Manufacturing method of aluminum alloy molded product, and manufacturing method of joined product using aluminum alloy molded product
A two-step anodization process using controlled electrolytic solutions forms oxide films on aluminum alloys, enhancing bonding strength and corrosion resistance, addressing industrial bonding challenges.
Patent Information
- Application Number
- JP2019203521
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-08
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2039-11-08
AI Technical Summary
Existing methods for bonding aluminum alloy materials with resins result in insufficient bonding strength and corrosion resistance, particularly when using electrolytic solutions with high concentrations and pH fluctuations, making them unsuitable for industrial applications.
A two-step anodization process using an electrolytic solution with 0.5 to 7 mol/L phosphoric acid and less than 0.5 mol/L sulfuric acid to form first and second oxide films on the aluminum alloy, with specific thicknesses, pore orientations, and pore diameters, followed by adhering a resin after a certain period.
The method produces aluminum alloy molded products with high bonding strength and excellent corrosion resistance, ensuring stable bonding even after prolonged periods, suitable for industrial use.
Smart Images

Figure 0007590714000002 
Figure 0007590714000003 
Figure 0007590714000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing an aluminum alloy formed product having an aluminum alloy base material whose surface is covered with an oxide film, and also to a method for producing a joint between the aluminum alloy formed product and resin. [Background technology]
[0002] Among alloy materials, aluminum alloys have a relatively high specific strength. In addition, aluminum alloys have excellent heat dissipation properties. For this reason, aluminum alloy molded products are widely used in the fields of transportation equipment such as automobiles and motorcycles, electronic equipment, building materials, leisure goods such as bicycles and fishing tackle, and daily necessities.
[0003] In recent years, there has been an increasing demand for bonded products formed by bonding an aluminum alloy substrate to a resin. Examples of such bonded products include bonded products in which an aluminum alloy molded product is bonded to another member via a resin adhesive, and bonded products in which an aluminum alloy molded product is bonded directly to a resin member. However, such bonded products formed by bonding different materials may have insufficient bonding strength.
[0004] Conventionally, a method for anodizing an aluminum alloy substrate using an aqueous phosphoric acid solution as an electrolyte has been known as a method for improving the bonding strength between an aluminum alloy molded product and a resin. However, this method has been problematic in industrial use because it is difficult to stably produce a bonded product with high bonding strength.
[0005] Patent Document 1 describes that a first oxide film is formed by anodizing an aluminum alloy substrate using an acidic electrolyte containing phosphoric acid and sulfuric acid, and then a second oxide film is formed by anodizing the substrate using an alkaline electrolyte in which phosphate is dissolved, and then a resin is bonded to the surface of the oxide film, thereby improving the bonding strength and corrosion resistance. However, the bonding strength and corrosion resistance of the bonded product are still insufficient in some cases. In addition, the electrolyte used to form the first oxide film is difficult to control because of its high concentration, and the electrolyte used to form the second oxide film is prone to pH fluctuations due to absorption of carbon dioxide in the air, which has been a problem in industrial use. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2015-89964 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made to solve the above problems, and aims to provide a method for producing an aluminum alloy molded product which can stably obtain high bonding strength when bonded to a resin and has excellent corrosion resistance, and a method for producing a bonded product by bonding the thus obtained aluminum alloy molded product to a resin. [Means for solving the problem]
[0008] The above-mentioned problem is solved by providing a method for producing an aluminum alloy formed product, which comprises anodizing an aluminum alloy substrate using an electrolytic solution containing 0.5 to 7 mol / L of phosphoric acid and less than 0.5 mol / L of sulfuric acid to form a first oxide film, and then anodizing the substrate using an electrolytic solution containing 0.5 to 5 mol / L of sulfuric acid to form a second oxide film.
[0009] In this case, it is preferable to form a first oxide film on the surface of the aluminum alloy base material, and then form a second oxide film between the aluminum alloy base material and the first oxide film. It is also preferable that the temperature of the electrolytic solution used to form the first and second oxide films is 0 to 50° C. 1 is 0.1 to 5 μm, and the thickness of the second oxide film T 2 It is also preferable that the first and second oxide films have pores oriented in the thickness direction, and the average pore diameter D of the first oxide film is 1 to 25 μm. 1 is the average pore diameter D of the second oxide film 2 It is also preferable that the .gamma.
[0010] The above problem can also be solved by providing a method for producing a bonded article, in which a resin is bonded to the first or second oxide film on the surface of the aluminum alloy molded article obtained by the above production method.
[0011] In this case, it is preferable to adhere the resin to the first or second oxide film three or more days after the second oxide film is formed on the aluminum alloy substrate.
[0012] The above problem is solved by an aluminum alloy formed product having an aluminum alloy substrate having a surface covered with an oxide film, the surface of the aluminum alloy substrate being covered with a second oxide film, the surface of the second oxide film being covered with a first oxide film, and the first oxide film having a thickness T 1 is 0.1 to 5 μm, and the thickness of the second oxide film T 2 The first and second oxide films have pores oriented in the thickness direction, and the average pore diameter D of the first oxide film is 1 to 25 μm. 1 is the average pore diameter D of the second oxide film 2 The above-mentioned problems are also solved by providing an aluminum alloy molded product having a size larger than 100 mm.
