conductive particles in the stretchable conductive ink are not sintered and are designed to be able to conform to the stretchable substrate together with the binder resin. However, when conductive printed materials using conventional conductive inks are repeatedly stretched and used over a long period of time, the stretching causes the conductive particles to peel off from the binder resin, resulting in the formation of voids (vacuum voids).When the material is further stretched and stretched repeatedly, these voids are also stretched, causing the contact points between the conductive particles to separate and tending to increase the resistance value. In response to this, the inventors conducted extensive research and discovered that by using chain-like silver particles of a specific crystallite size, the occurrence of the above-mentioned voids can be effectively suppressed and stable conductivity can be maintained both during contraction and expansion. In other words, by forming silver particles into a chain of a specific crystallite size, a cohesive force acts between the silver particles, making it easier to maintain contact between the silver particles both during contraction and expansion, thereby suppressing the occurrence of voids. As a result, it is possible to obtain a low volume resistivity while also obtaining good conductive stability, thereby achieving a high level of balance between the two.

[0024] In this embodiment, the silver particles in the conductive ink are a particle group, and the physical properties of the silver particles described below are average values ​​of the particle group.

[0025] (chained) In this embodiment, the silver particles contained in the conductive ink are in a chain shape. A chain shape refers to a state in which particles are linked together and aggregated to a certain extent, and the direction, length, number, and the like of the chain are not particularly limited. The chain shape of the silver particles may be either a chain shape or a branched shape, and among these, a dendritic branch shape is preferable. The silver particles may also be in the shape of a bunch of grapes, with many aggregates gathering together. The fact that the silver particles are in a chain form can be confirmed by a scanning electron microscope.

[0026] (Crystallite size) The crystallite size of the silver particles obtained by powder X-ray diffraction measurement is 25 nm or more and 37 nm or less. This reduces the degree to which the conductivity of the conductive ink changes when it expands and when it contracts, resulting in good conductivity stability.

[0027] The crystallite size of the silver particles is preferably 26 nm or more, and more preferably 27 nm or more. On the other hand, the crystallite size of the silver particles is preferably 36 nm or less, and more preferably 35 nm or less. By adjusting the crystallite size of the silver particles to be equal to or larger than the above lower limit, the electrical conductivity of the silver particles can be improved. On the other hand, by setting the crystallite size of the silver particles to be equal to or less than the above upper limit, deformation and fluctuation of the resin present between the silver particles can be suppressed, thereby reducing voids caused by deformation and fluctuation of the resin and making it easier to maintain good conductivity against elongation.

[0028] (Tap density) In this embodiment, since chain-like silver particles tend to be bulky because they are made up of numerous agglomerates resembling a bunch of grapes, the low tap density of the silver particles is intended to mean that the silver particles tend to be bulky and that the silver particles are chain-like. The tap density of the silver particles is preferably 1.3 g / cm 3 More preferably, it is 1.4 g / cm 3 That's all. On the other hand, the tap density of the silver particles is preferably 1.6 g / cm 3 More preferably, it is 1.5 g / cm 3 The following is the result. By setting the tap density of the silver particles to the above lower limit or more, the density of the silver particles in the conductive ink is increased, and the conductivity is easily improved. On the other hand, by setting the tap density of the silver particles to the above upper limit or less, the silver particles can be made to conform to expansion and contraction, and good conductive stability can be obtained.

[0029] (specific surface area) The specific surface area of ​​the silver particles is preferably 3.5 m 2 / g or more, more preferably 3.6m 2 / g or more. On the other hand, the specific surface area of ​​the silver particles is preferably 5.5 m 2 / g or less, more preferably 5.4m 2 / g or less. By setting the specific surface area of ​​the silver particles to be equal to or greater than the lower limit, the generation of voids during expansion and contraction can be suppressed, and the conductive stability can be improved. On the other hand, by setting the specific surface area of ​​the silver particles to be equal to or less than the upper limit, an increase in volume resistivity can be suppressed.

