Toner, toner storage unit, toner manufacturing method, image forming method and image forming apparatus
The toner manufacturing method addresses shape and fluidity issues by using a surfactant composition and polymerization process, enhancing toner stability and transfer efficiency for high-quality image formation.
Patent Information
- Application Number
- JP2020092500
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-27
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Conventional toner manufacturing methods result in amorphous particle shapes, poor fluidity, and low transfer efficiency, leading to image defects and increased consumption, with surfactants affecting chargeability and environmental stability.
A toner manufacturing method using a surfactant composition with over 60% long-chain hydrocarbon groups and 40% or less hydrophilic functional groups, combined with a specific polymerization process, to enhance toner scattering resistance, heat-resistant storage stability, and transferability.
The method produces toner with improved particle shape, fluidity, and charge stability, reducing image defects and toner consumption while maintaining high-quality image formation.
Smart Images

Figure 0007590690000004 
Figure 0007590690000001 
Figure 0007590690000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner, a toner storage unit, a toner manufacturing method, an image forming method, and an image forming apparatus. [Background technology]
[0002] Image formation by electrophotography is generally carried out through a series of processes, in which an electrostatic image is formed on a photoreceptor (electrostatic image carrier), the electrostatic image is developed with a developer to form a visible image (toner image), and the visible image is then transferred to a recording medium such as paper and fixed to form a fixed image. Known developers include two-component developers consisting of a carrier and a toner, and one-component developers (magnetic toner, non-magnetic toner) that do not require a carrier.
[0003] Conventionally, the toner used is a dry toner obtained by melting and kneading a toner binder such as a styrene-based resin or a polyester-based resin together with a colorant and finely pulverizing the toner. Attempts have been made to reduce the particle size of the toner in order to obtain high-quality images. However, in the manufacturing method using the normal kneading and pulverization method, the particle shape is indefinite, and when used as a two-component developer, the toner is further pulverized by stirring with the carrier in the development section, and when used as a one-component developer, by contact stress caused by contact with the development roller, toner supply roller, layer thickness regulating blade, tribocharging blade, etc. This causes problems such as the generation of extremely fine particles and the embedding of the fluidizing agent in the toner surface, resulting in a decrease in image quality.
[0004] In addition, due to its shape, the powder has poor flowability, requiring a large amount of fluidizing agent, and the filling rate in a toner bottle is low, which is an obstacle to compactification, and the benefits of small particle size are not fully realized. Also, with the pulverization method, there is a limit to the particle size of the particles that can be obtained, and it is not possible to respond to further particle size reduction.
[0005] Furthermore, the transfer process of an image formed with multi-color toner from a photoconductor to a transfer medium or paper in order to create a full-color image is becoming more complicated. For this reason, the transferability of an indefinite shape such as pulverized toner is poor, which can cause problems such as missing parts in the transferred image and increased toner consumption to compensate for this.
[0006] Therefore, there is an increasing demand for further improving the transfer efficiency to reduce the amount of toner consumed, obtain high-quality images without missing images, and reduce running costs. If the transfer efficiency is very high, a cleaning unit for removing untransferred toner from the photoconductor or transfer medium becomes unnecessary, which leads to a reduction in the size and cost of the device and also to no waste toner. For this reason, various methods for producing spherical toner have been devised, and methods for producing toner by, for example, the suspension polymerization method, the emulsion polymerization aggregation method, the polymer dissolution suspension method, etc. have been proposed.
[0007] The polymer dissolution suspension method is a process involving volume shrinkage, in which toner materials are dissolved or dispersed in a volatile solvent such as a low-boiling organic solvent, emulsified in an aqueous medium in the presence of a dispersant, and then the volatile solvent is removed (see Patent Document 1). Unlike the suspension polymerization method and the emulsion polymerization aggregation method, this method has a wide range of resins that can be used, and is excellent in that it can use polyester resins that are useful in full-color processes that require transparency and smoothness of image areas after fixing.
[0008] However, there is a problem that the polar group (e.g., acidic group) exists on the surface of the obtained toner particles, and the polar group is affected by the humidity environment, resulting in a decrease in the chargeability. In addition, the dispersant used is strongly adsorbed to the surface of the toner particles, and is difficult to remove even by a subsequent washing operation, resulting in a problem that the chargeability of the toner is largely determined by the dispersant used. For this reason, the average charge level of the obtained toner is low, the charging speed is slow, and the toner is strongly affected by humidity, causing the toner to aggregate and the chargeability to decrease, resulting in poor environmental stability.
[0009] Therefore, Patent Document 2 discloses a method of adding a surfactant having two or more hydrophobic groups in water and attaching it to the surface of toner particles. Patent Document 3 discloses a method of including one or more hydrophobic salts in which a cation derived from a first surfactant and an anion derived from a second surfactant are ionically bonded to the surface layer of a toner particle. Patent Document 4 discloses a toner for developing electrostatic images, which specifies that the amount of ionic functional groups derived from a surfactant in the toner measured by ToF-SIMS is 30,000 or less in terms of intensity value. Summary of the Invention [Problem to be solved by the invention]
[0010] However, in the toner manufacturing method described in Patent Document 2, a hydrophilic surfactant is used, and when such a surfactant adheres to the surface of a toner particle, water molecules tend to be adsorbed to the surface of the toner particle. In particular, in a high humidity environment, water molecules tend to be adsorbed to the surface of a toner particle, and when water molecules are adsorbed to the surface of a toner particle, the charge amount of the toner particle tends to decrease. In addition, the toner described in Patent Document 3 uses a second surfactant to increase the hydrophobicity of the surfactant on the toner surface, and the total amount of surfactant on the toner surface is increased by including this process. Therefore, there is a problem that the fluidity of the toner is deteriorated.
[0011] The present invention has been made in view of the above problems, and has an object to provide a toner for developing electrostatic latent images which has good toner scattering resistance, heat-resistant storage stability, transferability and cleanability. [Means for solving the problem]
[0012] In order to solve the above problems, the present invention relates to a toner described below. A toner for developing electrostatic latent images, characterized in that, of the surfactants contained on the toner surface, more than 60% by mass is a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups, and the surfactant having a long-chain hydrocarbon group and one hydrophilic functional group is not more than 40% by mass. Effect of the Invention
[0013] According to the present invention, it is possible to provide a toner having excellent properties such as toner scattering resistance, heat-resistant storage stability, transferability, and cleanability. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic diagram illustrating an example of an image forming apparatus according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] (Toner and its manufacturing method) The toner of the present invention is obtained by the toner producing method of the present invention. The toner of the present invention is obtained by dissolving or dispersing the toner materials in an organic solvent to prepare a solution or dispersion of the toner materials, emulsifying or dispersing the solution or dispersion in an aqueous medium using a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups, reacting a polymer in the aqueous medium to generate particles containing at least an adhesive base material, and granulating the toner.
[0016] <Toner granulation process> The toner granulation step is a step in which a solution or dispersion of toner materials is emulsified or dispersed in an aqueous medium to form toner particles.
[0017] --Surfactants-- In the present invention, it is extremely important that, in the surfactants used during the above-mentioned emulsification, the surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups accounts for more than 60 mass %, and the surfactant having a long-chain hydrocarbon group and one hydrophilic functional group accounts for 40 mass % or less. When the ratio of surfactants having two or more hydrophilic functional groups is more than 60% by mass, the particle size distribution of the toner during emulsification becomes sharp, and when the ratio of surfactants having one hydrophilic functional group is 40% by mass or less, a decrease in the charge amount of the toner can be suppressed. When the carbon number of the long chain hydrocarbon group in the hydrophobic group of the surfactant is 11 or more, the particle size distribution of the toner is improved. When the carbon number of the long chain hydrocarbon group in the hydrophobic group is less than 14, the toner scattering property and cleaning property are not deteriorated, so that it is preferably less than 14. From the viewpoint of the particle size distribution of the toner, it is preferable that the long chain hydrocarbon group of the surfactant has a straight chain structure. From the viewpoint of the particle size distribution of the toner and cleaning property, it is preferable that the type of the surfactant is anionic.
[0018] -Toner material solution or dispersion liquid- The solution of the toner materials is prepared by dissolving the toner materials in a solvent, and the dispersion of the toner materials is prepared by dispersing the toner materials in a solvent. The toner material is not particularly limited as long as it is capable of forming a toner, and can be appropriately selected depending on the purpose. For example, the toner material includes any one of a monomer, a polymer, an active hydrogen group-containing compound, and a polymer capable of reacting with the active hydrogen group-containing compound, and may include a crystalline polyester resin, and further includes other components such as a colorant, a release agent, a charge control agent, and resin fine particles, as necessary. The solvent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably, for example, an organic solvent.
[0019] --Organic solvents-- The organic solvent is not particularly limited as long as it is a solvent capable of dissolving or dispersing the toner material, and can be appropriately selected according to the purpose. For example, from the viewpoint of ease of removal, a volatile solvent having a boiling point of less than 150° C. is preferable, and examples thereof include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc. Among these, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, etc. are preferable, and ethyl acetate is particularly preferable. These may be used alone or in combination of two or more kinds. The amount of the organic solvent used is not particularly limited and can be appropriately selected depending on the purpose. For example, the amount is preferably 40 to 300 parts by mass, more preferably 60 to 140 parts by mass, and even more preferably 80 to 120 parts by mass, relative to 100 parts by mass of the toner materials.
[0020] -Aqueous medium- The aqueous medium is not particularly limited and can be appropriately selected from known aqueous media. Examples of the aqueous medium include water, solvents miscible with water, and mixtures thereof. The water-miscible solvent is not particularly limited as long as it is miscible with water, and examples thereof include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, and lower ketones. Examples of the alcohol include methanol, isopropanol, ethylene glycol, etc. Examples of the lower ketones include acetone, methyl ethyl ketone, etc. These may be used alone or in combination of two or more.
[0021] -Emulsification or dispersion- When the solution or dispersion of the toner materials is emulsified or dispersed in the aqueous medium, a dispersion (oil droplets) of the solution or dispersion of the toner materials is formed in the aqueous medium. The solution or dispersion of the toner materials is preferably emulsified or dispersed in the aqueous medium while stirring. The dispersion method is not particularly limited and can be appropriately selected using a known dispersing machine, etc., and examples of the dispersing machine include a low-speed shear dispersing machine, a high-speed shear dispersing machine, a friction dispersing machine, a high-pressure jet dispersing machine, an ultrasonic dispersing machine, etc. Among these, a high-speed shear dispersing machine is preferred because it can control the particle size of the dispersion (oil droplets) to 2 to 20 μm. When the high-speed shearing dispersing machine is used, the conditions such as the rotation speed, dispersion time, and dispersion temperature are not particularly limited and can be appropriately selected depending on the purpose, but for example, the rotation speed is preferably 1,000 to 30,000 rpm, more preferably 5,000 to 20,000 rpm, the dispersion time is preferably 0.1 to 5 minutes in the case of a batch method, and the dispersion temperature is preferably 0 to 150° C. under pressure, more preferably 40 to 98° C. Note that the higher the dispersion temperature, the easier the dispersion is generally.
[0022] -Granulation- The granulation method is not particularly limited and can be appropriately selected from known methods. Examples of the granulation method include a method of granulating a toner using a suspension polymerization method, an emulsion polymerization method, a solution suspension method, etc., and a method of granulating a toner by producing an adhesive base material described below while obtaining particles containing at least the adhesive base material. Among these, the method of granulating a toner while producing the adhesive base material is preferred.
[0023] The toner thus granulated contains at least an adhesive base material, and may contain a crystalline polyester resin, and further contains other components such as a colorant, a release agent, a charge control agent, and resin fine particles, as necessary.
[0024] --Adhesive base material-- The adhesive base material exhibits adhesiveness to a recording medium such as paper, and contains at least an adhesive polymer obtained by reacting the active hydrogen group-containing compound and a polymer reactive with the active hydrogen group-containing compound in the aqueous medium, and may further contain a binder resin appropriately selected from known binder resins.
[0025] The weight average molecular weight of the adhesive base material is not particularly limited and can be appropriately selected depending on the purpose, but is, for example, preferably 1,000 or more, more preferably 2,000 to 10,000,000, and particularly preferably 3,000 to 1,000,000. If the weight average molecular weight is less than 1,000, the hot offset resistance may deteriorate.