[0013] A bonded article obtained by bonding a resin to the first or second oxide film on the surface of the aluminum alloy molded article is a preferred embodiment of the molded article. Effect of the Invention
[0014] The aluminum alloy molded product obtained by the manufacturing method of the present invention and the resin joint have high joint strength. Moreover, since the aluminum alloy molded product has excellent corrosion resistance, a stable high joint strength can be obtained even when the aluminum alloy molded product is joined to the resin long after the manufacturing process. [Brief description of the drawings]
[0015] [Figure 1] FIG. 4 is a schematic diagram of a method for evaluating the bonding strength of a bonded article in the examples. [Diagram 2] 1 is an electron microscope photograph of a cross section of an aluminum alloy molded product in Example 1. [Diagram 3] 1 is an enlarged electron microscope photograph of a cross section of an aluminum alloy molded product in Example 1. [Figure 4] 1 is an electron microscope photograph of the surface of an aluminum alloy molded product in Example 1. [Diagram 5] 2 is an electron microscope photograph of the surface of an aluminum alloy molded product in Comparative Example 1. [Figure 6] 4 is an electron microscope photograph of the surface of an aluminum alloy molded product in Comparative Example 3. [Figure 7] 2 shows polarization curves obtained by electrochemical measurement of aluminum alloy molded articles in Examples 1 and 2 and Comparative Examples 1 to 3 and 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention provides a method for producing an aluminum alloy formed product, comprising anodizing an aluminum alloy substrate using an electrolytic solution containing 0.5 to 7 mol / L of phosphoric acid and less than 0.5 mol / L of sulfuric acid to form a first oxide film, and then anodizing the substrate using an electrolytic solution containing 0.5 to 5 mol / L of sulfuric acid to form a second oxide film.
[0017] The aluminum alloy substrate to be anodized is not particularly limited. The aluminum element content in the substrate is usually 50 mass% or more, preferably 75 mass% or more. The total content of elements other than aluminum in the substrate is usually 50 mass% or less, preferably 25 mass% or less. Such elements include magnesium, zinc, manganese, copper, nickel, silicon, iron, titanium, lead, tin, and chromium.
[0018] Examples of aluminum alloys that can be used as the material for the aluminum alloy substrate include wrought alloys, casting alloys, die-casting alloys, etc. Among these, wrought alloys and die-casting alloys are preferred.
[0019] Examples of wrought alloys include Al-Mg-based aluminum alloys, pure aluminum-based aluminum alloys, Al-Cu-based aluminum alloys, Al-Mn-based aluminum alloys, Al-Si-based aluminum alloys, Al-Mg-Si-based aluminum alloys, and Al-Zn-Mg-based aluminum alloys, among which Al-Mg-based aluminum alloys and pure aluminum-based aluminum alloys are preferred. Examples of Al-Mg-based aluminum alloys include A5052 as specified by the JIS standard, and examples of pure aluminum-based aluminum alloys include A1100 and A1050 as specified by the JIS standard.
[0020] Examples of the alloy for casting include Al-Mg-based aluminum alloys, Al-Mg-Zn-based aluminum alloys, Al-Cu-Mg-based aluminum alloys, Al-Si-Cu-based aluminum alloys, Al-Si-based aluminum alloys, and Al-Si-Mg-based aluminum alloys, among which Al-Mg-based aluminum alloys and Al-Mg-Zn-based aluminum alloys are preferred. Examples of the Al-Mg-based aluminum alloys include AC7A and the like defined by the JIS standard, examples of the Al-Cu-Mg-based aluminum alloys include AC1B and the like defined by the JIS standard, examples of the Al-Si-Cu-based aluminum alloys include AC2A and the like defined by the JIS standard, and examples of the Al-Si-Mg-based aluminum alloys include AC4CH and the like.
[0021] Examples of alloys for die casting include Al-Si based aluminum alloys such as ADC12 defined by the JIS standard, and Al-Si-Cu based aluminum alloys.
[0022] The aluminum alloy substrate is obtained by forming an aluminum alloy material. The forming method of the aluminum alloy is not particularly limited. A general forming method such as a stretching method such as pressing, forging, extrusion, rolling, etc., a casting method such as gravity casting, die casting, etc., or a cutting process can be appropriately selected. In addition, the aluminum alloy may be subjected to various tempering treatments such as a solution treatment and an aging treatment.
[0023] The aluminum alloy substrate thus obtained is anodized to form a first oxide film, which improves the bonding strength between the aluminum alloy substrate and the resin.
[0024] After forming the aluminum alloy, it is preferable to carry out pretreatment such as degreasing, removal of oxide film, removal of smut, and polishing, and then subject the aluminum alloy to anodization.
