Toner binder resin
The binder resin for toner, composed of monoester compounds and specific vinyl resins, addresses the issues of low-temperature fixability and fixing strength in existing toners, providing enhanced performance in energy-efficient copiers and laser printers.
Patent Information
- Application Number
- JP2021028376
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-25
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2041-02-25
AI Technical Summary
Existing non-magnetic toners, such as those described in Patent Document 1, do not have sufficient low-temperature fixability and fixing strength, which are crucial for energy-efficient copiers and laser printers.
A binder resin for toner is developed using a monoester compound in combination with a release agent, along with carboxy group-containing and glycidyl group-containing vinyl resins, to enhance low-temperature fixing properties and anti-offset properties. The resin includes specific molecular weight distributions and ratios of high and low molecular weight vinyl resins, along with a fatty acid metal salt to adjust viscosity and improve fixing strength.
The binder resin achieves excellent low-temperature fixing properties, anti-offset properties, and fixing strength, ensuring better durability and productivity of toner performance.
Smart Images

Figure 0007590890000001 
Figure 0007590890000002 
Figure 0007590890000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder resin for a toner. [Background technology]
[0002] Generally, energy saving performance is considered important for copiers and laser printers, and toner that can be fixed at a lower temperature is being actively developed in order to lower the fixing temperature of the toner.
[0003] For example, Patent Document 1 describes a non-magnetic toner having non-magnetic toner particles containing at least a binder resin, a colorant, a polymer having a sulfur atom, and a wax component, the non-magnetic toner particles being obtained by dispersing a polymerizable monomer composition containing at least a polymerizable monomer, a colorant, a polymer having a sulfur atom, and a wax component in an aqueous dispersion medium, granulating the composition, and polymerizing the polymerizable monomer in the granulated particles, the wax component containing an ester wax and a hydrocarbon wax, the non-magnetic toner having two different endothermic peaks P1 and P2 (P1 is on the lower temperature side than P2) derived from the wax component in a temperature range of 55 to 120°C in a DSC curve during temperature rise measured with a differential scanning calorimeter (DSC), P1 being a peak derived from the ester wax, P2 being a peak derived from the hydrocarbon wax, the intensity ratio of the endothermic peaks P1 and P2 being 0.1 to 10, and the average circularity being 0.960 to 0.995. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 4266658 Summary of the Invention [Problem to be solved by the invention]
[0005] According to the investigations of the present inventors, it has become clear that, for example, the non-magnetic toner described in Patent Document 1 does not provide sufficient low-temperature fixability and fixing strength.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a binder resin for toner which is excellent in low-temperature fixing property, offset resistance, and fixing strength. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems, and have found that by using a monoester compound as a crystalline component for low-temperature fixing together with a release agent other than the monoester compound, it is possible to prevent the viscosity from decreasing too much when melted due to crosslinking of the resin, and to thereby achieve excellent low-temperature fixing properties, offset resistance, and fixing strength, and have completed the present invention.
[0008] That is, according to the present invention, there is provided the following binder resin for toner.
[0009] [1] A carboxyl group-containing vinyl resin (C), A glycidyl group-containing vinyl resin (E); a reaction product of the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E); A toner binder resin comprising a monoester compound obtained from a linear saturated aliphatic monocarboxylic acid and a monohydric linear saturated aliphatic alcohol, A toner binder resin comprising at least one release agent other than the monoester compound. [2] The carboxyl group-containing vinyl resin (C), The glycidyl group-containing vinyl resin (E), The binder resin for toner according to the above-mentioned [1] contains the monoester compound in an amount of 4% by mass or more and 15% by mass or less, based on 100% by mass of the total of the reactants. [3] The binder resin for toner according to the above [1] or [2], wherein the release agent other than the monoester compound is one or more release agents selected from the group consisting of polyethylene wax, polypropylene wax, Fischer-Tropsch wax, paraffin wax, carnauba wax, and ester waxes having two or more ester bonds. [4] The binder resin for toner according to any one of the above [1] to [3], wherein the release agent other than the monoester compound is contained in an amount of 2% by mass or more and 8% by mass or less based on the entire binder resin for toner. [5] The carboxyl group-containing vinyl resin (C) has a molecular weight distribution of tetrahydrofuran soluble matter measured by gel permeation chromatography, which is as follows: Molecular weight is 2.5×10 4 More than 1.2 x 10 5 A high molecular weight vinyl resin (H) having a peak in the following region: Molecular weight is 2×10 3 More than 2×10 4 and a low molecular weight vinyl resin (L) having a peak in the following region: The binder resin for toner according to any one of the above [1] to [4], wherein a mass ratio (H / L) of the high molecular weight vinyl resin (H) to the low molecular weight vinyl resin (L) is 55 / 45 to 85 / 15. [6] The binder resin for toner according to any one of the above [1] to [5], which contains a fatty acid metal salt represented by the following general formula (1): TIFF0007590890000001.tif9153In the above general formula (1), n is an integer of 11 to 22, m is 2, and M is a metal atom selected from Zn and Ca. [7] The binder resin for toner according to any one of the above [1] to [6], wherein the tetrahydrofuran insoluble component in the binder resin for toner is 10% by mass to 40% by mass based on the entire binder resin. Effect of the Invention
[0010] According to the present invention, it is possible to provide a binder resin for a toner which is excellent in low-temperature fixing property, offset resistance, and fixing strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. Note that a numerical range of "A to B" means A or more and B or less unless otherwise specified. In this specification, the term "(meth)acrylic" includes acrylic, methacrylic, or both acrylic and methacrylic, unless otherwise specified.
[0012] <Binder resin for toner> The toner binder resin according to the present embodiment is A carboxyl group-containing vinyl resin (C); A glycidyl group-containing vinyl resin (E); a reaction product of the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E); A toner binder resin comprising at least a monoester obtained from a linear saturated aliphatic monocarboxylic acid and a monohydric linear saturated aliphatic alcohol, At least one release agent other than the monoester compound is included. In the toner binder resin according to this embodiment, by including a release agent (e.g., wax) other than the monoester compound, it is possible to prevent the viscosity from decreasing too much when melted due to crosslinking of the resin, and it is possible to obtain excellent low-temperature fixing property, offset resistance, and fixing strength.
[0013] The toner binder resin according to this embodiment will be described in detail below.
[0014] [Carboxylic group-containing vinyl resin (C)] The carboxyl group-containing vinyl resin (C) according to this embodiment is a resin containing one or more carboxyl groups and one or more vinyl groups in one molecule. Such a resin can be obtained, for example, by polymerizing a styrene-based monomer, a (meth)acrylic monomer, and a carboxyl group-containing monomer using a known method.
[0015] Examples of styrene monomers include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, 3,4-dichlorostyrene, p-ethylstyrene, 2,4-dimethylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, etc. Among these, styrene is preferred.
[0016] Examples of the (meth)acrylic monomer include acrylic esters such as methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, octyl acrylate, cyclohexyl acrylate, stearyl acrylate, benzyl acrylate, furfuryl acrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, dimethylaminomethyl acrylate, and dimethylaminoethyl acrylate; methacrylic esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, octyl methacrylate, cyclohexyl methacrylate, stearyl methacrylate, benzyl methacrylate, furfuryl methacrylate, hydroxyethyl methacrylate, hydroxyethyl methacrylate, hydroxybutyl methacrylate, dimethylaminomethyl methacrylate, and dimethylaminoethyl methacrylate; amides such as acrylamide, methacrylamide, N-substituted acrylamide, and N-substituted methacrylamide; acrylonitrile, methacrylonitrile, and the like. Of these, acrylic acid esters, methacrylic acid esters, acrylonitrile, and methacrylonitrile are preferred, and butyl acrylate, methyl methacrylate, butyl methacrylate, and hydroxyethyl acrylate are more preferred.