[0026] The glass transition temperature (Tg) of the adhesive substrate is not particularly limited and may be appropriately selected depending on the purpose, but is preferably, for example, 30 to 70° C., more preferably 40 to 65° C. In the toner of the present invention, since a polyester resin that has been crosslinked and elongated coexists, the toner exhibits good storage stability even though it has a lower glass transition temperature than conventional polyester toners. If the glass transition temperature (Tg) is less than 30° C., the heat-resistant storage stability of the toner may deteriorate, whereas if it exceeds 70° C., the low-temperature fixability may be insufficient.
[0027] The glass transition temperature can be measured, for example, by using a TG-DSC system TAS-100 (manufactured by Rigaku Denki Co., Ltd.) in the following manner: First, about 10 mg of toner is placed in an aluminum sample container, and the sample container is placed on a holder unit and set in an electric furnace. The sample is heated from room temperature to 150°C at a rate of 10°C / min, left at 150°C for 10 min, cooled to room temperature and left for 10 min. Then, heated to 150°C at a rate of 10°C / min under a nitrogen atmosphere, and a DSC curve is measured using a differential scanning calorimeter (DSC). From the obtained DSC curve, the glass transition temperature (Tg) can be calculated from the point of contact between the tangent of the endothermic curve near the glass transition temperature (Tg) and the baseline using the analysis system in the TG-DSC system TAS-100 system.
[0028] The storage modulus of the adhesive substrate is not particularly limited and can be appropriately selected depending on the purpose, but for example, the temperature (TG') at which the storage modulus becomes 10,000 dyne / cm2 at a measurement frequency of 20 Hz is usually 100° C. or higher, and preferably 110 to 200° C. If the (TG') is less than 100° C., the hot offset resistance may deteriorate. The viscosity of the adhesive substrate is not particularly limited and can be appropriately selected depending on the purpose, but for example, the temperature (Tη) at which the viscosity becomes 1,000 poise at a measurement frequency of 20 Hz is usually 180° C. or less, and preferably 90 to 160° C. If the temperature (Tη) exceeds 180° C., the low-temperature fixability may deteriorate. Therefore, from the viewpoint of achieving both hot offset resistance and low-temperature fixability, it is preferable that (TG') is higher than (Tη). That is, the difference between (TG') and (Tη), (TG'-Tη), is preferably 0° C. or more, more preferably 10° C. or more, and even more preferably 20° C. or more. The larger the difference, the better. From the viewpoint of achieving both low temperature fixability and heat-resistant storage stability, the (TG'-Tη) is preferably from 0 to 100°C, more preferably from 10 to 90°C, and even more preferably from 20 to 80°C.
[0029] Specific examples of the adhesive substrate are not particularly limited and can be appropriately selected depending on the purpose, but polyester resins are particularly preferred. The polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but a particularly preferred example is a urea-modified polyester resin. The urea-modified polyester resin is obtained by reacting, in the aqueous medium, an amine (B) as the active hydrogen group-containing compound with an isocyanate group-containing polyester prepolymer (A) as a polymer capable of reacting with the active hydrogen group-containing compound. The urea-modified polyester resin may contain a urethane bond in addition to the urea bond. In this case, the molar ratio of the urea bond to the urethane bond (urea bond / urethane bond) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 100 / 0 to 10 / 90, more preferably 80 / 20 to 20 / 80, and particularly preferably 60 / 40 to 30 / 70. When the number of urea bonds is less than 10, hot offset resistance may deteriorate.
[0030] Specific preferred examples of the urea-modified polyester resin include the following (1) to (10): (1) a mixture of a polyester prepolymer obtained by reacting a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A and isophthalic acid with isophorone diisocyanate, which is urea-modified with isophorone diamine, and a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A and isophthalic acid; (2) a mixture of a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A and isophthalic acid with isophorone diisocyanate; (3) A mixture of an ester prepolymer urea-treated with isophorone diamine and a polycondensate of bisphenol A ethylene oxide 2 mole adduct and terephthalic acid, (4) a polyester prepolymer obtained by reacting a polycondensate of bisphenol A ethylene oxide 2 mole adduct / bisphenol A propylene oxide 2 mole adduct and terephthalic acid with isophorone diisocyanate, and the polyester prepolymer is urea-treated with isophorone diamine, and a mixture of bisphenol A ethylene oxide 2 mole adduct / bisphenol A propylene oxide 2 mole adduct. and a polycondensate of terephthalic acid; (4) a polyester prepolymer obtained by reacting a polycondensate of bisphenol A ethylene oxide 2 mole adduct / bisphenol A propylene oxide 2 mole adduct and terephthalic acid with isophorone diisocyanate, which was ureated with isophorone diamine, and a mixture of the polycondensate of bisphenol A propylene oxide 2 mole adduct and terephthalic acid; (5) a mixture of the polycondensate of bisphenol A ethylene oxide 2 mole adduct and terephthalic acid reacted with isophorone diisocyanate. (6) a mixture of a polyester prepolymer urea-treated with hexamethylenediamine and a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A and terephthalic acid, (7) a mixture of a polyester prepolymer obtained by reacting a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A and terephthalic acid with isophorone diisocyanate, urea-treated with hexamethylenediamine, and a polycondensate of an ethylene oxide 2-mol adduct of bisphenol A / a propylene oxide 2-mol adduct of bisphenol A and terephthalic acid,(7) a mixture of a polyester prepolymer obtained by reacting a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A and terephthalic acid with isophorone diisocyanate, which is urea-treated with ethylenediamine, and a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A and terephthalic acid; (8) a mixture of a polyester prepolymer obtained by reacting a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A and isophthalic acid with diphenylmethane diisocyanate, which is urea-treated with hexamethylenediamine, and a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A and isophthalic acid; (9) a mixture of a 2-mol ethylene oxide adduct of bisphenol A / propanol-bisphenol A; Preferred examples of the polyester prepolymer include a mixture of a polyester prepolymer obtained by reacting a 2-mol ethylene oxide adduct of bisphenol A and a polycondensate of terephthalic acid / dodecenylsuccinic anhydride with diphenylmethane diisocyanate, which is urea-treated with hexamethylenediamine, and a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A / 2-mol propylene oxide adduct of bisphenol A and terephthalic acid; (10) a mixture of a polyester prepolymer obtained by reacting a 2-mol ethylene oxide adduct of bisphenol A and a polycondensate of isophthalic acid with toluene diisocyanate, which is urea-treated with hexamethylenediamine, and a polycondensate of a 2-mol ethylene oxide adduct of bisphenol A and isophthalic acid.
[0031] The amines (B) are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diamines (B1), tri- or higher polyamines (B2), amino alcohols (B3), amino mercaptans (B4), amino acids (B5), and blocked amino groups of the above B1 to B5 (B6). These may be used alone or in combination of two or more. Among these, diamine (B1) and a mixture of diamine (B1) and a small amount of trivalent or higher polyamine (B2) are particularly preferred.
[0032] Examples of the diamine (B1) include aromatic diamines, alicyclic diamines, and aliphatic diamines. Examples of the aromatic diamines include phenylenediamine, diethyltoluenediamine, and 4,4'diaminodiphenylmethane. Examples of the alicyclic diamines include 4,4'-diamino-3,3'dimethyldicyclohexylmethane, diaminecyclohexane, and isophoronediamine. Examples of the aliphatic diamines include ethylenediamine, tetramethylenediamine, and hexamethylenediamine. Examples of the trivalent or higher polyamine (B2) include diethylenetriamine, triethylenetetramine, and the like. Examples of the amino alcohol (B3) include ethanolamine and hydroxyethylaniline. Examples of the amino mercaptan (B4) include aminoethyl mercaptan, aminopropyl mercaptan, and the like. Examples of the amino acid (B5) include aminopropionic acid and aminocaproic acid. Examples of compounds (B6) obtained by blocking the amino group of B1 to B5 include ketimine compounds obtained from any of the amines (B1) to (B5) and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), and oxazoline compounds.
[0033] In addition, a reaction terminator can be used to terminate the elongation reaction, crosslinking reaction, etc. between the active hydrogen group-containing compound and the polymer that can react with the active hydrogen group-containing compound. The use of the reaction terminator is preferable in that the molecular weight, etc. of the adhesive substrate can be controlled to a desired range. Examples of the reaction terminator include monoamines (diethylamine, dibutylamine, butylamine, laurylamine, etc.) and those blocked therefrom (ketimine compounds).
[0034] The mixing ratio of the amines (B) to the isocyanate group-containing polyester prepolymer (A) is preferably such that the mixing equivalent ratio ([NCO] / [NHx]) of the isocyanate group [NCO] in the isocyanate group-containing prepolymer (A) to the amino group [NHx] in the amines (B) is 1 / 3 to 3 / 1, more preferably 1 / 2 to 2 / 1, and particularly preferably 1 / 1.5 to 1.5 / 1. If the mixing equivalent ratio ([NCO] / [NHx]) is less than 1 / 3, the low temperature fixing property may decrease, and if it exceeds 3 / 1, the molecular weight of the urea-modified polyester resin may become low, and the hot offset resistance may deteriorate.
[0035] ---Polymers that can react with compounds containing active hydrogen groups--- The polymer (hereinafter sometimes referred to as "prepolymer") capable of reacting with the active hydrogen group-containing compound is not particularly limited as long as it has at least a site capable of reacting with the active hydrogen group-containing compound, and can be appropriately selected from known resins and the like. Examples of the polymer include polyol resins, polyacrylic resins, polyester resins, epoxy resins, and derivative resins thereof. These may be used alone or in combination of two or more. Among these, polyester resins are particularly preferred in terms of high fluidity and transparency when melted.
[0036] The site in the prepolymer that can react with the active hydrogen group-containing compound is not particularly limited and can be appropriately selected from known substituents, etc., and examples thereof include an isocyanate group, an epoxy group, a carboxylic acid, and an acid chloride group. These may be contained alone or in combination of two or more. Among these, an isocyanate group is particularly preferred.
[0037] Among the above prepolymers, a urea bond-forming group-containing polyester resin (RMPE) is particularly preferred, since it is easy to adjust the molecular weight of the polymer component and can ensure oil-less low-temperature fixing properties in dry toners, particularly good releasability and fixability even when there is no mechanism for applying release oil to the heating medium for fixing. Examples of the urea bond-forming group include an isocyanate group. When the urea bond-forming group in the urea bond-forming group-containing polyester resin (RMPE) is an isocyanate group, the polyester resin (RMPE) is particularly preferably the isocyanate group-containing polyester prepolymer (A).
[0038] The isocyanate group-containing polyester prepolymer (A) is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be a polycondensate of a polyol (PO) and a polycarboxylic acid (PC), and may be obtained by reacting the active hydrogen group-containing polyester resin with a polyisocyanate (PIC).
[0039] The polyol (PO) is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diol (DIO), trihydric or higher polyol (TO), and a mixture of diol (DIO) and trihydric or higher polyol (TO). These may be used alone or in combination of two or more. Among these, the diol (DIO) alone, or a mixture of diol (DIO) and a small amount of trihydric or higher polyol (TO), etc. are preferred.
[0040] Examples of the diol (DIO) include alkylene glycols, alkylene ether glycols, alicyclic diols, alkylene oxide adducts of alicyclic diols, bisphenols, and alkylene oxide adducts of bisphenols. The alkylene glycol preferably has 2 to 12 carbon atoms, and examples thereof include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol. Examples of the alkylene ether glycol include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol. Examples of the alicyclic diol include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. Examples of the alkylene oxide adduct of the alicyclic diol include those obtained by adducting an alkylene oxide such as ethylene oxide, propylene oxide, or butylene oxide to the alicyclic diol. Examples of the bisphenols include bisphenol A, bisphenol F, and bisphenol S. Examples of the alkylene oxide adducts of the bisphenols include adducts of the bisphenols with alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide. Among these, alkylene glycols having 2 to 12 carbon atoms, alkylene oxide adducts of bisphenols, and the like are preferred, and alkylene oxide adducts of bisphenols, and mixtures of alkylene oxide adducts of bisphenols and alkylene glycols having 2 to 12 carbon atoms are particularly preferred.
[0041] The trihydric or higher polyol (TO) is preferably a trihydric to octahydric or higher polyol, and examples thereof include trihydric or higher polyhydric aliphatic alcohols, trihydric or higher polyphenols, and alkylene oxide adducts of trihydric or higher polyphenols. Examples of the trivalent or higher polyhydric aliphatic alcohols include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc. Examples of the trivalent or higher polyphenols include trisphenol PA, phenol novolac, cresol novolac, etc. Examples of the alkylene oxide adducts of the trivalent or higher polyphenols include those obtained by adducting the trivalent or higher polyphenols with alkylene oxides such as ethylene oxide, propylene oxide, butylene oxide, etc.