[0025] For the formation of the first oxide film, an electrolyte containing 0.5 to 7 mol / L of phosphoric acid and less than 0.5 mol / L of sulfuric acid is used. When the content of phosphoric acid in the electrolyte is within such a range, the bonding strength between the aluminum alloy substrate and the resin is improved. The content of phosphoric acid is preferably 0.8 mol / L or more, more preferably 1.2 mol / L or more, even more preferably 1.6 mol / L or more, particularly preferably 2 mol / L or more, and most preferably 2.4 mol / L or more. On the other hand, the content of phosphoric acid is preferably 6 mol / L or less, more preferably 5 mol / L or less, even more preferably 4 mol / L or less, particularly preferably 3.5 mol / L or less, and most preferably 3.2 mol / L or less. When the electrolyte contains polyphosphoric acid obtained by condensation of phosphoric acid, it contains phosphoric acid in the number of phosphate radicals obtained by hydrolysis of the polyphosphoric acid.
[0026] The content of sulfuric acid in the electrolytic solution used to form the first oxide film must be less than 0.5 mol / L. This allows the first oxide film to have excellent bonding strength with the resin. The content is preferably less than 0.3 mol / L, more preferably less than 0.1 mol / L, even more preferably less than 0.01 mol / L, and particularly preferably substantially none.
[0027] The pH of the electrolytic solution used to form the first oxide film is preferably 0 to 4. By setting the pH of the electrolytic solution in this range, the bonding strength between the aluminum alloy substrate and the resin is further improved. The pH is more preferably 0.1 or more, even more preferably 0.2 or more, particularly preferably 0.3 or more, and most preferably 0.4 or more. On the other hand, the pH is more preferably 3 or less, even more preferably 2 or less, particularly preferably 1.7 or less, and most preferably 1.5 or less. From the viewpoint of obtaining an aluminum alloy molded product with extremely high bonding strength, the pH is preferably 1.2 or less, more preferably 0.9 or less, and even more preferably 0.85 or less.
[0028] The aluminum alloy substrate is immersed in the electrolytic solution and then anodized. The bath temperature at this time is preferably 0 to 50°C. By keeping the bath temperature within this range, the bonding strength is further improved. The bath temperature is more preferably 5°C or higher, further preferably 10°C or higher, and particularly preferably 15°C or higher. On the other hand, the bath temperature is more preferably 40°C or lower, further preferably 35°C or lower, and particularly preferably 30°C or lower.
[0029] The electrolysis time when forming the first oxide film is usually 0.1 to 60 minutes. The electrolysis time is preferably 1 minute or more, and more preferably 5 minutes or more. On the other hand, the electrolysis time is preferably 45 minutes or less, and more preferably 30 minutes or less. The voltage applied during anodization is preferably 5 to 50 V. The voltage is more preferably 10 V or more. On the other hand, the voltage is more preferably 40 V or less, and even more preferably 30 V or less.
[0030] After the first oxide film is formed, the second oxide film is formed. To form the second oxide film, an electrolytic solution containing 0.5 to 5 mol / L of sulfuric acid is used. By forming the second oxide film using such an electrolytic solution, the corrosion resistance of the aluminum alloy molded product is improved.
[0031] Conventionally, a method of anodizing an aluminum alloy substrate using an aqueous phosphoric acid solution as an electrolytic solution has been known as a method for improving the bonding strength between an aluminum alloy molded product and a resin. However, this method is difficult to stably manufacture a bonded product with high bonding strength, which has been a problem in industrial use. In addition, according to a method in which an aluminum alloy substrate is anodized using an acidic electrolytic solution containing phosphoric acid and sulfuric acid to form a first oxide film, the substrate is anodized using an alkaline electrolytic solution in which phosphate is dissolved to form a second oxide film, and then a resin is bonded to the surface of the oxide film, the bonding strength and corrosion resistance are improved, but are still not sufficient. Furthermore, the electrolytic solution used to form the first oxide film is difficult to control because of its high concentration, and the electrolytic solution used to form the second oxide film is prone to pH fluctuations due to absorption of carbon dioxide in the air, which has been a problem in industrial use.
[0032] In order to solve these problems, the present inventors have conducted extensive research and found that the extremely low corrosion resistance of the anodized film formed using an aqueous phosphoric acid solution is the reason why a bonded product with high bonding strength cannot be stably obtained. The inventors have found that an aluminum alloy molded product having both excellent bonding strength and corrosion resistance can be obtained by forming a first oxide film using an electrolyte containing a predetermined amount of phosphoric acid and a small amount of sulfuric acid, and then forming a second oxide film using an electrolyte containing sulfuric acid. Moreover, each electrolyte used is easy to handle and suitable for industrial applications. The reason why both bonding strength and corrosion resistance are achieved is not clear, but one of the reasons is thought to be that by using two types of electrolytes in combination, a second oxide film with good corrosion resistance is formed relatively thick between the first oxide film with high bonding strength and the aluminum alloy substrate. It is thought that the improved corrosion resistance leads to a stable high bonding strength.
