Reflective mask blank and method for manufacturing a reflective mask

The reflective mask blank design with a varying oxygen content metal oxide film and oxidation suppressing layer addresses the reflectance loss issue during heat treatment, maintaining high reflectance and stability in EUV lithography processes.

JP7590915B2Active Publication Date: 2024-11-27SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021077133
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-30
Publication Date
2024-11-27
Estimated Expiration
2041-04-30

AI Technical Summary

Technical Problem

Reflective mask blanks experience a significant reduction in reflectance due to the formation of a RuSi diffusion layer at the interface between the Ru film and the Si film during heat treatment, which is exacerbated by oxygen penetration through a thin buffer layer, leading to oxidation and decreased performance.

Method used

A reflective mask blank design featuring a multilayer reflective film with a metal oxide film having varying oxygen content, where the oxygen content increases away from the substrate, and an oxidation suppressing layer to prevent reflectance loss during heat treatment, utilizing materials like Zr, Nb, Ti, and Y with an extinction coefficient less than 0.02 for EUV light, and a thickness of 0.5 nm to 3.5 nm.

Benefits of technology

Maintains high reflectance with minimal decrease even after heat treatment at 120 to 200°C, ensuring stable performance and reducing etching rates during absorber film processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590915000001
    Figure 0007590915000001
  • Figure 0007590915000002
    Figure 0007590915000002
  • Figure 0007590915000003
    Figure 0007590915000003
Patent Text Reader

Abstract

To provide a reflective mask blank that barely shows a decrease in reflectance even when subjected to a heat treatment, maintaining a high reflectance, and a method for producing a reflective mask using the reflective mask blank.SOLUTION: A reflective mask blank has a substrate 10; a multilayer reflective film 20 that is provided on the substrate 10 and reflects exposure light; a protective film 50 provided on the multilayer reflective film 20 and including a metal oxide film 51; and an absorber film 70 that is provided on the protective film 50 and absorbs exposure light. The multilayer reflective film 20 is configured such that: a Mo layer 22 and a Si layer 21 are alternately stacked, where the Si layer 21 is a layer on the side farthest from the substrate 10. The metal oxide film 51 is configured such that: the layer on the side remote from the substrate 10 has a higher oxygen content than that of the substrate-side layer.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask blank for producing a reflective mask used in the manufacture of semiconductor devices and the like, and a method for producing a reflective mask. [Background technology]

[0002] In the manufacturing process of semiconductor devices (semiconductor device), photolithography technology is repeatedly used, in which exposure light is irradiated onto a transfer mask, and the circuit pattern formed on the mask is transferred onto a semiconductor substrate (semiconductor wafer) via a reduced projection optical system. Conventionally, the wavelength of the exposure light has mainly been 193 nm using argon fluoride (ArF) excimer laser light, and a process called multi-patterning, which combines exposure processes and processing processes multiple times, has been used to ultimately form patterns with dimensions smaller than the exposure wavelength.

[0003] However, as device patterns continue to become finer, there is a need to form even finer patterns, and so EUV lithography technology, which uses extreme ultraviolet (EUV) light with an even shorter wavelength than ArF excimer laser light as exposure light, has come to be used. EUV light is light with a wavelength of about 0.2 to 100 nm, and more specifically, light with a wavelength of about 13.5 nm. This EUV light has extremely low transparency to materials, so that conventional transmission type projection optical systems and masks cannot be used, and therefore reflective optical elements are used. For this reason, reflective masks have been proposed as masks for pattern transfer.

[0004] A reflective mask is a mask in which a multilayer reflective film that reflects EUV light is formed on a substrate, and an absorber film that absorbs EUV light is formed in a pattern on the multilayer reflective film. On the other hand, a mask in a state before patterning the absorber film (including a state in which a resist film is formed) is called a reflective mask blank, and this is used as a material for a reflective mask (hereinafter, a reflective mask blank that reflects EUV light is also called an EUV mask blank). An EUV mask blank has a basic structure including a multilayer reflective film that reflects EUV light formed on a glass substrate, and an absorber film that absorbs EUV light formed thereon. As the multilayer reflective layer, a Mo / Si multilayer reflective film that ensures the reflectance of EUV light by alternately stacking molybdenum (Mo) layers and silicon (Si) layers is usually used. On the other hand, as the absorber film, a material mainly composed of tantalum (Ta), which has a relatively large extinction coefficient value for EUV light, is used.

[0005] Between the multilayer reflective film and the absorber film, a protective film for protecting the multilayer reflective film is formed. This protective film is intended to protect the multilayer reflective film from damage due to etching performed for the purpose of forming a pattern on the absorber film, pattern correction processing when defects are detected after pattern formation, and further, mask cleaning after mask pattern formation. As disclosed in JP-A-2002-122981 (Patent Document 1), ruthenium (Ru) is used as this protective film. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2002-122981 A Summary of the Invention [Problem to be solved by the invention]

[0007] Reflective mask blanks are generally made by forming a protective film mainly composed of Ru on a multilayer reflective film (multilayer periodic film) in which Mo layers and Si layers are alternately stacked, with the outermost layer being Si, and then performing a heat treatment at a temperature range of 120 to 200°C to stabilize the subsequent processes.