[0017] Examples of the carboxyl group-containing monomer include acrylic acid, methacrylic acid, maleic anhydride, maleic acid, fumaric acid, cinnamic acid, methyl fumarate, ethyl fumarate, propyl fumarate, butyl fumarate, octyl fumarate, methyl maleate, ethyl maleate, propyl maleate, butyl fumarate, octyl maleate, etc. Among these, preferred are acrylic acid, methacrylic acid, fumaric acid, methyl fumarate, ethyl fumarate, propyl fumarate, butyl fumarate, and octyl fumarate, and particularly preferred are acrylic acid and methacrylic acid.
[0018] The content of the carboxyl group-containing vinyl resin (C) is preferably 70% by mass or more and 98% by mass or less, more preferably 75% by mass or more and 98% by mass or less, and even more preferably 80% by mass or more and 97% by mass or less, when the entire toner binder resin according to the present embodiment is taken as 100% by mass. This makes it possible to obtain a toner having a better balance of fixing property, offset resistance, and storage stability.
[0019] The ratio of the carboxyl group-containing vinyl resin (C) to the glycidyl group-containing vinyl resin (E) described later, carboxyl group-containing vinyl resin (C) / glycidyl group-containing vinyl resin (E), can be, for example, 85 / 15 to 99 / 1, more preferably 87 / 13 to 97 / 3.
[0020] The carboxyl group-containing vinyl resin (C) according to this embodiment may use, as a monomer, a crosslinkable monomer having two or more double bonds, as necessary. Examples of the crosslinkable monomer include aromatic divinyl compounds such as divinylbenzene and divinylnaphthalene; diacrylate compounds such as ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentanediol diacrylate, 1,6-hexadiol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyoxyethylene (2)-2,2-bis(4-hydroxyphenyl)propane diacrylate, and polyoxyethylene (4)-2,2-bis(4-hydroxyphenyl)propane diacrylate, and methacrylate compounds thereof; and polyfunctional crosslinkable monomers such as pentaerythritol triacrylate, trimethylolethane triacrylate, trimethylolpropane triacrylate, trimethylolethane triacrylate, and tetramethylolmethane tetraacrylate, and methacrylate compounds thereof.
[0021] When these polyfunctional crosslinking monomers are used, the amount is preferably 0.5 parts by mass or less per 100 parts by mass of other monomers in the carboxyl group-containing vinyl resin (C). By making the amount less than the upper limit, the crosslinked body formed by the reaction of the carboxyl group and the glycidyl group described below is less likely to be broken during toner production.
[0022] The acid value of the carboxyl group-containing vinyl resin (C) according to the present embodiment is preferably 0.5 mgKOH / g or more, more preferably 1 mgKOH / g or more. When the acid value of the carboxyl group-containing vinyl resin (C) is equal to or more than the lower limit, the reaction with the glycidyl group-containing vinyl resin (E) proceeds smoothly, and a toner having excellent offset resistance can be obtained. On the other hand, the acid value of the carboxyl group-containing vinyl resin (C) is preferably 30 mgKOH / g or less, more preferably 25 mgKOH / g or less. When the acid value of the carboxyl group-containing vinyl resin (C) is the above upper limit or less, excessive crosslinking reaction with the glycidyl group-containing vinyl resin (E) is suppressed, and as a result, a decrease in offset resistance, which is considered to be caused by excessive phase separation of the crosslinked component obtained by the reaction of the carboxyl group-containing vinyl resin (C) with the glycidyl group-containing vinyl resin (E) from the non-crosslinked component, can be suppressed. The acid value here refers to the number of milligrams of potassium hydroxide required to neutralize 1 g of resin.
[0023] From the viewpoint of the overall balance of the toner's low-temperature fixing property, offset resistance, durability, etc., the carboxyl group-containing vinyl resin (C) is selected so that the molecular weight of the tetrahydrofuran (THF)-soluble matter measured by gel permeation chromatography (GPC) is 2.5×10 4 More than 1.2 x 10 5 A high molecular weight vinyl resin (H) with a peak in the following region and a molecular weight distribution of the THF-soluble fraction measured by GPC of 2.0×10 3 Above 2.0×10 4 It is preferable that the low molecular weight vinyl resin (L) has a peak in the following region: Here, the peak refers to the main peak (the peak with the greatest intensity among the peaks).
[0024] When the carboxyl group-containing vinyl resin (C) is composed of a high molecular weight vinyl resin (H) and a low molecular weight vinyl resin (L), the mass ratio (H / L) thereof is preferably 55 / 45 to 85 / 15, and more preferably 60 / 40 to 80 / 20, from the viewpoint of the overall balance of the toner fixing property, offset resistance, durability, etc. By setting the ratio of the high molecular weight vinyl resin (H) to the above lower limit or more, a toner having better durability and offset resistance can be obtained. By setting the ratio of the high molecular weight vinyl resin (H) to the above upper limit or less, a toner having better fixing properties and productivity can be obtained.
[0025] (High molecular weight vinyl resin (H)) In the present embodiment, the high molecular weight vinyl resin (H) has a molecular weight of 2.5×10 in the molecular weight distribution measured by GPC for the THF soluble content. 4 More than 1.2 x 10 5 It is preferable that the main peak is in the following region, and more preferably in the region of 3.0×10 4 Above 1.0×10 5 It is preferable that the toner has the following main peaks. This makes it possible to realize an excellent balance of fixing property, offset resistance, and durability. By making the main peak of the high molecular weight vinyl resin (H) equal to or higher than the lower limit, the strength of the resin is improved, and a toner having superior durability can be obtained. In addition, in the formation of a crosslinked product by a reaction with a glycidyl group described later, the crosslinking proceeds well, and therefore a toner having superior offset resistance can be obtained. In addition, by making the peak molecular weight equal to or less than the upper limit, even if the high molecular weight vinyl resin remains in an unreacted state, the viscosity of the toner during fixing is unlikely to increase, and a toner with superior fixing properties can be obtained. In addition, the strength of the resin becomes appropriate, and a toner with superior productivity can be obtained.
[0026] The high molecular weight vinyl resin (H) preferably has an acid value of 3 to 35 mgKOH / g, more preferably 5 to 30 mgKOH / g. Such an acid value is preferable in terms of the fixing property and offset resistance of the toner. When the acid value is equal to or more than the lower limit, the resin easily reacts with the glycidyl group-containing vinyl resin (E), and a toner having excellent offset resistance can be obtained. When the acid value is equal to or less than the upper limit, excessive reaction with the glycidyl group-containing vinyl resin (E) is suppressed, and as a result, the loss modulus in the fixing temperature range of the toner becomes appropriate, and a toner with excellent fixing properties can be obtained.