[0033] The content of sulfuric acid in the electrolytic solution used for forming the second oxide film is 0.5 to 5 mol / L, thereby improving the corrosion resistance of the aluminum alloy molded product. The content is preferably 1 mol / L or more, more preferably 1.5 mol / L or more, even more preferably 2 mol / L or more, particularly preferably 2.5 mol / L or more, and most preferably 3 mol / L or more. On the other hand, the content is preferably 4.5 mol / L or less, more preferably 4 mol / L or less.
[0034] In order to further improve corrosion resistance, the content of phosphate radicals in the electrolytic solution used to form the second oxide film is preferably less than 0.5 mol / L, more preferably less than 0.1 mol / L, even more preferably less than 0.01 mol / L, and particularly preferably substantially none.
[0035] From the viewpoint of further improving the corrosion resistance of the aluminum alloy molded product, the pH of the electrolytic solution used for forming the second oxide film is preferably less than 4. The pH is more preferably less than 3, even more preferably less than 2, particularly preferably less than 1, and most preferably less than 0.
[0036] The aluminum alloy substrate on which the first oxide film has been formed is immersed in the electrolytic solution, and then anodization is performed. The bath temperature at this time is preferably 0 to 50°C. By performing electrolysis at a relatively low temperature in this manner to form the second oxide film, the corrosion resistance is further improved. The bath temperature is more preferably 45°C or less, even more preferably 40°C or less, particularly preferably 35°C or less, and most preferably 30°C or less. On the other hand, if the bath temperature is less than 0°C, the second oxide film may not be sufficiently formed. The bath temperature is more preferably 10°C or more, and even more preferably 15°C or more.
[0037] The electrolysis time when forming the second oxide film is usually 0.1 to 60 minutes. The electrolysis time is preferably 1 minute or more, more preferably 5 minutes or more, even more preferably 10 minutes or more, particularly preferably 15 minutes or more, and most preferably 20 minutes or more. On the other hand, the electrolysis time is preferably 45 minutes or less. The voltage applied during anodization is preferably 3 to 20 V. Since the pore diameter of the pores in the first oxide film on the surface of the second oxide film is relatively large, the second oxide film is efficiently formed by such a relatively low voltage. The voltage is more preferably 18 V or less, and even more preferably 15 V or less. On the other hand, the voltage is more preferably 5 V or more, and even more preferably 10 V or more. In addition, it is preferable that the voltage applied when forming the first oxide film is higher than the voltage applied when forming the second oxide film.
[0038] The aluminum alloy formed product thus obtained has a surface of the aluminum alloy substrate covered with a second oxide film, and the surface of the second oxide film covered with a first oxide film. The second oxide film is formed on the surface of the aluminum alloy substrate. That is, the second oxide film is formed between the aluminum alloy substrate and the first oxide film. This improves the corrosion resistance of the aluminum alloy formed product.
[0039] The first oxide film has pores oriented in the thickness direction. When a first oxide film having such pores is formed on an aluminum alloy molded product, the bonding strength between the molded product and resin is improved. It is also believed that the first oxide film having pores makes it easier to form a second oxide film during anodization. From the viewpoints of further improving the bonding strength and more efficiently forming the second oxide film, it is preferable that at least some of the pores penetrate perpendicularly to the surface of the aluminum alloy molded product.
[0040] Average pore diameter D of the pores in the first oxide film 1 is not particularly limited, but is preferably 20 to 200 nm. 1 If the average pore diameter D is less than 20 nm, the second oxide film may not be easily formed, and the adhesive strength may decrease. 1 is more preferably 30 nm or more, further preferably 35 nm or more, and particularly preferably 40 nm or more. 1 If the average pore diameter D exceeds 200 nm, the bonding strength may decrease. 1 The average pore size of the pores formed in each coating can be determined from an electron microscope photograph of the surface or cross section of the aluminum alloy molded product.
[0041] The thickness of the first oxide film, T 1 The thickness T is preferably 0.1 to 5 μm. 1 is more preferably 0.2 μm or more, further preferably 0.3 μm or more, and particularly preferably 0.4 μm or more. 1 The thickness of each coating can be determined from an electron microscope photograph of the cross section of the aluminum alloy molded product.
[0042] The second oxide film has pores oriented in the thickness direction. In order to further improve the bonding strength and corrosion resistance, the average pore diameter D 2 The average pore diameter D is preferably 2 to 100 nm. 2 is more preferably 5 nm or more, further preferably 10 nm or more, particularly preferably 15 nm or more, and most preferably 20 nm or more. 2 The average pore diameter D is more preferably 80 nm or less, further preferably 60 nm or less, particularly preferably 50 nm or less, and most preferably 45 nm or less. 2 is preferably 40 nm or less.
[0043] In order to further improve corrosion resistance, the thickness of the second oxide film T 2 The thickness T is preferably 1 to 25 μm. 2 is more preferably 2 μm or more, further preferably 3 μm or more, particularly preferably 4 μm or more, and most preferably 5 μm or more. 2 It is more preferably 20 μm or less, further preferably 15 μm or less, particularly preferably 12 μm or less, and most preferably 9 μm or less.