[0008] However, in the combination of a protective film containing Ru and a multilayer reflective film with a Si surface layer, a RuSi diffusion layer is formed by heat treatment, which tends to significantly reduce the reflectance. In order to prevent the formation of a diffusion layer at the interface between the Ru film and the Si film by heat treatment, a configuration in which a Mo film or the like is formed as a buffer layer between the Ru film and the Si film has been considered. However, the protective film is thin and easily permeable to oxygen, and the buffer layer itself may be oxidized, which may cause a significant decrease in reflectance. If the protective film is made of a metal oxide film with a high oxygen content in advance, it is possible to suppress the reflectance fluctuation due to heat treatment, but there is a risk that the surface layer of the multilayer reflective film may be oxidized more than necessary when stacking, which may result in a significant decrease in reflectance.

[0009] The present invention has been made in consideration of these points, and provides a reflective mask blank that maintains high reflectance with little decrease in reflectance even when subjected to heat treatment, and a method for manufacturing a reflective mask using the reflective mask blank. [Means for solving the problem]

[0010] The reflective mask blank according to the present invention comprises: A substrate; a multilayer reflective film provided on the substrate and configured to reflect exposure light; a protective film including a metal oxide film provided on the multilayer reflective film; an absorber film provided on the protective film and configured to absorb exposure light; Equipped with the multilayer reflective film is formed by alternately laminating Mo layers and Si layers, and the layer furthest from the substrate is the Si layer; The metal oxide film may have a higher oxygen content in a layer on a side away from the substrate than in a side on the substrate.

[0011] In the reflective mask blank according to the present invention, The metal contained in the metal oxide film may be a metal having an extinction coefficient k of less than 0.02 for EUV light having a wavelength of 13.53 nm.

[0012] In the reflective mask blank according to the present invention, The protective film may function as an etching stopper when processing the absorber film.

[0013] In the reflective mask blank according to the present invention, The metal oxide film may contain one or more of the elements Zr, Nb, Ti and Y.

[0014] In the reflective mask blank according to the present invention, The oxygen content of the layer of the metal oxide film on the side away from the substrate may not change upon heat treatment at 120°C to 200°C.

[0015] In the reflective mask blank according to the present invention, The thickness of the metal oxide film may be 0.5 nm or more and less than 3.5 nm.

[0016] In the reflective mask blank according to the present invention, The metal oxide film has a multi-layer structure, The oxygen content may be higher in a second layer located on a side away from the substrate than in a first layer located on the substrate side.

[0017] In the reflective mask blank according to the present invention, The oxygen content of the metal oxide film may increase continuously with distance from the substrate.

[0018] In the reflective mask blank according to the present invention, The Si layer of the multilayer reflective film that is farthest from the substrate may contain a light element other than oxygen on the metal oxide film side.

[0019] In the reflective mask blank according to the present invention, an oxidation prevention layer including a light element other than oxygen on the metal oxide film side between the Si layer of the multilayer reflective film farthest from the substrate and the metal oxide film; The oxidation prevention layer may have a thickness of 0.2 nm or more and 3 nm or less.

[0020] In the reflective mask blank according to the present invention, The light element may be one or more of nitrogen, carbon, and boron.

[0021] In the reflective mask blank according to the present invention, When a first reflectance for EUV light having a wavelength of 13.53 nm before heat treatment at 120 to 200° C. is compared with a second reflectance for EUV light having a wavelength of 13.53 nm after heat treatment at 120 to 200° C., a change in the second reflectance from the first reflectance may be 0.5% or less.

[0022] In the method for producing a reflective mask according to the present invention, A reflective mask may be manufactured using the above-described reflective mask blank. Effect of the Invention

[0023] According to one aspect of the present invention, a reflective mask blank can be realized which exhibits little decrease in reflectance even when heat treatment is performed and which maintains a high reflectance. [Brief description of the drawings]

[0024] [Figure 1A] FIG. 1 is a cross-sectional view showing an example of a reflective mask blank according to an embodiment of the present invention. [Figure 1B] FIG. 2 is a cross-sectional view showing another example of a reflective mask blank according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating an example of a reflective mask blank having a SiN-containing layer according to an embodiment of the present invention. [Figure 3A]1 is a cross-sectional view showing an example of a protective film having a multi-layer structure used in an embodiment of the present invention. [Figure 3B] 11 is a cross-sectional view showing another example of a protective film having a multi-layer structure used in an embodiment of the present invention. FIG. [Figure 4] FIG. 2 is a cross-sectional view showing the oxygen content in an example of a protective film used in an embodiment of the present invention. [Diagram 5] FIG. 11 is a cross-sectional view showing the oxygen content in another example of a protective film used in an embodiment of the present invention. [Figure 6] FIG. 2 is a cross-sectional view showing an example of a reflective mask blank having an oxidation inhibition layer, a hard mask film, a reflectance reduction layer, and a conductive film according to an embodiment of the present invention. [Figure 7] FIG. 2 is a cross-sectional view showing an example of a reflective mask blank having an oxidation inhibition layer, a buffer layer, a hard mask film, and a conductive film according to an embodiment of the present invention. [Figure 8] FIG. 2 is a cross-sectional view showing an example of a reflective mask blank having a resist film according to an embodiment of the present invention. [Figure 9] 1 is a cross-sectional view showing an example of a reflective mask according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The present invention will now be described.