[0027] The high molecular weight vinyl resin (H) does not necessarily have to be a homopolymer, and two or more kinds of high molecular weight vinyl resins may be used. In that case, it is preferable that the high molecular weight vinyl resin (H) as a whole satisfies the above-mentioned characteristics. In addition, when producing a homopolymer, it is also possible to add a carboxyl group-containing monomer during polymerization, or to add it separately at the early and late stages of polymerization.
[0028] (Low molecular weight vinyl resin (L)) In the present embodiment, the low-molecular-weight vinyl resin (L) has a molecular weight of 2.0×10 in the molecular weight distribution measured by GPC for the THF-soluble content. 3 Above 2.0×10 4 It is preferable that the main peak is in the region of 2.5×10 3 Above 1.0×10 4 It is preferable that the toner has the following main peaks. This makes it possible to realize an excellent balance of fixing property, offset resistance, and durability.
[0029] By setting the peak molecular weight to be equal to or greater than the lower limit, a toner having superior durability can be obtained, whereas by setting the peak molecular weight to be equal to or less than the upper limit, a toner having superior fixability and productivity can be obtained.
[0030] The low molecular weight vinyl resin (L) preferably has an acid value of 1 to 20 mgKOH / g, and more preferably 2 to 18 mgKOH / g in order to exhibit excellent fixing performance and offset resistance. By making the acid value equal to or more than the above lower limit, compatibility with the high molecular weight vinyl resin (H) becomes good, and a toner having superior durability and offset resistance is obtained. In addition, by keeping the molecular weight equal to or less than the upper limit, inhibition of the reaction between the glycidyl group-containing vinyl resin (E) and the high molecular weight vinyl resin (H) by the low molecular weight vinyl resin (L) can be suppressed, and the low molecular weight vinyl resin (L) itself can be prevented from becoming too high in molecular weight, so that a toner having an excellent balance of offset resistance and fixing properties can be obtained.
[0031] The low molecular weight vinyl resin (L) does not necessarily have to be a homopolymer, and two or more kinds of low molecular weight vinyl resins may be used. In that case, it is preferable that the low molecular weight vinyl resin (L) as a whole satisfies the above-mentioned characteristics. In addition, when producing a homopolymer, it is also possible to add a carboxyl group-containing monomer during polymerization, or to add it separately at the early and late stages of polymerization.
[0032] In this embodiment, the carboxyl group-containing vinyl resin (C) can be produced by known polymerization methods such as solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, and combinations thereof. Solution polymerization is preferably used because of the ease of adjusting the molecular weight distribution, the mixability of the high molecular weight vinyl resin (H) and the low molecular weight vinyl resin (L), and the distribution of the carboxyl group and glycidyl group.
[0033] The carboxyl group-containing vinyl resin (C) according to the present embodiment can be obtained by polymerizing the high molecular weight vinyl resin (H) and the low molecular weight vinyl resin (L) independently in advance and mixing them in a molten state or in a solution state. Alternatively, it can be obtained by polymerizing either the high molecular weight vinyl resin (H) or the low molecular weight vinyl resin (L) independently and then polymerizing the other vinyl resin in the presence of the polymerized resin.
[0034] Solvents used in the solution polymerization include aromatic hydrocarbons such as benzene, toluene, ethylbenzene, xylene, and cumene, which may be used alone or in mixture, with xylene being preferred.
[0035] The polymerization may be carried out using a polymerization initiator, or may be carried out without using a polymerization initiator, i.e., so-called thermal polymerization. As the polymerization initiator, any one that can be used as a radical polymerization initiator can be used. For example, azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobisisobutyrate, 1,1-azobis(1-cyclohexanecarbonitrile), 2-(carbamoylazo)-isobutyronitrile, 2,2'-azobis(2,4,4-trimethylpentane), 2-phenylazo-2,4-dimethyl-4-methoxyvaleronitrile, and 2,2'-azobis(2-methylpropane); Ketone peroxides such as ketone peroxide, acetylacetone peroxide, and cyclohexanone peroxide; peroxyketals such as 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,1-bis(butylperoxy)cyclohexane, and 2,2-bis(t-butylperoxy)butane; hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, and 1,1,3,3-tetramethylbutyl hydroperoxide. peroxides; dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, di-cumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, α,α'-bis(t-butylperoxyisopropyl)benzene; isobutyryl peroxide, octanoyl peroxide, decanoyl peroxide, lauroyl peroxide, 3,5,5-trimethylhexanoyl peroxide, benzoyl peroxide, m-toluene diacyl peroxides such as diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di-2-ethoxyethyl peroxydicarbonate, di-methoxyisopropyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, and other peroxydicarbonates; sulfonyl peroxides such as acetylcyclohexyl sulfonyl peroxide;Examples of the initiator include peroxyesters such as t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxylaurate, t-butyl peroxybenzoate, t-butyl peroxyisopropyl carbonate, and di-t-butyl diperoxyisophthalate. These initiators may be used alone or in combination of two or more.
[0036] The type and amount of the polymerization initiator can be appropriately selected depending on the reaction temperature, monomer concentration, etc., and can usually be used in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the monomer used.
[0037] [Glycidyl group-containing vinyl resin (E)] The glycidyl group-containing vinyl resin (E) according to this embodiment can be obtained, for example, by using at least one styrene-based monomer, at least one (meth)acrylic monomer, and at least one glycidyl group-containing monomer by a known polymerization method.
[0038] As the styrene-based monomer and (meth)acrylic monomer used in the glycidyl group-containing vinyl resin (E), the monomers exemplified in the description of the carboxy group-containing vinyl resin (C) can be used.
[0039] Examples of the glycidyl group-containing monomer used in the glycidyl group-containing vinyl resin (E) include glycidyl acrylate, β-methylglycidyl acrylate, glycidyl methacrylate, β-methylglycidyl methacrylate, etc. Among these, preferred are glycidyl methacrylate and β-methylglycidyl methacrylate.
[0040] The glycidyl group-containing vinyl resin (E) preferably has a molecular weight of 1.0×10 in the molecular weight distribution of the THF-soluble portion measured by GPC. 4 Above 1.0×10 5 Less than or equal to 2.0×104 Above 8.0×10 4 The main peak is as follows: The epoxy value is preferably from 0.003 to 0.100 Eq / 100 g, and more preferably from 0.003 to 0.080 Eq / 100 g. If the peak molecular weight and epoxy value of the glycidyl group-containing vinyl resin (E) are equal to or greater than the lower limit, the durability of the toner is improved, and image deterioration due to toner destruction during long-term continuous printing is prevented, so-called development maintenance characteristics are improved. At the same time, the reaction between the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E) increases the molecular weight of the high molecular weight component, imparting appropriate elasticity to the binder resin, resulting in better offset resistance. Moreover, by setting the peak molecular weight to the above upper limit or less and the epoxy value to the above upper limit or less, excessive elasticity of the binder resin can be suppressed, and a toner with superior fixing properties can be obtained. In this embodiment, the epoxy value is the number of moles of epoxy groups present in 100 g of resin, and can be measured in accordance with JIS K-7236.
[0041] The glycidyl group-containing vinyl resin (E) does not necessarily have to be a homopolymer, and two or more kinds of glycidyl group-containing vinyl resins may be used. In that case, it is preferable that the glycidyl group-containing vinyl resin (E) as a whole satisfies the above-mentioned characteristics. In addition, when producing a homopolymer, it is also possible to add the glycidyl group-containing monomer during polymerization, or to add it separately at the early and late stages of polymerization.