[0030] (Average particle size D50) The average particle size D50 of the silver particles is preferably 4.5 μm or more, and more preferably 4.6 μm or more. On the other hand, the average particle size D50 of the silver particles is preferably 6.5 μm or less, and more preferably 6.3 μm or less. By setting the average particle size D50 of the silver particles to be equal to or more than the above lower limit, it is possible to improve the conductivity while maintaining good conductive stability. On the other hand, by setting the average particle size D50 of the silver particles to be equal to or less than the above upper limit, an increase in volume resistivity can be suppressed and good electrical conductivity can be maintained.

[0031] In this embodiment, the ratio of the particle size (average particle size D50; μm) corresponding to a cumulative 50% of the volume-based integrated fraction of the silver particles measured by a laser diffraction method to the crystallite size (nm) of the silver particles (average particle size D50 (μm) / crystallite size (nm)) is preferably 0.12 to 0.30, more preferably 0.13 to 0.25, and even more preferably 0.14 to 0.22. By setting this ratio (average particle size D50 (μm) / crystallite size (nm)) to the lower limit value or more, the generation of voids is suppressed and electrical conductivity stability is obtained. On the other hand, by setting the ratio (average particle size D50 (μm) / crystallite size (nm)) to the above upper limit or less, stable conductivity can be obtained.

[0032] In order to realize silver particles having the above crystallite size, specific surface area, tap density, and average particle size D50, it is important to select the type of silver particles, etc. For example, it is preferable to select multiple silver particles with different crystallite sizes, select multiple silver particles with different specific surface areas, or adjust the content of each type of silver particle.

[0033] The silver particles may be a mixture containing silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less and silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less, which allows the balance between electrical conductivity and conformability to be highly controlled, resulting in higher electrical conductivity stability. In addition, by using silver particles with different crystallite sizes, the silver particles (A1) act to fill in the gaps between the silver particles (A2) during elongation, complementing the contact points between the silver particles, making it easier to obtain good electrical conductivity.

[0034] In this case, the crystallite size of the silver particles (A1) is more preferably 26 nm or more and 29 nm or less, and even more preferably 27 nm or more and 28 nm or less. The crystallite size of the silver particles (A2) is more preferably 35 nm or more and 45 nm or less, and even more preferably 39 nm or more and 41 nm or less.

[0035] The mass ratio of the silver particles (A1) to the silver particles (A2) (silver particles (A1):silver particles (A2)) is preferably from 90:10 to 30:70, more preferably from 80:20 to 40:60, and even more preferably from 75:25 to 50:50.

[0036] In addition, silver particles have a specific surface area of ​​4m 2 / g, 6m 2 / g or less and silver particles (B1) with a specific surface area of ​​2m 2 / g or more, 4m 2 and silver particles (B2) having a silver content of not more than 1 g / g. This allows for precise control of the balance between electrical conductivity and conformability, resulting in higher electrical conductivity stability.

[0037] In this case, the specific surface area of ​​the silver particles (B1) is more preferably 5.2 m 2 / g or more, 5.6m 2 / g or less. The specific surface area of ​​the silver particles (B2) is preferably 2.1 m 2 / g or more, 2.8m 2 / g or less, and more preferably 2.3m 2 / g or more, 2.5m 2 / g or less.

[0038] The mass ratio of silver particles (B1) to silver particles (B2) (silver particles (B1):silver particles (B2)) is preferably 90:10 to 30:70, more preferably 80:20 to 40:60, and even more preferably 75:25 to 50:50.

[0039] The content of silver particles is preferably 70% by mass or more and 90% by mass or less, more preferably 75% by mass or more and 85% by mass or less, and even more preferably 78% by mass or more and 82% by mass or less, based on the total amount (solid content) of the conductive ink. By setting the content of silver particles to be equal to or greater than the above lower limit, electrical continuity during elongation can be maintained, whereas by setting the content of silver particles to be equal to or less than the above upper limit, the occurrence of cracks in the printed film during elongation can be suppressed.

[0040] [resin] The use of resins improves the handleability of the conductive ink, making it easier to obtain desired printed matter, and also imparts elasticity to the conductive ink.

[0041] The resin is not particularly limited as long as it has plasticity or elasticity, and any known conductive ink can be used. Specifically, for example, one or more selected from the group consisting of polyurethane resin, acrylic resin, polyamide resin, polyimide resin, silicone resin, and thermoplastic elastomer can be used. Among them, acrylic resin is preferable.