[0026] 1A and 1B, the EUV mask blank according to the present embodiment includes a substrate 10 made of glass or the like, and a multilayer reflective film 20 formed on the substrate 10 (on one main surface, in this embodiment, on the front surface) for reflecting exposure light, specifically, a multilayer reflective film 20 for reflecting EUV light. The multilayer reflective film 20 may be provided in contact with one main surface of the substrate 10. The wavelength of EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, and is usually light having a wavelength of about 13.5 nm (for example, 13.4 to 13.6 nm).

[0027] The substrate 10 preferably has low thermal expansion characteristics for use in EUV light exposure, and has a thermal expansion coefficient of, for example, ±2×10 -8 / ℃, preferably within ±5×10 -9 / °C. The substrate 10 used is preferably one having a sufficiently flat surface, and the surface roughness of the main surface of the substrate 10 is preferably 0.5 nm or less, particularly 0.2 nm or less, in terms of RMS value. Such a surface roughness can be obtained by polishing the substrate 10, or the like.

[0028] The multilayer reflective film 20 is a multilayer film in which low refractive index materials and high refractive index materials are alternately laminated, and is a film that reflects EUV light, which is exposure light. In this embodiment, the multilayer reflective film 20 has a Si / Mo laminated portion 25 composed of a multilayer in which Si (silicon) layers 21 and Mo (molybdenum) layers 22 are alternately laminated. The Si / Mo laminated portion 25 uses a layer of Si (Si layer 21) that is a material having a relatively high refractive index to EUV light and a layer of Mo (Mo layer 22) that is a material having a relatively low refractive index to EUV light, which are periodically laminated. Here, the Si layer 21 and the Mo layer 22 may be layers formed of simple silicon and simple molybdenum, respectively, or may contain other components at less than 10%. The number of layers of the Si layer 21 and the Mo layer 22 is preferably, for example, 40 periods or more (40 layers or more for each) and preferably 60 periods or less (60 layers or less for each). The thicknesses of the Si layer 21 and Mo layer 22 of the Si / Mo laminated portion 25 are appropriately set according to the exposure wavelength, and the thickness of the Si layer 21 is preferably 5 nm or less, and the thickness of the Mo layer 22 is preferably 4 nm or less. The lower limit of the thickness of the Si layer 21 is not particularly limited, but is usually 1 nm or more. The lower limit of the thickness of the Mo layer 22 is not particularly limited, but is usually 1 nm or more. The thicknesses of the Si layer 21 and Mo layer 22 may be set so as to obtain a high reflectance to EUV light. The thicknesses of the Si layer 21 and Mo layer 22 may be constant or may differ from one layer to another. The total thickness of the Si / Mo laminated portion 25 is usually about 250 to 450 nm.

[0029] The inventors of the present application have found that by increasing the oxygen content of the protective film 50 on the side away from the multilayer reflective film 20, oxidation of the film can be prevented, and by further decreasing the oxygen content of the layer in contact with the surface Si layer of the multilayer reflective film 20, oxidation of the multilayer reflective film 20 due to heat can be prevented, and that even when a heat treatment at 120 to 200° C. is performed after the formation of the multilayer reflective film 20, a reflective mask blank with little decrease in reflectance and maintaining high reflectance can be produced, leading to the invention. It has also been confirmed that it is particularly preferable for the protective film 50 to be made of a metal oxide film 51 having an extinction coefficient k of 0.02 or less for EUV light (13.53 nm), such as Zr, Nb, Ti, or Y.

[0030] In this embodiment, the Si / Mo laminated portion 25 may be formed such that a layer containing Si and N is formed in contact with both the Si layer 21 and the Mo layer 22 at one or more positions between the Si layer 21 and the Mo layer 22. The layer containing Si and N preferably does not contain oxygen. Specifically, the layer containing Si and N is preferably a SiN (here, SiN means that the constituent elements are only Si and N) layer (SiN-containing layer 26) (see FIG. 2). The N content of the layer containing Si and N is preferably 1 atomic % or more, particularly 5 atomic % or more, and is preferably 60 atomic % or less, particularly 57 atomic % or less. The thickness of the layer containing Si and N is preferably 2 nm or less, more preferably 1 nm or less. The lower limit of the thickness of the layer containing Si and N is not particularly limited, but is preferably 0.1 nm or more.

[0031] In this embodiment, the layer of the multilayer reflective film 20 that is farthest from the substrate 10 is the Si layer 21. The protective film 50 provided on the Si layer 21 may be a metal oxide film 51 made of a metal having an extinction coefficient k of EUV light (13.53 nm) of less than 0.02. By using a metal having an extinction coefficient k of less than 0.02 for the protective film, it is possible to suppress a reduction in reflectance due to the formation of the protective film. The protective film 50 may also include a film (for example, a metal film or a resin film) other than the metal oxide film 51. The oxygen content may be different in the metal oxide film 51. The oxygen content of the layer on the side of the metal oxide film 51 that is farther from the substrate 10 may be higher than that on the substrate 10 side. The metal oxide film 51 may include one or more elements of Zr, Nb, Ti, and Y. By adopting such an embodiment, a high reflectance can be obtained, and the etching rate during etching of the absorber film 70 on the side farther from the substrate 10 can be further reduced. Therefore, the protective film 50 functions as an etching stopper when the absorber film 70 is processed.