[0042] The toner binder resin according to this embodiment preferably contains a tetrahydrofuran (THF) insoluble component. From the viewpoint of a balance between good fixing property, offset resistance, durability, and toner productivity, the content of the THF-insoluble component is preferably 10% by mass or more and 40% by mass or less, when the entire binder resin according to this embodiment is taken as 100% by mass.
[0043] By setting the THF insoluble component to the above lower limit or more, a toner having excellent offset resistance can be obtained. Furthermore, when the release agent is kneaded, a sufficient kneading shear is applied, which improves the dispersion of the release agent and improves the resistance to contamination of the photoreceptor. In addition, when the toner components such as the charge control agent, colorant, and magnetic material are kneaded and pulverized with the binder resin of this embodiment to produce a toner, a sufficient kneading shear is applied, which improves the dispersion of the toner components and improves the resistance to contamination of the photoreceptor. By controlling the THF insoluble component to the above upper limit or less, a toner with superior fixing properties is obtained, poor dispersion of components due to excessively separated gel is prevented, and resistance to contamination of the photoreceptor is further improved. Here, the THF-insoluble components in the toner binder resin according to this embodiment are preferably a crosslinking component generated by the reaction between a carboxy group derived from the carboxy group-containing vinyl resin (C) and a glycidyl group derived from the glycidyl group-containing vinyl resin (E) and a component derived from the release agent.
[0044] [Reaction product of carboxyl group-containing vinyl resin (C) and glycidyl group-containing vinyl resin (E)] The toner binder resin according to the present embodiment contains a reaction product (hereinafter, sometimes simply referred to as a reaction product) between the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E). By containing the reaction product, it is possible to suppress the deterioration of high temperature offset caused by a decrease in melt viscosity.
[0045] The carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E) to obtain the reaction product may be, for example, one or more kinds selected from the above-mentioned compounds. The reaction product can be obtained, for example, by mixing the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E) and heating them to react with each other. For details, see the examples described later.
[0046] [Monoester compound obtained from linear saturated aliphatic monocarboxylic acid and monovalent linear saturated aliphatic alcohol] The toner binder resin according to the present embodiment contains a monoester compound obtained from a linear saturated aliphatic monocarboxylic acid and a monovalent linear saturated aliphatic alcohol. The monoester compound has crystallinity, has excellent sharp melting properties, and acts as a plasticizer for the resin of the present embodiment when melted. By forming a binder resin containing the monoester compound into a toner, the low-temperature fixing property and fixing strength of the toner are improved.
[0047] The linear saturated aliphatic monocarboxylic acid is not particularly limited as long as it is a monocarboxylic acid. Examples of the monocarboxylic acid include butanoic acid, pentanoic acid, octanoic acid, nonanoic acid, decanoic acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid, and more preferably palmitic acid, stearic acid, arachidic acid, behenic acid, and lignoceric acid.
[0048] The monovalent linear saturated aliphatic alcohol is not particularly limited as long as it is a linear aliphatic and monovalent alcohol. Examples of such alcohols include methanol, ethanol, propanol, butanol, pentanol, octanol, nonanol, decanol, laurinol, myristinol, pentadecinol, palmitinol, margarinol, stearyl alcohol, arachidinol, behenyl alcohol, etc., and more preferably palmityl alcohol, stearyl alcohol, arachidyl alcohol, behenyl alcohol, and lignoceryl alcohol. These monocarboxylic acids and monohydric alcohols can provide better dispersibility in the binder resin of the present embodiment.
[0049] In this case, the monoester compound is preferably contained in an amount of 4% by mass or more and 15% by mass or less relative to 100% by mass of the total of the carboxyl group-containing vinyl resin (C), the glycidyl group-containing vinyl resin (E) and the reaction products. When the amount of the monoester compound added is equal to or more than the lower limit, the low temperature fixability can be improved, whereas when the amount is equal to or less than the upper limit, the dispersibility can be improved and charging defects can be prevented.
[0050] [Release agent] The toner binder resin according to this embodiment contains a release agent (hereinafter, also referred to as wax) other than the monoester compound in order to achieve better fixing performance and offset resistance.
[0051] The type of release agent is not particularly limited as long as it is other than the above monoester compounds, but aliphatic hydrocarbon waxes such as polyethylene wax, polypropylene wax, paraffin wax, and Fischer-Tropsch wax are preferred. In addition to the above-mentioned aliphatic hydrocarbon waxes, examples of the waxes that can be used include vegetable waxes such as carnauba wax, candelilla wax, Japan wax, rice wax, and jojoba wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolatum; waxes mainly composed of fatty acid esters such as montanic acid esters and castor wax; fatty acid esters such as deoxidized carnauba wax; unsaturated fatty acids such as brassidic acid, eleostearic acid, and parinaric acid; polyhydric alcohols such as sorbitol; linoleic acid amide, oleic acid amide, lauric acid amide, and lauric acid amide. Examples of such fatty acid amides include fatty acid amides such as phosphoric acid amide; fatty acid bisamides such as methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N-dioleyl adipic acid amide, hexamethylene bisoleic acid amide, and N,N'-dioleyl sepamide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide; and ester waxes having two or more ester bonds, such as pentaerythritol tetrabehenate.
[0052] The content of the release agent other than the monoester compound is preferably 2% by mass or more and 8% by mass or less based on the entire toner binder resin, from the viewpoint of a balance between offset resistance and storage stability.
[0053] The melting point of the release agent is typically 75° C. or higher. If it is 75° C. or higher, the release effect can be sufficiently obtained. Also, the melting point of the release agent is typically 140° C. or lower. If it is 140° C. or lower, the low-temperature fixability can be further improved. The melting point can be measured, for example, by differential scanning calorimetry (DSC).
[0054] (Fatty acid metal salts) The toner binder resin according to this embodiment preferably contains a fatty acid metal salt represented by the following general formula (1): The fatty acid metal salt functions as a catalyst in the reaction between the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E), thereby making it possible to adjust the binder resin to an appropriate viscosity.
[0055] [ka]
[0056] In the above general formula (1), n is an integer of 11 to 22, m is 2, and M is a metal atom selected from Zn and Ca.
[0057] Examples of such fatty acid metal salts include zinc laurate ((C 11 H 23 COO)2Zn), calcium laurate ((C 11 H 23 COO)2Ca), zinc stearate ((C 17 H 35 COO)2Zn), calcium stearate ((C 17 H 35 COO)2Ca), zinc beherate ((C 21 H 43 COO)2Zn), calcium beherate ((C21 H 43 COO)2Ca) and the like.
[0058] <Production method of binder resin> Next, a method for producing the toner binder resin according to this embodiment will be described. An example of a method for producing the toner binder resin according to this embodiment is a method of melt-kneading a carboxyl group-containing vinyl resin (C), a glycidyl group-containing vinyl resin (E), a monoester compound, and a release agent, but is not limited thereto.
[0059] In such a method, for example, a carboxyl group-containing vinyl resin (C), a glycidyl group-containing vinyl resin (E), a monoester compound, and a release agent are charged into a reaction vessel equipped with a stirrer, and the like, and heated to react in a molten state. In particular, it is preferable to use a twin-screw kneader.
[0060] By melt-kneading the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E) in the presence of a monoester compound and a release agent to cause a crosslinking reaction, the release agent can be further finely dispersed while obtaining a reaction product. It is believed that the release agent is further finely dispersed due to an increase in stirring shear caused by an increase in viscosity during the crosslinking reaction between the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E).