[0044] In the aluminum alloy formed product of the present invention, the average pore diameter D of the pores in the first oxide film 1 is the average pore diameter D of the second oxide film 2 It is preferable that the average pore diameter D of the second oxide film is larger than 100 mm. This is believed to facilitate the formation of the second oxide film by anodizing, and to further improve the bonding strength and corrosion resistance. 2 Average pore size D of the first oxide film 1 Ratio of (D 1 / D 2 ) is more preferably 1.1 or more, further preferably 1.2 or more, and particularly preferably 1.5 or more.
[0045] In order to further improve corrosion resistance, it is also preferable that the second oxide film is thicker than the first oxide film. 1 Thickness of the second oxide film T 2 The ratio (T2 / T 1 ) is more preferably 1.2 or more, even more preferably 1.5 or more, particularly preferably 2 or more, and most preferably 5 or more.
[0046] In the aluminum alloy formed product of the present invention, the corrosion potential (natural potential) of the portion on which the first and second oxide films are formed is preferably not less than −0.55 V, more preferably not less than −0.52 V, and even more preferably not less than −0.50 V. The corrosion potential is determined from an anodic polarization curve obtained by electrochemically measuring the portion on which the first and second oxide films are formed, and specifically, is determined by the method described in the examples below.
[0047] An aluminum alloy formed product comprising an aluminum alloy substrate having a surface covered with an oxide film, the surface of the aluminum alloy substrate being covered with a second oxide film, the surface of the second oxide film being covered with a first oxide film, the first oxide film having a thickness of 0.1 to 5 μm, the second oxide film having a thickness of 1 to 25 μm, the first and second oxide films having pores oriented in the thickness direction, and an average pore diameter D of the first oxide film. 1 is the average pore diameter D of the second oxide film 2 Aluminium alloy mouldings larger than 100 mm are preferred embodiments of the present invention.
[0048] A method for producing a bonded article in which a resin is bonded to the surface of the first oxide film or the second oxide film on the surface of the aluminum alloy molded article thus obtained is also a preferred embodiment of the present invention. The bonded article produced by this method is one in which a resin is directly bonded to the surface of the first oxide film or the second oxide film formed on the aluminum alloy molded article. Examples of such bonded articles include a bonded article in which an aluminum alloy molded article and another member are bonded via a resin adhesive, and a bonded article in which a member made of resin is directly bonded to an aluminum alloy molded article.
[0049] In the manufacturing method of the joined product, it is preferable to bond the resin to the first or second oxide film 3 days or more after the second oxide film is formed on the aluminum alloy base material. As described above, the aluminum alloy formed product of the present invention has excellent corrosion resistance. Therefore, even when it is bonded to a resin a long time after production, high bonding strength is obtained, and it is easy to use industrially. It is more preferable to bond the resin to the first or second oxide film 5 days or more after the second oxide film is formed on the aluminum alloy base material, and even more preferably 7 days or more after the formation of the second oxide film on the aluminum alloy base material.
[0050] The resin to be bonded to the aluminum alloy molded product is not particularly limited, and may be appropriately selected depending on the application of the joined product, etc. For example, epoxy resin, polyurethane, polyamide such as nylon 6 and nylon 66, polyester such as polyethylene terephthalate and polybutylene terephthalate, polyolefin such as polyethylene and polypropylene, polyacetal, acrylic resin such as polymethyl methacrylate, polycarbonate, polyvinyl chloride, styrene resin such as polystyrene and ABS, fluoropolymer, polyphenylene sulfide, polyether ether ketone, polyphenylene ether, polysulfone, polyether sulfone, polyimide, polyetherimide, ethylene-propylene-diene ternary copolymer. Examples of the rubber include rubbers such as synthetic rubber, acrylonitrile-butadiene copolymer rubber, chloroprene rubber, chlorosulfonated polyethylene rubber, ethylene-propylene copolymer rubber, acrylic rubber, hydrin rubber, styrene-butadiene copolymer rubber, isobutylene-isoprene copolymer rubber, natural rubber, isoprene rubber, butadiene rubber, urethane-based rubber, silicone-based rubber, and fluorine-based rubber; and thermoplastic elastomers such as styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, urethane-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers.
[0051] The resin to be bonded to the aluminum alloy molded product may be a resin composition containing other components other than the resin. Examples of the other components include a crosslinking agent, a plasticizer, a filler, and a pigment. The content of the other components is not particularly limited as long as it does not impair the effects of the present invention. From the viewpoint of further improving the bonding strength, the content of the other components is preferably 50% by mass or less, and more preferably 20% by mass or less.
[0052] The resin adhesive to be bonded to the aluminum alloy molded product is not particularly limited and may be appropriately selected depending on the application of the bonded product, the type of member to be bonded to the aluminum alloy molded product, etc. Examples of the resin adhesive include hot melt adhesives, solvent volatilization type adhesives, hardener mixed type adhesives, thermosetting type adhesives, ultraviolet curing type adhesives, moisture curing type adhesives, anaerobic curing type adhesives, and emulsion type adhesives.