[0032] The oxygen content of the layer of the metal oxide film 51 on the side separated from the substrate 10 (typically the most distant Si layer 21a, which is the Si layer 21 most distant from the substrate 10) is preferably a stable layer with no change in oxygen content even when heat treatment is applied from 120°C to 200°C, particularly an oxygen-saturated state. Here, "no change in oxygen content even when heat treatment is applied from 120°C to 200°C" means that when comparing the state before heat treatment from 120°C to 200°C (first state) with the state after heat treatment from 120°C to 200°C (second state), the oxygen content in the second state is 95 atomic % or more of the oxygen content in the first state. When an oxygen-unsaturated layer is provided near the interface with the multilayer reflective film 20, it is possible to create a film with little reflectance fluctuation after heat treatment of the substrate and maintaining a high reflectance. The thickness of such an oxide layer is preferably 0.5 nm or more, particularly 1 nm or more, and less than 3.5 nm, particularly 3 nm or less, and further 2 nm or less.

[0033] As shown in Fig. 3A and Fig. 3B, the protective film 50 may have a multi-layer structure, and may be formed by stacking a plurality of metal oxide layers 55. The oxygen content of a certain metal oxide layer 55 located on the side separated from the substrate 10 may be higher than that of another metal oxide layer 55 located on the side separated from the substrate 10. For example, the oxygen content of the metal oxide layer 55 located on the side separated from the substrate 10 is equal to or lower than that of the metal oxide layer 55 located on the side separated from the substrate 10. As an example, the oxygen content of another metal oxide layer (second metal oxide layer) 55 located on the side separated from the substrate 10 is higher than that of a certain metal oxide layer (first metal oxide layer) 55 located on at least one substrate 10 side.

[0034] The oxygen content of the protective film 50 may be increased continuously as it is separated from the substrate 10 (see FIG. 4). The oxygen content contained in the metal oxide layer 55 may be increased stepwise as it is separated from the substrate 10 (see FIG. 5). As an example of an embodiment in which the oxygen content contained in the metal oxide layer 55 increases stepwise as it is separated from the substrate 10, the protective film 50 may have a multi-layer structure as shown in FIG. 3A. The increase may be in units of 1 atomic % to 10 atomic %. As shown in FIG. 3B, only two layers of the protective film 50 may be provided, and the oxygen content of the protective film 50 located on the side separated from the plate 10 may be higher than that of the protective film 50 located on the substrate 10 side. The difference in oxygen content in the protective film 50 may be about 15 atomic % to 50 atomic %. In other words, if the oxygen content of the protective film 50 closest to the substrate 10 is A and the oxygen content of the protective film 50 closest to the substrate 10 is B, then A×1.15≦B≦A×1.5 may be satisfied.

[0035] In addition, the Si layer 21 (the farthest Si layer 21a) of the multilayer reflective film 20 that is farthest from the substrate 10 may contain a light element other than oxygen on the metal oxide layer 55 side. In addition, an oxidation suppression layer 60 containing a light element other than oxygen may be provided on the metal oxide layer 55 side between the Si layer 21 (the farthest Si layer 21a) of the multilayer reflective film 20 that is farthest from the substrate 10 and the protective film 50 (see FIG. 6). The light element may be nitrogen, carbon, boron, or the like, and may be a light element other than oxygen. By adopting such an embodiment, oxidation of the surface layer Si can be reduced during the formation of the protective film 50 made of the metal oxide film 51, etc., and a high reflectance can be maintained. The thickness of the oxidation suppression layer 60 is preferably 0.2 nm or more and 3 nm or less. In this embodiment, the light element means an element that is heavier than oxygen. Furthermore, both the oxidation prevention layer 60 and the buffer layer 140 such as the SiN-containing layer 26 may be provided between the separating Si layer 21a and the protective film 50 (see FIGS. 2 and 7).

[0036] In a laminate of the multilayer reflective film 20 and the protective film 50 on the substrate 10, when a first reflectance for EUV light (13.53 nm) before heat treatment at 120 to 200°C is compared with a second reflectance for EUV light (13.53 nm) after heat treatment at 120 to 200°C, the change in the second reflectance from the first reflectance may be 0.5% or less.

[0037] A reflective mask as shown in FIG. 9 can be manufactured using the reflective mask blank of this embodiment, and this embodiment also provides a method for manufacturing a reflective mask.

[0038] The method of forming the Si / Mo laminated portion 25 includes a sputtering method in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and sputtering is performed, and an ion beam sputtering method in which an ion beam is irradiated onto the target. Examples of the sputtering method include a DC sputtering method in which a direct current voltage is applied to the target, and an RF sputtering method in which a high frequency voltage is applied to the target. The sputtering method is a film formation method in which a voltage is applied to the target with a sputtering gas introduced into a chamber, the gas is ionized, and the sputtering phenomenon caused by the gas ions is utilized, and the magnetron sputtering method is particularly advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering in which a negative bias applied to the target is reversed for a short period of time to prevent the target from being charged up.