[0042] In the mixture of the diol (DIO) and the trihydric or higher polyol (TO), the mixing mass ratio (DIO:TO) of the diol (DIO) to the trihydric or higher polyol (TO) is preferably 100:0.01-10, and more preferably 100:0.01-1.
[0043] The polycarboxylic acid (PC) is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polycarboxylic acid (PC) include dicarboxylic acid (DIC), tri- or higher carboxylic acid (TC), and a mixture of dicarboxylic acid (DIC) and tri- or higher carboxylic acid. These may be used alone or in combination of two or more. Among these, dicarboxylic acid (DIC) alone or a mixture of DIC and a small amount of trivalent or higher polycarboxylic acid (TC) is preferred. Examples of the dicarboxylic acid include alkylene dicarboxylic acids, alkenylene dicarboxylic acids, and aromatic dicarboxylic acids. Examples of the alkylene dicarboxylic acid include succinic acid, adipic acid, and sebacic acid. Examples of the alkenylene dicarboxylic acid include those having 4 to 20 carbon atoms, such as maleic acid and fumaric acid. Examples of the aromatic dicarboxylic acid include those having 8 to 20 carbon atoms, such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalene dicarboxylic acid. Among these, alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred.
[0044] The tri- or higher valent polycarboxylic acid (TO) is preferably one having a valence of 3 to 8 or more, and examples thereof include aromatic polycarboxylic acids. The aromatic polycarboxylic acid preferably has 9 to 20 carbon atoms, and examples thereof include trimellitic acid and pyromellitic acid.
[0045] The polycarboxylic acid (PC) may be any acid anhydride or lower alkyl ester selected from the dicarboxylic acid (DIC), the trivalent or higher polycarboxylic acid (TC), and a mixture of the dicarboxylic acid (DIC) and the trivalent or higher polycarboxylic acid. Examples of the lower alkyl ester include methyl ester, ethyl ester, and isopropyl ester.
[0046] The mixture mass ratio (DIC:TC) of the dicarboxylic acid (DIC) and the tri- or higher carboxylic acid (TC) in the mixture of the dicarboxylic acid (DIC) and the tri- or higher carboxylic acid (TC) is not particularly limited and can be appropriately selected depending on the purpose. For example, the ratio is preferably 100:0.01-10, and more preferably 100:0.01-1.
[0047] The mixing ratio when the polyol (PO) and the polycarboxylic acid (PC) are subjected to a polycondensation reaction is not particularly limited and may be appropriately selected depending on the purpose. For example, the equivalent ratio ([OH] / [COOH]) of the hydroxyl group [OH] in the polyol (PO) to the carboxyl group [COOH] in the polycarboxylic acid (PC) is usually preferably 2 / 1 to 1 / 1, more preferably 1.5 / 1 to 1 / 1, and particularly preferably 1.3 / 1 to 1.02 / 1.
[0048] The content of the polyol (PO) in the isocyanate group-containing polyester prepolymer (A) is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably from 0.5 to 40 mass%, more preferably from 1 to 30 mass%, and particularly preferably from 2 to 20 mass%. If the content is less than 0.5% by mass, the hot offset resistance may deteriorate, making it difficult to achieve both the heat resistant storage stability and the low-temperature fixability of the toner, whereas if the content exceeds 40% by mass, the low-temperature fixability may deteriorate.
[0049] The polyisocyanate (PIC) is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate (PIC) include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactam, etc. Examples of the aliphatic polyisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, 2,6-diisocyanatomethyl caproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, tetramethylhexane diisocyanate, etc. Examples of the alicyclic polyisocyanate include isophorone diisocyanate, cyclohexylmethane diisocyanate, etc. Examples of the aromatic diisocyanate include tolylene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthylene diisocyanate, diphenylene-4,4'-diisocyanate, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 3-methyldiphenylmethane-4,4'-diisocyanate, and diphenylether-4,4'-diisocyanate. Examples of the aromatic aliphatic diisocyanate include α,α,α',α'-tetramethylxylylene diisocyanate. Examples of the isocyanurates include tris-isocyanatoalkyl-isocyanurate, triisocyanatocycloalkyl-isocyanurate, and the like. These may be used alone or in combination of two or more.
[0050] Regarding the mixing ratio when reacting the polyisocyanate (PIC) with the active hydrogen group-containing polyester resin (e.g., hydroxyl group-containing polyester resin), the mixing equivalent ratio ([NCO] / [OH]) of the isocyanate group [NCO] in the polyisocyanate (PIC) to the hydroxyl group [OH] in the hydroxyl group-containing polyester resin is usually preferably 5 / 1 to 1 / 1, more preferably 4 / 1 to 1.2 / 1, and particularly preferably 3 / 1 to 1.5 / 1. If the isocyanate group [NCO] exceeds 5, the low temperature fixing property may deteriorate, whereas if it is less than 1, the offset resistance may deteriorate.
[0051] The content of the polyisocyanate (PIC) in the isocyanate group-containing polyester prepolymer (A) is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably 0.5 to 40 mass%, more preferably 1 to 30 mass%, and further preferably 2 to 20 mass%. If the content is less than 0.5% by mass, the hot offset resistance may deteriorate, making it difficult to achieve both heat resistance storage stability and low-temperature fixability, whereas if the content exceeds 40% by mass, the low-temperature fixability may deteriorate.
[0052] The average number of isocyanate groups contained per molecule of the isocyanate group-containing polyester prepolymer (A) is preferably 1 or more, more preferably 1.2 to 5, and even more preferably 1.5 to 4. If the average number of the isocyanate groups is less than 1, the molecular weight of the polyester resin (RMPE) modified with the urea bond-forming group becomes low, and the hot offset resistance may deteriorate.
[0053] The weight average molecular weight (Mw) of the polymer capable of reacting with the active hydrogen group-containing compound is preferably 1,000 to 30,000, more preferably 1,500 to 15,000, as determined by the molecular weight distribution of the tetrahydrofuran (THF) soluble matter by GPC (gel permeation chromatography). If the weight average molecular weight (Mw) is less than 1,000, the heat resistant storage stability may deteriorate, and if it exceeds 30,000, the low temperature fixability may deteriorate.
[0054] The measurement of the molecular weight distribution by gel permeation chromatography (GPC) can be carried out, for example, as follows. That is, first, the column is stabilized in a heat chamber at 40°C. At this temperature, tetrahydrofuran (THF) is passed as the column solvent at a flow rate of 1 ml per minute, and 50 to 200 μl of a tetrahydrofuran sample solution of the resin, the sample concentration of which is adjusted to 0.05 to 0.6 mass%, is injected and measured. In measuring the molecular weight of the sample, the molecular weight distribution of the sample is calculated from the relationship between the logarithm of a calibration curve prepared using several types of monodisperse polystyrene standard samples and the count number. As the standard polystyrene sample for preparing the calibration curve, a 6×10 2 , 2.1×10 2 , 4×10 2 , 1.75×10 4 , 1.1×10 5 , 3.9×10 5 , 8.6×10 5 , 2×10 6 , and 4.48×10 6 It is preferable to use at least about 10 standard polystyrene samples. As the detector, an RI (refractive index) detector can be used.
[0055] ---Binding resin--- The binder resin is not particularly limited and can be appropriately selected depending on the purpose. For example, polyester resins can be mentioned, and unmodified polyester resins (polyester resins that are not modified) are particularly preferred. When the unmodified polyester resin is contained in the toner, the low-temperature fixability and glossiness can be improved. The unmodified polyester resin may be the same as the urea bond-forming group-containing polyester resin, i.e., a polycondensate of polyol (PO) and polycarboxylic acid (PC), etc. From the viewpoint of low-temperature fixability and hot offset resistance, it is preferable that the unmodified polyester resin is partially compatible with the urea bond-forming group-containing polyester resin (RMPE), i.e., that they have similar structures that are compatible with each other.
[0056] The weight average molecular weight (Mw) of the unmodified polyester resin is preferably 1,000 to 30,000, more preferably 1,500 to 15,000, as determined by the molecular weight distribution of the tetrahydrofuran (THF) soluble matter by GPC (gel permeation chromatography). If the weight average molecular weight (Mw) is less than 1,000, the heat-resistant storage stability may deteriorate, so that the content of the component having a weight average molecular weight (Mw) of less than 1,000 is required to be 8 to 28% by mass, as described above. On the other hand, if the weight average molecular weight (Mw) exceeds 30,000, the low-temperature fixability may deteriorate. The glass transition temperature of the unmodified polyester resin is usually 30 to 70° C., more preferably 35 to 70° C., further preferably 35 to 50° C., and particularly preferably 35 to 45° C. If the glass transition temperature is lower than 30° C., the heat-resistant storage stability of the toner may deteriorate, and if it exceeds 70° C., the low-temperature fixability may become insufficient. The unmodified polyester resin preferably has a hydroxyl value of 5 mgKOH / g or more, more preferably 10 to 120 mgKOH / g, and even more preferably 20 to 80 mgKOH / g. If the hydroxyl value is less than 5, it may be difficult to achieve both heat-resistant storage stability and low-temperature fixability. The acid value of the unmodified polyester resin is preferably from 1.0 to 50.0 mgKOH / g, more preferably from 1.0 to 30.0 mgKOH / g, and even more preferably from 5.0 to 20.0 mgKOH / g. In general, by imparting an acid value to the toner, it becomes easier to achieve negative charging properties. When the unmodified polyester resin is contained in the toner, the mixing mass ratio (RMPE / PE) of the urea bond forming group-containing polyester resin (RMPE) to the unmodified polyester resin (PE) is preferably 5 / 95 to 25 / 75, and more preferably 10 / 90 to 25 / 75. If the mixing mass ratio of the unmodified polyester resin (PE) exceeds 95, the hot offset resistance may deteriorate, and it may become difficult to achieve both heat resistance storage stability and low temperature fixability. If the mixing mass ratio is less than 25, the gloss may deteriorate. The content of the unmodified polyester resin in the binder resin is, for example, preferably 50 to 100% by mass, more preferably 70 to 95% by mass, and even more preferably 80 to 90% by mass. If the content is less than 50% by mass, low-temperature fixability and image glossiness may be deteriorated.
[0057] ----Crystalline polyester resin---- The crystalline polyester resin has crystallinity and exhibits a thermal melting property that causes a sudden drop in viscosity near the fixing start temperature. That is, the heat-resistant storage stability is good due to the crystallinity until just before the melting start temperature, and a sudden drop in viscosity (sharp melt property) occurs at the melting start temperature and fixes, so a toner that has both excellent heat-resistant storage stability and low-temperature fixability can be produced. In addition, the toner has an excellent release width (the difference between the lowest low-temperature fixing temperature and the hot offset occurrence temperature).
[0058] The crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. Suitable examples include crystalline polyester resins represented by the following general formula (1) synthesized using a diol compound having 2 to 6 carbon atoms, particularly 1,4-butanediol, 1,6-hexanediol, or a derivative thereof, as an alcohol component, in an amount of 80 mol % or more, and preferably 85 to 100 mol %, and at least maleic acid, fumaric acid, succinic acid, or a derivative thereof as an acidic component.
[0059] [ka] (In the general formula (1), n and m represent the number of repeating units, L represents an integer of 1 to 3, R 1 and R 2 may be the same or different and represent a hydrogen atom or a hydrocarbon group.
[0060] In order to control the crystallinity and softening point of the crystalline polyester resin, when synthesizing the crystalline polyester, a non-linear polyester may be used which is obtained by adding a polyhydric alcohol having a valence of 3 or more, such as glycerin, to the alcohol component, or a polycarboxylic acid having a valence of 3 or more, such as trimellitic anhydride, to the acid component and carrying out condensation polymerization. The molecular structure of the crystalline polyester can be confirmed by solid-state NMR or the like. The weight average molecular weight (Mw) of the crystalline polyester resin, as determined by the molecular weight distribution of the orthodichlorobenzene soluble matter by GPC, is preferably 1,000 to 30,000, and more preferably 1,000 to 6,500. If the weight average molecular weight (Mw) is less than 1,000, the heat resistant storage stability may deteriorate, and if it exceeds 30,000, the low temperature fixability may deteriorate. The number average molecular weight (Mn) of the crystalline polyester resin is preferably 500 to 6,000, more preferably 500 to 2,000, as determined by GPC molecular weight distribution of the orthodichlorobenzene soluble portion. In the molecular weight distribution by GPC, it is preferable that the peak position in a molecular weight distribution chart in which the horizontal axis is log(M) and the vertical axis is mass % is in the range of 3.5 to 4.0, and the half width of the peak is 1.5 or less.