[0053] Examples of resins used in hot melt adhesives include polyolefins, polyurethanes, ethylene-ethyl acrylate copolymers, ethylene-acrylic acid copolymers, ethylene-vinyl acetate copolymers, polyamides, polyesters, thermoplastic elastomers, styrene-butadiene copolymers, and styrene-isoprene copolymers. Reactive hot melt adhesives may also be used. Epoxy resins and the like are used in reactive hot melt adhesives.
[0054] Resins used in solvent volatile adhesives include polyvinyl acetate, acrylic resin, etc. Curing agent mixed adhesives include epoxy resin-based and silicone rubber-based adhesives.
[0055] There is no particular limitation on the method for directly bonding a resin member to an aluminum alloy molded product, and examples thereof include an insert molding method, a press molding method, a lamination method, and a vulcanization adhesion method.
[0056] According to the manufacturing method of the present invention, a joined article of an aluminum alloy molded article and a resin having high joining strength can be obtained. A preferred embodiment of the manufacturing method of the joined article is a joined article obtained by adhering a resin to the first or second oxide film on the surface of the aluminum alloy molded article. Such joined articles are useful in the fields of transportation equipment such as automobiles and motorcycles, electronic equipment, building materials, leisure goods such as bicycles and fishing equipment, and daily necessities. EXAMPLES
[0057] The present invention will now be described in more detail with reference to examples.
[0058] (1) Electron microscope observation of the surface and cross section of aluminum alloy molded products Electron micrographs were taken using a field emission scanning electron microscope "JXA-8230 Electron Probe Microanalyzer" manufactured by JEOL Ltd. Test pieces for cross-sectional observation were prepared as follows. After embedding an aluminum alloy molded product in epoxy resin, it was cut in a direction perpendicular to the molded product surface. A diamond cutter was used to cut the molded product. A cross-session polisher "IB-09010CP" manufactured by JEOL Ltd. was used to process the cut surface of the molded product to obtain a test piece for cross-sectional observation.
[0059] (2) Electrochemical measurements of aluminum alloy molded products An anodic polarization curve was obtained in a 5% by mass sodium chloride aqueous solution at pH 6.5 using an electrochemical measurement device "HZ-7000" manufactured by Hokuto Denko Corporation. The test piece was 15 mm × 15 mm, and the measurement area was 1 cm 2 A silver-silver chloride electrode was used as the reference electrode, and a platinum electrode was used as the counter electrode. The temperature was kept at 20°C during the measurements, and a current-potential curve was measured by constant-speed potential scanning. The potential scanning rate was 40 mV / min. The corrosion potential (natural potential) of the anodized film and the substrate was obtained from the minimum value of the obtained polarization curve.
[0060] (3) Measurement of the bonding strength of the bonded parts FIG. 1 shows a schematic diagram of the method for evaluating the bond strength. As shown in FIG. 1, a polyamide-based hot melt sheet ("Elfan NT" manufactured by Nihon Matai Co., Ltd.) measuring 20 mm in length, 20 mm in width, and 50 μm in thickness was sandwiched between the aluminum alloy molded products 1, and then the three-layer laminate was held at 155°C for 60 seconds while a load (19.6 N) was applied to the laminated portion. The shear peel strength was determined by performing a tensile test on the resulting bonded product using Shimadzu Corporation's "Autograph" (shear rate 0.5 mm / sec). The tensile test was performed two to three times for one type of bonded product, and the bond strength of the bonded product was evaluated using the average value of the shear peel strength.
[0061] Example 1 The aluminum alloy substrate was A5052P, a wrought material specified by JIS H4000. The wrought material was cut to obtain an aluminum alloy substrate having a length of 100 mm, a width of 20 mm, and a thickness of 2 mm.
[0062] As a pretreatment, the aluminum alloy substrate was polished using a buffing machine (polished using #240 waterproof abrasive paper, then polished using #600 waterproof abrasive paper), then immersed in a sodium hydroxide-based degreasing solution for 5 minutes to degrease, and further immersed in 5% nitric acid for 10 seconds to remove smut. The pretreated aluminum alloy substrate was subjected to anodization at 15 V for 20 minutes in a phosphoric acid aqueous solution at 25°C (phosphoric acid 1.46 mol / L, pH 1.0) to form a first oxide film. The aluminum alloy substrate on which the first oxide film was formed was subjected to anodization at 12.5 V for 30 minutes in a sulfuric acid aqueous solution at 20 to 23°C (sulfuric acid 3.67 mol / L, pH <0) to form a second oxide film. The substrate after the treatment was washed with water and then dried. In this way, an aluminum alloy molded product on which the first and second oxide films were formed was obtained.