[0039] The Si / Mo stacked portion 25 can be formed by a sputtering method using, for example, a sputtering device capable of mounting multiple targets. Specifically, a silicon (Si) target for forming the Si layer 21 and a molybdenum (Mo) target for forming the Mo layer 22 are used. When forming the Si layer 21 and the Mo layer 22, a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, xenon (Xe) gas, etc. is used as the sputtering gas, and the Si target and the Mo target are sequentially sputtered to sequentially form the Si layer 21 and the Mo layer 22.

[0040] The metal oxide layer 55 can be formed by, for example, ion beam sputtering or magnetron sputtering, similarly to the multilayer reflective film 20. The metal oxide layer 55 can be formed by sputtering using the metal material used for the protective film 50 as a target and a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas, and, if necessary, a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas.

[0041] The EUV mask blank of this embodiment may have an absorber film 70 formed on the protective film 50 to absorb the exposure light. More specifically, an absorber film 70 that absorbs EUV light and reduces reflectance may be provided. The absorber film 70 is preferably provided in contact with the metal oxide layer 55. A conductive film 120 used for electrostatically chucking the EUV mask to an exposure device may be provided in contact with the other main surface (rear surface) of the substrate 10, which is the surface opposite to the one main surface, preferably the other main surface. In this embodiment, the one main surface of the substrate 10 is the front surface and the upper side, and the other main surface is the rear surface and the lower side, but the front and back and the top and bottom of both are determined for convenience. The one main surface and the other main surface are either of the two main surfaces (film formation surfaces) of the substrate 10, and the front and back and the top and bottom are interchangeable.

[0042] As described above, the buffer layer 140, which is a base film, may be provided between the most distant Si layer 21a and the protective film 50 (see FIG. 7). When the SiN-containing layer 26 is provided between the most distant Si layer 21a of the Si / Mo stacked portion 25 and the protective film 50 (metal oxide film 51), the SiN-containing layer 26 may function as a buffer layer (see FIG. 2). The buffer layer 140 may be made of a metal that is difficult to oxidize, such as Ru, or C, B4C, or the like.

[0043] From the EUV mask blank (mask blank for EUV exposure), an EUV mask (mask for EUV exposure) having an absorber pattern (pattern of the absorber film 70) formed by patterning the absorber film 70 is manufactured (see FIG. 9). The EUV mask blank and the EUV mask are a reflective mask blank and a reflective mask.

[0044] The absorber film 70 is a film formed on the multilayer reflective film 20, and absorbs the EUV light, which is the exposure light, to reduce the reflectance of the exposure light. In the EUV mask, a transfer pattern is formed due to the difference in reflectance between a portion where the absorber film 70 is formed and a portion where the absorber film 70 is not formed.

[0045] The material of the absorber film 70 is not limited as long as it absorbs EUV light and can be patterned. Examples of the material of the absorber film 70 include materials containing tantalum (Ta) or chromium (Cr). The material containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), or the like. Examples of the material containing Ta include a simple Ta element, and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of the material containing Cr include a simple Cr element, and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0046] The absorber film 70 can be formed by sputtering, and magnetron sputtering is preferable for sputtering. Specifically, metal targets such as chromium (Cr) targets and tantalum (Ta) targets, and metal compound targets such as chromium compound targets and tantalum compound targets (targets containing metals such as Cr and Ta and oxygen (O), nitrogen (N), carbon (C), boron (B), etc.) can be used. In addition, rare gases such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, and xenon (Xe) gas can be used as sputtering gas, and the absorber film 70 can be formed by reactive sputtering using a rare gas together with a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas.

[0047] A hard mask film 110 (an etching mask film for the absorber film 70) having etching characteristics different from those of the absorber film 70 may be provided on the side of the absorber film 70 away from the substrate 10, preferably in contact with the absorber film 70 (see Figs. 6 and 7). The hard mask film 110 functions as an etching mask when the absorber film 70 is dry-etched. After the absorber pattern is formed, the hard mask film 110 may be left as a reflectance reducing layer for reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection, and may be removed so as not to remain on the EUV mask. Materials for the hard mask film 110 include materials containing chromium (Cr). The hard mask film 110 formed of a material containing Cr is particularly suitable when the absorber film 70 is formed of a material containing Ta and not containing Cr. A layer (reflectance reduction layer) 160 that mainly serves the function of reducing the reflectance at the wavelength of light used in inspections such as pattern inspections may be formed on the absorber film 70 (see FIG. 6), and in this case, the hard mask film 110 may be formed on the reflectance reduction layer 160. The hard mask film 110 may be formed by, for example, a magnetron sputtering method. The thickness of the hard mask film 110 is not particularly limited, but is usually about 5 to 20 nm.