[0042] (others) In addition to the silver particles and resin, the conductive ink of this embodiment may further contain known additives such as solvents, fillers, pigments, silane coupling agents, leveling agents, thixotropic agents, and defoamers, depending on the application, etc.

[0043] [Manufacturing method] The method for producing the conductive ink of this embodiment includes a step of mixing the above-mentioned silver particles, a resin, and any other components. The silver particles are chain-shaped and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement. Alternatively, silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less and silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less may be used and mixed with a resin. In addition, the above silver particles have a specific surface area of ​​4 m 2 / g, 6m 2 / g or less and silver particles (B1) with a specific surface area of ​​2m 2 / g or more, 4m 2 Alternatively, silver particles (B2) of not more than 1 / g may be used and mixed with the resin.

[0044] The mixing method is not particularly limited, but for example, the ingredients can be mixed in a known mixer such as a meteor mixer, a dissolver, a bead mill, a Raikai mixer, a three-roll mill, a rotary mixer, or a twin-shaft mixer.

[0045] [Characteristics, usage] The conductive ink of this embodiment provides good conductive stability against expansion, contraction and flexibility, and is therefore suitable for use in printing on substrates that have at least one of expansion and contraction and flexibility. As a printing method, screen printing is preferably used.

[0046] The above-mentioned base material having at least one of elasticity and flexibility refers to a base material that can be stretched and contracted, or bent or folded, in part or in whole. Among them, a base material that can be stretched, bent or folded repeatedly is preferable. Examples of the substrate include resin materials processed into films, sheets, fabrics, bands, fibers, woven fabrics, nonwoven fabrics, knitted fabrics, etc.; crosslinked rubber materials such as nitrile rubber, styrene rubber, chloroprene rubber, urethane rubber, butyl rubber, and natural rubber; papers; and various components having moving parts. Specific examples of the resin material include polyimide, polyethylene terephthalate (PET), polycarbonate, polyethylene naphthalate (PEN), polyketone, polyether ether ketone, thermoplastic polyurethane elastomer (TPU), and cycloolefin polymer.

[0047] <Conductive printed materials, conductors, electronic devices> Furthermore, by using the conductive ink, it is possible to obtain a conductive printed matter, a conductor comprising a substrate having at least one of elasticity and flexibility and the conductive ink printed on the substrate, and an electronic device comprising a conductor. The conductive printed matter comprises at least a printed layer using the conductive ink on a substrate. The substrate can be a substrate having at least one of the above-mentioned elasticity and flexibility. This provides good conductive stability.

[0048] In addition, the method for producing a conductor of this embodiment includes a step of printing the above-mentioned conductive ink on a substrate having at least one of elasticity and flexibility, and a step of drying the printed film obtained by the printing to obtain a conductive film.

[0049] The conductive ink of the present embodiment is not sintered, and therefore can conform well to a substrate having at least one of flexibility and stretchability, and can maintain conductivity. Therefore, it can be applied to a substrate having low heat resistance, and the degree of freedom in designing conductive printed matter can be increased. Drying is preferably carried out by heating and blowing air, and the heating temperature is preferably 80 to 150° C. and the heating time is preferably 10 to 120 minutes.

[0050] The printing method may be one or more selected from screen printing, pad printing, stencil printing, screen offset printing, dispenser printing, gravure offset printing, reverse offset printing, and microcontact printing. Among these, screen printing is preferably used. In the screen printing method, for example, a fine mesh screen of 300 to 650 mesh can be used.

[0051] The thickness of the printed film may be appropriately adjusted depending on the desired conductivity, etc., and is not particularly limited, but may be, for example, 0.5 μm or more and 20 μm or less, or 1 μm or more and 15 μm or less.

[0052] The conductor may be a product itself or may be used as a component, for example, a wiring, an electrode, or an electromagnetic shielding layer, a heat dissipation layer, or the like.

[0053] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. EXAMPLES

[0054] Next, the present invention will be described in detail with reference to examples, but the contents of the present invention are not limited to the examples.

[0055] <Examples and Comparative Examples> Conductive ink was prepared using the following raw materials and evaluated in each step. [Raw materials] (Silver particles) Silver particles 1 to 4 having the physical properties shown in Table 1 below were prepared.