[0061] The melting temperature and F1 / 2 temperature of the crystalline polyester resin are preferably low within a range in which the heat-resistant storage stability is not deteriorated, and for example, the DSC endothermic peak temperature is preferably 50 to 150° C. If the melting temperature and F1 / 2 temperature are lower than 50° C., the heat-resistant storage stability is deteriorated and blocking is likely to occur at the temperature inside the developing device, whereas if they exceed 150° C., the minimum fixing temperature becomes high and low-temperature fixing property may be deteriorated.
[0062] The crystalline polyester resin preferably has an absorption based on δCH (out-of-plane bending vibration) of an olefin at at least one of 965±10 cm-1 and 990±10 cm-1 in an infrared absorption spectrum. When the absorption based on δCH of the olefin is present at the above position, low-temperature fixability is improved.
[0063] The acid value of the crystalline polyester is preferably 8 mgKOH / g or more, more preferably 20 mgKOH / g or more, in order to realize low-temperature fixability from the viewpoint of affinity between paper and resin, while it is preferably 45 mgKOH / g or less in order to improve hot offset resistance. The hydroxyl value of the crystalline polyester resin is preferably from 0 to 50 mgKOH / g, and more preferably from 5 to 50 mgKOH / g, from the viewpoint of improving low-temperature fixing property and charging property.
[0064] When the unmodified polyester resin (b) and the crystalline polyester resin (c) are contained in the toner, the mixing mass ratio of the urea bond-forming group-containing polyester resin (a), the unmodified polyester resin (b), and the crystalline polyester resin (c) is usually (a) / (b)+(c) 5 / 95 to 25 / 75, preferably 10 / 90 to 25 / 75, more preferably 12 / 88 to 25 / 75, and even more preferably 12 / 88 to 22 / 78, and the mass ratio of (b) to (c) is 99 / 1 to 50 / 50, preferably 95 / 5 to 60 / 40, and more preferably 90 / 10 to 65 / 35. If the mass ratio is out of the above numerical range, the hot offset resistance is deteriorated, and it may be difficult to achieve both heat-resistant storage stability and low-temperature fixability.
[0065] --Other ingredients-- The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include colorants, release agents, charge control agents, resin fine particles, inorganic fine particles, flowability improvers, cleaning property improvers, magnetic materials, and metal soaps.
[0066] The colorant is not particularly limited and can be appropriately selected from known dyes and pigments depending on the purpose. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake. , Anthrazan Yellow BGL, Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Par Manent Red F5R, Brilliant Carmine 6B, Pogment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cell Lian Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold,Acid Green Lake, Malachite Green Lake, Phthalocyanine Green, Anthraquinone Green, Titanium Oxide, Zinc Oxide, Lithobone, etc. These may be used alone or in combination of two or more.
[0067] The content of the colorant in the toner is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 1 to 15% by mass, and more preferably from 3 to 10% by mass. If the content is less than 1% by mass, a decrease in the coloring power of the toner is observed, whereas if the content exceeds 15% by mass, poor dispersion of the pigment in the toner occurs, which may lead to a decrease in the coloring power and a decrease in the electrical properties of the toner.
[0068] The colorant may be used as a master batch composited with a resin. The resin is not particularly limited and may be appropriately selected from known resins according to the purpose, and examples thereof include polymers of styrene or its substitutes, styrene copolymers, polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic hydrocarbon resins, alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, paraffin, etc. These may be used alone or in combination of two or more.
[0069] Examples of the polymer of styrene or its substitute include polyester resin, polystyrene, poly-p-chlorostyrene, polyvinyltoluene, etc. Examples of the styrene-based copolymer include styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α-methyl chloromethacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-acrylonitrile-indene copolymer, styrene-maleic acid copolymer, styrene-maleic acid ester copolymer, etc.
[0070] The master batch can be produced by mixing or kneading the master batch resin and the colorant under high shear force. In this case, it is preferable to add an organic solvent to enhance the interaction between the colorant and the resin. The so-called flushing method is also preferable because it allows the wet cake of the colorant to be used as is and does not require drying. The flushing method is a method in which an aqueous paste containing water of the colorant is mixed or kneaded with a resin and an organic solvent, and the colorant is transferred to the resin side to remove water and organic solvent components. For example, a high shear dispersion device such as a three-roll mill is preferably used for the mixing or kneading.
[0071] The releasing agent is not particularly limited and can be appropriately selected from known agents depending on the purpose. Suitable examples include waxes. Examples of the waxes include carbonyl group-containing waxes, polyolefin waxes, long chain hydrocarbons, etc. These may be used alone or in combination of two or more. Among these, carbonyl group-containing waxes are preferred. Examples of the carbonyl group-containing wax include polyalkanoic acid esters, polyalkanol esters, polyalkanoic acid amides, polyalkyl amides, and dialkyl ketones. Examples of the polyalkanoic acid esters include carnauba wax, montan wax, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, and 1,18-octadecanediol distearate. Examples of the polyalkanol esters include trimellitic acid tristearyl and distearyl maleate. Examples of the polyalkanoic acid amides include dibehenyl amide. Examples of the polyalkyl amides include trimellitic acid tristearyl amide. Examples of the dialkyl ketones include distearyl ketone. Among these carbonyl group-containing waxes, polyalkanoic acid esters are particularly preferred. Examples of the polyolefin wax include polyethylene wax and polypropylene wax. Examples of the long chain hydrocarbon include paraffin wax and sazol wax.
[0072] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 40 to 160°C, more preferably from 50 to 120°C, and particularly preferably from 60 to 90°C. If the melting point is less than 40° C., the wax may adversely affect the heat resistance storage stability, whereas if it exceeds 160° C., cold offset may easily occur during fixing at low temperatures. The melt viscosity of the release agent is preferably from 5 to 1000 cps, and more preferably from 10 to 100 cps, as measured at a temperature 20° C. higher than the melting point of the wax. If the melt viscosity is less than 5 cps, the releasability may decrease, whereas if it exceeds 1000 cps, the effect of improving hot offset resistance and low-temperature fixability may not be obtained.
[0073] The content of the release agent in the toner is not particularly limited and may be appropriately selected depending on the purpose, but is preferably from 0 to 40% by mass, and more preferably from 3 to 30% by mass. If the content exceeds 40% by mass, the fluidity of the toner may deteriorate.
[0074] The charge control agent is not particularly limited and can be appropriately selected from known agents according to the purpose, but since the use of a colored material may cause a change in color tone, a colorless or nearly white material is preferred, and examples thereof include triphenylmethane dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus alone or its compounds, tungsten alone or its compounds, fluorine-based activators, metal salts of salicylic acid, metal salts of salicylic acid derivatives, etc. These may be used alone or in combination of two or more. The charge control agent may be a commercially available product, and examples of the commercially available product include quaternary ammonium salt Bontron P-51, oxynaphthoic acid metal complex E-82, salicylic acid metal complex E-84, phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), quaternary ammonium salt molybdenum complex TP-302, TP-415 (all manufactured by Hodogaya Chemical Industry Co., Ltd.), quaternary ammonium salt copy charge PSYVP2038, triphenylmethane derivative copy blue PR, quaternary ammonium salt copy charge NEGVP2036, copy charge NXVP434 (all manufactured by Hoechst), LRA-901, boron complex LR-147 (manufactured by Nippon Carlit Co., Ltd.), quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts. The charge control agent may be melt-kneaded together with the master batch and then dissolved or dispersed, or may be added directly to the organic solvent together with each of the toner components when the charge control agent is dissolved or dispersed, or may be fixed to the surface of the toner after the toner particles are produced.
[0075] The content of the charge control agent in the toner varies depending on the type of the binder resin, the presence or absence of additives, the dispersion method, etc., and cannot be generally defined, but for example, it is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the binder resin. If the content is less than 0.1 parts by mass, charge controllability may not be obtained, and if it exceeds 10 parts by mass, the chargeability of the toner becomes too high, reducing the effect of the main charge control agent and increasing the electrostatic attraction force with the developing roller, which may lead to a decrease in the fluidity of the developer and a decrease in image density.
[0076] The resin fine particles are not particularly limited as long as they are capable of forming an aqueous dispersion in an aqueous medium, and can be appropriately selected from known resins depending on the purpose. They may be thermoplastic resins or thermosetting resins, such as vinyl resins, polyurethane resins, epoxy resins, polyester resins, polyamide resins, polyimide resins, silicon resins, phenolic resins, melamine resins, urea resins, aniline resins, ionomer resins, and polycarbonate resins. These may be used alone or in combination of two or more. Among these, it is preferable to use at least one resin selected from vinyl resin, polyurethane resin, epoxy resin, and polyester resin, since it is easy to obtain an aqueous dispersion of fine spherical resin particles. The vinyl resin is a polymer obtained by homopolymerizing or copolymerizing a vinyl monomer, and examples thereof include styrene-(meth)acrylic acid ester resin, styrene-butadiene copolymer, (meth)acrylic acid-acrylic acid ester polymer, styrene-acrylonitrile copolymer, styrene-maleic anhydride copolymer, and styrene-(meth)acrylic acid copolymer. Furthermore, as the resin fine particles, a copolymer containing a monomer having at least two unsaturated groups can also be used. The monomer having at least two unsaturated groups is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include sodium salt of methacrylic acid ethylene oxide adduct sulfate ester ("Eleminol RS-30" manufactured by Sanyo Chemical Industries, Ltd.), divinylbenzene, and 1,6-hexanediol acrylate.
[0077] The resin microparticles can be obtained by polymerization according to a known method appropriately selected according to the purpose, but it is preferable to obtain the resin microparticles as an aqueous dispersion.The method for preparing the aqueous dispersion of the resin microparticles includes, for example, (1) in the case of the vinyl resin, a method of directly producing an aqueous dispersion of the resin microparticles by any polymerization reaction selected from suspension polymerization, emulsion polymerization, seed polymerization and dispersion polymerization using a vinyl monomer as a starting material; (2) in the case of the polyaddition or condensation resin such as the polyester resin, polyurethane resin, or epoxy resin, a method of dispersing a precursor (monomer, oligomer, etc.) or its solvent solution in an aqueous medium in the presence of a suitable dispersant, and then curing by heating or adding a curing agent to produce an aqueous dispersion of the resin microparticles; (3) in the case of the polyaddition or condensation resin such as the polyester resin, polyurethane resin, or epoxy resin, a method of dispersing a precursor (monomer, oligomer, etc.) or its solvent solution (preferably liquid) in the case of the polyaddition or condensation resin.(4) a method in which a resin previously prepared by a polymerization reaction (which may be any polymerization reaction type such as addition polymerization, ring-opening polymerization, polyaddition, addition condensation, or condensation polymerization) is pulverized using a mechanical rotary or jet type fine grinder, and then classified to obtain fine resin particles, which are then dispersed in water in the presence of a suitable dispersant; (5) a method in which a resin previously prepared by a polymerization reaction (which may be any polymerization reaction type such as addition polymerization, ring-opening polymerization, polyaddition, addition condensation, or condensation polymerization) is dissolved in a solvent and a resin solution is sprayed into a mist to obtain fine resin particles, which are then dispersed in water in the presence of a suitable dispersant; (6) a method in which a resin previously prepared by a polymerization reaction (which may be any polymerization reaction type such as addition polymerization, ring-opening polymerization, polyaddition, addition condensation, or condensation polymerization) is dissolved in a solvent and a resin solution is sprayed into a mist to obtain fine resin particles, which are then dispersed in water in the presence of a suitable dispersant. (b) a method in which a poor solvent is added to a resin solution obtained by dissolving a resin prepared in advance in a solvent, or a resin solution previously dissolved in a solvent by heating is cooled to precipitate resin fine particles, the solvent is then removed to obtain resin particles, and the resin particles are then dispersed in water in the presence of a suitable dispersant; (7) a method in which a resin solution obtained by dissolving a resin previously prepared by a polymerization reaction (which may be any polymerization reaction type such as addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) in a solvent is dispersed in an aqueous medium in the presence of a suitable dispersant, and the solvent is then removed by heating or reducing pressure, etc.; and (8) a method in which a suitable emulsifier is dissolved in a resin solution obtained by dissolving a resin previously prepared by a polymerization reaction (which may be any polymerization reaction type such as addition polymerization, ring-opening polymerization, polyaddition, addition condensation, condensation polymerization, etc.) in a solvent, and water is then added to effect phase inversion emulsification.