[0048] The conductive film 120 provided on the back side preferably has a sheet resistance of 100Ω / □ or less, and there is no particular restriction on the material. Examples of the material of the conductive film 120 include materials containing tantalum (Ta) or chromium (Cr). In addition, the material containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), etc. Examples of the material containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Specific examples of the material containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0049] The thickness of the conductive film 120 is not particularly limited as long as it functions as an electrostatic chuck, but is usually about 5 to 100 nm. The thickness of the conductive film 120 is preferably formed so that the film stress is balanced with the multilayer reflective film 20 and the absorber pattern after forming it as an EUV mask, that is, after forming the absorber pattern. The conductive film 120 may be formed before forming the multilayer reflective film 20, or after forming all the films on the multilayer reflective film 20 side of the substrate 10. Also, the conductive film 120 may be formed after forming a part of the films on the multilayer reflective film 20 side of the substrate 10, and then the remaining films on the multilayer reflective film 20 side of the substrate 10 may be formed. The conductive film 120 can be formed, for example, by magnetron sputtering.

[0050] Furthermore, the EUV mask blank may have a resist film 170 formed on the side farthest from the substrate 10 (see FIG. 8). The resist film 170 is preferably an electron beam (EB) resist. The resist film 170 may be formed on the hard mask film 110 and the reflectance reduction layer 160 (see FIG. 6).

[0051] Using the above-mentioned reflective mask blank, pattern drawing and resist pattern formation are performed on the resist film 170 using normal electron beam lithography, and the absorber film 70 underneath is etched away using the resist pattern as an etching mask, forming an etched-away portion and an absorber pattern portion consisting of the absorber film pattern and the resist pattern. Thereafter, the remaining resist film pattern is removed to obtain a reflective mask having a basic structure (see FIG. 9). EXAMPLES

[0052] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0053] [Example 1] A multilayer reflective film 20 was formed on a substrate 10 made of quartz glass having a size of 152 mm square and a thickness of 6.35 mm by DC pulse magnetron sputtering using a molybdenum (Mo) target and a silicon (Si) target, with both targets facing the main surface of the substrate 10 and the substrate 10 rotating. Each target was mounted on a sputtering device capable of mounting two targets and discharging the targets one by one or both simultaneously, and the substrate 10 was placed thereon. First, power was applied to the silicon (Si) target while flowing argon (Ar) gas into the chamber, a silicon (Si) layer having a thickness of 4 nm was formed, and the application of power to the silicon (Si) target was stopped. Next, power was applied to the molybdenum (Mo) target while flowing argon (Ar) gas into the chamber, a molybdenum (Mo) layer having a thickness of 3 nm was formed, and the application of power to the molybdenum (Mo) target was stopped. The operation of forming these silicon (Si) layers and molybdenum (Mo) layers constitutes one cycle, and this was repeated 40 times to form the molybdenum (Mo) layer in the 40th cycle. Finally, after forming a silicon (Si) layer of 3.5 nm using the above-mentioned method, nitrogen (N) gas was further flowed into the chamber to form silicon nitride of about 0.5 nm, thereby forming the multilayer reflective film 20.

[0054] Next, a zirconium (Zr) target and a niobium (Nb) target were used on the multilayer reflective film 20, and the two targets were placed opposite the main surface of the substrate 10. While rotating the substrate 10, a metal oxide layer 55 was formed on the multilayer reflective film 20 by DC pulse magnetron sputtering. After the formation of the multilayer reflective film 20, the substrate 10 on which the multilayer reflective film 20 was formed was placed from the sputtering device on which the multilayer reflective film 20 was formed via a transport path maintained in a vacuum state, without being taken out into the atmosphere. Each target was placed in another sputtering device capable of mounting two targets and discharging the targets one by one or both at the same time, and the substrate 10 on which the multilayer reflective film 20 was formed was placed. First, while flowing argon (Ar) gas at 15 sccm and oxygen (O2) gas at 20 sccm into the chamber, a power of 500 W was applied simultaneously to each of the zirconium (Zr) target and the niobium (Nb) target to form a layer made of ZrO and NbO having a thickness of 0.5 nm. After that, while keeping the power applied to the targets the same, the argon (Ar) gas was changed to 12 sccm and the oxygen (O2) gas to 50 sccm to form a layer with a high oxygen content made of ZrO and NbO having a thickness of 1.5 nm, which was used as the metal oxide layer 55.

[0055] The composition of the protective film 50 is The layer in contact with the multilayer reflective film 20 is Zirconium (Zr) 32 atomic % Niobium (Nb) 23 atomic % The oxygen (O) content was 45 atomic %. The layer furthest from the multilayer reflective film 20 (the layer with the highest oxygen content) is Zirconium (Zr) 25.5 atomic % Niobium (Nb) 18.5 atomic % The oxygen (O) content was 56 atomic %.

[0056] The reflectance of the multilayer reflective film 20, protective film 50, and buffer layer SiN layer 26 on the substrate 10 to EUV light (wavelength 13 to 14 nm) at an incident angle of 6° was measured using euv tech.'s EUV mask fully automatic reflectometer LPR-1016 (same for the following reflectance measurements), and was 65.0%.

[0057] In addition, the multilayer reflective film 20, the protective film 50, and the SiN layer 26 serving as the buffer layer on the substrate 10 were subjected to a heat treatment in an air atmosphere at 200°C for 15 minutes using a hot plate type heating device, and the reflectance to EUV light with an incident angle of 6° was measured and found to be 65.2%, with the difference in reflectance before and after the heat treatment being 0.2%. This means that the heat treatment did not result in a decrease in reflectance, and instead the reflectance improved.