[0061] The temperature during melt kneading is not particularly limited since it varies depending on the functional groups and molecular weights of the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E), but is preferably 140°C or higher and 230°C or lower, more preferably 170°C or higher and 220°C or lower. By setting the temperature during melt kneading to be equal to or higher than the above lower limit, the crosslinked body is well formed, and the shear of the kneading becomes appropriate, so that the release agent can be further dispersed. In addition, by setting the temperature during melt kneading to the above upper limit or lower, the crosslinking reaction is prevented from proceeding excessively, and phase separation between the crosslinked component and the non-crosslinked component is suppressed, thereby making it possible to obtain a toner with superior offset resistance. In addition, depolymerization is suppressed, and concerns about problems such as poor development maintenance properties and odor of the toner due to the remaining volatile matter in the binder resin can be reduced.
[0062] In the method of melt-kneading using a twin-screw kneader, water can be injected into the twin-screw kneader through an inlet, and the water and volatile components can be removed by reducing the pressure through a pressure reduction port installed on the outlet side of the inlet. This method allows water to be thoroughly mixed into the resin, and makes it easier to remove volatile components such as monomers and solvents remaining in the resin when the pressure is reduced.
[0063] The resin thus obtained is cooled and pulverized to obtain a binder resin for toner. Any conventionally known method can be used for the cooling and pulverization method. As a cooling method, rapid cooling using a steel belt cooler or the like is also possible.
[0064] <Toner> Next, the toner according to the present embodiment will be described.
[0065] The toner according to the present embodiment includes a colorant as a toner component other than the binder resin for the toner according to the present embodiment. Furthermore, the toner according to the present embodiment may further include one or more selected from a charge control agent, a magnetic material, a surface treatment agent, etc. in addition to the binder resin for the toner. Hereinafter, the toner components other than the toner binder resin will be described.
[0066] As the colorant, conventionally known pigments and dyes can be used. Examples of pigments include mineral fast yellow, navel yellow, naphthol yellow S, Hansa yellow G, permanent yellow NCG, tartrazine lake, molybdenum orange, permanent orange GTR, pyrazolone orange, benzidine orange G, permanent red 4R, watching red calcium salt, eosin lake, brilliant carmine 3B, manganese purple, fast violet B, methyl violet lake, cobalt blue, alkali blue lake, Victoria blue lake, phthalocyanine blue, fast sky blue, indanthrene blue BC, chrome green, pigment green B, malachite green lake, and final yellow green G. Examples of magenta coloring pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 39, 40, 41, 48, 49, 50, 51, 52, 53, 54, 55, 57, 58, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 163, 202, 206, 207, 209, 238, CI Pigment Violet 19, CI Bat Red 1, 2, 10, 13, 15, 23, 29, 35, and the like. Examples of the cyan pigment include CI Pigment Blue 2, 3, 15, 15:1, 15:2, 15:3, 16, 17, CI Acid Blue 6, CI Acid Blue 45, or copper phthalocyanine pigments in which 1 to 5 phthalimidomethyl groups are substituted on the phthalocyanine skeleton. Examples of the yellow pigment include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 15, 16, 17, 23, 65, 73, 74, 83, 93, 97, 155, 180, 185, CI Bat Yellow 1, 3, 20, etc. Examples of the black pigment include carbon black such as furnace black, channel black, acetylene black, thermal black, and lamp black.Dyes include CI Direct Red 1, CI Direct Red 4, CI Acid Red 1, CI Basic Red 1, CI Mordant Red 30, CI Direct Blue 1, CI Direct Blue 2, CI Acid Blue 9, CI Acid Blue 15, CI Basic Blue 3, CI Basic Blue 5, CI Mordant Blue 7, CI Direct Green 6, CI Basic Green 4, CI Basic Green 6, Solvent Yellow 162, and the like. These colorants may be used alone or in combination of two or more kinds.
[0067] The content of the colorant in the toner is typically 0.05 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and even more preferably 0.2 to 10 parts by mass, based on 100 parts by mass of the binder resin.
[0068] A magnetic material can be used instead of a colorant. Examples of the magnetic material include metal oxides containing elements such as iron, cobalt, nickel, copper, magnesium, manganese, aluminum, and silicon. Specifically, examples of the magnetic material include iron tetraoxide, iron sesquioxide, zinc iron oxide, yttrium iron oxide, cadmium iron oxide, gadolinium iron oxide, copper iron oxide, lead iron oxide, nickel iron oxide, neodymium iron oxide, barium iron oxide, magnesium iron oxide, manganese iron oxide, lanthanum iron oxide, iron powder, cobalt powder, and nickel powder. Two or more of these magnetic materials may be used in combination as necessary. In addition, the shape of the magnetic material is preferably a sphere, an octahedron, or a hexahedron, and more preferably a sphere in order to disperse the magnetic material uniformly in the toner.
[0069] The content of the magnetic material is preferably 1 to 200 parts by mass, more preferably 10 to 170 parts by mass, and further preferably 20 to 150 parts by mass, relative to 100 parts by mass of the binder resin.
[0070] Furthermore, the toner according to the present embodiment may be used by partially adding a resin such as polyvinyl chloride, polyvinyl acetate, polyester, polyvinyl butyral, polyurethane, polyamide, polystyrene, rosin, polymerized rosin, modified rosin, terpene resin, phenolic resin, aromatic petroleum resin, PVC resin, styrene-butadiene resin, styrene-(meth)acrylic copolymer, chroman-indene resin, or melamine resin, as necessary, within a range that does not impair the effects of the present embodiment.
[0071] Also, for the purpose of improving the dispersion of the colorant, a method may be used in which the colorant is previously dispersed in a binder resin or a raw material resin thereof to prepare a so-called master batch, and this is then added to the toner. Specifically, 20 to 60% by mass of the colorant and 80 to 40% by mass of the resin component are mixed in a powder state, and the resulting mixture is kneaded with a batch-type kneader such as a twin-screw kneader, an open roll kneader, or a pressure kneader, and the resulting mixture is pulverized and used in the production of the toner.
[0072] The toner according to the present embodiment may contain a charge control agent to maintain positive or negative charging properties. Conventionally known charge control agents can be used as the charge control agent. Positively charging charge control agents include, for example, modified products of nigrosine and fatty acid metal salts, etc.; quaternary ammonium salts such as tributylbenzylammonium-1-hydroxy-4-naphthosulfonate and tetrabutylammonium tetrafluoroborate, and onium salts such as phosphonium salts which are analogues of these, and lake pigments thereof; triphenylmethane dyes and lake pigments thereof (lake pigments include phosphotungstic acid, phosphomolybdic acid, phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide, etc.); high-grade Examples of such copolymers include metal salts of fatty acids; diorganotin oxides such as dibutyltin oxide, dioctyltin oxide, and dicyclohexyltin oxide; diorganotin borates such as dibutyltin borate, dioctyltin borate, and dicyclohexyltin borate; guanidine compounds; imidazole compounds; imidazolium salts; and further, quaternary ammonium base-containing copolymers obtained by a method such as copolymerizing a dialkylaminoalkyl (meth)acrylate with a styrene-based monomer and, if necessary, a (meth)acrylic monomer, followed by quaternization with an alkyl paratoluenesulfonate.