[0078] The inorganic fine particles are not particularly limited and may be appropriately selected from known fine particles depending on the purpose, and examples thereof include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengalla, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, silicon nitride, etc. These may be used alone or in combination of two or more. The primary particle diameter of the inorganic fine particles is preferably 5 nm to 2 μm, and more preferably 5 nm to 500 nm. The specific surface area of the inorganic fine particles measured by the BET method is preferably 20 to 500 m. 2 / g is preferred. The content of the inorganic fine particles in the toner is preferably from 0.01 to 5.0% by mass, and more preferably from 0.01 to 2.0% by mass.
[0079] The flow improver refers to a material that is surface-treated to increase hydrophobicity and prevent deterioration of flow characteristics and charging characteristics even under high humidity conditions. Examples of such a material include silane coupling agents, silylation agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, and modified silicone oils. The cleaning property improver is added to the toner in order to remove the developer remaining on the photoconductor or primary transfer medium after transfer, and examples thereof include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles, etc. The polymer fine particles preferably have a relatively narrow particle size distribution, and are preferably ones having a volume average particle size of 0.01 to 1 μm. The magnetic material is not particularly limited and may be appropriately selected from known materials depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, a white material is preferable in terms of color tone.
[0080] As an example of the granulation, a method of granulating the toner while producing the adhesive base material will be described below. In the method of granulating the toner while producing the adhesive base material, for example, preparation of an aqueous medium phase, preparation of a solution or dispersion of the toner materials, preparation of an emulsion or dispersion, production of the adhesive base material, removal of the organic solvent, and other steps (synthesis of a polymer (prepolymer) capable of reacting with the active hydrogen group-containing compound, synthesis of the active hydrogen group-containing compound, etc.) are performed.
[0081] The aqueous medium phase can be prepared, for example, by dispersing the resin fine particles in the aqueous medium. The amount of the resin fine particles added to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, and is preferably, for example, 0.5 to 10% by mass. The solution or dispersion of the toner materials can be prepared by dissolving or dispersing the toner materials, such as the active hydrogen group-containing compound, the polymer capable of reacting with the active hydrogen group-containing compound, the crystalline polyester resin, the colorant, the release agent, the charge control agent, and the unmodified polyester resin, in the organic solvent. In addition, among the toner materials, components other than the polymer (prepolymer) capable of reacting with the active hydrogen group-containing compound may be added and mixed into the aqueous medium when dispersing the resin fine particles in the aqueous medium in preparing the aqueous medium phase, or may be added to the aqueous medium phase together with the solution or dispersion of the toner materials when the solution or dispersion is added to the aqueous medium phase.
[0082] The emulsion or dispersion can be prepared by emulsifying or dispersing the previously prepared solution or dispersion of the toner material in the previously prepared aqueous medium phase. During the emulsification or dispersion, the active hydrogen group-containing compound and the polymer capable of reacting with the active hydrogen group-containing compound are subjected to an elongation reaction or crosslinking reaction to produce the adhesive substrate. The adhesive base material (e.g., the urea-modified polyester resin) may be produced, for example, by: (1) emulsifying or dispersing a solution or dispersion of the toner material containing a polymer (e.g., the isocyanate group-containing polyester prepolymer (A)) capable of reacting with the active hydrogen group-containing compound together with the active hydrogen group-containing compound (e.g., the amines (B)) in the aqueous medium phase to form a dispersion, and causing an elongation reaction or crosslinking reaction between the two in the aqueous medium phase; (2) emulsifying or dispersing a solution or dispersion of the toner material in the aqueous medium to which the active hydrogen group-containing compound has been added in advance, to form a dispersion, and causing an elongation reaction or crosslinking reaction between the two in the aqueous medium phase; or (3) adding and mixing the solution or dispersion of the toner material in the aqueous medium, adding the active hydrogen group-containing compound to form a dispersion, and causing an elongation reaction or crosslinking reaction between the two from the particle interface in the aqueous medium phase. In the case of the above (3), the modified polyester resin is preferentially formed on the surface of the toner particles, and a concentration gradient can be provided in the toner particles.
[0083] The reaction conditions for producing the adhesive base material by the emulsification or dispersion are not particularly limited and can be appropriately selected depending on the combination of the polymer reactive with the active hydrogen group-containing compound and the active hydrogen group-containing compound. The reaction time is preferably 10 minutes to 40 hours, and more preferably 2 hours to 24 hours. The reaction temperature is preferably 0 to 150°C, and more preferably 40 to 98°C.
[0084] Examples of a method for stably forming the dispersion containing the polymer (e.g., the isocyanate group-containing polyester prepolymer (A)) capable of reacting with the active hydrogen group-containing compound in the aqueous medium phase include a method of adding a solution or dispersion of the toner materials, which is prepared by dissolving or dispersing the toner materials such as the polymer (e.g., the isocyanate group-containing polyester prepolymer (A)) capable of reacting with the active hydrogen group-containing compound, the colorant, the release agent, the charge control agent, and the unmodified polyester resin in the organic solvent, to the aqueous medium phase, and dispersing the toner materials by shear force. Details of the dispersion method are as described above.
[0085] In preparing the emulsion or dispersion, the amount of the aqueous medium used is preferably 50 to 2,000 parts by mass, and more preferably 100 to 1,000 parts by mass, based on 100 parts by mass of the toner materials. If the amount used is less than 50 parts by mass, the toner materials may be poorly dispersed, making it difficult to obtain toner particles having a desired particle size, whereas if the amount used is more than 2,000 parts by mass, the production cost may become high.
[0086] Examples of the poorly water-soluble inorganic compound dispersant include tricalcium phosphate, calcium carbonate, titanium oxide, colloidal silica, and hydroxyapatite. Examples of the polymer protective colloid include acids, (meth)acrylic monomers containing a hydroxyl group, vinyl alcohol or ethers with vinyl alcohol, esters of vinyl alcohol and a compound containing a carboxyl group, amide compounds or methylol compounds thereof, chlorides, homopolymers or copolymers of those having a nitrogen atom or a heterocycle thereof, polyoxyethylenes, celluloses, and the like. Examples of the acids include acrylic acid, methacrylic acid, α-cyanoacrylic acid, α-cyanomethacrylic acid, itaconic acid, crotonic acid, fumaric acid, maleic acid, maleic anhydride, etc. Examples of the (meth)acrylic monomers containing a hydroxyl group include β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, γ-hydroxypropyl acrylate, γ-hydroxypropyl methacrylate, 3-chloro 2-hydroxypropyl acrylate, 3-chloro-2-hydroxypropyl methacrylate, diethylene glycol monoacrylate, diethylene glycol monomethacrylate, glycerin monoacrylate, glycerin monomethacrylate, N-methylol acrylamide, N-methylol methacrylamide, etc. Examples of the vinyl alcohol or ethers with vinyl alcohol include vinyl methyl ether, vinyl ethyl ether, vinyl propyl ether, etc. Examples of the esters of vinyl alcohol and a compound containing a carboxyl group include vinyl acetate, vinyl propionate, and vinyl butyrate. Examples of the amide compounds or methylol compounds thereof include acrylamide, methacrylamide, diacetone acrylamide acid, or methylol compounds thereof. Examples of the chlorides include acrylic acid chloride and methacrylic acid chloride. Examples of the homopolymers or copolymers having a nitrogen atom or a heterocycle thereof include vinylpyridine, vinylpyrrolidone, vinylimidazole, and ethyleneimine. Examples of the polyoxyethylene-based compounds include polyoxyethylene, polyoxypropylene, polyoxyethylene alkylamines, polyoxypropylene alkylamines, polyoxyethylene alkylamides, polyoxypropylene alkylamides, polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl phenyl ether, polyoxyethylene stearyl phenyl ester, and polyoxyethylene nonylphenyl ester.Examples of the celluloses include methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose.
[0087] In preparing the emulsion or dispersion, a dispersion stabilizer may be used as necessary. The dispersion stabilizer may be, for example, a calcium phosphate or the like that is soluble in an acid or an alkali. When such a dispersion stabilizer is used, the calcium phosphate can be removed from the fine particles by dissolving the calcium phosphate with an acid such as hydrochloric acid, followed by washing with water or decomposing with an enzyme.
[0088] In preparing the emulsion or dispersion, a catalyst for the elongation reaction or the crosslinking reaction can be used, such as dibutyltin laurate or dioctyltin laurate.
[0089] The organic solvent is removed from the obtained dispersion (emulsion slurry). The organic solvent can be removed by (1) gradually increasing the temperature of the entire reaction system to completely evaporate and remove the organic solvent in the oil droplets, or (2) spraying the emulsified dispersion into a dry atmosphere to completely remove the water-insoluble organic solvent in the oil droplets to form toner particles, and at the same time, evaporating and removing the aqueous dispersant. When the organic solvent is removed, toner particles are formed. Then, the toner particles can be washed, etc.
[0090] Through the above steps, the solution or dispersion of the toner materials is emulsified or dispersed in the aqueous medium, and the toner is granulated.
[0091] <Other processes> The toner particles obtained through the toner granulation step and the toner hydrophobization step can be subjected to drying, etc., and further, if desired, classification, etc. The classification can be performed, for example, by removing fine particle portions in a liquid using a cyclone, a decanter, centrifugal separation, etc., and the toner particles may be obtained as a powder after drying and then classified.
[0092] In addition, by mixing the obtained toner particles with particles of the colorant, the release agent, the charge control agent, etc., or by further applying a mechanical impact force to the toner particles, it is possible to prevent the particles of the release agent, etc. from being detached from the surface of the toner particles. Examples of the method of applying the mechanical impact force include a method of applying an impact force to the mixture by a blade rotating at high speed, a method of introducing the mixture into a high-speed air current and accelerating it to collide the particles with each other or the composite particles with an appropriate collision plate, etc. Examples of the device used in this method include an Angmill (manufactured by Hosokawa Micron Corporation), a device modified from an I-type mill (manufactured by Japan Pneumatic Co., Ltd.) with a reduced grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), an automatic mortar, etc.
[0093] The toner of the present invention preferably has the following volume average particle size (Dv), volume average particle size (Dv) / number average particle size (Dn), average circularity, penetration, low-temperature fixability, offset non-occurrence temperature, thermal characteristics, glass transition temperature, image density, BET specific surface area, etc.
[0094] The volume average particle diameter (Dv) of the toner is, for example, preferably from 3 to 8 μm, more preferably from 4 to 7, and even more preferably from 5 to 6. If the volume average particle size is less than 3 μm, in the case of a two-component developer, the toner may fuse to the surface of the carrier during long-term stirring in a developing device, reducing the charging ability of the carrier. Also, in the case of a one-component developer, toner filming on the developing roller and toner fusion to components such as blades may occur easily due to the toner being made into a thin layer. If the volume average particle size exceeds 8 μm, it becomes difficult to obtain high-resolution, high-quality images, and the fluctuation in the particle size of the toner may become large when the toner balance in the developer is performed.
[0095] The ratio (Dv / Dn) of the volume average particle diameter (Dv) to the number average particle diameter (Dn) of the toner is, for example, preferably 1.20 or less, more preferably 1.00 to 1.20, further preferably 1.10 to 1.20, and particularly preferably 1.10 to 1.15. If the ratio (Dv / Dn) of the volume average particle diameter to the number average particle diameter is less than 1.00, in the case of a two-component developer, the toner may fuse to the surface of the carrier during long-term stirring in the developing device, reducing the charging ability of the carrier and worsening the cleaning ability. In addition, in the case of a one-component developer, the toner may film on the developing roller, or the toner may fuse to members such as a blade due to the thinning of the toner layer. If the ratio exceeds 1.20, it becomes difficult to obtain a high-resolution, high-quality image, and the fluctuation in the particle diameter of the toner may become large when the toner balance in the developer is performed.
[0096] The volume average particle diameter and the ratio of the volume average particle diameter to the number average particle diameter (Dv / Dn) can be measured using, for example, a particle size measuring device "Multisizer II" manufactured by Beckman Coulter.