[0058] Next, the compositions of the multilayer reflective film 20 and the protective film 50 before and after the heat treatment were confirmed by XPS, and it was found that the oxygen contents of the metal oxide layer 55 and the multilayer reflective film 20 did not change.

[0059] [Comparative Experiment Example 1] A multilayer reflective film 20 was formed in the same manner as in Experimental Example 1, except that the SiN layer 26 on the surface was replaced with the Si layer 21 (i.e., no SiN layer 26 was provided). Next, in the same manner as in Example 1, argon (Ar) gas was supplied at 12 sccm and oxygen (O2) gas was supplied at 50 sccm into the chamber while simultaneously applying 500 W of power to each of the zirconium (Zr) target and the niobium (Nb) target, forming a layer having a thickness of 2.0 nm and made of ZrO and NbO, similar to Example 1, and no layer with a low oxygen content was provided between the multilayer film.

[0060] The reflectance of the multilayer reflective film 20 and protective film 50 on the substrate 10 to EUV light (wavelength 13 to 14 nm) at an incident angle of 6° was measured using euv tech.'s EUV mask fully automatic reflectometer LPR-1016 (same for the following reflectance measurements), and was found to be 63.8%.

[0061] In addition, the multilayer reflective film 20 and protective film 50 (buffer layer and metal oxide layer 55) on the substrate 10 were subjected to a heat treatment in an air atmosphere at 200°C for 15 minutes using a hot plate type heating device, and the reflectance to EUV light with an incident angle of 6° was measured and found to be 63.8%, with the difference in reflectance before and after the heat treatment being 0.0%, and no decrease in reflectance due to the heat treatment was observed.

[0062] Next, the composition of the multilayer reflective film 20 and the protective film 50 before and after the heat treatment was confirmed by XPS. As a result, the oxygen content inside the metal oxide layer 55 and the multilayer reflective film 20 did not change. However, compared with Example 1, the oxygen content of the Si layer 21 provided on the front surface of the multilayer reflective film 20 was high at 35 atomic %, which may cause an inconvenience in that the reflectivity decreases.

[0063] [Comparative Example 1] The multilayer reflective film 20 was formed in the same manner as in Experimental Example 1, except that the SiN layer on the surface was replaced with the Si layer 21 (i.e., the SiN layer 26 was not provided). Next, a protective film in contact with the multilayer reflective film 20 was formed on the multilayer reflective film 20 by DC pulse magnetron sputtering using a ruthenium (Ru) target while rotating the substrate 10. After the formation of the multilayer reflective film 20, the substrate 10 on which the multilayer reflective film 20 was formed was placed via a transfer path maintained in a vacuum state from the sputtering device on which the multilayer reflective film 20 was formed, without being taken out into the atmosphere. Electric power was applied to the Ru target while flowing argon (Ar) gas into the chamber, and a Ru layer having a thickness of 2.0 nm was formed as the protective film 50.

[0064] The reflectance of the multilayer reflective film 20 and the protective film 50 on the substrate 10 to EUV light (wavelength 13 to 14 nm) at an incident angle of 6° was measured and found to be 65.3%.

[0065] In addition, the multilayer reflective film 20 and protective film 50 on the substrate 10 were subjected to a heat treatment in an air atmosphere at 200°C for 15 minutes using a hot plate type heating device, and then the reflectance to EUV light with an incident angle of 6° was measured and found to be 59.4%, with the difference in reflectance before and after the heat treatment being 5.9%.

[0066] Next, the compositions of the multilayer reflective film 20 and the protective film 50 before and after the heat treatment were confirmed by XPS, and it was found that a diffusion layer of Ru and Si had been formed, and in addition, oxidation of the surface layer of the multilayer reflective film 20 had progressed.

[0067] [Comparative Example 2] The multilayer reflective film 20 was formed in the same manner as in Experimental Example 1, except that a Mo layer 22 was formed to a thickness of 0.5 nm instead of the SiN layer on the surface. In this case, the Mo layer 22 constitutes the multilayer reflective film 20, and the Mo layer 22 is provided on the outermost surface of the multilayer reflective film 20. Next, a protective film in contact with the multilayer reflective film 20 was formed on the multilayer reflective film 20 by DC pulse magnetron sputtering using a ruthenium (Ru) target while rotating the substrate 10. After the formation of the multilayer reflective film 20, the substrate 10 on which the multilayer reflective film 20 was formed was placed from the sputtering device on which the multilayer reflective film 20 was formed via a transfer path maintained in a vacuum state, without being taken out into the atmosphere. Electric power was applied to the Ru target while flowing argon (Ar) gas in the chamber, and a Ru layer with a thickness of 2.5 nm was formed to serve as the protective film 50.

[0068] The reflectance of the multilayer reflective film 20 and the protective film 50 on the substrate 10 to EUV light (wavelength 13 to 14 nm) at an incident angle of 6° was measured and found to be 65.4%.

[0069] In addition, the multilayer reflective film 20 and protective film 50 on the substrate 10 were subjected to a heat treatment in an air atmosphere at 200°C for 15 minutes using a hot plate type heating device, and then the reflectance to EUV light with an incident angle of 6° was measured and found to be 62.9%, with the difference in reflectance before and after the heat treatment being 2.5%.