[0063] The cross section of the obtained aluminum alloy molded product was observed under an electron microscope (measurement of the film thickness of the first and second oxide films), and the surface was observed under an electron microscope (measurement of the pore size). An electron microscope photograph of the cross section of the obtained aluminum alloy molded product 1 is shown in FIG. 2. An enlarged electron microscope photograph of the cross section of the aluminum alloy molded product is shown in FIG. 3. In FIG. 2, the layer present on the aluminum alloy substrate 3 is the second oxide film 4. And the thin layer on the surface of the second oxide film 4 is the first oxide film 5. The thickness T of the first oxide film 5 measured from the electron microscope photograph of the cross section was 1 The thickness of the second oxide film 3 is 0.6 μm. 2 The evaluation results are also shown in Table 1.
[0064] An electron microscope photograph of the surface of an aluminum alloy molded product is shown in FIG. 4. In FIG. 4, the white mesh-like portion is the first oxide film 5. And the black dots seen in the pores of the first oxide film 5 are the pores 6 formed in the second oxide film 4. The average pore diameter D of the pores in the first oxide film 5 obtained from the electron microscope photograph of the surface of the aluminum alloy molded product was 1 The average pore diameter D was calculated by averaging the pore diameters measured at 10 points. 1 The average pore diameter D of the pores 6 formed in the second oxide film 4 was calculated. 2 The average pore diameter D was 30 nm. 2 is the average pore diameter D 1 The evaluation results are also shown in Table 1. The polarization curve obtained by electrochemical measurement of the aluminum alloy molded product (the portion on which the first and second oxide films were formed) is shown in FIG.
[0065] The aluminum alloy molded product 1 on which the second oxide film 4 was formed was washed with water, dried, and then left in the air for 7 days. A bonded product was manufactured using the aluminum alloy molded product 1 after the leaving, and the bond strength was evaluated. The average shear peel strength was calculated by performing a tensile test three times, and was 5.6 kN. The evaluation results are also shown in Table 1.
[0066] Example 2 Except for changing the phosphoric acid concentration of the phosphoric acid aqueous solution to 2.89 mol / L (pH 0.7), aluminum alloy molded products having first and second oxide films formed thereon were manufactured and evaluated in the same manner as in Example 1. The evaluation results (electron microscope photographs are omitted) are shown in Table 1 and FIG.
[0067] Comparative Example 1 An aluminum alloy molded product having only the first oxide film formed thereon was manufactured and evaluated in the same manner as in Example 1, except that the second oxide film was not formed. An electron microscope photograph of the surface of the obtained aluminum alloy molded product is shown in FIG. 5 (an electron microscope photograph of the cross section is omitted). In addition, an aluminum alloy molded product having only the first oxide film formed thereon was manufactured in the same manner as in Example 1, except that the second oxide film was not formed. Without being left in the air for 7 days, the molded product was subsequently used to manufacture a bonded product, and the bond strength was then measured. The results are shown in Table 1 and FIG. 7.
[0068] Comparative Example 2 Except for not forming a second oxide film and changing the phosphoric acid concentration of the phosphoric acid aqueous solution to 2.89 mol / L (pH 0.7), an aluminum alloy molded product having only a first oxide film was manufactured and evaluated in the same manner as in Example 1 (electron microscope photographs are omitted). The results are shown in Table 1 and Figure 7.
[0069] Comparative Example 3 An aluminum alloy molded product having only a second oxide film formed thereon was manufactured and evaluated in the same manner as in Example 1, except that the first oxide film was not formed. The results are shown in Table 1 and Figure 7. An electron microscope photograph of the surface of the obtained aluminum alloy molded product is shown in Figure 6 (an electron microscope photograph of the cross section is omitted).
[0070] Comparative Example 4 The aluminum alloy molded product was manufactured and evaluated in the same manner as in Example 1, except that an aqueous solution (pH<0) containing 11.69 mol / L phosphoric acid and 3.67 mol / L sulfuric acid was used as the electrolytic solution when forming the first oxide film, and the electrolysis conditions were changed as shown in Table 1 (electron microscope photographs are omitted). The results are shown in Table 1. No electrochemical measurement was performed on the aluminum alloy molded product.
[0071] Comparative Example 5 The two types of oxide films were formed in the same manner as in Example 1, except that an aqueous solution (pH<0) containing 11.69 mol / L phosphoric acid and 3.67 mol / L sulfuric acid was used as the electrolyte when the first oxide film was formed, an aqueous solution (pH12.3) containing 2.47 mol / L trisodium phosphate (in terms of phosphate radical) was used as the electrolyte when the second oxide film was formed, and the electrolysis conditions when forming the first and second oxide films were changed as shown in Table 1. The aluminum alloy substrate after anodization was immersed in a 5% aqueous nitric acid solution at 20°C for 10 seconds. The molded product after the treatment was washed with water and then dried. The aluminum alloy molded product thus obtained was evaluated (electron microscope photographs are omitted). The results are shown in Table 1. The electrochemical measurement of the aluminum alloy molded product was not performed.