[0097] The average circularity is a value obtained by dividing the perimeter of a circle having the same projected area as the shape of the toner by the perimeter of an actual particle, and is preferably 0.900 to 0.980, more preferably 0.950 to 0.975. It is preferable that the percentage of particles having an average circularity of less than 0.940 is 15% or less. If the average circularity is less than 0.900, it may not be possible to obtain a high-quality image with satisfactory transferability and no dust, whereas if it exceeds 0.980, in an image forming system employing blade cleaning or the like, poor cleaning of the photoconductor and transfer belt may occur, resulting in stains on the image. For example, in the case of forming an image with a high image area ratio such as a photographic image, toner that has formed an image that has not been transferred due to poor paper feed or the like may remain on the photoconductor as transfer residual toner, resulting in image stains. Alternatively, the charging roller that contact-charges the photoconductor may be contaminated, resulting in the original charging ability not being exhibited. The average circularity can be measured, for example, by an optical detection zone technique in which a suspension containing a toner is passed through an imaging detection zone on a flat plate, and particle images are optically detected and analyzed by a CCD camera. For example, the average circularity can be measured using a flow type particle image analyzer FPIA-2100 (manufactured by Sysmex Corporation).
[0098] The penetration, for example, as measured by a penetration test (JISK2235-1991) must be 15 mm or more, and is more preferably 20 to 30 mm. If the penetration is less than 15 mm, the heat-resistant storage stability may deteriorate. The penetration can be measured according to JIS K2235-1991, specifically, a 50 ml glass container is filled with toner and left in a thermostatic chamber at 50° C. for 20 hours. The toner is cooled to room temperature, and a penetration test is performed to measure the penetration. The larger the penetration value, the better the heat-resistant storage stability.
[0099] Regarding the low-temperature fixability, from the viewpoint of achieving both a reduction in the fixing temperature and no occurrence of offset, the lower the minimum fixing temperature, the more preferable, and the higher the offset non-reaction temperature, the more preferable. The temperature range in which a reduction in the fixing temperature and no occurrence of offset can be achieved is a temperature range in which the minimum fixing temperature is less than 150° C. and the offset non-reaction temperature is 200° C. or higher. The minimum fixing temperature is determined by, for example, using an image forming apparatus, setting transfer paper, performing a copy test, and rubbing the resulting fixed image with a pad to determine the fixing roll temperature at which the remaining image density is 70% or more. The temperature at which offset does not occur can be determined, for example, by using an image forming apparatus, setting transfer paper, adjusting the apparatus so that solid images of each of the single colors of yellow, magenta, cyan, and black, and solid images of each of the intermediate colors of red, blue, and green are developed in each single color, adjusting the temperature of the fixing belt so that it is variable, and measuring the temperature at which offset does not occur.
[0100] The thermal properties are also called flow tester properties, and are evaluated as, for example, softening temperature (Ts), flow start temperature (Tfb), 1 / 2 method softening point (T1 / 2), and the like. These thermal properties can be measured by an appropriately selected method, for example, they can be obtained from a flow curve measured using an elevated flow tester CFT500 type (manufactured by Shimadzu Corporation). The softening temperature (Ts) is not particularly limited and can be appropriately selected depending on the purpose, and is, for example, preferably 30° C. or higher, more preferably 50 to 120° C. If the softening temperature (Ts) is lower than 30° C., at least one of the heat-resistant storage stability and the low-temperature storage stability may deteriorate. The flow-out starting temperature (Tfb) is not particularly limited and can be appropriately selected depending on the purpose, and is, for example, preferably 50° C. or higher, more preferably 60 to 150° C. If the flow-out starting temperature (Tfb) is lower than 50° C., at least one of the heat-resistant storage stability and the low-temperature storage stability may deteriorate. The 1 / 2 method softening point (T1 / 2) is not particularly limited and can be appropriately selected depending on the purpose, and is, for example, preferably 60° C. or higher, more preferably 80 to 170° C. If the 1 / 2 method softening point (T1 / 2) is less than 60° C., at least one of the heat-resistant storage stability and the low-temperature storage stability may deteriorate.
[0101] The glass transition temperature is not particularly limited and can be appropriately selected depending on the purpose, but is, for example, preferably 40 to 70° C., more preferably 45 to 65° C. If the glass transition temperature (Tg) is less than 40° C., the heat-resistant storage stability of the toner may deteriorate, and if it exceeds 70° C., the low-temperature fixability may be insufficient. The glass transition temperature can be measured, for example, by using a differential scanning calorimeter ("DSC-60" manufactured by Shimadzu Corporation, etc.).
[0102] The image density, as measured using a spectrometer (X-Rite 938 Spectrodensitometer), is preferably, for example, 1.40 or more, more preferably 1.45 or more, and particularly preferably 1.50 or more. When the image density is less than 1.40, the image density is low and high image quality may not be obtained. The image density is measured, for example, by using a color copier ("PRETER 550" manufactured by Ricoh Co., Ltd.) to print a toner image on copying paper ("Type 6200" manufactured by Ricoh Co., Ltd.) with an amount of developer adhered of 0.4±0.05 mg / cm 2 2 A solid image is formed with a surface temperature of the fixing roller of 160±2°C, and the image density of any three points on the obtained solid image is measured using a spectrometer (X-Rite 938 Spectrodensitometer) and the average value is calculated.
[0103] The BET specific surface area of the toner is, for example, 0.5 to 8.0 m 2 / g is preferable, and 0.5 to 7.5m 2 / g is more preferred. The BET specific surface area is 0.5 m 2 If it is less than 8.0 m2 / g, the resin fine particles remaining on the toner surface will form a film or densely cover the entire toner surface, and the resin fine particles will inhibit the adhesion between the binder resin component inside the toner and the fixing paper, and an increase in the minimum fixing temperature may be observed. On the other hand, if it exceeds 8.0 m2 / g, the resin fine particles will inhibit the seepage of the wax, the release effect of the wax will not be obtained, and offset may occur. The specific surface area of the toner can be measured according to the BET method. For example, a specific surface area measuring device Tristar 3000 (manufactured by Shimadzu Corporation) can be used to adsorb nitrogen gas onto a sample surface and measure using the BET multipoint method.
[0104] The acid value of the toner is, for example, preferably 0.5 to 40.0 (KOHmg / g), more preferably 1.0 to 30.0, and even more preferably 5.0 to 20.0. By imparting an acid value to the toner, it becomes easier to have negative chargeability.
[0105] The coloring of the toner of the present invention is not particularly limited and can be appropriately selected depending on the purpose. It can be at least one type selected from black toner, cyan toner, magenta toner, and yellow toner, and the toner of each color can be obtained by appropriately selecting the type of colorant.
[0106] In the toner manufacturing method of the present invention, in the toner granulation step, the solution or dispersion of the toner materials is emulsified or dispersed in the aqueous medium using the surfactant to granulate the toner, so that a toner having good properties such as chargeability, anti-aggregation property, and fluidity, high hydrophobicity, and excellent environmental stability can be efficiently manufactured.
[0107] The toner of the present invention has a high hydrophobic surface, and therefore has good properties such as chargeability, anti-aggregation property, and flowability, and is excellent in environmental stability, and can form high-quality images. Furthermore, when the toner of the present invention contains particles containing at least the adhesive substrate obtained by reacting the active hydrogen group-containing compound and a polymer capable of reacting with the active hydrogen group-containing compound in an aqueous medium, the toner is further excellent in properties such as transferability and fixability.
[0108] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores toner. The developing device has a means for containing toner and developing the toner. The process cartridge is a cartridge that integrates at least an image carrier and a developing means, contains toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, and a cleaning means.
[0109] By mounting the toner storage unit of the present invention in an image forming apparatus and forming an image, the image is formed using the toner of any one of the first to fourth aspects of the present invention, so that it is possible to reduce the amount of toner consumed, obtain a high-quality image without missing images, and reduce running costs.
[0110] The image forming method of the present invention is carried out, for example, by an image forming apparatus using an electrophotographic process as shown in the schematic configuration diagram of Fig. 1. The schematic configuration of the image forming apparatus shown in Fig. 1 will be described below. While the photoconductor (image carrier) 1 is rotationally driven in the direction of the arrow, its surface is uniformly charged by the charger 2 (charging process). Next, the photoconductor 1 is irradiated with image light γ by an exposure means (not shown) at an exposure section downstream of the charger 2 in the rotational direction. As a result, the charge on the photoconductor surface at the portion irradiated with the image light γ disappears, and an electrostatic latent image corresponding to the image light is formed on the surface of the photoconductor 1.
[0111] A developing device 3 serving as a developing means is disposed downstream of the exposure section, and a toner 4 serving as a developer is contained within the developing device 3. The toner 4 is stirred and mixed by a paddle (stirring mechanism) 14 equipped with a conveying screw 13, triboelectrically charged to a predetermined polarity, and then conveyed by a developing sleeve 5 to a nip portion (developing area) between the developing sleeve 5 and the photoconductor 1. The toner conveyed to this developing area is moved from the surface of the developing sleeve 5 to the surface side of the photoconductor 1 by a developing electric field formed in the developing area by a developing bias application means (not shown), and adheres to the photoconductor surface, thereby forming a toner image (visible image) from the electrostatic latent image formed on the photoconductor surface (developing process).
[0112] The toner image thus formed on the photoconductor 1 is transferred onto a transfer sheet S as a transfer body fed to the transfer section by a registration roller 18 at a nip portion (transfer section) between the photoconductor 1 and a transfer conveyor belt 6 as a transfer means disposed downstream of the developing device 3 in close proximity to the photoconductor 1 (transfer process). The transfer sheet onto which the toner image has been transferred has the toner image fixed by a fixing roller (not shown) as a fixing means disposed downstream of the rotation direction of the transfer conveyor belt 6 (process of obtaining a fixed image), and is then discharged onto a paper discharge tray outside the main body of the apparatus by a paper discharge means (not shown). The transfer conveyor belt 6 is suspended on a bias roller 6a.
[0113] Meanwhile, toner (residual toner) remaining on the photoconductor 1 without being transferred to the transfer paper in the transfer section is removed from the photoconductor 1 by a cleaning blade 7, a recovery spring 8 and a recovery coil 9 of a cleaning device serving as cleaning means disposed downstream of the transfer section in the direction of rotation of the photoconductor. Residual charge remaining on the photoconductor 1 after cleaning of the residual toner is removed by a charge remover 20 consisting of a charge removing lamp or the like. Among the reference numerals in Fig. 1, 16 is a reflection density detection sensor (P sensor) and 17 is a toner concentration sensor. 10 represents the photoconductor and cleaning unit (PCU). EXAMPLES
[0114] Examples of the present invention will be described below, but the present invention is not limited to these examples. In the following description, unless otherwise specified, parts means parts by mass and % means % by mass.
[0115] In the following examples, the acid value, hydroxyl value, and weight average molecular weight of resins such as crystalline polyester resins, amorphous polyester resins, and polyester prepolymers were measured as follows.
[0116] <Acid value measurement> The measurement was carried out under the following conditions in accordance with the measurement method described in JIS K0070-1992. First, 0.5 g of the sample (0.3 g of the ethyl acetate soluble portion) was added to 120 mL of toluene and dissolved by stirring at room temperature (23° C.) for about 10 hours. Furthermore, 30 mL of ethanol was added to prepare a sample solution. The acid value was measured at 23°C using an automatic potentiometric titrator (DL-53Titrator, Mettler Toledo) and an electrode DG113-SC (Mettler Toledo), and the results were analyzed using the analysis software LabXLight Version 1.00.000. In addition, a mixed solvent of 120 mL of toluene and 30 mL of ethanol was used in the apparatus. The hydroxyl group was also measured under similar conditions. The acid value can be calculated by the above-mentioned measurement method, but specifically, it was calculated as follows: The sample was titrated with a standardized 0.1N potassium hydroxide / alcohol solution in advance, and the acid value was calculated from the titration amount according to the following formula. Acid value [KOHmg / g] = Titration volume [mL] × N × 56.1 [mg / mL] / sample mass [g] (where N is the factor of 0.1N potassium hydroxide / alcohol solution)
[0117] <Measurement of hydroxyl value> The measurement was carried out under the following conditions in accordance with the measurement method described in JIS K0070-1966. First, 0.5 g of a sample was precisely weighed into a 100-mL measuring flask, and 5 mL of an acetylation reagent was precisely added thereto. Thereafter, the sample was immersed in a bath at 100°C ± 5°C and heated. After 1-2 hours, the flask was removed from the bath and allowed to cool, after which water was added and the flask was shaken to decompose the acetic anhydride. Next, to complete the decomposition, the flask was heated again in the bath for 10 minutes or more, allowed to cool, and the walls of the flask were thoroughly washed with an organic solvent. This liquid was subjected to potentiometric titration with N / 2 potassium hydroxide ethyl alcohol solution using the above electrode to determine the hydroxyl value.