[0073] As the negatively charged charge control agent, for example, organic metal complexes and chelate compounds are effective, and there are monoazo metal complexes, acetylacetone metal complexes, aromatic hydroxycarboxylic acid metal complexes, aromatic dicarboxylic acid metal complexes, aromatic hydroxycarboxylic acids, aromatic monocarboxylic acids, aromatic polycarboxylic acids, and their metal salts, anhydrides, and esters, and bisphenol derivatives such as bisphenol. Furthermore, there are azo metal compounds in which the coordination center metal is selected from Sc, Ti, V, Cr, Co, Ni, Mn, and Fe and the cation is selected from hydrogen ion, sodium ion, potassium ion, and ammonium ion, and there are azo metal compounds in which the coordination center metal is selected from Cr, Co, Ni, Mn, Fe, Ti, Zr, Zn, Si, B, and Al and the cation is hydrogen ion, Examples of the charge control agent include metal compounds of aromatic hydroxycarboxylic acid derivatives and aromatic polycarboxylic acid derivatives selected from sodium ions, potassium ions, ammonium ions, and aliphatic ammonium (the aromatic hydroxycarboxylic acid and aromatic polycarboxylic acid may have an alkyl group, an aryl group, a cycloalkyl group, an alkenyl group, an alkoxy group, an aryloxy group, a hydroxyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an acyl group, an acyloxy group, a carboxy group, a halogen, a nitro group, a cyano group, an amide group, an amino group, or a carbamoyl group as a substituent), and polymers having a sulfonic acid group-containing monomer as a constituent component, such as a copolymer of a sulfonic acid group-containing acrylamide monomer, a styrene monomer, and a (meth)acrylic monomer. These charge control agents may be used alone or in combination of two or more.
[0074] The content of the charge control agent in the toner is preferably 0.05 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.2 to 3 parts by mass, per 100 parts by mass of the binder resin, in consideration of the balance between the charge amount and the fluidity of the toner. As the addition method, a method of adding the charge control agent inside the toner, a method of adding the charge control agent to the outside, or a combination of these methods can be applied.
[0075] In the toner according to the present embodiment, it is preferable to add a surface treatment agent to the surface of the toner so that the surface treatment agent is present between the toner and the carrier, or between the toner particles themselves. By adding a surface treatment agent, powder flowability, storage stability, charge stability, and environmental stability can be improved, and the life of the developer can also be improved.
[0076] As the surface treatment agent, a conventionally known one can be used. For example, silica fine powder, titanium oxide fine powder, and hydrophobic products thereof can be mentioned. As the silica fine powder, wet silica, dry silica, a composite of dry silica and a metal oxide, etc. can be used, and further, those which have been hydrophobized with an organosilicon compound can be used. As the hydrophobization treatment, for example, a method of treating silica fine powder produced by vapor phase oxidation of a silicon halide compound with a silane compound and then with an organosilicon compound can be mentioned. Examples of silane compounds used in the hydrophobization treatment include hexamethyldisilazane, trimethylsilane, trimethylchlorosilane, trimethylethoxysilane, dimethyldichlorosilane, methyltrichlorosilane, allyldimethylchlorosilane, allylphenyldichlorosilane, benzyldimethylchlorosilane, bromomethyldimethylchlorosilane, α-chloroethyltrichlorosilane, β-chloroethyltrichlorosilane, chloromethyldimethylchlorosilane, triorganosilylmercaptan, trimethylsilylmercaptan, triorganosilylacrylate, vinyldimethylacetoxysilane, dimethyldiethoxysilane, dimethyldimethoxysilane, diphenyldiethoxysilane, hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane, and 1,3-diphenyltetramethyldisiloxane. Examples of organosilicon compounds used in the hydrophobic treatment include silicone oils such as dimethyl silicone oil, methylphenyl silicone oil, α-methylstyrene modified silicone oil, chlorophenyl silicone oil, fluorine modified silicone oil, etc. In addition, titanium oxide fine powder treated with oil, vinyl resin fine particles of 0.03 μm to 1 μm, etc. may also be used.
[0077] Other surface treatment agents that may be used include lubricants such as polyethylene fluoride, zinc stearate, and polyvinylidene fluoride, abrasives such as cerium oxide, silicon carbide, strontium titanate, magnetic powder, and alumina, and conductivity imparting agents such as carbon black, zinc oxide, antimony oxide, and tin oxide. Furthermore, the shape of the surface treatment agent may be small particles having a particle size of 100 nm or less, large particles having a particle size of 100 nm or more, and particles having various shapes such as octahedral, hexahedral, needle, and fibrous shapes. The surface treatment agents may be used alone or in combination of two or more kinds.
[0078] The amount of the surface treatment agent added is preferably 0.1 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, in 100 parts by mass of the toner.
[0079] When the toner according to the present embodiment is used as a two-component developer, a conventionally known carrier can be used. For example, particles having a number-average particle size of 15 to 300 μm made of metals such as iron, cobalt, manganese, chromium, copper, zinc, nickel, magnesium, lithium, and rare earths, which are surface-oxidized or unoxidized, and their alloys or oxides, can be used. These carriers may be surface-coated with styrene resins, acrylic resins, silicone resins, polyester resins, fluorine resins, etc. Furthermore, a magnetic carrier having a magnetic fine particle dispersion core in which magnetic fine particles are dispersed in a resin and a coating layer containing a coating resin that coats the surface of the magnetic fine particle dispersion core may be used.
[0080] The toner according to the present embodiment can be used in various known development processes. Examples include, but are not limited to, a cascade development method, a magnetic brush method, a powder cloud method, a touch-down development method, a so-called microtoning method in which a magnetic toner produced by a pulverization method is used as a carrier, and a so-called bipolar magnetic toner method in which a required toner charge is obtained by frictional charging between magnetic toners. The toner according to the present embodiment can also be used in various cleaning methods such as a conventionally known fur brush method and a blade method. The toner according to the present embodiment can also be used in various conventionally known fixing methods. Specific examples include an oil-less heat roll method, an oil-coated heat roll method, a heat belt fixing method, a flash method, an oven method, and a pressure fixing method. The toner according to the present embodiment may also be used in a fixing device that employs an electromagnetic induction heating method. Furthermore, the toner may also be used in an image forming method having an intermediate transfer process.
[0081] <Toner manufacturing method> Next, a method for producing the toner according to the present embodiment will be described. The toner production method according to the present embodiment includes a step of mixing the toner binder resin according to the present embodiment with a colorant. In the step of mixing the toner binder resin with a colorant, toner components other than the toner binder resin may also be mixed.
[0082] The toner according to the present embodiment is manufactured by mixing the binder resin for toner and a colorant using the binder resin for toner according to the present embodiment. The mixing method may be a conventionally known method. For example, the binder resin, the colorant, and, if necessary, the toner components such as a charge control agent are thoroughly mixed by a powder mixer such as a Henschel mixer, and then melt-kneaded using a kneader such as a twin-screw kneader or an open roll kneader to thoroughly mix each component. After cooling, the mixture is crushed and classified to collect particles usually in the range of 4 to 15 μm, and a surface treatment agent is applied by a powder mixing method to obtain a toner. The toner may be subjected to a spheroidizing treatment using a surface treatment device or the like. Examples of the surface treatment method include a method of making the toner spherical by making the toner flow into a high-temperature air jet, and a method of removing the corners of the toner by mechanical impact. For the purpose of improving image quality, the average circularity measured by a flow-type particle image analyzer (e.g., FPIA-3000 manufactured by Sysmex Corporation) may be adjusted to 0.960 or more by carrying out such surface treatment. In the method of making the toner into a spherical shape by making the toner flow into a high-temperature air jet, the toner particles are heated with hot air, preferably at a temperature of 200° C. or higher and 400° C. or lower.