[0070] Next, the compositions of the multilayer reflective film 20 and the protective film 50 before and after the heat treatment were confirmed by XPS. It was found that the Mo layer 22 suppressed the formation of a diffusion layer of Ru and Si, but oxidation of the Mo layer 22 progressed.

[0071] [Comparative Example 3] A multilayer reflective film 20 was formed in the same manner as in Comparative Example 2. As described above, in this case, a Mo layer 22 was provided on the outermost surface of the multilayer reflective film 20. Next, in the same manner as in Comparative Experimental Example 1, a layer having a thickness of 2.0 nm and made of ZrO and NbO and having a high oxygen content similar to that of Example 1 was formed.

[0072] The reflectance of the multilayer reflective film 20 and protective film 50 on the substrate 10 to EUV light (wavelength 13 to 14 nm) at an incidence angle of 6° was measured to be 57.2%. Furthermore, the multilayer reflective film 20 and protective film 50 on the substrate 10 were subjected to a heat treatment in an air atmosphere at 200°C for 15 minutes using a hot plate type heating device, and then the reflectance of the multilayer reflective film 20 and protective film 50 on the substrate 10 to EUV light at an incidence angle of 6° was measured to be 56.8%, with a difference in reflectance before and after the heat treatment being 0.4%.

[0073] In Comparative Example 3, in which a metal oxide film 51 having a different oxygen content is provided and then a Mo layer is provided on the outermost surface, the decrease in reflectance after heat treatment is small, but the absolute value of the reflectance is small. On the other hand, in Example 1, even when a metal oxide film 51 having a different oxygen content is provided, by disposing a Si layer on the outermost surface instead of a Mo layer, it is very advantageous in that a high reflectance can be achieved while the decrease in reflectance after heat treatment is small. [Explanation of symbols]

[0074] 10 Substrate 20 Multilayer reflective coating 25 Si / Mo laminate 50 Protective film 51 Metal oxide film 55 Metal oxide layer 70 Absorber membrane

Claims

1. A substrate; a multilayer reflective film provided on the substrate and configured to reflect exposure light; a metal oxide film provided on the multilayer reflective film; an absorber film provided on the metal oxide film, containing Ta or Cr, and absorbing exposure light; Equipped with the multilayer reflective film is formed by alternately stacking Mo layers and Si layers, and the layer farthest from the substrate is the Si layer; the oxygen content of the metal oxide film is higher in a layer on a side away from the substrate than in a side on the substrate; the oxygen content of the metal oxide film increases continuously with increasing distance from the substrate throughout the entire range of the metal oxide film in the thickness direction; The reflective mask blank, wherein the metal oxide film does not contain Ru.

2. 2. The reflective mask blank according to claim 1, wherein the metal contained in the metal oxide film is a metal having an extinction coefficient k of less than 0.02 for EUV light having a wavelength of 13.53 nm.

3. 3. The reflective mask blank according to claim 1, wherein the metal oxide film functions as an etching stopper when the absorber film is processed.

4. 4. The reflective mask blank according to claim 1, wherein the metal oxide film contains one or more elements selected from the group consisting of Zr, Nb, Ti and Y.

5. 5. The reflective mask blank according to claim 1, wherein the oxygen content of the layer of the metal oxide film on the side away from the substrate does not change by heat treatment at 120° C. to 200° C.

6. 6. The reflective mask blank according to claim 1, wherein the thickness of the metal oxide film is 0.5 nm or more and less than 3.5 nm.

7. The metal oxide film has a multi-layer structure, A reflective mask blank as described in any one of claims 1 to 6, characterized in that the oxygen content in a second layer located away from the substrate is higher than that in a first layer located on the substrate side.

8. 8. The reflective mask blank according to claim 1, wherein the Si layer of the multilayer reflective film that is furthest from the substrate contains a light element other than oxygen on the metal oxide film side.

9. an oxidation prevention layer including a light element other than oxygen on the metal oxide film side between the Si layer of the multilayer reflective film that is farthest from the substrate and the metal oxide film; 9. The reflective mask blank according to claim 1, wherein the oxidation prevention layer has a thickness of 0.2 nm or more and 3 nm or less.

10. 10. The reflective mask blank according to claim 8, wherein the light element is at least one of nitrogen, carbon and boron.

11. The reflective mask blank according to any one of claims 1 to 10, characterized in that when a first reflectance for EUV light having a wavelength of 13.53 nm before a heat treatment at 120 to 200°C is compared with a second reflectance for EUV light having a wavelength of 13.53 nm after a heat treatment at 120 to 200°C, a change in the second reflectance relative to the first reflectance is 0.5% or less.

12. A method for producing a reflective mask by using the reflective mask blank according to claim 1 .

Citation Information

Patent Citations

  • Reflective photomask

    JP2002122981A

  • Reflective mask blank, method of manufacturing the same and method of manufacturing reflective mask

    JP2010092947A

  • Optical element, exposure device, and manufacturing method of device

    JP2014116498A

  • Reflective mask blank for EUV lithography and manufacturing method thereof

    JP2014127630A

  • Extreme ultraviolet capping layer, and method for manufacturing and lithography of extreme ultraviolet capping layer

    JP2017521711A