[0118] <Measurement of weight average molecular weight> The weight average molecular weight is measured as follows. The weight average molecular weight was measured by the following method: Gel permeation chromatography (GPC) Measurement device: GPC-8220GPC (Tosoh Corporation) Column: TSKgel Super HZM-H 15 cm triple column (Tosoh Corporation) Temperature: 40° C. Solvent: Tetrahydrofuran (THF) Flow rate: 0.35 mL / min Sample: 0.4 mL of 0.15% sample injected Sample pretreatment: The sample was dissolved in tetrahydrofuran (THF, containing stabilizer, Wako Pure Chemical Industries, Ltd.) at 0.15% and then filtered with a 0.2 μm filter, and the filtrate was used as the sample. 100 μL of tetrahydrofuran sample solution was injected and measured. In measuring the weight average molecular weight Mw of the crystalline polyester resin, the molecular weight distribution of the sample was calculated from the relationship between the logarithmic value and the count number of a calibration curve prepared using several types of monodisperse polystyrene standard samples. As standard polystyrene samples for preparing the calibration curve, Showdex STANDARD Std. Nos. S-7300, S-210, S-390, S-875, S-1980, S-10.9, S-629, S-3.0, S-0.580, and toluene manufactured by Showa Denko K.K. were used. The detector used was a refractive index (RI) detector.
[0119] <Synthesis example of crystalline polyester resin> 2,500 g of 1,12-decanediol, 2,330 g of 1,8-octanedioic acid, and 4.9 g of hydroquinone were placed in a 5-liter four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and reacted at 180°C for 20 hours, then heated to 200°C and reacted for 6 hours, and further reacted at 8.3 kPa for 10 hours to synthesize crystalline polyester resin (1). The resulting crystalline polyester resin (1) had a melting point of 64° C., a weight average molecular weight of 5720, and an acid value of 28 mgKOH / g.
[0120] (Example of wax dispersant synthesis) Into an autoclave reaction tank equipped with a thermometer and a stirrer, 600 parts of xylene and 300 parts of low molecular weight polyethylene (Sunwax LEL-400, softening point 128°C, manufactured by Sanyo Chemical Industries, Ltd.) were placed and thoroughly dissolved. After replacing with nitrogen, a mixed solution of 2,310 parts of styrene, 270 parts of acrylonitrile, 150 parts of butyl acrylate, 78 parts of di-t-butylperoxyhexahydroterephthalate, and 455 parts of xylene was added dropwise at 175°C over 3 hours to polymerize, and the mixture was maintained at this temperature for a further 30 minutes to synthesize wax dispersant (1).
[0121] (Example of synthesis of non-crystalline polyester (low molecular weight polyester) resin) -Production of amorphous polyester resin (1)- In a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 90 parts of bisphenol A ethylene oxide 2 mole adduct, 209 parts of bisphenol A propylene oxide 3 mole adduct, 208 parts of terephthalic acid, 46 parts of adipic acid, and 2 parts of dibutyltin oxide were charged and reacted for 12 hours at normal pressure and 230° C. Next, the reaction liquid was reacted for 5 hours under a reduced pressure of 10 to 15 mmHg, and then 25 parts of trimellitic anhydride was added to the reaction vessel and reacted for 2 hours at normal pressure and 180° C. to synthesize amorphous polyester (1). The resulting polyester resin had a hydroxyl value of 15 mgKOH / g, a weight average molecular weight [Mw] of 10,000, and an acid value of 5 mgKOH / g.
[0122] (Synthesis example of polyester prepolymer) Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 682 parts of ethylene oxide 2-mol adduct of bisphenol A, 81 parts of propylene oxide 2-mol adduct of bisphenol A, 283 parts of terephthalic acid, 22 parts of trimellitic anhydride, and 2 parts of dibutyltin oxide were placed and reacted under normal pressure at 230° C. for 8 hours. Further, the mixture was reacted for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to synthesize an intermediate polyester. Next, 410 parts of the synthesized intermediate polyester, 89 parts of isophorone diisocyanate, and 500 parts of ethyl acetate were placed in a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, and reacted at 100° C. for 5 hours to synthesize polyester prepolymer (1). The free isocyanate content of the resulting polyester prepolymer (1) was 1.53%.
[0123] (Surfactant synthesis example) ~Production of surfactant (1)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methyldecane (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added, and while introducing chlorine gas from the gas inlet tube, a liquid phase chlorination reaction was carried out at 100 to 120°C. 1684 parts of diphenyl ether (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 101 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and an alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product 1. The alkylation reaction product (1) was sulfonated for 60 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (1).
[0124] ~Production of surfactant (2)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methyldecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and a liquid phase chlorination reaction was carried out at 100 to 120°C while introducing chlorine gas from the gas inlet tube. 2595 parts of 1,4-diphenoxybenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 155 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was allowed to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product 2. The alkylation reaction product (2) was sulfonated for 60 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (2).
[0125] ~Production of surfactant (3)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methylnonane (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added, and a liquid phase chlorination reaction was carried out at 100 to 120°C while introducing chlorine gas from the gas inlet tube. 1850 parts of diphenyl ether (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 111 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (3). The alkylation reaction product 3 was sulfonated for 30 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (3).
[0126] ~Production of surfactant (4)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of undecane (manufactured by Tokyo Chemical Industry Co., Ltd.) were put in, and while introducing chlorine gas from the gas inlet tube, a liquid phase chlorination reaction was carried out at 100 to 120°C. 1684 parts of diphenyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were put into the chlorination product from which hydrogen chloride had been removed, and 101 parts of an alkylation catalyst with an AlCl3 content of 27% were also put in, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (4). The alkylation reaction product 4 was sulfonated for 30 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (4).
[0127] ~Production of surfactant (5)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of TRIDECANE, 7-METHYL- (manufactured by Dayang Chemicals Co., Ltd.) were added, and a liquid-phase chlorination reaction was carried out at 100 to 120°C while introducing chlorine gas from the gas inlet tube. 1327 parts of diphenyl ether (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 79 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (5). The alkylation reaction product 5 was sulfonated for 30 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (5).
[0128] ~Production of surfactant (6)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methyldecane (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added, and while introducing chlorine gas from the gas inlet tube, a liquid phase chlorination reaction was carried out at 100 to 120°C. 1684 parts of diphenyl ether (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 101 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and an alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (6). The alkylation reaction product 6 was sulfonated for 30 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (6).
[0129] ~Production of surfactant (7)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methyldecane (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and a liquid-phase chlorination reaction was carried out at 100 to 120°C while introducing chlorine gas from the gas inlet tube. 773 parts of benzene (manufactured by Tokyo Chemical Industry Co., Ltd.) was added to the chlorination product from which hydrogen chloride had been removed, and 46 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (7). The alkylation reaction product 7 was sulfonated for 30 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (7).
[0130] ~Production of surfactant (8)~ In a reaction vessel equipped with a cooling tube, a stirrer, and a gas inlet tube, 1000 parts of 2-methyldecane (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added, and a liquid phase chlorination reaction was carried out at 100 to 120°C while introducing chlorine gas from the gas inlet tube. 1684 parts of diphenyl ether (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added to the chlorination product from which hydrogen chloride had been removed, and 101 parts of an alkylation catalyst with an AlCl3 content of 27% were added, and the alkylation reaction was carried out at 100°C for about 60 minutes. The alkylation reaction product was left to stand, the catalyst was separated, and unreacted components were removed by distillation to obtain an alkylation reaction product (8). The alkylation reaction product 8 was sulfonated for 70 minutes using fuming sulfuric acid, and neutralized with NaOH to obtain a surfactant (8).
[0131] The number of hydrophilic functional groups, the proportion of those with one hydrophilic functional group, the number of carbon atoms in the long-chain hydrocarbon group, the structure of the long-chain hydrocarbon group, and the surfactant type of surfactants (1) to (8) are shown in Table 1 below.
[0132] [Table 1]
[0133] Example 1 <Toner Production> -Preparation of pigment and wax dispersion- In a container equipped with a stirring rod and a thermometer, 723 parts of the synthesized amorphous polyester resin (1), 110 parts of carnauba wax (WA-05 manufactured by Cerarica Noda Co., Ltd.), 77 parts of the synthesized wax dispersant (1) (content of wax dispersant relative to wax: 70%), 22 parts of a charge control agent (CCA, salicylic acid metal complex E-84 manufactured by Orient Chemical Industry Co., Ltd.), and 947 parts of ethyl acetate were charged, heated to 80°C with stirring, and maintained at 80°C for 5 hours, and then cooled to 30°C in 1 hour. Next, 155 parts of carbon black (Printex35, manufactured by Dexa) and 500 parts of ethyl acetate were charged into the vessel and mixed for 1 hour to obtain a raw material solution. 1,324 parts of the obtained raw material solution were transferred to a container, and the carbon black and wax were dispersed using a bead mill (Ultra Visco Mill, manufactured by Imex) under the following conditions: liquid delivery rate 1 kg / hr, disk peripheral speed 6 m / sec, 80 volume % filling of 0.5 mm zirconia beads, and 3 passes. Next, 1,042.3 parts of a 65% ethyl acetate solution of the non-crystalline polyester resin (1) synthesized above was added, and the mixture was passed once through the bead mill under the above conditions to obtain a pigment-wax dispersion (1). The solids concentration of the resulting pigment-wax dispersion was 50%.
[0134] - Preparation of amorphous polyester resin solution (1) - A 2 L metal container was charged with 100 parts of amorphous polyester resin (1) and 400 parts of ethyl acetate, and the mixture was heated to 40° C. to dissolve it. The mixture was then cooled in an ice-water bath to prepare an amorphous polyester resin solution (1).
[0135] - Preparation of oil phase - 664 parts of the pigment-wax dispersion liquid prepared above (wax content in the toner: 4%), 73 parts of the synthesized polyester prepolymer (1), 150 parts of the prepared amorphous polyester resin solution (1), and 7.8 parts of 5-amino-1,3,3-trimethylcyclohexanemethylamine (Sigma-Aldrich Japan Co., Ltd.) were placed in a container and mixed at 5,000 rpm for 1 minute using a TK Homomixer (Tokushu Kika Kogyo Co., Ltd.) to obtain an oil phase.
[0136] -Synthesis of organic fine particle emulsion- In a reaction vessel equipped with a stirring bar and a thermometer, 683 parts of water, 11 parts of sodium salt of methacrylic acid ethylene oxide adduct sulfate (Eleminol RS-30, manufactured by Sanyo Chemical Industries, Ltd.), 138 parts of styrene, 138 parts of methacrylic acid, and 1 part of ammonium persulfate were charged and stirred at 400 rpm for 15 minutes, producing a white emulsion. The obtained emulsion was heated to raise the temperature in the system to 75° C., and reacted for 5 hours. Further, 30 parts of 1% ammonium persulfate aqueous solution was added, and the mixture was aged at 75° C. for 5 hours to obtain a fine particle dispersion (1) of an aqueous dispersion of a vinyl resin (a copolymer of styrene-methacrylic acid-methacrylic acid ethylene oxide adduct sulfate sodium salt). The proportion of resin fine particles in the fine particle dispersion (1) was 20%.
[0137] - Preparation of aqueous phase - 884.0 parts of water, 16.0 parts of the fine particle dispersion (1), 210.0 parts of the surfactant (1), and 90.0 parts of ethyl acetate were mixed to obtain a milky white liquid, which was designated as the aqueous phase.
[0138] - Emulsification and desolvation - Next, 800 parts of the prepared oil phase and 1,200 parts of the prepared aqueous phase were placed in a container and mixed at 13,000 rpm for 20 minutes using a TK homomixer to obtain an emulsified slurry. 2,050 parts of the obtained emulsified slurry was mixed with 410 parts of ion-exchanged water and placed in a container equipped with a stirrer and a thermometer. The solvent was removed at 30°C for 8 hours, and then the mixture was aged at 45°C for 4 hours to obtain a dispersed slurry.