[0083] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. Furthermore, the present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0084] Hereinafter, the present embodiment will be described in detail with reference to examples. Note that the present embodiment is not limited to the description of these examples. Furthermore, in the table, St represents styrene, Mac represents methacrylic acid, BA represents n-butyl acrylate, and GMA represents glycidyl methacrylate.
[0085] <Production of monoester compound> A four-neck flask was equipped with a reflux condenser, a water separator, a nitrogen gas inlet tube, a thermometer, and a stirrer, and the alcohol component and the carboxylic acid component (1.05 times the alcohol component) were charged into the four-neck flask according to the composition shown in Table 1. Under a nitrogen gas flow, the internal temperature of the four-neck flask was kept at 220°C, and the reaction was carried out at normal pressure for 15 hours while removing water generated by the reaction, to obtain a crude product.
[0086] 20 parts by mass of toluene and 6 parts by mass of ethanol were added to 100 parts by mass of the obtained crude product. A 10% aqueous solution containing potassium hydroxide in an amount 1.5 times the acid value of the crude product was added, and the mixture was stirred at 70° C. for 30 minutes. After that, the mixture was left to stand for 30 minutes, and the aqueous layer was removed to deacidify.
[0087] Next, 20 parts by mass of ion-exchanged water was added to 100 parts by mass of the crude product, and the mixture was stirred at 70°C for 30 minutes. After that, the mixture was left to stand for 30 minutes, and the aqueous layer was removed. This water washing was repeated four times. The remaining ester layer was heated at 180°C and a reduced pressure of 1 kPa to remove the solvent. As a result, monoester compounds W1 to W4 were obtained.
[0088] [Table 1]
[0089] [Production of low molecular weight vinyl resin (L)] (L-1) 75 parts by mass of xylene was charged into a flask purged with nitrogen and heated. Under reflux of xylene, a mixed solution in which 5 parts by mass of t-butylperoxy-2-ethylhexanoate were mixed and dissolved in 100 parts by mass of the monomer shown in Table 2 was continuously added over 5 hours. Then, reflux was continued for another hour. Thereafter, the temperature inside the flask was maintained at 98° C., and 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was further added and the reaction was continued for 2 hours to obtain a polymerization liquid of L-1.
[0090] (L-2) 100 parts by mass of xylene was placed in a flask purged with nitrogen and heated. Under reflux of xylene, a mixed solution in which 100 parts by mass of the monomers shown in Table 2 were mixed and dissolved with 10 parts by mass of t-butylperoxy-2-ethylhexanoate was continuously added over 5 hours. Then, reflux was continued for another hour. Thereafter, the temperature inside the flask was maintained at 98° C., and 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was further added and the reaction was continued for 2 hours to obtain a polymerization liquid L-2.
[0091] (L-3) 75 parts by mass of xylene was charged into a flask purged with nitrogen and heated. Under reflux of xylene, a mixed solution in which 100 parts by mass of the monomer shown in Table 2 was mixed and dissolved with 2 parts by mass of t-butylperoxy-2-ethylhexanoate was continuously added over 5 hours. Then, reflux was continued for another hour. Thereafter, the temperature inside the flask was maintained at 98° C., and 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was further added and the reaction was continued for 2 hours to obtain a polymerization liquid L-3.
[0092] (L-4) 50 parts by mass of xylene was placed in a flask purged with nitrogen and heated. Under reflux of xylene, a mixed solution in which 100 parts by mass of the monomers shown in Table 2 were mixed and dissolved with 1.8 parts by mass of t-butylperoxy-2-ethylhexanoate was continuously added over 5 hours. Then, reflux was continued for another hour. Thereafter, the temperature inside the flask was maintained at 98° C., and 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was further added and the reaction was continued for 2 hours to obtain a polymerization liquid L-4.
[0093] [Table 2]
[0094] [Production of high molecular weight vinyl resin (H)] (H-1) 40 parts by mass of xylene was placed in a flask purged with nitrogen and heated. A mixed liquid prepared by mixing and melting 100 parts by mass of the monomers shown in Table 3 and 0.5 parts by mass of di-t-butyl peroxide was added continuously over 5 hours under reflux of xylene, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 130° C., 0.5 parts by mass of di-t-butyl peroxide was added, and the reaction was continued for 1 hour. Further, 0.5 parts by mass of di-t-butyl peroxide was added, and the reaction was continued for 1 hour to obtain a polymer H-1.
[0095] (H-2) 50 parts by mass of xylene was placed in a flask purged with nitrogen and heated. A mixed liquid in which 100 parts by mass of the monomers shown in Table 3 and 1 part by mass of t-butylperoxy-2-ethylhexanoate were mixed and melted was continuously added over 5 hours under reflux of xylene, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 98° C., 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 1 hour. Further, 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 2 hours to obtain a polymer of H-2.
[0096] (H-3) 20 parts by mass of xylene was placed in a flask purged with nitrogen and heated. A mixed liquid in which 100 parts by mass of the monomers shown in Table 3 and 1.8 parts by mass of t-butylperoxy-2-ethylhexanoate were mixed and melted was continuously added over 5 hours under reflux of xylene, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 98° C., 0.3 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 1 hour. Then, 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 2 hours to obtain a polymer of H-3.
[0097] (H-4) 50 parts by mass of xylene was placed in a flask purged with nitrogen and heated. A mixed liquid in which 100 parts by mass of the monomers shown in Table 3 and 1.8 parts by mass of t-butylperoxy-2-ethylhexanoate were mixed and melted was added continuously over 5 hours under reflux of xylene, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 98° C., 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 1 hour. Further, 0.5 parts by mass of t-butylperoxy-2-ethylhexanoate was added, and the reaction was continued for 2 hours to obtain a polymer H-4.
[0098] (H-5) 69 parts by mass of styrene, 23 parts by mass of butyl acrylate, and 15 parts by mass of xylene were charged into a flask purged with nitrogen, and the temperature inside the flask was raised to 110° C. A mixed solution containing 5 parts by mass of styrene, 3 parts by mass of methacrylic acid, 85 parts by mass of xylene, and 0.3 parts by mass of t-butylperoxy-2-ethylhexanoate was continuously added thereto over a period of 7 hours, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 130° C., 0.1 parts by mass of di-t-butyl peroxide was added, and the reaction was continued for 2 hours. Further, 0.1 parts by mass of di-t-butyl peroxide was added, and the reaction was continued for 2 hours to obtain a mixed solution H-5.
[0099] [Table 3]
[0100] <Production of glycidyl group-containing vinyl resin (E)> 50 parts by mass of xylene was placed in a flask purged with nitrogen and heated. Under reflux of xylene, a mixed solution prepared by mixing and dissolving 100 parts by mass of the monomers shown in Table 4 and 0.5 parts by mass of di-t-butyl peroxide was continuously added over 5 hours, and reflux was continued for another hour. Thereafter, the temperature inside the flask was kept at 130° C., 0.5 parts by mass of di-t-butyl peroxide was added, and the reaction was continued for 2 hours to obtain a polymerization liquid, which was then flushed in a vessel at 160° C. and 1.33 kPa to distill off the solvent and the like to obtain a resin (E).