[0056] [Table 1]

[0057] (binder resin) Binder resin 1: Acrylic block copolymer (MAM) "CLARITY (registered trademark)" (manufactured by Kuraray Co., Ltd.)

[0058] [Preparation of conductive ink] The binder resin was dissolved in butyl carbitol acetate to obtain the ratio (parts by mass) shown in Table 2, to which the silver particles were added and premixed in a planetary centrifugal mixer, and then further kneaded in a three-roll mill.

[0059] Furthermore, when the conductive inks were observed using a scanning electron microscope, it was confirmed that the silver particles in all of the conductive inks were in a chain form.

[0060] [evaluation] (Volume resistivity) (i) Each of the obtained conductive inks was applied to a glass substrate (slide glass; 76 mm × 52 mm × 1.3 mm) by screen printing. After application, the substrate was heat-treated at 100°C for 30 minutes. The thickness of the printed film was 40 to 50 μm. The volume resistivity (Ω·cm) of the printed film was then measured by the four-probe method using a Loresta (Loresta-GP MCP-T610, manufactured by Nitto Seiko Analytech Co., Ltd.) The results are shown in Table 2.

[0061] (Conductive stability) (ii) Each of the obtained conductive inks was printed on a polyurethane film (elastic substrate: Okura Kogyo Co., Ltd., ES85, thickness 100 μm) in the shape of a No. 7 dumbbell test piece so that the thickness after drying would be 20 μm, and after printing, it was dried at 100 ° C for 80 minutes to obtain a printed film. The part where the printed film was formed was punched out with a punch, and this was used as a test piece (No. 7 dumbbell test piece shape). A tensile test was performed on the test piece using a tensile tester (Stency, manufactured by Acroedge Co., Ltd.) connected to a resistance meter (RM3545, manufactured by HIOKI E.E. C.) to measure the resistance value (Ω) of the test piece. The tensile test consisted of repeating 100 extension cycles of 20% elongation at 50 mm / min followed by unloading at 50 mm / min. In each stretching cycle, the resistance value (Ω) fluctuation range (fluctuation resistance value: ΔΩ) from the time of no stretching (unloaded state: initial resistance value) to the time of 20% stretching (maximum resistance value) n (n is an integer between 1 and 100)) and measure the fluctuation range (fluctuation resistance value: ΔΩ) during repeated expansion and contraction cycles. n (n is an integer from 1 to 100)) was evaluated. In order to allow the test piece to adapt to the stretching, the first cycle was a preliminary tension. Thereafter, the results of the initial resistance value (Ω), maximum resistance value (Ω), and variable resistance value (ΔΩ) at the second and 100th cycles are shown in Table 2. Furthermore, as an example, FIG. 1 shows a graph in which the resistance values ​​measured in the stretching cycle of the tensile test in the evaluation of the electrical conductivity stability of Example 1 are sequentially plotted against the resistance values ​​measured in the stretching cycle of the tensile test in the evaluation of the electrical conductivity stability of Comparative Example 2, and FIG. 2 shows a graph in which the resistance values ​​measured in the stretching cycle of the tensile test in the evaluation of the electrical conductivity stability of Comparative Example 2 are sequentially plotted against the resistance values ​​measured in the stretching cycle of the tensile test in the evaluation of the electrical conductivity stability of Comparative Example 2.

[0062] (iii) The rate of increase A (%) of the variable resistance value (ΔΩ) during the 2nd to 100th extension and contraction cycles was calculated using the following formula. The results are shown in Table 2. Increase rate A(%)=(ΔΩ 100 / ΔΩ2)×100 As an example, FIG. 1 shows the fluctuation resistance value (fluctuation range) ΔΩ2 at the second stretching cycle and the fluctuation resistance value (fluctuation range) ΔΩ at the 100th stretching cycle for the tensile test of Example 1. 100 FIG. 2 shows the fluctuation resistance value (fluctuation range) ΔΩ2 at the second stretching cycle and the fluctuation resistance value (fluctuation range) ΔΩ at the 100th stretching cycle for the tensile test of Comparative Example 2. 100 showed.