[0139] -Washing and drying- 100 parts of the obtained dispersion slurry was filtered under reduced pressure, and then 100 parts of ion-exchanged water was added to the filter cake, and the mixture was mixed at 12,000 rpm for 10 minutes using a TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.), and then filtered. Next, 100 parts of a 10% aqueous sodium hydroxide solution was added, and the mixture was mixed at 12,000 rpm for 30 minutes using a TK homomixer, and then filtered under reduced pressure. Next, 100 parts of 10% hydrochloric acid was added, and the mixture was mixed at 12,000 rpm for 10 minutes using a TK homomixer, and then filtered. Next, 300 parts of ion-exchanged water was added, and the mixture was mixed for 10 minutes at 12,000 rpm using a TK homomixer, and then filtered twice to obtain a filter cake. The obtained filter cake was dried in a circulating air dryer at 45° C. for 48 hours and sieved through a 75 μm mesh to prepare toner base particles 1 of Example 1.
[0140] Example 2 <Toner Production> Toner base particles 2 of Example 2 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (2).
[0141] Example 3 <Toner Production> Toner base particles 3 of Example 3 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (3).
[0142] Example 4 <Toner Production> Toner base particles 4 of Example 4 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (4).
[0143] Example 5 <Toner Production> Toner base particles 5 of Example 5 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (5).
[0144] Example 6 <Toner Production> Toner base particles 6 of Example 6 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with Glycerol α-Monomyristate (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0145] Example 7 -Preparation of pigment and wax dispersion- The same procedure as in Example 1 was carried out to obtain a pigment-wax dispersion.
[0146] -Creating a solution of amorphous polyester resin (1)- The same procedure as in Example 1 was carried out to prepare a non-crystalline polyester resin solution.
[0147] - Preparation of oil phase - 664 parts of the pigment-wax dispersion prepared above (wax content in the toner: 4%) and 223 parts of the amorphous polyester resin solution prepared above were placed in a container and mixed at 5,000 rpm for 1 minute using a TK Homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) to form the oil phase.
[0148] - Preparation of aqueous phase - 884.0 parts of water, 16.0 parts of the fine particle dispersion (1), 210.0 parts of the surfactant (6), and 90.0 parts of ethyl acetate were mixed to obtain a milky white liquid, which was designated as the aqueous phase.
[0149] - Emulsification and desolvation - The same procedure as in Example 1 was carried out to obtain a dispersed slurry.
[0150] -Washing and drying- The same procedure as in Example 1 was carried out to prepare toner base particles 7 of Example 7.
[0151] Example 8 <Toner Production> Toner base particles 8 of Example 8 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (6).
[0152] Comparative Example 1 <Toner Production> Toner base particles 9 of Comparative Example 1 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (7).
[0153] Comparative Example 2 <Toner Production> Toner base particles 10 of Comparative Example 2 were prepared in the same manner as in Example 1, except that the surfactant (1) in Example 1 was replaced with the surfactant (8).
[0154] -Analysis of residual surfactant on toner surface- <Extraction of residual surfactant from toner surface> 10 ml of methanol was added to 0.1 g of the obtained toner base particles, and ultrasonic irradiation was performed for 30 minutes. The dispersion liquid after ultrasonic irradiation was filtered through a filter with an opening of 2 μm to obtain a surfactant extract.
[0155] <Analysis of residual surfactant in toner> The obtained surfactant extract was analyzed under the following conditions. Measurement device: LCMS-8030 (liquid chromatograph mass spectrometer: manufactured by Shimadzu Corporation) Column: InertSustainSwift (GL Sciences, Inc.) Mobile phase: ammonium acetate aqueous solution / methanol = 80 / 20, methanol (gradient elution) Flow rate: 0.3ml / min Injection volume: 0.2μl From each peak detected in the sample, the number of hydrophilic functional groups in each surfactant component, the proportion of those with one hydrophilic functional group, the carbon number of the long-chain hydrocarbon group, the structure of the long-chain hydrocarbon group, the surfactant type, and the mass proportion of each surfactant component were determined. The analytical results are shown in Table 2 together with the toner evaluation results.
[0156] -External additive treatment- 100 parts of the toner base particles 1 to 14 obtained in Examples 1 to 8 and Comparative Examples 1 to 2 were mixed with 0.7 parts of hydrophobic silica (HDKH2000, manufactured by Clariant Japan) and 0.3 parts of hydrophobic titanium oxide as external additives using a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.), and the mixture was subjected to an external addition treatment to prepare a toner.
[0157] Table 1 shows the production conditions and the analytical results of the surfactants in the above Examples 1 to 8 and Comparative Examples 1 and 2.
[0158] (Evaluation items) <Toner scattering resistance> A chart with an image area ratio of 20% was printed on 80,000 sheets continuously using a commercially available digital full-color printer (imagio MPC6000, A4 landscape color 50 sheets / min, Ricoh Co., Ltd.). The degree of toner contamination inside the printer was visually evaluated on a four-point scale according to the following criteria. "△" or better is usable.
[0159] [Evaluation Criteria] ◎: No toner stains were observed and the condition was good. ○: Slight staining is observed, but not problematic. △: Only a small amount of dirt is observed ×: Outside the acceptable range, very dirty and problematic
[0160] (Heat-resistant storage stability) The toner was stored at 50° C. for 8 hours, and then sieved through a 42 mesh sieve for 2 minutes, and the remaining rate on the wire mesh was used as an index of heat resistance storage stability. The heat resistance was evaluated according to the following three criteria. ◎: Less than 5% (no problem at all) ○: 5% or more and less than 20% (slightly poor preservability, but no practical problems) △: 20% or more but less than 30% (slightly poor preservability, but still acceptable for practical use) ×: 30% or more (level of practical problems)
[0161] <Transferability> Using an image forming apparatus MF2800 (manufactured by Ricoh Co., Ltd.), a 15 cm x 15 cm black solid image with an average image density of 1.38 or more measured with a Macbeth reflection densitometer was formed on a piece of recyclable paper 100. The transfer rate was calculated by the following formula (1). Transfer rate [%] = (amount of toner transferred onto recording paper / amount of toner developed onto photoconductor) × 100 (Equation (1)) The criteria for judging the transferability are as follows. ◎: Transferability is 97% or more (no problem at all) ○: Transfer rate is 95% or more but less than 97% (transferability is slightly poor, but not problematic for practical use) △: Transfer rate is 80% or more but less than 95% (slightly poor transferability, but still within the acceptable range for practical use) ×: Transfer rate is less than 80%, which is problematic for practical use.
[0162] <Cleaning ability> Using a digital full-color copier, imagioColor2800 (manufactured by Ricoh Co., Ltd.), the residual toner remaining on the photoconductor that had passed through the cleaning process was transferred onto a blank sheet of paper using Scotch tape (manufactured by Sumitomo 3M Co., Ltd.), which was then measured with a Macbeth reflection densitometer, RD514 model, and the difference from the blank was used as an index of cleaning performance. The criteria for cleaning performance are as follows: ◎: The difference with the blank is 0.00, which is a level that is not problematic at all. ◯: The difference from the blank is 0.01 or less, but some streaks are observed. Cleaning is slightly poor, but at a level that does not cause any problems in practical use. △: The difference from the blank is 0.02 or less, and the cleaning ability is slightly poor, but is at a level that is practically acceptable. ×: The difference from the blank exceeds 0.02. This is at a level that is problematic for practical use.
[0163] As is clear from the evaluation results in Table 2 below, the toners of Examples 1 to 8 have sufficiently excellent toner scattering properties, heat-resistant storage stability, transferability, and cleanability. In contrast, the toners of Comparative Examples 1 and 2 have practical problems in any of the toner scattering properties, heat-resistant storage stability, transferability, and cleanability.
[0164] [Table 2]
[0165] For example, aspects of the present invention are as follows. (1) A toner for developing electrostatic latent images, characterized in that, of the surfactants contained on the toner surface, more than 60% by mass is a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups, and the surfactant having a long-chain hydrocarbon group and one hydrophilic functional group is not more than 40% by mass. (2) The toner for developing electrostatic latent images according to the above (1), wherein the long-chain hydrocarbon group has 11 or more carbon atoms. (3) The toner for developing an electrostatic latent image according to the above (1) or (2), wherein the long chain hydrocarbon group has a branched chain structure. (4) The toner for developing electrostatic latent images according to any one of the above (1) to (3), wherein the surfactant is an anionic surfactant. (5) A toner storage unit containing the toner according to any one of (1) to (4) above. (6) A method for producing the toner according to any one of (1) to (4) above, comprising the steps of: The method comprises the steps of: preparing a toner material liquid (oil phase) by dissolving or dispersing toner materials including at least a binder resin and / or a binder resin precursor and a release agent in an organic solvent; and emulsifying or dispersing the oil phase in an aqueous medium (aqueous phase), and then removing the solvent to form base particles; A method for producing a toner, wherein the aqueous medium contains a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups. (7) forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; A fixing step of fixing the transferred image on the recording medium, An image forming method, comprising using the toner according to any one of (1) to (4) above as the toner. (8) An electrostatic latent image carrier, a charging means for charging the surface of the electrostatic latent image carrier, an exposure means for exposing the charged surface of the electrostatic latent image carrier to light to form an electrostatic latent image, a developing means for developing the electrostatic latent image with a toner to form a visible image, a transfer means for transferring the visible image to a recording medium, and a fixing means for fixing the transferred image transferred to the recording medium, 13. An image forming apparatus, comprising the toner according to claim 12, wherein the toner is a toner having a molecular weight of 100 or more. [Explanation of symbols]
[0166] 1 Photoconductor (image carrier) 2 Charger 3. Developing Machine 4. Toner 5 Developing sleeve 6 Transfer conveyor belt 6a Bias roller 7 Cleaning Blade 8 Recovery spring 9 Recovery coil 10 Photoconductor and cleaning unit 13 Conveying screw 14 paddle (stirring mechanism) 16 Reflection density detection sensor 17 Toner density sensor 18 Registration roller 20 Static eliminator γ Image light S Transfer Paper [Prior art documents] [Patent documents]
[0167] [Patent Document 1] Japanese Patent Application Publication No. 7-152202 [Patent Document 2] JP 2006-91081 A [Patent Document 3] JP 2016-224107 A [Patent Document 4] JP 2011-075704 A
Claims
1. of surfactants contained on the toner surface, more than 60% by mass and not more than 80% by mass is a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups, and 20% by mass or more and not more than 40% by mass is a surfactant having a long-chain hydrocarbon group and one hydrophilic functional group, The long chain hydrocarbon group has 11 or more carbon atoms.
2. A toner for developing electrostatic latent images.
2. 2. The toner for developing an electrostatic latent image according to claim 1, wherein the long chain hydrocarbon group has a branched chain structure.
3. 3. The toner for developing an electrostatic latent image according to claim 1, wherein the surfactant is an anionic surfactant.
4. A toner storage unit containing the toner according to any one of claims 1 to 3.
5. A method for producing the toner according to any one of claims 1 to 3, comprising the steps of: The method comprises the steps of: preparing a toner material liquid (oil phase) by dissolving or dispersing toner materials including at least a binder resin and / or a binder resin precursor and a release agent in an organic solvent; and emulsifying or dispersing the oil phase in an aqueous medium (aqueous phase), and then removing the solvent to form base particles; The method for producing a toner, wherein the aqueous medium contains a surfactant having a long-chain hydrocarbon group and two or more hydrophilic functional groups.
6. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; A fixing step of fixing the transferred image on the recording medium, An image forming method, comprising the step of: using the toner according to claim 1 as the toner.
7. the electrostatic latent image carrier; charging means for charging the surface of the electrostatic latent image carrier; exposure means for exposing the charged surface of the electrostatic latent image carrier to light to form an electrostatic latent image; developing means for developing the electrostatic latent image with a toner to form a visible image; transfer means for transferring the visible image to a recording medium; and fixing means for fixing the transferred image transferred to the recording medium; 4. An image forming apparatus, comprising the toner according to claim 1.
Citation Information
Patent Citations
Electrostatic charge developing toner, its production and developer
JP1995152202A
Electrostatic charge image developing toner and method for manufacturing electrostatic charge image developing toner
JP2005017829A
Electrophotographic toner
JP2005099120A
Toner and its manufacturing method, and image forming method