[0101] [Table 4]
[0102] <Release agent> As the release agent other than the monoester compound, the waxes shown in Table 5 were used.
[0103] [Table 5]
[0104] <Production of Carboxy Group-Containing Vinyl Resin (C)> Using the release agent shown in Table 5, the monoester compound (W), the high molecular weight vinyl resin (H), and the low molecular weight vinyl resin (L) were mixed to obtain the composition shown in Table 6. Then, the mixture was mixed for 30 minutes under xylene reflux. This was flushed in a vessel at 190°C and 1.33 kPa to distill off the solvent, etc., to obtain resin (C).
[0105] [Table 6]
[0106] <Production of binder resin (R)> The components were mixed so that the mass ratio of the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E) was the ratio shown in Table 7. Then, a kneading reaction was performed at 25 kg / hr and a motor rotation speed of 1400 rpm in a twin-shaft kneader (KEXN S-40 type, manufactured by Kurimoto Iron Works) set to the reaction temperature shown in Table 7, to obtain a kneaded product. This kneaded product was quenched using a steel belt cooler (NR3-Hi double cooler, manufactured by Nippon Belting) under the conditions of a cooling water temperature of 10°C, a cooling water amount of 90 L / min, and a belt speed of 6 m / min. Then, the mixture was pulverized to obtain a binder resin (R).
[0107] [Table 7]
[0108] <Toner (T) Production> To 100% by mass of the binder resin shown in Table 8, 6% by mass of carbon black (MA100; manufactured by Mitsubishi Chemical) as a colorant and 0.5% by mass of a charge control agent (T-77; manufactured by Hodogaya Chemical Industry Co., Ltd.) were added and mixed in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.). After that, the mixture was kneaded in a twin-screw extruder (PCM-30 type; manufactured by Ikegai Kikai) at a resin temperature of 110°C at the discharge port of the twin-screw kneader and a residence time of 30 seconds. After cooling, pulverization, and classification, 1% by mass of hydrophobic silica fine powder (R-812; manufactured by Nippon Aerosil) was added to 100% by mass of toner particles (T) and mixed in a Henschel mixer (manufactured by Nippon Coke and Kogyo Co., Ltd.). As a result, toners T-1 to T-34 with a volume median diameter D50 of about 7.5 μm were obtained, as measured with a Coulter Counter (manufactured by Beckman Coulter).
[0109] [Table 8]
[0110] <Evaluation> The obtained toners T-1 to T-34 were evaluated by the following methods. The obtained evaluation results are also shown in Table 8.
[0111] [Fixing offset evaluation] Unfixed images were created using a commercially available electrophotographic copier that was modified. The amount of toner attached to the paper was 0.5 mg / cm 2 An unfixed toner image was output, and the image was removed from the fixing section of the copying machine. The fixing member was adjusted so that the surface temperature of the fixing member could be measured with a non-contact thermometer, to prepare a heating belt type fixing test machine. When the temperature of the fixing member was increased from 90°C to 200°C in 5°C increments, the unfixed toner image was passed through a fixing tester at 150 mm / sec to fix the toner. The presence or absence of fusion of the toner to the fixing member was visually confirmed. The environmental conditions were a temperature of 22°C and a relative humidity of 55%. The temperature range in which the toner does not melt and adhere to the fixing member is defined as the offset-resistant temperature range, and the lower limit temperature on the low temperature side is defined as the low-temperature fixing temperature.
[0112] [Fixation strength evaluation] The temperature of the fixing member was set to 140°C, and a fixed image of the toner was obtained in the same manner as in the fixing offset evaluation method. The image density of the resulting fixed image was measured with a Macbeth reflection densitometer (RD918), and then the portion where the image density was measured was bent crosswise, and the toner peeled off from the paper was removed with a brush, and the image density was measured again. The fixing strength was calculated using the following formula.
[0113] Fixing strength={(image density after folding)÷(image density before folding)}×100
[0114] [Gloss rating] A fixed image of the toner was obtained in the same manner as in the fixing offset evaluation method, with the temperature of the fixing member set to 150° C. The 75° gloss of the resulting fixed image was measured with a gloss meter (GM-3D; manufactured by Murakami Color Research Laboratory).
[0115] As is clear from the results in Table 8, all of the toners produced in this example were excellent in low-temperature fixing property, offset resistance, and fixing strength.
Claims
1. A carboxyl group-containing vinyl resin (C); A glycidyl group-containing vinyl resin (E); a reaction product of the carboxyl group-containing vinyl resin (C) and the glycidyl group-containing vinyl resin (E); A toner binder resin comprising a monoester compound obtained from a linear saturated aliphatic monocarboxylic acid and a monohydric linear saturated aliphatic alcohol, At least one release agent other than the monoester compound is included, The monovalent linear saturated aliphatic alcohol is one or more selected from the group consisting of methanol, ethanol, propanol, butanol, pentanol, octanol, nonanol, decanol, laurinol, myristinol, pentadecinol, palmitinol, margarinol, stearyl alcohol, arachidinol and behenyl alcohol.
2. The carboxyl group-containing vinyl resin (C), The glycidyl group-containing vinyl resin (E), The binder resin for toner according to claim 1 , wherein the monoester compound is contained in an amount of 4% by mass to 15% by mass, based on 100% by mass of the total of the monoester compound and the reactants.
3. 3. The binder resin for toner according to claim 1, wherein the release agent other than the monoester compound is one or more release agents selected from the group consisting of polyethylene wax, polypropylene wax, Fischer-Tropsch wax, paraffin wax, carnauba wax, and ester waxes having two or more ester bonds.
4. 4. The toner binder resin according to claim 1, wherein the release agent other than the monoester compound is contained in an amount of 2% by mass or more and 8% by mass or less based on the entire toner binder resin.
5. The carboxyl group-containing vinyl resin (C) has a molecular weight distribution of tetrahydrofuran soluble matter measured by gel permeation chromatography, which is Molecular weight is 2.5 x 10 4 Above 1.2 x 10 5 A high molecular weight vinyl resin (H) having a peak in the following region: Molecular weight is 2.0 x 10 3 Above 2.0 x 10 4 and a low molecular weight vinyl resin (L) having a peak in the following region:
5. The toner binder resin according to claim 1, wherein a mass ratio (H / L) of the high molecular weight vinyl resin (H) to the low molecular weight vinyl resin (L) is 55 / 45 to 85 / 15.
6. The binder resin for toner according to any one of claims 1 to 5, comprising a fatty acid metal salt represented by the following general formula (1): In the above general formula (1), n is an integer of 11 to 22, m is 2, and M is a metal atom selected from Zn and Ca.
7. 7. The binder resin for toner according to claim 1, wherein the tetrahydrofuran insoluble component in the binder resin for toner is 10% by mass to 40% by mass based on the entire binder resin.
Citation Information
Patent Citations
Process for producing toner, and toner
JP2005266788A
toner
JP2010191218A
Toner and image forming method
JP4266658B2
Process for producing toner, and toner
US20080014522A1
Binder Resin for Color Toners and Color Toner Using the Same
US20100209837A1