[0063] (Void Observation) (iv) The cross section of the printed film of the test piece after 100 stretch cycles, which was used in the evaluation of the conductive stability, was observed with a scanning electron microscope (5000x magnification). Furthermore, the test piece was fixed in a 20% stretched state, and the cross section of the test piece cut parallel to the stretching direction was observed with a scanning electron microscope (5000x magnification). The observation results were evaluated according to the following criteria. ·standard Present: Voids were observed in at least one of the observations. None: No voids were observed in any observations.

[0064] [Table 2]

Claims

1. A conductive ink containing silver particles and a resin, the ink being used for printing on a substrate having at least one of flexibility and stretchability, The conductive ink, wherein the silver particles are chain-shaped and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement.

2. The conductive ink according to claim 1, The silver particles have a tap density of 1.3 g / cm 3 Above, 1.6g / cm 3 The following is a conductive ink.

3. The conductive ink according to claim 1 or 2, The specific surface area (BET method) of the silver particles is 3.5 m 2 / g or more, 5.5m 2 / g or less.

4. The conductive ink according to claim 1 or 2, The conductive ink has a particle size (average particle size D50) corresponding to a cumulative 50% of the volume-based integrated fraction of the silver particles as determined by a laser diffraction method of 4.5 μm or more and 6.5 μm or less.

5. The conductive ink according to claim 1 or 2, A conductive ink, wherein the ratio of a particle size (average particle size D50; μm) corresponding to a cumulative 50% of a volume-based integrated fraction of the silver particles measured by a laser diffraction method to the crystallite size (nm) of the silver particles is 0.12 or more and 0.30 or less.

6. The conductive ink according to claim 1 or 2, The resin is a conductive ink containing one or more resins selected from the group consisting of polyurethane resins, polystyrene resins, acrylic resins, polycarbonate resins, polyamide resins, polyamideimide resins, and thermoplastic elastomers.

7. The conductive ink according to claim 1 or 2, The silver particles are a mixture containing silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less, and silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less.

8. The conductive ink according to claim 1 or 2, The silver particles have a specific surface area (BET method) of 4 m 2 / g over 6m 2 / g or less and a specific surface area (BET method) of 2 m 2 / g or more, 4m 2 and silver particles (B2) having an average particle size of 100 nm or less.

9. The conductive ink according to claim 1 or 2, A conductive ink, wherein the content of the silver particles is 70 mass % or more and 90 mass % or less with respect to the total amount (solid content) of the conductive ink.

10. The conductive ink according to claim 1 or 2, Conductive ink used in screen printing.

11. A conductive printed matter using the conductive ink according to claim 1 or 2.

12. A conductor comprising a substrate having at least one of flexibility and stretchability, and the conductive ink according to claim 1 or 2 printed on the substrate.

13. An electronic device comprising the electrical conductor of claim 12.

14. A method for producing a conductive ink that contains silver particles and a resin and is used for printing on a substrate having at least one of flexibility and stretchability, comprising the steps of: The method includes a step of mixing the silver particles with the resin, A method for producing a conductive ink, wherein the silver particles are chain-shaped and have a crystallite size of 25 nm or more and 37 nm or less as determined by powder X-ray diffraction measurement.

15. A method for producing the conductive ink according to claim 14, comprising the steps of: In the mixing step, the silver particles (A1) having a crystallite size of 25 nm or more and 30 nm or less, the silver particles (A2) having a crystallite size of more than 30 nm and 50 nm or less, and the resin.

16. A method for producing a conductor, comprising the steps of: A step of printing the conductive ink according to claim 1 or 2 on a substrate having at least one of flexibility and stretchability; A step of drying the printed film obtained by the printing to obtain a conductive film; A method for producing a conductor, comprising:

17. A method for producing a conductor according to claim 16, comprising the steps of: A method for producing an electric conductor, wherein a screen printing method is used in the step of printing the conductive ink.

Citation Information

Patent Citations

  • Conductive ink for offset printing, and circuit pattern forming method using the same

    JP2009231059A

  • Silver coated particle and manufacturing method thereof

    JP2016146319A

  • Metal fine particle-containing ink

    JP2022099275A

  • Conductive composition, conductor, stretchable conductor, electronic device

    JP2023093906A

  • Film antenna, manufacturing method therefor, and film for use therein as antenna substrate