[0072] Comparative Example 6 Except for not forming the first and second oxide films, aluminum alloy molded products were produced, and the bonding strength and electrochemical measurements were carried out in the same manner as in Example 1. The results are shown in Table 1 and FIG.
[0073] [Table 1]
[0074] Aluminum alloy molded products (Examples 1 and 2) obtained by forming a first oxide film using an electrolyte containing phosphoric acid and then forming a second oxide film using an electrolyte containing sulfuric acid had high shear peel strength even when bonded to resin after being left in the air for 7 days. Furthermore, the corrosion potential (natural potential) of the anodized film formed on the surface was higher than that of an aluminum alloy molded product without an oxide film (Comparative Example 6) and an aluminum alloy molded product with only a first oxide film (Comparative Examples 1 and 2) (FIG. 7), and the aluminum alloy molded products had excellent corrosion resistance.
[0075] On the other hand, the aluminum alloy molded products obtained by forming only the first oxide film using an electrolyte containing phosphoric acid (Comparative Examples 1 and 2) had high shear peel strength when bonded immediately after forming the second oxide film (Comparative Example 1), but when bonded after leaving in the air for 7 days, the bond strength was significantly reduced, and the corrosion potential (natural potential) of the anodized film was lower than that of the aluminum alloy molded products obtained by forming the first and second oxide films (Examples 1 and 2), resulting in low corrosion resistance. Also, the aluminum alloy molded products obtained by forming the first oxide film using an electrolyte containing phosphoric acid and sulfuric acid (Comparative Examples 4 and 5) and the aluminum alloy molded product obtained by forming only the second oxide film (Comparative Example 3) had low shear peel strength. [Explanation of symbols]
[0076] 1. Aluminum alloy moldings 2. Hot melt sheet 3. Aluminum alloy substrate 4 Second oxide film 5 First oxide film 6 Pore
Claims
1. anodizing an aluminum alloy substrate using an electrolytic solution containing 0.5 to 7 mol / L of phosphoric acid and less than 0.5 mol / L of sulfuric acid to form a first oxide film, and then anodizing the substrate using an electrolytic solution containing 0.5 to 5 mol / L of sulfuric acid to form a second oxide film between the aluminum alloy substrate and the first oxide film; Thickness T of the first oxide film 1 is 0.1 to 5 μm, and the thickness T 2 The first and second oxide films have pores oriented in the thickness direction, the average pore diameter D 1 of the first oxide film is 40 to 200 nm, and the average pore diameter D 1 is the average pore diameter D of the second oxide film 2 The method for producing an aluminum alloy formed product,
2. The method according to claim 1, wherein the temperatures of the electrolytic solutions used in forming the first and second oxide films are each 0 to 50° C.
3. A method for producing a bonded article, comprising bonding a resin to the first oxide film on the surface of an aluminum alloy molded article obtained by the method according to claim 1 or 2.
4. 4. The method according to claim 3, wherein the resin is bonded to the first oxide film three or more days after the second oxide film is formed on the aluminum alloy substrate.
5. 5. The method for manufacturing a joined article according to claim 3, wherein the resin is a resin adhesive, and the aluminum alloy molded article and another member are joined via the resin adhesive.
6. 5. The method for manufacturing a bonded article according to claim 3 or 4, wherein the member made of the resin is directly bonded to the first oxide film by at least one method selected from the group consisting of an insert molding method, a press molding method, a lamination method, and a vulcanization bonding method.
7. An aluminum alloy molded product having an aluminum alloy substrate having a surface covered with an oxide film, a surface of the aluminum alloy base material is covered with a second oxide film, and a surface of the second oxide film is covered with a first oxide film; Thickness T of the first oxide film 1 is 0.1 to 5 μm, and the thickness T 2 is 5 to 25 μm, The first and second oxide films have pores oriented in the thickness direction, and the average pore diameter D of the first oxide film 1 is the average pore diameter D of the second oxide film 2 Larger than Average pore diameter D of the first oxide film 1 The aluminum alloy molded product is characterized in that the grain size is 40 to 200 nm.
8. A bonded article, comprising the first oxide film on the surface of the aluminum alloy molded article according to claim 7 and a resin bonded thereto.
9. 9. The joined article according to claim 8, wherein the resin is a resin adhesive, and the aluminum alloy molded article and another member are joined via the resin adhesive.
10. 9. The joined article according to claim 8, which is an insert molded article, a press molded article, a laminate or a vulcanization bonded article obtained by directly bonding a member made of the resin to the first oxide film on the surface of the aluminum alloy molded article.
11. The bonded article according to any one of claims 8 to 10, which is for transport equipment, electronic equipment, building materials, leisure goods, or daily necessities.
Citation Information
Patent Citations
Waterproof dyeing mobile phone shell and preparation method thereof
CN109986742A
Lithographic printing plate support, method of manufacturing the same, and original plate for lithographic printing
JP2011173413A
Bonded article production method
JP2015089964A
Method for anodizing aluminum materials
US20050150771A1
Lithographic printing plate precursors and method of use
US20180250925A1